Method for producing ultra-high molecular weight polypropylene
By adjusting catalyst ratios and employing a catalyst residue removal process, the method produces ultra-high molecular weight polypropylene with controlled molecular weight and low inorganic content, addressing limitations in existing production methods and enhancing performance in advanced materials.
Patent Information
- Application Number
- JP2024529815
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-18
- Filing Date
- 2022-11-15
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-11-15
AI Technical Summary
Existing methods for producing polypropylene are limited in achieving ultra-high molecular weights beyond 1 million g/mol, and the resulting polypropylene contains high levels of inorganic substances, which hinder its application in advanced materials like capacitor films and secondary battery separation membranes.
A method involving specific ratios of titanium compounds as main catalysts, alkyl aluminum as co-catalysts, and silicon compounds, along with controlled polymerization temperature and pressure, followed by a catalyst residue removal process using polar organic solvents and water, to produce ultra-high molecular weight polypropylene with reduced inorganic content.
The method enables the production of ultra-high molecular weight polypropylene with molecular weights ranging from 1 to 4 million g/mol and inorganic content below 30 ppm, suitable for high-performance applications such as secondary battery separation membranes and insulating materials.
Smart Images

Figure 2024540587000001 
Figure 2024540587000002 
Figure 2024540587000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing ultra-high molecular weight polypropylene, and more particularly to a method for producing ultra-high molecular weight polypropylene by adjusting the molecular weight according to the input ratio of titanium tetrachloride, alkyl aluminum, and an external electron donor, and to an ultra-high molecular weight polypropylene containing a very small amount of inorganic matter due to a catalyst residue removal process. [Background technology]
[0002] Generally, polypropylene polymerization is carried out using magnesium chloride as a carrier, titanium chloride containing phthalate, diether, and succinate compounds as internal electron donors as the main catalyst, alkylaluminum as a cocatalyst, and silicon compounds containing alkoxy groups as external electron donors as cocatalysts, and polymerization is carried out in a reactor such as slurry polymerization, bulk polymerization, or gas phase polymerization. At this time, hydrogen is used as a molecular weight regulator to regulate the molecular weight of the polypropylene being polymerized, and all polypropylene currently produced and supplied has an MI of 0.1 to 1,500 g / 10 min under a load of 2.16 kg according to the method proposed by ASTM D1238.
[0003] Polypropylene produced in this way can be used for a variety of purposes, including films, fibers, automotive interior and exterior materials, and pipes. The MI can be adjusted according to the application, or comonomers can be added to adjust the melting point and density.
[0004] Although such a wide variety of applications are possible, the development of processing technology and the demand for materials suitable for new applications necessitate the development of ultra-high molecular weight polypropylene with improved mechanical properties and new applications. However, there is a limit to the method of manufacturing polypropylene resin with a higher molecular weight by controlling the amount of hydrogen injection alone. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] European Patent EP3157966B1 [Patent Document 2] US Patent US8008417B2 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above problems, the method for producing ultra-high molecular weight polypropylene according to the present invention aims to provide ultra-high molecular weight polypropylene having a high molecular weight of 1,000,000 g / mol or more based on viscosity average molecular weight and high catalytic activity by selecting a main catalyst and adjusting the ratio of the main catalyst, cocatalyst, promoter, etc., and changing the polymerization temperature and pressure.
[0007] In addition, the method for producing ultra-high molecular weight polypropylene according to the present invention aims to provide ultra-high molecular weight polypropylene having a lower inorganic content and an average particle size of 400 μm or less in order to improve the performance of capacitor films and separators for secondary batteries. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention includes a method for producing ultra-high molecular weight polypropylene, which is characterized by producing ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more by adjusting the ratio of a main catalyst (a) which is a titanium compound, a co-catalyst (b) which is an alkylaluminum compound, and a promoter (c) which is a silicon compound, as well as the polymerization temperature and polymerization pressure, without adding hydrogen as a molecular weight regulator.
[0009] Here, the alkylaluminum compound co-catalyst Al may be contained in an amount of 10 to 500 moles per mole of Ti of the titanium compound main catalyst.
[0010] Here, the co-catalyst, which is the silicon compound, may contain 1 to 40 moles of Si per mole of Ti, which is the main catalyst, which is the titanium compound.
[0011] Here, the polymerization temperature is preferably from 30 to 90°C.
[0012] Here, the polymerization pressure is preferably 1 to 40 bar.
[0013] Here, in order to remove catalyst residues in the prepared ultra-high molecular weight polypropylene, the method may further include mixing the prepared ultra-high molecular weight polypropylene with a polar organic solvent (x), and separating, purifying, and drying using distilled water (y) or filtered water (y').
[0014] Here, the polar organic solvent (x) may be at least one compound selected from the group consisting of compounds represented by the following formula (4) and compounds represented by the following formula (5):
[0015] R-OH····Chemical formula (4) HO-R1-R2-OH·····Chemical formula (5) (In the above chemical formula (4), R is a linear or branched alkyl group having 1 to 12 carbon atoms, and the above chemical formula (4) may be any one or more compounds selected from the group consisting of methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol, and branched alkyl groups, namely, isopropanol, isobutanol, and isopentanol.
[0016] In the chemical formula (5), R1 and R2 are linear alkyl groups having 0 to 6 carbon atoms, and the chemical formula (5) may be any one or more compounds selected from the group consisting of methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol, and dodecanediol.
