Separator for electrochemical device, method for manufacturing same, and electrochemical device comprising same
By forming a porous coating on the lithium secondary battery separator and coating it with a dopamine coating of polydopamine and dextrin, the problem of insufficient dimensional stability of the separator under high temperature and humidity was solved, and the dimensional stability under high temperature and humidity was improved with low polymer binder content.
Patent Information
- Application Number
- CN202480002145.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-30
- Filing Date
- 2024-01-31
- Publication Date
- 2024-11-12
AI Technical Summary
Existing lithium-ion battery separators suffer from insufficient dimensional stability under high temperature and humid conditions due to reduced adhesion strength of polymer adhesives. This is especially true for cylindrical batteries where higher adhesion strength is required, but current technologies struggle to meet these requirements simultaneously.
A porous coating is formed on a porous polymer substrate, and a dopamine coating containing polydopamine and dextrin is coated on it. By cross-linking the polymer adhesive with polydopamine, the content of the polymer adhesive is reduced to less than 5% by weight, thereby improving the dimensional stability of the diaphragm under high temperature and humid conditions.
Under conditions above 130℃, the thermal shrinkage rate of the separator is reduced to below 5%, ensuring electrode stability, preventing electrode exposure caused by thermal shrinkage, and improving the high-temperature and wet-state performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0027540 filed in the Korean Intellectual Property Office on March 2, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a separator for an electrochemical device, a method of manufacturing the same, and an electrochemical device including the same. Background Art
[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions, and recently, lithium secondary batteries, which have high energy density and voltage and long cycle life and are applicable to various fields, have been widely used.
[0004] The lithium secondary battery may include an electrode assembly prepared with a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, and may be manufactured by storing the electrode assembly in a shell together with an electrolyte. The separator may include a porous coating comprising a polymer binder and inorganic particles on at least one surface of a porous substrate. One of the inorganic particles may be connected to another of the inorganic particles by a polymer binder to form an interstitial volume, and lithium ions may migrate through the interstitial volume. In addition to fixing the inorganic particles, the polymer binder may also provide adhesion strength for the porous coating, and the porous coating may adhere to each of the porous substrate and the electrode.
[0005] A porous coating layer comprising a polymer binder and inorganic particles can prevent thermal shrinkage of a porous polymer substrate, and a separator comprising a porous coating layer shows excellent dimensional stability in a dry state without an electrolyte. However, in a wet state where the separator is impregnated with an electrolyte, the polymer binder is swollen by the electrolyte, or the separator is exposed to a temperature of about 130°C or more as the lithium secondary battery comprising the separator is operated, and the adhesion strength of the polymer binder may decrease. In this high-temperature wet state, the separator shrinks significantly as the adhesion strength of the porous coating layer decreases. In particular, compared to pouch-type batteries, cylindrical batteries in which the electrode assembly is wound and inserted into the shell in a state with tension applied to the electrode assembly require relatively small adhesion strength between the electrode and the separator, thereby having a problem of further reduced dimensional stability in a wet state due to the low content of the polymer binder in the porous coating layer.
[0006] Therefore, research has been conducted on separators for maintaining a relatively low polymer binder content in a porous coating while ensuring dimensional stability under high temperature and wet conditions. Summary of the invention
[0007] Technical issues
[0008] The present disclosure aims to provide a separator for an electrochemical device having reduced dimensional change in a high-temperature wet state; a method for manufacturing the same; and an electrochemical device including the separator for an electrochemical device.
[0009] Technical Solution
[0010] One aspect of the present disclosure provides a separator for an electrochemical device, the separator comprising: a porous polymer substrate; a porous coating layer formed on at least one surface of the porous polymer substrate and comprising a polymer binder and inorganic particles; and a dopamine coating layer formed on the porous coating layer and comprising polydopamine and dextrin.
[0011] In the porous coating layer, the polymer binder may be included in an amount of 5 wt % or less based on the total weight of the porous coating layer.
[0012] The separator may include polydopamine and dextrin in a weight ratio of 1:500 to 1:1000.
[0013] The polymer binder may include an acrylic binder, and at least a portion of the acrylic binder may be cross-linked with the polydopamine.
[0014] The polymer binder may include one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber and acrylonitrile-butadiene-styrene rubber.
[0015] The porous coating layer may have a thickness greater than a thickness of the dopamine coating layer.
[0016] Another aspect of the present disclosure provides an electrochemical device, comprising: a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device according to the one aspect.
[0017] The electrochemical device may be a lithium secondary battery.
[0018] The electrochemical device may further include an electrolyte solution comprising EC / EMC in a weight ratio of 3 / 7.
[0019] Another aspect of the present disclosure provides a method for manufacturing a diaphragm for an electrochemical device, the method comprising: immersing a preliminary diaphragm in a solution comprising dopamine and dextrin for 1 hour to 50 hours, the preliminary diaphragm comprising a porous polymer substrate and a porous coating, the porous coating comprising a polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate; and forming a dopamine coating comprising polydopamine and the dextrin on at least one surface of the porous coating by controlling the amount of dissolved oxygen in the solution.
[0020] In the method of manufacturing a separator, the polymer binder may include an acrylic binder, and the method may further include thermally cross-linking the polymer binder and the polydopamine by exposing the separator to 60° C. to 90° C.
[0021] Beneficial Effects
[0022] The separator for an electrochemical device according to the present disclosure can provide improved dimensional stability in a wet state impregnated with an electrolyte. Specifically, the separator exhibits a thermal shrinkage of 5% or less in the TD direction under high temperature conditions of 130° C. or more, thereby preventing electrode exposure caused by thermal shrinkage of the separator. DETAILED DESCRIPTION
[0023] Hereinafter, each constitution of the present disclosure will be described in more detail so that those skilled in the art can easily implement the present disclosure, however, this is only an example, and the right scope of the present disclosure is not limited by the following description.
[0024] The term "comprising" used in this specification is used to list materials, compositions, devices and methods useful for the present disclosure and is not limited to the listed examples.
[0025] The terms “about” and “substantially” used in this specification are used to indicate a range of values or degrees or a meaning close thereto taking into account inherent manufacturing and material tolerances, and are used to prevent an infringer from taking unfair advantage of the present disclosure in which exact or absolute numbers are stated to aid understanding of the present disclosure.
[0026] The "electrochemical device" used in this specification may mean a primary battery, a secondary battery, a supercapacitor, or the like.
