Highly durable, perforation-resistant, polymeric, waterproof coil material and preparation method thereof
A multilayered polymeric waterproof coil material with specific compositions addresses oil leakage and aging issues in elastomer modified bituminous materials, ensuring superior waterproofing and root puncture resistance in planted roofs.
Patent Information
- Application Number
- JP2023576047
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-25
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Elastomer modified bituminous waterproof coil materials used in planted roofs suffer from oil leakage issues over time, affecting their waterproofing performance and failing to meet the required defense standards.
A multilayered structure comprising a polyethylene film layer, an elastomer-modified bituminous layer, a polyester felt layer, and another polyethylene film layer, with specific compositions of bitumen, dihydroxypolydimethylsiloxane, root-resistant agents, and antibacterial agents, is used to enhance oil penetration resistance and aging resistance.
The solution effectively prevents oil migration, enhances oil penetration resistance, and improves aging resistance, ensuring compliance with industry standards for waterproofing and root puncture resistance in planted roofs.
Smart Images

Figure 2024541160000001 
Figure 2024541160000002 
Figure 2024541160000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of waterproof coil material, and in particular to a highly durable, puncture-resistant polymeric waterproof coil material and a method for preparing the same. [Background technology]
[0002] Root-resistant waterproof coil material for planted roofs includes elastomer modified bitumen waterproof coil material, plastomer modified bitumen waterproof coil material, modified bitumen polyethylene tire waterproof coil material and other polymer modified bitumen waterproof coil material, polymer waterproof sheet, PVC waterproof coil material, TPO waterproof coil material, etc. Among these waterproof coil material products, elastomer modified bitumen waterproof coil material has the highest market share and the most widespread application.
[0003] The elastomer modified bitumen waterproof coil material is made of polyester fiber mat as padding, elastomer modified bitumen with added chemical root resistant agent as asphalt coating material, and polyethylene film insulation material. It has excellent waterproof performance and can maintain waterproof effect for a long time. When applied to planted roof, it can resist plant root puncture without affecting plant growth, and has a wide range of applications in construction sites such as underground and roof.
[0004] JGJ155~2013 "Technical Regulations for Planted Roof Construction" stipulates that the planted roof waterproof layer should meet the first-class waterproof grade protection requirements, the planted roof waterproof layer should not fall below two waterproof protection levels, and the upper waterproof layer should be root-resistant puncture waterproof material, that is, the root-resistant puncture waterproof material should be installed on the top of the normal waterproof layer. However, in practical application, the oil in the elastomer-modified bitumen-resistant root-resistant puncture waterproof coil material will transfer with the increase in use time, which will affect the waterproof quality. Therefore, it is urgently necessary to improve the oil penetration performance of the elastomer-modified bitumen-resistant root-resistant puncture waterproof coil material. Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides a highly durable puncture-resistant polymeric waterproof coil material and a preparation method thereof, and solves the problem of oil leakage of elastomer-modified bitumen root puncture-resistant waterproof coil material in the prior art. [Means for solving the problem]
[0006] The technical solution of the present invention is as follows: A highly durable, perforation-resistant polymer waterproof coil material comprising a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, the elastomer-modified bitumen layer including raw materials of prepreg and buttering material, the prepreg including components of 70-80 parts of 90# bitumen, 15-20 parts of dihydroxypolydimethylsiloxane, 0.5-1 part of root-resistant agent, and 0.1-0.2 parts of antibacterial agent by weight, and the buttering material including components of 50-70 parts of 90# bitumen, 5-8 parts of 10# bitumen, 20-30 parts of 200# bitumen, 5-10 parts of polyphenylpyrrolidone, 4-8 parts of SBS, 5-6 parts of plasticizer, 40-60 parts of filler, 1-1.5 parts of root-resistant agent, and 0.4-0.7 parts of antibacterial agent by weight.
[0007] As a further technical proposal, the mass ratio of 90# bitumen, 10# bitumen and 200# bitumen in the buttering material is 10:1:5.
[0008] In a further technical solution, the filler is one or more of talcum powder, swelling earth, diatomaceous earth, and fly ash.
[0009] In a further technical solution, the plasticizer is an arene oil.
[0010] In a further technical solution, the antibacterial agent is a nano-silver antibacterial agent.
[0011] As another technical solution, the prepreg is prepared by uniformly mixing 90# bitumen and dihydroxypolydimethylsiloxane at 165-170℃, further adding root-resistant agent and antibacterial agent, and mixing uniformly to obtain prepreg.
[0012] As a further technical proposal, when mixing the 90# bitumen and dihydroxypolydimethylsiloxane, the stirring speed is 80-100 rpm and the stirring time is 10-15 minutes.
