CATALYST FOR CATALYTIC CRACKING OF ETHYLENE, METHOD FOR PREPARATION THEREOF AND USE THEREOF
A catalyst made from crystalline TiO2 with a disordered surface layer, using used SCR catalysts, addresses the limitations of existing ethylene cracking catalysts by providing high activity, stability, and cost-effectiveness without noble metals.
Patent Information
- Application Number
- JP2024529233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-16
- Filing Date
- 2021-12-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-07
AI Technical Summary
Existing catalysts for ethylene cracking require expensive precious metals, suffer from thermal instability, and are prone to poisoning, necessitating the development of a low-cost, stable, and poison-resistant alternative.
A catalyst composed of crystalline TiO2 with an anatase crystal form and a disordered surface layer, utilizing used SCR denitrification catalysts as a raw material, which does not require noble metals, and is prepared through a process involving mixing, roasting, leaching, hydrolyzing, aging, and hydrogenating Ti-containing materials.
The catalyst achieves high ethylene cracking activity without noble metals, is resistant to poisoning, and can be easily regenerated, offering improved thermal stability and cost-effectiveness.
Smart Images

Figure 2024541397000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to Chinese Application No. 202111356393.6, filed on November 16, 2021, entitled "Catalyst for catalytic cracking of ethylene, its preparation method and its use," which is incorporated herein by reference.
[0002] The present disclosure relates to the technical field of catalytic degradation of ethylene, in particular to a catalyst for the catalytic degradation of ethylene, a method for preparing the same and its use. [Background technology]
[0003] Volatile organic compounds (hereinafter referred to as VOCs) are 2.5 and is an important precursor for the formation of O3. In order to further improve air quality, it is necessary to strengthen the comprehensive management of the coal chemical industry and other key industries related to VOC emissions. Current VOC treatment technologies are mainly classified into three categories: adsorption recovery technology, combustion technology, and adsorption concentration + combustion technology, and combustion technology is used to treat VOCs with insufficient recovery value. For example, volatile organic compounds generated in the coal chemical industry are mainly obtained from the coal gasification process and the process of washing tail gas with low-temperature methanol. VOCs have the characteristics of rich variety, low recovery value, large air volume, etc. Combustion technology can oxidize VOCs into harmless emissions of CO2 and H2O.
[0004] Catalytic combustion is one of the important means in combustion technology, and the key points of catalytic combustion technology include the design and fabrication of catalysts for the oxidation of VOCs. Catalysts for the oxidation of VOCs are typically composed of two parts, namely, supports and active components (precious metals). Ethylene is a common VOC gas in the coal chemical industry, and the commercially available catalysts for ethylene oxidation are mainly Pt / γ-Al2O3 catalysts. However, the active components, precious metals, are expensive, require a long supply cycle, and are basically dependent on imports from abroad. In addition, the commercially available Pt / γ-Al2O3 catalysts have defects such as undesirable thermal stability, low resistance to catalyst poisoning, etc.
[0005] In summary, it is essential to develop novel, low-cost, non-toxic, stable and environmentally friendly catalysts that can effectively reduce VOCs, which are air pollutants. Summary of the Invention [Problem to be solved by the invention]
[0006] The objective of the present disclosure is to overcome the problem in the prior art that a catalyst for catalytic cracking of ethylene requires a precious metal as an active component, and the present disclosure provides a catalyst for catalytic cracking of ethylene, a method for preparing the same and use thereof, and the catalyst for catalytic cracking of ethylene can achieve high catalytic activity for ethylene.
