Method for manufacturing transparent sintered silica using amorphous silica nanopowder
Optimal molding and heat treatment of spherical amorphous silica nanopowder address light scattering issues in sintered silica bodies, resulting in high-transmittance silica suitable for semiconductor and solar cell applications.
Patent Information
- Application Number
- JP2024527071
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-03
- Filing Date
- 2021-11-11
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-11-11
AI Technical Summary
The existing methods for producing transparent sintered silica bodies face issues with light scattering due to the presence of pores, grain boundaries, and crystal phases, leading to a sharp decrease in translucency.
A method involving optimal molding conditions and heat treatment processes to minimize and homogenize pore size, utilizing spherical amorphous silica nanopowder, and controlling sintering parameters to maximize densification through viscous flow.
The method produces a transparent silica sintered body with improved light transmission, achieving high transmittance in both ultraviolet and infrared regions, suitable for applications in semiconductor, display, and solar cell industries.
Smart Images

Figure 2024539762000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a transparent silica sintered body using an amorphous silica nanopowder. [Background technology]
[0002] Silica glass is a glass made of a high-purity amorphous phase and has a low thermal expansion coefficient (0.5×10 -6 / ℃), excellent chemical durability, and high electrical resistance (1,016 Ω·cm), making it used in lab equipment, insulators, etc. Quartz glass also has high transmittance in the ultraviolet and visible light ranges, making it the most widely used material for process parts in the semiconductor, display, and solar cell industries, such as lenses, optical materials, photomask substrates, and lens materials for excimer stepper equipment.
[0003] Quartz glass can be broadly divided into fused quartz glass and synthetic quartz glass, depending on the manufacturing method. The biggest difference between the two manufacturing methods is in the starting material. Fused quartz glass is manufactured by melting natural quartz at high temperatures. Therefore, it has the disadvantage of being somewhat inferior in transparency due to the presence of metal impurities and low purity, and requires high manufacturing costs because it is melted and processed at high temperatures of over 1,800°C.
[0004] Synthetic silica glass is manufactured by chemical vapor deposition method using silicon tetrachloride (SiCl4) and alkoxide method. Therefore, it has an advantage of having better optical properties because it has a lower impurity content than fused silica glass, but has a disadvantage of requiring high investment in consideration of corrosion resistance of equipment and human safety during the process due to the corrosiveness, volatility, and toxicity of harmful gases generated during the manufacturing process.
[0005] Unlike conventional manufacturing methods, amorphous transparent quartz can be manufactured through molding and sintering processes using nano-sized circular silica powder that exhibits an amorphous phase. The sintering behavior of materials that exhibit an amorphous phase is dominated by densification behavior using viscous flow, unlike sintering of crystalline phase. In this sintering behavior, particles move due to the increase in fluidity with increasing temperature, and grain boundaries and pores are removed, resulting in densification. When the amorphous phase material reaches a certain temperature or higher during the sintering process, crystallization occurs, and particle movement mechanisms such as diffusion are expressed. However, the energy required to densify the sintered body is consumed in switching from the amorphous phase to the crystalline phase, and therefore further densification by viscous flow does not occur. At this time, if there are pores, grain boundaries, and crystalline phases that could not be removed inside the sintered body, they scatter light, resulting in a rapid decrease in the translucency of the sintered body.
