Solid acid catalyzed paraffin alkylation using rare earth modified molecular sieve adsorbents

Rare earth modified molecular sieve adsorbents with specific structures and metals enhance paraffin alkylation catalyst stability, addressing deactivation issues in solid acid catalysts and improving reaction efficiency and selectivity.

JP2024540686APending Publication Date: 2024-10-31EXELUS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024547173
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current solid acid catalysts for paraffin alkylation suffer from rapid deactivation due to olefin polymerization and clogging by heavy hydrocarbons, leading to reduced catalyst life and increased production costs, while liquid acid catalysts pose safety and environmental hazards.

Method used

A method using a rare earth modified molecular sieve adsorbent with specific Si/Al molar ratio, sodalite and supercage structure, and transition metals like Pt, Pd, or Ni, which enhances catalyst stability and selectivity by minimizing secondary reactions.

Benefits of technology

The method achieves high olefin conversion to desired products with improved catalyst life and reduced side reactions, maintaining selectivity and stability over extended periods without regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540686000001_ABST
    Figure 2024540686000001_ABST
Patent Text Reader

Abstract

The present invention describes a process for alkylating isobutane, comprising a catalytic reaction system including a crystalline zeolite catalyst and a rare earth modified molecular sieve adsorbent (RE-MSA). The crystalline zeolite catalyst comprises sodalite cages and supercages, has a Si / Al molar ratio of 20 or less, less than 0.5 wt% alkali metal, contains up to 5 wt% Pt, Pd, or Ni, and has an acid site density (including both Lewis and Bronsted acid sites) of at least 100 mole / gm. The rare earth (RE) modified molecular sieve adsorbent (Re-MSA) comprises sodalite cages and supercages, has a Si / Al molar ratio of 20 or less, less than 1 wt% alkali metal, 10-30 wt% RE (rare earth element), 2 wt% to 10 wt% transition metal selected from group 9-11, and has an acid site density of 30 mole / gm or less. The present invention also includes a method for making the RE-MSA.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 256,516, filed October 15, 2021. [Background technology]

[0002] High octane alkylate is the cleanest gasoline blend stream produced by refineries. The term "alkylate" refers to the reaction product of isobutane with olefins. Alkylate is an ideal clean fuel component because it is less polluting and less toxic. Alkylate has been blended into gasoline for decades to improve the octane number and therefore the anti-knock properties of gasoline. The importance of alkylate to refiners continues to grow. It currently accounts for about 13% of North American fuels, or more than 12 million barrels per day. For refineries striving to meet more stringent motor fuel specifications mandated around the world, investment in alkylation capacity can lead to improved refinery flexibility and profitability. Currently, alkylate is produced using liquid acid catalysts. Refiners typically use either hydrofluoric acid (HF), which can be deadly if spilled, or sulfuric acid (H2SO4), which is potentially harmful and increases recycling costs.

[0003] In the alkylation reaction, light olefins react with isoparaffins (usually isobutane) in the presence of a strong acid catalyst. The alkylation of isobutane with C2-C5 olefins involves a series of sequential and simultaneous reactions that occur through a carbocation intermediate. The first step is the addition of a proton to isobutane to form a tert-butyl or t-butyl cation. The t-butyl cation then adds to an olefin to generate the corresponding C8 carbocation. These C8 carbocations can isomerize via hydride transfer and methyl shift to form more stable cations. The C8 cation then undergoes rapid hydride transfer with isobutane to form the desired isooctane molecule, and the t-butyl cation is regenerated to perpetuate the chain sequence.

[0004] Unfortunately, these are not the only reactions that occur during alkylation. In general, there are a number of secondary reactions that tend to reduce the quality of the alkylate. Polymerization occurs by the addition of a second olefin to the C8+ cation formed in the primary reaction, thereby forming C 12 Cations with more than eight carbon atoms, such as the + cation, are formed. 12 The + cation can continue to react with olefins to form larger cations. It is generally believed that the continued addition of olefins to the carbocation, or polymerization of olefins, is the main pathway to catalyst deactivation. The olefin addition reaction is sometimes called the polymerization step, while the hydride transfer reaction is called the main alkylation reaction. The polymerization reaction forms "coke". The heavier alkylate molecules can then crack over the acid sites to form lighter C5-C7 hydrocarbons. As a result, the alkylate is converted into light isopentane (C5H 12 ) to heavier (C 12 H 26 It is composed of paraffinic molecules up to 10 ...

[0005] Solid acid catalysts have been investigated for nearly 30 years as an alternative to liquid catalysts. These catalysts include AlC3; heteropolyacids such as tungstates; and liquid acids immobilized on silica, polymers, or other solid supports. Natural or synthetic zeolites have also been used. Solid acid catalysts can be tuned to improve selectivity and reduce production costs, but they tend to deactivate rapidly under alkylation reaction conditions by two mechanisms: 1) the formation of "coke" at the active sites from olefin polymerization reactions and 2) clogging of the pore mouths by heavy alkylate molecules. Heavy hydrocarbons tend to clog the pore structure of solid catalysts, thereby reducing access to the acid sites.

[0006] There has been great interest in developing improved solid acid alkylation catalysts. For example, JP-A-1-245853, U.S. Pat. Nos. 3,962,133 and 4,116,880, and British Patent Nos. 1,432,720 and 1,389,237 disclose H2SO4-enhanced superacid catalysts; U.S. Pat. Nos. 5,220,095, 5,731,256, 5,489,729, 5,364,976, 5,288,685, and European Patent Application No. 714,871A disclose CF3SO3H / silica catalysts; U.S. Pat. Nos. 5,391,527 and 5,739,074 disclose Pt-AlCl3-KCl / Al2O3 catalysts. US Patents 5,157,196, 5,190,904, 5,346,676, 5,221,777, 5,120,897, 5,245,101, 5,012,033, 5,157,197, and published WO 95 / 126,815, etc., disclose Lewis acid catalysts such as SbF5, BF3, and AlCl3; US Patents 5,324,881 and 5,475,178 disclose supported heteropolyacid catalysts; US Patents 3,917,738 and 4,384,161 disclose molecular sieve catalysts. However, despite more than 50 years of continuous efforts, there remains a need for improved, stable, and economical solid acid alkylation catalysts.