[0017] Here, 10 to 1000 parts by weight of the polar organic solvent (x) can be mixed with 100 parts by weight of the ultra-high molecular weight polypropylene produced.
[0018] Here, 100 to 3000 parts by weight of the distilled water (y) or filtered water (y') can be used with respect to 100 parts by weight of the polar organic solvent (x).
[0019] In order to achieve the above object, the present invention further discloses an ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more, which is produced by the method for producing ultra-high molecular weight polypropylene according to the present invention.
[0020] Here, the ultra-high molecular weight polypropylene may have a viscosity average molecular weight of 1,000,000 to 4,000,000 g / mol.
[0021] Here, the ultra-high molecular weight polypropylene may have an inorganic content of 30 ppm or less.
[0022] Here, the ultra-high molecular weight polypropylene may have a particle size of 400 μm or less. Effect of the Invention
[0023] According to the above-mentioned method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to control the molecular weight for producing ultra-high molecular weight polypropylene by adjusting the input ratio of the main catalyst, cocatalyst and promoter without adding hydrogen, which is used as a molecular weight regulator under general polymerization conditions.
[0024] In addition, the ultra-high molecular weight polypropylene produced according to the present invention contains a lower level of inorganic matter than commonly produced polypropylene resins due to the process of removing catalyst residue, and therefore has properties suitable for applications requiring separators and insulation for secondary batteries.
[0025] In addition, according to the method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to produce an ultra-high molecular weight polypropylene separator having excellent performance and a heterogeneous separator made of ultra-high molecular weight polyethylene and ultra-high molecular weight polypropylene by improving the kneadability and melting speed with ultra-high molecular weight polyethylene used in separators for secondary batteries through particle size control. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The terms used in this application are merely used to describe specific examples. Thus, for example, singular expressions include plural expressions unless the context clearly requires that they be singular. It should be noted that the terms "include" or "comprise" used in this application are used to clearly indicate the presence of features, steps, functions, components, or combinations thereof described in the specification, and do not preliminarily exclude the presence of other features, steps, functions, components, or combinations thereof.
[0027] On the other hand, unless otherwise defined, all terms used herein should be considered to have the same meaning as that commonly understood by a person having ordinary skill in the art to which the present invention pertains. Therefore, unless expressly defined herein, a particular term should not be construed in an overly ideal or formal sense.
[0028] The present inventors have confirmed that ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more can be produced by the present invention as described below, and have completed the present invention. Meanwhile, the term "ultra-high molecular weight" as used in this specification means a viscosity average molecular weight of 1,000,000 g / mol or more.
[0029] <Method of manufacturing ultra-high molecular weight polypropylene> As a result of research to solve the above-mentioned problems, the present inventors have come up with the following invention. This specification discloses a method for producing ultra-high molecular weight polypropylene, which is characterized by producing ultra-high molecular weight polypropylene of 1,000,000 g / mol or more by adjusting the ratio of main catalyst (a) which is a titanium compound, co-catalyst (b) which is an alkylaluminum compound, and promoter (c) which is a silicon compound, as well as the polymerization temperature and polymerization pressure, without adding hydrogen, which is a molecular weight regulator.
[0030] In order to achieve the above-mentioned object, the present invention provides a method for producing ultra-high molecular weight polypropylene, comprising the steps of: using a main catalyst having high stereoregularity; introducing a content of a cocatalyst capable of initiating the catalyst reaction and minimizing the detachment of the molecular backbone; and an optimal content of an external electron donor to carry out a polymerization reaction.
[0031] More specifically, the present invention provides a method for controlling the molecular weight of ultra-high molecular weight polypropylene according to the ratio of the main catalyst, cocatalyst and promoter.
[0032] The steps in the method for producing ultra-high molecular weight polypropylene of the present invention are as follows:
[0033] (x) mixing and charging the cocatalyst (b), the main catalyst (a) and the promoter (c) in a reactor in the presence of a hydrocarbon solvent having 1 to 20 carbon atoms;
[0034] (y) adding propylene (d) to the mixed solution obtained in step (x) in an atmosphere having a temperature of 30° C., and carrying out a polymerization reaction while maintaining the temperature at 30 to 90° C.; and
[0035] (z) after carrying out the steps (x) and (y), filtering the polypropylene resin powder from the obtained slurry reaction solution, and drying the obtained polypropylene resin powder.
[0036] Here, the step (x) is preferably carried out under a nitrogen atmosphere, i.e., the step (x) is preferably carried out in the presence of an inert gas.
[0037] In the method for producing ultra-high molecular weight polypropylene of the present invention, the hydrocarbon solvent having 1 to 20 carbon atoms in step (x) may include at least one solvent selected from the group consisting of aliphatic hydrocarbon solvents such as pentane, hexane, cyclohexane, methylcyclohexane, heptane, octane, decane, undecane, dodecane, tridecane, or tetradecane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, or ethylbenzene; and halogenated hydrocarbon solvents such as dichloropropane, dichloroethylene, trichloroethylene, carbon tetrachloride, or chlorobenzene. Alternatively, gas phase polymerization or bulk polymerization may be performed under high pressure propylene without a hydrocarbon.
[0038] In the method for producing ultra-high molecular weight polypropylene of the present invention, representative examples of the co-catalyst (b) in step (x) may include any one or more compounds selected from the group consisting of triethylaluminum, trimethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum bromide, diethylaluminum iodide, diethylaluminum fluoride, ethylaluminum dichloride, dimethylaluminum chloride, methylaluminum dichloride, and ethylaluminum sesquichloride.
