Film quality improving agent, thin film forming method using the same, semiconductor substrate and semiconductor device manufactured therefrom

The film quality improving agent addresses issues of molybdenum-based thin film deposition by forming a shielding region to adjust growth rate, improving step coverage and uniformity, and enhancing electrical properties, particularly for complex structures and room temperature deposition.

JP2024540610AActive Publication Date: 2024-10-31SOULBRAIN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529944
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-22
Filing Date
2022-11-08
Publication Date
2024-10-31
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Existing molybdenum-based thin film deposition methods face issues such as low deposition rate, high chlorine content, film contamination, particle contamination, and non-uniform vaporization, leading to poor step coverage and thin film uniformity, especially when forming films on complex structures or at room temperature.

Method used

A film quality improving agent is used to form a shielding region for molybdenum-based thin films, adjusting the growth rate and reducing deposition rate, which includes molybdenum, molybdenum oxide, or molybdenum nitride, with specific chemical formulas to enhance film quality, and a method involving vaporization, purging, and reaction gas supply in a controlled environment.

Benefits of technology

The method improves step coverage, thin film thickness uniformity, and electrical properties by reducing process by-products, preventing corrosion, and enhancing crystallinity, suitable for complex structures and room temperature deposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540610000001_ABST
    Figure 2024540610000001_ABST
Patent Text Reader

Abstract

The present invention relates to a film quality improver, a thin film formation method using the same, and a semiconductor substrate and a semiconductor device manufactured therefrom. A compound having a specific structure is provided as a film quality improver, and a shielding region for a molybdenum-based thin film is formed on a substrate to reduce the deposition rate of the molybdenum-based thin film. By controlling the thin film growth rate, even when a thin film is formed on a substrate having a complex structure using a compound that is solid at room temperature, the step coverage and the thickness uniformity of the thin film can be significantly improved, corrosion and deterioration are reduced, and the crystallinity of the thin film is improved, thereby improving the electrical properties of the thin film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film quality improver, a method for forming a thin film using the same, and a semiconductor substrate and a semiconductor device manufactured therefrom. More particularly, the present invention relates to a film quality improver that significantly improves film quality such as step coverage, thin film thickness uniformity, and resistivity when a thin film is formed on a substrate having a complex structure by forming a shielding region for the molybdenum-based thin film on the substrate and appropriately controls the thin film growth rate, and when a thin film is formed at room temperature using a solid precursor, the film quality improver, a method for forming a thin film using the same, and a semiconductor substrate manufactured therefrom. [Background technology]

[0002] Molybdenum (Mo) has excellent chemical and thermal stability, high electrical conductivity and low electrical resistivity (ρ=0.57X10 -5 Recently, it has been attracting attention as a material that meets the demands for miniaturization of elements, low power consumption, and high productivity.

[0003] Specifically, molybdenum (Mo) is used as an electrode, diffusion barrier, gas sensor, and catalyst material in various semiconductor and display metal processes. In particular, molybdenum-containing thin films are attracting attention as a two-dimensional semiconductor material that can replace graphene materials, and research into its applications is progressing rapidly.

[0004] A typical molybdenum compound used to form a molybdenum-containing thin film is molybdenum chloride (MoCl 5 However, according to Thin Solid Films, 166, 149 (1988), it has been reported that it has shortcomings such as low deposition rate, high chlorine content, and film contamination due to hydrogen chloride, etc. In particular, it has shortcomings such as particle contamination and inability to perform uniform precursor vaporization due to solid compounds.

[0005] In addition, Mo(NtBu) reported in Chem. Vap. Deposition (2008) 14, 71 2 (NiPR 2 ) 2 However, they have the disadvantages of being relatively poor in thermal stability, and due to the high stability of the imide ligand due to the π-bond between the molybdenum central metal and nitrogen, ligand decomposition does not occur well during the process, and carbon contamination is very serious.

[0006] U.S. Patent Publication 4,431,708 and J. dePhys. IV2(C2), 865 disclose the relatively high vapor pressure of Mo(CO). 6 Molybdenum-containing thin films formed by deposition using compounds have been reported, but these are likely to have low thermal stability and particle problems due to the non-uniform vaporization characteristics of solid compounds at room temperature.

[0007] Therefore, there is a need to develop a method for forming a thin film that does not contain halogens, which are likely to have a detrimental effect on semiconductor and display devices, and that is capable of forming a thin film with a complex structure even though it is in a solid form at room temperature, and that significantly improves step coverage and thin film thickness uniformity, as well as semiconductor substrates manufactured therefrom. Summary of the Invention [Problem to be solved by the invention]

[0008] In order to solve the above-mentioned problems of the prior art, the present invention aims to provide a film quality improver that reduces or increases the deposition rate of a molybdenum-based thin film by forming a shielding region for the molybdenum-based thin film on a substrate, appropriately controls the thin film growth rate to form a thin film on a substrate having a complex structure, and greatly improves film quality such as step coverage, thin film thickness uniformity, and resistivity when a thin film is formed at room temperature using a solid precursor, a thin film formation method using the same, and a semiconductor substrate manufactured therefrom.

[0009] The present invention aims to improve the crystallinity of a thin film, thereby improving the density and electrical properties of the thin film.

[0010] The above and other objects of the present invention can all be achieved by the present invention described below. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention provides a film quality improver for a molybdenum-based thin film, comprising:

[0012] The molybdenum-based thin film comprises molybdenum, molybdenum oxide, or molybdenum nitride on a substrate;

[0013] The film quality improving agent is represented by the following chemical formula 1

[0014] [Chemical formula 1]

[0015] TIFF2024540610000002.tif6468

[0016] (A is carbon (C) or silicon (Si), and X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I),

[0017] R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I);

[0018] R 2 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I).

[0019] The film quality improving agent may have a refractive index (a) in the range of 1.38 to 1.72, and at the same time, a value (b / a) obtained by dividing the vapor pressure (25°C, mmHg, b) by the refractive index (a) may be in the range of 0.003 to 0.043.

[0020] The film quality improving agent is 1 H-NMR spectrum comparison The film quality improver and molybdenum precursor were mixed in a 1:1 molar ratio and pressurized, and then the measurement was performed. 1 The compound may have an integral value of less than 0.1% at the apex of a newly generated peak in the H-NMR spectrum.

[0021] The molybdenum precursor here may be solid or liquid under conditions of 20° C. and 1 bar.

[0022] The film quality improver may provide a shielding region for the molybdenum-based thin film.

[0023] The molybdenum-based thin film shielding region may be formed on a substrate on which the molybdenum-based thin film is formed.

[0024] The shielding region for the molybdenum-based thin film does not remain in the molybdenum-based thin film, and the molybdenum-based thin film may contain carbon, silicon and halogen compounds in an amount of 1% or less.

[0025] The molybdenum-based thin film may be used as a diffusion barrier or an electrode.

[0026]

[0027] The present invention also relates to a compound represented by the following formula 1:

[0028] [Chemical formula 1]

[0029] TIFF2024540610000003.tif6373

[0030] (A is carbon (C) or silicon (Si), X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 2 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I).

[0031] The method for forming a molybdenum-based thin film may include the steps of: i) vaporizing the film quality improving agent to form a shielding region on a surface of a substrate loaded into a chamber; ii-a) primarily purging the interior of the chamber with a purge gas; iii-a) vaporizing a molybdenum precursor and adsorbing it in a region outside the shielding region; iv-a) secondly purging the interior of the chamber with a purge gas; va) supplying a reaction gas into the chamber; and vi-a) thirdly purging the interior of the chamber with a purge gas.

