Polyurethane multilayer film and its manufacturing method
A polyurethane multilayer film with a flexible coating and nano-modified silicon dioxide enhances smoothness and adhesive strength, addressing the poor smoothness and visibility issues of conventional TPU films, providing effective thermal insulation and protection for automotive applications.
Patent Information
- Application Number
- JP2024524427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-02-26
- Filing Date
- 2022-05-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-05-18
AI Technical Summary
Conventional thermoplastic polyurethane elastomer base films used for automotive paint protection and thermal insulation in cars suffer from poor smoothness due to high viscosity, leading to light scattering and visibility issues under high-temperature conditions, and they cannot be applied using the casting method.
A polyurethane multilayer film is manufactured using a flexible polyurethane coating with carboxylic acid silane-modified nano silicon dioxide and 8-mercapto-1-octanethiol, combined with plasma discharge treatment, to improve adhesive strength and smoothness, and includes a thermal barrier nanomaterial layer.
The film achieves superior smoothness, improved adhesive strength, and effective thermal barrier properties, with excellent scratch resistance and weatherability, maintaining visibility and protection under high-temperature conditions.
Smart Images

Figure 2024539688000001 
Figure 2024539688000002 
Figure 2024539688000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of film manufacturing, and in particular to a polyurethane multilayer film and a method for producing the same. [Background technology]
[0002] Traditionally, there are many types of automotive paint protection films on the market, and most of them are structured by attaching a general PVC (polyvinyl chloride) adhesive film to the automotive paint to protect it from external friction damage. As the plasticizer contained in the PVC base film gradually migrates to the surface over time, the PVC protection film gradually hardens and becomes brittle in the latter half of the usage period, and when the plasticizer is transferred to the adhesive layer, the protection film is scratched, bubbles are generated, peeled off, and other phenomena occur, resulting in a very poor appearance. Therefore, nowadays, thermoplastic polyurethane elastomer base film is gradually being used as an automotive paint protection film.
[0003] Furthermore, because polyurethane elastomer base films have the ability to absorb shock, in addition to being used as protective films for automobile paint, they are also beginning to replace the current PET heat-shielding adhesive films for automobile glass, providing heat-shielding properties as well as shock resistance and scratch resistance.
[0004] However, a problem with applying heat-shielding adhesive films to automobile windshields is that all general TPU (thermoplastic polyurethane elastomer rubber) base films are produced by melting and casting TPU particles at high temperatures (120-200°C) and then cooling them. Because the viscosity of the TPU melt is usually high, the smoothness of the TPU base film obtained by casting TPU particles is poor, and the final surface roughness of the TPU film is high. When used on automobile windshields, the windshield is inclined and forms an acute angle with the line of sight of the person, so the surface roughness of the TPU film scatters light and affects visibility. Therefore, a self-repairing heat-shielding adhesive film with better smoothness is needed. Summary of the Invention
[0005] The present invention relates to a polyurethane multilayer film and a method for producing the same.
[0006] The present invention employs a coating method and a core structure of soft PU coating / pressure-sensitive adhesive / soft PU coating to replace the traditional TPU base film, which solves the problem of poor smoothness of the TPU base film produced by the casting method.
[0007] According to the inventor's research results, a flexible polyurethane coating is directly formed using a flexible polyurethane coating liquid, and then the thin film layer is subjected to plasma discharge treatment. Since the flexible polyurethane coating contains carboxylic acid silane-modified nano-silicon dioxide and 8-mercapto-1-octanethiol, it can not only improve the adhesive strength of each thin film layer, but also effectively avoid the adverse effects of thin film particles causing light scattering, and the smoothness performance of the thin film can be improved.
[0008] The present invention provides a method for producing a polyurethane multilayer film, comprising the steps of: (1) A process of applying a flexible polyurethane coating liquid to the surface of a polyethylene terephthalate release film and drying it to form a flexible polyurethane film coating, followed by a plasma discharge treatment. (2) A step of applying a pressure-sensitive adhesive liquid to the surface of the flexible polyurethane film coating of step (1) to form a pressure-sensitive adhesive layer. (3) A process of applying a flexible polyurethane coating liquid to the surface of another polyethylene terephthalate release film and drying it to form a flexible polyurethane film coating, which is then subjected to a plasma discharge treatment, and then combined with the pressure-sensitive adhesive layer of step (2). (4) A process of peeling off two polyethylene terephthalate release films, applying a coating containing a heat-shielding nanomaterial to the surface of the flexible polyurethane film coating on one side, baking and hardening it, and applying a pressure-sensitive adhesive liquid to the surface of the other flexible polyurethane film coating. In steps (1) and (3), the raw material composition of the flexible polyurethane coating liquid is as follows: water-based polyurethane resin, carboxylic acid silane-modified nano silicon dioxide, metal oxide nanoparticles, 8-mercapto-1-octanethiol, a wetting agent, an antifoaming agent, and deionized water.