[0007] In the course of their research, the inventors of the present disclosure have discovered that the composition of a catalyst for catalytic cracking of ethylene contains K2O, Na2O, and TiO2 of anatase crystal form, and that the surface of the crystalline TiO2 has surface hydroxyl groups and Ti 3+ The present invention has been made by finding that when a catalyst is covered with a TiO2 disordered layer containing a noble metal, the catalyst can effectively decompose ethylene into CO2 and H2O without using a noble metal contained in the catalyst as an active component. [Means for solving the problem]
[0008] To achieve the above object, a first aspect of the present disclosure provides a catalyst for catalytic cracking of ethylene, comprising crystalline TiO2 and an auxiliary, the crystalline form of TiO2 being anatase type, and the surface of the crystalline TiO2 being covered with a TiO2 disordered layer containing surface hydroxyl groups.
[0009] In a second aspect, the present disclosure provides a method for making a catalyst for catalytic cracking of ethylene, comprising the steps of: (1) mixing a titanium source powder with an acid, and roasting the resulting mixture; (2) leaching the product obtained by roasting with water, followed by solid-liquid separation to obtain a Ti-containing filtrate; (3) hydrolyzing and aging the filtrate to obtain a metatitanic acid colloid containing auxiliary elements including Na and K; (4) washing, drying and calcining the metatitanic acid colloid to obtain nano-TiO2 powder; and (5) hydrogenating the nano-TiO2 powder to obtain a catalyst for catalytic cracking of ethylene; Wherein the titanium source powder is selected from spent SCR denitration catalyst containing Na2O and K2O.
[0010] In a third aspect, the present disclosure provides a catalyst for the catalytic cracking of ethylene made by the above method.
[0011] In a fourth aspect, the present disclosure provides a use of the above-mentioned catalyst for catalytic cracking of ethylene in cracking of ethylene.
[0012] Due to the above technical solutions, the present disclosure has the following beneficial effects: (1) The preparation method of the catalyst for catalytic cracking of ethylene according to the present disclosure, using the spent SCR catalyst containing Na2O and K2O additives as the raw material, can appropriately utilize the elements contained in the obtained anatase TiO2 prepared by the sulfuric acid method to provide acid sites for the hydrogenation of TiO2. Moreover, the structural defects of the prepared crystalline TiO2 can appropriately adjust its redox properties. (2) The catalyst for catalytic cracking of ethylene according to the present disclosure does not require the use of a transition metal or a precious metal as an active ingredient, so there is no need to deal with problems of catalyst poisoning or aging during the catalytic cracking of ethylene, and the catalyst can be easily regenerated after deactivation. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a process flow diagram illustrating a method for making a catalyst for catalytic cracking of ethylene according to the present disclosure. [Diagram 2] FIG. 2 is a diagram showing a comparison of the appearance between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and TiO2 powder. [Diagram 3] FIG. 2 is a comparison of X-ray diffraction patterns between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and TiO2 powder. [Figure 4] 1 is a comparative graph of nitrogen adsorption / desorption isotherms of the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure. [Diagram 5] FIG. 2 shows the EPR comparison between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and pure nano-TiO2. [Figure 6] 1 is a TEM image of a catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure. [Figure 7] FIG. 2 is a graph showing the relationship between the temperature and the ethylene conversion rate of the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure.
[0014] Explanation of symbols in the figure: 1 refers to TiO2 powder, and 2 refers to a catalyst for catalytic cracking of ethylene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The range endpoints and any values disclosed herein are not limited to the exact range or value, and such ranges or values should be understood to include the values adjacent to that range or value. With respect to numerical ranges, the various range endpoints, the various range endpoints and individual point values, and the individual point values can be combined with each other to generate one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0016] A first aspect of the present disclosure provides a catalyst for catalytic cracking of ethylene, the catalyst comprising crystalline TiO2 and an auxiliary, the crystalline form of the TiO2 being anatase type, and the surface of the crystalline TiO2 being covered with a disordered TiO2 layer containing surface hydroxyl groups.
[0017] The catalyst for catalytic cracking of ethylene provided by the present disclosure contains TiO2 in a crystalline form having a specific structure and an auxiliary, but does not contain a precious metal as an active component, and can provide a better catalytic cracking effect of ethylene.
