Biodegradable resin composition containing high calcium carbonate content
A biodegradable resin composition with a high calcium carbonate content, balanced with diol and dicarboxylic acid components, addresses the inefficiencies of existing polymers by maintaining mechanical properties and reducing costs, while enhancing biodegradability and preventing soil acidification.
Patent Information
- Application Number
- JP2024525405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-02
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Existing biodegradable polymers face challenges with high energy consumption, increased manufacturing costs, and reduced mechanical properties when incorporating calcium carbonate, limiting their effectiveness and efficiency in producing films and sheets.
A biodegradable resin composition with a high content of calcium carbonate, combined with specific ratios of diol and dicarboxylic acid components, and optionally nanocellulose, to maintain tensile strength and elongation while enhancing biodegradability and reducing production costs.
The composition achieves improved biodegradability, maintains mechanical properties, and reduces production costs by utilizing a high calcium carbonate content, while also neutralizing acid components during decomposition to prevent soil acidification.
Smart Images

Figure 2024540105000001_ABST
Abstract
Description
[Technical field]
[0001] The examples relate to a biodegradable resin composition containing a high content of calcium carbonate, a biodegradable polyester film, a biodegradable polyester sheet, and a method for producing the same. [Background technology]
[0002] In recent years, as concerns about environmental issues have increased, solutions are being sought for the disposal of various daily necessities, particularly disposable products. Specifically, polymeric materials are inexpensive and have excellent characteristics such as processability, and therefore are widely used to manufacture various products such as films, fibers, packaging materials, bottles, containers, etc. However, when used products reach the end of their life and are incinerated, they have the disadvantage that harmful substances are emitted and, depending on the type, it may take hundreds of years for them to completely decompose naturally.
[0003] To overcome these limitations of polymers, research is being actively conducted into biodegradable polymers that decompose in a relatively short time.Polylactic acid (PLA), polybutyleneadipate terephthalate (PBAT), polybutylene succinate (PBS), etc. are being introduced as alternative biodegradable polymers.
[0004] However, although polylactic acid, an aliphatic polyester, has good mechanical properties, it lacks flexibility due to its inherent crystal structure, and polybutylene adipate terephthalate, an aromatic aliphatic polyester, has poor mechanical properties such as strength, so its uses are limited.
[0005] To solve these problems, Patent Document 1 discloses a biodegradable polyester foil that has improved tear propagation properties by mixing a low content of calcium carbonate into a composition including PBAT, PBSet, PBAzt, PBST, etc. However, when the content of calcium carbonate is increased, the physical properties of the biodegradable polyester foil weaken, and the manufacturing process of the polyester foil requires high energy consumption, which increases manufacturing costs and reduces manufacturing efficiency. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] US Patent No. 9096758 Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the present invention aims to provide a biodegradable resin composition, a biodegradable polyester film, a biodegradable polyester sheet, and a manufacturing method thereof, which contain a high content of calcium carbonate and maintain excellent tensile strength and elongation, as well as excellent biodegradability, an effect of preventing soil acidification, and reduction in production costs. [Means for solving the problem]
[0008] The biodegradable resin composition according to one embodiment includes a biodegradable polyester resin and calcium carbonate (CaCO3), and has a reduction rate of the crystal peak represented by the following formula 1 of 50% or more.
[0009] Another embodiment of the biodegradable polyester film includes a biodegradable resin composition containing a biodegradable polyester resin and calcium carbonate (CaCO3), and the biodegradable resin composition has a reduction rate of the crystalline peak represented by the following formula 1 of 50% or more.
[0010] Another embodiment of the biodegradable polyester sheet includes a biodegradable resin composition containing a biodegradable polyester resin and calcium carbonate (CaCO3), and the biodegradable resin composition has a reduction rate of the crystalline peak represented by the following formula 1 of 50% or more. [Formula 1] Crystal peak reduction rate = (R p -C p ) / R p In the above formula 1, R p is the crystalline heat of fusion (J / g) of the biodegradable polyester resin in the temperature range of 70°C to 90°C measured by using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min, C p is the heat of crystalline fusion (J / g) of the biodegradable resin composition measured under the same conditions as above. Effect of the Invention
[0011] The biodegradable resin composition according to one embodiment contains calcium carbonate at a specific content, and thus the cost of the product can be reduced by using a high content of low-cost calcium carbonate, thereby reducing production costs. Also, the biodegradation starting point can be increased and the chemical decomposition reaction can be accelerated, thereby improving biodegradability.
[0012] Furthermore, the acid components generated during decomposition of products using the biodegradable resin composition can be neutralized, thereby preventing soil acidification.
[0013] According to one embodiment, the biodegradable resin composition contains a high content of calcium carbonate to change the flow properties of the polymer, thereby adjusting the glass transition temperature (Tg) and crystallization peak of the biodegradable resin composition.
[0014] A biodegradable resin composition according to one embodiment can maintain a low isothermal weight loss rate despite having a high calcium carbonate content, and can maintain a high calcium carbonate content even during high temperature processing.
[0015] Molded articles, particularly biodegradable polyester films, produced from biodegradable resin compositions according to other embodiments can maintain tensile strength, elongation and tear strength at or above a certain level despite containing a low content of biodegradable polyester resin. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 shows the results of differential scanning calorimetry of the biodegradable resin compositions of the practical examples and the reference examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below with reference to examples. The examples are not limited to the contents disclosed below, and may be modified in various forms without departing from the spirit of the invention.
[0018] In this specification, when a part is said to "comprise" a certain component, unless specifically stated to the contrary, it does not mean that it excludes other components, but that it may further include other components.
[0019] In addition, all numerical ranges expressing physical properties, dimensions, and the like of components described in this specification should be understood to be modified in all cases by the term "about" unless otherwise specified.
[0020] In this specification, terms such as first, second, primary, secondary, etc. are used to describe various components, and the components are not limited by the terms. The terms are used only to distinguish one component from another.
[0021] [Biodegradable resin composition] The biodegradable resin composition according to one embodiment includes a biodegradable polyester resin and calcium carbonate (CaCO3), and has a reduction rate of the crystal peak represented by the following formula 1 of 50% or more. [Formula 1] Crystal peak reduction rate = (R p -C p ) / R p In the above formula 1, R p is the crystalline heat of fusion (J / g) of the biodegradable polyester resin in the temperature range of 70°C to 90°C measured by using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min, C p is the heat of crystalline fusion (J / g) of the biodegradable resin composition measured under the same conditions as above.
[0022] [Biodegradable polyester resin] The biodegradable polyester resin includes a first repeating unit and a second repeating unit, the first repeating unit includes a diol component and an aromatic dicarboxylic acid component, and the second repeating unit includes a diol component and an aliphatic dicarboxylic acid component.
[0023] -Diol component- The diol component includes 1,4-butanediol or a derivative thereof.
[0024] Specifically, the diol component may contain 95 mol % or more, 97 mol % or more, 98 mol % or more, 99 mol % or more, or 100 mol % of 1,4-butanediol or a derivative thereof based on the total number of moles of the diol component.
[0025] When the diol component contains 1,4-butanediol or a derivative thereof, biodegradability, flexibility, and strength can be improved. In particular, when the diol component consists of only 1,4-butanediol, the effects of improving biodegradability and strength can be maximized.
[0026] Optionally, the diol component may further comprise a second diol different from the first diol, which is 1,4-butanediol or a derivative thereof.
[0027] The second diol may be at least one selected from the group consisting of propanediol, hexanediol, cyclohexanedimethanol, and ethylene glycol. Specifically, the second diol may be at least one selected from the group consisting of 1,3-propanediol, 1,2-propanediol, 1,2-hexanediol, 1,3-hexanediol, 1,4-hexanediol, 1,6-hexanediol, 2,3-hexanediol, 2,4-hexanediol, 2,5-hexanediol, 2,6-hexanediol, 3,4-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and ethylene glycol.
[0028] Additionally, the diol component may further include 5 mol % or less, 3 mol % or less, 2 mol % or less, or 1 mol % or less of a second diol, based on the total number of moles of the diol component.
[0029] -Dicarboxylic acid component- The dicarboxylic acid component of the present invention includes an aliphatic dicarboxylic acid component and an aromatic dicarboxylic acid component.
[0030] The aromatic dicarboxylic acid component is at least one selected from the group consisting of terephthalic acid, dimethyl terephthalic acid and derivatives thereof.
[0031] The aliphatic dicarboxylic acid component is at least one selected from the group consisting of adipic acid, succinic acid, and derivatives thereof.
[0032] Specifically, the aromatic dicarboxylic acid component may be terephthalic acid or dimethylterephthalic acid, and the aliphatic dicarboxylic acid component may be adipic acid or succinic acid.
[0033] The dicarboxylic acid component may contain the aromatic dicarboxylic acid component in an amount of 15 mol% or more, 30 mol% or more, 45 mol% or more, 50 mol% or more, or 75 mol% or more, or in an amount of 30 mol% to 90 mol%, 35 mol% to 80 mol%, 40 mol% to 75 mol%, 45 mol% to 65 mol%, or 45 mol% to 55 mol%, based on the total number of moles of the dicarboxylic acid components.