[0009] Of these, the pressure-sensitive adhesive liquid is preferably an acrylic pressure-sensitive adhesive.
[0010] In the present invention, 8-mercapto-1-octanethiol can effectively improve the dispersibility of particles, and the mercapto group at the end of the molecule can modify nano-silica and metal oxide nanoparticles, making the particles easier to disperse.The other hydroxyl group at the end of the molecule can participate in the curing reaction of the aqueous polyurethane resin to form a spatial network structure, which can make the particles more uniformly dispersed in the polyurethane coating solution, and can also improve the adhesive and mechanical properties of the flexible polyurethane coating.
[0011] Of these, the metal oxide nanoparticles are preferably one or more of titanium dioxide nanoparticles, alumina nanoparticles, and zinc oxide nanoparticles.
[0012] Among them, the wetting agent is preferably dispersant SN-5040.
[0013] Among them, the defoamer is preferably defoamer CF-16, and the water-based polyurethane resin is preferably polyurethane dispersion SYNTEGRA® purchased from Dow, or polyurethane dispersion Bayhydrol® purchased from Bayer.
[0014] Of these, the gas used in the plasma discharge treatment is preferably nitrogen.
[0015] Of these, the carboxylic acid silane is preferably 4(4-carboxyanisyl)silane.
[0016] Among them, the carboxylic acid silane modified nano silicon dioxide is preferably produced by mixing silicon dioxide sol and carboxylic acid silane in a solvent DMF, and then heating and reacting them in a vacuum sealed state. The heating reaction temperature is preferably 90 to 100°C, and the heating reaction time is preferably 20 to 30 hours. The baking hardening temperature in step (4) is preferably 70 to 120° C., and the time is preferably 1 to 8 minutes.
[0017] The present invention also provides a polyurethane multi-layer film produced by the above-mentioned production method.
[0018] The polyurethane multilayer film of the present invention has a laminated structure in which, from the bottom up, a pressure-sensitive adhesive layer, a soft polyurethane coating, a pressure-sensitive adhesive layer, a soft polyurethane coating, and a heat-shielding nanomaterial layer are laminated together. It is preferred that the pressure sensitive adhesive layer has a thickness of from 10 to 20 microns. Preferably the flexible polyurethane coating has a thickness of 20 to 50 microns. The thermal barrier nanomaterial layer preferably has a thickness of 5 to 15 microns. Any combination of the above optimum conditions within the scope of common knowledge in the art will result in each optimum embodiment of the present invention. All reagents and materials used in the present invention are commercially available.
[0019] The positive effect of the present invention is that the core structure of flexible PU coating / pressure sensitive adhesive / flexible PU coating can be used to replace the traditional TPU base film, solving the problem of poor smoothness of the TPU base film produced by the casting method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Specific Examples The present invention will be further described below through examples, but the present invention is not limited to the scope of the examples. In the following examples, the experimental methods not specifically described should be performed according to the usual methods and conditions or according to the product instructions.
[0021] Solvent resistance test method: 1 ml of 2-methylbenzene is sprayed onto the surface of the test material, and after 30 seconds, it is wiped off with a wipe. If there is no obvious change in the appearance of the material (such as melting deformation or peeling of the coating), it is considered to have passed the solvent resistance test.
[0022] Self-repair test method: A straight wire brush is used to make brush marks on the surface of the thin film, and then the brush marks are observed to see if they disappear naturally after one hour or if they are exposed to a heat source (such as hot water). If they disappear, the material is considered to have a self-repair function.
[0023] Gloss evaluation method: A soft polymer substrate with a self-repairing coating is attached to a black metal plate, and the gloss of the material surface is observed from the front and side (45 degrees). If the surface is smooth, reflective, and the reflection is clear and sharp, it is considered to have a good gloss, otherwise it is considered to have a bad gloss.
