Thermoplastic resin composition, its manufacturing method and molded article manufactured therefrom

A thermoplastic resin composition with specific copolymers and a lubricant addresses the limitations of ASA resins and PVC resin, providing enhanced calendering properties and safety, ensuring high-quality appearance and durability.

JP2024539824AActive Publication Date: 2024-10-31LG CHEM LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024516510
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-20
Filing Date
2023-07-17
Publication Date
2024-10-31
Estimated Expiration
2043-07-17

AI Technical Summary

Technical Problem

Existing ASA resins for calenders have insufficient stretching properties, leading to poor calender processability and durability, and PVC resin is harmful due to phthalate compounds and toxic gas emission during fires.

Method used

A thermoplastic resin composition comprising alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymers with varying particle sizes and an aromatic vinyl compound-vinyl cyanide compound copolymer, along with a lubricant, to enhance calendering properties and durability, while avoiding phthalates and toxic gas emission.

Benefits of technology

The composition achieves superior tensile strength, elongation, surface gloss, and surface hardness, ensuring appearance quality and durability, replacing PVC resin in applications like furniture finishing without harmful compounds or toxic gas release.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539824000001
    Figure 2024539824000001
  • Figure 2024539824000002
    Figure 2024539824000002
  • Figure 2024539824000003
    Figure 2024539824000003
Patent Text Reader

Abstract

The present invention relates to a thermoplastic resin composition, its manufacturing method, and a molded article manufactured therefrom. More specifically, the present invention relates to a thermoplastic resin composition, characterized in that the composition contains 100 parts by weight of a base resin containing (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm, (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant, and the total rubber content measured by FT-IR is 15 to 21% by weight relative to 100% by weight of the total thermoplastic resin composition, the manufacturing method thereof, and a molded article manufactured therefrom. According to the present invention, the material does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, and has equal or better processability than PVC resin, which is a conventional material for calendars, and is excellent in tensile strength, elongation, surface gloss and surface hardness, thereby ensuring the quality of appearance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0135350 dated October 20, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.

[0002] The present invention relates to a thermoplastic resin composition, a manufacturing method thereof, and a molded article manufactured from the same. More specifically, the present invention relates to a thermoplastic resin composition which does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, and has equal or better processability than PVC resin, a conventional material for calendars, and is excellent in tensile strength, elongation, surface gloss, and surface hardness, thereby ensuring appearance quality and durability, a manufacturing method thereof, and a molded article manufactured from the same. [Background technology]

[0003] A calendar is a rolling machine with an arrangement of multiple heated rollers. The process of forming films and sheets using a calendar, and coating the surface of cloth, paper, etc. with plastic, is called calendaring. Calendaring has the disadvantage of requiring a higher capital investment than the extrusion process, but it is often used, especially when manufacturing PVC films, because the quality is superior to that of the extrusion process.

[0004] Polyvinyl chloride resin (hereinafter referred to as "PVC resin") is a homopolymer of vinyl chloride or a hybrid polymer containing 50% or more by weight of vinyl chloride, and is one of the five major general-purpose thermoplastic resins manufactured by suspension polymerization and emulsion polymerization. Among them, PVC resin manufactured by suspension polymerization is widely used in the manufacture of films, sheets, electric wires, pipes, etc. by mixing plasticizers, stabilizers, fillers, pigments, titanium dioxide (TiO2) and auxiliary materials with special functions and processing them in various ways. Currently, PVC resin is widely used as a surface finishing material for furniture due to its low cost, excellent physical properties and high processability. However, due to the characteristics of the material, it is difficult to reprocess, and it is very harmful in the event of a fire because it generates chlorine and hydrogen chloride gases when burned. It is also harmful to the human body due to the phthalate compounds, which are plasticizers used to give flexibility, and it generates harmful substances during manufacturing and disposal. Therefore, the market is making efforts to move away from this and replace it with environmentally friendly materials.

[0005] In the T-die extrusion market, polyethylene terephthalate resin is attracting attention due to its excellent physical properties and high colorability, while in calendaring extrusion, polypropylene resin is used in some cases due to its high economic efficiency, but its applications are limited due to the difficulty in achieving a high-quality appearance due to its low colorability and gloss, etc., and there is an increasing demand for environmentally friendly materials that can be used for calendaring extrusion.

[0006] In order to solve these problems, active research is being conducted into materials that can replace PVC resin, and among them, acrylonitrile-styrene-acrylate resin (hereinafter referred to as "ASA resin") is used in a wide range of fields such as automobiles, building materials, and miscellaneous goods because it has excellent weather resistance, light resistance, colorability, chemical resistance, and impact resistance as well. In particular, ASA resin has been attracting attention as an environmentally friendly material because it has better processing stability than PVC resin and does not contain heavy metal components.

[0007] However, existing ASA resins for calendaring have problems in that they have insufficient stretching properties, resulting in poor calendaring processability and insufficient durability after molding, resulting in poor quality of the produced sheets.

[0008] Therefore, there is a need to develop an ASA resin for calendaring that is excellent in calendar processability and durability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Publication No. 10-2006-0118820 Summary of the Invention [Problem to be solved by the invention]

[0010] In order to solve the above-mentioned problems of the prior art, the present invention aims to provide a thermoplastic resin composition which does not contain phthalate compounds, which are endocrine disrupting substances harmful to the human body, does not emit toxic gases in the event of a fire, and has excellent tensile strength and elongation, and therefore has equal or better processability than PVC resin, which is a conventional material for calendaring, and excellent durability, as well as a manufacturing method thereof and a molded product manufactured therefrom.

