Polyimide powder with improved conductivity using graphene and its manufacturing method

By polymerizing graphene with dianhydride and diamine monomers in a mixed organic solvent, the polyimide powder achieves electrical conductivity and prevents static charging with minimal impact on mechanical properties.

JP2024540617AInactive Publication Date: 2024-10-31PI ADVANCED MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024529994
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-11-30
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polyimide powders exhibit high surface resistance, leading to static charging issues, and adding conductive fillers to reduce this resistance results in decreased tensile strength and elongation.

Method used

Polymerizing graphene with dianhydride and diamine monomers in a mixed organic solvent to produce polyimide powder, ensuring good dispersibility and maintaining mechanical properties.

Benefits of technology

The resulting polyimide powder achieves electrical conductivity while minimizing decreases in tensile strength and elongation, with a surface resistance of 10^1 Ω/cm² or lower, preventing static electricity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540617000001
    Figure 2024540617000001
  • Figure 2024540617000002
    Figure 2024540617000002
  • Figure 2024540617000003
    Figure 2024540617000003
Patent Text Reader

Abstract

The present invention relates to a polyimide powder and a manufacturing method thereof. The polyimide powder according to the present invention is obtained by polymerizing a diamine monomer and a dianhydride monomer with graphene, thereby providing a polyimide powder that exhibits electrical conductivity and is antistatic while minimizing the decrease in tensile strength and elongation.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a graphene-based polyimide powder having improved conductivity and a method for preparing the same. [Background technology]

[0002] Generally, polyimide (PI) is a polymer of imide monomer formed by solution polymerization of dianhydride and diamine or diisocyanate, and has excellent mechanical properties such as strength, chemical resistance, weather resistance, and heat resistance due to the chemical stability of the imide ring. In addition, polyimide is in the spotlight as a highly functional polymer material that can be applied to a wide range of industrial fields such as electronics, communications, and optics due to its excellent electrical properties such as insulation properties and low dielectric constant.

[0003] Generally, polyimide is produced by first synthesizing the precursor polyamic acid by reacting dianhydride and diamine in a solvent, and then imidizing the polyamic acid in the next step, and the reaction solvent used is mainly a polar organic solvent such as N-methyl-2-pyrrolidone (NMP). This general method has two steps: polyamic acid production step and polyamic acid imidization step, and the process is complicated, the solvent is harmful, it is difficult to obtain high molecular weight polyimide, and there are problems such as the need for additional catalyst and high heat of over 300℃ in the imidization step.

[0004] On the other hand, polyimide has electrical properties such as insulating properties and low dielectric constant as mentioned above, but conventional polyimide powder has high surface resistance (>10 15 ) and has a high possibility of electrostatic charge. In order to reduce the high surface resistance of such conventional polyimide powder, a conductive filler is added, but when a large amount of the conductive filler is added, the tensile strength and elongation of the polyimide are reduced.

[0005] Therefore, research is currently required into a method that can exhibit electrical conductivity and prevent static electricity while minimizing the decrease in tensile strength and elongation of polyimide. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to solve the problems and technical issues of the prior art as described above.

[0007] The present invention provides a polyimide powder capable of exhibiting electrical conductivity and preventing static electricity while minimizing the decrease in tensile strength and elongation of polyimide, and a method for producing the same. [Means for solving the problem]

[0008] The present invention relates to a polyimide powder and a method for producing the same.

[0009] The polyimide powder according to the present invention has polymerized units of a dianhydride monomer component and a diamine monomer component.

[0010] Conventional polyimide powders have high surface resistance (>10 15 ) and thus has a high possibility of electrostatic charge. In order to reduce the high surface resistance of such conventional polyimide powder, conductive fillers are added, but when a large amount of the conductive filler is added, the tensile strength and elongation of the polyimide are reduced.

[0011] The present invention provides a polyimide powder that exhibits electrical conductivity and is antistatic while minimizing the decrease in tensile strength and elongation by polymerizing a dianhydride monomer component and a diamine monomer component together with graphene.