[0018] In some embodiments of the present disclosure, the catalyst preferably comprises TiO2 in an amount of 99.9 to 99.99 wt%, based on the total weight of the catalyst.
[0019] In some embodiments of the present disclosure, the catalyst further comprises an auxiliary agent, which can advantageously promote the technical effect of improving the catalytic cracking of ethylene. Preferably, the auxiliary agent comprises K2O and Na2O, and the catalyst comprises K2O in an amount of 0.002-0.006 wt. % and Na2O in an amount of 0.006-0.098 wt. %, based on the total weight of the catalyst.
[0020] In some embodiments of the present disclosure, the catalyst may further comprise a pore structure that is favorable for the catalytic cracking reaction of ethylene. Preferably, the catalyst has a pore structure of 80 to 120 m 2 Specific surface area of 0.2-0.8 cm / g 3 / g, and pore diameters of 8 to 13 nm.
[0021] In some embodiments of the present disclosure, the TiO2 disordered layer preferably has a thickness of 1.8 to 3 nm. Structural defects formed by the crystalline TiO2 in the catalyst may form a TiO2 disordered layer on the surface of the crystalline TiO2, and may include surface hydroxyl groups.
[0022] In some embodiments of the present disclosure, the TiO2 disordered layer preferably contains Ti 3+ The crystalline form of TiO2 of the present disclosure contains the above defects, and the amount of the defects is 3+ When the molar percentage is within the above range, the catalyst can be controlled to be more appropriately matched with the above coagent and to exhibit better catalytic activity for the decomposition reaction of ethylene. 3+ The amount can be determined by X-ray photoelectron spectroscopy.
[0023] In the present disclosure, the surface hydroxyl groups are Ti 3+ and can be represented as Ti-OH.
[0024] In the present disclosure, the catalyst for catalytic cracking of ethylene has an earth yellow appearance and a spherical morphology.
[0025] In a second aspect, the present disclosure provides a method for making a catalyst for catalytic cracking of ethylene, as shown in FIG. 1, comprising the steps of: (1) mixing a titanium source powder with an acid, and roasting the resulting mixture; (2) leaching the product obtained by roasting with water, followed by solid-liquid separation to obtain a Ti-containing filtrate; (3) hydrolyzing and aging the filtrate to obtain a metatitanic acid colloid containing auxiliary elements including Na and K; (4) washing, drying and calcining the metatitanic acid colloid to obtain nano-TiO2 powder; and (5) hydrogenating the nano-TiO2 powder to obtain a catalyst for catalytic cracking of ethylene; Including, Here, the titanium source powder is selected from spent SCR denitration catalyst containing Na2O and K2O.
[0026] In some embodiments of the present disclosure, steps (1) and (2) can be used to extract mainly Ti element to obtain one or more soluble Ti-containing compounds, and also extract Na and K elements. Preferably, the acid is concentrated sulfuric acid, and preferably, the concentration of the acid is 85-92 wt%, more preferably 88-91 wt%. The requirement of extracting useful elements, mainly Ti element, should be met.
[0027] In some embodiments of the present disclosure, preferably the mixing conditions include a temperature of 20-30° C. and a time of 2-6 hours, more preferably a temperature of 22-28° C. and a time of 3-5 hours.
[0028] In some embodiments of the present disclosure, the mass ratio of the titanium source powder to the acid is preferably 1:(1.5-2). The titanium source powder may further contain an auxiliary preferably containing Na2O and K2O, and more preferably, the titanium source powder contains K2O in an amount of 0.1-0.3 wt% and Na2O in an amount of 0.2-0.8 wt% based on the total weight of the titanium source powder, thereby ensuring that the finally prepared catalyst for catalytic cracking of ethylene contains specified amounts of Na2O and K2O, and further improving the catalytic activity for the cracking of ethylene.
[0029] In some embodiments of the present disclosure, the roasting temperature is preferably within the range of 150 to 300° C., and the roasting time is preferably 30 to 90 minutes.