[0034] Furthermore, the dicarboxylic acid component may contain the aliphatic dicarboxylic acid component at 15 mol% or more, 30 mol% or more, 45 mol% or more, 50 mol% or more, or 75 mol%, or may contain 30 mol% to 90 mol%, 35 mol% to 80 mol%, 40 mol% to 75 mol%, 45 mol% to 65 mol%, or 45 mol% to 55 mol%, based on the total number of moles of the dicarboxylic acid components.
[0035] The molar ratio of the aromatic dicarboxylic acid component to the aliphatic dicarboxylic acid component may be 0.5 to 1.5: 1, 0.7 to 1.3: 1, or 0.8 to 1.2: 1. When the molar ratio of the aromatic dicarboxylic acid component to the aliphatic dicarboxylic acid component satisfies the above range, biodegradability and processability can be improved.
[0036] The molar ratio of the diol component to the dicarboxylic acid component may be 0.5 to 2: 1. For example, the molar ratio of the diol component to the dicarboxylic acid component may be 0.5 to 1.8: 1, 0.7 to 1.5: 1, or 0.9 to 1.2: 1. When the molar ratio of the diol component to the dicarboxylic acid component satisfies the above range, biodegradability, strength, and processability can all be improved without discoloration such as yellowing.
[0037] -Nanocellulose- The biodegradable polyester resin of the present invention may further comprise nanocellulose.
[0038] The nanocellulose is a natural substance in the form of a gel or dry powder, and can improve the dispersion stability, strength, and processability of biodegradable polyester resins containing the nanocellulose.
[0039] The biodegradable polyester resin may contain nanocellulose in an amount of 0.01% to 3% by weight based on the total weight of the biodegradable polyester resin. For example, the content of the nanocellulose may be 0.01% to 2.5% by weight, 0.05% to 2% by weight, 0.07% to 1.8% by weight, 0.1% to 1.2% by weight, 0.1% to 1% by weight, or 0.15 to 0.7% by weight based on the total weight of the biodegradable polyester resin. By satisfying the above ranges for the content of nanocellulose, biodegradability and strength can be further improved.
[0040] The nanocellulose may be in the form of a dry powder or gel having secondary particles aggregated with a particle size of 1 μm to 50 μm. For example, the nanocellulose may be in the form of a dry powder or gel having secondary particles aggregated rather than a single particle, and the size of the secondary particles may be 2 μm to 45 μm or 5 μm to 50 μm. The nanocellulose may also be in the form of a powder that has been freeze-dried to reduce the volume for easier storage and transportation.
[0041] The nanocellulose may have a diameter of 1 nm to 100 nm. For example, the nanocellulose may have a diameter of 1 nm to 95 nm, 5 nm to 90 nm, 10 nm to 80 nm, 5 nm to 60 nm, or 15 nm to 60 nm.
[0042] The length of the nanocellulose may be 5 nm to 10 μm. For example, the length of the nanocellulose may be 5 nm to 5 μm, 5 nm to 1 μm, 10 nm to 700 nm, 20 nm to 500 nm, 60 nm to 300 nm, 80 nm to 200 nm, or 100 nm to 250 nm.
[0043] When the diameter and length of the nanocellulose satisfy the above ranges, the strength, particularly the tear strength, can be further improved.
[0044] In addition, the nanocellulose can function as a crystal nucleating agent to improve the crystallization rate of the biodegradable resin composition and increase the crystallization temperature of the biodegradable resin composition.
[0045] The nanocellulose is one or more selected from the group consisting of cellulose nanocrystals, cellulose nanofibers, and microfibrillated cellulose, and cellulose nanocrystals or cellulose nanofibers are preferred from the viewpoint of strength and thermal properties. When the nanocellulose is contained in the biodegradable polyester resin, the biodegradability, strength, and thermal properties can be further improved.
[0046] The biodegradable resin composition containing the nanocellulose may have suitable UV resistance, biodegradation rate and hydrolysis rate.
[0047] More specifically, the nanocellulose may be one or more selected from the group consisting of hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, cellulose acetate, methylcellulose, ethylcellulose, propylcellulose, butylcellulose, pentylcellulose, hexylcellulose, and cyclohexylcellulose.
[0048] The average particle size of nanocellulose according to the embodiment may be 200 nm or less, and the particle size deviation may be 20% or less. Specifically, the average particle size of the water-dispersed nanocellulose may be 190 nm or less or 185 nm or less, and the particle size deviation may be 18% or less or 16% or less. When the average particle size and particle size deviation of nanocellulose satisfy the above ranges, both the dispersibility and durability of the nanocellulose are excellent.
[0049] According to another embodiment, the nanocellulose may be bead mill pre-treated or ultrasonic pre-treated. Specifically, the nanocellulose may be water-dispersed nanocellulose that has been bead mill pre-treated or ultrasonic pre-treated.
[0050] For example, the nanocellulose may be prepared by dispersing cellulose nanocrystals in a dry powder or gel form having a particle size of 1 μm to 50 μm in water, followed by bead mill pretreatment or ultrasonic pretreatment.
[0051] If the nanocellulose, specifically water-dispersed nanocellulose, is bead mill pretreated or ultrasonically pretreated, the number of nanocellulose particles may be higher, maximizing dispersibility.
[0052] The nanocellulose may be pretreated with 0.01% to 10% by weight of a silane coupling agent based on the total weight of the nanocellulose. For example, the nanocellulose may be pretreated with 0.05% to 8% by weight, 0.1% to 8% by weight, 0.5% to 6% by weight, or 0.7% to 6% by weight of a silane coupling agent based on the total weight of the nanocellulose.
[0053] By satisfying the above range of the content of the silane coupling agent, the interfacial adhesion, dispersibility and compatibility can be maximized, and the mechanical properties and durability, particularly the hydrolysis resistance, of the biodegradable polyester resin containing the same can be further improved.
[0054] -Calcium carbonate (CaCO3)- The biodegradable resin composition according to one embodiment contains 30% by weight to 80% by weight of calcium carbonate based on the total weight of the biodegradable resin composition.
[0055] For example, the biodegradable resin composition may contain the calcium carbonate (CaCO3) in an amount of 30.5% by weight or more, 35% by weight or more, 45% by weight or more, 50% by weight or more, 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, or 75% by weight or more, based on the total weight of the biodegradable resin composition, or may contain 30% to 70% by weight, 40% to 75% by weight, 45% to 70% by weight, 30% to 45% by weight, 45% to 55% by weight, 45% to 49% by weight, 55% to 65% by weight, 60% to 75% by weight, 65% to 72% by weight, 60% to 70% by weight, or 65% to 70% by weight.
[0056] When the biodegradable resin composition contains calcium carbonate in the above range, the raw material is readily available and low-cost calcium carbonate can be used at a high content, thereby reducing the cost of the product and reducing production costs; the biodegradability can be improved by raising the biodegradation starting point; and despite the high content of calcium carbonate, the dispersibility can be improved and deterioration of the physical properties of the product can be prevented.
[0057] In addition, when a molded article made of the biodegradable resin composition is decomposed, an acid component is generated. The acid component reacts with calcium carbonate to generate carbon dioxide gas and water, which improves the biodegradation rate at the molecular level. As shown in the following reaction formula 1, calcium carbonate neutralizes the acid component, reducing the environmental load and preventing soil acidification. [Reaction Scheme 1] CaCO3(s)+2H + (aq) → CO2(g) + H2O(l) + Ca 2+ (aq)
[0058] The calcium carbonate may be natural calcium carbonate obtained by mechanically crushing or classifying natural calcium carbonate containing CaCO3 as a main component, such as limestone, chalk, marble, shells, and coral, or may be synthetic calcium carbonate prepared by a chemical precipitation reaction or the like. Natural calcium carbonate is preferred because it increases the surface area between the biodegradable particles and calcium carbonate, thereby enhancing the efficiency of biodegradation.
[0059] In order to increase the dispersibility or reactivity of calcium carbonate, the surface of calcium carbonate may be modified by a physical or chemical treatment. For example, the physical surface modification method may be a physical method such as plasma treatment or corona treatment, or a chemical treatment of the surface with a coupling agent such as a silane coupling agent or a titanium coupling agent, or a surfactant.
[0060] The particle size of the calcium carbonate is calculated from the measurement result of the specific surface area by an air permeability method using a specific surface area measuring device, and the average particle size may be 0.1 μm to 10.0 μm, specifically 0.5 μm to 5.0 μm or 1.0 μm to 3.0 μm.
[0061] When the particle size of calcium carbonate is within the above range, the viscosity when kneading the biodegradable polyester resin and calcium carbonate can be maintained within a certain range, and the uniformity of the particle size can be increased, making it easier to produce molded products.