[0032] The method for forming a molybdenum-based thin film may further include the steps of: ib) vaporizing a molybdenum precursor and adsorbing the precursor on a surface of a substrate loaded in a chamber; ii-b) primarily purging the interior of the chamber with a purge gas; iii-b) vaporizing the film quality improving agent and injecting the vaporized film quality improving agent onto a surface of a substrate loaded in the chamber; iv-b) secondary purging the interior of the chamber with a purge gas; vb) supplying a reaction gas into the chamber; and vi-b) tertiary purging the interior of the chamber with a purge gas.

[0033] The molybdenum precursor may be a solid or liquid under conditions of 20° C. and 1 bar, and may be a molybdenum precursor having a vapor pressure of 0.1 mTorr to 100 Torr at 30° C.

[0034] The molybdenum precursor may be at least one selected from the compounds represented by the following Formulas 2 to 36:

[0035] [Chemical Formula 2 to Chemical Formula 19]

[0036] TIFF2024540610000004.tif153164

[0037] [Chemical formula 20 to chemical formula 32]

[0038] TIFF2024540610000005.tif107165

[0039] [Chemical formula 33 to chemical formula 36]

[0040] TIFF2024540610000006.tif51148

[0041] (In Formula 2 to Formula 36, ​​the lines are bonds, the points where bonds that do not specify other elements intersect are carbons, hydrogens that satisfy the valence of the carbons are omitted, and R' and R" are each hydrogen or an alkyl group having 1 to 5 carbons, and R' may be linked to the adjacent R'.)

[0042]

[0043] The chamber may be an ALD chamber or a CVD chamber.

[0044] The film quality improving agent or the molybdenum precursor may be vaporized and injected, and then a plasma post-treatment may be performed.

[0045] In the steps ii) and iv), the amount of the purge gas introduced into the chamber may be 10 to 100,000 times the volume of the film improving agent introduced.

[0046] The reaction gas, the film quality improving agent, and the molybdenum precursor may be delivered into the chamber by a VFC method, a DLI method, or an LDS method.

[0047] The substrate loaded in the chamber may be heated to 50 to 400° C., and the ratio of the film quality improving agent and the molybdenum precursor input into the chamber (mg / cycle) may be 1:1.5 to 1:20.

[0048] The reactive gas may be a reducing agent, a nitriding agent or an oxidizing agent.

[0049] The molybdenum-based thin film forming method may be performed at a deposition temperature of 50 to 700°C.

[0050] The molybdenum-based thin film may be an oxide film, a nitride film, or a metal film.

[0051]

[0052] The present invention also provides a semiconductor substrate which is manufactured by the above-mentioned method for forming a molybdenum-based thin film.

[0053] The molybdenum-based thin film may have a multi-layer structure of two or three layers.

[0054]

[0055] The present invention also provides a semiconductor device including the semiconductor substrate described above.

[0056] The semiconductor substrate may be low resistive metal gate interconnects, high aspect ratio 3D metal-insulator-metal (MIM) capacitors, DRAM trench capacitors, 3D Gate-All-Around (GAA), or 3D NAND. Effect of the Invention

[0057] According to the present invention, there is an effect of providing a film quality improver that reduces the deposition rate of a molybdenum-based thin film by forming a shielding region for the molybdenum-based thin film on a substrate, controls the thin film growth rate, and improves step coverage even when a thin film is formed from a solid compound at room temperature on a substrate having a complex structure.

[0058] In addition, during the formation of the thin film, process by-products are more effectively reduced, corrosion and deterioration are prevented, and the crystallinity of the thin film is improved, thereby improving the electrical properties of the thin film.

[0059] In addition, the amount of process by-products during thin film formation can be reduced, improving step coverage and thin film density, and thus providing a thin film formation method using the same and a semiconductor substrate manufactured therefrom. [Brief description of the drawings]

[0060] [Figure 1] FIG. 11 is a graph comparing the results of an experiment in which the film quality improving agent proposed by the present invention was pre-injected and post-injected into MoO2Cl2, and the results of Example 6 in which the film quality improving agent was not used. The left side is a graph showing the measurement results of resistivity, and the right side is a graph showing the measurement results of deposition rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0061]

[0062] The film quality improver for molybdenum-based thin films described herein, the method for forming a molybdenum-based thin film using the same, and the semiconductor substrate produced therefrom will be described in detail below.

[0063] In this description, the term "shielding" means, unless otherwise specified, not only reducing, preventing or blocking molybdenum precursors for forming molybdenum-based thin films from being adsorbed onto a substrate, but also reducing, preventing or blocking process by-products from being adsorbed onto a substrate.

[0064] The present inventors have confirmed that when a film quality improver that blocks molybdenum precursors for forming a molybdenum-based thin film on a substrate surface loaded into a chamber is used, a blocking region that does not remain in the molybdenum-based thin film is formed to form a relatively rough thin film, and the growth rate of the formed thin film is controlled, so that even if the thin film is applied to a substrate with a complex structure, the uniformity of the thin film is ensured and the step coverage is greatly improved, and in particular, it is possible to deposit a thin film, and the amount of halide remaining as a process by-product and the amount of carbon that is difficult to reduce even when excessive hydrogen gas is used are improved. Based on this, the present invention has been completed by conducting research into a film quality improver that provides a blocking region.

[0065]

[0066] The film quality improver of the present invention provides a film quality improver for molybdenum-based thin films.

[0067] The molybdenum-based thin film may be provided as one or more precursors selected from compounds represented by the following Formulae 2 to 36, for example, and in this case, the effects to be achieved by the present invention can be sufficiently obtained.

[0068] [Chemical Formula 2 to Chemical Formula 19]

[0069] TIFF2024540610000007.tif150159

[0070] [Chemical formula 20 to chemical formula 32]

[0071] TIFF2024540610000008.tif110165

[0072] [Chemical formula 33 to chemical formula 36]

[0073] TIFF2024540610000009.tif54161

[0074] (In Formula 2 to Formula 36, ​​the lines are bonds, the points where bonds that do not specify other elements intersect are carbons, hydrogens that satisfy the valence of the carbons are omitted, and R' and R" are each hydrogen or an alkyl group having 1 to 5 carbons, and R' may be linked to the adjacent R'.)

[0075] The molybdenum-based thin film may be used not only as a diffusion barrier film which is generally used, but also as an electrode in a semiconductor device.

[0076]

[0077] The film quality improving agent is represented by the following chemical formula 1

[0078] [Chemical formula 1]

[0079] TIFF2024540610000010.tif6371

[0080] (A is carbon (C) or silicon (Si), X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 2are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I). In this case, when a molybdenum-based thin film is formed, a shielding region that does not remain in the molybdenum-based thin film is formed to form a relatively rough thin film, and at the same time, side reactions are suppressed to control the thin film growth rate, and by-products in the thin film process are reduced, thereby reducing corrosion and deterioration, and the crystallinity of the thin film is improved, and even when a thin film is formed on a substrate having a complex structure, step coverage and thickness uniformity of the thin film are greatly improved.

[0081] In the above Chemical Formula 1, A is carbon or silicon, and is preferably carbon.