[0039] In step (x), the cocatalyst (b) is preferably added in an amount of 5 to 500 moles per mole of the main catalyst (a), more preferably in an amount of 10 to 500 moles, and most preferably in an amount of 100 to 500 moles, but is not limited thereto. More specifically, it is preferable that the cocatalyst (b) which is an alkylaluminum compound contains 5 to 500 moles of Al per mole of Ti in the main catalyst (a) which is a titanium compound. For example, when the cocatalyst (b) which is an alkylaluminum compound contains less than 5 moles of Al per mole of Ti in the main catalyst (a) which is a titanium compound, a problem may occur in which the polymerization reaction does not occur sufficiently. Conversely, when the cocatalyst (b) which is an alkylaluminum compound contains more than 500 moles of Al per mole of Ti in the main catalyst (a) which is a titanium compound, a problem may occur in which ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more is not sufficiently obtained, even if the polymerization reaction occurs.
[0040] In step (x), the main catalyst (a) contains a silicon compound including phthalate, diether, and succinate as an internal electron donor, and is preferably a Ziegler-Natta titanium chloride catalyst supported by magnesium chloride, such as titanium trichloride or titanium tetrachloride, and more preferably a catalyst that provides high stereoregularity depending on the form of the internal electron donor, and a commonly available catalyst may be used.
[0041] In step (x), the co-catalyst (c) may be at least one compound selected from the group consisting of a compound represented by the following formula (1), a compound represented by the following formula (2), and a compound represented by the following formula (3): [ka] [ka] [ka] In the above chemical formulas (1) to (3), R a, R 7 , R 8 and R 9 are each independently an alkyl group, a cycloalkyl group, an aryl group, an allyl group, or a vinyl group having 1 to 12 carbon atoms; R b is an alkyl group having 1 to 6 carbon atoms or an aryl group, and R is an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group, an aryl group, an allyl group, or -OR c In this case, R c is an alkyl group or an aryl group having 1 to 6 carbon atoms, and n is an integer from 0 to 6.
[0042] Specifically, representative examples of the compound of the formula (1) include cyclohexylmethyldimethoxysilane (CMCD), cyclohexyl-n-propyldimethoxysilane (CPDM), cyclohexyl-i-propyldimethoxysilane (CIPDM), cyclohexyl-n-butyldimethoxysilane (CBDM), cyclohexyl-i-butyldimethoxysilane (CIBDM), cyclohexyl-n-hexyldimethoxysilane (CHDM), cyclohexyl-n-octyldimethoxysilane (CODM), cyclohexyl-n-decyldimethoxysilane (CDeDM), dimethyldimethoxysilane, dimethyldiethoxysilane, and the like. and any one or more compounds selected from the group consisting of silane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane. Representative examples of the compound of the above chemical formula (1) may include any one or more compounds selected from the group consisting of dimethyldimethoxysilane, dimethyldiethoxysilane, dicyclopentyldimethoxysilane, cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane.
[0043] Representative examples of the compound of the chemical formula (2) include 1,1,3,3-tetramethoxy-1,3-dimethyl-1,3-disilanepropane (TMDMDP), 1,1,3,3-tetramethoxy-1-methyl-3-hexyl-1,3-disilanepropane (TMMHDP), 1,1,3,3-tetramethoxy-1,3-di-n-hexyl-1,3-disilanepropane (TMDHDP), 1,1,3,3-tetramethoxy-1-methyl-3-cyclohexyl-1,3-disilanepropane (TMDHDP), Examples of the compound include one or more compounds selected from the group consisting of 1,1,3,3-tetramethoxy-1,3-dicyclohexyl-1,3-disilanepropane (TMMCDP), 1,1,3,3-tetramethoxy-1,3-dicyclohexyl-1,3-disilanepropane (TMDCDP), 1,1,8,8-tetramethoxy-1,8-dicyclohexyl-1,8-disilaneoctane (TMDCDO) and 1,1,3,3-tetramethoxy-1,3-dimethyldisiloxane (TMDMDS).
[0044] Representative examples of the compound of the chemical formula (3) include one or more compounds selected from the group consisting of methyl(trimethylsilylmethyl)dimethoxysilane (MTDM), n-propyl(trimethylsilylmethyl)dimethoxysilane (PTDM), i-propyl(trimethylsilylmethyl)dimethoxysilane (IPTDM), n-butyl(trimethylsilylmethyl)dimethoxysilane (BTDM), i-butyl(trimethylsilylmethyl)dimethoxysilane (IBTDM), n-pentyl(trimethylsilylmethyl)dimethoxysilane (PnTDM), n-hexyl-(trimethylsilylmethyl)dimethoxysilane (HTDM), cyclopentyl(trimethylsilylmethyl)dimethoxysilane (CpTDM) and cyclohexyl(trimethylsilylmethyl)dimethoxysilane (CTDM).
[0045] In step (x), the co-catalyst (c) is preferably added in an amount of 1 to 40 moles per mole of the main catalyst (a), but is not limited thereto. More specifically, it is preferable that the co-catalyst (c) contains 1 to 40 moles of Si, which is a silicon compound, per mole of Ti, which is a titanium compound, of the main catalyst. For example, if the co-catalyst (c) contains less than 1 mole of Si, which is a silicon compound, per mole of Ti, which is a titanium compound, of the main catalyst (a), the polymerization reaction may not occur sufficiently. Conversely, if the co-catalyst (c) contains more than 40 moles of Si, which is a silicon compound, per mole of Ti, which is a titanium compound, of the main catalyst (a), the polymerization reaction may occur, but the ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more may not be obtained sufficiently.