[0062] The specific surface area of the calcium carbonate was measured by a nitrogen gas adsorption method, and the specific surface area was 0.1 m 2 / g~10.0m 2 / g, specifically 0.2m 2 / g~5.0m 2 / g or 1.0m 2 / g~3.0m 2 / g.
[0063] When the specific surface area of calcium carbonate is within the above range, the biodegradable reaction surface area of the biodegradable polyester resin in a molded article produced from the biodegradable resin composition is increased, and biodegradability in a natural environment is favorably promoted, while the decrease in processability of the biodegradable resin composition caused by blending calcium carbonate can be reduced.
[0064] The amorphousness of the calcium carbonate is expressed based on the sphericity of the calcium carbonate, and the sphericity of the calcium carbonate may be 0.30 to 0.95, 0.50 to 0.93, or 0.60 to 0.90.
[0065] When the sphericity of calcium carbonate is within the above range, the interface between the biodegradable polyester resin and the calcium carbonate contains a large number of fine voids that are generated due to very weak adhesion or no adhesion, thereby enhancing biodegradability in a natural environment and preventing a decrease in the strength and moldability of the product.
[0066] -Additives- If necessary, additives may be added as auxiliary agents to the biodegradable resin composition of the present invention.
[0067] The additives may include, for example, fillers, lubricants, plasticizers, colorants, antioxidants, flame retardants or foaming agents, chain extenders, etc., in addition to calcium carbonate, and may include any additives that can be generally added to polyester biodegradable resin compositions, such as coupling agents, flow improvers, dispersants, UV absorbers, stabilizers, and antistatic agents. These additives may be used alone or in combination of two or more. Preferably, the biodegradable resin composition may further include one or more selected from the group consisting of lubricants, plasticizers, antioxidants, chain extenders, and dispersants.
[0068] For example, the biodegradable resin composition contains a plasticizer and an antioxidant. The additives may be added in the kneading step, or may be added to the biodegradable resin composition before the kneading step.
[0069] In the biodegradable resin composition of the present invention, the amount of these other additives added is not particularly limited as long as it is within a range in which the effects of the present invention can be achieved. However, it is preferable that each of the other additives is 0.01% by weight to 5% by weight, based on the total weight of the biodegradable resin composition, and that the total weight of the other additives is 10% by weight or less, based on the total weight of the biodegradable resin composition.
[0070] Examples of fillers other than calcium carbonate include magnesium carbonate, zinc oxide, titanium oxide, silica, alumina, clay, talc, kaolin, aluminum hydroxide, magnesium hydroxide, aluminum silicate, magnesium silicate, calcium silicate, aluminum sulfate, magnesium sulfate, calcium sulfate, magnesium phosphate, barium sulfate, quartz sand, carbon black, zeolite, molybdenum, diatomaceous earth, sericite, white sand, calcium sulfite, sodium sulfate, potassium titanate, bentonite, and graphite.
[0071] Examples of the lubricant include fatty acid-based lubricants including stearic acid, fatty alcohol-based lubricants, fatty amide-based lubricants including stearamide, aliphatic ester-based lubricants such as n-butyl stearate, methyl hydroxystearate, polyhydric alcohol fatty acid esters, saturated fatty acid esters, and ester waxes, and fatty acid metal soap-based lubricants.
[0072] The lubricant may be a stearic acid-based lubricant, and may include one or more selected from the group consisting of calcium stearate, zinc stearate, barium stearate, magnesium stearate, glycerin stearate, and butyl stearate.
[0073] The stearic acid-based lubricant reduces heat generation due to friction during mixing, melting and processing of raw materials, has excellent dispersing effect for biodegradable polyester resins for its cost, and has excellent lubricating effect, so that production efficiency can be improved.
[0074] The content of the lubricant may be 5 wt % or less, 1 wt % or less, less than 1 wt %, 0.9 wt % or less, 0.8 wt % or less, 0.7 wt % or less, 0.5 wt % or less, 0.3 wt % or less, or 0.1 wt % or less, based on the total weight of the biodegradable resin composition.
[0075] The lubricant may be included in an amount of 0.1% by weight to 1% by weight, specifically 0.1% by weight to 0.5% by weight or 0.2% by weight to 0.3% by weight, based on the total weight of the biodegradable resin composition.
[0076] When the content of the lubricant is within the above range, the physical properties of the biodegradable resin composition are not deteriorated, and the production efficiency of the biodegradable resin composition can be improved.
[0077] Plasticizers are added to impart processability and flexibility to the resulting molded article and can be glycerol, acrylates, glycerin, glycerol monostearate (GMS), sorbitol, or mixtures thereof.
[0078] In the biodegradable resin composition of the present invention, the content of these plasticizers is not particularly limited as long as it is within a range in which the effects of the present invention can be achieved, but the content of the plasticizer is 0 to 15 wt % based on the total weight of the biodegradable resin composition, and specifically, it can be 0 to 13 wt %, 0.1 wt % to 3 wt %, 4 wt % to 11 wt %, 8 wt % to 11 wt %, 4 wt % to 8 wt %, 2 wt % to 4 wt %, 1 wt % to 3 wt %, or 1 wt % to 2 wt %.
[0079] When the content of the plasticizer is within the above range, the elongation percentage of a molded article formed from the biodegradable resin composition can be improved, and the tearability can be improved.
[0080] The coloring agent may be any of organic pigments or inorganic pigments or dyes. Specific examples of the coloring agent include organic pigments such as azo-based, anthraquinone-based, phthalocyanine-based, quinacridone-based, isoindolinone-based, deoxazine-based, perinone-based, quinophthalone-based, and perylene-based pigments, and inorganic pigments such as ultramarine, titanium oxide, titanium yellow, iron oxide, chromium oxide, zinc oxide, and carbon black.
[0081] The antioxidant is selected from the group consisting of phosphorus-based antioxidants, phenol-based antioxidants, and pentaerythritol-based antioxidants, and each antioxidant may be used alone or in combination of two or more. When two or more antioxidants are used, it is preferable to use a combination of a phosphorus-based antioxidant and a phenol-based antioxidant to obtain effects in various temperature ranges.
[0082] The phosphorus-based antioxidant is a triester, diester or monoester of phosphorous acid such as triphenyl phosphite, trisnonylphenyl phosphite or tris(2,4-di-t-butylphenyl) phosphite, trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, tricresyl phosphate, tris(nonylphenyl) phosphate or 2-ethylphenyldiphenyl phosphate.
[0083] The phenolic antioxidants include α-tocopherol, butyl hydroxytoluene, sinaphyl alcohol, vitamin E, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenylacrylate, 2,6-di-t-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-t-butyl-4-hydroxybenzylphosphonate diethyl ester, 2,2-bis({[3-(3,5-di-t pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], or tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxymethyl]methane.
[0084] In addition, the antioxidant may be one or more selected from the group consisting of BHT, ascorbic acid, catechin, quercetin, dodecyl gallate, TBHQ, Ralox, registered trademark, Irganox, registered trademark 1135, Irganox 1076, nordihydroguaiaretic acid, epicatechin gallate, epigallocatechin gallate, epigallocateine, propyl gallate, 2,3,5-trihydroxybutyrophenone, butylated hydroxyanisole, 4-hydroxymethyl-2,6-di-tert-butylphenol, α-tocopherol, resveratrol, rutin, astastin, lycopene, beta-carotene, or melatonin.
[0085] The antioxidant is, based on the total weight of the biodegradable resin composition, 5 wt % or less, 3 wt % or less, 2 wt % or less, 1.5 wt % or less, 1 wt % or less, 0.5 wt % or less, or 0.3 wt % or less, and may be 0 to 5 wt %, 0.01 wt % to 4 wt %, 0.1 wt % to 3 wt %, 1 wt % to 3 wt %, 1 wt % to 2 wt %, 0.01 wt % to 0.3 wt %, or 0.05 wt % to 0.3 wt %.
[0086] When the antioxidant includes both a phosphorus-based antioxidant and a phenol-based antioxidant, the weight ratio of the phosphorus-based antioxidant to the phenol-based antioxidant can be 1:10 to 10:1, 1:5 to 5:1, 1:1 to 5:1, 2:1 to 4:1, 2.5:1 to 3.5:1, 1:5 to 1:1, 1:2 to 1:4, or 1:2.5 to 1:3.5.
[0087] By mixing the phosphorus-based antioxidant and the phenol-based antioxidant in the above range, desired effects can be obtained in various temperature ranges.
[0088] The flame retardant may utilize a halogen-based flame retardant, a phosphorus-based flame retardant, or a non-phosphorus-based halogen-based flame retardant such as a metal hydrate.
[0089] Examples of halogen-based flame retardants include halogenated bisphenol-based compounds such as halogenated bisphenylalkanes, halogenated bisphenyl ethers, halogenated bisphenyl thioethers, and halogenated bisphenyl sulfones, and bisphenol-bis(alkyl ether)-based compounds such as brominated bisphenol A, brominated bisphenol S, chlorinated bisphenol A, and chlorinated bisphenol S.