[0082] R 1 , R 2 and R 3 are each independently an alkyl group having 1 to 3 carbon atoms, and at least one of them has 2 or 3 carbon atoms. 1 , R 2 and R 3 Any one of the R has 1 carbon atom, and the remaining two have 2 or 3 carbon atoms. More preferably, the R 1 , R 2 and R 3 The carbon number of one of them is 1, and the carbon numbers of the remaining two are 2. Within this range, there are advantages in that the effect of reducing process by-products is large, step coverage is excellent, the effect of improving thin film density, and the electrical properties of the thin film are more excellent.

[0083] In the formula 1, X is a halogen element, and is preferably fluorine, chlorine or bromine, and more preferably chlorine or bromine, and within this range, there are advantages in that the reduction of process by-products and the improvement of step coverage are more excellent. In addition, X may be, for example, fluorine, which is advantageous in that it is more suitable for processes requiring high temperature deposition.

[0084] In Formula 1, X may be iodine as another preferred example. Within this range, the thin film crystallinity is improved, and side reactions are suppressed to reduce process by-products.

[0085]

[0086] The compound represented by Chemical Formula 1 is a halogen-substituted tertiary alkyl compound, and specific examples thereof include 2-chloro-2-methylpropane, 2-chloro-2-methylbutane, 2-chloro-2-methylpentane, 3-chloro-3-methylpentane, 3-chloro-3-methylhexane, 3-chloro-3-ethylpentane, 3-chloro-3-ethylhexane, 4-chloro-4-methylheptane, 4-chloro-4-ethylheptane, 4-chloro-4-propylheptane, 2-bromo-2-methylpropane, 2-bromo-2-methylbutane, 2-bromo-2-methylhexane ... Pentane, 3-bromo-3 methylpentane, 3-bromo-3 methylhexane, 3-bromo-3 ethylpentane, 3-bromo-3 ethylhexane, 4-bromo-4 methylheptane, 4-bromo-4 ethylheptane, 4-bromo-4 propylheptane, 2-iodo-2 methylpropane, 2-iodo-2 methylbutane, 2-iodo-2 methylpentane, 3-iodo-3 methylpentane, 3-iodo-3 methylhexane, 3-iodo-3 ethylpentane, 3-iodo-3 ethylhexane, 4-iodo-4 methylheptane, 4-iodo-4 ethylheptane The fluorocarbon ether is at least one selected from the group consisting of 2-chloro-2-methylpropane, 2-chloro-2-methylbutane, 2-fluoro-2-methylpentane, 3-fluoro-3-methylpentane, 3-fluoro-3-methylhexane, 3-fluoro-3-ethylpentane, 3-fluoro-3-ethylhexane, 4-fluoro-4-methylheptane, 4-fluoro-4-ethylheptane, and 4-fluoro-4-propylheptane, and is preferably at least one selected from the group consisting of 2-chloro-2-methylpropane, 2-chloro-2-methylbutane, and 3-chloro-3 The molybdenum thin film may be formed by depositing a molybdenum thin film on a substrate, and may be formed by depositing a molybdenum thin film on a substrate. The molybdenum thin film ...

[0087]

[0088] The compound represented by Formula 1 may be, for example, a saturated compound having a refractive index (a) in the range of 1.38 to 1.72 and a vapor pressure (mmHg, b) measured at 25° C. divided by the refractive index (a) (b / a) in the range of 0.003 to 0.043. In this case, a shielding region for the molybdenum-based thin film is formed on the substrate to reduce the deposition rate of the molybdenum-based thin film, and the thin film growth rate is controlled to significantly improve step coverage and thin film thickness uniformity even when a thin film is formed on a substrate having a complex structure, and the adsorption of not only the thin film precursor but also process by-products is prevented, thereby effectively protecting the surface of the substrate and effectively removing the process by-products.

[0089] In the present invention, the refractive index can be measured by a method known in the art unless otherwise specified. As a specific example, it can be measured at 25° C. using an Abbe refractometer based on ASTM D542.

[0090] The compound represented by Formula 1 may be, for example, a saturated compound having a refractive index (a) of 1.385 to 1.72 and a vapor pressure (mmHg, b) measured at 25° C. divided by the refractive index (a) of 0.032 to 0.043 (b / a), and preferably a saturated compound having a refractive index (a) of 1.388 to 1.719 and a vapor pressure (mmHg, b) measured at 25° C. divided by the refractive index (a) of 0.0035 to 0.043 (b / a). In this case, a shielding region for a molybdenum-based thin film is formed on a substrate to reduce the deposition rate of the molybdenum-based thin film, and the thin film growth rate is controlled to significantly improve step coverage and thin film thickness uniformity even when a thin film is formed on a substrate having a complex structure, and the adsorption of not only the thin film precursor but also process by-products is prevented, thereby effectively protecting the surface of the substrate and effectively removing the process by-products.

[0091]

[0092] The reactivity of the film quality improver and the molybdenum precursor is expressed as the impurity content (%) of less than 0.1% when the integrated value of the NMR peak apex generated by comparing the H-NMR spectrum measured before mixing the film quality improver and the molybdenum precursor with the H-NMR spectrum measured after pressurizing a 1:1 molar mixture for 1 hour is taken as the impurity content. When the film quality improver is used, the adsorption of the molybdenum precursor is not hindered, and the deposition rate is adjusted while reducing process by-products, thereby controlling the thin film growth rate, and even when a thin film is formed on a substrate having a complex structure, the step coverage and film quality can be improved, and the crystallinity of the thin film can be improved by preventing corrosion and deterioration, thereby improving the resistivity and electrical properties of the thin film.

[0093] Due to the above-mentioned reactivity, the film quality improver has the advantage that it can easily adjust the viscosity and vapor pressure of the molybdenum precursor and does not interfere with the behavior of the molybdenum precursor.

[0094] An example of a film quality improver exhibiting such reactivity may be a halogen-substituted straight or branched chain alkane compound or cycloalkane compound.

[0095] Specific examples include one or more selected from the group consisting of 1-iodobutane, 2-iodobutane, 2-iodo-3-methylbutane, 3-iodo-2,4-dimethylpentane, cyclohexyl iodide, cyclopentyl iodide, 1-bromobutane, 2-bromobutane, 2-bromo-3-methylbutane, 3-bromo-2,4-dimethylpentane, cyclohexyl bromide, and cyclopentyl bromide, and preferably one or more selected from the group consisting of 1-iodobutane and 2-iodobutane. In this case, there are advantages in that the adsorption of the molybdenum precursor is not hindered, and the substrate surface is effectively protected as a film quality improving agent, and process by-products are effectively removed.

[0096]

[0097] The film quality improving agent is characterized in that it does not remain in the molybdenum-based thin film.

[0098] In this case, unless otherwise specified, "not remaining" refers to the presence of C element at 1.0 atomic % (atom %), Si element at less than 1.0 atomic % (atom %), N element at less than 1.0 atomic % (atom %), and halogen elements at less than 1.0 atomic % (atom %) when analyzed by XPS.

[0099]

[0100] The molybdenum-based thin film may be used as a diffusion barrier or an electrode, but is not limited thereto.

[0101] The film quality improving agent may preferably be a compound having a purity of 99.9% or more, a compound having a purity of 99.95% or more, or a compound having a purity of 99.99% or more. For reference, when a compound having a purity of less than 99% is used, impurities may be formed, so it is preferable to use a substance having a purity of 99% or more as much as possible.

[0102]

[0103] The compound represented by Formula 1 is preferably used in an atomic layer deposition (ALD) process, and in this case, has the advantages of not interfering with the adsorption of a molybdenum precursor, effectively protecting the substrate surface as a film quality improver, and effectively removing process by-products.