[0006] All patents and references mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication was individually and specifically indicated by reference. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention relates to a method for producing a transparent silica sintered body by sintering amorphous silica nanopowder. The object of the present invention is to provide a method for producing a transparent silica sintered body, which can solve the problem that if unremoved pores, grain boundaries, and crystal phases exist inside the silica sintered body, the light is scattered, and the light transmittance of the sintered body is rapidly reduced. [Means for solving the problem]
[0008] In order to overcome the conventional problems in producing a transparent sintered silica body by sintering silica, the present invention provides a method for producing a transparent sintered silica body, including optimal molding conditions under which the pore size in an amorphous silica molded body is minimized and homogenized, thereby smoothly removing pores, and optimal heat treatment conditions under which the densification process due to viscous flow in the molded body is maximized. Effect of the Invention
[0009] The present invention provides a method for producing a silica molded body in which the pore size is minimized and homogenized, and thus pores can be easily removed, and a heat treatment method for producing a silica sintered body with excellent transparency by maximizing the densification process due to viscous flow in the silica molded body during sintering. Therefore, the present invention has an advantage that transparent quartz glass with improved light transmittance can be produced by using amorphous silica nanopowder. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 shows the results of analysis of the amorphous silica nanopowder of the present invention, where panel (a) shows the microstructure of the amorphous silica nanopowder, panel (b) shows the crystallinity of the amorphous silica nanopowder, and panel (c) shows the Fourier transform infrared spectroscopy (FT-IR) analysis of the amorphous silica nanopowder. [Diagram 2] The results are shown below, which are the results of a transparent silica sintered body of the present invention being produced by heat treatment at 1200 to 1350° C. for 1 hour. [Diagram 3] The results are shown below, which are the results of the transparent silica sintered body of the present invention being produced by heat treatment at 1350° C. for 1 hour. [Figure 4]1 shows the results of scanning electron microscopy (SEM) analysis of a cut surface of a transparent silica sintered body of the present invention. Panel (a) shows a sintered body produced by heat treatment at 1200°C, panel (b) shows a sintered body produced by heat treatment at 1250°C, panel (c) shows a sintered body produced by heat treatment at 1275°C, panel (d) shows a sintered body produced by heat treatment at 1300°C, panel (e) shows a sintered body produced by heat treatment at 1325°C, and panel (f) shows a sintered body produced by heat treatment at 1350°C. [Diagram 5] 1 shows the results of analyzing the transparent silica sintered body of the present invention by X-ray diffraction (XRD). [Figure 6] The transparent silica sintered body of the present invention was produced by sintering at 1325° C. Panel (a) shows a photograph of the sintered body, and panel (b) shows the surface microstructure. [Figure 7] The results are shown for the transparent silica sintered body of the present invention, which was produced by heat treating it at 1215° C. for 12 hours, 18 hours, 24 hours, and 30 hours. [Figure 8] 1 shows the results of scanning electron microscopy (SEM) analysis of cut sections of the transparent silica sintered body of the present invention, where panel (a) shows a sintered body produced by heat treatment at 1215° C. for 12 hours, panel (b) shows a sintered body produced by heat treatment at 1215° C. for 18 hours, panel (c) shows a sintered body produced by heat treatment at 1215° C. for 24 hours, and panel (d) shows a sintered body produced by heat treatment at 1215° C. for 30 hours. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention provides a method for producing a transparent silica sintered body using sintering, the method including: a first step of preparing a silica powder; a second step of compressing and molding the silica powder to produce a molded body; and a third step of heat-treating the molded body at a temperature of 1310 to 1340°C at a heating rate of 2°C / min for 50 to 240 minutes, or at a temperature of 1200 to 1230°C at a heating rate of 2°C / min for 20 to 28 hours to produce a transparent silica sintered body.
[0012] The silica powder is characterized in that it has an amorphous spherical particle shape, and the molded body is manufactured by subjecting the silica powder to a primary molding by uniaxial pressing and then a secondary molding by cold isostatic pressing.
[0013] The transparent silica sintered body produced by the above-mentioned manufacturing method is characterized in that the shrinkage of the molded body after heat treatment is 45.5 to 47.5%, and that it transmits 19% to 58% of light in the ultraviolet range (wavelength of 200 to 380 nm) and 84% to 85% of light in the infrared range (2000 to 2400 nm).
[0014] (Mode for carrying out the invention) The present invention provides a method for producing a transparent silica sintered body, comprising the steps of:
[0015] The method includes a first step of preparing a silica powder, a second step of compression-molding the silica powder to produce a molded body, and a third step of heat-treating the molded body at a temperature of 1310 to 1340°C at a heating rate of 2°C / min for 50 to 240 minutes, or at a temperature of 1200 to 1230°C at a heating rate of 2°C / min for 20 to 28 hours to produce a transparent silica sintered body.