[0090] The phosphorus-based flame retardants include aluminum tris(diethylphosphinate), bisphenol A bis(diphenyl phosphate), triaryl isopropyl phosphate, cresyl di-2,6-xylenyl phosphate, and aromatic condensed phosphate esters.
[0091] The metal hydrate may be, for example, aluminum trihydrate, magnesium dihydroxide, or a combination thereof.
[0092] As a flame retardant assistant to improve the flame retardant effect, it is also possible to use antimony oxides such as antimony trioxide and antimony pentoxide, zinc oxide, iron oxide, aluminum oxide, molybdenum oxide, titanium oxide, calcium oxide, magnesium oxide, etc. in combination as a flame retardant assistant.
[0093] The foaming agent is mixed with or injected under pressure into the molten biodegradable resin composition, and changes phase from solid to gas or liquid to gas, or is a gas itself, and is used to control the foaming ratio (foam density) of the foam sheet.
[0094] Examples of the blowing agent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclobutane, cyclopentane, and cyclohexane; halogenated hydrocarbons such as chlorodifluoromethane, difluoromethane, trifluoromethane, trichlorofluoromethane, dichloromethane, dichlorofluoromethane, dichlorodifluoromethane, chloromethane, chloroethane, dichlorotrifluoroethane, dichloropentafluoroethane, tetrafluoroethane, difluoroethane, pentafluoroethane, trifluoroethane, dichlorotetrafluoroethane, trichlorotrifluoroethane, tetrachlorodifluoroethane, and perfluorocyclobutane; inorganic gases such as carbon dioxide, nitrogen, and air; and water.
[0095] The dispersant is intended to enhance the dispersibility of the solvent and solute, and may be one or more selected from the group consisting of aliphatic polyester, poly(lactic acid) (hereinafter, PLA), poly(glycolic acid) (hereinafter, PGA), polycaprolactone (hereinafter, PCL), and polyhydroxyalkanoate (hereinafter, PHA), but is not limited thereto.
[0096] The biodegradable resin composition of the present invention further contains one or more dispersants selected from the group consisting of polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate.
[0097] The content of the dispersant is not particularly limited as long as it is within a range in which the effects of the present invention can be achieved, but the dispersant may be contained in an amount of 1 wt% to 20 wt% based on the total weight of the biodegradable resin composition, and specifically, the dispersant may be contained in an amount of 1 wt% to 15 wt%, 1 wt% to 13 wt%, 1 wt% to 11 wt%, 2 wt% to 10 wt%, 5 wt% to 15 wt%, 7 wt% to 12 wt%, 2 wt% to 8 wt%, 5 wt% to 8 wt%, or 2 wt% to 5 wt%.
[0098] The chain extender is an aromatic diisocyanate, an aliphatic diisocyanate, an isocyanurate, a bisoxazoline, a carboxylic acid anhydride, or an epoxide.
[0099] The aromatic diisocyanate includes tolylene 2,4-diisocyanate, tolylene 2,6-diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, naphthylene 1,5-diisocyanate, or xylylene diisocyanate, among which 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 4,4'-diphenylmethane diisocyanate are particularly preferred.
[0100] The aliphatic diisocyanate refers to 1,6-hexamethylene diisocyanate, isophorone diisocyanate, or methylene bis(4-isocyanatocyclohexane). Particularly preferred aliphatic diisocyanates are isophorone diisocyanate, and particularly preferred are 1,6-hexamethylene diisocyanate.
[0101] The isocyanurate includes isophorone diisocyanate or methylene bis(4-isocyanatocyclohexane).
[0102] The bisoxazoline is 2,2'-bis(2-oxazoline), bis(2-oxazolinyl)methane, 1,2-bis(2-oxazolinyl)ethane, 1,3-bis(2-oxazolinyl)propane, or 1,4-bis(2-oxazolinyl)butane, in particular 1,4-bis(2-oxazolinyl)benzene, 1,2-bis(2-oxazolinyl)benzene, or 1,3-bis(2-oxazolinyl)benzene.
[0103] The epoxide refers to an epoxy-containing copolymer based on styrene, acrylic esters and / or methacrylic esters, preferably with a copolymer content of glycidyl (meth)acrylate of more than 20 wt%, more than 30 wt%, or more than 50 wt%, with an epoxy equivalent weight (EEW) of 150 g / Eq to 3000 g / Eq or 200 g / Eq to 500 g / Eq. The weight average molecular weight (Mw) is in the range of 2000 to 25000 or 3000 to 8000, the number average molecular weight (Mn) is 400 to 6000 or 1000 to 4000, and the polydispersity (Q) is generally 1.5 to 5. The epoxide is available from BASF Resins BV under the name Joncryl® ADR.
[0104] The chain extender is present in an amount of 1.5% by weight or less, 1% by weight or less, 0.5% by weight or less, or 0.3% by weight or less, based on the total weight of the biodegradable resin composition, and may be present in an amount of 0 to 1.5% by weight, 0.01% to 1% by weight, 0.1% to 1% by weight, 0.01% to 0.5% by weight, 0.01% to 0.3% by weight, or 0.1% to 0.5% by weight.
[0105] The COOH end group of the biodegradable polyester resin is 10 to 50 eq / 10 6 gr, 15-40eq / 10 6 gr, or 20-30eq / 10 6 It can be gr.
[0106] Differential scanning calorimeter (DSC) uses a differential scanning calorimeter to measure the heat flow associated with the thermal transitions of a sample, and can obtain qualitative information from the position, shape, and number of peaks, as well as quantitative information on the change in heat quantity from the area of the peaks (glass transition temperature (Tg), cold crystallization temperature (Tcc), crystallization temperature (Tmc), melting temperature (Tm), etc.).
[0107] When the biodegradable polyester resin is subjected to DSC temperature rise measurement by differential scanning calorimetry, the glass transition temperature is measured at about -20°C, and a crystal melting temperature curve is shown in which a crystallization peak due to butanediol (crystal fusion heat of 1-5 J / g or 1-3 J / g) appears in the temperature range of 70°C to 90°C, and a crystallization peak due to the biodegradable polyester resin (PBAT) itself (crystal fusion heat of 5-20 J / g or 13-17 J / g) is detected in the temperature range of 100°C to 150°C.
[0108] In the case of the biodegradable resin composition of the present invention, in the DSC temperature rise measurement by differential scanning calorimetry, the reduction rate of the crystallization peak according to formula 1 in the temperature range of 70°C to 90°C is 50% or more, 70% or more, 80% or more, 85% or more, 90% or more, 95% or more, 97% or more, 99% or more, or 100%. This means that in the DSC temperature rise measurement of the biodegradable resin composition, the crystallization peak due to butanediol is significantly reduced. This indicates that in the case of a biodegradable resin composition containing an excess amount of calcium carbonate, the inorganic calcium carbonate prevents the self-crystallization due to butanediol, resulting in a change in crystallization behavior.
[0109] In a DSC temperature rise measurement of the biodegradable resin composition of the present invention, the reduction rate of the crystal peak according to Formula 1A in the temperature range of 100°C to 150°C is 15% or more, 24% or more, 30% or more, 45% or more, 50% or more, 60% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more, for example, 45% to 98%, 45% to 96%, or 50% to 90%.
[0110] [Formula 1A] Crystal peak reduction rate = (R p1 -C p1 ) / R p1 In the above formula 1A, R p1 is the crystalline heat of fusion (J / g) of the biodegradable polyester resin in the temperature range of 100°C to 150°C measured using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min, Cp1 is the heat of crystalline fusion (J / g) of the biodegradable resin composition measured under the same conditions as above.
[0111] This means that in the DSC temperature rise measurement of the biodegradable resin composition, the crystallization peak due to the biodegradable polyester resin (PBAT) itself is significantly reduced. In the case of a biodegradable resin composition containing an excessive amount of calcium carbonate, the flow of polymer within a certain unit volume is suppressed by calcium carbonate, which is an inorganic substance, and this prevents the biodegradable polyester resin from self-crystallizing, thereby changing the crystallization behavior.
[0112] When the biodegradable resin composition is analyzed by differential scanning calorimetry, the glass transition temperature (Tg) may be -50° C. or more, -40° C. or more, -30° C. or more, -20° C. or more, -10° C. or more, or 30° C. or less, 20° C. or less, or 10° C. or less. This is because, in the case of a biodegradable resin composition containing an excessive amount of calcium carbonate, calcium carbonate, which is an inorganic substance, generates steric hindrance between polymer chains, suppressing the fluidity of the polymer chains, and the glass transition temperature (Tg) tends to be high.
[0113] The melting temperature (Tm) of the biodegradable resin composition may be 60°C or more, 80°C or more, 90°C or more, 100°C or more, or 110°C or more, and 150°C or less, 140°C or less, 130°C or less, or 120°C or less.
[0114] The crystallization temperature (Tmc) of the biodegradable resin composition may be -10°C or higher, -5°C or higher, or 0°C or higher, and may be 80°C or lower, 60°C or lower, 50°C or lower, or 40°C or lower.
