Separator for electrochemical element, manufacturing method thereof, and electrochemical element equipped with said separator
A crosslinked acrylic binder polymer with a benzophenone functional group addresses the challenge of achieving both peel strength and heat resistance in lithium secondary battery separators, ensuring stability and safety through a crosslinked organic-inorganic composite structure.
Patent Information
- Application Number
- JP2024529392
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-02-14
- Filing Date
- 2023-01-13
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-01-13
AI Technical Summary
Existing separators for lithium secondary batteries face challenges in achieving both high peel strength and heat resistance due to the low crosslinking density of crosslinked acrylic binder polymers, which affect the adhesive strength between the porous polyolefin base material and the coating layer.
A separator for electrochemical devices is developed with a crosslinked acrylic binder polymer containing a benzophenone functional group, which ensures both peel strength and heat resistance by forming a crosslinked structure via ultraviolet irradiation, combining a porous polymer base material with an organic-inorganic composite porous layer.
The separator achieves excellent peel strength and heat resistance, maintaining stability under high temperatures and preventing thermal shrinkage, thereby enhancing the safety and performance of electrochemical devices.
Smart Images

Figure 2024540498000001 
Figure 2024540498000002 
Figure 2024540498000003
Abstract
Description
[Technical field]
[0001] The present invention claims the benefit of the filing date of Korean Patent Application No. 10-2022-0019171, filed in the Korean Intellectual Property Office on February 14, 2022, the entire contents of which are incorporated herein by reference. The present invention relates to a separator for an electrochemical element, a manufacturing method thereof, and an electrochemical element including the separator. [Background technology]
[0002] In recent years, interest in energy storage technology has been increasing. As the fields of application are expanding to include mobile phones, camcorders, laptops, and even the energy of electric vehicles, there is a growing need for electrochemical devices used as power sources for such electronic devices with high energy density. Lithium secondary batteries are the electrochemical device that best meets such needs, and research into them is currently being actively conducted.
[0003] Such lithium secondary batteries are composed of a positive electrode, a negative electrode, an electrolyte, and a separator. Among these, the separator is required to have high ionic conductivity to increase the permeability of lithium ions, in addition to high insulating properties and high porosity to separate and electrically insulate the positive and negative electrodes.
[0004] As such a separator, a separator in which a polyolefin-based porous substrate is coated with a mixture of fine inorganic particles and a crosslinked acrylic binder polymer has been used. However, when the crosslinking density of the crosslinked acrylic binder polymer is low, the storage modulus is low, which is disadvantageous in terms of heat resistance, and when the crosslinking density is high, the storage modulus at high temperatures increases, but the adhesive strength decreases, which is disadvantageous in terms of peel strength between the polyolefin-based porous substrate and the coating layer.
[0005] Therefore, there is still a strong need for a separator using a cross-linked acrylic binder polymer that can ensure both heat resistance and peel strength between a polyolefin porous substrate and a coating layer. Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, an object of the present invention is to provide a separator for an electrochemical device, which includes a cross-linked acrylic binder polymer that can ensure both the peel strength between a porous polymer substrate and an organic-inorganic composite porous layer and heat resistance, and an electrochemical device including the separator.
[0007] Another object of the present invention is to provide a method for producing a separator for an electrochemical device, comprising a crosslinked acrylic binder polymer, which can ensure both the peel strength between a porous polymer substrate and an organic-inorganic composite porous layer and heat resistance. [Means for solving the problem]
[0008] In order to achieve the above object, according to one aspect of the present invention, there is provided a separator for an electrochemical device according to the following embodiment.
[0009] The first embodiment relates to a separator for an electrochemical device, comprising: a porous polymer substrate; and an organic-inorganic composite porous layer located on at least one surface of the porous polymer substrate and including inorganic particles and a particulate acrylic binder polymer; wherein the particulate acrylic binder polymer has a structure crosslinked via a benzophenone functional group.
[0010] In the second embodiment, in the first embodiment, the particle-type acrylic binder polymer may include an acrylic monomer having a benzophenone functional group.
[0011] In the third embodiment, in the second embodiment, the particulate acrylic binder polymer may further include a branched or unbranched (meth)acrylic acid monomer having 1 to 20 carbon atoms, a branched or unbranched (meth)acrylate monomer having 1 to 20 carbon atoms, an acrylonitrile monomer, a vinylpyrrolidone monomer, a vinyl acetate monomer, or two or more thereof.
[0012] In a fourth embodiment, in any one of the first to third embodiments, the particle-type acrylic binder polymer may have a structure represented by the following Formula 1: [ka]
[0013] In the above Chemical Formula 1, m, n, o, and p are each an integer of 1 or more.
[0014] In a fifth embodiment, in any one of the first to fourth embodiments, the particulate acrylic binder polymer may have a storage modulus of 20,000 Pa to 300,000 Pa at 50° C.
[0015] In a sixth embodiment, in any one of the first to fifth embodiments, the particulate acrylic binder polymer may have a glass transition temperature of -70°C to 70°C.
[0016] In a seventh embodiment, in any one of the first to sixth embodiments, the particulate acrylic binder polymer may have a gel fraction of 10% to 90%.
[0017] In an eighth embodiment, in any one of the first to seventh embodiments, the particulate acrylic binder polymer may have an average particle size of 0.001 μm to 10 μm.
[0018] The ninth embodiment is any one of the first to eighth embodiments, wherein the inorganic particles are BaTiO, BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb1- x La x Zr1- y Ti y O3 (PLZT, where 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Al(OH)3, ZrO2, Y2O3, Al2O3, γ - AlOOH, SiC, TiO2, lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y -based glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2), SiS2 - based glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5 - based glass (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7), or can include two or more of these.
[0019] In a tenth embodiment, in any one of the first to ninth embodiments, the inorganic particles may have an average particle size of 0.1 nm to 2.0 μm.
[0020] In an eleventh embodiment, in any one of the first to tenth embodiments, the organic-inorganic composite porous layer may further include a non-particle type binder polymer.
[0021] In a twelfth embodiment, in the eleventh embodiment, the non-particle type binder polymer may include carboxymethyl cellulose, polyacrylic acid, polyacrylamide, or two or more thereof.
[0022] The thirteenth embodiment is any one of the first to twelfth embodiments, in which the weight ratio of the inorganic particles to the binder polymer may be 99.9:0.1 to 70:30, and the binder polymer may include a particle-type acrylic binder polymer.
[0023] In a fourteenth embodiment, in any one of the eleventh to thirteenth embodiments, the weight ratio of the particulate acrylic binder polymer to the non-particulate binder polymer may be 5:95 to 95:5.
[0024] In a fifteenth embodiment, in any one of the first to fourteenth embodiments, the organic-inorganic composite porous layer may have a thickness of 0.1 μm to 10 μm.
[0025] As a 16th embodiment, in any one of the 1st to 15th embodiments, the separator for an electrochemical device may have a thermal shrinkage rate of 10% or less in the machine direction (MD) and 10% or less in the transverse direction (TD) after being left at 135°C for 30 minutes.