[0013] As another technical solution, the buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen and 200# bitumen at 130~140℃, adding plasticizer and SBS, uniformly mixing at 155~175℃, grinding until fully expanded, adding filler, root-resistant agent and antibacterial agent, and uniformly mixing to obtain the buttering agent.
[0014] The present invention relates to Step S1 of dip-coating a prepreg for a polyester felt layer at 175 to 185 ° C.; Step S2: Coating the polyester felt layer with a buttering agent dip-coated at 175 to 185°C to form an elastomer-modified bitumen layer on the entire upper and lower surfaces of the polyester felt layer; S3: further covering the upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer-modified bitumen layer, with polyethylene film to obtain a polyethylene film layer, which is cooled and shaped to obtain a highly durable, perforation-resistant polymeric waterproof coil material; There is further provided a method for preparing a durable, puncture-resistant, waterproof polymeric coil stock, comprising: Effect of the Invention
[0015] The operating principle and beneficial effects of the present invention are as follows.
[0016] 1. The present invention adds dihydroxypolydimethylsiloxane to the immersion coating material of the elastomer modified bituminous layer, and adds polyphenylpyrrolidone as a buttering material, which have a synergistic effect, which can prevent the transfer of oil in the elastomer modified bituminous layer, and thereby enhance the oil penetration resistance of the waterproof paint. The oil penetration performance requirement of the produced waterproof coil material is less than or equal to one sheet, and complies with the requirements of GB / T35468-2017 "Root-resistant waterproof coil material for planted roofs".
[0017] 2. In the present invention, dihydroxypolydimethylsiloxane is added to the dip coating material of the elastomer modified bitumen layer, and polyphenylpyrrolidone is added to the buttering material, which have a synergistic effect, thereby significantly improving the aging resistance of the waterproof coil material.
[0018] 3. In the present invention, 10# and 200# bitumen are added to the buttering material of the elastomer modified bitumen layer, and some of the arene oil plasticizer is replaced by 10# and 200# bitumen, which further reduces the transfer of oil in the elastomer modified bitumen layer, while the specific mass ratio of 10# and 200# bitumen has synergy with 90# bitumen, thereby improving the aging resistance of the waterproof coil material. Best Mode for Carrying Out the Invention
[0019] The present invention provides a clear and complete description of the technical solutions of the embodiments in combination with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and are not all of the embodiments. All other embodiments obtained based on the embodiments in the present invention, on the premise that a person skilled in the art does not pay creative work, are related to the scope of protection of the present invention. Example 1
[0020] Example 1 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0021] S0. Preparation of raw materials.
[0022] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0023] The buttering agent contains 50 parts of 90# bitumen, 5 parts of 10# bitumen, 20 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene oil, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130℃, adding 10# arene oil and SBS, stirring uniformly at 155℃, grinding until the mixture expands, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0024] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0025] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0026] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0027] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 2
[0028] Example 2 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0029] S0. Reserve of raw materials.
[0030] The prepreg contains 80 parts of 90# bitumen, 20 parts of dihydroxypolydimethylsiloxane, 1 part of root-resistant agent, and 0.2 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 170°C, the stirring speed is 100 rpm, and the stirring time is 10 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0031] The buttering agent contains 70 parts of 90# bitumen, 8 parts of 10# bitumen, 30 parts of 200# bitumen, 10 parts of polyphenylpyrrolidone, 8 parts of SBS, 6 parts of 10# arene oil, 60 parts of swelling soil, 1.5 parts of root-resistant agent, and 0.7 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 140℃, adding 10# arene oil and SBS, stirring uniformly at 155℃, grinding until all the mixture expands, adding swelling soil, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0032] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0033] S1. At 185℃, the polyester felt layer is dip-coated with prepreg.
[0034] S2. The polyester felt layer is dip-coated at 185℃ and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0035] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 3
[0036] Example 3 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0037] S0. Preparation of raw materials.
[0038] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0039] The buttering agent contains 50 parts of 90# bitumen, 5 parts of 10# bitumen, 25 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene oil, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130℃, adding 10# arene oil and SBS, stirring uniformly at 155℃, grinding until the entire mixture expands, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0040] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0041] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0042] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0043] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 4
[0044] Example 4 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0045] S0. Preparation of raw materials.
[0046] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0047] The buttering agent contains 50 parts of 90# bitumen, 5 parts of 10# bitumen, 30 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 140℃, adding 10# arene oil and SBS, stirring uniformly at 130℃, grinding until it expands completely, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0048] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0049] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0050] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0051] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 5
[0052] Example 5 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0053] S0. Reserve of raw materials.
[0054] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0055] The buttering agent contains 50 parts of 90# bitumen, 6 parts of 10# bitumen, 25 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130~140℃, adding 10# arene oil and SBS, stirring uniformly at 155~175℃, grinding until it expands completely, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0056] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0057] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0058] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0059] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 6
[0060] Example 6 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0061] S0. Reserve of raw materials.
