Methods for improving the biological availability of nanomaterials on plant foliage

The preparation of nanocomposites with carbon dot CDs enhances adhesion and stability on plant foliage, addressing the issue of material loss, thereby improving nanomaterial effectiveness through increased adhesion and prolonged biological activity.

JP2024541159AActive Publication Date: 2024-11-08JIANGNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023575832
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-12
Filing Date
2023-07-19
Publication Date
2024-11-08
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

Current methods for applying nanomaterials on plant foliage result in reduced adhesion and efficacy due to material falling off, limiting the biological effectiveness of nanopesticides and fertilizers.

Method used

A method involving the preparation of nanocomposites by mixing resorcinol with aqueous ammonia, deionized water, and ethanol, followed by the addition of formaldehyde and tetraethyl orthosilicate, then calcination, and combining with carbon dot CDs to enhance adhesion and stability on plant foliage.

Benefits of technology

The nanocomposites demonstrate improved adhesion by 50.6% to 79.8% and rain resistance, with enhanced photosynthesis by 110% to 140% and biomass increase by 2 to 4 times, extending the effective period of action to over 10 days.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541159000001_ABST
    Figure 2024541159000001_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the biological effectiveness of nanomaterials on the foliage of plants, which belongs to the field of fertilizer technology. The method for improving the biological effectiveness of nanomaterials on the foliage of plants according to the present invention includes preparing NanoSi and CDs, dissolving the obtained NanoSi in ethanol, then adding carbon dots CDs, and slowly stirring the solution until it evaporates to obtain a solid nanocomposite material Nano-CDs. The adhesion ability of the obtained NanoSi-CDs is improved by 50.6%-79.8% compared with CDs, the rain resistance ability is improved by 1 cm, and after spraying NanoSi-CDs on the foliage, the photosynthesis of corn is improved by 110%-140% compared with CDs, the biomass amount is 2-4 times, and the effective period of action is extended by more than 10 days.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention specifically relates to a method for improving the biological availability of nanomaterials on the foliage of plants, which is in the field of fertilizer technology. [Background technology]

[0002] At present, the demand for food is increasing significantly, but the ideal yield of crops cannot be achieved, and serious environmental problems are generally caused. In recent years, the application of nanomaterials in agriculture has become more widespread, where the environmental load of nanomaterials is smaller, and due to their own characteristics, the particle size is smaller, the activity is stronger, and the biological effectiveness is higher, so the utilization efficiency of nano pesticides and fertilizers is improved by 10% to 30% compared to traditional agricultural fertilizers, and the higher utilization efficiency is determined by the way of spraying the material, and generally, spraying on the leaves is about 10% to 40% more efficient than spraying on the roots. Therefore, from the perspective of the biological effectiveness of the above materials, it can provide a reliable idea to solve the crisis of agricultural production. However, when spraying the material on the leaves, the material may fall off, so the biological effectiveness of the material can be further improved by further improving the collection rate of the material on the leaves. Summary of the Invention

[0003] In view of the above technical challenges and application objectives, the objective of the present invention is to enhance and improve the biological effectiveness of nanomaterials.

[0004] The technical solution of the present invention is: A method for improving the biological availability of nanomaterials on the foliar surface of a plant is provided, (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate and stirring to obtain a mixture, then continuing to add formaldehyde and resorcinol to the mixture and stirring to react, and after completion, centrifuging, collecting solids, washing, drying and calcining to obtain NanoSi; and (2) dissolving the obtained NanoSi in ethanol, adding carbon dots-CDs, and slowly stirring the solution until it evaporates to obtain a solid nanocomposite material, Nano-CDs.

[0005] The present invention provides a method for preparing a nanocomposite material having high biological availability on the foliage of a plant, (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate and stirring to obtain a mixture, then continuing to add formaldehyde and resorcinol to the mixture and stirring to react, and after completion, centrifuging, collecting solids, washing, drying and calcining to obtain NanoSi; and (2) dissolving the obtained NanoSi in ethanol, adding carbon dots-CDs, and slowly stirring the solution until it evaporates to obtain a solid nanocomposite material, Nano-CDs.

[0006] In one embodiment of the present invention, in the mixture in step (1), the concentration of aqueous ammonia is 28 wt %.