[0011] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]

[0012] In order to achieve the above object, the present disclosure provides a thermoplastic resin composition comprising 100 parts by weight of a base resin including (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm, (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyanide compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant, wherein the total content of the rubber measured by FT-IR is 15 to 21% by weight based on 100% by weight of the total thermoplastic resin composition.

[0013] The present disclosure also provides a thermoplastic resin composition comprising 100 parts by weight of a base resin including (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm, (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant, the thermoplastic resin composition having a surface hardness of 95 or more as measured in accordance with ASTM D785.

[0014] The (A-1) graft copolymer may preferably contain, based on its total weight, 30 to 70% by weight of an alkyl acrylate rubber, 20 to 50% by weight of an aromatic vinyl compound, and 1 to 25% by weight of a vinyl cyan compound.

[0015] The (A-2) graft copolymer may preferably contain, based on its total weight, 30 to 70% by weight of an alkyl acrylate rubber, 20 to 50% by weight of an aromatic vinyl compound, and 1 to 25% by weight of a vinyl cyan compound.

[0016] The weight ratio (A-1:A-2) of the graft copolymer (A-1) to the graft copolymer (A-2) may be preferably 1:1.5 to 1:7.

[0017] The (B) copolymer may preferably have a weight average molecular weight of 50,000 to 180,000 g / mol.

[0018] The (B) copolymer may preferably contain, based on its total weight, 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.

[0019] The (C) lubricant may preferably be at least one selected from the group consisting of aliphatic amide-based lubricants, fatty acid ester-based lubricants, montan-based waxes, and olefin-based waxes.

[0020] The thermoplastic resin composition may include an antioxidant, a UV stabilizer, or a mixture thereof.

[0021] The thermoplastic resin composition preferably has a tensile strength of 450 kgf / cm as measured in accordance with ASTM D638. 2 It may be more than that.

[0022] The thermoplastic resin composition may preferably have an elongation of 28% or more as measured in accordance with ASTM D638.

[0023] The present disclosure also provides a method for producing a thermoplastic resin composition, comprising: 100 parts by weight of a base resin including (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm, (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant; and kneading and extruding the mixture under conditions of 200 to 300°C and 100 to 300 rpm to produce an extrudate, wherein the produced extrudate has a total rubber content of 15 to 21% by weight measured by FT-IR relative to the total 100% by weight.

[0024] The present disclosure also provides a method for producing a thermoplastic resin composition, comprising: 100 parts by weight of a base resin including (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm; (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm to 600 nm; and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant; and kneading and extruding the resulting mixture under conditions of 200 to 300°C and 100 to 300 rpm, wherein the produced thermoplastic resin composition has a surface hardness of 95 or more as measured in accordance with ASTM D785.

[0025] The present disclosure also provides a molded article comprising the thermoplastic resin composition.

[0026] The molded article may preferably be a calendered article. Effect of the Invention

[0027] According to the present invention, there is provided a thermoplastic resin composition which does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, and has equal or better processability than PVC resin, which is a conventional material for calendars, and is excellent in tensile strength, elongation, surface gloss and surface hardness, thereby ensuring appearance quality and durability, as well as a manufacturing method thereof and a molded article manufactured from the same.

[0028] In addition, since the thermoplastic resin composition according to the present invention has excellent calendering processability, it can be effectively used as a surface finishing material, particularly for furniture, by producing it into a film as a substitute for PVC resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The thermoplastic resin composition of the present invention, its production method and molded articles produced therefrom will be described in detail below.

[0030] The present inventors have confirmed that when a base resin containing two kinds of alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymers with different average particle sizes and an aromatic vinyl compound-vinyl cyanide compound copolymer in a predetermined content ratio is used, a lubricant is added in a predetermined content, and the rubber content in the thermoplastic resin composition is adjusted within a predetermined range, the thermoplastic resin composition does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, has equal or better processability than PVC resin, which is a conventional material for calendars, and is excellent in tensile strength, elongation, surface glossiness, and surface hardness, thereby ensuring appearance quality and durability, and is effective as a substitute for PVC materials. Based on this, they have further pursued research and completed the present invention.

[0031] The thermoplastic resin composition of the present invention is characterized by comprising 100 parts by weight of a base resin containing (A-1) 3-22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle diameter of 50-200 nm, (A-2) 20-40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle diameter of more than 200 nm to 600 nm, and (B) 50-72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6-1.9 parts by weight of a lubricant; and the total content of rubber measured by FT-IR is 15-21% by weight based on 100% by weight of the total thermoplastic resin composition. In this case, it does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, has excellent tensile strength and elongation, has equal or greater processability than PVC resin, which is a conventional material for calendars, and has excellent scratch resistance, ensuring durability, and has the advantage of replacing PVC materials.

[0032] Hereinafter, the thermoplastic resin composition of the present invention will be described in detail with respect to each component.

[0033] (A-1) Alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing alkyl acrylate rubber having an average particle size of 50 to 200 nm The alkyl acrylate rubber of the graft copolymer (A-1) may have, for example, an average particle size of 50 to 200 nm, preferably 80 to 180 nm, and more preferably 110 to 160 nm. Within this range, excellent mechanical properties and processability can be imparted.

[0034] In this description, the average particle size can be measured using dynamic light scattering, specifically, using a particle size analyzer (product name: Nicomp380, manufacturer: PSS) in Gaussian mode to measure the intensity value. In this case, as a specific measurement example, a sample is prepared by diluting 0.1g of latex (TSC 35-50wt%) 1,000-5,000 times with deionized water or distilled water, i.e., diluting appropriately so as not to deviate significantly from the intensity setpoint of 300kHz, and putting it into a glass tube. The measurement method is auto-dilution and measurement with a flow cell, the measurement mode is dynamic light scattering / intensity 300KHz / intensity-weight Gaussian analysis, and the setting values ​​are a temperature of 23°C, a measurement wavelength of 632.8nm, and a channel width of 10μsec.