[0115] 1 shows the results of differential scanning calorimetry when heating measurements were performed twice at a rate of 20°C per minute, and for the 100% biodegradable polyester resin (PBAT resin) of Reference Example A1, the glass transition temperature (Tg) was measured to be -24.2°C, the melting temperature (Tm) was measured to be 113.9°C, and the crystallization temperature (Tmc) was measured to be 33°C, and the cold crystallization temperature (Tcc) was not measured separately. In addition, the crystalline fusion heat due to the butanediol peak is 1 J / g, and the crystalline fusion heat due to the peak of the biodegradable polyester resin (PBAT) itself is 15 J / g.
[0116] In FIG. 1, the biodegradable resin composition of Example A2 containing 65% calcium carbonate and 35% PBAT resin had a measured glass transition temperature (Tg) of −23.1° C., a crystalline heat of fusion due to the butanediol peak of 0.02 J / g, and a crystalline heat of fusion due to the peak of the biodegradable polyester resin (PBAT) itself of 2.5 J / g.
[0117] Thermogravimetric analysis (TGA) is an analytical technique in which the weight of a sample is continuously measured as a function of time or temperature while the temperature is increased under constant conditions.
[0118] According to TGA analysis, when the biodegradable resin composition is maintained at an isothermal temperature of 210° C. for 1 hour, the isothermal weight loss of the biodegradable resin composition may be 5% or less.
[0119] Specifically, the isothermal weight loss is 4% or less, 3% or less, 2.5% or less, 2% or less, 1.5% or less, 1% or less, or 0.5% or less, and may be 0% or more, or 0.1% or more.
[0120] The isothermal weight loss was calculated as (W0-W1) / W0 × 100, where W0 is the initial pellet weight and W1 is the change in pellet weight after the pellet was left at 210 °C isothermal condition for 1 h.
[0121] When the isothermal weight loss is within the above range, the heat resistance of the biodegradable resin composition is ensured, vapor generation and molecular weight reduction due to heat during extrusion can be prevented, and mechanical properties can be maintained at a certain level or higher.
[0122] According to TGA analysis, when the biodegradable resin composition is heated at a rate of 20°C / 1 min, the calcium carbonate content variability of the biodegradable resin composition at 600°C may be 5% or less.
[0123] Specifically, the calcium carbonate content variability is 4% or less, 3% or less, 2.5% or less, 2% or less, 1.5% or less, 1% or less, or 0.8% or less, and may be 0% or more or 0.1% or more.
[0124] The variability of calcium carbonate content is (W c0 -W c1 ) / W c0 × 100, and the initial weight of calcium carbonate in the pellets of the biodegradable resin composition (W c0 ) and the weight (W) of calcium carbonate of the biodegradable resin composition at 600°C when the pellets of the biodegradable resin composition are heated at a rate of 20°C / 1 min. c1 ).
[0125] When the calcium carbonate content variability in the TGA analysis is within the above range, the biodegradable resin composition can maintain a high calcium carbonate (CaCO3) content even after a high-temperature processing process.
[0126] [Molded products] According to an embodiment, a molded article made from the biodegradable resin composition can be provided.
[0127] Specifically, the molded article is manufactured by molding the biodegradable resin composition by a method known in the art, such as extrusion or injection, and the molded article may be, but is not limited to, an injection molded article, an extrusion molded article, a thin film molded article, or a blow molded article.
[0128] For example, the molded product may be in the form of a film or sheet that can be used as agricultural mulching film, disposable gloves, food packaging materials, garbage bags, etc., or in the form of a fiber that can be used as a woven fabric, knitted fabric, nonwoven fabric, rope, etc., or in the form of a container that can be used as a food packaging container such as a lunch box.
[0129] In particular, since the molded article can be formed from the biodegradable resin composition, which can improve not only strength and processability but also durability, it can exhibit excellent properties when applied to packaging materials for products stored and transported at low temperatures, or garbage bags, mulching films, or disposable products that require excellent durability and elongation.
[0130] The biodegradable resin composition or a molded article produced therefrom is 60% to 100% biodegradable within 45 to 180 days under natural conditions, and can be composted under constant temperature conditions of 20°C to 60°C and constant humidity conditions of 30% to 90%.
[0131] -Biodegradable polyester film- A biodegradable polyester film, which is one example of the molded article, contains the biodegradable resin composition.
[0132] The biodegradable polyester film includes a biodegradable resin composition containing a biodegradable polyester resin and calcium carbonate (CaCO3), and the biodegradable resin composition has a reduction rate of a crystal peak represented by formula 1 of 50% or more.
[0133] The thickness of the biodegradable polyester film may be 5 μm to 200 μm. For example, the thickness of the biodegradable polyester film may be 5 μm to 180 μm, 5 μm to 160 μm, 10 μm to 150 μm, 15 μm to 130 μm, 20 μm to 100 μm, 25 μm to 80 μm, 10 μm to 50 μm, 10 μm to 30 μm, or 25 μm to 60 μm.
[0134] The tensile strength of the biodegradable polyester film may be 5 MPa or more. For example, the tensile strength of the biodegradable polyester film may be 7 MPa or more, 9 MPa or more, 10 MPa or more, or 11 MPa or more, and may be 30 MPa or less, 27 MPa or less, 25 MPa or less, 23 MPa or less, or 21 MPa or less.
[0135] When the tensile strength of the biodegradable polyester film is within the above range, it can be stretched within a certain range while containing a high content of calcium carbonate, has excellent mechanical properties, and can be used in a variety of applications. After biodegradation has begun, the biodegradation rate can be further improved.
[0136] The tear strength of the biodegradable polyester film may be 75 N / mm or more. For example, the tear strength of the biodegradable polyester film may be 75 N / mm or more, 80 N / mm or more, 85 N / mm or more, or 90 N / mm or more, and 200 N / mm or less, 180 N / mm or less, 150 N / mm or less, or 135 N / mm or less.
[0137] When the tear strength of the biodegradable polyester film is within the above range, the film has excellent mechanical properties such that it is difficult to tear in a certain direction despite having a high calcium carbonate content, making it possible to use the film in a variety of applications, and the biodegradation rate can be further improved after biodegradation has begun.
[0138] The elongation of the biodegradable polyester film may be 85% or more. For example, the elongation of the biodegradable polyester film may be 90% or more or 95% or more, and 700% or less, 650% or less, 600% or less, or 550% or less.
[0139] When the elongation percentage of the biodegradable polyester film is within the above range, certain parts of the film can be stretched well, ensuring stretchability during product packaging, and the film can withstand a certain load.
[0140] The seal strength of the biodegradable polyester film may be 500 gf or more. For example, the seal strength of the biodegradable polyester film may be 600 gf or more, 700 gf or more, or 800 gf or more.
[0141] -Biodegradable polyester sheet- A biodegradable polyester sheet, which is one example of the molded article, contains the biodegradable resin composition.
[0142] The biodegradable polyester sheet includes a biodegradable resin composition containing a biodegradable polyester resin and calcium carbonate (CaCO3), and the biodegradable resin composition has a reduction rate of the crystal peak represented by formula 1 of 50% or more.
[0143] The thickness of the biodegradable polyester sheet can be 5 μm to 180 μm, 5 μm to 160 μm, 10 μm to 150 μm, 15 μm to 130 μm, 20 μm to 100 μm, 25 μm to 80 μm, 10 μm to 50 μm, or 10 μm to 30 μm.
[0144] The tensile strength of the biodegradable polyester sheet may be 5 MPa or more. For example, the tensile strength of the biodegradable polyester sheet may be 6 MPa or more, 9 MPa or more, 10 MPa or more, 11 MPa or more, or 12 MPa or more, and may be 40 MPa or less, 35 MPa or less, 30 MPa or less, 27 MPa or less, 25 MPa or less, 23 MPa or less, or 21 MPa or less.
[0145] When the tensile strength of the biodegradable polyester sheet is within the above range, it can be stretched within a certain range while containing a high content of calcium carbonate, has excellent mechanical properties, and can be used in a variety of applications, and can further improve the biodegradation rate after biodegradation has begun.
[0146] The modulus of the biodegradable polyester sheet may be 110 MPa to 350 MPa. For example, the modulus of the biodegradable polyester sheet may be 120 MPa to 340 MPa, 150 MPa to 330 MPa, or 200 MPa to 330 MPa.
[0147] The elongation of the biodegradable polyester sheet may be 10% or more. For example, the elongation of the biodegradable polyester sheet may be 15% or more, 20% or more, 50% or more, or 70% or more, and may be 700% or less, 650% or less, 550% or less, 500% or less, or 450% or less.
[0148] When the elongation percentage of the biodegradable polyester sheet is within the above range, certain parts of the sheet can be stretched well, ensuring stretchability during product packaging, and the sheet can withstand a certain load.
