Method for producing a catalyst on a substrate
By applying a metal layer to a substrate and exposing it to a corrosive solution, the method addresses the limitations of current catalyst supports in AWS systems, producing cost-effective and scalable catalysts with enhanced electrocatalytic performance.
Patent Information
- Application Number
- JP2024524386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-22
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-08
AI Technical Summary
Current catalyst supports for alkaline water splitting (AWS) systems are limited by the need for high-temperature processes, lack of variety, and the requirement for expensive materials, which hampers scalability and increases costs.
A method involving the application of a metal layer, such as nickel, on a substrate followed by exposure to a corrosive solution to form a catalyst, which can include earth-abundant metals like nickel and nickel-based materials, forming a sacrificial layer that protects the substrate and enhances catalytic activity.
This method allows for the production of cost-effective, scalable catalysts that maintain structural integrity and enhance electrocatalytic performance, reducing the need for high-temperature processes and enabling the use of diverse substrate materials.
Smart Images

Figure 2024541221000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to methods for producing catalysts on substrates. The present disclosure also relates to methods for regenerating catalysts on metal surfaces. The present disclosure also relates to catalysts produced using the methods disclosed herein. The present disclosure also relates to substrates and electrodes including catalysts produced using the methods disclosed herein. [Background technology]
[0002] As climate change becomes an increasingly important issue, it becomes more urgent to shift energy production from fossil fuels to renewable sources. Converting currently intermittent renewable energy sources into stable, storable chemical fuels is key to ensuring the sustainable delivery of renewable energy to citizens.
[0003] Hydrogen production via water splitting, where water molecules split into hydrogen and oxygen at the cathode and anode, respectively, is an attractive alternative to traditional renewable energy production. When used as fuel in fuel cells, hydrogen offers many advantages, such as a high energy density per unit mass, allowing for efficient energy production. Furthermore, hydrogen production is harmless to the environment, as the only by-product released is water.
[0004] From an industrial perspective, alkaline water splitting (AWS) systems hold particular promise as they are versatile and relatively easy to scale and upgrade, thanks to the wide range of catalysts they can use, including the inexpensive, non-precious metal catalysts used in hydrogen production processes.
[0005] Solar generation of molecular hydrogen from water is therefore a key component of the clean hydrogen economy of the future.
[0006] The challenges in developing suitable electrodes for AWS remain manifold: ensuring high performance in electrocatalysis at the anode is crucial, given the need to overcome the relatively slow rate of the oxygen evolution reaction (OER) compared to the hydrogen evolution reaction (HER) at the cathode.
[0007] Catalysis or electrocatalysis plays a key role in overcoming the kinetic energy barrier for the electrochemical reaction of water, oxygen and hydrogen in water splitting cells and fuel cells.
[0008] However, due to the reaction conditions of the water splitting process and the manufacturing conditions of current catalyst manufacturing methods, the variety of catalyst support materials is currently limited.
[0009] Catalyst supports are required to be electrically conductive and chemically robust against the harsh corrosive conditions encountered during water splitting operations. In addition, the high temperature reaction conditions of existing electrocatalyst deposition methods require the same supports to have good temperature stability. Currently, titanium and steel substrates meet all of the above criteria and are the primary supports for current AWS systems.
[0010] The limited number of catalyst supports available for hydrogen production severely impacts the scalability of the process at industrial level, and therefore there is a need to increase the variety of materials that can be used as catalyst supports, as well as a need for cheaper alternatives, e.g. non-metallic substrates.
[0011] There is also a need for the development of highly active, stable, and inexpensive electrochemical catalysts that can maximize hydrogen production. In this regard, there is also a need for catalytic systems that utilize relatively inexpensive, earth-abundant materials. As used herein, "earth-abundant" means present in the earth's crust at concentrations greater than 1 ppm.
[0012] Where any prior art is referenced in this specification, it should be understood that such reference is not an admission that that prior art forms part of the common general knowledge in the field in Australia or any other country. Summary of the Invention
[0013] According to one aspect, there is provided a method for producing a catalyst on a substrate, the method comprising the steps of: Providing a substrate having a metal layer thereon; and contacting the metal layer with a corrosive solution to form a catalyst.
[0014] As used herein, the term "catalyst" has its ordinary art meaning of a substance that increases the rate of a chemical reaction without itself undergoing any permanent chemical change.
[0015] The method may further include forming a layer of metal on the substrate to form a metallized substrate.
[0016] In some embodiments, the metal layer comprises an earth abundant metal. The metal layer may comprise one or more transition metals. The metal layer may comprise one or more metals selected from, for example, nickel, molybdenum, iron, cobalt, copper, manganese, zinc, and / or combinations thereof. Nickel (Ni) and Ni-based materials have shown good catalytic activity in electrolysis processes, such as hydrogen production via water splitting. Ni is also cheap and readily available, and has shown relatively good catalytic performance in both the oxygen evolution reaction (OER) and the hydrogen evolution reaction (HER).