[0024] Stain resistance evaluation method: Mark the coating surface with an oil-based black marker Dixie 6881, leave the mark for one day after it dries, then wipe it off directly with a glasses cloth or wipe it off with a glasses cloth soaked in anhydrous alcohol to observe the removal of the mark. If the mark can be completely wiped off and no trace remains, it is considered to have excellent stain resistance, if the mark cannot be wiped off, it is considered to have poor stain resistance, and if the mark can be wiped off but only a slight trace remains, it is considered to have good stain resistance.
[0025] Breaking elongation test method: Cut the test material into a strip 5 cm wide and 2 cm long, mark the center 2 cm long, apply force to stretch it to both sides, measure the length of the marked part at the time when a crack appears as L1, and then calculate the breaking elongation according to the following formula. Breaking elongation rate (%) = (L1-2) / 2
[0026] The weather resistance test method is as follows: Use Eye Super UV Tester W-151 (Iwasaki Electric Co., Ltd.) to perform weather resistance performance test. One cycle is kept under 63℃ temperature, 50% relative humidity, 50 watts / square centimeter illuminance, water spray 10 seconds / hour for 5 hours, and then kept under 30℃ temperature and 95% relative humidity for 1 hour. After repeating the above weather resistance cycle 300 times, observe the coating with the naked eye and a microscope (×250). If no cracks or local peeling are found, it indicates that the coating surface is good and the weather resistance performance is excellent. All compositions are listed by weight.
[0027] The pressure sensitive adhesive layer is a pressure sensitive adhesive formulation commonly used in the art, specifically, acrylic acid, methyl acrylate, myristic, [ka] , butadiene, and toluene.
[0028] For the coating of the thermal barrier nanomaterial, a thermal barrier coating commonly used in the art is adopted; all values in the following examples are by weight.
[0029] Example 1 The manufacturing process of polyurethane multilayer film is as follows:
[0030] (1) The flexible polyurethane coating liquid is applied to the surface of a polyethylene terephthalate release film and dried to form a flexible polyurethane film coating, and then a plasma discharge treatment is performed; the gas used in the plasma discharge treatment is nitrogen, and the time is 10 minutes.
[0031] (2) An acrylic pressure-sensitive adhesive liquid is applied to the surface of the soft polyurethane film coating of step (1) to form a pressure-sensitive adhesive layer.
[0032] (3) A flexible polyurethane coating liquid is applied to the surface of another polyethylene terephthalate release film and dried to form a flexible polyurethane film coating, which is then subjected to plasma discharge treatment (the gas used for the plasma discharge treatment is nitrogen, and the treatment time is 10 minutes), and then combined with the pressure-sensitive adhesive layer from step (2).
[0033] (4) Peel off the two polyethylene terephthalate release films, apply a coating containing a heat-shielding nanomaterial to the surface of the polyurethane film coating on one side and bake to harden it (bake at 70°C for 8 minutes); apply an acrylic pressure-sensitive adhesive liquid to the surface of the other polyurethane film coating.
[0034] In this example, the raw material formulation of the flexible polyurethane coating solution includes the following weight amounts: 20 parts waterborne polyurethane resin, 10 parts carboxylic acid silane modified nano silicon dioxide, 5 parts metal oxide nanoparticles, 3 parts 8-mercapto-1-octanethiol, 1 part wetting agent, 1 part defoamer, and 20 parts deionized water.
[0035] In this example, the metal oxide nanoparticles are titanium dioxide nanoparticles, the wetting agent is dispersant SN-5040, the defoamer is defoamer CF-16, and the waterborne polyurethane resin is polyurethane dispersion SYNTEGRA® purchased from Dow.
[0036] The carboxylic acid silane modified nano silicon dioxide was prepared by mixing silicon dioxide sol and 4(4-carboxyanisyl)silane in the solvent DMF and heating the mixture in a vacuum sealed state at 90°C for 30 hours.
[0037] The polyurethane multilayer film produced in this embodiment is a laminated composite of a pressure-sensitive adhesive layer, a flexible polyurethane coating, a pressure-sensitive adhesive layer, a flexible polyurethane coating, and a heat-shielding nanomaterial layer, from the bottom up. The thickness of the pressure-sensitive adhesive layer is 10 microns. The thickness of the flexible polyurethane coating is 20 microns. The thickness of the heat-shielding nanomaterial layer is 5 microns.