[0027] The “wet state” used in the present specification may refer to a state in which the separator is impregnated with at least a portion of the electrolyte.
[0028] One embodiment of the present disclosure provides a separator for an electrochemical device, the separator comprising: a porous polymer substrate; a porous coating layer formed on at least one surface of the porous polymer substrate and comprising a polymer binder and inorganic particles; and a dopamine coating layer formed on the porous coating layer and comprising polydopamine and dextrin.
[0029] The porous polymer substrate is a porous film formed with a plurality of pores, and can prevent short circuits by electrically insulating the positive electrode and the negative electrode. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate can be an ion-conducting barrier that allows lithium ions to pass while blocking electrical contact between the positive electrode and the negative electrode. At least some of the pores can form a three-dimensional network connecting the surface and the interior of the porous polymer substrate, and the fluid can pass through the porous polymer substrate through the pores.
[0030] As a porous polymer substrate, a material that is physically and chemically stable to an electrolyte (organic solvent) can be used. Examples of porous polymer substrates can include resins, such as polyolefins, such as polyethylene, polypropylene and polybutylene, polyvinyl chloride, polyethylene terephthalate, polycycloolefins, polyethersulfones, polyamides, polyimides, polyimide amides, nylons, polytetrafluoroethylene and copolymers or mixtures thereof, but are not limited thereto. Preferably, polyolefin-based resins can be used. Polyolefin-based resins can be processed to be relatively thin, and coating slurries can be easily coated thereon, and are therefore suitable for manufacturing electrochemical devices with higher energy density.
[0031] The porous polymer substrate may have a monolayer or multilayer structure. The porous polymer substrate may include two or more polymer resin layers with different melting points (Tm), and may provide a closed-cell function during a runaway of the battery at high temperatures. For example, the porous polymer substrate may include a polypropylene layer with a relatively high melting point and a polyethylene layer with a relatively low melting point. Preferably, the porous polymer substrate may have a three-layer structure in which polypropylene, polyethylene and polypropylene are laminated in sequence. When the polyethylene layer melts as the battery temperature rises to above a predetermined temperature, the pores are closed and thermal runaway of the battery can be prevented.
[0032] The porous polymer substrate may have a thickness of 1 μm or more and 100 μm or less. Specifically, the porous polymer substrate may have a thickness of 10 μm or more and 90 μm or less, 20 μm or more and 80 μm or less, 30 μm or more and 70 μm or less, or 40 μm or more and 60 μm or less. Preferably, the polymer substrate may have a thickness of 1 μm or more and 30 μm or less. More preferably, the polymer substrate may have a thickness of 5 μm or more and 15 μm or more and 13 μm or less. By adjusting the thickness of the porous polymer substrate within the above range, the volume of the electrochemical device can be minimized while electrically insulating the positive and negative electrodes, thereby increasing the amount of active material contained in the electrochemical device.
[0033] The porous polymer substrate may include pores having an average diameter of 0.01 μm or more and 1 μm or less. Specifically, the size of the pores contained in the porous polymer substrate may be 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Preferably, the size of the pores may be 0.02 μm or more and 0.06 μm or less. By adjusting the size of the pores of the porous polymer substrate within the above range, the air permeability and ion conductivity of the manufactured diaphragm as a whole may be controlled.
[0034] The porous polymer substrate may have an air permeability of more than 10 seconds / 100 cc and less than 100 seconds / 100 cc. Specifically, the porous polymer substrate may have an air permeability of more than 10 seconds / 100 cc and less than 90 seconds / 100 cc, more than 20 seconds / 100 cc and less than 80 seconds / 100 cc, more than 30 seconds / 100 cc and less than 70 seconds / 100 cc, or more than 40 seconds / 100 cc and less than 60 seconds / 100 cc. Preferably, the porous polymer substrate may have an air permeability of more than 50 seconds / 100 cc and less than 70 seconds / 100 cc. When the porous polymer substrate has an air permeability within the above range, the air permeability of the manufactured separator can be provided within a range suitable for ensuring the output and cycle characteristics of the electrochemical device.
[0035] Air permeability (seconds / 100 cc) refers to the time (seconds) it takes for 100 cc of air to pass through a porous polymer substrate or membrane with a predetermined area at a constant pressure. Air permeability can be measured using an air permeability tester (Gurley air permeability tester) according to ASTM D726-58, ASTM D726-94, or JIS-P8117. For example, a 4110N air permeability tester from Gurley can be used to measure air permeability at an air pressure of 0.304 kPa or 1.215 kN / m 2100 cc of air passes through 1 square inch (or 6.54 cm 2 ) sample. For example, the time it takes for 100 cc of air to pass through a 1 square inch sample at a constant pressure of 4.8 inches of water at room temperature can be measured using an Asahi Seiko EG01-55-1MR tester.
[0036] The porous polymer substrate may have a porosity of 10% by volume or more and 60% by volume or less. Specifically, the porous polymer substrate may have a porosity of 15% by volume or more and 55% by volume or less, 20% by volume or more and 50% by volume or less, 25% by volume or more and 45% by volume or less, or 30% by volume or more and 40% by volume or less. Preferably, the porous polymer substrate may have a porosity of 30% by volume or more and 50% by volume or less. When the porous polymer substrate has a porosity within the above range, the ionic conductivity of the manufactured diaphragm may be provided within a range suitable for ensuring the output and cycle characteristics of the electrochemical device.
[0037] Porosity refers to the ratio of the volume of pores to the total volume of the porous polymer substrate. Porosity can be measured using methods known in the art. For example, porosity can be measured using the BET (Brunol-Emmett-Teller) measurement method using nitrogen adsorption, capillary flow porosimetry, or water or mercury permeametry.
[0038] The porous coating layer is formed on at least one surface of the porous polymer substrate and may include a polymer binder and inorganic particles. The dopamine coating layer is formed on the porous coating layer and may include polydopamine and dextrin.
[0039] The diaphragm can be formed by coating at least one surface of a porous polymer substrate with a coating slurry comprising a polymer binder, inorganic particles and a dispersion medium and a solution comprising dopamine and dextrin in sequence. For example, a preliminary diaphragm having a porous coating can be prepared by coating a coating slurry on at least one surface of a porous polymer substrate and drying the resultant, and the preliminary diaphragm is immersed in a solution and dried to form a dopamine coating, thereby manufacturing a diaphragm. The porous coating includes a gap volume obtained by connecting inorganic particles through a polymer binder, and adheres to the porous polymer substrate to prevent thermal shrinkage of the porous polymer substrate while allowing lithium ions to pass. The polydopamine contained in the dopamine coating can be formed by polymerizing the dopamine contained in the solution. The dopamine coating also has a porous structure formed by polydopamine and dextrin, and can allow lithium ions to pass.