[0046] On the other hand, in step (y), the polymerization temperature at which propylene (d) is added to the mixed solution and the polymerization reaction is carried out is preferably within the range of 30 to 90° C., but is not limited thereto. If the polymerization temperature is less than 30° C., a problem may arise in that the polymerization reaction does not proceed sufficiently, and conversely, if the polymerization temperature exceeds 90° C., a problem may arise in that even if the polymerization reaction does proceed, a sufficient amount of ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more cannot be obtained.
[0047] In step (y), the polymerization pressure at which propylene (d) is added to the mixed solution and the polymerization reaction is carried out is preferably within the range of 1 to 40 bar, but is not limited thereto. If the polymerization pressure is less than 1 bar, the polymerization reaction may not proceed sufficiently, and conversely, if the polymerization pressure exceeds 40 bar, even if the polymerization reaction does proceed, the ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more may not be sufficiently obtained.
[0048] Meanwhile, in step (y), the polymerization reaction may be carried out in liquid, slurry, bulk phase or gas phase polymerization, but is not limited thereto.
[0049] <Catalyst Residue Removal Process> In order to achieve the above-mentioned object, the present invention provides a method for producing ultra-high molecular weight polypropylene and a process for removing catalyst residues, and provides a method for removing inorganic substances such as magnesium, titanium, aluminum, and silicon used as catalysts in the polymerization process.
[0050] The method for removing catalyst residues in ultra-high molecular weight polypropylene of the present invention includes the following steps: In order to remove catalyst residues in the ultra-high molecular weight polypropylene produced according to the present invention, the method may further include the steps of mixing the ultra-high molecular weight polypropylene produced with a polar organic solvent (x), and separating, purifying and drying the mixture using distilled water (y) or filtered water (y').
[0051] More specifically, the method may include the steps of mixing the ultra-high molecular weight polypropylene produced by the present invention with a polar organic solvent; separating the ultra-high molecular weight polypropylene produced from the polar organic solvent by contacting with water; and drying the separated ultra-high molecular weight polypropylene.
[0052] In this case, the mixing ratio of the ultra-high molecular weight polypropylene and the polar organic solvent may be 0.1 to 10 times the weight of the ultra-high molecular weight polypropylene, and preferably 0.5 to 3 times the weight of the ultra-high molecular weight polypropylene.
[0053] That is, it is preferable to mix 10 to 1,000 parts by weight of the polar organic solvent (x) with 100 parts by weight of the produced ultra-high molecular weight polypropylene, and it is more preferable to mix 30 to 300 parts by weight of the polar organic solvent (x) with 100 parts by weight of the produced ultra-high molecular weight polypropylene.
[0054] The polar organic solvent used to remove catalyst residues in the ultra-high molecular weight polypropylene produced according to the present invention may be a compound represented by the following formula (4): R-OH····Chemical formula (4) HO-R1-R2-OH·····Chemical formula (5) In the chemical formula (4), R is a linear or branched alkyl group having 1 to 12 carbon atoms. Specifically, representative examples of the compound corresponding to the chemical formula (4) may include one or more compounds selected from the group consisting of linear alkalis such as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, undecanol, and dodecanol, and branched alkyl groups such as isopropanol, isobutanol, and isopentanol.
[0055] In the chemical formula (5), R1 and R2 are linear alkyl groups having 0 to 6 carbon atoms. Specifically, representative examples of the compound corresponding to the chemical formula (5) may include one or more compounds selected from the group consisting of methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol, and dodecanediol.
[0056] The water used to separate the polar organic solvent dissolving the catalyst residue from the produced ultra-high molecular weight polypropylene may be distilled water or filtered water, and may be used in an amount 1 to 30 times, preferably 5 to 20 times, the weight of the polar organic solvent used.
[0057] That is, it is preferable to use 100 to 3,000 parts by weight of distilled water (y) or filtered water (y') per 100 parts by weight of the polar organic solvent (x). It is also recommended to use 500 to 2000 parts by weight of distilled water (y) or filtered water (y') per unit weight. The mixture of the produced ultra-high molecular weight polypropylene and the polar organic solvent is contacted with water and then separated into layers, where the polar organic solvent of the molecules is mixed in the water layer and the produced ultra-high molecular weight polypropylene floats on the upper layer of the water, which is separated using filter paper or a filter and then dried in a dryer at 90 to 105°C to obtain ultra-high molecular weight polypropylene from which inorganic substances such as magnesium, titanium, aluminum, and silicon used as catalysts in the polymerization process have been removed.
[0058] <Adjusting particle size of ultra-high molecular weight polypropylene> In order to achieve the above object, the present invention provides a method for adjusting the particle size of ultra-high molecular weight polypropylene by adjusting the particle size and polymerization degree of the catalyst. The particle size and shape of ultra-high molecular weight polypropylene are determined by the particle size and particle size of the main catalyst used in the polymerization of ultra-high molecular weight polypropylene, and in particular, the particle size is determined by the polymerization degree. Therefore, in order to ensure a particle size required by a processing method of ultra-high molecular weight polypropylene, the present invention provides a method for adjusting the polymerization degree and selecting polymerization conditions such as polymerization pressure, polymerization temperature, and polymerization time that affect the polymerization degree, and the particle size of the main catalyst used.