[0007] Solid acid catalysts, e.g., multiple H + or zeolite catalysts with acid sites, are less toxic and dangerous. However, such catalysts are more prone to oxidation than liquid acid catalysts. + , i.e., there are few acidic sites, and only a fraction of such acidic sites are strong enough to catalyze the alkylation reaction. Fundamentally different from liquid acids, zeolites have a diverse population of sites that vary widely in nature (Brønsted and Lewis acids) and strength. Depending on the type of zeolite, aluminum content, and exchange procedure, a wide range of strengths and concentrations of Brønsted and Lewis acid sites exist. Zeolites exhibit a much lower concentration of protons (acid sites) than liquid acids. For example, 1 g of H2SO4 contains 20 × 10 -3 moles of protons, 1 g of zeolite HY with a Si / Al ratio of 5 contains 1 × 10 -3 They contain less than 100 moles of protons, of which 20-30% are strong enough to catalyze the alkylation reaction. As a result, the useful life of solid acid catalysts is typically two orders of magnitude shorter than that of liquid acid catalysts, making it difficult to develop a commercially viable paraffin alkylation technology using solid acid catalysts.

[0008] A method for preparing a zeolite catalyst with improved alkylation properties is described by Lercher et al. in U.S. Pat. No. 7,459,412. The catalyst described in this patent includes a crystalline zeolite with a silica (SiO2) to alumina (Al2O3) molar ratio of less than 10 and an alkali metal content of 0.2% by weight or less. In the examples, Lercher et al. treated commercial zeolite X with lanthanum nitrate and then ammonium nitrate and calcined at 450° C. in a stream of air to produce a zeolite catalyst with low alkali metal content. Lercher et al. reported that the catalyst should have as high a concentration of Bronsted acid centers as possible and a low concentration of strong Lewis acid centers. The Lewis acid centers are catalytically inactive but bind olefins which promote oligomerization and deactivation of the catalyst. Lercher et al. reported that the Lewis acid centers arise from aluminum cations that are released from the crystal lattice during the calcination process.

[0009] Prior art processes that do not combine rare earth and deammoniation processes describe deammoniation temperatures of at least 500° C. See U.S. Patents 3,893,942, 3,851,004, and 5,986,158.

[0010] The release of aluminum from the zeolite crystal lattice is known as dealumination and occurs at high temperatures in the presence of water vapor. For example, Lutz et al. reported in Investigations of the Mechanism of Dealumination of Zeolite Y by Steam: Tuned Mesopore Formation Versus the Si / Al Ratio,” in the Proceedings of the 14th Int'l Zeolite Conf., pp. 25-30 (2004) that dealumination of zeolite Y with 1 bar water vapor at 500°C, 600°C, and 700°C shows an increasing dealumination rate with increasing temperature. Summary of the Invention [Problem to be solved by the invention]

[0011] It is well known in the literature that molecular sieve adsorbents can be used to separate olefins from paraffins. The adsorbents used in the separation process are generally crystalline aluminosilicates modified with metals. Specifically, NaX zeolite can be used as an adsorbent in the separation field because its strong framework polarity allows it to generate stronger interactions with polar groups. Harden et al. studied the liquid-phase adsorption of 1-octene and octane on ion-exchanged X zeolite. 1They showed that the heat of immersion is higher for 1-octene than for octane, probably due to the specific interaction of 1-octene with the cations. Their results also showed that the nature of the cations in the zeolite has a strong influence. For example, the self-diffusivity of 1-octene was shown to decrease in the order KX>NaX>BaX. However, adsorbents such as zeolites exchanged with alkalis and alkaline earths exhibit van der Waals interactions mainly between the framework and sorbates and are not selective enough to completely remove less polar pollutants. In many cases, separation by more specific interactions between the adsorbent and the adsorbate is required. In many cases, metals are ion-exchanged on zeolites, which generally increases the capacity of the sieve for the adsorption of unsaturated compounds. The d-orbitals of these metals can participate in bond formation with unsaturated hydrocarbons in a non-classical manner. This type of bond is widely called π-complexation. 2、3 Many metals, especially transition metals such as Cu, Ag, Co, and Ni, have been investigated for this purpose. π-complexation has been successfully applied to olefin / paraffin separations using solutions containing silver or cuprous ions. 4~6 The selective adsorption of olefins relative to paraffins in the liquid phase has been successfully used for various applications. For example, Liu et al. 7 found that a mixture of CuCl and chloroaluminate ionic liquid catalyzed the alkylation reaction of isobutane / butene more efficiently than pure chloroaluminate ionic liquid, because the resulting CuAlCl4 could reversibly adsorb part of the butenes, thus increasing the isobutane / butene ratio in the reaction, which resulted in a reduction in side reactions and an improvement in the selectivity of TMP.