[0040] The coating slurry comprises a dispersion medium, so as to dissolve or disperse at least a portion of the polymer binder, and inorganic particles can be dispersed. As a coating slurry, those having a polymer binder and inorganic particles uniformly dispersed by controlling the type and content of the dispersion medium can be used. For example, the dispersion medium can be one selected from the group consisting of water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile and a combination thereof. Preferably, the dispersion medium can be a mixture or water of water and isopropyl alcohol. Using the dispersion medium of the above type, a porous coating uniformly dispersed with polymer binders and inorganic particles can be formed.
[0041] By further comprising additives such as dispersants, surfactants, defoamers and flame retardants, the coating slurry can improve dispersibility and flame retardancy, and improve the uniformity of the porous coating formed. For example, the dispersant may include one or more selected from the group consisting of polyacrylic acid, oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid and pyrogallic acid. The use of the above-mentioned type of dispersant can improve the stability of the coating slurry, and can ensure the uniformity of the porous coating formed by the coating slurry.
[0042] Based on the total weight of the coating slurry, the content of the additive may be 0% by weight or more and 5% by weight or less. Specifically, the content of the additive may be 0.01% by weight or more and 4% by weight or less, 0.1% by weight or more and 3% by weight or less, or 1% by weight or more and 2% by weight or less. Preferably, the content of the additive may be 1% by weight or more and 5% by weight or less. By adjusting the content of the additive within the above range, uniform dispersion and stability of the inorganic particles contained in the coating slurry may be achieved.
[0043] The dispersion medium contained in the coating slurry can be removed by drying or heating after forming the porous coating. For example, the porous coating can contain a dispersion medium in an amount of less than 5ppm. Preferably, the porous coating can be formed by a polymer binder and inorganic particles. During the process of removing the dispersion medium, a plurality of holes can be formed on the surface or inside of the porous coating. The hole can include the interstitial volume formed between the inorganic particles, and can have a structure that allows fluid to pass through by forming a three-dimensional network.
[0044] The solution may be an alkaline buffer solution in which dopamine and dextrin are mixed. Dopamine may undergo a cyclization reaction through an oxidation process without an initiator and then form polydopamine through a polymerization reaction.
[0045] The solution may have a pH of 7 or more and 12 or less. Specifically, the solution may have a pH of 7.5 or more and 11.5 or less, 8 or more and 11 or less, 8.5 or more and 10.5 or less, or 9 or more and 10 or less. Preferably, the solution may have a pH of 7.5 or more and 8.5 or less. By adjusting the pH of the solution within the above range, the loading amount of polydopamine required for the dopamine coating and the uniform distribution of polydopamine can be achieved.
[0046] The sum of the thickness of the porous coating layer and the thickness of the dopamine coating layer may be 1 μm or more and 15 μm or less. Specifically, the sum of the thickness of the porous coating layer and the thickness of the dopamine coating layer may be 2 μm or more and 14 μm or less, 3 μm or more and 13 μm or less, 4 μm or more and 12 μm or less, 5 μm or more and 11 μm or less, 6 μm or more and 10 μm or less, or 7 μm or more and 9 μm or less. Preferably, the sum of the thickness of the porous coating layer and the thickness of the dopamine coating layer may be 1 μm or more and 5 μm or less. By adjusting the thickness of the porous coating layer and the dopamine coating layer within the above range, the shrinkage of the porous polymer substrate is minimized, and stable adhesion to the porous polymer substrate may be obtained.
[0047] The thickness of the porous coating layer may be greater than the thickness of the dopamine coating layer. For example, the thickness of the porous coating layer may be greater than 0.1 μm and less than 14 μm. Specifically, the thickness of the porous coating layer may be greater than 1 μm and less than 13 μm, greater than 2 μm and less than 12 μm, greater than 3 μm and less than 11 μm, greater than 4 μm and less than 10 μm, greater than 5 μm and less than 9 μm, or greater than 6 μm and less than 8 μm. Preferably, the thickness of the porous coating layer may be greater than 0.1 μm and less than 5 μm. The thickness of the dopamine coating layer may be greater than 0.001 μm and less than 5 μm. Specifically, the thickness of the dopamine coating layer may be greater than 0.01 μm and less than 4 μm, greater than 0.1 μm and less than 3 μm, or greater than 1 μm and less than 2 μm. Preferably, the thickness of the dopamine coating layer may be greater than 0.005 μm and less than 1 μm. By adjusting the thickness of the porous coating layer and the dopamine coating layer within the above range, the shrinkage of the porous polymer substrate is minimized and stable adhesion to the porous polymer substrate can be obtained. When the thickness of the dopamine coating layer is greater than the thickness of the porous coating layer, the porous coating layer and the porous polymer substrate are peeled off.
[0048] The porous coating layer may include a polymer binder and inorganic particles. The polymer binder may bind the inorganic particles contained in the porous coating layer and may provide adhesion strength for the porous coating layer. The polymer binder may have a spherical or elliptical shape, but may also include other shapes besides an amorphous shape.
[0049] The polymer binder may be an acrylic binder. For example, the polymer binder may include one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.
[0050] When the polymer binder is an acrylic binder, at least a portion of the acrylic binder may be cross-linked with polydopamine contained in the dopamine coating. The acrylic binder may be cross-linked with polydopamine contained in the dopamine coating by a condensation reaction. Compared with a fluorine-based binder, the acrylic binder may be cross-linked with polydopamine to form and maintain a bond between the porous coating and the dopamine coating, and as a result, the thermal shrinkage of the separator may be reduced even when the separator is in a wet state.
[0051] In the porous coating, the content of the polymer binder may be 5% by weight or less based on the total weight of the porous coating. Specifically, based on the total weight of the porous coating, the content of the polymer binder may be 0.1% by weight or more and 5% by weight or less, 0.5% by weight or more and 4.5% by weight or less, 1% by weight or more and 4% by weight or less, 1.5% by weight or more and 3.5% by weight or less, or 2% by weight or more and 3% by weight or less. Preferably, the content of the polymer binder may be 3% by weight or more and 5% by weight or less. By adjusting the content of the polymer binder within the above range, the wet heat shrinkage of the diaphragm may be improved by the combination of the inorganic particles, the stable adhesion to the porous polymer substrate, and the crosslinking with the polydopamine contained in the dopamine coating.