[0017] The thickness of the metal layer can be adjusted as desired. However, the thickness is preferably sufficient to retain suitable structural flexibility for adhesion to the bulk of the support. Additionally, the thickness of the metal layer is preferably thick enough to prevent complete film etching / removal during the solution corrosion process. Thus, the metal layer must contain the amount of metal required for the corrosion process to occur and the catalyst to form while maintaining the desired electrical conductivity of the metal layer required for the intended application, such as performance as an electrode in electrochemical applications such as hydrogen production via water splitting.
[0018] The substrate may be completely covered by the metal layer such that no part of the substrate is exposed during the subsequent etching step.
[0019] In some embodiments, the metal layer has a minimum thickness of 0.5 μm. In some embodiments, the metal layer has a minimum thickness of 1.0 μm. In some embodiments, the metal layer has a minimum thickness of 1.5 μm. In some embodiments, the metal layer has a minimum thickness of 2 microns. In some embodiments, the metal layer has a minimum thickness of 2.5 μm.
[0020] In one embodiment, the metal layer has a thickness of up to 10 microns. In one embodiment, the metal layer has a thickness of up to 8 microns. In one embodiment, the metal layer has a thickness of up to 7 microns. In one embodiment, the metal layer has a thickness of up to 5 microns. In one embodiment, the metal layer has a thickness of up to 3 microns.
[0021] Apart from acting as a sacrificial metal layer for catalyst generation, the metal layer also serves as a chemical protection layer for the underlying substrate, which would otherwise be damaged in the harsh chemical environments that may be present during, for example, electrolysis operations or water splitting reactions. The metal layer obviates the need for the substrate to be a chemically stable material, for example to serve as an electrode substrate.
[0022] In some embodiments, forming a metal layer on the substrate comprises electroplating a metal on the substrate. The metal layer may be applied, for example, by electroplating the substrate using a metal halide electrolyte. In one embodiment, the metal layer is applied by electroplating the substrate using an electrolyte including a chloride solution of an earth abundant metal. The earth abundant metal may be a transition metal. In one embodiment, the metal layer is applied by metal plating the substrate using a Ni(II) chloride solution as the electrolyte to form a Ni layer on the substrate. In another embodiment, a Ni(II) sulfate solution is used as the electrolyte to apply the Ni layer on the substrate. In yet another embodiment, a Ni(II) acetate solution is used as the electrolyte to apply the Ni layer on the substrate.
[0023] In some embodiments, another suitable metal deposition method may be used to apply the metal layer on the substrate, for example, in some embodiments, the metal layer is applied by one or more of electroless plating, chemical vapor deposition, or wet chemical methods.
[0024] The deposited metal layer may include only one metal, such as Ni, or in other embodiments, the deposited metal layer may include two or more metals. The metal layer may include nickel. The metal combination may further include one or more of Mo, Co, Fe, Cu, Mn, and Zn. Examples of metal combinations that may be present in the metal layer include Ni-Mo, Ni-Co, Ni-Fe, Ni-Fe-Cu, Ni-Mo-Zn, Ni-Fe-Mo, and Ni-Mn-Fe-Mo.
[0025] In some other embodiments, forming a metal layer on the substrate comprises attaching a metal plate or flake onto the substrate. In some embodiments, the metal plate or flake is attached to the substrate using an adhesive layer, such as Ag paint. In other embodiments, the metal plate or flake is attached to the back side of the substrate by soldering.
[0026] Substrates may be selected from a wide variety of materials including, but not limited to, semiconductors (e.g., Si and / or GaAs), metals (e.g., copper mesh, copper plate or stainless steel), non-metals and polymers (e.g., polyethylene terephthalate (PET), polypropylene (PP), high density polyethylene (HDPE)).
[0027] In some embodiments, the substrate is an electrode.
[0028] In one embodiment, the substrate is a photovoltaic cell.In one embodiment, the substrate is a GaAs PV cell.
[0029] When the method of the present invention is applied to the preparation of catalysts on semiconductors, it has the advantage that it avoids solution-induced corrosion of the semiconductor, which may impair the performance and life of the photoelectrode. Furthermore, when the semiconductor forms part of a semiconductor-based photoelectrode device, the metal layer formed on the semiconductor substrate during the implementation of the method of the present invention protects the semiconductor during the water splitting operation, thereby stabilizing the performance of the photoelectrode device.
[0030] The method of the present invention includes contacting a metal layer on a substrate with a corrosive solution to form a catalyst. As used herein, the term "corrosive solution" refers to an aqueous solution that chemically reacts with and oxidizes the metal layer.