[0062] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0063] The buttering agent contains 50 parts of 90# bitumen, 7 parts of 10# bitumen, 25 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130-140℃, adding 10# arene oil and SBS, stirring uniformly at 155-175℃, grinding until it expands completely, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0064] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0065] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0066] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0067] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 7
[0068] Example 7 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0069] S0. Preparation of raw materials.
[0070] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0071] The buttering agent contains 50 parts of 90# bitumen, 8 parts of 10# bitumen, 25 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130~140℃, adding 10# arene oil and SBS, stirring uniformly at 155~175℃, grinding until it expands completely, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0072] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0073] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0074] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0075] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained. Example 8
[0076] Example 8 A highly durable, perforation-resistant polymeric waterproof coil material includes a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, a polyethylene film layer, a polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer, which are arranged from top to bottom, and a preparation method thereof includes the following steps:
[0077] S0. Preparation of raw materials.
[0078] The prepreg contains 70 parts of 90# bitumen, 15 parts of dihydroxypolydimethylsiloxane, 0.5 parts of root-resistant agent, and 0.1 parts of nano-silver antibacterial agent. The 90# bitumen and dihydroxypolydimethylsiloxane are mixed uniformly at 165°C, the stirring speed is 80 rpm, and the stirring time is 15 minutes. The root-resistant agent and nano-silver antibacterial agent are further added and mixed uniformly to obtain the prepreg.
[0079] The buttering agent contains 60 parts of 90# bitumen, 5 parts of 10# bitumen, 25 parts of 200# bitumen, 5 parts of polyphenylpyrrolidone, 4 parts of SBS, 5 parts of 10# arene, 40 parts of talcum powder, 1 part of root-resistant agent, and 0.4 parts of nano silver antibacterial agent. The buttering agent is prepared by uniformly mixing 90# bitumen, 10# bitumen, and 200# bitumen at 130~140℃, adding 10# arene oil and SBS, stirring uniformly at 155~175℃, grinding until it expands completely, adding talcum powder, root-resistant agent, and nano silver antibacterial agent, and stirring uniformly to obtain the buttering agent.
[0080] The polyester felt layer is obtained by weaving polyester filaments into a polyester padding.
[0081] S1. At 175℃, the polyester felt layer is dip-coated with prepreg.
[0082] S2. The polyester felt layer is dip-coated at 175°C and then coated by buttering, so that an elastomer-modified bitumen layer is formed on the upper and lower surfaces of the polyester felt layer.
[0083] S3. The upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer modified bitumen layer, are further coated with polyethylene film to obtain a polyethylene film layer. After cooling and shaping, a highly durable, perforation-resistant polymeric waterproof coil material is obtained.
[0084] Comparison 1 The only difference from Example 1 is that the dihydroxypolydimethylsiloxane in the prepreg is replaced with a dimethyl silicone polymer.
[0085] Comparison 2 The only difference from Example 1 is that dihydroxypolydimethylsiloxane is not incorporated into the prepreg.
[0086] Comparison 3 The only difference from Example 1 is that polyphenylpyrrolidone is not added to the buttering agent.
[0087] The highly durable, perforation-resistant, waterproof polymeric coil materials obtained in Examples 1 to 8 and Comparative Examples 1 to 3 were subjected to the following performance tests.
[0088] (1) Oil penetration performance is measured based on the method specified in GB / T18242~2008 "Elastomer-modified bituminous waterproof coil material."
[0089] (2) Artificial climate accelerated aging shall be measured in accordance with the method specified in GB / T18244-2000 "Aging test method for building waterproof materials."
[0090] The test results are shown in the table below.
[0091] Table 1. Test results of waterproof coil materials for Examples 1 to 8 and Comparative Examples 1 to 3 JPEG2024541160000001.jpg7298
[0092] From the data in the above table, it is known that the oil penetration performance requirements of the waterproof coil material in Examples 1 to 8 are all ≦1 sheet, and the tensile retention rate (horizontal and vertical directions) after accelerated aging by artificial air conditioning is all ≧91%, which complies with the requirements of GB / T35468-2017 "Root-resistant waterproof coil material for planted roofs".
[0093] In comparison with Examples 3 to 8, Example 1 illustrates that the aging resistance of the waterproof coil material in Example 3 is better, and that the aging resistance of the waterproof coil material can be enhanced by the synergistic effect of 10# bitumen and 200# bitumen with a specific mass ratio and 90# bitumen.
[0094] In Example 1, compared with Comparative Examples 1 to 3, the tension of the oil penetration performance is lower, and the tensile retention rate is higher after accelerated aging by artificial air conditioning. This shows that the addition of dihydroxypolydimethylsiloxane to the dip coating material of the elastomer-modified bitumen layer in the present invention and the addition of polyphenylpyrrolidone to the buttering material effectively prevents the transfer of oil in the elastomer-modified bitumen layer, thereby enhancing the oil penetration resistance of the waterproof coating material, and further significantly increasing the aging resistance of the waterproof coil material.