[0035] The (A-1) graft copolymer may be, for example, 3 to 22% by weight, preferably 3 to 17% by weight, and more preferably 4 to 10% by weight, based on the total weight of the base resin. Within this range, the effect of excellent mechanical properties such as tensile strength and elongation, surface gloss, surface hardness, and fluidity is achieved.

[0036] The (A-1) graft copolymer may preferably comprise an alkyl acrylate rubber (core) and a shell surrounding the core, the shell containing an aromatic vinyl compound and a vinyl cyanide compound. In this case, the graft copolymer has excellent tensile strength, elongation, and surface gloss.

[0037] The (A-1) graft copolymer may contain, for example, 30 to 70% by weight, preferably 35 to 65% by weight, and more preferably 40 to 60% by weight of alkyl acrylate rubber relative to its total weight, and within this range, the copolymer has excellent tensile strength, elongation, and processability.

[0038] The (A-1) graft copolymer may contain, for example, 20 to 50% by weight, preferably 25 to 45% by weight, and more preferably 30 to 40% by weight of an aromatic vinyl compound relative to its total weight. Within this range, the copolymer has excellent surface gloss, surface hardness, and processability.

[0039] The (A-1) graft copolymer may contain, for example, 1 to 25% by weight, preferably 5 to 20% by weight, and more preferably 10 to 20% by weight of a vinyl cyan compound relative to the total weight of the copolymer. Within this range, the copolymer has the effect of providing excellent surface gloss, surface hardness, and processability.

[0040] The alkyl acrylate rubber described in the present invention may be, for example, one or more selected from the group consisting of alkyl acrylate rubbers having an alkyl group with 1 to 10 carbon atoms, preferably one or more selected from the group consisting of ethyl acrylate rubber, propyl acrylate rubber, butyl acrylate rubber, hexyl acrylate rubber, octyl acrylate rubber, and 2-ethylhexyl acrylate rubber, more preferably butyl acrylate rubber, 2-ethylhexyl acrylate rubber, or a mixture thereof, in which case there is an effect of excellent gloss and surface hardness.

[0041] In the present description, the aromatic vinyl compound may be, for example, one or more selected from the group consisting of styrene, α-methylstyrene, ο-methylstyrene, ρ-methylstyrene, m-methylstyrene, ethylstyrene, isobutylstyrene, t-butylstyrene, ο-bromostyrene, ρ-bromostyrene, m-bromostyrene, ο-chlorostyrene, ρ-chlorostyrene, m-chlorostyrene, vinyltoluene, vinylxylene, fluorostyrene, and vinylnaphthalene, and may be preferably styrene.

[0042] The vinyl cyanide compound described herein may be, for example, one or more selected from the group consisting of acrylonitrile, methacrylonitrile, phenylacrylonitrile, and α-chloroacrylonitrile, and is preferably acrylonitrile.

[0043] In this description, a polymer comprising a certain compound (monomer) means a polymer that is polymerized containing that compound (monomer), and the units in the polymerized polymer are derived from that compound.

[0044] The (A-1) graft copolymer may be prepared by, for example, emulsion polymerization, in which case, it has the effect of providing excellent surface gloss and surface hardness.

[0045] The emulsion polymerization is not particularly limited as long as it is an emulsion polymerization method commonly used in the technical field to which the present invention belongs, and may be, for example, an emulsion graft polymerization method.

[0046] (A-2) An alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm The alkyl acrylate rubber of the graft copolymer (A-2) may have, for example, an average particle size of more than 200 nm and not more than 600 nm, preferably 250 to 570 nm, more preferably 300 to 550 nm, and even more preferably 400 to 550 nm. Within this range, excellent gloss, tensile strength, and surface hardness can be imparted.

[0047] The (A-2) graft copolymer may be, for example, 20 to 40% by weight, preferably 23 to 35% by weight, and more preferably 23 to 30% by weight, based on the total weight of the base resin. Within this range, the effect of excellent fluidity and tensile strength is achieved.

[0048] The (A-2) graft copolymer may preferably comprise an alkyl acrylate rubber and a shell containing an aromatic vinyl compound and a vinyl cyanide compound surrounding the alkyl acrylate rubber. In this case, the effect of excellent mechanical properties, processability and surface gloss is obtained.

[0049] The (A-2) graft copolymer may contain, for example, 30 to 70% by weight, preferably 35 to 65% by weight, and more preferably 40 to 60% by weight of alkyl acrylate rubber relative to its total weight. Within this range, the copolymer has excellent mechanical properties such as tensile strength and elongation, surface gloss, surface hardness, and processability.

[0050] The (A-2) graft copolymer may contain, for example, 20 to 50% by weight, preferably 25 to 45% by weight, and more preferably 30 to 40% by weight of an aromatic vinyl compound relative to the total weight of the copolymer. Within this range, the copolymer has excellent tensile strength, elongation, and processability.

[0051] The (A-2) graft copolymer may contain, for example, 1 to 25% by weight, preferably 5 to 20% by weight, and more preferably 10 to 20% by weight of a vinyl cyan compound relative to the total weight of the copolymer. Within this range, the copolymer has the effect of providing excellent surface gloss, surface hardness, and processability.

[0052] The types of the alkyl acrylate rubber, aromatic vinyl compound, and vinyl cyan compound contained in the (A-2) graft copolymer may be within the same category as the types of the alkyl acrylate rubber, aromatic vinyl compound, and vinyl cyan compound contained in the (A-1) graft copolymer of the present invention.

[0053] The (A-2) graft copolymer may be produced, for example, by emulsion polymerization, and in this case, it has the effect of being excellent in tensile strength, elongation, gloss and surface hardness.