[0012] A method for preparing a polyimide powder according to an embodiment of the present invention includes the steps of: preparing a polyamic acid solution by solution-polymerizing a dianhydride monomer and a diamine monomer in an organic solvent containing graphene; heating the polyamic acid solution to prepare a polyimide mixture; and filtering and drying a precipitate present in the mixture to obtain a polyimide powder.

[0013] In the past, polyimide powder was manufactured by dispersing a dianhydride monomer and a diamine monomer in an aqueous solvent to prepare a dispersion, and then heat-treating the dispersion. However, when the aqueous solvent further contains graphene to prepare a dispersion, there was a problem that hydrophobic graphene aggregated in the dispersion and the dispersibility was reduced.

[0014] In the method for producing a polyimide powder according to an embodiment of the present invention, a dianhydride monomer, a diamine monomer, and graphene are dispersed in a mixed organic solvent to form a polymerization solution (varnish), which is then heat-treated to produce a polyimide powder, thereby providing good dispersibility of hydrophobic graphene.

[0015] The content of the graphene in the organic solvent may be, for example, 5 to 80 parts by weight, 7 to 60 parts by weight, 8 to 55 parts by weight, or 10 to 50 parts by weight, based on 100 parts by weight of the total of the dianhydride monomer and the diamine monomer. If the content of graphene is too low, it is difficult to obtain a desired surface resistance, and if the content is too high, mechanical properties such as tensile strength and elongation may decrease.

[0016] The organic solvent of the present invention may be a mixed solvent of an aprotic solvent and a protic solvent. When a mixed solvent is used, it has advantages of excellent moldability and processability compared to when an aprotic solvent or a protic solvent is used alone.

[0017] Without being bound by theory, it is believed that in the case of aprotic solvents, it acts as a kind of imidization catalyst, while in the case of protic solvents, it acts to grow the molecular weight.

[0018] The aprotic solvent is not particularly limited, but may be at least one selected from the group consisting of toluene, xylene, naphtha, anisole, cresol, ethylbenzene, propylbenzene, chlorobenzene, dichlorobenzene, trichlorobenzene, biphenyl, terphenyl, diphenyl ether, diphenyl sulfide, acetophenone, chlorinated biphenyl, and chlorinated diphenyl ether. The protic solvent is not particularly limited, but may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc), dimethylpropanamide (DMPA), N,N-dimethylacetamide (DEAc), 3-methoxy-N,N-dimethylpropanamide (KJCMPA), and gamma butyrolactone (GBL).

[0019] The mixed solvent may contain 10-50% by weight of aprotic solvent and 50-90% by weight of protic solvent. If the content of aprotic solvent is too small, imidization is not sufficiently performed in the heating process, moldability cannot be ensured, and the intrinsic viscosity (IV) is low. If the content is too large, the molecular weight of the polymerization liquid is formed too slowly (the chain is too small), and moldability cannot be ensured during subsequent molding of the molded product.

[0020] The step of preparing the polyamic acid solution may be carried out at 50 to 100°C, for example, 60 to 90°C, 65 to 85°C, or 70 to 80°C, and the step of preparing the polyimide mixture may be carried out at 160 to 200°C, for example, 170 to 190°C or 175 to 185°C.

[0021] If the heating temperature is lower than the above range, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability. Also, if the heating temperature is higher than the above range, the color of the powder may become dark and the particle size may increase.

[0022] The step of preparing the polyamic acid solution and / or the step of preparing the polyimide mixed solution may be performed under pressurized conditions, for example, at 1 to 10 bar. In particular, in one embodiment of the present invention, the dianhydride monomer, the diamine monomer, and graphene are dispersed in a mixed solvent and polymerized, so that the polymerization reaction may be performed under normal pressure or at a pressurized condition of 1 to 3 bar. The pressurization may be performed by injecting an inert gas into the reactor or using water vapor generated in the reactor. The inert gas may be nitrogen, argon, helium, neon, or the like.

[0023] If the pressure conditions are lower than the above range, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability.If the pressure conditions are higher than the above range, the color of the powder may become dark and the particle size may increase.