[0026] The seventeenth embodiment is any one of the first to sixteenth embodiments, wherein the separator for an electrochemical device has a peel strength between the porous polymer substrate and the organic / inorganic composite porous layer of 5 to 1000 g. f / 15mm.
[0027] In order to achieve the above object, according to one aspect of the present invention, there is provided a method for manufacturing a separator for an electrochemical device, according to the following embodiment.
[0028] An eighteenth embodiment relates to a method for manufacturing a separator for an electrochemical element, comprising: preparing a slurry for forming an organic-inorganic composite porous layer, the slurry including inorganic particles and a non-crosslinked particle-type acrylic binder polymer including a benzophenone functional group; coating and drying the slurry for forming the organic-inorganic composite porous layer on at least one surface of a porous polymer substrate; and irradiating with ultraviolet light.
[0029] In the 19th embodiment, in the 18th embodiment, the non-crosslinked particle type acrylic binder polymer may include a first acrylic monomer and a second acrylic monomer, and the first acrylic monomer may include benzophenone methacrylate, 6-(4-benzoylphenoxy)hexyl methacrylate, benzophenone acrylate, or two or more thereof.
[0030] The twentieth embodiment is the 19th embodiment, wherein the second acrylic monomer may include branched or unbranched (meth)acrylic acid having 1 to 20 carbon atoms, branched or unbranched (meth)acrylate having 1 to 20 carbon atoms, acrylonitrile, vinylpyrrolidone, vinyl acetate, or two or more thereof.
[0031] The 21st embodiment is any one of the 18th to 20th embodiments, wherein the non-crosslinked particle type acrylic binder polymer may include a copolymer of the following Chemical Formula 2: [ka]
[0032] In the above Chemical Formula 2, m, n, o, and p are each an integer of 1 or more.
[0033] In a twenty-second embodiment, in any one of the nineteenth to twenty-first embodiments, the content of the first acrylic monomer may be 500 ppm to 20,000 ppm based on the weight of the second acrylic monomer.
[0034] In a 23rd embodiment, in any one of the 18th to 22nd embodiments, the non-crosslinked particle-type acrylic binder polymer may have a storage modulus of 10,000 Pa to 80,000 Pa at 50° C. before UV irradiation.
[0035] In a 24th embodiment, in any one of the 18th to 23rd embodiments, the change rate of storage modulus at 50° C. before and after UV irradiation of the particulate acrylic binder polymer may be 20% to 300%.
[0036] In a twenty-fifth embodiment, in any one of the eighteenth to twenty-fourth embodiments, the ultraviolet ray irradiation amount may be 0.1J to 10J.
[0037] In a twenty-sixth embodiment, in any one of the eighteenth to twenty-fifth embodiments, the ultraviolet light may have a wavelength of 200 nm to 400 nm.
[0038] In a twenty-seventh embodiment, in the twenty-sixth embodiment, the ultraviolet light may have a wavelength of 230 nm to 350 nm.
[0039] In order to achieve the above object, according to one aspect of the present invention, there is provided an electrochemical device according to the following embodiment.
[0040] The 28th embodiment relates to an electrochemical device comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator comprises a separator for electrochemical devices according to any one of the 1st to 17th embodiments. Effect of the Invention
[0041] The separator for an electrochemical device according to one embodiment of the present invention includes a particulate acrylic binder polymer crosslinked via a benzophenone functional group, and has excellent peel strength and heat resistance between a porous polymer substrate and an organic-inorganic composite porous layer.
[0042] In the method for producing a separator for an electrochemical element according to an embodiment of the present invention, the particulate acrylic binder polymer is not crosslinked during the coating process of the slurry for forming the organic-inorganic composite porous layer, so that the peel strength between the porous polymer substrate and the organic-inorganic composite porous layer can be ensured, and after the coating process, the particulate acrylic binder polymer is crosslinked via the benzophenone functional group by irradiation with ultraviolet light, so that heat resistance can be ensured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] Hereinafter, preferred embodiments of the present invention will be described in detail. Prior to that, the terms or words used in the specification and claims should not be interpreted limitedly to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that is consistent with the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention.
[0044] Therefore, it should be understood that the configurations described in the embodiments of this specification are merely the most preferred embodiments of the present invention and do not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application.
[0045] A method for producing a separator for an electrochemical element according to one aspect of the present invention includes the steps of: preparing a slurry for forming an organic-inorganic composite porous layer, the slurry including inorganic particles and a non-crosslinked particle-type acrylic binder polymer including a benzophenone functional group; coating and drying the slurry for forming the organic-inorganic composite porous layer on at least one surface of a porous polymer substrate; and irradiating with ultraviolet light.
[0046] Hereinafter, the main parts of a method for producing a separator for an electrochemical element according to one embodiment of the present invention will be described.
[0047] First, a slurry for forming an organic-inorganic composite porous layer is prepared, which contains inorganic particles and a non-crosslinked particle-type acrylic binder polymer containing a benzophenone functional group.
[0048] The inorganic particles are not particularly limited as long as they are electrochemically stable. In other words, the inorganic particles that can be used in the present invention are those that can be used in the operating voltage range (e.g., Li / Li + There are no particular limitations as long as oxidation and / or reduction reactions do not occur at a potential of 0 to 5 V relative to the potential of the electrolyte. In particular, when inorganic particles having a high dielectric constant are used as the inorganic particles, it may be easy to improve the ionic conductivity of the electrolyte by contributing to an increase in the degree of dissociation of an electrolyte salt, for example, a lithium salt, in the liquid electrolyte.
[0049] In one embodiment of the present invention, the inorganic particles may include high dielectric constant inorganic particles having a dielectric constant of 5 or more, preferably 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb1- x La x Zr1- y Ti y O3(PLZT, 0 <x<1、0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3)Examples include O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, or mixtures thereof.
[0050] In another embodiment of the present invention, as the inorganic particles, inorganic particles having lithium ion transfer ability, that is, inorganic particles containing a lithium element but having a function of moving lithium ions without storing lithium can be used. Non-limiting examples of inorganic particles having lithium ion transfer ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y -based glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2), SiS2-based glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5-based glass (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7), or two or more of these can be included.
[0051] In one embodiment of the present invention, the inorganic particles may have an average particle size of 0.1 nm to 2.0 μm, or 0.1 μm to 1 μm, or 0.2 μm to 0.8 μm. When the average particle size of the inorganic particles satisfies the above-mentioned range, the dispersibility of the inorganic particles is maintained, making it easy to adjust the physical properties of the separator, and it is easy to prevent the thickness of the organic-inorganic composite porous layer from increasing, thereby improving the mechanical properties. In addition, it is easy to reduce the probability of an internal short circuit occurring during charging and discharging of the battery due to an excessively large pore size of the organic-inorganic composite porous layer.