[0052] The polymer binder may have a weight average molecular weight (Mw) of 1,000 or more and 10,000,000 or less. Specifically, the weight average molecular weight of the polymer binder may be 1,000 or more and 10,000,000 or less, 10,000 or more and 9,000,000 or less, 100,000 or more and 8,000,000 or less, 200,000 or more and 7,000,000 or less, 300,000 or more and 6,000,000 or less, 500,000 or more and 5,000,000 or less, 1,000,000 or more and 4,000,000 or less, or 2,000,000 or more and 3,000,000 or less. By adjusting the weight average molecular weight of the polymer binder within the above range, the mechanical properties of the porous coating are ensured, and a diaphragm provided with a durable porous coating can be manufactured.
[0053] The weight average molecular weight can be measured by gel permeation chromatography (GPC, PL GPC220, Agilent Technologies Inc.). For example, the weight average molecular weight can be measured using a PL Olexis (Polymer Laboratories, Inc.) column (column temperature 160° C.), TCB (trichlorobenzene) as a solvent, and an Agilent high temperature RI detector under the conditions of a sample concentration of 1.0 mg / mL, a flow rate of 1.0 mL / min, and an injection volume of 200 μl (standard: polystyrene).
[0054] The porous coating layer may include a polymer binder and inorganic particles in a weight ratio of 5:80 to 5:95. Specifically, the polymer binder and inorganic particles in the porous coating layer may have a weight ratio of 5:80 to 5:95 or 5:85 to 5:90. By adjusting the composition of the porous coating layer within the above range, the formation of the gap volume caused by the bonding between the inorganic particles and the adhesion strength of the porous coating layer to the separator can be ensured at the same time.
[0055] As the inorganic particles, those that are electrochemically stable can be used. The inorganic particles are not particularly limited as long as they are within the operating voltage range of the electrochemical device (for example, based on Li / Li + In particular, the use of inorganic particles with a high dielectric constant as inorganic particles helps to increase the dissociation degree of the electrolyte salt (e.g., lithium salt) in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the above reasons, the inorganic particles preferably include high dielectric constant inorganic particles with a dielectric constant of 5 or more, preferably 10 or more. Non-limiting examples of inorganic particles with a dielectric constant of 5 or more may include BaTiO 3 、Pb(Zr,Ti)O 3 (PZT), Pb 1-x La x Zr 1-y Ti y O 3 (PLZT, 0 <x<1,0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3 ) 3 -PbTiO 3 (PMN-PT), hafnium dioxide (HfO 2 )、SrTiO 3 SnO 2 、CeO 2 , MgO, NiO, CaO, ZnO, ZrO 2 、SiO 2 , Y 2 O 3 、Al 2 O 3 、Al(OH)3 , SiC, AlOOH, TiO 2 , and their mixtures, etc.
[0056] In addition, as the inorganic particles, inorganic particles having lithium ion transfer ability can be used, that is, inorganic particles containing lithium element but having the function of transporting lithium ions instead of storing lithium. Non-limiting examples of inorganic particles having lithium ion transfer ability may include lithium phosphate (Li 3 PO 4 ), lithium titanium phosphate (Li x Ti y (PO 4 ) 3 , 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO 4 ) 3 , 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y series glasses (0 < x < 4, 0 < y < 13) such as 14Li 2 O - 9Al 2 O 3 - 38TiO 2 - 39P 2 O 5 , lithium lanthanum titanate (Li x La y TiO 3 , 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5) such as Li 3.25 Ge 0.25 P 0.75 S 4 , lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2) such as Li 3 N, SiS 2 series glasses (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) such as Li 3 PO 4 - Li 2 S - SiS 2 , P 2 S 5Series of glasses (Li x P y S z , where 0 < x < 3, 0 < y < 3, 0 < z < 7), such as LiI-Li 2 S-P 2 S 5 and their mixtures, etc.
[0057] In addition, as the inorganic particles, those particles that can impart flame retardant properties to the separator as inorganic particles with flame retardancy or prevent a rapid increase in temperature inside the electrochemical device can be used. Non-limiting examples of inorganic particles with flame retardancy may include Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , SrTiO 3 , SnO 2 , CeO 2 , MgO, Mg(OH) 2 , NiO, CaO, ZnO, Zn 2 SnO 4 , ZnSnO 3 , ZnSn(OH) 6 , ZrO 2 , Y 2 O 3 , SiO 2 , Al 2 O 3 , AlOOH, Al(OH) 3 , SiC, TiO 2 , H 3 BO 3 , HBO 2 and their mixtures, etc.
[0058] The inorganic particles may have an average particle size (D50) of 50 nm or more and 5,000 nm or less. Specifically, the inorganic particles may have an average particle size (D50) of 100 nm or more and 4,500 nm or less, 200 nm or more and 4,000 nm or less, 300 nm or more and 3,000 nm or less, 400 nm or more and 2,000 nm or less, or 500 nm or more and 1,000 nm or less. When the inorganic particles have an average particle size of less than 50 nm, as the specific surface area increases, an additional polymer binder for binding the inorganic particles is required, which is disadvantageous in terms of resistance. Inorganic particles with an average particle size greater than 5,000 nm may reduce the uniformity of the coating surface and cause damage to the porous polymer substrate or the electrode during lamination.
[0059] The inorganic particles may have an aspect ratio of 1 or more and 2 or less. Specifically, the inorganic particles may have an aspect ratio of 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. By adjusting the aspect ratio of the inorganic particles within the above range, the polymer binder can easily move through the pores between the inorganic particles, and by forming a membrane region after the polymer binder moves, a porous coating layer in which the membrane region is uniformly distributed can be formed.