[0149] [Method for producing biodegradable polyester film or biodegradable polyester sheet] A method for producing a biodegradable polyester film or a biodegradable polyester sheet according to an embodiment includes the steps of: preparing a prepolymer by esterifying a diol component and a dicarboxylic acid component; preparing a biodegradable polyester resin (polymer) by polycondensation of the prepolymer; mixing the biodegradable polyester resin with calcium carbonate to prepare a biodegradable resin composition; producing pellets from the biodegradable resin composition; and drying and melt-extrusion of the pellets.
[0150] First, a diol component and a dicarboxylic acid component are subjected to an esterification reaction to prepare a prepolymer.
[0151] The biodegradable resin composition is a composition containing a diol component including 1,4-butanediol or a derivative thereof, and one or more dicarboxylic acid components selected from the group consisting of terephthalic acid, dimethylterephthalic acid, adipic acid, succinic acid, and derivatives thereof, and is subjected to an esterification reaction to prepare a prepolymer.
[0152] The diol component, the aromatic dicarboxylic acid component and the aliphatic dicarboxylic acid component are as described above.
[0153] The step of preparing the prepolymer may involve a one-step esterification reaction of a composition including the diol component, the aromatic dicarboxylic acid component, the aliphatic dicarboxylic acid component, and optionally the nanocellulose, or may involve a two-step esterification reaction consisting of a first esterification reaction and a second esterification reaction.
[0154] The two-step esterification reaction may include: (1) a step of performing a first esterification reaction between the diol component and the aromatic dicarboxylic acid component; and (2) a step of performing a second esterification reaction by adding the diol component and the aliphatic dicarboxylic acid component to the reaction product of the step (1).
[0155] When the biodegradable polyester resin of the present invention contains the nanocellulose, the binding strength of the nanocellulose can be improved by adding the nanocellulose in the second esterification reaction step when preparing the prepolymer by the two-step esterification reaction. Specifically, adding the nanocellulose, i.e., water-dispersed nanocellulose, in the second esterification reaction step can further improve durability.
[0156] In addition, the nanocellulose is preferably added at a temperature of 100° C. to 160° C., preferably 110° C. to 140° C., in order to improve hydrolysis resistance.
[0157] Furthermore, the nanocellulose can be added at a rate of 2 kg / min to 10 kg / min, 2.5 kg / min to 9.5 kg / min, or 3 kg / min to 8 kg / min to further improve hydrolysis resistance while preventing aggregation and maintain an appropriate process speed. When the addition rate is within the above range, additional processes are not required, process efficiency can be improved, and re-aggregation of nanocellulose can be prevented.
[0158] More specifically, the two-step esterification reaction may include (1) a step of performing a first esterification reaction between the diol component and the first dicarboxylic acid component, and (2) a step of performing a second esterification reaction by adding the diol component, the second dicarboxylic acid component, and the nanocellulose to the reaction product of the step (1).
[0159] Prior to the esterification reaction, the titanium-based catalyst, the germanium-based catalyst, the antimony-based catalyst, the additives, and the stabilizers may be added to the composition. The catalysts, the additives, and the stabilizers are as described above.
[0160] The esterification reaction may be carried out at 250° C. or less for 0.5 to 5 hours. Specifically, the esterification reaction may be carried out at 240° C. or less, 235° C. or less, 180° C. to 250° C., 185° C. to 240° C., or 200° C. to 240° C., at normal pressure until the by-products of water and methanol reach 90% theoretically. For example, the esterification reaction may be carried out for 0.5 to 4.5 hours, 0.5 to 3.5 hours, or 1 to 3 hours, but is not limited thereto.
[0161] The number average molecular weight of the prepolymer may be 500 to 10000. For example, the number average molecular weight of the prepolymer may be 500 to 8500, 500 to 7000, 1000 to 6000, or 2500 to 5500. When the number average molecular weight of the prepolymer satisfies the above range, the molecular weight of the polymer can be efficiently increased in the polycondensation reaction, and strength properties can be further improved.
[0162] The number average molecular weight may be measured using gel permeation chromatography (GPC). Specifically, data obtained by gel permeation chromatography includes various items such as Mn, Mw, and Mp, among which the molecular weight may be measured based on the number average molecular weight (Mn).
[0163] Thereafter, the prepolymer is subjected to a polycondensation reaction to prepare a biodegradable polyester resin (polymer).
[0164] The polycondensation reaction may be carried out at 180° C. to 280° C. and 1.0 Torr or less for 1 hour to 6 hours. For example, the polycondensation reaction may be carried out at 190° C. to 270° C., 210° C. to 260° C., or 230° C. to 255° C., at 0.9 Torr or less, 0.7 Torr or less, 0.2 Torr to 1.0 Torr, 0.3 Torr to 0.9 Torr, or 0.5 Torr to 0.9 Torr, for 1.5 hours to 5.5 hours, 2 hours to 5 hours, or 3.5 hours to 4.5 hours.
[0165] The intrinsic viscosity of the biodegradable polyester resin may be from 0.05 dL / gr to 10 dL / gr.
[0166] The melt viscosity of the biodegradable polyester resin is 100s -1 When measured by RDS (rheometrics dynamic spectrometer) under the above conditions, the viscosity may be 1,000 to 30,000 poise.
[0167] The number average molecular weight (Mn) of the biodegradable polyester resin may be 40000 or more. For example, the number average molecular weight of the biodegradable polyester resin may be 43000 or more, 45000 or more, or 40000 to 70000.
[0168] The weight average molecular weight (Mw) of the biodegradable polyester resin may be 60000 or more. For example, the weight average molecular weight of the biodegradable polyester resin may be 65000 or more, 75000 or more, 80000 or more, or 85000 to 100000.
[0169] The polydispersity index (PDI) of the biodegradable polyester resin may be 1.2 to 2.0. For example, the polydispersity index of the biodegradable polyester resin may be 1.5 to 1.9 or 1.6 to 1.8.
[0170] When the number average molecular weight, weight average molecular weight or polydispersity index of the biodegradable polyester resin falls within the above range, strength and processability can be further improved.
[0171] The acid value of the biodegradable polyester resin may be 1.8 mgKOH / g or less. For example, the acid value of the biodegradable polyester resin may be 1.5 mgKOH / g or less, 1.3 mgKOH / g or less, or 1.25 mgKOH / g or less. When the acid value of the biodegradable polyester resin satisfies the above range, improvement in hydrolysis resistance can be maximized.
[0172] Thereafter, the biodegradable polyester resin and calcium carbonate are mixed to prepare a biodegradable resin composition.
[0173] The mixing of the biodegradable polyester resin and calcium carbonate can be appropriately set according to the molding method (extrusion molding, injection molding, vacuum molding, etc.), for example, the biodegradable polyester resin and calcium carbonate can be kneaded and melted before being charged into a molding machine from a hopper, or the biodegradable polyester resin and calcium carbonate can be kneaded and melted simultaneously with molding integrally with the molding machine. The melt kneading is preferably performed by uniformly dispersing calcium carbonate in the biodegradable polyester resin and applying high shear stress to the resin, for example, by kneading with a kneader reactor, an extrusion molding machine equipped with a single screw, or a twin-screw kneader.
[0174] In addition, in the mixing step, one or more of the plasticizer or the additives may be further added. The mixing stage may consist of one or more mixing stages.
[0175] As an example, in the case of a one-stage mixing step, the biodegradable resin composition may be prepared in a single mixing step containing 61% by weight to 80% by weight or 65% by weight to 72% by weight of calcium carbonate based on the total weight of the biodegradable resin composition.
[0176] As another example, in the case of a two-stage mixing step, it may be composed of a preliminary mixing step for preparing a biodegradable resin composition containing 61 wt% to 80 wt% or 65 wt% to 72 wt% of calcium carbonate based on the total weight of the biodegradable resin composition, and a secondary mixing step for preparing a biodegradable resin composition containing 30 wt% to 60 wt%, 40 wt% to 60 wt%, or 45 wt% to 55 wt% of calcium carbonate based on the total weight of the biodegradable resin composition.
[0177] The one or more mixing stages may be a tandem continuous process.
[0178] The temperature of the mixing step may be 150° C. to 190° C., 150° C. to 180° C., or 160° C. to 180° C. When the temperature of the mixing step is within the above range, the torque required during mixing can be reduced, and thermal decomposition of the mixed biodegradable resin composition can be prevented.
[0179] Thereafter, pellets are produced from the biodegradable resin composition. The biodegradable resin composition is fed into an extruder equipped with a single screw or an extruder equipped with a twin screw, extruded at a temperature of 150°C to 180°C, cut with a hot-cut pellet cutter, and cooled to 50°C or less, 40°C or less, 30°C or less, 25°C or less, 5°C to 50°C, 10°C to 30°C, 15°C to 25°C, or 20°C to 25°C to produce pellets.
[0180] The cutting step can be performed using any pellet cutter available in the art, and the pellets can have a variety of shapes.
[0181] Finally, the pellets are dried and melt extruded. The pellets are dried and melt extruded to produce a biodegradable polyester film or sheet.