[0052] Throughout this specification, the average particle size is D 50 It means particle size, and "D 50 "Particle size" refers to the particle size at 50% of the cumulative distribution of the number of particles according to the particle size. The particle size can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500). When the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution. The D50 particle size can be measured by calculating the diameter of the particle at 50% of the cumulative distribution of the number of particles according to the particle size in the measuring device.
[0053] The non-crosslinked particulate acrylic binder polymer containing a benzophenone functional group has a structure in which an acrylic copolymer has a particulate shape and contains a benzophenone functional group, and is in a state before crosslinking and does not include a crosslinked structure.
[0054] The non-crosslinked particulate acrylic binder polymer containing a benzophenone functional group has a low storage modulus before being irradiated with ultraviolet light, and can ensure excellent peel strength between the porous polymer substrate and the organic-inorganic composite porous layer.
[0055] The benzophenone functional group plays a role in cross-linking the acrylic copolymers when irradiated with ultraviolet light. Specifically, when irradiated with ultraviolet light, hydrogen atoms in the benzophenone functional group are removed by hydrogen abstraction to form radicals, which form radicals in the acrylic copolymers, thereby cross-linking the acrylic copolymers.
[0056] After irradiation with ultraviolet light, the acrylic copolymers in the non-crosslinked particulate acrylic binder polymer are crosslinked with each other, so that the particulate acrylic binder polymer has a high storage modulus and can ensure heat resistance.
[0057] In one embodiment of the present invention, the non-crosslinked particle type acrylic binder polymer may include a first acrylic monomer and a second acrylic monomer.
[0058] In this case, the first acrylic monomer may include benzophenone methacrylate, 6-(4-benzoylphenoxy)hexyl methacrylate, benzophenone acrylate, or two or more thereof.
[0059] In one embodiment of the present invention, the second acrylic monomer may include branched or unbranched (meth)acrylic acid having 1 to 20 carbon atoms, branched or unbranched (meth)acrylate having 1 to 20 carbon atoms, acrylonitrile, vinylpyrrolidone, vinyl acetate, or two or more of these.
[0060] The branched or unbranched (meth)acrylic acid having 1 to 20 carbon atoms and the branched or unbranched (meth)acrylate having 1 to 20 carbon atoms can include, for example, an alkyl (meth)acrylate, an alicyclic (meth)acrylate, and a hydroxy (meth)acrylate.
[0061] When the second acrylic monomer includes one of the above-mentioned types, it may be easier to maintain the particle shape in an aqueous dispersion medium.
[0062] In one embodiment of the present invention, the content of the first acrylic monomer may be 500 ppm to 20,000 ppm, or 1,000 ppm to 10,000 ppm, or 5,000 ppm to 10,000 ppm, based on the weight of the second acrylic monomer. When the content of the first acrylic monomer satisfies the above-mentioned range, crosslinking may occur at a desired level, and it may be easier to prevent the problem of polymer chain breakage due to radicals generated by the first acrylic monomer.
[0063] In one embodiment of the present invention, the non-crosslinked particle type acrylic binder polymer may include a copolymer of the following Chemical Formula 2: [ka]
[0064] In the above Chemical Formula 2, m, n, o, and p are each an integer of 1 or more.
[0065] The non-crosslinked particulate acrylic binder polymer containing a benzophenone functional group has a low storage modulus at high temperatures before UV irradiation, and can ensure excellent peel strength between the porous polymer substrate and the organic-inorganic composite porous layer. For example, the storage modulus of the non-crosslinked particulate acrylic binder polymer at 50°C before UV irradiation may be 10,000 Pa to 80,000 Pa. When the storage modulus of the non-crosslinked particulate acrylic binder polymer at 50°C satisfies the above-mentioned range, it may be easier to ensure peel strength between the porous polymer substrate and the organic-inorganic composite porous layer.
[0066] Herein, the storage modulus can be measured by dynamic mechanical analysis (DMA). For example, the sample can be tested at a constant frequency of 1 Hz, a preload force of 0.01 N, an amplitude of 20 μm, and a force track of 120%, from −100° C. to 150° C. at a tensile force of 1° C. / min.
[0067] In one embodiment of the present invention, the organic-inorganic composite porous layer forming slurry can contain an aqueous dispersion medium. When the organic-inorganic composite porous layer forming slurry contains an aqueous dispersion medium, it has an advantage that it is environmentally friendly and does not require excessive heat for drying. It also has an advantage that it does not require additional explosion-proof facilities.
[0068] In one embodiment of the invention, the aqueous dispersion medium may comprise water, methanol, ethanol, ethylene glycol, diethylene glycol, glycerol alcohol, or two or more of these.
[0069] The organic-inorganic composite porous layer forming slurry may be prepared by dispersing the non-crosslinked particle-type acrylic binder polymer in a dispersion medium, and then adding and dispersing the inorganic particles, but the method for preparing the slurry is not limited thereto.
[0070] In one embodiment of the present invention, the weight ratio of the inorganic particles to the binder polymer may be 99:1 to 70:30, or 97:3 to 90:10. In this case, the binder polymer may include a non-crosslinked particle type acrylic binder polymer. When the weight ratio of the inorganic particles to the binder polymer satisfies the above range, the organic-inorganic composite porous layer may be stably maintained.
[0071] In one embodiment of the present invention, the organic-inorganic composite porous layer forming slurry may further include a non-particle-type binder polymer. In this case, it may be advantageous to ensure heat resistance by increasing the adhesive force between inorganic particles. In addition, in the weight ratio of the inorganic particles to the binder polymer, the binder polymer may include a non-crosslinked particle-type acrylic binder polymer and a non-particle-type binder polymer.
[0072] In one embodiment of the present invention, the non-particle type binder polymer may be an aqueous binder polymer, that is, a binder polymer that is dissolved in an aqueous solvent under aqueous conditions or dispersed by an aqueous dispersion medium.
[0073] In one embodiment of the present invention, the non-particulate binder polymer may include carboxymethyl cellulose, polyacrylic acid, polyacrylamide, or two or more of these.
[0074] In one embodiment of the present invention, the weight ratio of the non-crosslinked particulate acrylic binder polymer and the non-particulate binder polymer may be 5:95 to 95:5. When the weight ratio of the non-crosslinked particulate acrylic binder polymer and the non-particulate binder polymer satisfies the above-mentioned range, it is easier to ensure processability during coating and heat resistance.
[0075] In one embodiment of the present invention, the organic-inorganic composite porous layer forming slurry may further include a dispersant.
[0076] In one embodiment of the invention, the dispersant may comprise polymethacrylate, polymethacrylic acid, sodium polymethacrylate, polyvinyl alcohol, sodium polyacrylate, or two or more of these.
[0077] Next, the organic / inorganic composite porous layer forming slurry is coated on at least one surface of a porous polymer substrate and dried.