[0007] In one embodiment of the present invention, in the mixture in step (1), the volume ratio of ammonia water, deionized water and ethanol is 3:10:70.

[0008] In one embodiment of the present invention, in the mixture in step (1), the formaldehyde solution is a 37 wt% aqueous solution.

[0009] In one embodiment of the present invention, in the mixture in step (1), the mass ratio of formaldehyde solution to deionized water is (0.25-0.3):10.

[0010] In one embodiment of the present invention, the amount of resorcinol added to the mixture in step (1) is 0.2 g / 10 mL of deionized water.

[0011] In one embodiment of the present invention, in the mixture in step (1), the volume fraction of tetraethyl orthosilicate to deionized water is 6%.

[0012] In one embodiment of the present invention, in step (1), as the formaldehyde and resorcinol are continued to be added to the mixture, the amount of resorcinol added is twice the amount of resorcinol in the mixture.

[0013] In one embodiment of the present invention, in step (1), while continuing to add formaldehyde and resorcinol to the mixture, the amount of formaldehyde added is twice the amount of formaldehyde in the mixture.

[0014] In one embodiment of the present invention, in step (1), the calcination may be performed continuously at 550° C. for 5 hours.

[0015] In one embodiment of the present invention, step (1) comprises: The process specifically involves adding aqueous ammonia (28 wt%, 3 mL), deionized water (10 mL) and ethanol (AR, 95%, 70 mL) to a solution composed of formaldehyde solution (37 wt%, 0.28 g) and resorcinol (0.2 g), magnetically stirring the mixture at room temperature at a speed of 500 rpm for 6 hours, then adding tetraethyl orthosilicate (TEOS, AR, >98%, 0.6 mL) and stirring for 30 minutes, then adding resorcinol (0.4 g) and formaldehyde solution (37 wt%, 0.56 g) and stirring the mixture for 2 hours, centrifuging the solid at a speed of 4000 rpm for 10 minutes, washing with ethanol and drying at 50 °C, and finally calcining the obtained solid continuously at 550 °C (the heating rate is 2 °C / min) for 5 hours to obtain NanoSi.

[0016] In one embodiment of the present invention, in step (2), carbon dot-CDs are obtained by synthesis from citric acid and ethylenediamine via a hydrothermal method.

[0017] In one embodiment of the present invention, the amounts of citric acid and ethylenediamine used are (1 to 2) g:(300 to 350) μL.

[0018] In one embodiment of the present invention, the hydrothermal reaction conditions are 200° C. for 12 hours.

[0019] In one embodiment of the present invention, in step (2), the amount of ethanol used relative to NanoSi is 450 mL / 100 mg.

[0020] In one embodiment of the present invention, in step (2), the mass ratio of NanoSi to carbon dots CDs is 1:1.

[0021] In one embodiment of the present invention, in step (2), the rotation speed of the slow stirring is 150 rpm.

[0022] The present invention further prepares a nanocomposite material with high biological availability on the foliage of plants based on the above method.

[0023] The present invention further provides an application of said method or said nanocomposite material for improving agricultural yields.

[0024] The present invention has the following beneficial technical effects:

[0025] In the present invention, the adhesion ability of NanoSi-CDs is improved by 50.6% to 79.8% compared to CDs, and the rain resistance is improved by 1 cm.

[0026] In the present invention, after spraying NanoSi-CDs on the leaves, the photosynthesis of corn is improved by 110% to 140% compared to CDs, the biomass amount is 2 to 4 times, and the effective period of action is extended for more than 10 days (slow release performance). [Brief description of the drawings]