[0054] The emulsion polymerization is not particularly limited as long as it is an emulsion polymerization method commonly used in the technical field to which the present invention belongs, and may be, for example, an emulsion graft polymerization method.

[0055] The weight ratio (A-1:A-2) of the graft copolymer (A-1) to the graft copolymer (A-2) may be, for example, 1:1.5 to 1:7, preferably 1:2.5 to 1:6, more preferably 1:3 to 1:6, and even more preferably 1:4 to 1:5.5. Within this range, the tensile strength, elongation, gloss, surface hardness, and processability are all excellent.

[0056] The difference between the average particle size of the acrylate rubber of the graft copolymer (A-1) and the average particle size of the acrylate rubber of the graft copolymer (A-2) may be, for example, 100 to 550 nm, preferably 150 to 500 nm, more preferably 200 to 450 nm, and even more preferably 250 to 450 nm. Within this range, there is an effect of further improving the tensile strength, elongation, surface gloss, and surface hardness.

[0057] The sum of the (A-1) graft copolymer and the (A-2) graft copolymer may be, for example, 25 to 50% by weight, preferably 30 to 45% by weight, and more preferably 30 to 40% by weight, relative to 100% by weight of the total base resin. Within this range, the tensile strength, elongation, surface gloss, surface hardness, and fluidity are further improved, resulting in improved processability.

[0058] (B) Aromatic vinyl compound-vinyl cyanide copolymer The (B) copolymer may be, for example, 50 to 72% by weight, preferably 55 to 70% by weight, and more preferably 60 to 70% by weight, based on the total weight of the base resin. Within this range, there are advantages in that the tensile strength, elongation, surface hardness, and processability are excellent.

[0059] The (B) copolymer may have a weight average molecular weight of, for example, 50,000 to 180,000 g / mol, preferably 60,000 to 180,000 g / mol, more preferably 70,000 to 180,000 g / mol, and even more preferably 80,000 to 180,000 g / mol. Within this range, the copolymer has the effect of being excellent in mechanical properties such as tensile strength and elongation, surface gloss and surface hardness.

[0060] In this description, unless otherwise specified, the weight average molecular weight can be measured using GPC (Gel Permeation Chromatography, water breeze). As a specific example, the weight average molecular weight can be measured as a relative value to a standard PS (standard polystyrene) sample through GPC using THF (tetrahydrofuran) as an eluent. In this case, as a specific example of the measurement, the measurement can be performed under the following conditions: solvent: THF, column temperature: 40°C, flow rate: 0.3ml / min, sample concentration: 20mg / ml, injection amount: 5μl, column model: 1×PLgel 10μm MiniMix-B (250×4.6mm)+1×PLgel 10μm MiniMix-B (250×4.6mm)+1×PLgel 10μm MiniMix-B Guard (50×4.6mm), equipment name: Agilent 1200 series system, refractive index detector: Agilent G1362 RID, RI temperature: 35°C, data processing: Agilent ChemStation S / W, test method (Mn, Mw and PDI): OECD TG 118.

[0061] The (B) copolymer may, for example, contain 50 to 90% by weight, preferably 60 to 80% by weight, and more preferably 65 to 75% by weight of an aromatic vinyl compound relative to the total weight of the copolymer. Within this range, the copolymer has the effect of being excellent in mechanical properties such as tensile strength and elongation, surface gloss and surface hardness.

[0062] The (B) copolymer may contain, for example, 10 to 50% by weight, preferably 20 to 40% by weight, and more preferably 25 to 35% by weight of a vinyl cyan compound relative to the total weight of the copolymer. Within this range, the copolymer has the effect of being excellent in mechanical properties such as tensile strength and elongation, surface gloss and surface hardness.

[0063] The types of aromatic vinyl compounds and vinyl cyan compounds contained in the copolymer (B) may be within the same category as the types of aromatic vinyl compounds and vinyl cyan compounds contained in the graft copolymer (A-1) described herein.

[0064] The (B) copolymer is preferably a styrene-acrylonitrile copolymer (SAN resin), an α-methylstyrene-acrylonitrile copolymer (heat-resistant SAN resin), or a mixture thereof, and more preferably a styrene-acrylonitrile copolymer (SAN resin). In this case, the copolymer has the effect of providing excellent surface gloss, surface hardness, and processability.

[0065] The copolymer (B) may be produced by, for example, solution polymerization, bulk polymerization, emulsion polymerization or suspension polymerization, and preferably by bulk polymerization, which has the effect of providing excellent mechanical properties.

[0066] The solution polymerization, bulk polymerization, emulsion polymerization and suspension polymerization are not particularly limited as long as they are solution polymerization, bulk polymerization, emulsion polymerization and suspension polymerization methods commonly used in the technical field to which the present invention pertains.

[0067] (C)Lubricant The amount of the (C) lubricant may be, for example, 0.6 to 1.9 parts by weight, preferably 0.8 to 1.8 parts by weight, and more preferably 0.8 to 1.5 parts by weight, based on 100 parts by weight of the base resin. Within this range, the tensile strength, elongation, gloss, and surface hardness are all excellent, and the calendering processability is excellent, so that the sheet is not deformed or damaged during calendering and can be attached and detached on the rolls, and therefore, it has the effect of replacing PVC materials.

[0068] The lubricant (C) may be, for example, one or more selected from the group consisting of an aliphatic amide-based lubricant, a fatty acid ester-based lubricant, a montan-based wax, and an olefin-based wax, and is preferably a fatty acid ester-based lubricant, and more preferably pentaerythrityl tetrastearate. In this case, since the tensile strength, elongation, gloss, and surface hardness are all excellent, calendar processing can be performed in place of PVC resin, and there is an effect of excellent calendar processability.