[0060] The inorganic particles may have a size of 5 m 2 / g or more and 25m 2 / g or less. Specifically, the inorganic particles may have a BET specific surface area of 6m 2 / g or more and 24m 2 / g or less, 7m 2 / g or more and 23m 2 / g or less, 8m 2 / g or more and 22m 2 / g or less, 9m 2 / g or more and 21m 2 / g or less, 10m 2 / g or more and 20m 2 / g or less, 11m 2 / g or more and 19m 2 / g or less, 12m 2 / g or more and 18m 2 / g or less, 13m 2 / g or more and 17m 2 / g or less or 14m 2 / g or more and 26m 2 By adjusting the BET specific surface area of the inorganic particles within the above range, the migration of the polymer binder through the pores between the inorganic particles can be controlled.
[0061] The polydopamine can act as an agent for preventing thermal shrinkage of the dopamine coating and the porous coating, while providing adhesion strength to the dopamine coating by providing inherent adhesion strength. At least a portion of the polydopamine forms crosslinks with the above-mentioned polymer binder through an amine group to prevent the inorganic particles contained in the porous coating from detaching, and by maintaining the bonding between the porous coating and the dopamine coating, the thermal shrinkage of the porous polymer substrate can be reduced even in a wet state.
[0062] The polydopamine may have a decomposition temperature (T d). Specifically, polydopamine may have a decomposition temperature of 290° C. or more and 310° C. or less. The decomposition temperature of polydopamine may be analyzed by a thermogravimetric analysis (TGA) method. When the decomposition temperature of the polydopamine satisfies the above numerical range, the dimensional stability of the separator in a wet state under high temperature conditions is improved, while preventing the detachment of the inorganic particles contained in the porous coating layer, thereby preventing the thermal shrinkage of the separator without hindering the transfer of lithium ions.
[0063] The molecular weight of the polydopamine may be 10,000 to 1,000,000. Specifically, the polydopamine may have a molecular weight of 100,000 to 900,000, 200,000 to 800,000, 300,000 to 700,000 or 400,000 to 600,000. Preferably, the polydopamine may have a molecular weight of 20,000 to 500,000. When the molecular weight of polydopamine satisfies the above numerical range, the thermal shrinkage of the diaphragm may be reduced in a high temperature wet state.
[0064] The polydopamine contained in the dopamine coating may have a 2 Above and 0.01g / m 2 Specifically, the polydopamine may have a loading of 0.0005 g / m 2 Above and 0.009g / m 2 Below, 0.001g / m 2 Above and 0.008g / m 2 Below, 0.002g / m 2 Above and 0.007g / m 2 Below, 0.003g / m 2 Above and 0.006g / m 2 Below or 0.004g / m 2 Above and 0.005g / m 2 Preferably, the polydopamine may have a loading of 0.0005 g / m 2 Above and 0.002g / m 2 By adjusting the loading amount of polydopamine within the above range, the heat shrinkage rate of the separator in a wet state under high temperature conditions can be reduced.
[0065] In the manufacturing process of the separator, while the preliminary separator is immersed in the dopamine solution, polydopamine may also be included in the porous coating. The loading amount of polydopamine included in the dopamine coating may be greater than the loading amount of polydopamine included in the porous coating. For example, the polydopamine included in the dopamine coating may have a loading amount of 0.0005 g / m 2 Above and 0.01g / m 2Specifically, the polydopamine contained in the dopamine coating may have a loading of 0.001 g / m 2 Above and 0.009g / m 2 Below, 0.002g / m 2 Above and 0.008g / m 2 Below, 0.003g / m 2 Above and 0.007g / m 2 Below or 0.004g / m 2 Above and 0.006g / m 2 The polydopamine contained in the porous coating layer may have a loading of 0.0001 g / m 2 Above and 0.005g / m 2 Specifically, the polydopamine contained in the porous coating layer may have a loading of 0.0001 g / m 2 Above and 0.004g / m 2 Below or 0.001g / m 2 Above and 0.003g / m 2 By adjusting the loading amount of the polydopamine contained in the porous coating layer and the dopamine coating layer within the above range, the amount of the polydopamine exposed to the outermost layer of the separator can be controlled, and as a result, the wet heat shrinkage rate of the separator can be reduced even under high temperature conditions.
[0066] The dextrin provides durability to the dopamine coating, thereby improving the dimensional stability of the diaphragm comprising the dopamine coating. The dopamine coating comprising dextrin can maintain dimensional stability even when subjected to external forces generated when an electrode attached to or disposed adjacent to the diaphragm shrinks or expands. The dextrin improves the dispersibility of polydopamine to form a dopamine coating in which polydopamine is uniformly dispersed. For example, even when dopamine has not yet been completely dissolved in a solution comprising dopamine, dextrin can keep dopamine in a uniformly dispersed state. The dextrin can be a cyclodextrin, for example, one or more selected from the group consisting of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.
[0067] The separator may contain polydopamine and dextrin in a weight ratio of 1:500 to 1:1000. Specifically, the separator may contain polydopamine and dextrin in a weight ratio of 1:600 to 1:900 or 1:700 to 1:800. By adjusting the content of polydopamine and dextrin within the above range, the effect of reducing the wet heat shrinkage rate of the separator at high temperature by polydopamine can be achieved through uniform dispersion of polydopamine contained in the dopamine coating.
[0068] Specifically, it can be said that when impregnated with an electrolyte at a high temperature of 135°C or more, the separator of the present disclosure is in a high temperature wet state. When the separator is exposed to a high temperature wet state for more than 30 minutes, when the heat shrinkage in the MD direction is less than 10% and the heat shrinkage in the TD direction is less than 7%, it can be evaluated as a decrease in heat shrinkage. In addition, after the separator is fixed on a slide glass, etc., when the surface is peeled off at 300 mm / min in a direction of 180° relative to the adhesion direction using UTM, the adhesion strength between the porous polymer substrate and the porous coating in the separator can be evaluated by peeling strength. When the peel strength is 50gf / 15mm or more, the porous coating and the dopamine coating can be evaluated as stably adhering to the porous polymer substrate. When polydopamine is included in an amount greater than the above range, polydopamine aggregates during the dopamine coating formation process, and the effect of reducing the heat shrinkage of the separator at high temperature may not be ensured, and the stability of the separator may be reduced. When dextrin is included in an amount greater than the above range, the peel strength between the separator substrate and the porous coating may increase due to the inherent adhesion strength of dextrin, however, the effect of reducing the thermal shrinkage of the separator at high temperatures may not be ensured. The separator for electrochemical device may have an air permeability of 20 seconds / 100 cc or more and 90 seconds / 100 cc or less. Specifically, the separator may have an air permeability of 25 seconds / 100 cc or more and 85 seconds / 100 cc or less, 30 seconds / 100 cc or more and 80 seconds / 100 cc or less, 35 seconds / 100 cc or more and 75 seconds / 100 cc or less, 40 seconds / 100 cc or more and 70 seconds / 100 cc or less, 45 seconds / 100 cc or more and 65 seconds / 100 cc or less, or 50 seconds / 100 cc or more and 55 seconds / 100 cc or less. Preferably, the separator may have an air permeability of 80 sec / 100 cc or more and 90 sec / 100 cc or less. When the separator has an air permeability within the above range, output, stability, and cycle characteristics of the electrochemical device may be ensured.