[0059] The above-mentioned degree of polymerization is inversely proportional to the polymerization pressure and polymerization time. Therefore, by lowering the polymerization pressure and shortening the polymerization time, an ultra-high molecular weight polypropylene resin having a small particle size due to a low degree of polymerization can be obtained. Furthermore, the smaller the particle size of the main catalyst, the smaller the particle size of the resin can be obtained at the same degree of polymerization. Therefore, a catalyst having an appropriate particle size and particle size distribution can be selected to obtain the desired particle size and particle size of the resin.
[0060] <Ultra-high molecular weight polypropylene produced by the present invention> Meanwhile, the present specification further discloses ultra-high molecular weight polypropylene produced by the method for producing ultra-high molecular weight polypropylene of the present invention.
[0061] The ultra-high molecular weight polypropylene of the present invention produced by the method for producing ultra-high molecular weight polypropylene of the present invention has a viscosity average molecular weight of preferably 1,000,000 to 4,000,000 g / mol, and more preferably 1,000,000 to 2,500,000 g / mol, under conditions in which no hydrogen or a very small amount of hydrogen is added, preferably under conditions in which no hydrogen is added.
[0062] In addition, as described above, the ultra-high molecular weight polypropylene of the present invention can maintain the inorganic content at a level of 30 ppm or less by undergoing the catalyst residue removal process. More specifically, the inorganic content of the ultra-high molecular weight polypropylene of the present invention is preferably 1 to 30 ppm, and more preferably 5 to 20 ppm.
[0063] In addition, the ultra-high molecular weight polypropylene of the present invention can maintain a particle size of 400 μm or less by adjusting the particle size and polymerization degree of the catalyst as described above. More specifically, the particle size of the ultra-high molecular weight polypropylene of the present invention is preferably 10 to 400 μm, and more preferably 30 to 300 μm.
[0064] In addition, in the method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to produce ultra-high molecular weight polypropylene having an inorganic content of 30 ppm or less, which can be used as a separator or insulating material for secondary batteries that require a low inorganic content, by using a catalyst residue removal technology, and it is also possible to produce ultra-high molecular weight polypropylene resin particles having a particle size of 400 μm or less, which is suitable for gel films, gel spinning, etc. EXAMPLES
[0065] The claims of this specification will be described in more detail with reference to the accompanying drawings and examples. However, the drawings and examples presented in this specification can be modified in various ways by ordinary skilled artisans to have various forms, and the description of this specification should not be construed as limiting the present invention to the specific disclosed form, but should be considered as including all equivalents or alternatives within the spirit and technical scope of the present invention. The accompanying drawings are presented to help ordinary skilled artisans to more accurately understand the present invention, and may be exaggerated or reduced in size.
[0066] {Examples and Evaluation} <Experimental Example 1> Polymerization and property measurement of ultra-high molecular weight polypropylene resin Example 1 A 2L stainless steel reactor equipped with a stirrer was evacuated at room temperature, and 900mL of hexane was poured in as an organic solvent, followed by stirring. 900mg of triethylaluminum and 30mg of dicyclopentyldimethoxysilane were added at room temperature, and 30mg of Ziegler-Natta series titanium catalyst was added as the main catalyst. The reactor was then placed in a thermostatic chamber maintained at 70℃, and when the temperature was raised to 60℃, propylene was added up to 10bar and polymerized for 2 hours. After the reaction was completed, the unreacted propylene was vented, the reactor was opened, and the organic solvent and polymerized resin were separated, and the resin was dried in a dryer to obtain polypropylene resin. The amount of the catalyst used, the catalytic activity, and the physical properties of the resin were measured and are shown in Table 1 below.
[0067] Example 2 The same procedure was carried out as in Example 1, except that the amount of triethylaluminum added was reduced from 900 mg to 300 mg.
[0068] Example 3 The same procedure was followed as in Example 2, except that the amount of dicyclopentyldimethoxysilane added was increased from 30 mg to 90 mg.
[0069] Example 4 The same procedure was repeated except that 1240 mg of triisobutylaluminum was used instead of 900 mg of triethylaluminum in Example 1.
[0070] Example 5 The same procedure was carried out as in Example 4, except that the amount of triisobutylaluminum added was reduced from 1240 mg to 410 mg.
[0071] Example 6 The same procedure as in Example 5 was repeated, except that the amount of dicyclopentyldimethoxysilane added was increased from 30 mg to 90 mg.
[0072] Example 7 The same procedure was repeated, except that 2290 mg of trioctyl aluminum was used instead of 900 mg of triethyl aluminum in Example 1.
[0073] Example 8 The same procedure was carried out as in Example 7, except that the amount of trioctylaluminum added was reduced from 2290 mg to 760 mg.
[0074] Example 9 The same procedure as in Example 8 was repeated, except that the amount of dicyclopentyldimethoxysilane added was increased from 30 mg to 90 mg.
[0075] Example 10 The same procedure was carried out as in Example 1, except that the amount of propylene fed was adjusted from 10 bar to 3 bar.
[0076] Example 11 The same procedure as in Example 3 was carried out, except that the propylene supply temperature was set to 40°C and the temperature of the thermostatic bath was fixed at 50°C.