[0016] The manufacturing method of the present invention provides a transparent silica sintered body having high light transmittance and high transparency. To this end, the present invention establishes optimal molding conditions to make the pore size in the molded body small and uniform, and optimal sintering conditions to maximize densification due to viscous flow of the molded body.
[0017] The silica powder is characterized in that it has the shape of amorphous spherical particles, and is preferably spherical amorphous silica powder with an average particle diameter of 10 to 900 nm. The silica powder is characterized in that it is manufactured by performing a primary molding by uniaxial pressing and a secondary molding by cold isostatic pressing. The uniaxial pressing refers to a method of compressing powder by applying pressure in a single axial direction in an inelastic mold, and the cold isostatic pressing refers to a method of compressing powder by applying pressure in an elastic mold by isostatic pressure using a liquid. The cold isostatic pressing has the advantage of having a constant molding density regardless of size, shape, and position because it is molded by isostatic pressure. The primary molding is a process of mainly forming the shape of the molded body, and the secondary molding is a process of making the pore size in the molded body small and uniform.
[0018] According to an embodiment of the present invention, the molding density of the molded body obtained by the primary molding by the uniaxial pressing and the secondary molding by the cold isostatic pressing is 1 to 1.2 g / cm 3 For this purpose, molding is preferably performed at a molding pressure of 170 to 230 MPa and for a holding time of 3 to 7 minutes.
[0019] The molded body produced using the primary and secondary moldings is heat-treated at a temperature of 1310 to 1340°C at a heating rate of 2°C / min for 50 to 240 minutes, or at a temperature of 1200 to 1230°C at a heating rate of 2°C / min for 20 to 28 hours to produce a transparent silica sintered body.
[0020] The condition of sintering at a temperature of 1310 to 1340°C has an advantage that a transparent sintered body can be produced by heat treatment for only 50 to 240 minutes. If the sintering temperature is lower than 1310°C or if the heat treatment is performed at a temperature exceeding 1340°C, the transparency of the sintered body may decrease.
[0021] The sintering temperature of 1200 to 1230°C is a condition in which a transparent sintered body can be produced by carrying out a heat treatment for 20 to 28 hours. If the sintering temperature is less than 1200°C or if the heat treatment is carried out at a temperature exceeding 1230°C, the transparency of the sintered body may decrease.
[0022] The transparent silica sintered body produced by the production method of the present invention is characterized in that the shrinkage of the molded body after heat treatment is 45.5 to 47.5%, and the density of the sintered body is 2.15 g / cm 3 The study is characterized by an increase in the
[0023] The transparent silica sintered body produced by the production method of the present invention is characterized by transmitting 19% to 58% of light in the ultraviolet region (wavelengths of 200 to 380 nm) and 84% to 85% of light in the infrared region (2000 to 2400 nm).
[0024] The present invention will be described in detail below with reference to examples.
[0025] Working Example
[0026] 1. Experimental Method
[0027] 1) Silica raw powder
[0028] The silica raw material powder for producing the molded body of the present invention was purchased from Sukgyung AT Co., Ltd., Korea (SG-700). The particle size and shape of the silica raw material powder were observed using a Field Emission Scanning Electron Microscope (JSM-7100F, manufactured by JEOL Co., Ltd.). In addition, the crystal phase and bond structure of the starting powder were analyzed using an X-Ray Diffractometer (Smartlab®, manufactured by Rigaku Co., Ltd.) and a Fourier transform infrared spectrometer (FT-Infrared Spectrometer, Spectrum400, manufactured by PerkinElmer Co., Ltd.).