[0024] The reaction time for the step of preparing the polyamic acid solution and / or the step of preparing the polyimide mixture may be 1 to 20 hours, for example, 1 to 10 hours, 1 to 8 hours, 1 to 6 hours, or 1 to 4 hours.

[0025] If the reaction time is shorter than the above range, the reaction yield may decrease, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability. Also, if the reaction time is longer than the above range, the color of the powder may become dark and the particle size may increase.

[0026] The step of obtaining the polyimide powder includes filtering and drying a precipitate present in the mixture to obtain the polyimide powder.

[0027] The method of the filtration and drying is not particularly limited, and for example, vacuum drying or oven drying may be performed.

[0028] The dianhydride monomer is not particularly limited as long as it can react with the diamine monomer to form a polyimide. For example, the dianhydride monomer according to the present invention may include at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA) and p-phenylenebis(trimellitate anhydride) (TAHQ).

[0029] The diamine monomer is not particularly limited as long as it can react with the dianhydride monomer to form a polyamic acid. For example, the diamine monomer according to the present invention may include at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).

[0030] In this case, the molar ratio (b / a) representing the number of moles (b) of the diamine monomer component to the number of moles (a) of the dianhydride monomer component is not more than 1. For example, the upper limit of the molar ratio (b / a) of the diamine monomer component to the dianhydride monomer component may be 0.99 or less, 0.98 or less, 0.97 or less, 0.96 or less, or 0.95 or less, and the lower limit of the molar ratio may be 0.9 or more, 0.91 or more, 0.92 or more, 0.93 or more, or 0.94 or more, and specifically, the molar ratio of the diamine monomer component to the dianhydride monomer component may be 0.9 to 0.99, 0.93 to 0.99, 0.94 to 0.99, 0.95 to 0.99, 0.95 to 0.98, or 0.96 to 0.98.

[0031] For example, in the present invention, the number of moles of the diamine monomer component is less than the number of moles of the dianhydride monomer component. Stoichiometrically, the dianhydride monomer and the diamine monomer may be reacted in a 1:1 ratio to produce a polyimide, but the reaction is mainly carried out in the presence of a solvent and / or a catalyst, and at this time, a side reaction between the functional group of the solvent or catalyst and the diamine may occur. In general, the diamine is added in an excess amount, or the dianhydride and the diamine are added in equal moles.

[0032] The solid content in the mixed solvent may be 1 to 30% by weight. The solid content refers to the dianhydride monomer component and the diamine monomer component. For example, the solid content in the mixed solvent may be 1 to 20% or 10 to 20%. By having the above solid content, the intrinsic viscosity of the polyimide powder can be adjusted to have appropriate processability.

[0033] In particular, in the method for producing a polyimide powder according to an embodiment of the present invention, a dianhydride monomer component, a diamine monomer component, and graphene are dispersed in a mixed solvent to form a polymerization solution (varnish), which is then heat-treated to produce a polyimide powder. As a result, the polyimide powder has a higher intrinsic viscosity (>0.9 dL / g) than conventional aqueous polymerization methods, and has excellent moldability and processability.

[0034] A polyimide powder according to another embodiment of the present invention includes a polyimide matrix having polymerized units derived from dianhydride monomers and diamine monomers, and graphene dispersed within the polyimide matrix.

[0035] The graphene may be contained in an amount of 0.01 to 50 parts by weight, preferably 0.1 to 50 parts by weight, based on 100 parts by weight of the polyimide powder. The graphene may be contained during polymerization of the polyimide powder, or may be mixed in powder form with the polyimide powder.

[0036] The polyimide powder may have a tensile strength of 70 MPa or more as measured by ASTM D1708. For example, the polyimide powder according to the present invention may have a lower limit of the tensile strength of 60 MPa or more, 70 MPa or more, 80 MPa or more, or 90 MPa or more as measured by ASTM D1708, and an upper limit of the tensile strength of 110 MPa or less, or 105 MPa or less.

[0037] The polyimide powder may have an elongation of 7% or more as measured by ASTM D1708. For example, the polyimide powder according to the present invention may have a lower limit of elongation of 7% or more, 7.5% or more, or 8% or more as measured by ASTM D1708, and an upper limit of elongation of 10% or less, or 15% or less.