[0030] In some embodiments of the present disclosure, the titanium source powder preferably has an average particle size of 10 to 1,000 μm, preferably 50 to 200 μm. The above conditions can facilitate more efficient extraction of Ti, Na and K elements to obtain one or more soluble Ti-containing compounds.
[0031] In some embodiments of the present disclosure, step (2) can achieve dissolution of Ti element and also achieve dissolution of auxiliary elements such as Na and K. Preferably, the water leaching conditions include a temperature of 60-120°C and a time of 60-180 minutes, more preferably a temperature of 80-100°C and a time of 80-120 minutes.
[0032] In some embodiments of the present disclosure, preferably the mass ratio of product to water used in the water leaching is 1:(2-6), more preferably 1:(3-5).
[0033] In some embodiments of the present disclosure, step (3) can be used mainly for the precipitation of Ti. Preferably, the hydrolysis temperature is in the range of 80 to 110°C, more preferably 85 to 105°C, and the hydrolysis time is in the range of 2 to 5 hours, more preferably 2.5 to 4 hours.
[0034] In some embodiments of the present disclosure, the hydrolysis is followed by an aging treatment, and the aging time is preferably within a range of 15 to 30 hours, more preferably 16 to 26 hours, and the aging temperature is within a range of 10 to 50°C, more preferably 20 to 35°C.
[0035] In the present disclosure, the aged material is suction filtered and separated, and washed with water to obtain a metatitanic acid colloid containing auxiliary elements.
[0036] In some embodiments of the present disclosure, step (4) is carried out to purify the metatitanic acid colloid. For example, this step can be used to remove impurities and remove water. A water washing process is used to remove impurities from the metatitanic acid colloid by a process including mixing the metatitanic acid colloid with water, stirring the mixture, filtering, and removing the filtrate. The water washing and filtering may be carried out several times. Preferably, the drying temperature is in the range of 65-95°C, and the drying time is 60-120 minutes.
[0037] In some embodiments of the present disclosure, the firing temperature is preferably within the range of 450-700° C., the firing time is 2-8 hours, and the heating rate is 5-10° C. / min. Preferably, firing is performed at a temperature of 500-600° C. and a heating rate of 5-7° C. / min for 5-6 hours to obtain better results.
[0038] In the present disclosure, the crystal form of the nano-TiO2 powder obtained after calcination is anatase type.
[0039] Preferably, the nano-TiO2 powder further comprises auxiliary agents such as Na2O and K2O dispersed in the nano-TiO2 powder.
[0040] In some embodiments of the present disclosure, the nano TiO2 powder is subjected to surface hydrogenation and reduction in step (5), which generates a defect structure after the hydrogenation process. Preferably, the conditions for hydrogenation include a hydrogenation temperature of 400-550°C, a hydrogenation temperature ramp rate of 5-10°C / min, a hydrogenation time of 2-12 hours, a hydrogen concentration of 90-100% by volume, and a hydrogen flow rate of 100-300 mL / min. The TiO2 powder is heated from room temperature to the hydrogenation temperature at a hydrogenation ramp rate in the presence of a set flow rate of hydrogen, and then hydrogenation is carried out at a constant temperature. Preferably, the hydrogenation is carried out at normal pressure, 420-460°C for 4-12 hours, and in an atmosphere of 100% by volume H2, with a hydrogen flow rate of 100-150 mL / min, to obtain more desirable effects.
[0041] In a third aspect, the present disclosure provides a catalyst for the catalytic cracking of ethylene made by the above method.
[0042] Preferably, the catalyst for catalytic cracking of ethylene prepared by the above method comprises crystalline TiO2 and an auxiliary, and the catalyst comprises K2O in an amount of 0.002-0.006 wt% and Na2O in an amount of 0.006-0.098 wt% based on the total weight of the catalyst. The crystalline form of TiO2 is anatase type, and the catalyst comprises TiO2 in an amount of 99.9-99.99 wt%. The surface of the crystalline TiO2 is covered with a TiO2 disordered layer. The TiO2 disordered layer has a thickness of 1.8-3 nm. In the TiO2 disordered layer, Ti 3+ The molar percentage of titanium is 2.15% to 10.37%, preferably 5.15% to 8.66%. 2 Specific surface area of 0.2-0.8 cm / g 3 / g, and pore diameters of 8 to 13 nm.