[0069] The aliphatic amide lubricant may be at least one selected from the group consisting of stearamide, behanamide, ethylene bis(stearamide), N,N'-ethylene bis(12-hydroxystearamide), erucamide, oleamide, and ethylene bisoleamide. In this case, the aliphatic amide lubricant has excellent tensile strength, elongation, gloss, and surface hardness, and therefore can be calendered instead of PVC resin, resulting in excellent calendering processability.

[0070] The fatty acid ester-based lubricant may be, for example, at least one selected from the group consisting of fatty acid esters of alcohols or polyhydric alcohols, hardened oils, butyl stearate, stearic acid monoglyceride, pentaerythritol tetrastearate, stearyl stearate, ester wax, and alkyl phosphate esters, and is preferably pentaerythritol tetrastearate. In this case, since the tensile strength, elongation, gloss, and surface hardness are all excellent, calendar processing can be performed in place of PVC resin, and there is an effect of excellent calendar processability.

[0071] The montan wax may be, for example, a montan wax or a montan ester wax. In this case, since it has excellent tensile strength, elongation, gloss and surface hardness, it can be used for calendar processing instead of PVC resin, and has an effect of excellent calendar processability.

[0072] The olefin wax may be, for example, a polyolefin wax, preferably a polyethylene wax, a polypropylene wax, or a mixture thereof, more preferably a polyethylene wax, and even more preferably an oxidized high density polyethylene wax. In this case, since the olefin wax has excellent tensile strength, elongation, gloss, and surface hardness, it can be calendered instead of PVC resin, and has an effect of excellent calendering processability.

[0073] Additives The thermoplastic resin composition may include, for example, an antioxidant, a UV stabilizer, or a mixture thereof. In this case, the inherent physical properties of the thermoplastic resin composition described herein are not deteriorated, and the required physical properties are effectively achieved.

[0074] The antioxidant may be, for example, 0.1 to 2 parts by weight, preferably 0.2 to 1.5 parts by weight, and more preferably 0.3 to 1 part by weight, per 100 parts by weight of the base resin, and within this range, there is an effect of improving heat resistance.

[0075] The antioxidant may be, for example, one or more selected from the group consisting of a phenol-based antioxidant, a phosphite-based antioxidant, and a thioether-based antioxidant, and is preferably a phenol-based antioxidant or a phosphite-based antioxidant.

[0076] The phenol-based antioxidant may be, for example, one or more selected from the group consisting of tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, 1,3,5-tris-(4-t-butyl-3-hydroxy-2,6-dimethylbenzene)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, and 1,3,5-tris-(3,5-di-t-butyl-4-hydroxybenzyl)-s-triazine-2,4,6-(1H,3H,5H)-trione.

[0077] The phosphite-based antioxidant may be, for example, tris-nonylphenyl phosphite, tris-(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, or a mixture thereof.

[0078] The thioether-based antioxidant may be, for example, one or more selected from the group consisting of dilauryl thiodipropionate, dimyristyl thiodipropionate, lauryl stearyl thiodipropionate, distearyl thiodipropionate, dimethyl thiodipropionate, 2-mercaptobenzimidazole, phenothiazine, octadecyl thioglycolate, butyl thioglycolate, octyl thioglycolate, and thiocresol.

[0079] The UV stabilizer may be, for example, 0.1 to 3 parts by weight, preferably 0.3 to 1.5 parts by weight, and more preferably 0.5 to 1 part by weight, relative to 100 parts by weight of the base resin, in which case there is an effect of improving weather resistance.

[0080] The UV stabilizer may be, for example, a hindered amine light stabilizer (HALS), and is preferably 1,1-bis(2,2,6,6-tetramethyl-4-piperidyl)succinate, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-N-butyl-3,5-di-tert-butyl-4-hydroxybenzyl, or bis(1,2,2,6,6-pentamethyl-4-piperidyl)-N-butyl-3,5-di-tert-butyl-4-hydroxybenzyl. malonate, 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidine and succinic acid condensation products, linear or cyclic condensation products of N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)hexamethylenediamine and 4-tert-octylamino-2,6-dichloro-1,3,5-triazine, tris(2,2,6,6-tetramethyl-4-piperidyl)nitrilotriacetate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butene Tantalum tetracarboxylate, 1,1'-(1,2-ethanediyl)-bis(3,3,5,5-tetramethylpiperazinone), 4-benzoyl-2,2,6,6-tetramethylpiperidine, 4-stearyloxy-2,2,6,6-tetramethylpiperidine, linear or cyclic condensation products of N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)hexamethylenediamine with 4-morpholino-2,6-dichloro-1,3,5-triazine, 7,7,9,9-tetramethyl-2-cycloundecyl-1-oxa-3, and poly[[6-(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino], more preferably bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate (Bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol), poly[[6-(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino], or a mixture thereof. It may be a mixture of bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (Bis(2,2,6,6-tetramethyl-4-piperidyl)), poly[[6-(1,1,3,3-tetramethylbutyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imino], or a mixture thereof, and in such a case, there is an advantage that the impact strength and fluidity are not impaired and the weather resistance is greatly improved.

[0081] The thermoplastic resin composition may optionally contain one or more selected from the group consisting of dyes, pigments, colorants, antistatic agents, antibacterial agents, processing aids, metal deactivators, flame retardants, smoke suppressants, anti-dripping agents, anti-friction agents and anti-wear agents in an amount of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, more preferably 0.1 to 2 parts by weight, and even more preferably 0.5 to 1 part by weight, based on 100 parts by weight of the total base resin. Within this range, the inherent physical properties of the thermoplastic resin composition described herein are not deteriorated, and the required physical properties are effectively realized.