[0077] Example 12 The same procedure as in Example 3 was carried out, except that the propylene charging temperature was set to 25°C and the temperature of the thermostatic bath was fixed at 30°C.
[0078] Example 13 The same procedure as in Example 3 was repeated, except that propylene was added instead of hexane, which is an organic solvent, and polymerization was carried out at 70° C. under a propylene saturated vapor pressure of 32 bar.
[0079] Comparative Example 1 The same procedure as in Example 1 was followed, except that 20 mL of hydrogen gas was injected.
[0080] Comparative Example 2 The same procedure as in Comparative Example 1 was followed, except that 80 mL of hydrogen gas was injected.
[0081] Comparative Example 3 The same procedure was carried out as in Example 1, except that the amount of triethylaluminum added was reduced from 900 mg to 10 mg.
[0082] Comparative Example 4 The same procedure was carried out as in Example 1, except that the amount of triethylaluminum added was increased from 900 mg to 1,270 mg.
[0083] Comparative Example 5 The same procedure was carried out as in Example 1, except that the amount of triethylaluminum added was increased from 900 mg to 1,730 mg.
[0084] Comparative Example 6 The same procedure was followed as in Example 2, except that the amount of dicyclopentyldimethoxysilane added was reduced from 30 mg to 3 mg.
[0085] Comparative Example 7 The same procedure was followed as in Example 2, except that the amount of dicyclopentyldimethoxysilane added was increased from 30 mg to 150 mg.
[0086] Methods for measuring the physical properties of polypropylene resin (1) Melt Index (MI): The melt index was measured according to ASTM D1238 under the conditions of 230° C. and kilogram (kg).
[0087] (2) Viscosity average molecular weight (Mv): The viscosity average molecular weight was measured by obtaining the intrinsic viscosity according to the intrinsic viscosity measurement method defined in ASTM D5020 and ISO 1628-3, and the value was calculated by the Margolies Equation. Mv = 5.37 × 10 4 ×[η] 1.49 η: Intrinsic viscosity
[0088] (3) Catalytic activity: The catalytic activity was expressed as the amount of polypropylene resin obtained after the completion of polymerization divided by the amount of the main catalyst added.
[0089] (4) Particle size: Measurement was performed using a Malvern Mastersizer 2000, and the average particle size (D[0.5]) was reported.
[0090] (5) Inorganic matter content (Ash): 50 g of the obtained polypropylene resin was completely combusted, and the weight of the remaining amount was calculated and expressed.
[0091] Polypropylene resin physical property measurement results The results of physical property measurements of polypropylene produced by each ratio of main catalyst / cocatalyst / promoter in Examples 1 to 13 and Comparative Examples 1 to 7, including the catalyst residue removal process, and the polymerization reaction (polymerization process) conditions are shown in Table 1 below.
[0092] [Table 1]
[0093] Referring to Table 1, it can be seen that the MI and viscosity average molecular weight of ultra-high molecular weight polypropylene according to an embodiment of the present invention depending on the ratio of main catalyst, cocatalyst and cocatalyst added can be confirmed, and it can be seen that as the ratio of cocatalyst is reduced and the ratio of cocatalyst is increased, a polypropylene with a higher molecular weight can be obtained. Similarly, it can be seen that the catalyst residue can be removed depending on the amounts of resin, polar organic solvent and water used in the catalyst residue removal process according to an embodiment of the present invention, and it can be seen that the particle size of the polypropylene resin produced can be controlled by controlling the degree of polymerization.
[0094] More specifically, from Examples 1 and 2 and Comparative Examples 3 to 5, it can be confirmed that when 10 to 500 moles of Al, the co-catalyst which is an alkylaluminum compound, are contained per 1 mole of Ti, the main catalyst which is a titanium compound, it is possible to produce an ultra-high molecular weight polypropylene resin having a controlled resin particle size and a viscosity average molecular weight of 1,000,000 g / mol or more. Similarly, from Examples 2 and 3 and Comparative Examples 6 and 7, it can be confirmed that when 1 to 40 moles of Si, the co-catalyst which is a silicon compound, are contained per 1 mole of Ti, the main catalyst, it is possible to produce an ultra-high molecular weight polypropylene resin having a controlled resin particle size and a viscosity average molecular weight of 1,000,000 g / mol or more.
[0095] Comparing the results of producing ultra-high molecular weight polypropylene according to an embodiment of the present invention, it was confirmed that the molecular weight can be controlled depending on the molecular structure (molecular weight) of the cocatalyst as in Examples 1, 4, and 7 and Examples 2, 5, and 8, under the same polymerization process conditions. As a result, it was confirmed that the molecular weight can be controlled depending on the molecular structure (molecular weight) of the cocatalyst. As disclosed in Comparative Examples 1 and 2, in addition to controlling the molecular weight by hydrogen, it was confirmed that the viscosity average molecular weight of the ultra-high molecular weight polypropylene can be controlled from 1 million g / mol to 4 million g / mol depending on the amount of cocatalyst and promoter added.
[0096] In addition, from Examples 1, 12 and 13, it can be confirmed that when the ultra-high molecular weight polypropylene of the present invention is produced, when the polymerization pressure is 1 to 40 bar, it is possible to produce an ultra-high molecular weight polypropylene resin having a controlled resin particle size and a viscosity average molecular weight of 1,000,000 g / mol or more.