[0069] When a cell is manufactured using the separator for an electrochemical device, the cell may have a resistance of 0.5 ohms to 1.5 ohms. Specifically, the cell may have a resistance of 0.6 ohms to 1.4 ohms, 0.7 ohms to 1.3 ohms, 0.8 ohms to 1.2 ohms, or 0.9 ohms to 1.1 ohms. Preferably, the cell may have a resistance of 0.6 ohms to 0.8 ohms.
[0070] Another embodiment of the present disclosure provides a method for manufacturing a separator for an electrochemical device, the method comprising: immersing a preliminary separator in a solution comprising dopamine and dextrin for 1 to 50 hours, the preliminary separator comprising a porous polymer substrate and a porous coating, the porous coating comprising a polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate; and forming a dopamine coating comprising polydopamine and the dextrin on at least one surface of the porous coating by controlling the amount of dissolved oxygen in the solution. Contents repeated with those described in the separator for an electrochemical device are replaced with the description of the embodiment provided above.
[0071] The preparatory diaphragm is immersed in the solution and can also include preparing the preparatory diaphragm by coating at least one surface of the porous polymer substrate with a coating slurry comprising a polymer binder and inorganic particles. The preparatory diaphragm is formed with a porous coating on at least one surface of the porous polymer substrate, and the porous coating comprises a polymer binder and inorganic particles. For example, the coating can be formed using a method such as a rod coater, a wire rod coater, a roller coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a blade coater, a slot die coater, a hot melt coater, a comma coater and a direct metering coater, but the method is not limited thereto. Preferably, the formation of the porous coating can use a rod coater or a slot die coater to coat the coating slurry on both surfaces of the porous polymer substrate simultaneously.
[0072] The preparation of the preliminary separator may also include corona discharge on at least one surface of the porous polymer substrate. After the corona discharge, the coating slurry may be applied to the porous polymer substrate. The corona discharge on at least one surface of the porous polymer substrate prevents the adhesion strength between the surface of the porous polymer substrate and the surface of the porous coating from decreasing at high temperatures, and may prevent the adhesion strength between the surface of the polymer substrate and the surface of the porous coating from decreasing due to the electrolyte.
[0073] Corona discharge treatment can be at least one surface of a porous polymer substrate treated with a voltage of more than 0.1 kV and less than 10 kV in air. Specifically, corona discharge treatment can be treated with a voltage of more than 0.2 kV and less than 9 kV, more than 0.3 kV and less than 8 kV, more than 0.4 kV and less than 7 kV, more than 0.5 kV and less than 6 kV, more than 0.6 kV and less than 5 kV, more than 0.7 kV and less than 4 kV, more than 0.8 kV and less than 3 kV, more than 0.9 kV and less than 2 kV or more than 1.0 kV and less than 2 kV in air. Preferably, corona discharge treatment can be treated with a voltage of 1.8 kV in air. By adjusting the applied voltage of corona discharge treatment within the above range, an appropriate number of functional groups are formed on the surface of the polymer substrate, and damage to the surface of the polymer substrate can be prevented.
[0074] The preparation of the preliminary separator may further include removing the dispersion medium contained in the coating slurry. Specifically, the removal of the dispersion medium is performed by drying or heating the porous polymer substrate coated with the coating slurry to evaporate the dispersion medium contained in the coating.
[0075] The impregnation of the preparatory diaphragm is to immerse the preparatory diaphragm in a solution comprising dopamine and dextrin for 1 hour to 50 hours to apply a dopamine coating comprising polydopamine and dextrin. Specifically, the preparatory diaphragm can be immersed for 4 hours to 48 hours, 8 hours to 44 hours or 12 hours to 40 hours. Preferably, the immersion time can be 40 hours to 48 hours. Within the above time range, the loading amount of polydopamine contained in the dopamine coating can be adjusted within the above range.
[0076] The formation of the dopamine coating can be achieved by controlling the amount of dissolved oxygen in the solution while immersing the preliminary membrane in the solution. In order to form a dopamine coating containing polydopamine from a solution containing dopamine, dopamine can be oxidized to form cyclic dopamine and then polymerized. The degree of dopamine oxidation can be controlled by exposing the solution to oxygen, for example, the amount of dissolved oxygen in the solution can be adjusted by controlling the degree of opening and closing of a reaction vessel containing the solution.
[0077] Specifically, the amount of dissolved oxygen contained in the solution in which the preliminary diaphragm is impregnated may be 8.0 ppm to 12.0 ppm. Specifically, the amount of dissolved oxygen in the solution may be greater than 8.5 ppm and less than 11.5 ppm, greater than 9.0 ppm and less than 11.0 ppm, or greater than 9.5 ppm and less than 10.5 ppm. When the amount of dissolved oxygen in the solution is adjusted within the above range, polymerization of polydopamine and loading within the above range may be achieved. As an analytical method for measuring the amount of dissolved oxygen, for example, Winkler azide modification using manganese sulfate and alkaline potassium iodide sodium azide solution may be employed.
[0078] The method for manufacturing a separator according to the embodiment may further include, after forming the dopamine coating, thermally crosslinking the polymer binder and the polydopamine by exposing the separator to 60°C to 90°C. For example, the separator having the dopamine coating formed thereon may be dried or heated at 60°C to 90°C for 1 to 12 hours. Preferably, the separator may be dried or heated at 70°C to 80°C for 6 to 12 hours. The polymer binder may be an acrylic binder, and the high temperature wet dimensional stability of the separator may be improved by thermally crosslinking the acrylic binder with the polydopamine contained in any one or more of the porous coating and the dopamine coating.