[0031] In some embodiments, contacting the metal layer with the corrosive solution includes immersing a substrate with a metal layer thereon in the corrosive solution.
[0032] In other embodiments, contacting the metal layer with the corrosive solution includes spraying or otherwise applying the corrosive solution to the metal layer.
[0033] In some embodiments, the etching solution is a halide solution. The etching solution may be, for example, a metal halide solution. In certain embodiments, the etching solution is a transition metal halide solution.
[0034] The metal halide may be present in the solution at a minimum concentration of 1 mM. In another embodiment, the metal halide may be present in the solution at a minimum concentration of 1.5 mM. In another embodiment, the metal halide may be present in the solution at a minimum concentration of 5 mM. In another embodiment, the metal halide may be present in the solution at a minimum concentration of 10 mM.
[0035] The metal halide may be present in the solution at a maximum concentration of 1 M. In an embodiment, the metal halide may be present in the solution at a maximum concentration of 0.5 M. In another embodiment, the metal halide may be present in the solution at a maximum concentration of 0.1 M. In another embodiment, the metal halide may be present in the solution at a maximum concentration of 0.05 M. In another embodiment, the metal halide may be present in the solution at a maximum concentration of 0.01 M.
[0036] The pH of the etching solution may be acidic. The pH may be less than 7. The pH may be at least 2. In an embodiment, the pH is at least 2.5. In another embodiment, the pH is at least 3.
[0037] The etching solution may include one or more metal salts. The metal salts may include one or more transition metal salts.
[0038] The etching solution may be, for example, a metal chloride solution.
[0039] The corrosion solution may include one or more transition metal chlorides. The transition metal chlorides may include nickel chloride and / or iron chloride.
[0040] The etching solution may include one or more transition metal nitrates. The transition metal nitrates may include nickel nitrate and / or iron nitrate.
[0041] In some embodiments, the etching solution is a mixture of chlorides of Ni(II) and Fe(III), while in other embodiments, the etching solution is a mixture of nitrates of Ni(II) and Fe(III).
[0042] The molar ratio of Ni:Fe may be at least 1:2. In some embodiments, the molar ratio is at most 2:1. In one embodiment, the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the mixture of Ni(II) and Fe(III) nitrates is 1:1. In another embodiment, the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the mixture of Ni(II) and Fe(III) nitrates is 1:2. In yet another embodiment, the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the mixture of Ni(II) and Fe(III) nitrates is 2:1.
[0043] The temperature of the etching step can be room temperature or an elevated temperature. By "elevated temperature" it is meant a temperature higher than room temperature. In some embodiments, the step of contacting the metal layer with the etching solution is carried out at room temperature. In other embodiments, the step of contacting the metal layer with the etching solution is carried out at a temperature of at least 40° C. In other embodiments, the step of contacting the metal layer with the etching solution is carried out at a temperature of at least 60° C. In yet other embodiments, the step of contacting the metal layer with the etching solution is carried out at a temperature of at most 90° C. In yet other embodiments, the step of contacting the metal layer with the etching solution is carried out at a temperature of at most 80° C.
[0044] The metal layer may be exposed to the corroding solution for a sufficient period of time to initiate corrosion of the metal and form a corrosion product. The time the metal layer is exposed to the corroding solution may be adjusted as desired, with longer periods resulting in greater conversion of the metal to catalyst. The optimal time depends on many factors, including the concentration and temperature of the corroding solution. The metal layer may be exposed to the corroding solution for up to 60 minutes. In one embodiment, the metal layer is exposed to the corroding solution for up to 30 minutes. In another embodiment, the metal layer is exposed to the corroding solution for up to 15 minutes. In another embodiment, the metal layer is exposed to the corroding solution for up to 10 minutes. In another embodiment, the metal layer is exposed to the corroding solution for up to 5 minutes.
[0045] During the etching step, the etching solution reacts with at least a portion of the metal in the metal layer to form a corrosion product. The corrosion product may be formed in situ on the outer surface of the metal layer, thereby forming a layer of the corrosion product on the unreacted metal of the metal layer. The corrosion product may include a catalyst.
[0046] In some embodiments, the catalyst is an electrocatalyst.
[0047] In some embodiments, the catalyst comprises one or more metal hydroxides.
[0048] In some embodiments, the catalyst is a monometallic hydroxide.
[0049] In some embodiments, the catalyst is a multimetallic hydroxide.
[0050] In some embodiments, the catalyst is a polymetallic layered double hydroxide (LDH).
[0051] In some embodiments, the catalyst comprises one or more transition metals. The one or more transition metals may be selected from Ni, Fe, Co, Mo, and Cu. The catalyst may comprise at least nickel. In some embodiments, the catalyst is selected from NiFe hydroxide, NiCoFe hydroxide, NiMo hydroxide, NiCuFe hydroxide, and / or combinations thereof.