[0027] [Figure 1](A) is a TEM image of NanoSi, (B) is a TEM image of CDs, (C) is a TEM image of NanoSi-CDs, (D) is a TEM image of the crystal lattice of CDs loaded on NanoSi, (E) is the PL spectra of CDs and NanoSi-CDs, and (F), (G), and (H) are the UV-vis, FTIR, and XPS chromatography of CDs, NanoSi, and NanoSi-CDs, respectively. [Diagram 2] (A) and (B) are the contact angles when the leaf surface growth angle of CDs and NanoSi-CDs is 0°, respectively, and (C) and (D) are the contact angles when the leaf surface growth angle of CDs and NanoSi-CDs is 30°, respectively. [Diagram 3] The effect of rainfall on washing away foliar fertilizers CDs, NanoSi and NanoSi-CDs is shown. A is an artificial rainfall device, B is a photo of the effect of 2.5cm precipitation on the 20th day, C, D and E are comparative examples, respectively, showing the net photosynthetic rate, electron transport rate and chlorophyll content after experiments with 0.5cm, 1.5cm and 2.5cm precipitation by treatment with NanoSi, CDs and NanoSi-CDs. [Figure 4] (A) is a photograph of the effect on the 1st, 10th and 20th days after spraying the materials from left to right, respectively, and (B)~(H) are the photosynthetic parameters such as net photosynthetic rate, chlorophyll A, chlorophyll B, electron transport rate, photosystem 2 (PSII) activity-related genes, photosystem 1 (PSI) activity-related genes and the photosynthetic pathway diagram. [Diagram 5] 1 is a TEM photograph of the composite material obtained in Comparative Example 1. [Figure 6] 1 is a TEM photograph of the composite material obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The present invention will be further described below in conjunction with specific examples.

[0029] The embodiments provided below do not limit the scope of the present invention, and the steps described do not limit the order of execution. Those skilled in the art will recognize that any improvements made to the present invention in accordance with the conventional common knowledge should be included in the scope of the present invention.

[0030] Example 1: Preparation of nanomaterials (CDs and NanoSi) and their composites (NanoSi-CDs) (1) Ammonia water (28 wt%, 3 mL), deionized water (10 mL) and ethanol (AR, 95%, 70 mL) are added to a solution composed of formaldehyde (37 wt%, 0.28 g) and resorcinol (0.2 g). At room temperature, the mixture is magnetically stirred at a speed of 500 rpm for 6 h, then tetraethyl orthosilicate (TEOS, AR, >98%, 0.6 mL) is added and stirred for 30 min. Then, resorcinol (0.4 g) and formaldehyde (37 wt%, 0.56 g) are added and the mixture solution is stirred for 2 h. Then, the solid is centrifuged at a speed of 4000 rpm for 10 min, washed with ethanol and dried at 50 °C. Finally, the obtained solid is continuously calcined at 550 °C (the heating rate is 2 °C / min) for 5 h to obtain NanoSi.

[0031] (2) CDs are synthesized from citric acid (1.05 g) and ethylenediamine (335 μL) by a hydrothermal method (200 °C and 12 h).

[0032] (3) 100 mg of NanoSi is dissolved in 450 mL of ethanol and sonicated for 6 h, after which 100 mg of CDs is added. Finally, the solution is slowly stirred at 60 °C with a rotation speed of 150 rpm until the solution evaporates to obtain the solid Nano-CDs composite.

[0033] Transmission electron microscopy (TEM) was used to show the morphology and dimensions of CDs, NanoSi and NanoSi-CDs. The results showed that NanoSi was spherical, with a large amount of hair-like material on the surface, with a diameter of 250.6±30.5nm and a hair-like length of 30.5±6.8nm (Fig. 1A). The particle size of CDs was 2.55±0.23nm (Fig. 1B). Carbon dot crystal lattices were found in NanoSi (Fig. 1D), proving that CDs were successfully loaded onto NanoSi. Fluorescence spectra (Fig. 1E) again prove that NanoSi has carbon dot fluorescence. UV-vis, FITR and XPS spectra (Fig. 1F-H) of CDs, NanoSi and NanoSi-CDs further prove that CDs were loaded onto NanoSi (Fig. 1F-H).

[0034] Example 2: Measurement of adhesion performance of NanoSi A contact angle meter was used to measure the contact angles of 1 μL, 3 μL, and 5 μL of CDs and NanoSi-CDs, respectively, at growth angles of 0° and 30° on the corn leaf surface (Figure 2). The results showed that the contact angle of NanoSi-CDs on the corn leaf surface was much smaller than that of CDs, and the smaller the contact angle, the more hydrophilic the material is, i.e., it is less likely to fall off, and the adhesion ability of the material on the leaf surface is improved. Table 1 shows the adhesion effect measured by the contact angle meter, which further proves that NanoSi-CDs after loading has a higher adhesion ability than CDs, i.e., the adhesion ability of NanoSi-CDs is improved by 50.6% to 79.8% compared to CDs.