[0104] The compound represented by the formula 1 is preferably liquid at room temperature (22° C.) and has a density of 0.8 to 2.5 g / cm 3 or 0.8 to 1.5 g / cm 3The vapor pressure (20°C) may be 0.1 to 300 mmHg or 1 to 300 mmHg, and the solubility in water (25°C) may be 200 mg / L or less. Within this range, a shielding region is effectively formed, and there is an effect of excellent step coverage, thin film thickness uniformity, and film quality improvement.

[0105] More preferably, the compound represented by Formula 1 has a density of 0.75 to 2.0 g / cm 3 or 0.8 to 1.3 g / cm 3 The vapor pressure (20°C) may be 1 to 260 mmHg, and the solubility in water (25°C) may be 160 mg / L or less. Within this range, a shielding region is effectively formed, and there is an effect of excellent step coverage, thin film thickness uniformity, and film quality improvement.

[0106]

[0107] In the method for forming a molybdenum-based thin film of the present invention,

[0108] [Chemical formula 1]

[0109] TIFF2024540610000011.tif6985

[0110] (A is carbon (C) or silicon (Si), X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I), and R 2 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), or iodine (I).) into a substrate and adsorbed on the substrate surface. In this case, a shielding region for a molybdenum-based thin film is formed on the substrate to reduce the deposition rate of the molybdenum-based thin film, and the thin film growth rate is controlled, so that even when a thin film is formed on a substrate having a complex structure, not only is step coverage and thin film thickness uniformity improved, but also a film quality improvement effect such as improved resistivity can be provided.

[0111] In the step of shielding the film quality improving agent on the substrate surface, the feeding time of the film quality improving agent on the substrate surface is preferably 0.01 to 5 seconds, more preferably 0.02 to 3 seconds, even more preferably 0.04 to 2 seconds, and even more preferably 0.05 to 1 second per cycle. Within this range, there are advantages in that the thin film growth rate is low, and step coverage and cost performance are excellent.

[0112] In this description, the feeding time of the film quality improving agent is based on a chamber volume of 15 to 20 L and a flow rate of 0.5 to 5 mg / s, and more specifically, on a chamber volume of 18 L and a flow rate of 1 to 2 mg / s.

[0113]

[0114] In a preferred embodiment, the method for forming a thin film may include the steps of: ia) vaporizing the film quality improving agent and shielding it on the surface of a substrate loaded in an ALD chamber; ii-a) first purging the inside of the chamber with a purge gas; iii-a) vaporizing a molybdenum precursor and adsorbing it on the surface of a substrate loaded in the chamber; iv-a) second purging the inside of the chamber with a purge gas; va) supplying a reaction gas into the chamber; and via) tertiary purging the inside of the chamber with a purge gas. In this case, the steps ia) to vi-a) may be repeated as a unit cycle until a thin film of a desired thickness is obtained. In this manner, when the film quality improving agent of the present invention is introduced before the molybdenum precursor in one cycle and adsorbed on the substrate, there are advantages that the thin film growth rate can be appropriately reduced even when deposition is performed at a high temperature, and the resistivity of the thin film is reduced by effectively removing the process by-products generated, and the step coverage is greatly improved.

[0115]

[0116] In another preferred embodiment, the method for forming a thin film may include steps ib) vaporizing a molybdenum precursor and adsorbing it on a surface of a substrate loaded in a chamber; ii-b) first purging the inside of the chamber with a purge gas; iii-b) vaporizing the film quality improving agent and adsorbing it on a surface of a substrate loaded in the chamber; iv-b) second purging the inside of the chamber with a purge gas; vb) supplying a reaction gas into the chamber; and vi-b) third purging the inside of the chamber with a purge gas. In this case, steps ib) to vi-b) may be used as a unit cycle, and the cycle may be repeated until a thin film of a desired thickness is obtained. In this way, when the film quality improving agent of the present invention is introduced after the molybdenum precursor in one cycle and adsorbed on the substrate, the film quality improving agent can act as a growth activator for thin film formation, and in this case, there are advantages in that the thin film growth rate is increased, the density and crystallinity of the thin film are increased, the resistivity of the thin film is reduced, and electrical properties are greatly improved.

[0117]

[0118] As a preferred example of the thin film formation method of the present invention, the film quality improving agent of the present invention may be added prior to the molybdenum precursor within one cycle to be adsorbed onto the substrate. In this case, even when the thin film is deposited at a high temperature, the thin film growth rate can be appropriately reduced, thereby significantly reducing process by-products and significantly improving step coverage. The crystallinity of the thin film can be increased to reduce the resistivity of the thin film. Even when applied to a semiconductor device having a large aspect ratio, the thickness uniformity of the thin film is significantly improved, ensuring the reliability of the semiconductor device.

[0119]

[0120] In the thin film formation method, for example, when the film quality improver is deposited before or after the deposition of the molybdenum precursor, the unit cycle may be repeated 1 to 99,999 times as necessary, preferably 10 to 10,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within these ranges, the desired thin film thickness can be obtained and the effects to be achieved by the present invention can be sufficiently obtained.

[0121] In the present invention, the chamber may be, for example, an ALD chamber or a CVD chamber.

[0122] In the present invention, the film quality improving agent or the molybdenum precursor may be vaporized and injected, followed by a plasma post-treatment, which can improve the thin film growth rate while reducing process by-products.

[0123]

[0124] In the case where the film quality improving agent is first adsorbed on the substrate and then the molybdenum precursor is adsorbed, or in the case where the film quality improving agent is first adsorbed on the substrate and then the molybdenum precursor is adsorbed, the amount of purge gas introduced into the chamber in the step of purging the unadsorbed film quality improving agent is not particularly limited as long as it is an amount sufficient to remove the unadsorbed film quality improving agent. For example, it may be 10 to 100,000 times, preferably 50 to 50,000 times, more preferably 100 to 10,000 times, and within this range, the unadsorbed film quality improving agent can be sufficiently removed to form a thin film evenly and prevent deterioration of the film quality. Here, the amounts of the purge gas and the film quality improving agent introduced are based on one cycle, and the volume of the film quality improving agent means the volume of the vaporized film quality improving agent.

[0125] As a specific example, when the film quality improving agent is injected at a flow rate of 1.66 mL / s and an injection time of 0.5 sec (per cycle), and a purge gas is injected at a flow rate of 166.6 mL / s and an injection time of 3 sec (per cycle) in the step of purging the unadsorbed film quality improving agent, the amount of purge gas injected is 602 times the amount of film quality improving agent injected.

[0126]

[0127] In addition, the amount of purge gas introduced into the ALD chamber in the step of purging the unadsorbed molybdenum precursor is not particularly limited as long as it is an amount sufficient to remove the unadsorbed molybdenum precursor. For example, the amount may be 10 to 10,000 times, preferably 50 to 50,000 times, more preferably 100 to 10,000 times, based on the volume of the molybdenum precursor introduced into the ALD chamber, and within this range, the unadsorbed molybdenum precursor can be sufficiently removed to form a thin film evenly and prevent deterioration of the film quality. Here, the amounts of the purge gas and the molybdenum precursor introduced are each based on one cycle, and the volume of the molybdenum precursor means the volume of the vaporized molybdenum precursor.

[0128]

[0129] In addition, in the purge step performed immediately after the reaction gas supply step, the amount of purge gas introduced into the ALD chamber may be, for example, 10 to 10,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times the volume of the reaction gas introduced into the ALD chamber, and the desired effect can be sufficiently obtained within this range. Here, the amounts of the purge gas and the reaction gas introduced are each based on one cycle.