[0012] There have also been many attempts to use π-complexation to separate olefin / paraffin mixtures in gas-solid systems. Padin et al. 8showed that monolayer dispersed AgNO3 / SiO2 exhibited higher selectivity and capacity for 1-butene over 1-butane and acted like an excellent separation adsorbent. Purification of 1-butene by removing traces of 1,3-butadiene was achieved by using Ag+ exchanged Y-zeolite. The effect of changing the silver content in Ag-Y on the adsorption of 1,3-butadiene was systematically studied using Ag-Y and Ag+-Na+ mixed ion exchanged zeolites (AgNa-Y) with different Si / Al ratios. 9 AgNa-Y with a silver content of 26 wt% has been reported to show excellent purification properties for this application. 10 reported that the conversion of Cu2+ to Cu+ in ion-exchanged zeolite Y produced a new adsorbent for 1-butene / 1,3-butadiene separation. They reported that the performance of Cu(I)-Y was found to be about one order of magnitude better than that of Ag-Y. Furthermore, Cu-Y also showed better poisoning resistance than Ag-Y with respect to exposure to H2S / H2. Jin et al. 11 developed a new mesoporous adsorbent, Fe-Cu / MCM-41, for selective separation of 1-butene / n-butane. The authors reported that co-impregnation of Fe2+ and Cu+ ions in the mesopores of MCM-41 resulted in superior 1-butene / n-butane separation ability compared to Cu-MCM-41, possibly due to the fact that Fe 2+ The species acts as a kind of redox buffer and improves the chemical stability of the Cu+ species responsible for the formation of π-complexes with olefins. Other adsorbents based on π-complex formation have also been reported in the literature for selective olefin adsorption: Ag+-exchange resins, 12、13 Monolayer CuCl on pillared clay, 14 and single layer AgNO3 / SiO2 15~17 .

[0013] Denayer et al. 18、19evaluated a series of (transition) metal-exchanged zeolites with different topologies and Si / Al ratios for their potential to remove cyclopentadiene (CPD) from 1-octene. Co-, Ni-, and Ag-exchanged high alumina zeolites were selected as candidates for site-specific interactions. The authors reported that, among all the materials tested, zeolite X (denoted CoCaX50), which was first exchanged with calcium ions, then calcined and then exchanged with cobalt ions, showed the highest adsorption selectivity and adsorption capacity.

[0014] The effect of H2 and H2S exposure on the adsorption of 1,3-butadiene / 1-butene by Ag-Y was investigated in Ref. 9、20 Based on XPS analysis, Ag+ in Ag-Y reacted with H2S to form Ag2S, which caused a decrease in the adsorption capacity. However, the separation factor of 1,3-butadiene / 1-butene was high enough to make purification applications feasible. Meanwhile, H2 exposure to Ag-Y was detrimental due to the reduction of Ag+ to Ag0, which resulted in a significant deterioration of π-complex formation. Oxidative regeneration was proposed as a solution, which was demonstrated, and optimal oxidation conditions for olefin adsorption were identified. [Means for solving the problem]

[0015] In a first aspect, the present invention provides a method for alkylating isobutane, the method comprising: The method includes passing a feed mixture of excess isobutane and C2-C5 olefins through a reaction chamber; the reaction chamber includes a crystalline zeolite catalyst having sodalite cages and supercages, a Si / Al molar ratio of 20 or less, less than 0.5 wt.% alkali metal, up to 5 wt.% Pt, Pd, or Ni, and an acid site density (including both Lewis and Bronsted acid sites) of at least 100 μmole / gm; and a rare earth (RE) modified molecular sieve adsorbent (MSA) having sodalite cages and supercages, a Si / Al molar ratio of 20 or less, less than 1 wt.% alkali metal, 10-30 wt.% RE, 2 wt.% to 10 wt.% transition metal selected from Groups 9-11, and an acid site density of 30 μmole / gm or less. Note that these values ​​are for the zeolite and not for binders, fillers, or other structural components. Acid site density can be measured by conventional means, such as those defined in ASTM D4824-94 (reapproved in 1998). Preferably, the catalyst and adsorbent are in the form of pellets or beads.

[0016] The present invention also includes a catalytic reaction system comprising a catalyst and an adsorbent as defined above. The system can be further characterized by features of the equipment and reaction conditions.

[0017] The invention may be further characterized by one or any combination of the following features: at steady state, at least 90% of the C2-C5 olefins are converted to products, the Research Octane Number (RON) is maintained at 90 or greater, and the process is run over the same catalyst without regeneration for 2.5 or more catalyst ages, where steady state means that the selectivity to C8 isomers changes by 10% or less over the entire period over which the catalyst age is measured; the crystalline zeolite catalyst contains rare earth elements in the range of 10-35 wt.%, and the Re-MSA has a pore diameter of at least 8 Angstroms, or 8-12 Å; the process is run at a pressure of 250-400 psig. the concentration of C2-C5 olefins in the feed is 1 wt% to 30 wt%; the ratio of the concentration of isobutane to the concentration of C2-C5 olefins at the inlet of the catalyst bed is 100 to 1000 moles / mole; the space velocity of olefins is 0.05 / hr to 0.5 / hr; the catalyst and Re-MSA are regenerated in a flowing gas stream which is essentially hydrogen at a temperature of at least 250°C; the catalyst is doped with an element selected from the group consisting of Pt, Pd, Ni, and combinations thereof in an amount of 0.1 wt% to 5 wt%. % by weight, or 0.5-4% by weight, or 1.0-3.0% by weight; the catalyst and Re-MSA are regenerated using a gas stream that is at least 50% by volume hydrogen; the catalyst and Re-MSA are regenerated in flowing hydrogen at a temperature of at least 250° C. and a GHSV of at least 500; the process is carried out continuously for 2-3.5 catalyst ages without regenerating the catalyst or Re-MSA; the reaction chamber comprises a packed catalyst bed followed by a bed of Re-MSA; the reaction chamber the reaction chamber comprises a packed bed of Re-MSA followed by a catalyst bed; the reaction chamber comprises alternating beds of catalyst and Re-MSA comprising at least two catalyst beds and two Re-MSA beds; the reaction chamber comprises a packed bed of a mixture of catalyst and Re-MSA; the ratio of Re-MSA weight to catalyst weight in the reaction chamber is 0.1-10 wt / wt; the reaction chamber comprises a packed bed of particles comprising catalyst and Re-MSA, at least 95 wt% of the particles being at least 0.1 mm particle size; said process is carried out at a temperature of 45-90°C; said C2-C5 olefins contain less than 100 ppm water; carrying out said process with a catalyst age of at least 2.5 or at least 3.0 or in the range of 2.5 to 5.0 or 4.0; and / or the MSA is a 13X molecular sieve.