[0038] The test results are as follows: (1) The adhesive strength of the polyurethane coating is excellent, does not peel off easily, and reaches ASTM 5B in cross-cut tests.
[0039] (2) The breaking elongation reaches 400% and the breaking strength reaches 45 MPa.
[0040] (3) It has excellent abrasion resistance, and will not be scratched even if it is rubbed back and forth more than 1,000 times with a load of 1 kg of 0000# steel wire.
[0041] (4) Excellent weather resistance: after 300 weather cycles, no cracks or localized peeling was still observed on the coating surface.
[0042] (5) The thin film is smooth and has excellent smoothness performance, with a gloss level of 98 at 20 degrees.
[0043] Example 2 The manufacturing process of polyurethane multilayer film is as follows:
[0044] (1) A flexible polyurethane coating solution is applied to the surface of a polyethylene terephthalate release film and dried to form a flexible polyurethane film coating, and then a plasma discharge treatment is performed. The gas used in the plasma discharge treatment is nitrogen, and the time is 15 minutes.
[0045] (2) An acrylic pressure-sensitive adhesive liquid is applied to the surface of the soft polyurethane film coating of step (1) to form a pressure-sensitive adhesive layer.
[0046] (3) A flexible polyurethane coating liquid is applied to the surface of another polyethylene terephthalate release film and dried to form a flexible polyurethane film coating, which is then subjected to plasma discharge treatment (the gas used for the plasma discharge treatment is nitrogen, and the treatment time is 15 minutes), and then combined with the pressure-sensitive adhesive layer from step (2).
[0047] (4) Two polyethylene terephthalate release films are peeled off, and a coating containing a heat-shielding nanomaterial is applied to the surface of one of the polyurethane film coatings and baked for hardening (baked at 100°C for 5 minutes). An acrylic pressure-sensitive adhesive liquid is applied to the surface of the other polyurethane film coating.
[0048] In this example, the raw material formulation for the flexible polyurethane coating solution includes the following weight amounts: 25 parts waterborne polyurethane resin, 13 parts carboxylic acid silane modified nano silicon dioxide, 7 parts metal oxide nanoparticles, 3 parts 8-mercapto-1-octanethiol, 1 part wetting agent, 1 part defoamer, and 30 parts deionized water.
[0049] In this example, the metal oxide nanoparticles are alumina nanoparticles, the wetting agent is dispersant SN-5040, the defoamer is defoamer CF-16, and the water-based polyurethane resin is a polyurethane dispersion Bayhydrol® purchased from Bayer.
[0050] The carboxylic acid silane modified nano silicon dioxide was prepared by mixing silicon dioxide sol and 4(4-carboxyanisyl)silane in the solvent DMF and heating the mixture in a vacuum sealed state at 100°C for 25 hours.
[0051] The polyurethane multilayer film produced in this embodiment is a laminated composite of a pressure-sensitive adhesive layer, a flexible polyurethane coating, a pressure-sensitive adhesive layer, a flexible polyurethane coating, and a heat-shielding nanomaterial layer, from the bottom up. The thickness of the pressure-sensitive adhesive layer is 20 microns. The thickness of the flexible polyurethane coating is 50 microns. The thickness of the heat-shielding nanomaterial layer is 15 microns.
[0052] The test results are as follows: (1) The adhesive strength of the polyurethane coating is excellent, does not peel off easily, and reaches ASTM 5B in cross-cut tests.
[0053] (2) The breaking elongation reaches 400% and the breaking strength reaches 46 MPa.
[0054] (3) It has excellent abrasion resistance, and will not be scratched even if it is rubbed back and forth more than 1,000 times with a load of 1 kg of 0000# steel wire.
[0055] (4) Excellent weather resistance: after 300 weather cycles, no cracks or localized peeling was still observed on the coating surface.
[0056] (5) The thin film is smooth and has excellent smoothness performance, with a gloss level of 99 at 20 degrees.
[0057] Comparative Example 1 In this comparative example, the raw material formulation of the flexible polyurethane coating solution does not contain carboxylic acid silane modified nano-silicon dioxide, and other parameters are the same as those in Example 1 to prepare a polyurethane multi-layer film. When its performance is tested, the surface of the thin film is not smooth to the naked eye, and the gloss value at 20 degrees is 81.