[0130]

[0131] The film quality improving agent and the molybdenum precursor may be delivered into the ALD chamber preferably by a VFC method, a DLI method or an LDS method, and more preferably by an LDS method.

[0132] The substrate loaded in the chamber may be heated to, for example, 50 to 700° C., specifically, 300 to 700° C., and the film quality improver or molybdenum precursor may be injected onto the substrate in a heated or unheated state, or the heating conditions may be adjusted during the deposition process after being injected unheated according to deposition efficiency. For example, the film quality improver or molybdenum precursor may be injected onto the substrate at 50 to 700° C. for 1 to 20 seconds.

[0133]

[0134] The ratio of the amounts (mg / cycle) of the film quality improver and the molybdenum precursor fed into the chamber may be preferably 1:1.5 to 1:20, more preferably 1:2 to 1:15, even more preferably 1:2 to 1:12, and even more preferably 1:2.5 to 1:10. Within this range, the effect of improving step coverage and the effect of reducing process by-products are large.

[0135]

[0136] In the present invention, the molybdenum precursor may be mixed with a non-polar solvent and then introduced into the chamber. In this case, there is an advantage that the viscosity and vapor pressure of the molybdenum precursor can be easily adjusted.

[0137] The non-polar solvent may be at least one selected from the group consisting of alkanes and cycloalkanes. In this case, the non-polar solvent has the advantage of improving step coverage even when the deposition temperature is increased during thin film formation, while containing an organic solvent having low reactivity and solubility and easy moisture management.

[0138] As a more preferred example, the non-polar solvent may include a C1 to C10 alkane or a C3 to C10 cycloalkane, preferably a C3 to C10 cycloalkane, which has the advantages of low reactivity and solubility and easy moisture management.

[0139] In this description, C1, C3 etc. refer to carbon numbers.

[0140] The cycloalkane may be preferably a C3 to C10 monocycloalkane, and among the monocycloalkanes, cyclopentane is liquid at room temperature and has the highest vapor pressure, making it preferable for the vapor deposition process, but is not limited thereto.

[0141] The non-polar solvent has, for example, a solubility in water (25° C.) of 200 mg / L or less, preferably 50 to 400 mg / L, and more preferably 135 to 175 mg / L. Within this range, the non-polar solvent has the advantages of low reactivity with the molybdenum precursor and easy moisture management.

[0142] In the present description, the solubility is not particularly limited and may be determined according to the measurement method or standard commonly used in the technical field to which the present invention pertains. As an example, a saturated solution may be measured by the HPLC method.

[0143] The non-polar solvent may be contained in an amount of preferably 5 to 95% by weight, more preferably 10 to 90% by weight, even more preferably 40 to 90% by weight, and most preferably 70 to 90% by weight, based on the total weight of the molybdenum precursor and the non-polar solvent.

[0144] If the content of the non-polar solvent exceeds the upper limit, impurities are generated, and the number of impurities in the resistor and thin film increases. If the content of the organic solvent is less than the lower limit, the effect of improving step coverage and the effect of reducing impurities such as chlorine (Cl) ions by adding the solvent are not so good.

[0145]

[0146] In the molybdenum-based thin film formation method, for example, when the film quality improving agent is used, the decrease rate of the thin film growth rate per cycle (Å / cycle) calculated by the following Equation 1 is −5% or less, preferably −10% or less, more preferably −20% or less, even more preferably −30% or less, still more preferably −40% or less, and most preferably −45% or less. Within this range, the method has excellent step coverage and film thickness uniformity.

[0147] [Formula 1]

[0148] Thin film growth rate reduction rate per cycle (%) = [(thin film growth rate per cycle when using a film quality improvement agent - thin film growth rate per cycle when not using a film quality improvement agent) / thin film growth rate per cycle when not using a film quality improvement agent] x 100

[0149] In Equation 1, the thin film growth rate per cycle in the case where the film quality improving agent was used and in the case where the film quality improving agent was not used means the thin film deposition thickness (Å / cycle) per cycle, i.e., the deposition rate. For example, the deposition rate can be calculated as an average deposition rate by measuring the final thickness of the thin film by ellipsometry and then dividing the measured thickness by the total number of cycles.

[0150] In Equation 1, "when no film quality improving agent was used" refers to a case where a thin film is manufactured by adsorbing only a molybdenum precursor onto a substrate in a thin film deposition process. A specific example of the case is a case where a thin film is formed without adsorbing a film quality improving agent and purging unadsorbed film quality improving agent in the thin film formation method.

[0151]

[0152] In the molybdenum-based thin film forming method, the residual halogen intensity (c / s) in the thin film based on a thickness of 100 Å, as measured by SIMS, is preferably 100,000 or less, more preferably 70,000 or less, even more preferably 50,000 or less, and even more preferably 10,000 or less. In a preferred embodiment, it is 5,000 or less, more preferably 1,000 to 4,000, and even more preferably 1,000 to 3,800. Within such ranges, the effect of preventing corrosion and deterioration is excellent.

[0153] In this description, the purge is preferably 1,000 to 50,000 sccm (Standard Cubic Centimeter per Minute), more preferably 2,000 to 30,000 sccm, and even more preferably 2,500 to 15,000 sccm. Within this range, the thin film growth rate per cycle is appropriately controlled, and deposition is performed to a single atomic layer or close to it, which is advantageous in terms of film quality.

[0154]

[0155] The ALD (atomic layer deposition) process is highly advantageous in the fabrication of integrated circuits (ICs) that require high aspect ratios, and has advantages such as excellent conformality, uniformity, and precise thickness control due to its self-limiting thin film growth mechanism.

[0156] The thin film formation method may be carried out at a deposition temperature ranging from, for example, 50 to 800° C., preferably from 300 to 700° C., and more preferably from 350 to 650° C. Within this range, it is effective to grow a thin film with excellent film quality while implementing the characteristics of the ALD process.

[0157] The thin film forming method may be carried out at a deposition pressure ranging from 0.01 to 30 Torr, preferably from 0.1 to 30 Torr, more preferably from 1 to 30 Torr, and most preferably from 5 to 20 Torr, in order to obtain a thin film having a uniform thickness.

[0158] In this description, deposition temperature and deposition pressure can be measured as the temperature and pressure formed within a deposition chamber or as the temperature and pressure applied to a substrate within the deposition chamber.

[0159] The method for forming a molybdenum-based thin film may preferably include the step of raising the temperature in the chamber to a deposition temperature before introducing the film quality improving agent into the chamber; and / or the step of injecting an inert gas into the chamber to purge the chamber before introducing the film quality improving agent into the chamber.

[0160] The present invention may also include a thin film manufacturing apparatus capable of implementing the molybdenum-based thin film manufacturing method, the thin film manufacturing apparatus including an ALD chamber, a first vaporizer for vaporizing a film quality improving agent, a first transfer means for transferring the vaporized film quality improving agent into the ALD chamber, a second vaporizer for vaporizing a thin film precursor, and a second transfer means for transferring the vaporized thin film precursor into the ALD chamber. Here, the vaporizer and the transfer means are not particularly limited as long as they are vaporizers and transfer means commonly used in the technical field to which the present invention pertains.

[0161]

[0162] As a specific example, the method of forming the thin film will be described. First, a substrate on which a thin film is to be formed is placed in a deposition chamber capable of atomic layer deposition.