[0095] The waterproof coil material of Example 1 is sent to Beijing Municipal Institute of Garden Science to test its root puncture resistance.
[0096] The detection results showed that the plant growth in the test boxes reached 80% (height and trunk diameter) of that in the control boxes during the entire test period, and there was no root puncture phenomenon in any of the test boxes.
[0097] The detection conclusion is that the root puncture resistance performance of the detected elastomer-modified bitumen root-puncture resistant waterproof coil material (sample number: 2019B013) complies with the provisions of "Root-puncture resistant waterproof coil material for planted roofs" (GB / T35468~2017).
[0098] The waterproof coil material of Example 1 was sent to the National Building Materials Industrial Building Enclosure Materials and Pipe Products Quality Supervision and Testing Center. The items tested were thickness, mildew resistance, mildew corrosion resistance, seam peel strength, area, unit area mass, thickness, appearance, soluble matter content, heat resistance, low temperature flexibility, watertightness, maximum peak tension, maximum peak elongation, mass increase after immersion in water, heat aging, oil penetration performance, seam peel strength, thickness of the bituminous coating layer on the coil material bottom surface, and aging accelerated by artificial air conditioning. The test conclusion is that after the sample is tested, the tested items comply with the indicator requirements of GB / T35468~2017 "Root-resistant waterproof coil material for planted roofs".
[0099] The above are only preferred embodiments of the present invention, and are not intended to limit the present invention. Any modifications, equivalent replacements and improvements within the spirit and principle of the present invention will fall within the protection scope of the present invention.
Claims
1. A polyethylene film layer, an elastomer-modified bitumen layer, a polyester felt layer, an elastomer-modified bitumen layer, and a polyethylene film layer are arranged from top to bottom, the elastomer-modified bitumen layer includes raw materials of prepreg and buttering material, the prepreg includes components of 70-80 parts of 90# bitumen, 15-20 parts of dihydroxypolydimethylsiloxane, 0.5-1 part of root-resistant agent, and 0.1-0.2 parts of antibacterial agent by weight, the buttering material includes components of 50-70 parts of 90# bitumen, 5-8 parts of 10# bitumen, 20-30 parts of 200# bitumen, 5-10 parts of polyphenylpyrrolidone, 4-8 parts of SBS, 5-6 parts of plasticizer, 40-60 parts of filler, 1-1.5 parts of root-resistant agent, and 0.4-0.7 parts of antibacterial agent by weight, The prepreg is prepared by uniformly mixing 90# bitumen and dihydroxypolydimethylsiloxane at 165-170°C, then adding and uniformly mixing the root-resistant agent and antibacterial agent to obtain the prepreg. The mass ratio of 90# bitumen, 10# bitumen and 200# bitumen in the buttering agent is 10:1:5; A highly durable, perforation-resistant, waterproof polymer coil material.
2. 2. The highly durable, perforation-resistant, waterproof polymeric coil material according to claim 1, wherein the filler is one or more of talcum powder, swelling earth, diatomaceous earth, and fly ash.
3. 3. The highly durable, perforation-resistant, waterproof polymer coil material according to claim 2, wherein the plasticizer is arene oil.
4. The highly durable, puncture-resistant, waterproof polymer coil material according to claim 1, wherein the antibacterial agent is a nano-silver antibacterial agent.
5. The highly durable, perforation-resistant polymeric waterproof coil material according to claim 1, characterized in that when mixing the 90# bitumen and dihydroxypolydimethylsiloxane, the stirring speed is 80 to 100 revolutions per minute and the stirring time is 10 to 15 minutes.
6. Step S1 of dip-coating a prepreg for a polyester felt layer at 175 to 185°C; Step S2: applying a buttering agent for a polyester felt layer dip-coated at 175 to 185° C. to form an elastomer-modified bitumen layer on the entire upper and lower surfaces of the polyester felt layer; S3: further covering the upper and lower surfaces of the coated polyester felt layer, i.e., the surface of the elastomer-modified bitumen layer, with polyethylene film to obtain a polyethylene film layer, and cooling and shaping the polyethylene film layer to obtain a highly durable, perforation-resistant polymeric waterproof coil material; The method for preparing a highly durable, puncture-resistant, waterproof polymeric coil material according to any one of claims 1 to 5, comprising:
Citation Information
Patent Citations
Aqueous PVC foaming material
CN109291551A
High polymer modified asphalt waterproof roll and production process thereof
CN110318259A
Indoor decoration thermal insulation and waterproof material and construction method thereof
CN111472507A
Roofing product with increased tear strength comprising a release agent
US20100255743A1