[0182] The drying may be performed for 2 to 12 hours at 60° C. to 100° C. Specifically, the drying may be performed for 3 to 12 hours or 4 to 10 hours at 65° C. to 95° C., 70° C. to 90° C., or 75° C. to 85° C. When the pellet drying process conditions satisfy the above ranges, the quality of the produced biodegradable polyester film can be further improved.
[0183] The melt extrusion may be performed at 270° C. or less. For example, the melt extrusion may be performed at 265° C. or less, 260° C. or less, 255° C. or less, 130° C. to 270° C., 130° C. to 250° C., 140° C. to 230° C., 150° C. to 200° C., or 150° C. to 180° C. The melt extrusion may be performed by a blown film process or a pressing process, but is not limited thereto.
[0184] The torque during the melt extrusion may be 100 Nm to 300 Nm or 150 Nm to 250 Nm.
[0185] The above contents will be explained in more detail with reference to the following examples. However, the following examples are only for illustrating the present invention, and the scope of the examples is not limited to these examples.
[0186] (Experimental Example) (Experimental Example 1: Isothermal Weight Loss) For pellets produced from the biodegradable resin compositions of the Examples and Reference Examples, the initial pellet weight (W0) and the weight change (W1) of the pellet after leaving the film under isothermal conditions at 210°C for 1 hour were measured, and the isothermal weight loss was calculated using the formula (W0-W1) / W0×100%.
[0187] (Experimental Example 2: Variability of calcium carbonate content) For the biodegradable resin composition samples of the Examples and Reference Examples, a Q500 model TGA device from TA Instruments was used to heat the samples to 600°C at a heating rate of 20°C per minute (Dynamic mode), after which the remaining amount of Ca was confirmed and converted into calcium carbonate (CaCO3), thereby calculating the content of calcium carbonate in the pellets.
[0188] (Experimental Example 3: Glass transition temperature (Tg)) The biodegradable resin composition samples of the Examples and Reference Examples are subjected to heating measurements twice at a rate of 20° C. per minute using a DSC device, and Tg is calculated from the results of differential scanning calorimetry of the samples.
[0189] (Experimental Example 4: Crystallization temperature (Tc) and heat of fusion of crystals (△Hmc)) Using a differential scanning calorimeter (DSC), the biodegradable resin composition samples of the Examples and Reference Examples were heated from 40°C to 180°C at a rate of 10°C / min, then isothermally incubated for 5 minutes to carry out a first thermal history removal process, and then cooled from 180°C to -50°C at a rate of 10°C / min, and was then isothermally incubated for 5 minutes to carry out a second cooling process.
[0190] During the secondary cooling process, a graph of heat flow versus temperature was prepared to confirm the crystallization temperature (°C), crystallization peak, and heat of fusion of crystal (J / g).
[0191] (Experimental Example 5: Tensile strength) The biodegradable polyester films or sheets of the Examples, Comparative Examples, and Reference Examples were cut to a length of 100 mm and a width of 15 mm, and then tested in accordance with ASTM D 882 using an INSTRON universal testing machine (4206-001, UTM) with a chuck spacing of 50 mm and at a tensile speed of 500 mm / min. The tensile strength was then measured using a program built into the machine.
[0192] (Experimental Example 6: Elongation) The biodegradable polyester films or sheets of the Examples, Comparative Examples, and Reference Examples were cut to a length of 100 mm and a width of 15 mm, and the maximum deformation just before breakage was measured at a speed of 500 mm / min using an INSTRON universal testing machine (4206-001, UTM), and the ratio of the maximum deformation to the initial length was calculated.
[0193] (Experimental Example 7: Tear strength) The biodegradable polyester films of the Examples and Reference Examples were cut according to KPS M 1001-0806, and a constant speed of 500 mm / min was applied to measure the maximum load applied until the film was cut, and the tear strength was calculated according to the following formula 2. [Formula 2] Tear strength (N / cm) = Maximum load until breaking (N) / thickness of test piece (cm)
[0194] (Experimental Example 8: Modulus) The biodegradable polyester sheets of the Examples and Comparative Examples were cut to a length of 100 mm and a width of 15 mm, and then the modulus was measured using an Instron universal testing machine (4206-001, UTM) based on ASTM D 882.
[0195] (Example) [Production of biodegradable polyester resin] (Production Example 1) 50 mol % of 1,4-butanediol and 50 mol % of dimethyl terephthalic acid were mixed, and 200 ppm of a titanium-based catalyst, tetrabutyl titanate (manufactured by Aldrich), was added to the mixture, and a primary esterification reaction was carried out at 210° C. and normal pressure for 2 hours.
[0196] To the reaction product, 50 mol% of 1,4-butanediol, 50 mol% of adipic acid, 0.1 wt% of pretreated nanocellulose, and 150 ppm of titanium-based catalyst tetrabutyl titanate (manufactured by Aldrich) were added, and a secondary esterification reaction was carried out at 210°C and normal pressure for 2 hours to prepare a prepolymer with a number average molecular weight of 5,000.
[0197] 200 ppm of tetrabutyl titanate (manufactured by Aldrich) as a polycondensation catalyst was added to the prepolymer, and the temperature was raised to 240° C., after which a polycondensation reaction was carried out at 0.5 torr for 4 hours to prepare a biodegradable polyester resin having a number average molecular weight of 50,000.
[0198] (Production Example 2) A biodegradable polyester resin of Preparation Example 2 was prepared in the same manner as Preparation Example 1, except that no pretreated nanocellulose was added.
[0199] Alternatively, instead of Production Example 2, Kingfa's A400 may be used as a PBAT resin of the same composition but without nanocellulose.
[0200] The mechanical and thermal properties of the biodegradable polyester resins of Production Examples 1 and 2 of the present invention are shown in Table 1.
[0201] [Table 1]
[0202] [Production of biodegradable resin composition] (Examples A1 to A8) The polymer of Preparation Example 1 or Preparation Example 2, except that the components of the composition were changed based on Tables 2 and 3 below, was added with calcium carbonate (WS-2200), and one or more selected from the group consisting of a plasticizer (acetylated monoglyceride, Biocizer (registered trademark)), additive 1 (polycaprolactone; PCL), additive 2 (polylactic acid; PLA), antioxidant 1 (phenolic antioxidant, AO-60) or antioxidant 2 (phosphorus-based antioxidant, 2112 (AO)). The mixture was then charged into a kneader reactor and kneaded at a temperature of 175°C. The mixture was extruded with an extruder equipped with a single screw, cut with a hot-cut pellet cutter, and cooled to produce pelletized biodegradable resin compositions.
[0203] (Examples A9 and A10) The composition of Example A7 or Example A8 kneaded in a kneader reactor was charged into an extruder equipped with a twin screw, and the polymer of Preparation Example 1 or Preparation Example 2 was further added to adjust the content of the composition components in the following Table 3. This was extruded through an extruder equipped with a single screw, cut with a hot-cut pellet cutter, and cooled to prepare pellets of a biodegradable resin composition.
[0204] (Examples A11 to A13) The polymer of Preparation Example 1 or Preparation Example 2, except for the different components of the composition according to Table 4 below, was mixed with additives including PLA, calcium carbonate (WS-2200), plasticizer (acetylated monoglyceride), stabilizer (tris-2,4-teiary buthyl phenyl phosphate, 2112 RG grade), and chain extender (Joncryl), and the mixture was charged into a kneader reactor and kneaded at a temperature of 175°C. The mixture was extruded with an extruder equipped with a single screw, cut with a hot-cut pellet cutter, and cooled to prepare pelletized biodegradable resin compositions.
[0205] (Reference Examples A1 and A2) 100% by weight of the polymer of Preparation Example 1 (Reference Example A1) or Preparation Example 2 (Reference Example A2) was charged into a kneader reactor and kneaded at a temperature of 175°C, extruded using an extruder equipped with a single screw, cut using a hot-cut pellet cutter, and cooled to produce a pellet-shaped biodegradable resin composition.
[0206] [Table 2]
[0207] [Table 3]
[0208] [Table 4]
[0209] The measurement results for the thermal properties of the biodegradable resin composition of the present invention are shown in Table 5.
[0210] [Table 5]
[0211] The biodegradable resin compositions of Examples A1 to A10, despite containing a high content of calcium carbonate, exhibit a low weight loss rate at high temperatures (210°C) compared to the biodegradable resin compositions of Reference Examples A1 and A2 containing 100% by weight of the resin of Preparation Example 1 or 2. In particular, the weight loss rate of Examples A1, A2, A4, and A9 is 1% or less. In the calcium carbonate content variability experiment, the biodegradable resin compositions of Examples A1 to A10 all showed a change in calcium carbonate content of 2.5% or less, indicating that they can maintain a high CaCO3 content even after high-temperature processing.