[0079] Another embodiment of the present disclosure provides an electrochemical device comprising: a positive electrode; a negative electrode; and a separator disposed between the positive electrode and the negative electrode, wherein the separator is a separator for an electrochemical device of the above-mentioned embodiment. The electrochemical device can be manufactured by inserting an electrode assembly comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode into a shell or a bag and sealing the shell or the bag. Before sealing the shell or the bag, an electrolyte can be injected to impregnate the electrode assembly with the electrolyte. The shape of the shell or the bag is not limited. For example, the electrochemical device can be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery.
[0080] The positive electrode and the negative electrode may be a coating formed by coating an electrode active material on at least one surface of each current collector and drying. As a current collector, a material having conductivity without causing chemical changes in the electrochemical device may be used. For example, the current collector for the positive electrode may include aluminum, nickel, titanium, baked carbon, stainless steel; aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc., but is not limited thereto. For example, the current collector for the negative electrode may include copper, nickel, titanium, baked carbon, stainless steel; copper or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc., but is not limited thereto. The current collector may have various forms, such as a thin metal plate, a film, a foil, a mesh, a porous body, and a foam.
[0081] The positive electrode includes a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive agent and a binder resin on at least one surface of the current collector. The positive electrode active material may include a lithium manganese composite oxide (LiMn 2 O 4 、LiMnO 2 etc.), lithium cobalt oxide (LiCoO 2 ) or lithium nickel oxide (LiNiO 2 ) or a layered compound substituted by one or more transition metals; lithium manganese oxide, such as Li 1+x Mn 2-x O 4 (here, x is 0 to 0.33), LiMnO 3 、LiMn 2 O 3 or LiMnO 2 ; Lithium copper oxide (Li 2 CuO 2 ); Vanadium oxides, such as LiV 3 O 8 ,LiV 3 O 4 、V 2 O 5 or Cu 2 V 2 O 7 ; By chemical formula LiNi 1-x M x O 2 (herein, M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3) Ni-site lithium nickel oxide represented by the chemical formula LiMn 1-x M x O 2 (here, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li 2 Mn 3 MO 8 (herein, M=Fe, Co, Ni, Cu or Zn) represented by a lithium manganese composite oxide; LiMn wherein a portion of Li in the chemical formula is replaced by alkaline earth metal ions 2 O 4 ; disulfide compounds; and Fe 2 (MoO 4 ) 3 , or a mixture of two or more thereof.
[0082] The negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive agent, and a binder resin on at least one surface of the current collector. As the negative electrode active material, the negative electrode may include one or a mixture of two or more selected from the following: lithium metal oxides; carbon, such as non-graphitizable carbon or graphitic carbon; Li x Fe 2 O 3 (0 ≤ x ≤ 1), Li x WO 2 (0 ≤ x ≤ 1); silicon-based materials, such as Si, SiO x (0 < x < 2), SiC, and Si alloys; metal composite oxides, such as Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups 1, 2, and 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloys; tin-based alloys; metal oxides, such as SnO, SnO 2 , PbO, PbO 2 , Pb 2 O 3 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , GeO, GeO 2 , Bi 2 O 3 , Bi 2 O 4 and Bi 2 O 5 ; conductive polymers, such as polyacetylene; Li-Co-Ni-based materials; and titanium oxides.
[0083] The conductive agent may be any one selected from the group consisting of graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, carbon nanotube, activated carbon, and polyphenylene derivative, or a mixture of two or more of these conductive materials. Carbon nanotubes have cylindrical graphite sheets with a nanoscale diameter and have sp 2Bonding structure, and depending on the angle and structure of the curling of the graphite sheet, it exhibits the characteristics of a conductor or a semiconductor. According to the number of bonds forming the wall, carbon nanotubes can be divided into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT) and multi-walled carbon nanotubes (MWCNT), and these carbon nanotubes can be appropriately selected according to the purpose of the dispersion. More specifically, the conductive agent can be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, Danka black, aluminum powder, nickel powder, zinc oxide, potassium titanate and titanium oxide, or a mixture of two or more conductive materials therein.
[0084] As the binder resin, a binder resin commonly used in electrodes of electrochemical devices can be used. Non-limiting examples of such binder resins can include polyvinylidene fluoride-hexafluoropropylene copolymers, polyvinylidene fluoride-trichloroethylene copolymers, polymethyl methacrylate, polyethylhexyl acrylate, polybutyl acrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-vinyl acetate copolymers, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, etc., but are not limited thereto.
[0085] The electrolyte is obtained by dissolving or dissociating a salt having a structure such as A in an organic solvent. + B - The structure of A + Contains alkali metal cations (such as Li + 、Na + or K + or a combination thereof), and B - Contains anions such as PF 6 - , BF 4 - , Cl - Br - ,I - , ClO 4 - , AsF 6 - , CH 3 CO 2 - CF 3 SO 3 - 、N(CF 3 SO 2 ) 2 - or C(CF 2SO 2 ) 3 - or a combination thereof), the organic solvent is composed of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone (gamma-butyrolactone) or a mixture thereof. Preferably, as the electrolyte, EC / EMC with a weight ratio of 3 / 7 can be used as a solvent, and the dimensional stability of the separator according to the embodiment can be maximized.
[0086] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including a unit cell, a battery pack including a battery module, and a device including a battery pack as a power source. The device may include small devices such as computers, mobile phones, and power tools, as well as medium and large devices such as motor vehicles driven by motors, including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc.; electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and systems for power storage, but not limited thereto.
[0087] Hereinafter, the present disclosure will be described in more detail through specific embodiments and experimental examples. The following embodiments and experimental examples are for illustrative purposes only, and the present disclosure is not limited to the following embodiments and experimental examples.
[0088] Example 1
[0089] Preparation of coating slurry
[0090] 100 mL of an aqueous dispersion medium was prepared by mixing water and isopropyl alcohol at a weight ratio of 95:5 at room temperature (25° C.). 2 g of an acrylic polymer binder (styrene-acrylic, particle size: 350 nm to 400 nm, T g : 40°C) and 30g of inorganic particles (Al 2 O 3 , particle size: 400 nm), and the mixture was stirred using an oscillator for 60 minutes to prepare a coating slurry in which a polymer binder and inorganic particles were dispersed.
[0091] Preparation of porous substrates
[0092] As the porous substrate, a polyethylene film (MI: 0.2 g / 10 min, T m : 135℃, porosity: 45%, average pore size: 45nm).