[0163] The substrate may include a semiconductor substrate, such as a silicon substrate, silicon oxide, or the like.

[0164] The substrate may further include a conductive layer or an insulating layer formed thereon.

[0165] In order to deposit a thin film on a substrate placed in the deposition chamber, the above-mentioned film quality improving agent and a molybdenum precursor, or a mixture thereof with a non-polar solvent, are prepared.

[0166] The prepared film quality improving agent is then injected into a vaporizer, converted into a vapor phase, and delivered to a deposition chamber to be adsorbed onto a substrate, and then purged to remove any unadsorbed film quality improving agent.

[0167] Next, the prepared molybdenum precursor or a mixture of the same and a non-polar solvent (thin film forming composition) is injected into a vaporizer, converted into a vapor phase, and delivered to a deposition chamber to be adsorbed onto a substrate, and unadsorbed molybdenum precursor / thin film forming composition is purged.

[0168] In the present description, the steps of adsorbing the film quality improving agent onto a substrate and then purging to remove any unadsorbed film quality improving agent; and adsorbing a molybdenum precursor onto a substrate and purging to remove any unadsorbed molybdenum precursor may be performed in a different order as necessary.

[0169] In this description, the method of delivering the film quality improver and the molybdenum precursor (thin film forming composition) to the deposition chamber may be, for example, a method of delivering a vaporized gas using a vapor flow controller (MFC) method (Vapor Flow Control; VFC) or a method of delivering a liquid using a liquid mass flow controller (LMFC) method (Liquid Delivery System; LDS), and preferably, the LDS method is used.

[0170] At this time, the carrier gas or dilution gas for moving the film quality improving agent and the molybdenum precursor onto the substrate is argon (Ar), nitrogen (N 2 ), helium (He), or a mixture of two or more gases may be used, but is not limited thereto.

[0171] In the present description, the purge gas may be, for example, an inert gas, and preferably, the carrier gas or dilution gas.

[0172]

[0173] Next, a reaction gas is supplied. The reaction gas is not particularly limited as long as it is a reaction gas commonly used in the technical field to which the present invention belongs, and may preferably contain a reducing agent, a nitriding agent, or an oxidizing agent. The nitriding agent reacts with the molybdenum precursor adsorbed on the substrate to form a nitride film, the reducing agent reacts with the molybdenum precursor adsorbed on the substrate to form a metal film, and the oxidizing agent reacts with the molybdenum precursor adsorbed on the substrate to form an oxide film.

[0174] Preferably, the nitriding agent is nitrogen gas (N 2 ), hydrazine gas (N 2 H 4), or a mixture of nitrogen gas and hydrogen gas, and the oxidant is oxygen gas (O 2 ), ozone gas or a mixture of oxygen gas and ozone gas, and the reducing agent may be hydrogen gas (H 2 ) etc.

[0175] In the thin film formation method, the deposition temperature is, for example, 50 to 800° C., preferably 200 to 700° C., and specific examples are 250 to 500° C., 250 to 450° C., 380 to 420° C., or 400 to 450° C., and within this range, there is an advantage that the thin film resistivity, step coverage, etc. are greatly improved.

[0176] Next, the remaining unreacted reactant gas is purged with an inert gas, which removes not only the excess reactant gas but also any by-products that are produced.

[0177] As described above, the molybdenum-based thin film forming method may, for example, include a unit cycle including a step of shielding a film quality improving agent on a substrate, a step of purging unadsorbed film quality improving agent, a step of adsorbing a molybdenum precursor / a thin film forming composition on a substrate, a step of purging unadsorbed molybdenum precursor / a thin film forming composition, a step of supplying a reaction gas, and a step of purging remaining reaction gas, and the unit cycle may be repeated to form a thin film of a desired thickness.

[0178] In another example, the molybdenum-based thin film forming method may have a unit cycle including a step of adsorbing a molybdenum precursor / a composition for forming a thin film on a substrate, a step of purging unadsorbed molybdenum precursor / a composition for forming a thin film, a step of adsorbing a film quality improving agent on a substrate, a step of purging unadsorbed film quality improving agent, a step of supplying a reactive gas, and a step of purging remaining reactive gas, and the unit cycle may be repeated to form a thin film of a desired thickness.

[0179] The unit cycle may be repeated, for example, 1 to 99,999 times, preferably 10 to 1,000 times, more preferably 50 to 5,000 times, and even more preferably 100 to 2,000 times, and within this range, the desired thin film characteristics are effectively expressed.

[0180]

[0181] The present invention also provides a semiconductor substrate, which is manufactured by the method for forming a molybdenum-based thin film described herein. In this case, the thin film has excellent step coverage and thickness uniformity, and has excellent density and electrical properties.

[0182]

[0183] The thin film thus produced preferably has a thickness of 20 nm or less, a resistivity of 0.1 to 400 μΩ cm based on a 10 nm thin film thickness, a halogen content of 10,000 ppm or less, and a step coverage rate of 90% or more. Within these ranges, the thin film has excellent performance as a diffusion barrier film and is effective in reducing corrosion of metal wiring materials, but is not limited thereto.

[0184] The thin film may have a thickness of, for example, 1 to 20 nm, preferably 1 to 20 nm, more preferably 3 to 25 nm, and even more preferably 5 to 20 nm, and within this range, there is an effect that the thin film characteristics are excellent.

[0185] For example, the thin film may have a resistivity of 0.1 to 400 μΩ cm, preferably 15 to 300 μΩ cm, more preferably 20 to 290 μΩ cm, and even more preferably 25 to 280 μΩ cm based on a thin film thickness of 10 nm, and within this range, there is an effect that the thin film characteristics are excellent.

[0186] The thin film may have a halogen content of preferably 10,000 ppm or less, or 1 to 9,000 ppm, more preferably 5 to 8,500 ppm, and even more preferably 100 to 1,000 ppm. Within this range, the thin film has excellent thin film properties while reducing the thin film growth rate. Here, the halogen remaining in the thin film is, for example, Cl. 2 , Cl, or Cl - The lower the residual halogen content in the thin film, the better the film quality, which is preferable.

[0187] The thin film has, for example, a step coverage rate of 90% or more, preferably 92% or more, and more preferably 95% or more. Within this range, even thin films with complex structures can be easily deposited onto a substrate, and this has the advantage that they can be applied to next-generation semiconductor devices.

[0188] In the present invention, unless otherwise specified, the step coverage may be calculated in a manner known in the art. For example, the thickness of a thin film deposited on an upper portion (top deposition thickness) and the thickness of a thin film deposited on a side portion (side deposition thickness) may be measured, and the top deposition thickness may be divided by the side deposition thickness to be expressed as a percentage.

[0189] The thin film has, for example, a resistivity of 1500 μΩ.cm or less, preferably 1400 μΩ.cm or less, and more preferably 1300 μΩ.cm or less, and the smaller the value, the more preferable. Within this range, thin films with complex structures can provide the electrical characteristics required, and have the advantage of being applicable to next-generation semiconductor devices.

[0190]

[0191] The thin film thus produced may include, for example, a molybdenum film, a molybdenum oxide film, or a molybdenum nitride film, which is advantageous in that it is useful as a diffusion barrier film or an electrode for a semiconductor device.

[0192]

[0193] The thin film may have a multilayer structure of two or three layers as required, for example. The multilayer film having a two-layer structure may have a lower layer film-middle layer film structure, and the multilayer film having a three-layer structure may have a lower layer film-middle layer film-upper layer film structure.