[0052] In certain embodiments, when a metal layer is contacted with a corrosive solution, a redox process occurs on the metal surface where the metal is oxidized to form a monometallic or polymetallic layered double hydroxide (LDH) catalyst.
[0053] In one embodiment, the catalyst is a NiFe LDH catalyst.
[0054] In some embodiments, the inventive method further comprises applying a seed layer to the substrate prior to forming or applying the metal layer. The seed layer may promote adhesion of the metal layer to the substrate.
[0055] In some embodiments, the seed layer has a thickness of a minimum of 50 nm.
[0056] In some embodiments, the seed layer has a thickness of approximately 100 nm.
[0057] In some embodiments, the composition of the seed layer includes Ti and / or Ni.
[0058] In some embodiments, the seed layer includes at least one of a Ti layer and a Ni layer.
[0059] In some embodiments, the Ti layer has a minimum thickness of 50 nm.
[0060] In some embodiments, the Ni layer has a minimum thickness of 50 nm.
[0061] In some embodiments, applying a seed layer to the substrate comprises depositing the seed layer by electron beam evaporation. In some other embodiments, applying a seed layer to the substrate comprises depositing the seed layer by thermal evaporation. In yet some embodiments, applying a seed layer to the substrate comprises depositing the seed layer by sputter deposition.
[0062] According to another aspect, there is provided a method of regenerating a catalyst on a metal surface, the method comprising: removing any spent or residual catalyst from the metal surface to produce a clean metal surface; and contacting the clean metal surface with the corrosive solution to regenerate new catalyst on the metal surface.
[0063] The method provides an effective way to regenerate catalyst on used metal or metal plate substrates, and further reduces the cost of replacing the metal substrate or redepositing onto a new substrate before producing new catalyst on the substrate.
[0064] In some embodiments, the metal surface comprises a surface of a metal foil.
[0065] In another embodiment, the metal surface comprises a metallized substrate surface.
[0066] In some embodiments, removing any spent or residual catalyst from the metal surface comprises treating the metal surface with an etchant.
[0067] In some embodiments, the etchant comprises a mineral acid. In one embodiment, the etchant comprises hydrochloric acid (HCl). In some other embodiments, the etchant comprises sulfuric acid (H2SO4). In some other embodiments, the etchant comprises a combination of hydrochloric acid (HCl) and sulfuric acid (H2SO4).
[0068] According to another aspect, there is provided a catalyst produced by a method according to any of the embodiments discussed above.
[0069] According to another aspect, there is provided a substrate including thereon a catalyst produced according to any of the embodiments discussed above.
[0070] According to another aspect, there is provided an electrode comprising a catalyst produced by a method according to any of the embodiments discussed above.
[0071] Advantages of the method of the present invention include: The method can be inexpensive. -Can be adapted to a variety of metallic surfaces. The method does not require high temperatures and can be carried out at room temperature. Given that the method may occur widely on metallic surfaces and may not require high temperature activation, the substrate may comprise a wide variety of compositions having a suitable thin conductive metal layer thereon. [Brief description of the drawings]
[0072] Embodiments will now be described, by way of example only, with reference to the accompanying drawings in which: [Figure 1] 1 is a schematic diagram illustrating an embodiment of a manufacturing process disclosed herein. [Diagram 2] Photographs of Ni electroplated on various substrates before and after forming NiFe LDHs are shown. [Figure 3(a)] FIG. 13 is an EDS mapping image of a cross-sectional area of NiFe LDHs formed on a Ni surface. References for the reference EDS mapping images of Ni, Fe, and O are shown on the right. [Figure 3(b)-(c)] (b) is an SEM image of Ni electroplated on a Si surface, and (c) is an SEM image of NiFe LDHs formed on the Ni surface. [Figure 4(a)-(c)]Graph showing the performance comparison of Ni electroplated Si with and without NiFe LDH catalyst: (a) forward LSV scan at 0.01 V / s, (b) EIS Nyquist spectrum at RHE reference potential 1.49 V, (c) chronopotentiometry results at 10 mA cm-2 of NiFe LDH catalyst formed on Ni deposited on various substrates. [Figure 4(d)-(e)] Overpotential measurements of NiFe LDH. (d) Measurements of the overpotential of NiFe LDH deposited on various substrates at 10 and 50 mA cm-2. (e) Measurements of the overpotential of NiFe LDH deposited on various substrates at 10 mA cm-2 after varying the number of depositions and etchings with 0.1 M HCl (Si substrate). [Figure 5(a)] Schematic of a photovoltaically assisted GaAs photoanode with NiFe LDH deposited on the backside. [Figure 5(b)-(d)] Current-voltage and chronoamperometry characteristics of the photoanode in Figure 4(a). (b) JV curve of the photoanode and applied bias photon-to-current efficiency (ABPE) in 1.0 M KOH measured under AM 1.5G 1 solar illumination. (c) Incident photon-to-current conversion efficiency (IPCE) of the photovoltaically assisted GaAs photoelectrode with NiFe LDH catalyst measured relative to the AM 1.5G solar spectrum. (d) Chronoamperometry results at 1.3 V RHE reference. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0073] In the following detailed description, reference is made to the accompanying drawings, which form a part of the detailed description. The exemplary embodiments described in the detailed description are represented in the drawings and defined in the claims, and are not intended to be limiting. Other embodiments may be utilized, and other changes may be made, without departing from the spirit and scope of the subject matter presented. It will be readily understood that the aspects of the present disclosure, as broadly described herein and depicted in the drawings, can be arranged, substituted, combined, separated, and designed in a wide variety of different configurations, all of which are contemplated to be within the present disclosure.