[0082] thermoplastic resin composition The thermoplastic resin composition may preferably have a total rubber content of 15 to 21% by weight, more preferably 15 to 20% by weight, even more preferably 15 to 19% by weight, and even more preferably 15 to 18% by weight, based on the total weight of the thermoplastic resin composition, as measured by FT-IR. Within this range, the composition has excellent tensile strength, elongation, gloss, and surface hardness, and is also excellent in calendar processability, making it advantageous in that it can replace PVC resin.

[0083] The thermoplastic resin composition preferably has a tensile strength of 450 kgf / cm, measured at the point where a test piece having a thickness of 3 mm is broken after being pulled at a crosshead speed of 50 mm / min in accordance with ASTM D638. 2 More preferably, 470kgf / cm 2 More preferably, 500 kgf / cm 2 More preferably, 500 to 650 kgf / cm 2 Within this range, the resin has an excellent balance of physical properties and excellent processability, particularly calender processability, and is therefore advantageous in that it can be used as an alternative to PVC resin.

[0084] The thermoplastic resin composition may preferably have an elongation of 28% or more, more preferably 28 to 60%, even more preferably 28 to 50%, and even more preferably 28 to 45%, as measured on a test piece having a thickness of 3 mm at a crosshead speed of 50 mm / min in accordance with ASTM D638. Within this range, the composition has an excellent balance of physical properties and excellent processability, particularly calender processability, and thus has the advantage of being able to replace PVC resin.

[0085] The thermoplastic resin composition may preferably have a surface hardness of 95 or more, more preferably 100 or more, and even more preferably 100 to 115, as measured in accordance with ASTM D785. Within this range, the composition has the advantages of excellent balance of physical properties and excellent durability.

[0086] The thermoplastic resin composition preferably has a surface gloss of 90 GU or more, more preferably 90 to 100 GU, as measured at 45° on an injection test piece having a thickness of ¼" in accordance with ASTM D528. Within this range, the composition has an excellent balance of physical properties and excellent transparency, resulting in a beautiful appearance.

[0087] The thermoplastic resin composition may preferably have a pencil hardness of B or more, preferably HB or more, measured in accordance with ASTM D219. Within this range, the thermoplastic resin composition has the advantages of having an excellent balance of physical properties and excellent durability.

[0088] The thermoplastic resin composition is preferably produced as a sheet having a thickness of 0.3 mm at a roll temperature of 180 to 220°C, a calendar roll speed of 8 to 12 rpm, and a gap between the calendar rolls of 0.3 mm. When the thermoplastic resin composition is plasticized on the surface of the roll and stabilized for application within 3 minutes, the formed sheet can be attached and detached on the roll without deformation or damage, and has excellent calendar processability.

[0089] The following describes the method for producing the thermoplastic resin composition of the present invention and the molded article containing the composition. In describing the method for producing the thermoplastic resin composition of the present invention and the molded article containing the composition, all of the above-mentioned thermoplastic resin composition is included.

[0090] Method for producing thermoplastic resin composition The method for producing a thermoplastic resin composition according to the present invention includes the steps of kneading and extruding 100 parts by weight of a base resin containing (A-1) 3-22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50-200 nm, (A-2) 20-40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50-72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer under conditions of 200-300°C and 100-300 rpm, and the produced extrudate is characterized in that the total rubber content measured by FT-IR is 15-21% by weight based on the total 100% by weight. In such cases, it does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, and has the same or better processability as PVC resin, a conventional calendar material, and is excellent in tensile strength, elongation, surface gloss and surface hardness, ensuring appearance quality and durability.It also has excellent calendar processability, making it an advantageous substitute for PVC resin.

[0091] The kneading and extrusion may be carried out, for example, through a single screw extruder, a twin screw extruder, or a Banbury mixer. In this case, the composition can be uniformly dispersed and has excellent compatibility.

[0092] The kneading and extrusion may be carried out, for example, at a barrel temperature in the range of 200 to 300°C, preferably 210 to 280°C, and more preferably 220 to 270°C. In this case, the processing amount per unit time is appropriate, sufficient melt kneading is possible, and problems such as thermal decomposition of the resin component are not caused.

[0093] The kneading and extrusion may be carried out under conditions where the screw rotation speed is, for example, 100 to 500 rpm, 150 to 400 rpm, 100 to 350 rpm, or 200 to 310 rpm, preferably 250 to 350 rpm. Within this range, the throughput per unit time is high, and the process efficiency is excellent.

[0094] The extrudate may preferably be in the form of pellets or plates.

[0095] In this description, the plate-like shape is not particularly limited as long as it is defined as a normal plate-like shape in the technical field to which the present invention belongs, and examples thereof include a flat shape, a sheet shape, a film shape, etc.

[0096] molded product The molded article described herein may, for example, contain the thermoplastic resin composition described herein. In this case, the molded article does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, and has the same or better processability as PVC resin, a conventional material for calendars, and is excellent in tensile strength, elongation, surface gloss and surface hardness, ensuring appearance quality and durability, and has the advantage of being applicable as a high-quality finishing material in place of PVC resin.

[0097] The molded product may be, for example, a calendered product, and may preferably be a building finishing material, a roof finishing material, or a furniture finishing material. In this case, it has the advantage that it has excellent appearance quality and durability, and can be provided with a quality higher than that required in the market.