[0194] The underlayer film is, for example, Si, SiO 2 , MgO, Al 2 O 3 , CaO, ZrSiO 4 , ZrO 2 , HfSiO 4 , Y 2 O 3 , HfO 2 , LaLuO 2 , Si 3 N 4 , SrO, La 2 O 3 , Ta 2 O 5 , BaO, TiO 2 It may comprise one or more selected from the group consisting of:

[0195] The intermediate layer is, for example, Ti x N y , preferably TN.

[0196] The upper layer film may contain, for example, one or more elements selected from the group consisting of W and Mo.

[0197]

[0198] In order to aid in the understanding of the present invention, preferred embodiments and drawings are presented below. The following embodiments and drawings are merely illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of ​​the present invention, and it is natural that such changes and modifications fall within the scope of the attached claims.

[0199]

[0200] [Example]

[0201] Examples 1 to 5, Comparative Examples 1 to 3, Reference Example 1

[0202] The combinations shown in Table 1 below were selected as the film quality improving agent and molybdenum precursor to be used in the experiments.

[0203] [Table 1]

[0204] Example 1

[0205] Among the compounds listed in Table 1 above, t-butyl iodide was used as a film quality improver, and the compound represented by formula 34, MoO 2 Cl 2 The prepared film quality improving agent and thin film precursor compound were each placed in a canister and supplied to a vaporizer heated to 150° C. at a flow rate of 0.05 g / min using a LMFC (Liquid Mass Flow Controller) at room temperature.

[0206] The film quality improving agent and the thin film precursor compound vaporized in the vapor phase by the vaporizer were each fed into the deposition chamber loaded with the Si substrate at a 1:1 feed ratio for 1 second, and then argon gas was supplied at 5000sccm for 2 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5Torr.

[0207] Next, 1000 sccm of ammonia was introduced into the reaction chamber as a reactive gas for 3 seconds, and then argon purging was performed for 3 seconds. At this time, the substrates on which the metal thin film was to be formed were heated to 380° C. as shown in Table 2 below. This process was repeated 200 to 400 times to form a MoN thin film, which is a self-limiting atomic layer having a thickness of 10 nm.

[0208]

[0209] Example 2

[0210] Among the compounds listed in Table 1 above, t-butyl iodide was used as a film quality improver, and the compound represented by formula 34, MoO 2 Cl 2 The prepared film quality improving agent and thin film precursor compound were each placed in a canister and supplied to a vaporizer heated to 150° C. at a flow rate of 0.05 g / min using a LMFC (Liquid Mass Flow Controller) at room temperature.

[0211] The film quality improving agent and the thin film precursor compound vaporized in the vapor phase by the vaporizer were each fed into the deposition chamber loaded with the Si substrate at a 1:1 feed ratio for 1 second, and then argon gas was supplied at 5000sccm for 2 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5Torr.

[0212] Next, 1000 sccm of ammonia was introduced into the reaction chamber as a reactive gas for 3 seconds, and then argon purging was performed for 3 seconds. At this time, the substrate on which the metal thin film was to be formed was heated to a temperature of 400° C. as shown in Table 2 below. This process was repeated 200 to 400 times to form a MoN thin film, which is a self-limiting atomic layer having a thickness of 10 nm.

[0213]

[0214] Example 3

[0215] Among the compounds listed in Table 1 above, t-butyl iodide was used as a film quality improver, and the compound represented by formula 34, MoO 2 Cl 2 The prepared film quality improving agent and thin film precursor compound were each placed in a canister and supplied to a vaporizer heated to 150° C. at a flow rate of 0.05 g / min using a LMFC (Liquid Mass Flow Controller) at room temperature.

[0216] The film quality improving agent and the thin film precursor compound vaporized in the vapor phase by the vaporizer were each fed into the deposition chamber loaded with the Si substrate at a 1:1 feed ratio for 1 second, and then argon gas was supplied at 5000sccm for 2 seconds to perform argon purging. At this time, the pressure inside the reaction chamber was controlled at 2.5Torr.

[0217] Next, 1000 sccm of ammonia was introduced into the reaction chamber as a reactive gas for 3 seconds, and then argon purging was performed for 3 seconds. At this time, the substrates on which the metal thin film was to be formed were heated to 420° C. as shown in Table 2 below. This process was repeated 200 to 400 times to form a MoN thin film, which is a self-limiting atomic layer having a thickness of 10 nm.

[0218]

[0219] Comparative Examples 1 to 3

[0220] The same steps as in Examples 1 to 3 were repeated, except that no film quality improving agent was added.

[0221] As a result, a self-limiting atomic layer of MoN thin film with a thickness of 10 nm was formed.

[0222]

[0223] Example 4

[0224] The same process as in Example 1 was repeated, except that the film quality improving agent and the thin film precursor compound vaporized in the vapor phase in the vaporizer were sequentially fed in a 1:1 feed ratio into a deposition chamber loaded with a substrate for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging.

[0225] Specifically, the film quality improving agent vaporized in the vapor phase by the vaporizer was introduced into the deposition chamber with the substrate loaded for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging. Thereafter, the molybdenum precursor vaporized in the vapor phase by the vaporizer was introduced into the deposition chamber with the substrate loaded for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging.

[0226] As a result, a MoN thin film, which is a self-limiting atomic layer of 10 nm in thickness, was formed by repeating the process 200 to 400 times.

[0227]

[0228] Example 5

[0229] The same process as in Example 1 was repeated, except that the thin film precursor and the film quality improving agent vaporized in the vapor phase in the vaporizer were sequentially fed in a 1:1 feed ratio into a deposition chamber loaded with a substrate for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging.

[0230] Specifically, the molybdenum precursor vaporized in the vapor phase by the vaporizer was introduced into the deposition chamber with the substrate loaded for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging. Thereafter, the film quality improving agent vaporized in the vapor phase by the vaporizer was introduced into the deposition chamber with the substrate loaded for 1 second, and then argon gas was supplied at 5000 sccm for 2 seconds to perform argon purging.

[0231] As a result, a MoN thin film, which is a self-limiting atomic layer of 10 nm in thickness, was formed by repeating the process 200 to 400 times.

[0232]

[0233] Reference example 1

[0234] The same process as in Example 1 was repeated, except that t-butyl iodide was replaced with iodobutane as the film quality improving agent.

[0235] As a result, a MoN thin film was formed, which is a self-limiting atomic layer with a thickness of 10 nm.

[0236]

[0237] [Experimental Example]

[0238] 1) Deposition evaluation (deposition rate per cycle, GPC)

[0239] The deposition rate was evaluated by dividing the thickness of the thin film measured by an ellipsometer, a device that can measure optical properties such as the thickness and refractive index of a thin film using the polarization properties of light, by the number of cycles to calculate the thickness of the thin film deposited per cycle, and the results are shown in Table 2 below.

[0240]

[0241] 2) Thin film resistance evaluation (resistivity)

[0242] The surface resistance of the thin film was measured using a four-point probe method to obtain the sheet resistance, and the specific resistance (μΩ.cm) was calculated from the thickness of the thin film. The results are shown in Table 2 below.

[0243] [Table 2]

[0244] As shown in Table 2, when t-butyl iodide of the present invention was used as a film quality improver together with the thin film precursor compound (Examples 1 to 3), the deposition rate was equal to or similar to that when no film quality improver was used (Comparative Examples 1 to 3), while the resistivity was reduced to 919 to 1884 μΩ.cm. This confirmed that the thin film growth rate was appropriately controlled, thereby improving the electrical properties.