[0093] Preparation of the preliminary diaphragm
[0094] The coating slurry was coated on both surfaces of the polyethylene film using a bar coater to form porous coating layers each having a coating thickness of 2 μm.
[0095] The process of removing the dispersion medium by applying a low-temperature air stream to the polyethylene film on which the coating layer was formed was repeated 5 times, and as a result, a preliminary separator having a total thickness of 13 μm was prepared.
[0096] Preparation of a solution containing dopamine and dextrin
[0097] Dopamine and dextrin were added to an alkaline buffer solution (20 mM tris-HCl buffer) at a concentration of 2 mg / mL and 50 mg / mL, respectively, using a culture dish at room temperature (25°C), and the amount of addition was adjusted so that dopamine and dextrin had a final content ratio of 1:1000. After preparation, the lid of the culture dish was partially opened to prepare a solution of dopamine and dextrin with a dissolved oxygen content of 9 ppm and a pH of 8. The prepared membrane was immersed in the solution for 48 hours and then dried at 60°C for 12 hours to produce a membrane having a total thickness of 14 μm (porous coating thickness of 2.0 μm, dopamine coating thickness of 0.5 μm) and containing polydopamine and dextrin in a weight ratio of 1:1000.
[0098] Example 2
[0099] A separator was manufactured in the same manner as in Example 1, except that when manufacturing the separator, the preliminary separator was impregnated and then dried at 90°C for 12 hours to manufacture a separator with a total thickness of 14 μm (porous coating thickness of 2.3 μm, dopamine coating thickness of 0.2 μm).
[0100] Example 3
[0101] A separator including polydopamine and dextrin at a weight ratio of 1:500 was manufactured in the same manner as in Example 1, except that dopamine was added at a concentration of 10 mg / mL and the addition amount was adjusted so that dopamine and dextrin had a final content ratio of 1:500.
[0102] Comparative Example 1
[0103] A separator was manufactured in the same manner as in Example 1, except that, when manufacturing the separator, the preliminary separator was immersed in a solution containing dopamine but not containing dextrin.
[0104] Comparative Example 2
[0105] A separator was manufactured in the same manner as in Example 1, except that, when manufacturing the separator, the preliminary separator was immersed in a solution containing dextrin but not dopamine.
[0106] Comparative Example 3
[0107] A membrane comprising polydopamine and dextrin in a weight ratio of 1:400 was manufactured in the same manner as in Example 1, except that dopamine and dextrin were added to the solution at concentrations of 20 mg / mL and 20 mg / mL, respectively, and the added amounts were adjusted so that dopamine and dextrin had a final content ratio of 1:400.
[0108] Experimental example: Confirmation of diaphragm properties
[0109] Air permeability measurement
[0110] As the air permeability, a Gurley air permeability tester (Gurley Company, 4110N) was used to measure the air penetration of 100 cc with a diameter of 28.6 mm and an area of 645 mm. 2 The time it takes to diaphragm.
[0111] Confirmation of dimensional stability
[0112] Each separator of the embodiment and the comparative example was prepared into a size of 5 cm × 5 cm and inserted into an aluminum bag of 7 cm × 10 cm. 1 g of electrolyte was injected into the bag and the bag was sealed. As the electrolyte, 3 mol of vinylene carbonate (VC), 1.5 mol of propane sultone (PS), 1 mol of ethylene sulfate (ESa) and 1 mol of lithium salt LiPF were used in a solvent mixed with ethylene carbonate (EC) / ethyl methyl carbonate (EMC) in a weight ratio of 3 / 7. 6 As a solution additive.
[0113] The sealed bag was exposed in an oven at 135° C. for 30 minutes, then the bag was opened and the shrinkage in the TD direction was measured. The results are shown in Table 1 below.
[0114] Measurement of the peel strength of the separator
[0115] Each of the separators of Examples and Comparative Examples was sampled to have a width of 20 mm, and attached to a slide glass using a double-sided tape (3M Company) having a width of 18 mm to prepare a sample for testing.
[0116] When the separator was peeled from the glass slide at a speed of 300 mm / min in a direction of 180° relative to the attachment direction using UTM, the strength of the peeled porous coating layer was measured, and the results are shown in Table 1 below.
[0117]
Claims
1. A diaphragm for an electrochemical device, the diaphragm comprising: porous polymer substrate; a porous coating layer formed on at least one surface of the porous polymer substrate and comprising a polymer binder and inorganic particles; and A dopamine coating layer is formed on the porous coating layer and comprises polydopamine and dextrin.
2. The electrochemical device separator according to claim 1, in, In the porous coating layer, the polymer binder may be contained in an amount of 5 wt % or less based on the total weight of the porous coating layer. 3 . The separator for an electrochemical device according to claim 1 , comprising polydopamine and dextrin in a weight ratio of 1:500 to 1:1000.
4. The electrochemical device separator according to claim 1, in, The polymer binder includes an acrylic binder, and at least a portion of the acrylic binder is cross-linked with the polydopamine.
5. The electrochemical device separator according to claim 1, in, The polymer binder comprises one or more selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethylhexyl acrylate, methyl methacrylate, styrene-butadiene rubber, nitrile rubber, acrylonitrile-butadiene rubber and acrylonitrile-butadiene-styrene rubber.
6. The electrochemical device separator according to claim 1, in, The thickness of the porous coating layer is greater than the thickness of the dopamine coating layer.
7. A diaphragm for an electrochemical device, comprising: positive electrode; negative electrode; and A separator disposed between the positive electrode and the negative electrode, The separator is a separator for an electrochemical device according to any one of claims 1 to 6. 8 . The separator for an electrochemical device according to claim 7 , further comprising an electrolyte solution containing EC / EMC at a weight ratio of 3 / 7.
9. A method for manufacturing a separator for an electrochemical device, the method include: immersing a preliminary separator in a solution comprising dopamine and dextrin for 1 to 50 hours, the preliminary separator comprising a porous polymer substrate and a porous coating layer comprising a polymer binder and inorganic particles and formed on at least one surface of the porous polymer substrate; as well as By controlling the amount of dissolved oxygen in the solution, a dopamine coating layer including polydopamine and the dextrin is formed on at least one surface of the porous coating layer.
10. The method of claim 9, further comprising thermally crosslinking the polymer binder and the polydopamine by exposing the separator to 60°C to 90°C, The polymer binder comprises an acrylic binder.
Citation Information
Cited By
Separator, electrochemical device, and electronic device
CN119651064A