[0038] The polyimide powder has a surface resistivity of 10 9 Ω / cm 2 Below, 10 7 Ω / cm 2 Below, 10 5 Ω / cm 2 Below, 10 3 Ω / cm 2 Less than or equal to 10 2 Ω / cm 2 For example, the polyimide powder according to the present invention may have a surface resistance of 10 or less as measured by ASTM D257. 1 Ω / cm 2 or more, and the upper limit of the surface resistance is 10 9Ω / cm 2 It may be the following.

[0039] The present invention also provides a method for producing a polyimide molded product, comprising the step of compressing and molding the polyimide powder described above.

[0040] The pressure molding step may be performed at a pressure of 30 to 1000 MPa, and may be performed at 200 to 400°C. The pressure molding step may be performed at room temperature, and may further include a step of sintering the pressure molded polyimide powder at 200 to 400°C. If the pressure is lower than the above range, the moldability of the powder during molding may be insufficient, and if it is higher, the processability of the molded product may be reduced. If the temperature is lower than the above range, the molecular fluidity may not be ensured, and the moldability may be significantly reduced, and if it is higher, some parts may be oxidized due to overheating.

[0041] The present invention further provides a molded article produced by using the polyimide powder. The polyimide powder produced by the present invention may be produced as a molded article by various molding methods, for example, compression molding, injection molding, slush molding, blow molding, extrusion molding or spinning methods may be used to produce the required molded article. The form of the molded article is not limited, and may be a film, sheet, pellet, tube, belt, injection molded article or extrusion molded article.

[0042] The polyimide powder produced by the present invention may be used in various fields such as electrical / electronic, semiconductor, display, automotive, medical, battery and aerospace. Effect of the Invention

[0043] The polyimide powder of the present application exhibits electrical conductivity and is antistatic, while minimizing the decrease in tensile strength and elongation.

[0044] The polyimide powder according to the present application has a molded product standard surface resistance of 10 1 Ω / cm 2 It is possible to reduce the temperature to below 50°C and prevent static electricity by exhibiting electrical conductivity.

[0045] In addition, the polyimide powder according to the present application contains graphene as a filler, and therefore, unlike other conductive fillers, it is possible to exhibit conductivity while maintaining an elongation of 6% or more. Therefore, it is possible to ensure the desired conductivity even when a small amount is added compared to other conductive fillers, and it is possible to minimize the decrease in tensile strength and elongation.

[0046] In addition, the polyimide powder according to the present application is produced by dispersing and polymerizing graphene in a high-boiling point mixed organic solvent, rather than by a conventional method of adding graphene to an aqueous solvent and polymerizing it. This allows for excellent dispersibility of graphene, making it possible to ensure the desired conductivity even when a small amount is added compared to other conductive fillers, and minimizes decreases in tensile strength and elongation.

[0047] However, the effects of the present invention are not limited to the effects mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the following description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0048] The present invention will be described in more detail below with reference to examples according to the present invention and comparative examples not according to the present invention, but the scope of the present invention is not limited to the following examples. EXAMPLES

[0049] <Example 1> A polyamic acid solution was prepared by sequentially adding 900g of a mixed solvent of 30wt% m-xylene and 70wt% NMP (N-methylpyrrolidone), 46g ODA, 10g graphene, 40g PMDA, and 14g ODPA to a glass reactor and stirring at 75°C for 2 hours. The completed polyamic acid solution was heated at 180°C for 2 hours at normal pressure to prepare a polyimide mixed solution. The powder precipitated in the mixed solution was filtered, washed with ethanol, and dried for 24 hours to prepare a polyimide powder. The powder was pressurized at >50MPa and >300°C to prepare a molded product.

[0050] <Example 2> A molded article was produced in the same manner as in Example 1, except that 20 g of graphene was used.

[0051] <Example 3> A molded article was produced in the same manner as in Example 1, except that 30 g of graphene was used.

[0052] <Example 4> A molded article was produced in the same manner as in Example 1, except that 50 g of graphene was used.

[0053] <Comparative Examples 1 to 5> Polyimide powder was prepared in the same manner as in Example 1, except that the filler components were different as shown in Table 1 below.