[0029] 2) Manufacturing of molded bodies
[0030] A primary green body having a disk shape with a size of Φ15mm×2mm was produced by placing 0.5g of silica powder in a circular mold with a diameter of 15mm and uniaxially pressing it for 1 minute at a pressure of 100psi. In order to increase the packing density of the primary green body, cold isostatic pressing was performed for 5 or 10 minutes at a pressure of 150MPa to 250MPa to obtain a secondary green body (final green body). The green density of the green body was measured using a dimensional measurement method and compared.
[0031] 3) Sintering of the green body
[0032] The secondary compact was sintered in an electric furnace under an air atmosphere. The sintering was performed by heat treatment at 1200-1350°C for 1 hour at a heating rate of 2°C / min. SEM and XRD analyses were performed on the sintered compacts (specimens) sintered under different temperature conditions to examine the microstructure and the presence or absence of crystallization.
[0033] In addition, we attempted to manufacture transparent sintered bodies by adjusting the sintering holding time to 12, 18, 24, and 30 hours at 1215°C, a relatively low temperature at which crystallization does not occur, and analyzed the density, microstructure, and crystal phase of the obtained specimens.
[0034] The transmittance of the sintered body was analyzed and compared using an ultraviolet-visible light spectrophotometer (UV-Vis Spectrometer, Lambda365, manufactured by PerkinElmer).
[0035] 2. Experimental Results
[0036] As shown in FIG. 1, the silica powder used in the present invention was confirmed to have an amorphous spherical particle shape and a particle size of about 700 nm. Panel (c) of FIG. 1 shows the FT-IR spectrum results obtained by analyzing the powder structure. As a result of the experiment, no peaks such as those of hydroxyl groups other than the silica structure were observed. In the FT-IR spectrum results shown in FIG. 1, -1 The peak at 808 cm represents the bending vibration of the Si–O bond. -1 The peak at 1,103 cm represents the symmetrical stretching vibration of Si-O-Si, which connects oxygen between tetrahedra. -1 The peak indicates the Si-O-Si asymmetric stretching structure of the bridging oxygen in the tetrahedron.
[0037] Hydroxyl groups and impurities promote the nucleation of amorphous silica particles and at the same time lower the crystallization temperature of amorphous silica to promote the formation of a crystalline phase, so it is preferable that they are not present in order to produce a dense light-transmitting sample. Therefore, it is recognized that the silica powder used in the present invention is a very suitable powder.
[0038] During the cold isostatic pressing process using the silica powder, various green bodies were manufactured by adjusting the forming pressure (MPa) and holding time (min). Table 1 shows the green density (g / cm) of each green body manufactured by this method. 3 ) is shown.
[0039] [Table 1]
[0040] The green compact produced by molding for 5 minutes at a pressure of 200 MPa had a green density of 1.12 g / cm 3 It was confirmed that even if a higher pressure and holding time were applied, a relatively constant green density value was maintained. Therefore, it was decided that all subsequent green bodies would be manufactured by molding for 5 minutes under a pressure of 200 MPa.
[0041] Fig. 2 shows a visual comparison of the degree of translucency of sintered samples heat-treated at each sintering temperature of the present invention. It can be seen that the translucency of the samples increases as the sintering temperature increases from 1200°C to 1325°C. In particular, the samples heat-treated at 1325°C showed the best translucency.
[0042] However, when the sintering temperature was further increased, it was confirmed by visual inspection that the material became opaque again. In particular, unlike the sintered body heat-treated at a lower temperature, the specimen sintered at 1350℃ showed a transparent interior, although the exterior was opaque. Figure 3 shows the difference between the surface and interior of the specimen sintered at 1350℃.
[0043] Figure 4 shows the microstructure of the fracture surface of the samples sintered at each temperature. At 1200°C, it was observed that necks began to form between the particles, and pores between the circular particles were distributed relatively uniformly. At 1250°C, the contact area between the particles increased, the grain boundary area became wider, and the open pores became more uniform in diameter. At 1275°C, the pores were almost all closed, and the grain boundaries and residual pores gradually disappeared due to the movement of particles caused by active viscous flow. At 1300°C, the grain boundaries were almost all disappeared due to viscous flow, and the diffusion of atoms inside the pores continued, resulting in the observation of a few circular residual pores. At 1325°C, neither grain boundaries nor pores were observed. At 1350℃, a clear difference was observed between the inside and outside of the specimen. The inside surface, which showed translucency, had no pores or grain boundaries, as was evident from the microstructure, but crystallization occurred in the outside, and circular crystals of the cristobalite phase were observed.