[0212] In addition, the biodegradable resin compositions of Examples A1 to A10 exhibit the effect of decreasing the glass transition temperature (Tg) compared to the biodegradable resin compositions of Reference Examples A1 and A2 containing 100% by weight of the resin of Production Example 1 or 2.
[0213] With reference to Reference Example A1, the biodegradable resin compositions of Examples A1, A3, A4, A7, and A9 had a 70% to 100% reduction in crystalline heat of fusion at 70°C to 90°C, and a 32% to 90% reduction in crystalline heat of fusion at 100°C to 150°C.
[0214] With reference to Reference Example A2, the biodegradable resin compositions of Examples A2, A5, A6, A8, and A10 had a 50% to 100% reduction in crystalline heat of fusion at 70°C to 90°C, and a 24.7% to 96% reduction in crystalline heat of fusion at 100°C to 150°C.
[0215] [Production of biodegradable polyester film] (Examples B1 to B4 and Reference Example B1) Pellets prepared from the biodegradable resin compositions of Examples A9 to A13 in Tables 3 and 4 were dried at 80°C for 5 hours, and then melt-extruded at 160°C using a blown film extruder (Blown Film Extrusion Line, manufactured by Yujin Engineering Co., Ltd.) to prepare biodegradable polyester films having a thickness of 15 μm.
[0216] The measurement results of the mechanical properties of the biodegradable polyester film of the present invention are shown in Table 6.
[0217] [Table 6]
[0218] It was confirmed that the biodegradable polyester films containing high amounts of calcium carbonate in Examples B1 and B2 had excellent tensile strength and elongation, and also maintained excellent levels of tear strength. In the case of the biodegradable polyester films containing high amounts of calcium carbonate in Examples B3 and B4, the tensile strength, elongation, and tear strength decreased compared to Examples B1 and B2 due to the addition of PLA, but were still maintained at levels required for commercialization.
[0219] [Production of biodegradable polyester sheets] (Sheets 1-4) Pellets produced from Production Example 1, Production Example 2 (Kingfa, A400), Resin A (JINHUI, Ecoworld), Resin B (TUNHE, TH80IT) or Resin C (BASF, Ecoflex® C1200) were dried at 80°C for 5 hours and then melt extruded under the mold conditions in Tables 7 and 8 to produce biodegradable polyester sheets with a thickness of 20 μm.
[0220] (Example C1, Comparative Examples C1 and C2) Except for changing the components of the composition according to Table 7 below, a biodegradable resin composition was prepared by adding calcium carbonate to Preparation Example 1 or Resin A (JINHUI, Ecoworld) or Resin B (TUNHE, TH80IT) in the same manner as in Example A1, and then a biodegradable polyester sheet was produced by the same manner as in Sheet 1.
[0221] (Examples C2 to C13) Except for varying the components of the composition based on Table 8 below, a biodegradable resin composition was produced by adding one or more selected from the group consisting of calcium carbonate (WS-2200), a plasticizer (acetylated monoglyceride, Biocizer), polycaprolactone (PCL) and polylactic acid (PLA) to the biodegradable polyester resin of Production Example 1 or Production Example 2 using the same production method as in Example A1, and then a biodegradable polyester sheet was produced using the same production method as in Sheet 1.
[0222] [Table 7]
[0223] Conventional biodegradable polyester sheets containing a high content of calcium carbonate (Comparative Examples C1 and C2) require high torque under the molding conditions required for production, which is disadvantageous in terms of energy and cost, and the reduction in tensile strength or elongation is very large compared to sheets 3 and 4, making them unsuitable for the production of molded products. On the other hand, the biodegradable polyester sheet of the present invention (Example C1) was able to reduce the energy and cost required for molding. In addition, the biodegradable polyester film of the present invention contains a high content of calcium carbonate, which shows the effect of reducing raw material costs, and is also able to enhance the biodegradability of the polyester film and adjust the acidity of the decomposition products.
[0224] [Table 8]
[0225] Conventional biodegradable polyester sheets containing a high content of calcium carbonate showed a significant decrease in tensile strength or elongation (Comparative Examples C1 and C2 in Table 7) and were not suitable for producing molded products. However, the biodegradable polyester sheets of the present invention (Examples C2 to C13 in Table 8) were able to maintain tensile strength and elongation at or above a certain level compared to Sheet 1 or Sheet 2.
Claims
1. Biodegradable polyester resin and calcium carbonate (CaCO 3 ), A biodegradable resin composition having a reduction rate of a crystal peak represented by the following formula 1 of 50% or more: [Formula 1] Crystal peak reduction rate = (R p -C p ) / R p In the above formula 1, R p is the heat of crystalline fusion (J / g) of the biodegradable polyester resin in the temperature range of 70°C to 90°C, measured using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min; C p is the crystalline heat of fusion (J / g) of the biodegradable resin composition measured under the same conditions as above.
2. The calcium carbonate (CaCO 3 2. The biodegradable resin composition according to claim 1, wherein the biodegradable resin composition contains 30% by weight to 80% by weight of the polyvinyl chloride copolymer.
3. The calcium carbonate (CaCO 3 2. The biodegradable resin composition according to claim 1, wherein the biodegradable resin composition contains 40% by weight to 75% by weight of the polyvinyl chloride (PVC) based on the total weight of the biodegradable resin composition.
4. the biodegradable resin composition contains a plasticizer and an antioxidant, The plasticizer comprises one or more selected from the group consisting of glycerol, acrylate, glycerin, glycerol monostearate, and sorbitol; 2. The biodegradable resin composition according to claim 1, wherein the antioxidant comprises two or more selected from the group consisting of phosphorus-based antioxidants, phenol-based antioxidants, and pentaerythritol-based antioxidants.
5. Based on the total weight of the biodegradable resin composition, The plasticizer is present in an amount of 1% to 3% by weight. The biodegradable resin composition according to claim 4, comprising the antioxidant in an amount of 0.01% by weight to 4% by weight.
6. the antioxidant comprises the phosphorus-based antioxidant and the phenol-based antioxidant; 5. The biodegradable resin composition according to claim 4, wherein a weight ratio of the phosphorus-based antioxidant to the phenol-based antioxidant is 1:10 to 10:
1.
7. The biodegradable resin composition according to claim 1, wherein the biodegradable polyester resin contains nanocellulose in an amount of 0.01% by weight to 3% by weight based on the total weight of the biodegradable polyester resin.
8. The biodegradable resin composition further comprises a chain extender, The biodegradable resin composition according to claim 1, wherein the chain extender is contained in an amount of 0.01% by weight to 1% by weight based on the total weight of the biodegradable resin composition.
9. The biodegradable resin composition further contains one or more dispersants selected from the group consisting of polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate; The biodegradable resin composition according to claim 1, wherein the dispersant is contained in an amount of 1% by weight to 20% by weight based on the total weight of the biodegradable resin composition.
10. The biodegradable resin composition according to claim 1, wherein the isothermal weight loss of the biodegradable resin composition is 5% or less when the composition is maintained at an isothermal temperature of 210°C for 1 hour.
11. The biodegradable resin composition according to claim 1, wherein the calcium carbonate content has a variability of 5% or less at 600°C when the biodegradable resin composition is heated at a rate of 20°C / 1 min.
12. Biodegradable polyester resin and calcium carbonate (CaCO 3 The biodegradable resin composition includes The biodegradable resin composition is a biodegradable polyester film having a reduction rate of a crystal peak represented by the following formula 1 of 50% or more: [Formula 1] Crystal peak reduction rate = (R p -C p ) / R p In the above formula 1, R p is the heat of crystalline fusion (J / g) of the biodegradable polyester resin in the temperature range of 70°C to 90°C, measured using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min; C p is the crystalline heat of fusion (J / g) of the biodegradable resin composition measured under the same conditions as above.
13. The tensile strength is 5 MPa or more, The elongation rate is 85% or more, The biodegradable polyester film according to claim 12, having a tear strength of 75 N / mm or more.
14. Biodegradable polyester resin and calcium carbonate (CaCO 3 The biodegradable resin composition includes The biodegradable resin composition is a biodegradable polyester sheet having a reduction rate of a crystal peak represented by the following formula 1 of 50% or more: [Formula 1] Crystal peak reduction rate = (R p -C p ) / R p In the above formula 1, R p is the heat of crystalline fusion (J / g) of the biodegradable polyester resin in the temperature range of 70°C to 90°C, measured using a differential scanning calorimeter (DSC) in the process of heating from 40°C to 180°C at a rate of 10°C / min and then cooling to -50°C at a rate of 10°C / min; C p is the crystalline heat of fusion (J / g) of the biodegradable resin composition measured under the same conditions as above.
15. The tensile strength is 5 MPa or more, 15. The biodegradable polyester sheet according to claim 14, having an elongation of 10% or more.
Citation Information
Patent Citations
Polylactic acid-based mulching film
JP2014162799A
Biodegradable sheet
JP2014513640A
Biodegradable odor barrier film
JP2016526946A
Biodegradable film having tear propagation resistance
JP2017119850A
Production method of resin composite material
JP2020063370A