[0043] In a fourth aspect, the present disclosure provides a use of the above-mentioned catalyst for catalytic cracking of ethylene in cracking of ethylene.
[0044] According to the present disclosure, specifically, the present application involves carrying out a catalytic cracking reaction of ethylene by contacting an organic volatile gas containing ethylene with the catalyst for catalytic cracking of ethylene of the present disclosure.
[0045] According to the present disclosure, the present application is carried out under temperature conditions which may be in the range of 100-500°C.
[0046] According to the present disclosure, the volume concentration of ethylene in the organic volatile gas may be in the range of 10 to 1,000 ppm.
[0047] According to the present disclosure, the volumetric space velocity of the organic volatile gas is 4,000 to 40,000 h -1 It is.
[0048] The present disclosure will now be described in detail with reference to examples. EXAMPLES
[0049] In the following examples and comparative examples: (1) The crystal structure of the prepared ethylene catalytic cracking catalyst was measured by XRD analysis using a Bruker D8 ADVANCE, Germany. The test and scanning rates were in the range of 0.5° / min to 5° / min. (2) The pore structure and mesopore size of the prepared ethylene catalytic cracking catalyst were measured by N2 adsorption method using an ASAP 2020 physical adsorption apparatus manufactured by Micromeritics, Inc., USA. The adsorption medium was N2. (3) The morphology of the prepared ethylene catalytic cracking catalyst was measured by TEM using a JEM ARM 200F transmission electron microscope (JEOL, Japan). (4) Electron paramagnetic resonance (EPR) imaging analysis was performed using an electron paramagnetic resonance spectrometer. (5) The titanium source powder was a spent SCR catalyst with an average particle size of 74 μm, and its chemical composition was measured using XRF fluorescence spectrometry (RIPP 117-90 standard method), and the results are shown in Table 1. The components of the catalyst and their contents were also measured by XRF fluorescence spectrometry.
[0050] [Table 1]
[0051] Example 1 (1) A used SCR catalyst (particle size 120 μm) and concentrated sulfuric acid (concentration 90 wt%) were mixed in a mass ratio of 1:1.8 to obtain a mixture, which was then roasted at a temperature of 180° C. for 1 hour.
[0052] (2) The product obtained by roasting was leached with water at a temperature of 100°C for 100 minutes so that the mass ratio of the product to water was 1:4, and the mixture was subjected to solid-liquid separation to obtain a Ti-containing filtrate.
[0053] (3) The filtrate was successively hydrolyzed and aged under hydrolysis conditions of a hydrolysis temperature of 100°C for 3 hours and an aging condition of an aging temperature of 25°C for 20 hours. The solid phase product was analyzed and found to be a metatitanic acid colloid containing auxiliary agents, which included Na2O and K2O.
[0054] (4) The metatitanic acid colloid was washed with water, and the solid obtained by separation was dried at 80°C for 60 minutes, heated at a temperature increase rate of 7°C / min, and finally calcined in a muffle furnace at 500°C for 6 hours to obtain nano-TiO2 powder. Analysis showed that the particle size of the nano-TiO2 powder was approximately 30 nm, and the crystal form of the nano-TiO2 powder was anatase type.
[0055] (5) This nano-TiO2 powder was hydrogenated in a tubular furnace at a pressure of 0.1 MPa, a hydrogen concentration of 100 volume%, a hydrogen flow rate of 120 mL / min, and a hydrogenation temperature increase rate of 10 °C / min so that the hydrogenation temperature reached 420 °C. After hydrogenation for 12 hours while insulated, the temperature was cooled to room temperature to produce a catalyst for the catalytic cracking of ethylene, designated T-1.