[0035] Table 1. Adhesion behavior of CDs and NanoSi-CDs on leaf surfaces TIFF2024541159000002.tif23170Example 3: Raintightness experiment To simulate the effect of rainwater washing away NanoSi-CDs, artificial rainwater is designed, and 3 μmol Mg(NO3)2, 7 μmol MgCl2, 15 μmol CaCl2, 6 μmol NH4Cl, 10 μmol Na2SO4, 62 μmol NaCl, and 8 μmol KCl are dissolved in ultrapure water. The spray bottle method (Figure 3A) is used to simulate the process of rainfall. The artificial rainwater is poured into a spray bottle, and the "rainwater" is sprayed from the front side by a bottle attached with a spraying device with a trigger pump, the height of the bottle above the ground is 0.5 meters, and the distance to the leaf surface of the corn is about 0.3 meters. The spray bottle is adjusted to spray 80 milliliters of artificial rainwater, which corresponds to about 0.5 centimeters of precipitation, every 100 sprays. The effect of washing away NanoSi-CDs is measured with precipitation of 0.5, 1.5, and 2.5 cm. Ten repeats are performed for each sample. After the rainfall test, the corn crop's various indicators were measured. The results showed that CDs had almost no effect on corn photosynthesis at 1.5 cm of precipitation, proving that CDs were almost entirely washed away by rainwater at this precipitation, while NanoSi-CDs still maintained a high photosynthesis-promoting effect at 2.5 cm of precipitation, further proving that NanoSi can improve the adhesion ability of CDs on the leaf surface.

[0036] Example 4: Biological Effects of Improved Biological Availability of Materials Corn seedlings that had germinated and grown uniformly were selected and transferred to pots (each pot had two plants) containing 1.5 kg of soil. Each plant was then infused with 5 mL of CDs, NanoSi and NanoSi-CDs dispersions (each with a concentration of 10 mg L−1). -1 The control group was ultrapure water (CK). After that, the corn foliage was collected on the 1st, 5th, 10th, 15th, and 20th days after the materials were sprayed for 7 consecutive days, and the photosynthetic parameters were measured.

[0037] The results showed that after spraying NanoSi-CDs on the leaves, the photosynthesis of corn was improved by 110%-140% compared to CDs, the biomass was 2-4 times higher, and the effective period of action was extended by more than 10 days.

[0038] Comparative Example 1: Referring to Example 1, the amount of ethanol used in step (3) is converted to 300 mL and 600 mL (i.e., NanoSi), respectively, and the other matters are not changed to obtain the corresponding composite material.

[0039] The morphology of the corresponding composites was characterized, and no crystal lattice of carbon dots was found on the surface of any of the obtained corresponding composites, clearly indicating that the method could not achieve effective loading of carbon dots.

[0040] Comparative Example 2: Referring to Example 1, in step (3), the rotation speed is converted from 150 rpm to 100 rpm and 300 rpm respectively, while other things are not changed, and the corresponding composite material is obtained.

[0041] The morphology of the corresponding composites was characterized, and no crystal lattice of carbon dots was found on the surface of any of the obtained corresponding composites, clearly indicating that the method could not achieve effective loading of carbon dots.

Claims

1. 1. A method for improving the biological availability of a nanomaterial on the foliar surface of a plant, comprising: (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate, stirring to obtain a mixture, then adding formaldehyde and resorcinol to the mixture, stirring to react, and after completion, centrifuging, collecting solid, washing, drying and calcining to obtain NanoSi; (2) dissolving the obtained NanoSi in ethanol, then adding carbon dots-CDs, and slowly stirring the solution until the solution evaporates to obtain a solid nanocomposite material Nano-CDs; In the mixture in step (1), the volume fraction of tetraethyl orthosilicate to deionized water is 6%; In step (1), while continuing to add formaldehyde and resorcinol to the mixture, the amount of resorcinol added is twice the amount of resorcinol in the mixture and the amount of formaldehyde added is twice the amount of formaldehyde in the mixture; In step (2), the amount of ethanol used relative to NanoSi is 450 mL / 100 mg; In step (2), the mass ratio of NanoSi to carbon dots CDs is 1:1; A method for improving the biological availability of nanomaterials on the leaf surface of a plant, characterized in that in step (2), the rotation speed of the slow stirring is 150 rpm.