[0078] The porous polymer substrate can be used without any particular limitation as long as it can be used as a material for a separator for an electrochemical element. Such a porous polymer substrate is a thin film containing a polymer material, and non-limiting examples of the polymer material include polymer resins such as polyolefin resin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene. In addition, the porous polymer substrate can be a nonwoven fabric formed from the polymer material as described above, or a porous polymer film, or a laminate of two or more of them. Specifically, the porous polymer substrate can be any one of the following a) to e).
[0079] a) a porous film formed by melting and extruding a polymer resin; b) a multilayer film in which two or more of the porous films of a) are laminated; c) a nonwoven fabric web produced by accumulating filaments obtained by melting / spinning a polymer resin; d) a multilayer film in which two or more of the nonwoven fabric webs of c) are laminated; and e) a multilayer porous film including two or more of a) to d).
[0080] In order to ensure excellent breathability and porosity from the above-mentioned materials, the porous polymer substrate may be prepared by forming pores through a conventional method known in the art, for example, a wet method using a solvent, diluent, or pore-forming agent, or a dry method using a stretching method.
[0081] In one embodiment of the present invention, the thickness of the porous polymer substrate is not particularly limited, and may be 1 μm to 100 μm, or 1 μm to 30 μm. When the thickness of the porous polymer substrate is within the above-mentioned range, it is possible to easily ensure the energy density while preventing the problem that the separator is easily damaged during use of the battery.
[0082] The pore size and porosity of the porous polymer substrate are not particularly limited as long as they are suitable for use in electrochemical devices, and the pore size may be 0.01 μm to 50 μm, or 0.1 μm to 20 μm, and the porosity may be 5% to 95%. When the pore size and porosity are within the above-mentioned ranges, it may be easy to prevent the porous polymer substrate from acting as a resistor, and it may be easy to maintain the mechanical properties of the porous polymer substrate.
[0083] The porosity and pore size of the porous polymer substrate can be measured by a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Bell Japan Inc, Belsorp-II mini) using a nitrogen gas adsorption flow method in a BET 6-point method.
[0084] Non-limiting examples of the method for coating one side of the porous polymer substrate with the slurry for forming the organic / inorganic composite porous layer include a dip coating method, a die coating method, a roll coating method, a comma coating method, a microgravure coating method, a doctor blade coating method, a reverse roll coating method, and a direct roll coating method.
[0085] The drying may be carried out by any method known in the art and may be carried out in a batch or continuous manner using an oven or heated chamber at a temperature range that takes into account the vapor pressure of the aqueous dispersion medium used.
[0086] In one embodiment of the present invention, the drying may be performed at 40° C. to 100° C. When the drying is performed within the above range, it may be easier to prevent the organic-inorganic composite porous layer-forming slurry from being partially undried, and it may be easier to prevent the porous polymer substrate from being deformed due to high temperatures.
[0087] Next, the mixture is irradiated with ultraviolet light, which causes the acrylic copolymers in the non-crosslinked particle-type acrylic binder polymer to crosslink with each other via the benzophenone functional groups.
[0088] After UV irradiation, the acrylic copolymers in the non-crosslinked particulate acrylic binder polymer are crosslinked with each other, so that the particulate acrylic binder polymer has a high storage modulus at high temperatures and can ensure heat resistance. For example, the change rate of the storage modulus of the particulate acrylic binder polymer at 50°C before and after UV irradiation may be 20% to 300%. When the change rate of the storage modulus of the particulate acrylic binder polymer at 50°C before and after UV irradiation satisfies the above-mentioned range, it may be easier for the separator to ensure heat resistance while ensuring the adhesive strength between the porous polymer substrate and the organic-inorganic composite porous layer.
[0089] The rate of change in storage modulus at 50° C. can be measured as follows: Rate of change in storage modulus at 50°C = (storage modulus at 50°C after UV irradiation - storage modulus at 50°C before UV irradiation) / (storage modulus at 50°C before UV irradiation)
[0090] The ultraviolet irradiation may be performed by using an ultraviolet crosslinking device, and the ultraviolet irradiation time and the irradiation light amount may be appropriately adjusted in consideration of conditions such as the content ratio of the benzophenone functional group. For example, the ultraviolet irradiation time and the irradiation light amount may be set under conditions that the polymer chains in the particulate acrylic binder polymer are sufficiently crosslinked to ensure the desired heat resistance, while the separator is not damaged by the heat generated by the ultraviolet lamp. In addition, the ultraviolet lamp used in the ultraviolet crosslinking device may be appropriately selected from a high pressure mercury lamp, a metal lamp, a gallium lamp, an LED lamp, etc., and the emission wavelength and capacity of the ultraviolet lamp may be appropriately selected according to the process.
[0091] In one embodiment of the present invention, the dose of the ultraviolet light may be 0.1J to 10J, or 0.3J to 6J.
[0092] The dose of the UV rays can be measured using a portable light meter called an H-type UV bulb and a UV power puck manufactured by Miltec. When measuring the dose using an H-type UV bulb manufactured by Miltec, three wavelength values, UVA, UVB, and UVC, are obtained according to wavelength, and the UV rays of the present invention correspond to UVA. The UV power puck is passed on a conveyor under a light source under the same conditions as the sample, and the UV light dose value displayed on the UV power puck at this time is referred to as the "ultraviolet light dose."
[0093] In one embodiment of the present invention, the ultraviolet ray may have a wavelength of 200 nm to 400 nm, or 230 nm to 350 nm. In particular, when the ultraviolet ray has a wavelength of 230 nm to 350 nm, ultraviolet absorption by the benzophenone functional group can occur most actively.
[0094] Conventional acrylic binders have the problem that when the degree of crosslinking is low, the heat resistance is poor, and when the degree of crosslinking is high, the adhesive strength is reduced.
[0095] In the method for producing a separator for an electrochemical element according to one embodiment of the present invention, the particulate acrylic binder polymer is not crosslinked before the organic-inorganic composite porous layer-forming slurry is irradiated with ultraviolet light, and therefore the particulate acrylic binder polymer is excellent in adhesive properties and can ensure adhesive strength between the porous polymer substrate and the organic-inorganic composite porous layer. In addition, after the organic-inorganic composite porous layer-forming slurry is irradiated with ultraviolet light, the particulate acrylic binder polymer is crosslinked and can ensure heat resistance. As a result, the finally produced separator for an electrochemical element can have excellent heat resistance while ensuring sufficient adhesive strength between the porous polymer substrate and the organic-inorganic composite porous layer.
[0096] As described above, a separator for an electrochemical device may be manufactured according to the method for manufacturing a separator for an electrochemical device according to an embodiment of the present invention.
[0097] According to one aspect of the present invention, there is provided a separator for an electrochemical device, comprising: a porous polymer substrate; and an organic-inorganic composite porous layer located on at least one surface of the porous polymer substrate, the organic-inorganic composite porous layer including inorganic particles and a particulate acrylic binder polymer; wherein the particulate acrylic binder polymer has a structure crosslinked via a benzophenone functional group.
[0098] For the porous polymer substrate and the inorganic particles, please refer to the above description.