[0044] Figure 5 shows the XRD analysis results of the specimens according to the sintering temperature. From 1200°C to 1250°C, an amorphous state with no specific peaks is observed, but from 1275°C, fine cristobalite peaks are observed, and even in the specimens heat-treated at 1325°C, which has the best light transmittance, cristobalite crystalline phase was observed. The specimens heat-treated at 1350°C were analyzed separately for the surface and the interior. As a result, an amorphous peak was observed in the interior, and a strong peak of the cristobalite phase was observed on the surface (outside). The difference between the surface and the interior is considered to be the result of nuclei being generated and growing from the surface as heat is transferred from the surface to the inside during heat treatment.
[0045] The relational equation for the sintering model of viscous flow in the Frenkel model is as follows:
[0046]
number
[0047] ρ0 is the initial density, ρ g is the density of the glass, γ is the surface energy of the glass, and η(T) is the viscosity value depending on the temperature.
[0048] The density as a function of time (ρ(t)) depends on the viscosity value as a function of temperature and the surface energy of the glass, but since the change in surface energy during sintering is not significant, the density ultimately depends on the temperature, which determines the viscosity. This theoretical formula can also be confirmed from the shrinkage rate of the sintered body, and a comparison of shrinkage rates as a function of temperature is shown in Table 2.
[0049] [Table 2]
[0050] It was confirmed that the higher the sintering temperature (℃), the higher the shrinkage (%), and especially, a large shrinkage was observed between 1275℃ and 1300℃. This means that the grains grow and the pores disappear in a very short temperature range.
[0051] In addition to the sintering temperature, the holding time also affects the sintering. Figure 6 shows a sintered body produced by holding for 5 hours at 1325°C, which shows high translucency. As a result of the experiment, an opaque sintered body was obtained, unlike the one held for 1 hour. As a result of observing the microstructure, it was determined that the translucency was reduced due to crystallization, and it can be seen that the holding time is also an important variable in the crystallization of silica. Considering the characteristics of silica, which is easily crystallized depending on the holding time even at a temperature where translucency is expressed, and the temperature difference at which the translucency is reduced is only 25°C, it was determined that there is a problem in controlling the translucency by controlling the temperature. Therefore, in order to prevent crystallization that causes a decrease in translucency, sintering was performed by adjusting the holding time at 1215°C, a relatively low temperature at which crystallization does not occur. Table 3 shows the density value of the sintered body according to the holding time. As a result of the experiment, it was confirmed that the sintered density also increases as the holding time is extended.
[0052] [Table 3]
[0053] Figure 7 shows the results of comparing the translucency of sintered specimens according to holding time. As a result of the experiment, the specimens were opaque for up to 12 hours, but translucency began to appear from 18 hours, and the highest translucency was observed at a holding time of 24 hours. However, it was visually confirmed that the translucency decreased again when the specimens were held for more than 24 hours.
[0054] Table 4 shows the comparison results of the shrinkage rate according to the holding time. The results in Table 4 confirm that in the viscous flow sintering mechanism, the degree of sintering shrinkage is proportional to time.
[0055] [Table 4]
[0056] Figure 8 shows the results of observing the microstructure of sintered specimens with different holding times. As a result of the experiment, at a holding time of 12 hours, only necks between particles were formed and no densification occurred, resulting in grain boundaries and a large number of pores. At holding times of 18 and 24 hours, no pores or grain boundaries were observed, but at a holding time of 30 hours, bent parts began to appear.