[0054] Specifically, Comparative Example 1 is a case where no filler was added, and Comparative Examples 2 to 5 are cases where various fillers that are conventionally added were added.

[0055] Experimental Example The physical properties of the prepared polyimide powder were measured by the following methods, and the results are shown in Table 1 below.

[0056] Experimental Example 1 - Measurement of elongation and tensile strength To analyze the tensile strength, a compression molded specimen of polyimide powder was used to prepare a dog bone-shaped specimen according to the ASTM D1708 standard. The polyimide powder was compressed at room temperature with a compression force of 6 ton / cm. 2 The specimens were compressed at 40°C for 5 minutes and then sintered in an oven at 390°C for 1 hour to prepare analytical specimens. A 25-ton hydraulic press was used for compression molding, and the tensile strength was measured using an Instron 5564 UTM instrument.

[0057] Experimental Example 2: Measurement of surface resistance To measure the surface resistance, compression molded test pieces of polyimide powder were used, and the surface resistance of the examples and comparative examples was measured according to the ASTM D257 standard. Specifically, the surface resistance was measured according to the ASTM-D257 measurement method under conditions of 55% RH, 23°C, and an applied voltage of 500V, and the measurement equipment was a 4-point probe meter (CMT-SR 1000N, AIT).

[0058] [Table 1]

[0059] Referring to Table 1, in the case of Examples 1 to 4, which are polyimide powders having a dianhydride monomer component and a diamine monomer component as polymerization units according to the present invention and further containing graphene, the surface resistance is 10 9 Ω / cm 2 In particular, in the case of Example 4, the graphene content is 5 wt % and the surface resistance is 10 1 Ω / cm 2 As a result, in the cases of Examples 1 to 4 of the present invention, the reference surface resistance of the molded product was reduced to 10 1 Ω / cm 2 In the case of Examples 1 to 4 of the present invention, the surface resistance of the molded product can be reduced to 10 1 Ω / cm 2 The surface resistance can be reduced to 100 MPa and the elongation can be expressed to be antistatic through the expression of electrical conductivity. In addition, the tensile strength is about 90 MPa to 102 MPa, and the elongation is 8% to 9%, so the decrease in tensile strength and elongation is not significant. It can be seen that the tensile strength and elongation can be maintained at or above the target values ​​compared to conventional conductive fillers, while the conductivity can be expressed and antistatic is possible. On the other hand, in the case where no filler was added (Comparative Example 1) and in the case where conventional fillers were added to reduce the surface resistance (Comparative Examples 2 to 5), the surface resistance was reduced to 100 MPa and the elongation was increased to 8% to 9%, so ... 15 Ω / cm 2 Even in the case of Comparative Example 4, the surface resistance increases to 10 8 Ω / cm2 However, since the filler content is too high, there is a problem in that the tensile strength and elongation are reduced.

[0060] Table 2 below shows the experimental results comparing the intrinsic viscosity (IV), moldability, and processability of an example using a mixed solvent of an aprotic solvent and a protic solvent according to one embodiment of the present invention and a comparative example using an aprotic solvent alone or a protic solvent alone.

[0061] Specifically, Comparative Example 6 is a case where m-cresol was used alone, and Comparative Example 7 is a case similar to Example 1 except that NMP was used alone. Moreover, Example 6 is a case where a 50 / 50 wt% mixed solution of m-cresol / NMP was used, Example 7 is a case where a 30 / 70 wt% mixed solution of m-cresol / NMP was used, and Example 8 is a case similar to Example 1 except that a 70 / 30 wt% mixed solution of m-cresol / NMP was used.

[0062] [Table 2]

[0063] As shown in Table 2, in Comparative Examples 6 and 7, where a protic solvent or an aprotic solvent was used alone, the intrinsic viscosity (IV) was low, and it was difficult to ensure moldability and processability. On the other hand, in Examples 6 to 8, where a mixed solvent of a protic solvent and an aprotic solvent was used as in the embodiment of the present invention, the intrinsic viscosity (IV) was high, and the moldability and processability were all excellent.