[0099] The organic-inorganic composite porous layer may be formed on one or both sides of the porous polymer substrate, and the organic-inorganic composite porous layer may prevent the porous polymer substrate from exhibiting severe thermal shrinkage behavior at high temperatures due to inorganic particles, thereby improving the safety of the separator.
[0100] In the organic-inorganic composite porous layer, the particulate acrylic binder polymer adheres the inorganic particles to each other (i.e., the particulate acrylic binder polymer connects and fixes the inorganic particles) so that the inorganic particles and the porous polymer substrate can be maintained in a bound state.
[0101] The particulate acrylic binder polymer has a crosslinked structure, specifically, a structure in which acrylic copolymers are crosslinked with each other via benzophenone functional groups.
[0102] In one embodiment of the present invention, the crosslinked particle-type acrylic binder polymer may include an acrylic monomer having a benzophenone functional group, and the acrylic monomer having a benzophenone functional group may have a structure crosslinked via the benzophenone functional group. For example, the particle-type acrylic binder polymer may include a 4-benzoylphenyl methacrylate monomer as the acrylic monomer having a benzophenone functional group.
[0103] In one embodiment of the present invention, the particulate acrylic binder polymer may further include a branched or unbranched (meth)acrylic acid monomer having 1 to 20 carbon atoms, a branched or unbranched (meth)acrylate monomer having 1 to 20 carbon atoms, an acrylonitrile monomer, a vinylpyrrolidone monomer, a vinyl acetate monomer, or two or more of these. The branched or unbranched (meth)acrylic acid monomer having 1 to 20 carbon atoms and the branched or unbranched (meth)acrylate monomer having 1 to 20 carbon atoms may include alkyl (meth)acrylate, alicyclic (meth)acrylate, hydroxy (meth)acrylate, acrylonitrile, vinylpyrrolidone, vinyl acetate, etc.
[0104] In one embodiment of the present invention, the crosslinked particle-type acrylic binder polymer may have a structure of the following Chemical Formula 1: [ka]
[0105] In the above Chemical Formula 1, m, n, o, and p are each an integer of 1 or more.
[0106] In one embodiment of the present invention, the crosslinked particulate acrylic binder polymer may have a storage modulus of 20,000 Pa to 300,000 Pa at 50° C. When the storage modulus of the crosslinked particulate acrylic binder polymer at 50° C. satisfies the above-mentioned range, a separator including the particulate acrylic binder polymer may have excellent heat resistance. For example, the separator may have a thermal shrinkage rate of 10% or less in the machine direction (MD) and 10% or less in the transverse direction (TD) after being left at 135° C. for 30 minutes.
[0107] In one embodiment of the present invention, the crosslinked particulate acrylic binder polymer may have a glass transition temperature of −70° C. to 70° C. When the crosslinked particulate acrylic binder polymer satisfies the above-mentioned glass transition temperature, it may be easier to realize adhesive strength between the porous polymer substrate and the organic-inorganic composite porous layer.
[0108] The glass transition temperature of the particulate acrylic binder polymer can be measured using a differential scanning calorimetry (DSC). Specifically, the glass transition temperature can be measured at a temperature rise rate of 10°C / min (-50°C to 250°C) using a differential scanning calorimetry. For example, the glass transition temperature can be measured using DSC 250 (TA).
[0109] In one embodiment of the present invention, the crosslinked particulate acrylic binder polymer may have a gel fraction of 10% to 90%. When the gel fraction of the particulate acrylic binder polymer is in the above-mentioned range, the particulate acrylic binder polymer may more easily have a high-temperature storage modulus to such an extent that the particulate acrylic binder polymer has excellent heat resistance. For example, the particulate acrylic binder polymer may easily have a storage modulus of 20,000 Pa to 300,000 Pa at 50°C.
[0110] The gel fraction of the crosslinked particulate acrylic binder polymer is calculated as a percentage of the initial weight by measuring the weight of the crosslinked particulate acrylic binder polymer after immersing the crosslinked particulate acrylic binder polymer in a xylene solution at 135° C. and boiling for 12 hours according to ASTM D 2765.
[0111] In one embodiment of the present invention, the particulate acrylic binder polymer may have an average particle size of 0.001 μm to 10 μm. When the particulate acrylic binder polymer has an average particle size within the above range, the processability during coating may be ensured, and the stability of the organic-inorganic composite porous layer may be more easily achieved.
[0112] In one embodiment of the present invention, the organic-inorganic composite porous layer may have a structure in which the inorganic particles are filled and in contact with each other and bound to each other by the particulate acrylic binder polymer, thereby forming interstitial volumes between the inorganic particles, and the interstitial volumes between the inorganic particles may become vacant spaces to form pores.
[0113] In one embodiment of the present invention, the organic-inorganic composite porous layer may have a thickness of 0.1 μm to 10 μm. When the thickness of the organic-inorganic composite porous layer satisfies the above-mentioned range, appropriate adhesive strength and heat resistance can be achieved.
[0114] In one embodiment of the present invention, the organic-inorganic composite porous layer may have an average pore size in the range of 0.001 μm to 30 μm, or 0.01 μm to 10 μm. The porosity of the organic-inorganic composite porous layer may be in the range of 5 to 95%, 10 to 95%, 20 to 90%, or 30 to 80%. The porosity corresponds to a value obtained by subtracting the volume converted into the weight and density of each component of the organic-inorganic composite porous layer from the volume calculated from the thickness, width, and length of the organic-inorganic composite porous layer.
[0115] Meanwhile, in the present invention, the porosity and average pore size of the organic-inorganic composite porous layer can be measured by a BET 6-point method using a scanning electron microscope (SEM) image, a mercury porosimeter, a capillary flow porometer, or a porosimetry analyzer (Belsorp-II mini, Bell Japan Inc.) by a nitrogen gas adsorption flow method.
[0116] The separator for an electrochemical element according to one embodiment of the present invention includes a particulate acrylic binder polymer having a structure crosslinked via a benzophenone functional group, and thus has excellent adhesive strength and heat resistance between a porous polymer substrate and an organic-inorganic composite porous layer.
[0117] In one embodiment of the present invention, the separator for electrochemical devices may have a thermal shrinkage rate after being left at 135°C for 30 minutes in a machine direction (MD) of 10% or less, or 0 to 10%, or 0 to 6%, and a thermal shrinkage rate in a transverse direction (TD) of 10% or less, or 0 to 10%, or 0 to 6%.
[0118] In one embodiment of the present invention, the separator for an electrochemical element has a peel strength between the porous polymer substrate and the organic-inorganic composite porous layer of 5 g f / 15mm~1000g f / 15mm, or 10g f / 15mm~300g f / 15mm, or 30g f / 15mm or more.
[0119] The peel strength between the porous polymer substrate and the organic / inorganic composite porous layer can be measured by fixing a separator on a glass plate using double-sided tape, firmly attaching the tape to the exposed organic / inorganic composite porous layer, and measuring the force required to peel off the tape using a tensile strength measuring device. For example, the tensile strength measuring device can be an 11 oyd LS-1.