[0074] The present disclosure provides methods for producing catalysts on various substrates and / or supports, the methods including (i) coating a metal layer on a substrate to form a metallized substrate, and (ii) contacting the metal layer with a corrosive solution to form a catalyst layer.
[0075] A method for producing a catalyst on a substrate is described herein, by way of example, with reference to the Figures.
[0076] According to the embodiment illustrated in FIG. 1, the method includes coating a seed layer on a substrate and then coating a metal layer, where the seed layer promotes adhesion of the metal layer to the substrate.
[0077] In the described embodiment, the seed layer is deposited on one side of the substrate using electron beam evaporation, although any other suitable deposition method may be used, for example in some embodiments the seed layer is coated by chemical bath deposition.
[0078] In the described embodiment, the composition of the seed layer includes Ti and Ni. In particular, the seed layer is composed of a 50 nm Ti layer and a 50 nm Ni layer. In the described embodiment, the Ti layer is deposited on the substrate and the Ni layer is deposited on the Ti layer.
[0079] The seed layer improves or provides conductivity to the underlying substrate, and the Ti layer also helps improve adhesion of the metal layer (in this case, the Ni layer) during the subsequent plating step.
[0080] However, the composition and thickness of the seed layer can be selected as desired and tailored to the particular application of the catalyst in the catalytic process.
[0081] The substrate shown in FIG. 1 is approximately 1 cm 2 Although the present invention has a geometric area of 0.1 m, the method is scalable and applicable to larger areas.
[0082] According to the described embodiment, after deposition of the seed layer, a metal layer is coated onto the substrate by electroplating. Note that deposition of the seed layer is optional, and that in some embodiments, the metal layer is directly coated onto the substrate.
[0083] In the described embodiment, the Ni layer is applied by electroplating, in particular by depositing the Ni layer on the substrate using a Ni(II) chloride solution as the electrolyte.
[0084] Electroplating was performed using a 0.36 M Ni(II) chloride solution at 20 mA / cm 2 It will be carried out.
[0085] 1, the thickness of the metal layer according to the described embodiment is approximately 2-3 microns, however, the thickness of the metal layer can be adjusted as desired and / or according to the particular requirements of the catalytic reaction.
[0086] 1, after Ni electroplating onto the substrate, the deposited metal layer is contacted with a corrosion solution by immersing the substrate in the corrosion solution. As will be described in more detail below with reference to the described embodiments, the corrosion reaction converts a portion of the deposited metal into a catalytic material.
[0087] In the described embodiment, the substrate is immersed in a 15 mM mixed solution of Ni(II) and Fe(III) chlorides in a 1:1 molar ratio for 1 min. The chloride ions in the solution initiate the corrosion process of the electroplated Ni layer and form NiFe double hydroxides on the film surface. The substrate is then dried at 70° C. for 1 h. EXAMPLES
[0088] Substrates made from a variety of materials, including semiconductors (Si and GaAs), metals (copper mesh, copper plate, stainless steel), and polymers (PET), were coated using the method described in FIG. 1. In particular, one side of the substrate (approximate geometric area: 1 cm 2 ) was coated with a Ti / Ni layer (50 nm / 50 nm) using electron beam evaporation to serve as a conductive seed layer.
[0089] The substrate was then electrochemically stained with 20 mA / cm using 0.36 M Ni(II) chloride solution as the electrolyte. 2 The copper was electroplated with Ni at 370.
[0090] After Ni electroplating, the substrate was immersed for 1 min in a 15 mM mixed solution of Ni(II) and Fe(III) chlorides with a molar ratio of 1:1. The chloride ions in the solution initiated the corrosion process of the electroplated Ni film, and NiFe double hydroxides were formed on the film surface.
[0091] Finally, the substrate was dried at 70°C for 1 h.