[0056] The obtained catalyst for catalytic cracking of ethylene was subjected to XRD analysis, and it was found that the catalyst for catalytic cracking of ethylene contained TiO2 in a crystalline form having an anatase crystal form. As can be seen from the TEM image in Figure 6, the catalyst contained a TiO2 disordered layer with a thickness of 2.74 nm and Ti 3+ The molar percentage of was 6.73%. The catalyst further contained K2O and Na2O, the components of which are shown in Table 2.
[0057] 2 shows a comparison of appearance between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and TiO2 powder. As can be seen from the figure, the TiO2 powder was a white powder, while the catalyst for catalytic cracking of ethylene of the present disclosure had an earth yellow appearance and a spherical morphology.
[0058] Figure 3 shows the comparison of X-ray diffraction patterns between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and TiO2 powder. As can be seen from Figure 3, the diffraction peaks of the catalyst for catalytic cracking of ethylene of the present disclosure are all consistent with the diffraction peaks of TiO2 powder, without impurities, and consistent with the XRD spectrum of mesoporous TiO2 reported in the literature. In addition, the XRD diffraction peaks of the catalyst for catalytic cracking of ethylene are obviously broader and lower, indicating that the crystallite size and structure of the microcrystals have changed slightly, which is due to the generation of trivalent titanium and oxygen vacancies during the hydrogenation and reduction process.
[0059] FIG. 4 is a comparative graph of the nitrogen adsorption / desorption isotherms of the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure, in which there were two curves, one being the adsorption curve and the other being the desorption curve. FIG. 4 shows that the catalyst for catalytic cracking of ethylene of the present disclosure was of Langmuir IV type, which belonged to the typical adsorption curve of mesoporous materials, i.e., there was a large hysteresis loop with increasing adsorption partial pressure. Furthermore, the value of the relative pressure p / p0 corresponding to the point where the adsorption capacity increases dramatically in the adsorption isotherm indicates the pore size of the sample, and as can be seen from the pore size distribution in FIG. 4, the catalyst for catalytic cracking of ethylene of the present disclosure had a highly ordered mesoporous structure, a uniform pore size distribution, and ordered flow channels.
[0060] FIG. 5 shows an EPR comparison between the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure and TiO2 powder. The signal peaks with g values less than 2 are oxygen vacancies (V O * )Ti 3+ As can be seen from FIG. 5, 1 represents the TiO2 powder, 2 represents the catalyst for catalytic cracking of ethylene according to the present disclosure, and the oxygen vacancies (V O * )Ti 3+ This indicates that more oxygen vacancies were generated on the surface of the material by hydrogenation, which promoted the progress of the denitrification reaction.
[0061] Figure 6 is a TEM image of the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure. As can be seen in Figure 6 (marked with multiple dotted lines and arrows below the center), the edges of the TiO2 crystal nuclei appear to be etched, forming a thin irregular layer, further indicating that the TiO2 has been successfully hydrogenated.
[0062] Fig. 7 is a graph showing the reaction activity of the catalyst for catalytic cracking of ethylene prepared in Example 1 of the present disclosure. As can be seen from Fig. 7, the catalyst for catalytic cracking of ethylene had an ethylene cracking activity of more than 50% at temperatures of 325 to 500°C, and the catalyst for catalytic cracking of ethylene had an ethylene cracking activity of more than 90% at temperatures exceeding 450°C.
[0063] Example 2 (1) A used SCR catalyst (particle size 50 μm) and concentrated sulfuric acid (concentration 88 wt%) were mixed in a mass ratio of 1:1.5 to obtain a mixture, which was then roasted at a temperature of 150° C. for 0.5 hours.
[0064] (2) The product obtained by roasting was leached with water at a temperature of 90°C for 80 minutes so that the mass ratio of the product to water was 1:3. The mixture was then subjected to solid-liquid separation to obtain a Ti-containing filtrate.