[0120] An electrochemical device can be produced by interposing the separator for an electrochemical device between a positive electrode and a negative electrode.
[0121] The electrochemical device can be in various shapes, such as cylindrical, rectangular, or pouch-shaped.
[0122] The electrochemical device may be a lithium secondary battery, which may include a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0123] The electrode to be used together with the separator for an electrochemical device according to an embodiment of the present invention is not particularly limited, and may be prepared in a form in which an electrode active material layer including an electrode active material, a conductive material, and a binder is bound to a current collector according to a conventional method known in the art.
[0124] Among the electrode active materials, non-limiting examples of the positive electrode active material include layered compounds such as lithium cobalt complex oxide (LiCoO2) and lithium nickel oxide (LiNiO2), and compounds substituted with one or more transition metals; 1+x Mn 2-x O4 (where x = 0-0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O5, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M xLithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01-0.3). 2-x M x Examples of lithium manganese composite oxides include, but are not limited to, lithium manganese composite oxides represented by the chemical formula LiMn2O4 in which part of the Li is replaced by an alkaline earth metal ion; disulfide compounds; and Fe2(MoO4)3.
[0125] Non-limiting examples of the negative electrode active material include conventional negative electrode active materials that can be used in the negative electrodes of conventional electrochemical devices, and in particular, lithium metal or lithium alloys, lithium adsorbent materials such as carbon, petroleum coke, activated carbon, graphite, or other carbons, etc., can be used.
[0126] Non-limiting examples of positive current collectors include foils made of aluminum, nickel, or combinations thereof, and non-limiting examples of negative current collectors include foils made of copper, gold, nickel, or copper alloys, or combinations thereof.
[0127] In one embodiment of the present invention, the conductive material used in the negative electrode and the positive electrode may be added in an amount of 1% by weight to 30% by weight based on the total weight of each active material layer. Such a conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fibers such as carbon fiber and metal fiber; carbon fluoride; metal powder such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives.
[0128] In one embodiment of the present invention, the binder used in the negative and positive electrodes is a component that aids in binding between the active material and the conductive material and the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of each active material layer. Examples of such binders include polyvinylidene fluoride (PVdF), polyacrylic acid (PAA), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, various copolymers, and the like.
[0129] In one embodiment of the present invention, the electrochemical device includes an electrolyte solution, and the electrolyte solution may include an organic solvent and a lithium salt. The electrolyte solution may be an organic solid electrolyte, an inorganic solid electrolyte, or the like.
[0130] Examples of the organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0131] The lithium salt is a substance that is easily dissolved in the organic solvent, such as LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylborate, imides, and the like may be used.
[0132] In addition, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. may be added to the electrolyte solution in order to improve charge / discharge characteristics, flame retardancy, etc. In some cases, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further added to impart non-flammability, and carbon dioxide gas may be further added to improve high-temperature storage characteristics.
[0133] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.
[0134] As the inorganic solid electrolyte, for example, nitrides, halides, sulfates, etc. of Li, such as LiN, LiI, LiNI, LiN-LiI-LiOH, LiSiO, LiSiO-LiI-LiOH, LiSiS, LiSiO, LiSiO-LiI-LiOH, LiPO-LiS-SiS2, etc., may be used.
[0135] The electrolyte injection may be performed at a suitable stage during the battery manufacturing process depending on the manufacturing process and the required properties of the final product, i.e., before the battery assembly or at the final stage of the battery assembly.
[0136] In one embodiment of the present invention, a process for applying the separator for an electrochemical device to a battery may include a lamination or stack process of the separator and the electrodes and a folding process in addition to a general winding process.
[0137] In one embodiment of the present invention, the separator for an electrochemical device may be interposed between a positive electrode and a negative electrode of an electrochemical device, or may be interposed between adjacent cells or electrodes when a plurality of cells or electrodes are assembled to form an electrode assembly. The electrode assembly may have various structures such as a simple stack type, a jelly-roll type, a stack-folding type, and a lamination-stack type.
[0138] The present invention will be described in detail below with reference to examples to aid in understanding the present invention. However, the examples of the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0139] Example 1 [Preparation of non-crosslinked particle type acrylic binder polymer] 2-Ethylhexyl acrylate monomer (LG Chem), butyl acrylate monomer, and 2-hydroxyethyl acrylate monomer were polymerized in a weight ratio of 75:10:15, and then the polymer and 10,000 ppm of 4-benzoylphenyl methacrylate (LG Chem) monomer were polymerized at 60°C to produce a non-crosslinked particle-type acrylic binder polymer (average particle size (D50): 1 μm).
[0140] [Production of separator for electrochemical element] 4.5 wt% of the non-crosslinked particle type acrylic binder polymer prepared above, 93.5 wt% of Al2O3 (Sumitomo, average particle size (D50): 500 nm) as inorganic particles, 1.5 wt% of carboxymethylcellulose (weight average molecular weight: 173,000, GL Chem), and 0.5 wt% of polyacrylate (San Nopco) as a dispersant were added to water as a dispersion medium, and then milled and dispersed for 120 minutes at 25°C using a bead mill to prepare a slurry for forming an organic-inorganic composite porous layer.
[0141] This was coated to a thickness of 2 μm on the cross section of a 9 μm thick polyethylene porous substrate (Toray), and then dried at 60° C. for 10 minutes.
[0142] Next, a separator for an electrochemical element was manufactured by irradiating the substrate with ultraviolet light at an irradiation dose of 3 J. At this time, the intensity of the ultraviolet light irradiation was 80% of that of the ultraviolet light source.
[0143] Example 2 [Preparation of non-crosslinked particle type acrylic binder polymer] 2-Ethylhexyl acrylate monomer (LG Chemical), butyl acrylate monomer, and 2-hydroxyethyl acrylate monomer were polymerized in a weight ratio of 75:10:15, and then the polymer and 5,000 ppm of 4-benzoylphenyl methacrylate (LG Chemical) were polymerized at 60°C to produce a non-crosslinked particle-type acrylic binder polymer (average particle size (d50): 1 μm).
[0144] [Production of separator for electrochemical element] A separator for an electrochemical device was manufactured in the same manner as in Example 1, except that the non-crosslinked particle-type acrylic binder polymer prepared above was used.
[0145] Comparative Example 1 [Preparation of non-crosslinked particle type acrylic binder polymer] 2-Ethylhexyl acrylate monomer (LG Chemical), butyl acrylate monomer, and 2-hydroxyethyl acrylate monomer were polymerized at 60°C in a weight ratio of 75:10:15 to produce a non-crosslinked particle-type acrylic binder polymer (average particle size (d50): 500 nm).
[0146] [Production of separator for electrochemical element] A separator for an electrochemical device was manufactured in the same manner as in Example 1, except that the non-crosslinked particle-type acrylic binder polymer prepared above was used.
[0147] Comparative Example 2 A separator for an electrochemical device was prepared in the same manner as in Example 1, except that ultraviolet irradiation was not performed.