[0057] The above results are considered to be an early phenomenon of the onset of crystallization, and in order to confirm this, XRD analysis was performed according to the holding time. Figure 9 shows the XRD analysis results. As a result of the analysis, it was confirmed that an amorphous phase was observed from 12 to 24 hours, but a peak of cristobalite crystals was observed at 30 hours.
[0058] FIG. 10 and Table 5 show the transmittance as measured by a UV-Vis spectrometer to determine the degree of translucency as judged visually.
[0059] [Table 5]
[0060] The measurements showed that the specimens sintered for 12 hours had a transmittance of 0% for all wavelength bands, while the specimens sintered for 24 hours had a transmittance of 19%-58% in the ultraviolet region (wavelengths of 200-380 nm) and 84%-85% in the infrared region (2000-2400 nm).
[0061] 4. Conclusion
[0062] In the present invention, a translucent silica sintered body was manufactured using amorphous spherical nano-silica powder with uniform particle size and no impurities. Translucency was induced by densification by controlling variables such as the manufacturing conditions of the molded body, sintering temperature, and holding time, and the powder molded body showed a sintering mechanism behavior due to viscous flow. As densification progressed, pores and grain boundaries disappeared and translucency was expressed, and crystallization of cristobalite, which is sensitively dependent on temperature and holding time, reduced translucency.
[0063] In order to produce a more stable amorphous sintered body, the holding time was adjusted at 1215℃, a relatively low temperature at which crystallization does not occur, and an amorphous silica sintered body with translucency was obtained. This sintered body exhibits a transmittance of 19% to 58% for light in the ultraviolet range (wavelengths of 200 to 380 nm) and 84% to 85% for light in the infrared range (2000 to 2400 nm). These results are considered to be applicable to the production of ultraviolet-transmitting lenses made from existing quartz glass.
[0064] The specific embodiments described in this specification are meant to represent preferred implementations or examples of the present invention, and are not intended to limit the scope of the present invention in any way. It will be apparent to those skilled in the art that modifications and other uses of the present invention do not depart from the scope of the invention as defined in the claims of this specification. [Industrial Applicability]
[0065] The present invention provides a method for producing a transparent silica sintered body, which can solve the problem that if unremoved pores, grain boundaries, and crystal phases exist inside the silica sintered body, light is scattered, causing a rapid decrease in the light transmittance of the sintered body. Therefore, it is possible to produce materials for process parts that are most widely used in the semiconductor, display, and solar cell industries, such as lenses, optical materials, photomask substrates, and lens materials for excimer stepper equipment.
Claims
1. A first step of providing a silica powder; A second step of compressing and molding the silica powder to produce a molded body; A third step of producing a transparent silica sintered body by heat-treating the molded body at a temperature of 1310 to 1340° C. for 50 to 240 minutes at a heating rate of 2° C. / min, or at a temperature of 1200 to 1230° C. for 20 to 28 hours at a heating rate of 2° C. / min; A method for producing a transparent silica sintered body using sintering, comprising:
2. The method for producing a transparent silica sintered body using sintering according to claim 1, wherein the silica powder has an amorphous spherical particle shape.
3. 2. The method for producing a transparent silica sintered body using sintering according to claim 1, wherein the green body is produced by performing a primary molding by uniaxial pressing on the silica powder and then performing a secondary molding by cold isostatic pressing.
4. The method for producing a transparent silica sintered body using sintering according to claim 1, characterized in that the transparent silica sintered body has a shrinkage of 45.5 to 47.5% after heat treatment of the molded body.
5. The transparent silica sintered body according to claim 1, characterized in that the transparent silica sintered body transmits 19% to 58% of light in the ultraviolet region (wavelength of 200 to 380 nm) and 84% to 85% of light in the infrared region (2000 to 2400 nm).
Citation Information
Patent Citations
Production of formed glass
JP1989275438A
Production of quartz glass
JP1997048623A
Method for manufacturing quartz glass product, silica granules used therefor and its production method
JP2008266087A
Silica-sintered article
JP2018002526A