[0098] The method for producing a molded article according to the present invention includes the steps of kneading and extruding 100 parts by weight of a base resin containing (A-1) 3-22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50-200 nm, (A-2) 20-40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 50-72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer, and (C) 0.6-1.9 parts by weight of a lubricant, under conditions of 200-300°C and 100-300 rpm to produce an extrudate, and calendering the extrudate at a molding temperature of 120-300°C to produce a molded article, wherein the extrudate has a total rubber content of 15-21% by weight measured by FT-IR relative to the total 100% by weight. In this case, since it does not contain phthalate compounds, which are environmental hormones harmful to the human body, and does not emit toxic gases in the event of a fire, and has excellent tensile strength and elongation, it has equal or better processability than PVC resin, which is a conventional material for calendars, and has excellent surface gloss and scratch resistance, ensuring durability and appearance quality, and has the advantage of being used as a high-quality finishing material that can replace PVC resin.

[0099] The calendering, for example, rolls the extrudate by a calendering process including a calender roll, and is not particularly limited if it is a method commonly used in the technical field to which the present invention belongs, but preferably includes a step of mixing the raw materials of the sheet in a mixer at 130 to 220° C., a step of producing the mixed raw materials as a base sheet at 170 to 240° C., and a step of producing the base sheet as a sheet using a calender roll at 140 to 220° C. Here, for example, a mixing roll can be used in the base sheet production step.

[0100] In describing the thermoplastic resin composition, its production method, and molded products, other conditions, equipment, etc. not explicitly described herein can be appropriately selected within the range commonly used in the art, and it is clearly stated that there are no particular limitations.

[0101] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical spirit of the present invention. Naturally, such changes and modifications also fall within the scope of the appended claims.

[0102] [Example] *(A-1) ASA graft copolymer: ASA graft copolymer produced by emulsion polymerization, with an average particle size of alkyl acrylate rubber of 150 nm (graft copolymer containing 50% by weight of butyl acrylate rubber, 35% by weight of styrene, and 15% by weight of acrylonitrile) *(A-2) ASA graft copolymer: ASA graft copolymer produced by emulsion polymerization, with an average particle size of alkyl acrylate rubber of 450 nm (graft copolymer containing 50% by weight of butyl acrylate rubber, 35% by weight of styrene, and 15% by weight of acrylonitrile) *(B) Bulk polymerization SAN copolymer: A copolymer containing 70% by weight of styrene and 30% by weight of acrylonitrile (weight average molecular weight 150,000 g / mol) *(C) Lubricant: Pentaerythritol tetrastearate *(D) Additives: - Antioxidant: Irganox 1076 (BASF) 0.5 parts by weight, Irgafox 168 (BASF) 0.5 parts by weight -UV stabilizer: Tinuvin 770 (BASF) 0.5 parts by weight, Sunsorb 329 (SUNFINE GLOBAL) 0.5 parts by weight

[0103] Examples 1 to 7 and Comparative Examples 1 to 9 The components and contents of the additives, each of which is listed in Tables 1 and 2 below, were mixed and extruded in an extruder (SM Twin screw extruder, 25Φ) at an extrusion temperature of 230°C, a feed rate of 20 kg / hr, and a screw speed of 300 rpm to produce pellets. The produced pellets were extruded in an injector (ENGEL 120MT) at an injection temperature of 200-240°C and a screw speed of 100-200 rpm to produce test pieces for measuring appearance and physical properties. In addition, in a roll mill (MR-LM0820, MIRAE RPM Co., Ltd.) in which two calendar rolls with a diameter of 30 cm were installed at an interval of 0.3 mm, the extruded pellet-shaped resin was calendered in a state in which the rolls were maintained at 180-210°C to produce a sheet with a thickness of 0.3 mm.

[0104] [Test example] The properties of the pellets and injection test pieces produced in Examples 1 to 7 and Comparative Examples 1 to 9 were measured by the following methods, and the results are shown in Tables 1 and 2 below. *Rubber content (wt%): Quantitatively measured using FT-IR. * Tensile strength (kgf / cm 2 ): According to ASTM D638, the point at which a 3 mm thick test piece was broken was measured after pulling at a crosshead speed of 50 mm / min. *Elongation (%): The elongation was measured on a 3 mm thick test piece at a crosshead speed of 50 mm / min in accordance with ASTM D638. *Surface hardness: Rockwell hardness was measured on a 1 / 4" thick test piece using the R scale in accordance with ASTM D785. *Surface gloss (GU): Measured using a gloss meter on an injection test piece with a thickness of 3.2 mm at an incidence angle of 45° in accordance with ASTM D523. The higher the gloss at 45°, the better the surface gloss. Here, the unit of surface gloss is GU (Gloss Unit). *Pencil hardness: Pencil hardness was measured in accordance with ASTM D219. *Processability: When extruding the thermoplastic resin composition pellets into a sheet having a thickness of 0.3 mm through a roll mill at a roll temperature of 180 to 220°C, a calendar roll speed of 8 to 12 rpm, and a gap between the calendar rolls of 0.3 mm, the plasticization, roll application, and roll stabilization times of the thermoplastic resin composition were measured and evaluated as follows: If the roll stabilization time was within 3 minutes, the processability was evaluated as excellent. ○: When the sheet is formed, the resin is stably applied to the surface of the roll and stabilized within 3 minutes, and the formed sheet can be attached and detached on the roll without deformation or damage. ×: When the sheet is formed, the resin is applied unstably on the surface of the roll, the stabilization time exceeds 3 minutes, and deformation or damage occurs when the formed sheet is attached to or detached from the roll.

[0105] [Table 1] [Table 2] (In Tables 1 and 2, the contents of (A-1), (A-2) and (B) are in weight percent based on the total weight of these, and the contents of (C) and (D) are in parts by weight based on 100 parts by weight of the total weight of (A-1), (A-2) and (B).)

[0106] As shown in Tables 1 and 2, the thermoplastic resin compositions according to the present invention (Examples 1 to 7) are superior in tensile strength, elongation, surface hardness, surface gloss, pencil hardness and processability compared to Comparative Examples 1 to 9, and therefore it has been confirmed that they can be applied to calendar molded products with high quality.