[0148] Evaluation example 1: Evaluation of physical properties before and after crosslinking of particulate acrylic binder polymer The glass transition temperature (Tg), gel fraction before and after crosslinking, and storage modulus before and after crosslinking of the particulate acrylic binder polymers prepared in Examples 1 and 2 and Comparative Example 1 were measured and are shown in Table 1 below.
[0149] [Measurement of glass transition temperature after ultraviolet irradiation] The glass transition temperature of the particulate acrylic binder polymer after ultraviolet irradiation was measured using a DSC 250 (TA Corporation) at a heating rate of 10°C / min (-50°C to 250°C).
[0150] [Measurement of gel fraction before and after crosslinking] The non-crosslinked particle-type acrylic binder polymer before UV irradiation was immersed in a xylene solution at 135°C according to ASTM D 2765, boiled for 12 hours, and the remaining weight was measured, and the gel fraction was measured as a percentage of the remaining weight relative to the initial weight.
[0151] The crosslinked particulate acrylic binder polymer after UV irradiation was immersed in a xylene solution at 135°C according to ASTM D 2765, boiled for 12 hours, and the remaining weight was measured, and the gel fraction was measured as a percentage of the remaining weight to the initial weight.
[0152] [Measurement of storage modulus before and after crosslinking] The particulate acrylic binder polymer before UV irradiation was tested at a constant frequency of 1 Hz, a preload force of 0.01 N, an amplitude of 20 μm, and a force track of 120%, at a tensile force of 1°C / min from -100°C to 150°C to measure the storage modulus.
[0153] After UV irradiation, the particulate acrylic binder polymer was subjected to a tensile test at 1°C / min from -100°C to 150°C with a constant frequency of 1 Hz, a preload force of 0.01 N, an amplitude of 20 μm, and a force track of 120%, to measure the storage modulus.
[0154] [Table 1]
[0155] As can be seen from Table 1, the particulate acrylic binder polymers prepared in Examples 1 and 2 contained benzophenone functional groups, and thus it was confirmed that the storage modulus and gel fraction were increased after crosslinking compared to before crosslinking.
[0156] On the other hand, the particulate acrylic binder polymer prepared in Comparative Example 1 does not contain a benzophenone functional group, and therefore is not crosslinked even when irradiated with ultraviolet light. Therefore, it was confirmed that the increase in the storage modulus and gel fraction after ultraviolet light irradiation was negligible compared to before ultraviolet light irradiation.
[0157] Evaluation example 2: Evaluation of separator properties The thickness, air permeability, basis weight, packing density, peel strength between the porous polymer substrate and the organic-inorganic composite porous layer, heat shrinkage rate, and electrical resistance (ER) of the separators prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were measured and are shown in Table 2 below.
[0158] [Air permeability measurement] Air permeability (Gurley) was measured in accordance with ASTM D726-94. Gurley, as used herein, is the resistance to air flow and is measured by a Gurley densometer. Air permeability values reported herein are calculated by measuring the resistance of 100 cc of air at 12.2 inH2O pressure through 1 in of separator. 2 It is expressed as the time (in seconds) it takes for air to pass through a cross section of the material, i.e., the ventilation time.
[0159] [Basis weight measurement] Basis weight (g / m 2 ) was evaluated by preparing a sample of the separator with a width and length of 1m each and measuring its weight.
[0160] [Measurement of Packing Density] The packing density was calculated according to Equation 1 below: Packing density = loading amount / thickness of organic-inorganic composite porous layer
[0161] [Measurement of Peel Strength Between Porous Polymer Substrate and Organic-Inorganic Composite Porous Layer] The separator was fixed onto a glass plate using double-sided tape, and then tape (3M transparent tape) was firmly attached to the exposed organic-inorganic composite porous layer. The force required to peel off the tape was then measured using an 11oyd LS-1.
[0162] [Thermal shrinkage measurement] The separator was cut to a size of 50 mm (length) x 50 mm (width) to prepare a test specimen, which was then placed in an oven heated to 135°C for 30 minutes, after which the test specimen was removed and the change in length in the machine direction and the transverse direction was measured and calculated: Heat shrinkage rate at 135℃ (%) = {(dimension before shrinkage - dimension after shrinkage) / dimension before shrinkage} x 100
[0163] [Electrical resistance measurement] Coin cells were prepared using the separators prepared in Examples 1 and 2 and Comparative Examples 1 and 2, and the coin cells were left at room temperature for one day, after which the resistance of the separators was measured by an impedance measurement method. The coin cells were prepared as follows.
[0164] A negative electrode slurry was prepared by mixing artificial graphite as a negative electrode active material, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in a weight ratio of 75:5:20, and adding N-methylpyrrolidone (NMP) as a solvent.
[0165] The negative electrode slurry was charged to 3.8 mAh / cm 2 The mixture was coated on a copper current collector in a loading amount of 1000g and dried to prepare a negative electrode.
[0166] A positive electrode active material slurry was prepared by adding LiCoO2 as a positive electrode active material, denka black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder in a weight ratio of 85:5:10 to a solvent, N-methylpyrrolidone (NMP). The positive electrode active material slurry was coated on a sheet-shaped aluminum current collector and dried to obtain a final positive electrode loading of 3.3 mAh / cm. 2 The positive electrode active material layer was formed so as to have the following structure.
[0167] Between the negative electrode and the positive electrode prepared as described above, the separators of the Examples and Comparative Examples were interposed, and a non-aqueous electrolyte (1M LIPF6, ethylene carbonate (EC) / propylene carbonate (PC) / diethyl carbonate (DEC)) (volume ratio: 3:3:4) was injected to prepare a coin cell.
[0168] [Table 2]
[0169] As can be seen from Table 2, the separators prepared in Examples 1 and 2 were found to have excellent heat resistance while ensuring peel strength by including a particulate acrylic binder polymer having a structure crosslinked via a benzophenone functional group.
[0170] Specifically, it was confirmed that the separators prepared in Examples 1 and 2 had superior heat resistance compared to the separators prepared in Comparative Examples 1 and 2, which contained a particulate acrylic binder polymer that did not have a structure crosslinked via a benzophenone functional group.
Claims
1. A porous polymeric substrate; and an organic-inorganic composite porous layer located on at least one surface of the porous polymer substrate, the organic-inorganic composite porous layer including inorganic particles and a particulate acrylic binder polymer; The particulate acrylic binder polymer has a structure crosslinked via a benzophenone functional group.
2. 2. The separator for an electrochemical element according to claim 1, wherein the particulate acrylic binder polymer comprises an acrylic monomer having a benzophenone functional group.
3. 3. The separator for an electrochemical element according to claim 2, wherein the particulate acrylic binder polymer further comprises a branched or unbranched (meth)acrylic acid monomer having 1 to 20 carbon atoms, a branched or unbranched (meth)acrylate monomer having 1 to 20 carbon atoms, an acrylonitrile monomer, a vinylpyrrolidone monomer, a vinyl acetate monomer, or two or more of them.