[0018] In another aspect, the present invention provides a method for producing a RE modified molecular sieve adsorbent (Re-MSA), the method comprising: providing a molecular sieve adsorbent (MSA) comprising sodalite cages and supercages, the MSA having a Si / Al molar ratio of 20 or less and a first concentration of alkali metal; contacting the MSA with a solution comprising a rare earth metal; calcining the catalyst by heating the Re-MSA to a temperature of at least 575°C to produce a Re-MSA intermediate comprising a rare earth metal and a second concentration of alkali metal lower than the first concentration of alkali metal; contacting the RE-MSA intermediate with a solution of a transition metal salt selected from Groups 9 to 11, drying to remove excess solution, and heating to a temperature to convert the transition metal salt to an oxide form.

[0019] The invention may further be characterized by one or any combination of the following features: the step of calcining to a temperature of at least 575°C, preferably 600°C, provides a RE-MSA in which a portion of the alkali metal cation sites are replaced with rare earth metal cation sites; the step of contacting with a solution of a transition metal salt provides a catalyst in which a portion of the alkali metal cation sites are replaced with rare earth metal cation sites and another portion of the alkali metal cation sites are replaced with transition metal cation sites; the heating to a temperature step does not exceed 450°C and is performed in the presence of air; the rare earth metal is selected from the group consisting of lanthanum, cerium, neodymium, and praseodymium, and the rare earth metal cations are selected from the group consisting of lanthanum cations, cerium cations, neodymium cations, and praseodymium cations; the rare earth metal comprises lanthanum; the alkali metal cation sites comprise at least 90% by weight of sodium cation sites; the catalyst has a silica to alumina ratio of about 2 to about 35. the catalyst has a silica to alumina ratio of about 2 to about 10; the rare earth metal-containing solution comprises an aqueous La(NO)3 solution; the rare earth metal-containing solution comprises an aqueous La2(SO4)3 solution; the rare earth metal-containing solution comprises an aqueous LaCl3 solution; the rare earth metal-containing solution contains at least 0.1M lanthanum ion, or at least 0.2M La, or at least 0.4M La, or at least 0.6M La, or at least 0.8M La, or 0.2-0.8M La. the catalyst is contacted with a rare earth metal solution at a temperature between 60 and 90°C; the catalyst is contacted with the rare earth metal solution for about 2 hours; the calcination step does not exceed 600°C; the calcination step is carried out for 2 to 8 hours; during the calcination step, the Re-MSA is heated in the presence of air having a moisture content not exceeding 2.0% by weight, or not exceeding 0.2% by weight; the solution of transition metal salt is at least 0.1M, or at least 0.2M, or at least 0.3M, or at least 0.5M, or at least 1M of metal ion; the step of contacting a solution of transition metal salt to provide a RE-MSA in which a portion of the alkali metal cation sites are replaced with transition metal cation sites includes an aqueous solution of nitrate, chloride, sulfate, acetate, citrate, or oxalate; the MSA is 13X. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 shows a schematic of the test unit used for screening adsorbents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Glossary Catalyst Age - "Catalyst Age" is the mass of olefin fed to the reactor divided by the mass of catalyst plus the mass of adsorbent.

[0022] Catalyst Life - The age of a catalyst at which the olefin conversion falls below 90% is defined as the "catalyst life".

[0023] Calcination Temperature - The term "calcination temperature" refers to the maximum temperature utilized as an intermediate step in the catalyst synthesis procedure to remove the hydrated spheres from the lanthanum ions and allow for solid-phase exchange between the lanthanum and sodium cations within the sodalite and supercages.

[0024] Regeneration temperature - The solid acid catalyst can be regenerated by flowing hydrogen gas at elevated temperatures in order to hydrocrack the heavier hydrocarbons and remove them from the zeolite structure. The maximum temperature used in this step is called the "regeneration temperature".

[0025] Conversion - The term "conversion of reactants" refers to the change in moles or mass of reactant between the material entering the reactor and the material leaving the reactor divided by the moles or mass of reactant in the material entering the reactor. For example, if 100 grams of olefin are fed to the reactor and 10 grams of olefin leave the reactor, the conversion is [(100-10) / 100] = 90% conversion of olefin.

[0026] By "crystalline zeotype material" it is meant that the material has a three-dimensional silica framework with open channels within the material that can be detected by X-ray diffraction. This material is also referred to as a zeolite structure. A description of numerous zeolite structures can be found in the Zeomics Structure Compendium at the website http: / / helios.princeton.edu / zeomics / . However, measurements of channel openings for a particular catalyst must be determined by conventional techniques. Although typical zeolites are aluminosilicates, the catalysts used in the present invention do not require aluminum (preferably containing less than 1 wt% Al, preferably less than 0.5 wt% or less than 0.1 wt% or less than 0.01 wt% Al). Unless otherwise stated, these compositions refer to catalysts with binders or, in some preferred embodiments, to compositions in the crystalline phase. The crystalline zeotype catalysts used to convert methane and / or DME to olefins can be referred to as Si / Ti zeotype catalysts, indicating Ti in the zeolite Si-O framework.

[0027] "RON" stands for Research Octane Number and is a well-known measure of fuel quality.