[0097] Furthermore, from Examples 3, 11 and 12, it can be confirmed that when the ultra-high molecular weight polypropylene of the present invention is produced at a polymerization temperature of 30 to 90°C, it is possible to produce an ultra-high molecular weight polypropylene resin having a controlled resin particle size and a viscosity average molecular weight of 1,000,000 g / mol or more.
[0098] According to the above-mentioned method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to control the molecular weight for producing ultra-high molecular weight polypropylene by adjusting the input ratio of the main catalyst, cocatalyst and promoter without adding hydrogen, which is used as a molecular weight regulator under general polymerization conditions.
[0099] <Experimental Example 2> Removal process of catalyst residue from ultra-high molecular weight polypropylene resin Example 14 The resin produced in Example 2 in Table 1 above is used. After opening a 2L stainless steel reactor equipped with an agitator, 50g of ultra-high molecular weight polypropylene resin is added. The reactor is placed in a vacuum at room temperature and 200mL of hexane as an organic solvent is added and stirred. 5g of methanol as a polar organic solvent is added and stirred for 10 minutes. Then, 900mL of distilled water is added and stirred for another 10 minutes. After stirring is completed, the powdered ultra-high molecular weight polypropylene resin and the liquid component consisting of hexane, polar organic solvent, and water are separated through filter paper. The separated resin is thoroughly dried in a dryer at 100°C and the ash component is analyzed.
[0100] Example 15 The same procedure was carried out as in Example 14, except that the amount of methanol added was increased from 5 g to 25 g.
[0101] Example 16 The same procedure was carried out as in Example 14, except that the amount of methanol added was increased from 5 g to 50 g.
[0102] Example 17 The same procedure was carried out as in Example 14, except that the amount of methanol added was increased from 5 g to 150 g.
[0103] Example 18 The same procedure was carried out as in Example 16, except that the amount of distilled water added was increased from 200 mL to 1,000 mL.
[0104] Example 19 The same procedure as in Example 15 was followed except that the stirring time was increased from 10 minutes to 1 hour.
[0105] Comparative Example 8 The same procedure was carried out as in Example 16, except that the amount of distilled water added was reduced from 200 mL to 40 mL.
[0106] Comparative Example 9 The same procedure was carried out as in Example 16, except that the amount of distilled water added was increased from 200 mL to 2,000 mL.
[0107] Comparative Example 10 The results of analysis of ash of the resin produced in Example 2 are shown in [Table 1].
[0108] Comparative Example 11 The same procedure was carried out as in Example 14, except that the amount of methanol added was reduced from 5 g to 3 g.
[0109] Comparative Example 12 The same procedure was carried out as in Example 14, except that the amount of methanol added was increased from 5 g to 550 g, and the amount of distilled water added was increased from 200 mL to 1,000 mL.
[0110] Comparative Example 13 The same procedure as in Comparative Example 11 was repeated except that the stirring time was increased from 10 minutes to 1 hour.
[0111] Measurement results of inorganic content of ultra-high molecular weight polypropylene resin The ash components of the ultra-high molecular weight polypropylene resins prepared under each control condition of the catalyst residue removal process of the present invention and according to Examples 14 to 19 and Comparative Examples 8 to 13 were analyzed, and the measurement results of the inorganic content are shown in Table 2 below.
[0112] [Table 2]
[0113] Referring to Table 2, in the catalyst residue removal process according to the present invention, the ultra-high molecular weight polypropylene prepared is mixed with a polar organic solvent (x), and distilled water (y) or filtered water (y') is added. It has been confirmed that by carrying out the steps of separation, purification and drying using the above-mentioned polypropylene resin, an ultra-high molecular weight polypropylene resin having an inorganic matter content of 30 ppm or less can be obtained.
[0114] On the other hand, the ultra-high molecular weight polypropylene resin of Comparative Example 10 means a resin that has not been subjected to a separate process for removing catalyst residues.
[0115] In particular, from the ultra-high molecular weight polypropylene resins of Examples 14 to 17 and Comparative Examples 11 and 12, it can be confirmed that when 10 to 1000 parts by weight of polar organic solvent (x) is mixed with 100 parts by weight of ultra-high molecular weight polypropylene, the inorganic content of the ultra-high molecular weight polypropylene is maintained at a level of 30 ppm or less.
[0116] In addition, from the ultra-high molecular weight polypropylene resins of Examples 16 and 18 and Comparative Examples 8 and 9, when 100 parts by weight of polar organic solvent (x) is mixed with 100 to 3,000 parts by weight of distilled water (y) or filtered water (y'), the inorganic content of the ultra-high molecular weight polypropylene is 30 ppm or less. It can be seen that the lower level will be maintained.
[0117] In addition, from the ultra-high molecular weight polypropylene resins of Examples 15 and 19, it can be confirmed that when the stirring time after adding methanol is 10 to 60 minutes, the inorganic content of the ultra-high molecular weight polypropylene is maintained at a level of 30 ppm or less.
[0118] According to the above-mentioned method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to control the molecular weight for producing ultra-high molecular weight polypropylene by adjusting the input ratio of the main catalyst, cocatalyst and promoter without adding hydrogen, which is used as a molecular weight regulator under general polymerization conditions.
[0119] In addition, the ultra-high molecular weight polypropylene prepared according to the present invention contains a low level of inorganic matter compared to polypropylene resins generally prepared by a process for removing catalyst residues, and thus has properties suitable for applications requiring separators and insulation properties for secondary batteries.