[0058] Comparative Example 2 In this comparative example, 8-mercapto-1-octanethiol in the raw material formulation of the flexible polyurethane coating solution is replaced with normal octanethiol, and other parameters are the same as those in Example 1 to produce a polyurethane multilayer film. When its performance is tested, the surface of the thin film is not smooth to the naked eye, with a gloss value of 20 degrees and an orange peel value of 85.
Claims
1. (1) applying a flexible polyurethane coating liquid onto a surface of a polyethylene terephthalate release film and drying the same to form a flexible polyurethane film coating, followed by plasma discharge treatment; (2) applying a pressure-sensitive adhesive liquid to the surface of the flexible polyurethane film coating of step (1) to form a pressure-sensitive adhesive layer; (3) applying a flexible polyurethane coating liquid onto the surface of another polyethylene terephthalate release film and drying it to form a flexible polyurethane film coating, and then carrying out plasma discharge treatment, and then combining with the pressure-sensitive adhesive layer of step (2); (4) Peel off the two polyethylene terephthalate release films, apply a coating containing a heat-shielding nano material to the surface of the soft polyurethane film coating on one side, and bake to harden it; applying a pressure sensitive adhesive liquid to the surface of the other soft polyurethane film coating; In steps (1) and (3), The raw material formulation of the flexible polyurethane coating liquid is as follows: water-based polyurethane resin, carboxylic acid silane modified nano silicon dioxide, metal oxide nanoparticles, 8-mercapto-1-octanethiol, wetting agent, defoamer, and deionized water. A method for producing a polyurethane multilayer film comprising the steps of:
2. 2. The method for producing a polyurethane multilayer film according to claim 1, wherein the pressure-sensitive adhesive liquid is an acrylic pressure-sensitive adhesive.
3. 2. The method for producing a polyurethane multilayer film according to claim 1, wherein the metal oxide nanoparticles are at least one of titanium dioxide nanoparticles, alumina nanoparticles, and zinc oxide nanoparticles.
4. the wetting agent is dispersant SN-5040, the defoamer is defoamer CF-16, 2. The method for producing a polyurethane multilayer film according to claim 1, wherein the aqueous polyurethane resin is a polyurethane dispersion SYNTEGRA (registered trademark) purchased from Dow Chemical or a polyurethane dispersion Bayhydrol (registered trademark) purchased from Bayer.
5. The gas used in the plasma discharge treatment is nitrogen. The method for producing the polyurethane multilayer film according to claim 1.
6. The carboxylic acid silane is 4(4-carboxyanisyl)silane. A method for producing the polyurethane multilayer film according to claim 1.
7. The carboxylic acid silane modified nano silicon dioxide is produced by the following method: Silicon dioxide sol and carboxylic acid silane are mixed in a solvent DMF, and reacted by heating in a vacuum sealed state. The temperature of the heating reaction is preferably 90 to 100°C. The heating reaction time is preferably 20 to 30 hours. The method for producing the polyurethane multilayer film according to claim 1.
8. The method for producing a polyurethane multilayer film according to any one of claims 1 to 8, characterized in that the baking hardening in step (4) is carried out at a temperature of 70 to 120°C for a time of 1 to 8 minutes.
9. A polyurethane multilayer film produced by the method according to any one of claims 1 to 8.
10. The polyurethane multilayer film is formed by laminating a pressure-sensitive adhesive layer, a flexible polyurethane coating, a pressure-sensitive adhesive layer, a flexible polyurethane coating, and a thermal barrier nanomaterial layer in order from the bottom; Preferably, the pressure sensitive adhesive layer has a thickness of 10 to 20 microns; Preferably, the soft polyurethane coating has a thickness of 20 to 50 microns; The thickness of the thermal barrier nanomaterial layer is preferably 5 to 15 microns; The polyurethane multilayer film according to claim 9.
Citation Information
Patent Citations
Flexible window-shield made of plastic
JP1983171953A
Multi-layer polyurethane protective film
JP2008539107A
Aqueous polyurethane resin dispersion and use thereof
JP2017048304A
Aqueous coating composition for applying uv resistant topcoats in coil coating processes
JP2018516163A
Protective film for windshield of vehicle
JP2022022055A