[0245] 3) Impurity reduction properties

[0246] In order to compare the reduction characteristics of impurities, i.e., process by-products, in the manufactured 10 nm-thick thin film, XPS (X-ray Photoelectron Spectroscopy) analysis was performed for the elements of (Ti), nitrogen (N), Cl (chlorine), carbon (C), and oxygen (O), and the results are shown in Table 3 below.

[0247] [Table 3]

[0248] As shown in Table 3, when the film quality improver according to the present invention was used simultaneously with the thin film precursor compound (Example 1), not only did the results show a similar level to when no film quality improver was used (Comparative Example 1), but also the Cl and C intensities were all reduced to the 0.01% level compared to when another film quality improver was used (Reference Example 1), demonstrating superior impurity reduction properties. In particular, in the case of Comparative Example 1, since no film quality improver was added, carbon should theoretically not be detected, but trace amounts of CO and / or CO contained in the thin film precursor compound, purge gas, and reaction gas were detected. 2 It can be seen that carbon, which is believed to be caused by the above, was detected, and it can be seen that in Example 1 of the present invention, the carbon intensity was reduced compared to Comparative Example 1, even though a film quality improver, which is a hydrocarbon compound, was added during thin film deposition, which means that the film quality improver of the present invention has excellent impurity reduction properties.

[0249] In particular, in Reference Example 1, a compound having a halide structure similar to the film quality improving agent of the present invention was added, but the impurity intensity was much higher than in Example 1 and Comparative Example 1, and it was confirmed that there was no effect of improving film quality.

[0250]

[0251] Furthermore, in order to confirm the effect of each injection step of the film quality improving agent, the following additional experiment was carried out.

[0252]

[0253] Example 6

[0254] MoO 2 Cl 2 was used as the Mo precursor and ALD deposition evaluation was performed using the VFC supply method.

[0255] MoO 2 Cl 2 The canister heating temperature was 90° C., and the deposition evaluation temperatures were 380° C., 400° C., and 420° C., respectively. The process pressure was 6 torr, and the flow rates of the ammonia reaction gas and Ar purge gas were all 1000 sccm.

[0256] In order to confirm the effect of improving resistivity and GPC, a MoN thin film was evaporated and compared.

[0257] Specifically, MoO 2 Cl 2 After injection, t-butyl iodide was injected after Ar purging, Ar was injected, NH3 reaction gas was injected, and then Ar was injected to perform an ALD deposition experiment (post-injection). 2 Cl 2 After Ar injection, NH 3 After conducting an ALD deposition experiment by changing the order of injecting the reaction gas and then Ar (first injection), the resistivity and deposition rate were measured using the method presented in the above experimental example. The resistivity and deposition rate were also measured in the same way for a MoN thin film fabricated as a control group without adding the film quality improver.

[0258] The results of each measurement are shown in Figure 1 below. 2 Cl 2 10 is a graph comparing the results of an experiment in which the membrane quality improving agent proposed by the present invention was pre-injected and post-injected with the results of Example 6, a control experiment in which no membrane quality improving agent was used.

[0259] As can be seen from FIG. 1 below, the resistivity shown in the left hand drawing was improved in both the pre-injection and post-injection compared to the control group, with the pre-injection showing the greatest improvement. The deposition rate shown in the right hand drawing was also improved further in the pre-injection, confirming that the pre-injection of the film quality improving agent has a more excellent effect than the post-injection.

Claims

1. A film quality improver for a molybdenum-based thin film, comprising: The molybdenum-based thin film comprises molybdenum metal, molybdenum oxide, or molybdenum nitride on a substrate; The film quality improving agent is represented by the following formula 1 [Chemical formula 1] (A is carbon (C) or silicon (Si), X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I); The R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I); The R 2 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I).

2. 2. The film quality improver for molybdenum-based thin films according to claim 1, wherein the film quality improver has a refractive index (a) in the range of 1.38 to 1.72, and a vapor pressure (25° C., mmHg, b) divided by the refractive index (a) (b / a) in the range of 0.003 to 0.

043.

3. The film quality improver was measured after mixing the film quality improver and a molybdenum precursor in a molar ratio of 1:1 and applying pressure. 1 2. The film quality improver for a molybdenum-based thin film according to claim 1, wherein the molybdenum precursor is a solid or liquid under conditions of 20° C. and 1 bar, and wherein the integrated value of the apex of a newly generated peak in a H-NMR spectrum is less than 0.1%.

4. 2. The film quality improver for a molybdenum-based thin film according to claim 1, wherein the film quality improver does not remain on the molybdenum-based thin film.

5. 2. The film quality improver for a molybdenum-based thin film according to claim 1, wherein the molybdenum-based thin film is used as a diffusion barrier film or an electrode.

6. The following chemical formula 1 [Chemical formula 1] (A is carbon (C) or silicon (Si), X is fluorine (F), chlorine (Cl), bromine (Br) or iodine (I); The R 1 and R 3 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I); The R 2 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br), iodine (I), or a group of the formula BR 4 R 5 R 6 wherein B is carbon or silicon, and R 4 , R 5 and R 6 are independently hydrogen, an alkyl group having 1 to 5 carbon atoms, fluorine (F), chlorine (Cl), bromine (Br) or iodine (I).

7. 7. The method of claim 6, wherein the thin film is an oxide film, a nitride film or a metal film.

8. 7. The method of claim 6, wherein the film quality improving agent is delivered into the chamber by a VFC method, a DLI method or an LDS method, and the chamber is an ALD chamber or a CVD chamber.

9. 7. The method of claim 6, further comprising the steps of: i-a) vaporizing the film quality improving agent to form a shielding region on a surface of a substrate loaded into a chamber; ii-a) primarily purging the interior of the chamber with a purge gas; iii-a) vaporizing a molybdenum precursor and adsorbing it in a region outside the shielding region; iv-a) secondly purging the interior of the chamber with a purge gas; v-a) supplying a reaction gas into the chamber; and vi-a) thirdly purging the interior of the chamber with a purge gas.

10. 7. The method of claim 6, further comprising the steps of: i-b) vaporizing a molybdenum precursor and adsorbing it onto a surface of a substrate loaded in a chamber; ii-b) primarily purging the interior of the chamber with a purge gas; iii-b) vaporizing the film quality improving agent and injecting it onto a surface of a substrate loaded in the chamber; iv-b) secondly purging the interior of the chamber with a purge gas; v-b) supplying a reaction gas into the chamber; and vi-b) thirdly purging the interior of the chamber with a purge gas.

11. A semiconductor substrate produced by the molybdenum-based thin film forming method according to claim 6.

12. 12. The semiconductor substrate according to claim 11, wherein the molybdenum-based thin film has a multi-layer structure of two or three layers.

13. A semiconductor device comprising the semiconductor substrate of claim 11.

Citation Information

Patent Citations

  • Thin film manufacturing method, and thin film manufacturing apparatus

    JP2021050410A

  • Position adjustment assembly for adjusting combined position of jig pin

    KR1020210138334A

  • Growth inhibitor for forming thin film, method for forming thin film and semiconductor substrate prepared therefrom

    KR102254394B1

  • Halogen-Containing Silane-Based Metal Silicide As Nucleation Layer For Tungsten ALD

    US20170350013A1

  • Gap fill methods using catalyzed deposition

    WO2021183728A1