[0092] Figure 2 shows photographs of Ni electroplated substrates before and after the formation of NiFe LDHs. After the electroplating process, all substrates showed a uniform thickness of Ni film across the substrate, with good substrate-film adhesion. Although some corrosion of the Ni film is required for catalyst formation, the integrity of the film remained intact up to this step, as shown in Figure 3(a). Figure 3(a) is an energy-dispersive spectroscopy (EDS) image of a cross-sectional area of a Ni electroplated substrate immersed in a solution mixture of Ni(II) and Fe(III), showing NiFe LDHs formed on the Ni surface. The EDS image shows a bottom layer (10-20 nm thick) composed of Ni, and a characteristic Fe / O layer (10-20 nm thick) on top of the Ni layer. The Fe / O layer indicates successful catalyst formation on the Ni surface by the corrosion process. As shown in Figure 3(a), the Fe / O layer did not infiltrate the entire Ni metal layer, preserving its integrity and reusability.
[0093] Upon completion of the chloride immersion process, a visible change in the appearance of the Ni film was observed on all substrates, with a brown, rust-like appearance evident, in contrast to the metallic grey appearance typically seen in untreated Ni films.
[0094] Figures 3(b) and (c) show top-view scanning electron microscope (SEM) images of the Ni film, which showed a significantly corroded appearance on the previously shiny textured surface, suggesting the formation of a thin catalytic layer on the surface.
[0095] Voltammetry measurements of Ni electroplated Si substrates with and without catalyst were carried out to determine the improvement in catalytic properties brought about by NiFe LDH. In particular, the OER performance of Ni electroplated Si substrates with and without catalyst was compared by connecting the substrate as the working electrode in a three-electrode cell with Pt plate and Ag / AgCl as counter and reference electrodes, respectively, in 1.0 M KOH solution (pH 13). The linear sweep voltammetry (LSV) curves (Figure 4(a)) of Ni electroplated on Si with and without NiFe LDH show that the OER performance at 10 mA cm -2 , showing a clearly lower overpotential in the presence of bimetallic hydroxide catalyst (308 mV) compared to the pure Ni layer (630 mV).
[0096] Furthermore, Nyquist plots (Fig. 4(b)) obtained from electrochemical impedance spectroscopy (EIS) of Ni-electroplated Si substrates with and without catalyst showed that the catalyst-supported Si substrates exhibited higher OER reaction rates than untreated Ni-electroplated Si due to lower charge transfer resistance.
[0097] From the viewpoint of stability, the NiFe LDH catalyst has a maximum catalytic activity of 10 mA cm -2 At this temperature, the OER activity could be sustained at the required overpotential for 24 h without significant deviation (Figure 4(c)), and similar results were also observed for Ni-plated stainless steel and GaAs substrates.
[0098] The OER performance test was carried out on all the evaluated substrates in Figure 2(a), and the results showed that the OER performance was 2 The overpotential values were relatively consistent across the substrate (Figure 4(d)), suggesting that the catalytic performance is independent of the substrate.
[0099] To demonstrate the reusability of the metal layer coated on the substrate for multiple catalyst regeneration steps, the NiFe LDH catalyst was removed from the catalyst-supported Si substrate by treating the substrate with an etching solution (0.1 M hydrochloric acid (HCl)) for 10 min. The cleaned metal surface was then immersed in a 15 mM mixed solution of Ni(II) and Fe(III) chlorides using the same immersion conditions as in the first immersion step. The etching-corrosion step was repeated four times. The overpotential was measured after each cycle to monitor the change in the catalytic performance.
[0100] Figure 3(e) shows the overpotential measurements of NiFe LDH catalyst on Si substrate before and after multiple cycles of etching the catalyst in 0.1 M hydrochloric acid (HCl) for 10 min, followed by regeneration of NiFe LDH using the same soaking conditions as the first soaking step. After each of the four etching-corrosion cycles, the catalyst performance remained relatively similar without any noticeable deterioration in performance. This suggests that the Ni layer deposited on the substrate can be reused multiple times to form a catalyst layer without the need to coat a new metal layer on the substrate each time.
[0101] The disclosed method can also be used to stabilize catalysts in photoelectrode devices based on III-V semiconductors, which perform well in (photovoltaic) PV and water splitting cells, but can suffer from photocorrosion in harsh electrolyte environments.
[0102] As outlined in FIG. 5(a), a commercial single-junction GaAs PV cell was electroplated with Ni on the backside and immersed in an etching solution to form a catalyst layer as described above.