[0107] Specifically, Comparative Examples 1 and 2, in which the rubber content was outside the range of the present invention and the content of the graft copolymer (A-1) or the content of the graft copolymer (A-2) was outside the range of the present invention, had low elongation and pencil hardness and poor processability.

[0108] In addition, Comparative Example 3, in which the rubber content exceeded the range of the present invention, had low tensile strength and surface hardness, and Comparative Examples 4 and 5, in which the rubber content exceeded the range of the present invention and did not satisfy the range of the content of copolymer (B) and did not satisfy the range of the content of graft copolymer (A-1) or graft copolymer (A-2), had poor tensile strength, surface hardness and pencil hardness.

[0109] In addition, Comparative Examples 6 and 7, in which the content of lubricant (C) was outside the range of the present invention, had poor processability. In particular, Comparative Example 6 had a low elongation percentage, and Comparative Example 8, in which the content of rubber exceeded the range of the present invention, had poor tensile strength, surface hardness, and pencil hardness.

[0110] In addition, although the rubber content was within the range of the present invention, Comparative Example 9, in which the contents of the graft copolymer (A-1) and the graft copolymer (A-2) were outside the range of the present invention, had poor processability during sheet molding, and the sheet was damaged.

[0111] In conclusion, the thermoplastic resin composition according to the present invention, which contains a base resin containing two types of alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymers having different average particle sizes and an aromatic vinyl compound-vinyl cyanide compound copolymer in a predetermined content ratio, contains a lubricant in a predetermined content, and adjusts the rubber content in the thermoplastic resin composition within a predetermined range, does not contain phthalate compounds, which are environmental hormones harmful to the human body, does not emit toxic gases in the event of a fire, has equal or higher processability than PVC resin, which is a conventional material for calendars, and is excellent in tensile strength, elongation, surface glossiness and surface hardness, so that the appearance quality and durability are ensured.

Claims

1. 100 parts by weight of a base resin including: (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm; (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm; and (B) 50 to 72% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; (C) 0.6 to 1.9 parts by weight of a lubricant, A thermoplastic resin composition, characterized in that the total content of rubbers measured by FT-IR is 15 to 21% by weight based on 100% by weight of the total thermoplastic resin composition.

2. The thermoplastic resin composition according to claim 1, wherein the (A-1) graft copolymer contains, based on its total weight, 30 to 70% by weight of an alkyl acrylate rubber, 20 to 50% by weight of an aromatic vinyl compound, and 1 to 25% by weight of a vinyl cyan compound.

3. The thermoplastic resin composition according to claim 1, wherein the (A-2) graft copolymer contains, based on its total weight, 30 to 70% by weight of an alkyl acrylate rubber, 20 to 50% by weight of an aromatic vinyl compound, and 1 to 25% by weight of a vinyl cyan compound.

4. The thermoplastic resin composition according to claim 1, wherein the weight ratio (A-1:A-2) of the graft copolymer (A-1) to the graft copolymer (A-2) is 1:1.5 to 1:

7.

5. The thermoplastic resin composition according to claim 1, wherein the copolymer (B) has a weight average molecular weight of 50,000 to 180,000 g / mol.

6. The thermoplastic resin composition according to claim 1, wherein the copolymer (B) contains, based on its total weight, 50 to 90% by weight of an aromatic vinyl compound and 10 to 50% by weight of a vinyl cyan compound.

7. 2. The thermoplastic resin composition according to claim 1, wherein the lubricant (C) is at least one selected from the group consisting of an aliphatic amide-based lubricant, a fatty acid ester-based lubricant, a montan wax, and an olefin wax.

8. 10. The thermoplastic resin composition of claim 1, wherein the thermoplastic resin composition comprises an antioxidant, a UV stabilizer, or a mixture thereof.

9. The thermoplastic resin composition according to claim 1, wherein the thermoplastic resin composition has a surface hardness of 95 or more as measured in accordance with ASTM D785.

10. The thermoplastic resin composition has a tensile strength of 450 kgf / cm as measured in accordance with ASTM D638. 2 The thermoplastic resin composition according to claim 1, characterized in that

11. The thermoplastic resin composition according to claim 1, wherein the thermoplastic resin composition has an elongation of 28% or more as measured in accordance with ASTM D638.

12. (A-1) 3 to 22% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of 50 to 200 nm, (A-2) 20 to 40% by weight of an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer containing an alkyl acrylate rubber having an average particle size of more than 200 nm and not more than 600 nm, and (B) 100 parts by weight of an aromatic vinyl compound-vinyl cyan compound copolymer; and (C) 0.6 to 1.9 parts by weight of a lubricant; and a step of kneading and extruding the mixture under conditions of 200 to 300° C. and 100 to 300 rpm to produce an extrudate, A method for producing a thermoplastic resin composition, characterized in that the produced extrudate has a total rubber content of 15 to 21 wt. % based on 100 wt. % of the total extrudate as measured by FT-IR.

13. A molded article comprising the thermoplastic resin composition according to any one of claims 1 to 11.

14. The molded article according to claim 13, characterized in that the molded article is a calendered article.

Citation Information

Patent Citations

  • Thermoplastic resin composition, material for lighting fixture of vehicle and housing part for lighting fixture of vehicle

    JP2007091970A

  • Thermoplastic resin composition and method for producing the same

    JP2008504387A

  • Thermoplastic resin composition and method for producing the same

    JP2017031362A

  • Thermoplastic resin composition, its method of manufacture and molded article containing same

    JP2022516346A

  • Alkyl acrylate compound-vinyl cyanide compound-aromatic vinyl compound graft copolymer, its production method and thermoplastic resin composition containing the same

    JP2022522518A