[0065] (3) The filtrate was successively hydrolyzed and aged under hydrolysis conditions of a hydrolysis temperature of 85°C and a hydrolysis time of 2.5 hours, and aging conditions of an aging temperature of 20°C and a aging time of 16 hours. The solid phase product was analyzed and found to be a metatitanic acid colloid containing auxiliary agents, which included Na2O and K2O.
[0066] (4) The metatitanic acid colloid was washed with water, and the solid obtained by separation was dried at 95°C for 120 minutes, heated at a temperature increase rate of 5°C / min, and finally calcined in a muffle furnace at 600°C for 5 hours to obtain nano-TiO2 powder. Analysis showed that the particle size of the nano-TiO2 powder was approximately 20 nm, and the crystal form of the nano-TiO2 powder was anatase type.
[0067] (5) This nano-TiO2 powder was hydrogenated in a tubular furnace at a pressure of 0.1 MPa, a hydrogen concentration of 100 volume%, a hydrogen flow rate of 100 mL / min, and a hydrogenation temperature increase rate of 5°C / min so that the hydrogenation temperature reached 430°C. After hydrogenation for 4 hours under insulation, the temperature was cooled to room temperature to produce a catalyst for the catalytic cracking of ethylene, designated T-2.
[0068] Catalyst T-2 was analyzed, and the results are shown in Table 2. Comparisons were made of appearance, XRD, nitrogen adsorption / desorption isotherm, EPR, and TEM. The results obtained from the photographs, curves, and spectrograms were similar to those obtained in Example 1.
[0069] Example 3 (1) A mixture was obtained by mixing a used SCR catalyst (particle size 200 μm) and concentrated sulfuric acid (concentration 91 wt%) in a mass ratio of 1:2, and this mixture was roasted at a temperature of 300° C. for 1.5 hours.
[0070] (2) The product obtained by roasting was leached with water at a temperature of 80°C for 120 minutes so that the mass ratio of the product to water was 1:5, and the mixture was subjected to solid-liquid separation to obtain a Ti-containing filtrate.
[0071] (3) The filtrate was successively hydrolyzed and aged under hydrolysis conditions of a hydrolysis temperature of 105°C and a hydrolysis time of 4 hours, and aging conditions of an aging temperature of 35°C and a aging time of 26 hours. The solid phase product was analyzed and found to be a metatitanic acid colloid containing auxiliary agents, which included Na2O and K2O.
[0072] (4) The metatitanic acid colloid was washed with water, and the solid obtained by separation was dried at 65°C for 100 minutes, heated at a temperature increase rate of 6°C / min, and finally calcined in a muffle furnace at 550°C for 5 hours to obtain nano-TiO2 powder. Analysis showed that the particle size of the nano-TiO2 powder was approximately 40 nm, and the crystal form of the nano-TiO2 powder was anatase type.
[0073] (5) This nano-TiO2 powder was hydrogenated in a tubular furnace at a pressure of 0.1 MPa, a hydrogen concentration of 100 volume%, a hydrogen flow rate of 150 mL / min, and a hydrogenation temperature increase rate of 8°C / min so that the hydrogenation temperature reached 460°C. After hydrogenation for 9 hours under insulation, the temperature was cooled to room temperature to produce a catalyst for the catalytic cracking of ethylene, designated T-3.
[0074] Catalyst T-3 was analyzed, and the results are shown in Table 2. The appearance, XRD, nitrogen adsorption / desorption isotherm, EPR, and TEM were compared. The results obtained from the photographs, curves, and spectrograms were similar to those obtained in Example 1.
[0075] Example 4 A catalyst was prepared in the same manner as in Example 1, except that the "hydrogenation temperature 420° C." was changed to "hydrogenation temperature 400° C.." The prepared catalyst for catalytic cracking of ethylene was designated as T-4.