[0028] Olefins - As used herein, the term "olefin" has its normal meaning in the art and is used to refer to any unsaturated hydrocarbon containing one or more pairs of carbon atoms joined by a double bond. The term light olefin refers to C2-C6 olefins. In this invention, C2-C6 olefins refers to ethylene, propylene, n-butylene, isobutylene, and the various isomers of pentene and hexene. The phrase "C2-C6 olefin" has its standard meaning to include any combination of olefins in the C2-C6 range, with no minimum requirement for any of the C2-C6 compounds.

[0029] Those skilled in the art will understand how to determine pore size (e.g., smallest pore size, average smallest pore size) in a catalyst. For example, X-ray diffraction (XRD) can be used to determine atomic coordinates. XRD techniques for determining pore size are described, for example, in Pecharsky, VK et al., "Fundamentals of Powder Diffraction and Structural Characterization of Materials," Springer Science+Business Media, Inc., New York, 2005. Other techniques that may be useful for determining pore size (e.g., zeolite pore size) include, for example, helium pycnometry or low-pressure argon adsorption techniques. These and other techniques are described in Magee, JS et al., "Fluid Catalytic Cracking: Science and Technology," Elsevier Publishing Company, July 1, 1993, pp. 185-195. The pore size of mesoporous catalysts can be determined, for example, using nitrogen adsorption techniques, as described in Gregg, SJ et al., "Adsorption, Surface Area and Porosity," 2nd Ed., Academic Press Inc., New York, 1982, and Rouquerol, F. et al., "Adsorption by powders and porous materials. Principles, Methodology and Applications," Academic Press Inc., New York.

[0030] As is conventional, the phrase "having molecular dimensions of 5.1-5.6 Å" (or similar) refers to the largest channel opening (not the largest cavity size) in the MFI structure, which limits the size of compounds that can escape from the interior of the zeolite. This is also known as the pore-limiting diameter. The presence of the MFI structure can be characterized by X-ray diffraction (XRD), N2 adsorption / desorption isotherms. An example is given by Silvestre-Albero et al., "Desilication of TS-1 zeolite for the oxidation of bulky molecules," Cat. Comm. 44 (2014) 35-39. As is conventionally understood, the phrase "tetrahedral titania" does not require that the titania be exactly tetrahedral, but rather means that it meets the characteristic values ​​of Ti-substituted zeolites as mentioned in connection with the Silvestre-Albero et al. paper. As is known in the art, the described molecular dimensions in the crystal structure can be determined by known techniques, in particular the conventional gas adsorption / desorption technique as described in Silvestre-Albero et al. The techniques for determining the pore structure should converge to the same values. However, in case of large discrepancies, the gas adsorption / desorption technique as described in Silvestre-Albero et al. is decisive.

[0031] Selectivity - The term "selectivity" refers to the production of a particular product (or products) as a percentage of all products resulting from a reaction. For example, if a reaction produces 100 grams of products and these products include 80 grams of octane, then the selectivity for octane among all products is 80 / 100=80%. Selectivity can be calculated on a mass basis, as in the previous example, or on a molar basis, calculated by dividing the moles of a particular product by the moles of all products. Unless otherwise specified, selectivity is on a mass basis.

[0032] Yield - The term "yield" as used herein refers to the amount of product leaving the reactor divided by the amount of reactants entering the reactor, usually expressed as a percentage or fraction. Mass yield is the mass of a particular product divided by the weight of feed used to prepare that product.

[0033] Unless otherwise stated, "%" means mass %, which is equivalent to weight %. Ideal gas behavior is assumed to be the same as mole % and volume % in the gas phase.

[0034] As in standard patent terminology, the term "comprises" means "comprises" and does not exclude additional components. Any aspect of the invention described in conjunction with the term "comprises" also includes narrower embodiments in which the term "comprises" is replaced with the narrower terms "consisting essentially of" or "consisting of." As used herein, the terms "comprises" or "comprising" should not be construed as limiting the invention, but rather as listing exemplary components. As a standard term, a "system" includes devices and materials (such as reactants and products) and conditions within the devices.

[0035] The present invention is further described in the following examples. In some preferred embodiments, the present invention may be further characterized by any description selected from the examples, for example, within ±20% (or within ±10%) of any value in the examples, tables, or figures. However, the scope of the present invention is not limited by these examples in its broader aspects. EXAMPLES

[0036] Example 1 The starting material was a commercially available 13X molecular sieve from Sigma Aldrich with a SiO2 / Al2O3 molar ratio of 2.8 (Si / Al of 1.4) and a sodium content of 15 wt.%. This adsorbent was designated adsorbent A.

[0037] Example 2 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecule in 150 mL of 0.2 M lanthanum nitrate solution and heating to 80° C. with stirring for 2 hours. The lanthanum solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450° C. for 4 hours. This adsorbent is designated as adsorbent B.

[0038] Example 3 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M nickel nitrate solution and heating to 80° C. with stirring for 2 hours. The solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450° C. for 4 hours. This adsorbent is designated as adsorbent C.

[0039] Example 4 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M copper nitrate solution and heating to 80° C. with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450° C. for 4 hours. This adsorbent is designated as adsorbent D.

[0040] Example 5 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M barium nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450 °C for 4 hours.

[0041] The ion-exchanged molecular sieve was suspended in 0.5M ammonium nitrate solution and heated at 80°C for 2 hours with stirring. The ammonium solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450°C for 4 hours. This adsorbent is designated as adsorbent E.

[0042] Example 6 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M calcium nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450 °C for 4 hours.

[0043] The ion-exchanged molecular sieve was suspended in 0.5M ammonium nitrate solution and heated at 80°C for 2 hours with stirring. The ammonium solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450°C for 4 hours. This adsorbent is designated as adsorbent F.

[0044] Example 7 Alkylation activity experiments were performed using an isothermal packed bed reactor setup shown in Figure 1. T / dP >10 and L / d P >50. Heating was controlled using an Omega temperature control unit and ceramic heating elements. The feed was sent through a preheater approximately 75 cm long before entering the reactor.