[0064] The present invention described above is not limited to the above-described embodiments, since various substitutions and modifications can be made by a person having ordinary knowledge in the technical field to which the present invention pertains without departing from the technical concept of the present invention.

Claims

1. preparing a polyamic acid solution by solution polymerization of a dianhydride monomer and a diamine monomer in an organic solvent containing graphene; heating the polyamic acid solution to prepare a polyimide mixture; and filtering and drying the precipitate present in the mixed solution to obtain a polyimide powder.

2. 2. The method of claim 1, wherein the content of the graphene contained in the organic solvent is 5 to 70 parts by weight based on 100 parts by weight of the dianhydride monomer and the diamine monomer combined.

3. 2. The method for producing a polyimide powder according to claim 1, wherein the organic solvent is a mixed solvent of an aprotic solvent and a protic solvent.

4. the aprotic solvent is at least one selected from the group consisting of toluene, xylene, naphtha, anisole, cresol, ethylbenzene, propylbenzene, chlorobenzene, dichlorobenzene, trichlorobenzene, biphenyl, terphenyl, diphenyl ether, diphenyl sulfide, acetophenone, chlorinated biphenyl, and chlorinated diphenyl ether; 4. The method for producing a polyimide powder according to claim 3, wherein the protic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc), dimethylpropanamide (DMPA), N,N-dimethylacetamide (DEAc), 3-methoxy-N,N-dimethylpropanamide (KJCMPA), and gamma-butyrolactone (GBL).

5. 4. The method for producing a polyimide powder according to claim 3, wherein the mixed solvent contains 10 to 50% by weight of an aprotic solvent and 50 to 90% by weight of a protic solvent.

6. 2. The method of claim 1, wherein the step of preparing the polyamic acid solution is performed at 50 to 100.degree. C.

7. 2. The method of claim 1, wherein the step of preparing the polyimide mixture is performed at a temperature of 140 to 200.degree.

8. 2. The method for producing a polyimide powder according to claim 1, wherein the dianhydride monomer comprises at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA), and p-phenylenebis(trimellitate anhydride) (TAHQ).

9. The diamine monomers include 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine ( 2. The method for producing a polyimide powder according to claim 1, wherein the polyimide powder comprises at least one selected from the group consisting of 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).

10. a polyimide matrix having polymerized units derived from dianhydride and diamine monomers; and comprising graphene dispersed within the polyimide matrix, The tensile strength measured by ASTM D1708 is 70 MPa or more, the elongation measured by ASTM D1708 is 7% or more, and the surface resistance measured by ASTM D257 is 10 9 Ω / cm 2 The polyimide powder is as follows:

11. The polyimide powder according to claim 10, comprising 0.01 to 50 parts by weight of graphene per 100 parts by weight of the polyimide powder.

12. 11. The polyimide powder according to claim 10, wherein the dianhydride monomer comprises at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA), and p-phenylenebis(trimellitate anhydride) (TAHQ).

13. The diamine monomers include 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine, and the like.

11. The polyimide powder according to claim 10, comprising at least one selected from the group consisting of M-TOLIDINE, 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).

14. A method for producing a polyimide molded product, comprising the step of compressing and molding the polyimide powder according to claim 10.

15. The method for producing a polyimide molded product according to claim 14, wherein the pressure molding step is performed at a pressure of 30 to 1,000 MPa.

16. The method for producing a polyimide molded product according to claim 14, wherein the pressure molding is performed at 200 to 450°C.

17. The method for producing a polyimide molded article according to claim 14, further comprising the step of sintering the pressed polyimide powder at 200 to 450°C.

18. A polyimide molded product produced by the method according to any one of claims 14 to 17.

Citation Information

Patent Citations

  • Polyimide and preparation method thereof, and polyimide sealing ring and preparation method thereof

    CN113307972A

  • Polyimide film for graphite sheet containing graphene-containing spherical PI filler, its manufacturing method, and graphite sheet manufactured using the same

    JP2021515824A

  • Manufacturing method of polyimide powder and polyimide powder manufactured by the same

    KR102203211B1

  • Process for producing polyimide

    WO2001068742A1