4. 2. The separator for an electrochemical device according to claim 1, wherein the particulate acrylic binder polymer has a structure of the following formula 1: [Formula 1] In the above Chemical Formula 1, m, n, o, and p are each an integer of 1 or more.
5. 2. The separator for an electrochemical element according to claim 1, wherein the particulate acrylic binder polymer has a storage modulus of 20,000 Pa to 300,000 Pa at 50° C.
6. 2. The separator for an electrochemical element according to claim 1, wherein the particulate acrylic binder polymer has a glass transition temperature of -70°C to 70°C.
7. 2. The separator for an electrochemical element according to claim 1, wherein the particulate acrylic binder polymer has a gel fraction of 10% to 90%.
8. 2. The separator for an electrochemical element according to claim 1, wherein the particulate acrylic binder polymer has an average particle size of 0.001 μm to 10 μm.
9. The inorganic particles are BaTiO 3 , Pb(Zr,Ti)O 3 (PZT), Pb 1 - x La x Zr 1 - y Ti y O 3 (PLZT, where 0<x<1, 0<y<1), Pb(Mg 1/3 Nb 2/3 ) O 3 -PbTiO 3 (PMN-PT), hafnia (HfO 2 ), SrTiO 3 , SnO 2 , CeO 2 , MgO, Mg(OH) 2 , NiO, CaO, ZnO, Al(OH) 3 , ZrO 2 , Y 2 O 3 , Al 2 O 3 , AlOOH, SiC, TiO 2 , lithium phosphate (Li 3 P.O. 4 ), lithium titanium phosphate (Li x Ti y (P.O. 4 ) 3 , 0<x<2, 0<y<3), lithium aluminum titanium phosphate (Li x A y Ti z (P.O. 4 ) 3 , 0<x<2, 0<y<1, 0<z<3), (LiAlTiP) x O yLithium lanthanum titanate (Li x La y TiO 3 , 0<x<2, 0<y<3), lithium germanium thiophosphate (Li x Ge y P z S w , 0<x<4, 0<y<1, 0<z<1, 0<w<5), lithium nitride (Li x N y , 0<x<4, 0<y<2), SiS 2 Li-based glass x S y S z , 0<x<3, 0<y<2, 0<z<4), P 2 S 5 Li-based glass x P y S z 2. The separator for an electrochemical element according to claim 1, comprising:
10. 2. The separator for an electrochemical element according to claim 1, wherein the inorganic particles have an average particle size of 0.1 nm to 2.0 μm.
11. The separator for an electrochemical device according to claim 1 , wherein the organic-inorganic composite porous layer further comprises a non-particle type binder polymer.
12. 12. The separator for an electrochemical element according to claim 11, wherein the non-particle type binder polymer comprises carboxymethyl cellulose, polyacrylic acid, polyacrylamide, or two or more of them.
13. 2. The separator for an electrochemical element according to claim 1, wherein a weight ratio of the inorganic particles to the binder polymer is 99.9:0.1 to 70:30, and the binder polymer includes a particulate acrylic binder polymer.
14. 12. The separator for an electrochemical element according to claim 11, wherein a weight ratio of the particulate acrylic binder polymer to the non-particulate binder polymer is 5:95 to 95:
5.
15. 2. The separator for an electrochemical device according to claim 1, wherein the organic-inorganic composite porous layer has a thickness of 0.1 μm to 10 μm.
16. 2. The separator for an electrochemical element according to claim 1, wherein the separator for an electrochemical element has a thermal shrinkage rate of 10% or less in a machine direction (MD) and 10% or less in a transverse direction (TD) after being left at 135° C. for 30 minutes.
17. The separator for an electrochemical device has a peel strength between the porous polymer substrate and the organic / inorganic composite porous layer of 5 g. f / 15mm~1000g f 2. The separator for an electrochemical element according to claim 1, wherein the thickness of the separator is 15 mm.
18. A step of preparing a slurry for forming an organic-inorganic composite porous layer, the slurry including inorganic particles and a non-crosslinked particle-type acrylic binder polymer having a benzophenone functional group; Coating the organic / inorganic composite porous layer-forming slurry on at least one surface of a porous polymer substrate and drying the same; and A method for producing a separator for an electrochemical element, comprising the step of irradiating with ultraviolet light.
19. The non-crosslinked particle type acrylic binder polymer includes a first acrylic monomer and a second acrylic monomer, 20. The method for manufacturing a separator for an electrochemical element according to claim 18, wherein the first acrylic monomer comprises benzophenone methacrylate, 6-(4-benzoylphenoxy)hexyl methacrylate, benzophenone acrylate, or two or more thereof.
20. 20. The method for producing a separator for an electrochemical element according to claim 19, wherein the second acrylic monomer comprises branched or unbranched (meth)acrylic acid having 1 to 20 carbon atoms, branched or unbranched (meth)acrylate having 1 to 20 carbon atoms, acrylonitrile, vinylpyrrolidone, vinyl acetate, or two or more of them.
21. 20. The method for manufacturing a separator for an electrochemical element according to claim 18, wherein the non-crosslinked particle type acrylic binder polymer comprises a copolymer represented by the following Formula 2: [chemical 2] In the above Chemical Formula 2, m, n, o, and p are each an integer of 1 or more.
22. 20. The method for producing a separator for an electrochemical element according to claim 19, wherein the content of the first acrylic monomer is 500 to 20,000 ppm based on the weight of the second acrylic monomer.
23. 19. The method for producing a separator for an electrochemical element according to claim 18, wherein the non-crosslinked particulate acrylic binder polymer has a storage modulus of 10,000 Pa to 80,000 Pa at 50° C. before ultraviolet irradiation.
24. 19. The method for producing a separator for an electrochemical element according to claim 18, wherein the particulate acrylic binder polymer has a storage modulus at 50° C. change rate of 20% to 300% before and after ultraviolet irradiation.
25. The method for producing a separator for an electrochemical element according to claim 18, wherein the ultraviolet ray irradiation dose is 0.1 J to 10 J.
26. The method for producing a separator for an electrochemical element according to claim 18, wherein the ultraviolet light has a wavelength of 200 nm to 400 nm.
27. The method for producing a separator for an electrochemical element according to claim 26, wherein the ultraviolet light has a wavelength of 230 nm to 350 nm.
28. A battery comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, An electrochemical element, comprising the separator for electrochemical elements according to any one of claims 1 to 17.
Citation Information
Patent Citations
Separator comprising CMC, particulate binder, and soluble binder
EP3614458A1
Method for crosslinking radiation crosslinkable pressure-sensitive contact film
JP1999189664A
Composite materials and electrochemical batteries
JP2002529891A
Electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery, and method of manufacturing electrode for nonaqueous electrolyte secondary battery
JP2013069495A
UV-curable acrylic polymer, production method of the same and UV-curable hot-melt adhesive
JP2019031643A