[0045] The ExSact-3000 catalyst (15 grams) and the desired adsorbent (10 grams) were initially loaded into the reactor and activated by flowing 1 LPM of nitrogen at 350°C for 4 hours, and then cooled to the reaction temperature of 45°C. The reactor was then pressurized to 300 psig with isobutane. A reaction feed mixture of excess isobutane and 1-butene was fed to the reactor at a WHSV of 1 / hr. The recycle rate was maintained at 40 vol / vol. Product samples were taken every hour and analyzed using a gas chromatograph equipped with a Petrocol DH100m column. The effect of the adsorbent on the performance of the ExSact3000 catalyst in the alkylation of 1-butene with isobutane is shown in Table 1.

[0046] [Table 1]

[0047] Table 1 shows the advantages of using RE-exchanged molecular sieves as adsorbents.

[0048] Example 8 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0049] The ion-exchanged molecular sieve was suspended in 0.2 M barium nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent G.

[0050] Example 9 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0051] The ion-exchanged molecular sieve was suspended in 0.2 M lithium nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent H.

[0052] Example 10 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0053] The ion-exchanged molecular sieve was suspended in 0.2 M calcium nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent I.

[0054] Example 11 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450 °C for 4 hours.

[0055] The ion-exchanged molecular sieve was suspended in 0.8 M aluminum nitrate solution and heated to 80 °C with stirring for 2 h. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 600 °C for 4 h. This adsorbent is designated as adsorbent J.

[0056] Example 12 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0057] The ion-exchanged molecular sieve was suspended in 0.2M phosphoric acid solution and heated to 80°C with stirring for 2 hours. The acid solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450°C for 4 hours. This adsorbent is designated as adsorbent K.

[0058] Example 13 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0059] The ion-exchanged molecular sieve was suspended in 0.2 M lanthanum nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent L.

[0060] Example 14 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0061] The ion-exchanged molecular sieve was suspended in 0.2 M boric acid solution and heated at 80 °C for 2 h with stirring. The acid solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent M.

[0062] Example 15 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0063] The ion-exchanged molecular sieve was suspended in 0.2 M nickel nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent N.

[0064] Example 16 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0065] The ion-exchanged molecular sieve was suspended in 0.2 M copper nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as Adsorbent O.

[0066] Example 17 The 13X molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.8 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 600 °C for 4 hours.

[0067] The ion-exchanged molecular sieve was suspended in 0.2 M cobalt nitrate solution and heated at 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL of water each. The ion-exchanged molecular sieve was then dried and calcined at 450 °C for 4 h. This adsorbent is designated as adsorbent P.

[0068] Example 18 Alkylation activity experiments were performed as described in Example 7. The results are summarized in Table 2.

[0069] [Table 2]

[0070] Table 2 shows the advantage of a second ion exchange with either cobalt (group 9), nickel (group 10), or copper (group 11) when using RE-exchanged molecular sieves as the adsorbent.

[0071] Example 19 The starting material was a commercially available NaY molecular sieve from Sigma Aldrich with a SiO2 / Al2O3 molar ratio of 5.2 and a sodium content of 13 wt%. This adsorbent is designated as Adsorbent Q.

[0072] Example 19 The NaY molecular sieve was ion-exchanged by suspending 15 grams of the molecular sieve in 150 mL of 0.2 M lanthanum nitrate solution and heating to 80 °C with stirring for 2 hours. The nitrate solution was decanted and replaced with fresh solution. The ion-exchange was repeated two more times, followed by two washes with 75 mL of water each. The molecular sieve was then dried at room temperature. After ion-exchange, the molecular sieve was calcined in a muffle furnace at a temperature of 450 °C for 4 hours.

[0073] The RE-exchanged NaY molecular sieves were suspended in 0.2 M copper nitrate solution and heated to 80 °C for 2 h with stirring. The nitrate solution was decanted and replaced with fresh solution. This ion exchange was carried out three times, followed by two washes with 75 mL water each. The ion-exchanged molecular sieves were then dried and calcined at 450 °C for 4 h. This adsorbent is designated as Adsorbent R.

[0074] Example 20 The adsorbent was prepared by adding copper nitrate solution onto high surface area g-alumina support by incipient wetness technique. The adsorbent was then dried at room temperature. Following impregnation, the adsorbent was dried and calcined in a muffle furnace at a temperature of 450 °C for 4 h. This adsorbent is designated as adsorbent S.

[0075] Example 21 Alkylation activity experiments were performed as described in Example 7. The results are summarized in Table 3.

[0076] [Table 3]

[0077] Table 3 shows that neither Y zeolite re-exchanged with copper nor copper impregnated on g-alumina offers any advantage as an adsorbent for the alkylation of paraffins.