[0120] In addition, according to the method for producing ultra-high molecular weight polypropylene of the present invention, it is possible to produce an ultra-high molecular weight polypropylene separator having excellent performance and a heterogeneous separator made of ultra-high molecular weight polyethylene and ultra-high molecular weight polypropylene by improving the kneadability and melting speed with ultra-high molecular weight polyethylene used in separators for secondary batteries through particle size control.
[0121] The above description is merely an illustrative example of the technical concept of the present invention, and various modifications and variations can be made by those having ordinary knowledge in the technical field to which the present invention pertains without departing from the essential characteristics of the present invention.
[0122] Therefore, the embodiments disclosed in the present invention are for illustration purposes only and are not intended to limit the technical idea of the present invention, and the scope of the technical idea of the present invention is not limited by such embodiments. The scope of protection of the present invention should be interpreted according to the following claims, and any technical idea within the scope equivalent thereto should be interpreted as being included in the scope of the present invention. [Industrial Applicability]
[0123] According to the present invention, it is possible to control the molecular weight for producing ultra-high molecular weight polypropylene by adjusting the ratio of the main catalyst, cocatalyst and promoter to be added, without adding hydrogen, which is used as a molecular weight regulator under general polymerization conditions.
[0124] In addition, the ultra-high molecular weight polypropylene according to the present invention contains a low level of inorganic matter compared to polypropylene resins generally produced by a process for removing catalyst residues, and thus has properties suitable for applications requiring separators and insulation properties for secondary batteries.
[0125] In addition, according to the present invention, by adjusting the particle size, it is possible to improve the kneadability and melting speed with ultra-high molecular weight polyethylene used in the separator of a secondary battery, thereby producing an ultra-high molecular weight polypropylene separator with excellent performance and a heterogeneous separator of ultra-high molecular weight polyethylene and ultra-high molecular weight polypropylene.
Claims
1. Adding a mixture of a main catalyst which is a titanium compound, a co-catalyst which is an alkylaluminum compound, and a co-catalyst which is a silicon compound in the presence of a hydrocarbon solvent containing 1 to 20 carbon atoms without adding hydrogen which is a molecular weight regulator; and Adding propylene monomer to the mixed solution to carry out a polymerization reaction, A method for producing ultra-high molecular weight polypropylene, comprising producing ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 g / mol or more.
2. The method for producing ultra-high molecular weight polypropylene according to claim 1, characterized in that the co-catalyst Al, which is the alkylaluminum compound, is contained in an amount of 10 to 500 moles per mole of Ti, which is the main catalyst, which is the titanium compound.
3. The method for producing ultra-high molecular weight polypropylene according to claim 1, wherein the co-catalyst, which is a silicon compound, contains 1 to 40 moles of Si per mole of Ti in the main catalyst, which is a titanium compound.
4. The method for producing ultra-high molecular weight polypropylene according to claim 1, wherein the polymerization reaction temperature is 30 to 90°C.
5. The method for producing ultra-high molecular weight polypropylene according to claim 1, wherein the polymerization reaction pressure is 1 to 40 bar.
6. The ultra-high molecular weight polypropylene according to claim 1, further comprising a step of mixing the ultra-high molecular weight polypropylene with a polar organic solvent (x) and separating, purifying and drying the ultra-high molecular weight polypropylene using distilled water (y) or filtered water (y') in order to remove catalyst residues in the ultra-high molecular weight polypropylene. Method for producing low molecular weight polypropylene.
7. The polar organic solvent (x) is at least one compound selected from the group consisting of a compound represented by the following formula (4) and a compound represented by the following formula (5): R-OH...Chemical formula (4) HO-R1-R2-OH...Chemical formula (5) (In the above chemical formula (4), R is a linear or branched alkyl group having 1 to 12 carbon atoms, and in the above chemical formula (5), R1 and R2 are linear alkyl groups having 1 to 6 carbon atoms.)
8. The method for producing ultra-high molecular weight polypropylene according to claim 7, wherein the formula (4) is at least one compound selected from the group consisting of methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol, and branched alkyl groups, such as isopropanol, isobutanol, and isopentanol.
9. 8. The method for producing ultra-high molecular weight polypropylene according to claim 7, wherein the formula (5) is at least one compound selected from the group consisting of methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol, and dodecanediol.
10. The method for producing ultra-high molecular weight polypropylene according to claim 6, characterized in that 10 to 1000 parts by weight of the polar organic solvent (x) is mixed with 100 parts by weight of the produced ultra-high molecular weight polypropylene.
11. The ultra-high molecular weight polymer according to claim 6, wherein 100 to 3000 parts by weight of the distilled water (y) or filtered water (y') is used per 100 parts by weight of the polar organic solvent (x). A method for producing polypropylene.
12. Produced by the production method according to any one of claims 1 to 11, The viscosity average molecular weight is 1,000,000 g / mol or more, The inorganic content is 1 to 30 ppm; Ultra-high molecular weight polypropylene having a particle size of 10 to 400 μm.
13. The ultra-high molecular weight polypropylene according to claim 12, characterized in that the viscosity average molecular weight is 1 million to 4 million g / mol.
Citation Information
Patent Citations
Production of ultrahigh-MW poly-alpha-olefin
JP1987022808A
Polymeric materials formed using blends of electron donors
JP2002514666A
Polymers, their manufacturing process, and applications
JP2010516842A
Polypropylene resin composition for microporous film formation
WO2010079799A1
Process for the polymerization of propylene
EP3157966B1