[0103] As shown in Figure 5(b), under AM 1.5G 1 solar irradiance, the photoanode device outputs approximately 27 mA / cm 2A saturated photocurrent density of 1.01 nm was achieved (Figure 5(b)), which is within the expected range for a single-junction GaAs PV cell. The device also showed good photoresponse throughout the measured potential range, as shown by a comparison of the photocurrents generated under illumination and in the dark. From the resulting J-V curves, the ABPE was calculated to be approximately 11.7% at 0.52 V compared to the RHE (see Figure 5(b)). This is an excellent ABPE value for the photoanode. Furthermore, an incident photon-to-current efficiency (IPCE) of approximately 80% was achieved with this photoelectrode design in the specific range of 500–800 nm (Figure 5(c)). This indicates an overall good conversion efficiency of the photoelectrode, although some losses are expected due to absorption and reflection by the encapsulating glass in the illuminated region of the PV cell. The stability of the photoanode device was evaluated at the onset potential of the saturated photocurrent density (1.3 V vs. RHE), and the device performance lasted for 100 h (Figure 5(d)).
[0104] The experimental results discussed above and illustrated in the accompanying drawings demonstrate that methods according to the present disclosure can be used to construct and stabilize semiconductor electrodes for solar water splitting, achieving record photoanode efficiencies.
[0105] It will be understood that where any prior art publication is referenced to this specification, such reference is not an admission that that publication forms part of the common general knowledge in the art in Australia or any other country.
[0106] In the following claims, and in the foregoing description of the invention, unless otherwise required by clear language or necessary implication in the context, the term "comprises" and its conjugations are used in their inclusive sense, i.e., to specify the presence of stated features, but not to exclude the presence or addition of further features in various embodiments of the invention.
Claims
1. 1. A method for producing a catalyst on a substrate, comprising the steps of: providing a substrate having a metal layer thereon; contacting the metal layer with a corrosive solution to form a catalyst; A method for producing a catalyst comprising the steps of:
2. The method of claim 1 further comprising forming a metal layer on the substrate to form a metallized substrate.
3. The method of claim 1 or 2, wherein forming the metal layer on the substrate comprises electroplating a metal onto the substrate.
4. 4. The method of claim 1, wherein the metal layer is applied onto the substrate by electroplating the substrate using a metal halide electrolyte.
5. 5. The method of claim 1, wherein the metal layer is applied onto the substrate by electroplating on the substrate using an electrolyte comprising a chloride solution of an earth abundant metal.
6. 6. The method of claim 5, wherein the metal layer is applied onto the substrate by electroplating the substrate using a Ni(II) chloride solution as an electrolyte to form a Ni layer on the substrate.
7. 6. The method of claim 5, wherein the metal layer is applied onto the substrate by electroplating the substrate using a Ni(II) sulfate solution as an electrolyte to form a Ni layer on the substrate.
8. The method according to claim 1 , wherein the metal layer consists of only one metal, such as Ni.
9. The method of claim 1 , wherein the metal layer comprises two or more metals.
10. 10. The method of claim 9, wherein the metal layer comprises Ni and one or more metals selected from Mo, Co, Fe, Cu, Mn and Zn.
11. The method of claim 1 , wherein forming a metal layer on the substrate comprises applying a metal plate or foil onto the substrate.
12. The method according to claim 11 , wherein the metal plate or foil is attached to the substrate using an adhesive layer, for example Ag paint.
13. The method of claim 11 , wherein the metal plate or foil is attached to the back side of the substrate by soldering.
14. 14. The method of claim 1, further comprising applying a seed layer to the substrate, followed by forming the metal layer.
15. The method of claim 1 , wherein the substrate is an electrode.
16. The method of claim 1 , wherein the substrate is a photovoltaic cell.
17. 17. The method of claim 1, wherein the substrate is a GaAs PV cell.
18. 1. A method for regenerating a catalyst on a metal surface, comprising: removing any spent or residual catalyst from said metal surface to produce a clean metal surface; and contacting the cleaned metal surface with a corrosive solution to regenerate fresh catalyst on the cleaned metal surface; A method comprising:
19. The method of claim 18 , wherein the metal surface comprises a surface of a metal foil.
20. The method of claim 18 , wherein the metal surface comprises a metallized substrate surface.
21. 21. The method of any one of claims 1 to 20, wherein the catalyst is an electrocatalyst.
22. 22. The method of any one of claims 1 to 21, wherein the catalyst comprises one or more metal hydroxides.
23. 23. The method of any one of claims 1 to 22, wherein the catalyst comprises one or more transition metals.
24. 24. The method of claim 23, wherein the one or more transition metals are selected from Ni, Fe, Co, Mo and Cu.
25. 25. The method of claim 24, wherein the catalyst comprises at least nickel.
26. 26. The method of any one of claims 1 to 25, wherein the catalyst is selected from NiFe hydroxide, NiCoFe hydroxide, NiMo hydroxide, NiCuFe hydroxide, and / or combinations thereof.
27. 27. The method of any one of claims 1 to 26, wherein contacting the metal layer or the cleaned metal surface with a corrosive solution comprises initiating an oxidation-reduction process at the metal surface, in which the metal is oxidized to form a monometallic or polymetallic layered double hydroxide (LDH) catalyst.
28. 28. The method of claim 27, wherein the catalyst is a NiFe LDH catalyst.