[0078] References 1. Herden, H. et al. “Liquid phase adsorption studies of octene-1 and octane on X-zeolites.” Journal of Colloid and Interface Science 102 (1984): 227-231. 2. RW Rousseau, Handbook of Separation Process Technology, John Wiley & Sons, New York, 1987, p. 1024. 3. Cotton, FA; Wilkinson, G. Advanced Inorganic Chemistry, 2nd ed.; Interscience: New York, 1966; Chapters 25 and 28. 4. Quinn, HW In Progress in Separation and Purification; Perry, ES Ed.; Interscience: New York, 1971; Vol. 4. 5. Ho, WS; Doyle, G.; Savage, DW; Pruett, RL Ind. Eng. Chem. Res. 1998, 27, 334. 6. Blytas, GC In Separation and Purification Technology, Li, NN, Calo, JM, Eds.; Marcel Dekker: New York, 1992. (10) Safarik, DJ; Eldridge, RB Ind. Eng. Chem. Res. 1998, 37, 2571. 7. Liu, Y.; Li, R.; Sun, H.; Hu, R. Effects of catalyst composition on the ionic liquid catalyzed isobutane / 2-butene alkylation. J. Mol. Catal. A: Chem. 2015, 398, 133-139. 8. Padin, J.; Yang, R. T.; Munson, C. L. Ind. Eng. Chem. Res. 1999, 38, 3614. 9. Takahashi, A.; Yang, R. T.; Munson, C. L.; Chinn, D. Ind. Eng. Chem. Res. 2001, 40, 3979. 10. Takahashi, A.; Yang, R. T.; Munson, C. L.; Chinn, D. Cu(I)-Y Zeolite as a Superior Adsorbent for Diene / Olefin Separation. Langmuir 2001, 17, 8405-8413. 11. Jin, M.; Kim, S. S.; Kim, Y. D.; Park, J.-N.; Kim, J. H.; Ko, C. H.; Kim, J.-N.; Kim, J. M. Redox-buffer effect of Fe2+ ions on the selective olefin / paraffin separation and hydrogen tolerance of a Cu+- based mesoporous adsorbent. J. Mater. Chem. A 2013, 1, 6653-6657. 12. Yang, R. T.; Kikkinides, E. S. AIChE J. 1995, 41, 509. 13. Wu, Z.; Han, SS; Cho, SH; Kim, JN; Chue, KT; Yang, RT Ind. Eng. Chem. Res. 1997, 36, 2749. 14. Cheng, LS; Yang , RT Adsorption 1995 , 1 , 61 . 15. Padin, J.; Yang, RT Ind. Eng. Chem. Res. 1997, 36, 4224. 16. Rain, SU; Padin, J.; Yang , RT AIChE J. 1998 , 44 , 799 . 17. Padin, J.; Yang , RT Chem. Eng. Sci. 2000, 55, 2607. 18. Denayer, Joeri & Huybrechts, Bart & Depla, Anouschka & Hermans, Yves & Gemoets, Frederik & Buren, Frederik & Kirschhock, Christine & Baron, Gino & Pierre, Jacobs. (2007). Removal of cyclopentadiene from 1-octene by transition metal containing zeolites. Part 1: Screening of the adsorption properties. Microporous and Mesoporous Materials. 103. 1-10. 19. Denayer, Joeri & Depla, Anouschka & Vermandel, Walter & Gemoets, Frederik & Buren, Frederik & Martens, Johan & Kirschhock, Christine & Baron, Gino & Pierre, Jacobs. (2007). Removal of cyclopentadiene from 1-octene by transition metal containing zeolites - Part 2: Stabilization of CoCaX zeolite by its cation distribution. Microporous and Mesoporous Materials. 103. 11-19. 20. Jayaraman, A.; Yang, R. T.; Munson, C. L.; Chinn, D., “Deactivation of L-Complexation Adsorbents by Hydrogen and Rejuvenation by Oxidation.” Ind. Eng. Chem. Res., 2001, 40, 4370.

Claims

1. 1. A process for alkylating isobutane, comprising the steps of: passing a feed mixture comprising excess isobutane and C2 to C5 olefins into a reaction chamber; The reaction chamber comprises: a crystalline zeolite catalyst comprising sodalite cages and supercages, a Si / Al molar ratio of 20 or less, less than 0.5 wt.% alkali metal, up to 5 wt.% Pt, Pd, or Ni, and having an acid site density (including both Lewis and Bronsted acid sites) of at least 100 μmole / gm; an RE-modified molecular sieve adsorbent (Re-MSA) comprising sodalite cages and supercages, a Si / Al molar ratio of 20 or less, less than 1 wt% alkali metal, 10-30 wt% RE, 2-10 wt% transition metal selected from Groups 9-11, and an acid site density of 30 μmole / gm or less; A method comprising:

2. At steady state, at least 90% of the C2-C5 olefins are converted to products; The research octane number (RON) is maintained above 90, and the process for catalyst ages of 2.5 or more is carried out on the same catalyst without regeneration.

2. The process of claim 1, wherein steady state means that the selectivity to C8 isomers changes by no more than 10% over the entire period over which the catalyst age is measured.

3. The crystalline zeolite catalyst comprises a rare earth element in the range of 10 to 35 wt. %; The method of claim 1 or 2, wherein the Re-MSA has a pore diameter of at least 8 Angstroms, or in the range of 8 to 12 Å.

4. The process of any one of claims 1 to 3, carried out at a pressure of from 250 to 400 psig.

5. The process according to any one of claims 1 to 3, wherein the concentration of C2 to C5 olefins in the feedstock is from 1 wt% to 30 wt%.

6. 4. The process according to any one of claims 1 to 3, wherein the ratio of the concentration of isobutane to the concentration of C2-C5 olefins at the inlet of the catalyst bed is from 100 to 1000 mol / mol.

7. The process according to any one of claims 1 to 3, wherein the space velocity of the olefin is from 0.05 / hr to 0.5 / hr.

8. 4. The method of any one of claims 1 to 3, wherein the catalyst and Re-MSA are regenerated in a flowing gas stream that is essentially hydrogen at a temperature of at least 250°C, and the catalyst comprises 0.1 wt% to 5 wt%, or 0.5 to 4 wt%, or 1.0 to 3.0 wt% of an element selected from the group consisting of Pt, Pd, Ni, and combinations thereof.

9. The method of any one of claims 1 to 4, wherein the catalyst and Re-MSA are regenerated using a gas stream that is at least 50% by volume hydrogen.

10. The process according to any one of claims 1 to 4, wherein the catalyst and Re-MSA are regenerated in flowing hydrogen at a temperature of at least 250°C and a GHSV of at least 500.