2. 1. A method for preparing a nanocomposite material having high biological availability on the foliage of a plant, comprising: (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate, stirring to obtain a mixture, then adding formaldehyde and resorcinol to the mixture, stirring to react, and after completion, centrifuging, collecting solid, washing, drying and calcining to obtain NanoSi; (2) dissolving the obtained NanoSi in ethanol, then adding carbon dots-CDs, and slowly stirring the solution until the solution evaporates to obtain a solid nanocomposite material Nano-CDs; In the mixture in step (1), the volume fraction of tetraethyl orthosilicate to deionized water is 6%; In step (1), while continuing to add formaldehyde and resorcinol to the mixture, the amount of resorcinol added is twice the amount of resorcinol in the mixture and the amount of formaldehyde added is twice the amount of formaldehyde in the mixture; In step (2), the amount of ethanol used relative to NanoSi is 450 mL / 100 mg; In step (2), the mass ratio of NanoSi to carbon dots CDs is 1:1; A method for preparing a nanocomposite material with high biological availability on the foliage of plants, characterized in that in step (2), the rotation speed of the slow stirring is 150 rpm.

3. 1. A method for improving the biological availability of a nanomaterial on the foliar surface of a plant, comprising: (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate, stirring to obtain a mixture, then adding formaldehyde and resorcinol to the mixture, stirring to react, and after completion, centrifuging, collecting solid, washing, drying and calcining to obtain NanoSi; and (2) dissolving the obtained NanoSi in ethanol, then adding carbon dots-CDs and slowly stirring the solution until it evaporates, thereby obtaining a solid nanocomposite material, Nano-CDs.

4. 1. A method for preparing a nanocomposite material having high biological availability on the foliage of a plant, comprising: (1) Mixing ammonia water, deionized water, ethanol, formaldehyde solution and resorcinol, stirring uniformly, then adding tetraethyl orthosilicate, stirring to obtain a mixture, then adding formaldehyde and resorcinol to the mixture, stirring to react, and after completion, centrifuging, collecting solid, washing, drying and calcining to obtain NanoSi; and (2) dissolving the obtained NanoSi in ethanol, then adding carbon dots-CDs, and slowly stirring the solution until it evaporates, thereby obtaining a solid nanocomposite material Nano-CDs.

5. 3. The method according to claim 1 or 2, characterized in that in the mixture in step (1), the volume fraction of tetraethyl orthosilicate to deionized water is 6%.

6. 3. The method according to claim 1 or 2, wherein in step (1), during the process of continuing to add formaldehyde and resorcinol to the mixture, the amount of resorcinol added is twice the amount of resorcinol in the mixture, and the amount of formaldehyde added is twice the amount of formaldehyde in the mixture.

7. The method according to claim 1 or 2, characterized in that in step (2), the amount of ethanol used relative to NanoSi is 450 mL / 100 mg.

8. The method according to claim 1 or 2, characterized in that in step (2), the mass ratio of NanoSi to carbon dots CDs is 1:

1.

9. The method according to claim 1 or 2, characterized in that in step (2), the rotation speed of the slow stirring is 150 rpm.

10. A nanocomposite material having high biological availability on the foliage of plants obtained by the method according to claim 1 or 2.

11. A nanocomposite material having high biological availability on the foliage of plants obtained by the method according to claim 3 or 4.

12. Application of the method of claim 1 for improving agricultural production.

13. 11. The application of the nanocomposite material according to claim 10 for improving agricultural yields.

14. 12. Application of the nanocomposite material according to claim 11 for improving agricultural yields.

Citation Information

Patent Citations

  • Formulation, its manufacturing method, and hydrogen supply method

    JP2021178320A

  • Photosynthesis stimulators based on hybrid carbon nanoparticles, related methods of preparation and related uses as nanobiostimulants and nanofertilizers in agricultural crops

    JP2023514979A

  • Control method of corn armyworm using nanosilicon quantum dots

    JP2023529548A

  • Photosynthesis stimulator based on hybrid carbon nanoparticles, related production method and related use as nanobiostimulants and nanofertilizers in agricultural crops