29. 29. The method of any one of claims 1 to 28, wherein the etching solution is a halide solution.
30. 30. The method of claim 29, wherein the etching solution is a metal halide solution.
31. 30. The method of claim 29, wherein the etching solution is a transition metal halide solution.
32. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in the solution at a minimum concentration of 1 mM.
33. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in solution at a minimum concentration of 1.5 mM.
34. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in solution at a minimum concentration of 5 mM.
35. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in the solution at a minimum concentration of 10 mM.
36. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in the solution at a maximum concentration of 1 M.
37. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in solution at a maximum concentration of 0.5 M.
38. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in solution at a maximum concentration of 0.1 M.
39. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in solution at a maximum concentration of 0.05M.
40. 32. The method of claim 30 or 31, wherein the metal halide or the transition metal halide is present in the solution at a maximum concentration of 0.01 M.
41. 41. The method of any one of claims 1 to 40, wherein the etching solution has an acidic pH.
42. 42. The method of any one of claims 1 to 41, wherein the pH of the etching solution is less than 7.
43. 42. The method of any one of claims 1 to 41, wherein the pH of the etching solution is at least 2.
44. 42. The method of any one of claims 1 to 41, wherein the pH of the etching solution is at least 2.
5.
45. 42. The method of any one of claims 1 to 41, wherein the pH of the etching solution is at least 3.
46. 46. The method of any one of claims 1 to 45, wherein the corrosive solution may include one or more metal salts.
47. 47. The method of claim 46, wherein the metal salt can include one or more transition metal salts.
48. 48. The method of any one of claims 1 to 47, wherein the etching solution comprises one or more transition metal chlorides.
49. 49. The method of any one of claims 1 to 48, wherein the corrosive solution is a metal chloride solution.
50. 50. The method of any one of claims 1 to 49, wherein the etching solution comprises one or more transition metal nitrates.
51. 51. The method of claim 50, wherein the transition metal nitrate comprises nickel nitrate and / or iron nitrate.
52. 52. The method of any one of claims 1 to 51, wherein the corrosive solution comprises nickel chloride and / or iron chloride.
53. 53. The method of claim 52, wherein the etching solution is a mixture of Ni(II) and Fe(III) chlorides.
54. 53. The method of claim 52, wherein the etching solution is a mixture of nitrates of Ni(II) and Fe(III).
55. 55. The method of any one of claims 52 to 54, wherein the molar ratio of Ni:Fe is at least 1:
2.
56. 55. The method of any one of claims 52 to 54, wherein the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the molar ratio of the mixture of Ni(II) and Fe(III) nitrates is 1:
1.
57. 55. The method of any one of claims 52 to 54, wherein the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the molar ratio of the mixture of Ni(II) and Fe(III) nitrates is 1:
2.
58. 55. The method of any one of claims 52 to 54, wherein the molar ratio of the mixture of Ni(II) and Fe(III) chlorides or the molar ratio of the mixture of Ni(II) and Fe(III) nitrates is 2:
1.
59. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer with the corrosive solution is carried out at room temperature.
60. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out at an elevated temperature.
61. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out at a minimum of 40°C.
62. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out at a temperature of at least 60°C.
63. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out at a temperature of up to 90°C.
64. 59. The method of any one of claims 1 to 58, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out at a temperature of up to 80°C.
65. 65. The method of any one of claims 1 to 64, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out for a period of up to 60 minutes.
66. 65. The method of any one of claims 1 to 64, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out for a period of up to 30 minutes.
67. 65. The method of any one of claims 1 to 64, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out for a period of up to 15 minutes.
68. 65. The method of any one of claims 1 to 64, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution is carried out for a period of up to 5 minutes.
69. 69. The method of any one of claims 1 to 68, wherein the step of contacting the metal layer or the cleaned metal surface with a corrosive solution comprises immersing a substrate having a metal layer thereon in the corrosive solution.
70. 70. The method of any one of claims 1 to 69, wherein the metal layer or surface comprises an earth abundant metal.
71. 71. The method of any one of claims 1 to 70, wherein the metal layer or surface comprises one or more transition metals.
72. 72. The method of any one of claims 1 to 71, wherein the metal layer or surface comprises one or more metals selected from, for example, nickel, molybdenum, iron, cobalt, copper, manganese, zinc, and / or combinations thereof.
73. 73. A catalyst produced using the method of any one of claims 1 to 72.
74. 73. A substrate comprising a catalyst produced using the method of any one of claims 1 to 72.
75. 73. An electrode comprising a catalyst produced using the method of any one of claims 1 to 72.
Citation Information
Patent Citations
Electrode for generating gas from alkaline electrolyte and production thereof
JP1982116785A
Light-transmitting oxygen evolution catalyst and production method of the same, and chemical reactor using the same