11. The process according to any one of claims 1 to 10, wherein the process is carried out continuously for 2 to 3.5 catalyst ages without regenerating the catalyst or the Re-MSA.

12. The process of any one of claims 1 to 7, wherein the reaction chamber comprises a packed catalyst bed followed by a bed of Re-MSA.

13. The process according to any one of claims 1 to 7, wherein the reaction chamber comprises a packed Re-MSA bed followed by a catalyst bed.

14. The process according to any one of claims 1 to 7, wherein the reaction chamber contains alternating beds of catalyst and Re-MSA, comprising at least two catalyst beds and two Re-MSA beds.

15. The process of any one of claims 1 to 7, wherein the reaction chamber comprises a packed bed of a mixture of catalyst and Re-MSA.

16. The method according to any one of claims 1 to 9, wherein the ratio of Re-MSA weight to catalyst weight in the reaction chamber is from 0.1 to 10 weight / weight.

17. The method of any one of claims 1 to 7, wherein the reaction chamber comprises a packed bed of particles comprising catalyst and Re-MSA, at least 95% by weight of the particles having a particle size of at least 0.1 mm.

18. The process according to any one of claims 1 to 17, carried out at a temperature of from 45 to 90°C.

19. 19. The process of any one of claims 1 to 18, wherein the C2 to C5 olefins contain less than 100 ppm water.

20. 20. The process of any one of claims 1 to 19, comprising carrying out the process at a catalyst age of 2.5 or at a catalyst age of 3.

0.

21. A method for producing an RE-modified molecular sieve adsorbent (Re-MSA), comprising: providing a molecular sieve adsorbent (MSA) comprising sodalite cages and supercages, the MSA having a Si / Al molar ratio of 20 or less and a first concentration of an alkali metal; contacting the MSA with a solution containing a rare earth metal; calcining the catalyst by heating the Re-MSA to a temperature of at least 575° C. to produce a Re-MSA intermediate comprising a rare earth metal and a second concentration of an alkali metal that is less than the first concentration of the alkali metal; contacting said RE-MSA intermediate with a solution of a transition metal salt selected from Groups 9-11; Drying to remove excess solution; and Heating the transition metal salt to a temperature that converts it to its oxide form. The method includes:

22. calcining to a temperature of at least 575°C, preferably 600°C, to obtain a RE-MSA in which a portion of the alkali metal cation sites are replaced with rare earth metal cation sites; contacting the catalyst with a solution of a transition metal salt to provide a catalyst having a portion of the alkali metal cation sites substituted with rare earth metal cation sites and another portion of the alkali metal cation sites substituted with transition metal cation sites; 22. The method of claim 21, wherein the heating to a temperature step does not exceed 450°C and is performed in the presence of air.

23. 23. The method of any one of claims 21 to 22, wherein the rare earth metal is selected from the group consisting of lanthanum, cerium, neodymium, and praseodymium, and the rare earth metal cation is selected from the group consisting of lanthanum cations, cerium cations, neodymium cations, and praseodymium cations.

24. 24. The method of any one of claims 21 to 23, wherein the rare earth metal comprises lanthanum.

25. 23. The method of claim 22, wherein the alkali metal cation sites comprise at least 90% by weight of sodium cation sites.

26. 26. The method of any one of claims 21 to 25, wherein the catalyst has a silica to alumina ratio of from about 2 to about 35.

27. 26. The method of any one of claims 21 to 25, wherein the catalyst has a silica to alumina ratio of from about 2 to about 10.

28. The solution containing the rare earth metal is La(NO) 3 The method of any one of claims 21 to 27, comprising an aqueous solution.

29. The solution containing the rare earth metal is La 2 (SO 4 ) 3 The method of any one of claims 21 to 27, comprising an aqueous solution.

30. The solution containing the rare earth metal is LaCl 3 The method of any one of claims 21 to 27, comprising an aqueous solution.

31. 28. The method of any of claims 21 to 27, wherein the solution containing a rare earth metal comprises an aqueous solution of at least 0.1 M lanthanum ion, or at least 0.2 M La, or at least 0.4 M La, or at least 0.6 M La, or at least 0.8 M La, or in the range of 0.2 to 0.8 M La.

32. The process of any one of claims 21 to 31, wherein the catalyst is contacted with the rare earth metal solution at a temperature of from 60 to 90°C.

33. 33. The method of claim 32, wherein the catalyst is contacted with the rare earth metal solution for about 2 hours.

34. A method according to any one of claims 21 to 33, wherein the calcination step does not exceed 600°C.

35. A method according to any one of claims 21 to 34, wherein the calcination step is carried out for a period of from 2 to 8 hours.

36. 22. The method of claim 21, wherein during the calcination step, the Re-MSA is heated in the presence of air having a moisture content not exceeding 2.0 wt.%, or not exceeding 0.2 wt.%.

37. 37. A method according to any one of claims 21 to 36, wherein the solution of transition metal salt comprises an aqueous solution of at least 0.1 M, or at least 0.2 M, or at least 0.3 M, or at least 0.5 M, or at least 1 M metal ion.

38. 38. The method of claim 37, wherein the step of contacting with a solution of a transition metal salt to provide an RE-MSA having a portion of the alkali metal cation sites substituted with transition metal cation sites comprises an aqueous solution of a nitrate, chloride, sulfate, acetate, citrate, or oxalate.

39. 22. The method of claim 21 , wherein the MSA is 13X.

Citation Information

Patent Citations

  • Hydrocarbon adsorbent, and method of adsorbing hydrocarbon

    JP2022108644A

  • Granulated zeolite catalyst and process for producing the catalyst

    US4036782A

  • Catalyst for acid-catalyzed by hydrocarbon conversions

    US7459412B2

  • Improved catalyzed alkylation, alkylation catalysts, and methods of making alkylation catalysts

    WO2016210006A2