[0076] Catalyst T-4 was analyzed, and the results are shown in Table 2. The appearance, XRD, nitrogen adsorption / desorption isotherm, EPR, and TEM were compared. The results obtained from the photographs, curves, and spectrograms were similar to those obtained in Example 1.
[0077] Example 5 A catalyst was prepared in the same manner as in Example 1, except that the "hydrogenation time of 12 hours" was changed to "hydrogenation time of 2 hours." The prepared catalyst for catalytic cracking of ethylene was designated as T-5.
[0078] Catalyst T-5 was analyzed, and the results are shown in Table 2. The appearance, XRD, nitrogen adsorption / desorption isotherm, EPR, and TEM were compared. The results obtained from the photographs, curves, and spectrograms were similar to those obtained in Example 1.
[0079] Comparative Example 1 Commercially available TiO2 was used, and the catalyst parameters are shown in Table 2.
[0080] Comparative Example 2 A catalyst was prepared in the same manner as in Example 1, except that the "hydrogen concentration 100 volume %" was changed to "hydrogen concentration 50 volume %." The parameters of the prepared catalyst are shown in Table 2.
[0081] Comparative Example 3 A catalyst was prepared according to the same method as in Example 1, except that the "hydrogenation time of 12 hours" was changed to "hydrogenation time of 0.5 hours" and the "hydrogenation temperature of 420° C." was changed to "hydrogenation temperature of 200° C. The parameters of the prepared catalyst are shown in Table 2.
[0082] [Table 2]
[0083] As can be seen from the results in Table 2, in Comparative Example 1, TiO2 containing no impurities was used for hydrogenation, in Comparative Example 2, low-concentration hydrogen gas was used for hydrogenation, and in Comparative Example 3, hydrogenation was performed using conditions for the hydrogenation time and temperature outside the ranges defined in the present disclosure. As a result, the catalysts for catalytic cracking of ethylene prepared in Examples 1 to 5 by using the preparation method of the present disclosure had an irregular layer of a specific thickness and a Ti content of titanium element. 3+ It was shown that the molar percentage of
[0084] Application Examples The catalysts prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were applied to the decomposition reaction of ethylene. In the organic volatile gas undergoing catalytic oxidative decomposition, the volume concentration of ethylene was 700 ppm, and for the other gases, the content of O2 was 10 volume %, N2 was the balance gas, the total flow rate was 1,000 mL / min, and the volumetric space velocity of the organic volatile gas was 100,000 h -1 The results are shown in Table 3.
[0085] Decomposition efficiency %=(inlet ethylene concentration−outlet ethylene concentration) / inlet ethylene concentration×100%.
[0086] [Table 3]
[0087] As can be seen from the results in Table 3, when the non-hydrogenated titanium oxide of Comparative Example 1 was used, no ethylene decomposition efficiency was observed. In Comparative Examples 2 and 3, the hydrogenation time, temperature and hydrogen concentration were not within the above ranges, the obtained catalyst did not have the structure of the catalyst of the present disclosure, and the catalytic decomposition effect of ethylene was inferior to the catalytic decomposition effect of the catalyst described in Examples 1 to 5 of the present disclosure. Furthermore, the titanium oxide of Comparative Example 1 was calcined under the conditions of step (4) of Example 1 to obtain anatase type crystals, and was hydrogenated according to the method of step (5) of Example 1, but the prepared catalyst did not contain the auxiliary agents K2O and Na2O, and had a thickness and Ti defined in the present disclosure. 3+ Since the catalyst cannot have a molar percentage of disordered layers, it cannot produce an excellent catalytic cracking effect of ethylene.
[0088] Although the preferred embodiments of the present disclosure have been described in detail above, the present disclosure is not limited thereto. Various simple modifications may be made to the technical solutions of the present disclosure, including combinations of individual technical features in any other suitable manner, within the scope of the technical ideas of the present disclosure, and such simple modifications and combinations thereof are also considered as the contents disclosed by the present disclosure, and each of them is included in the protection scope of the present disclosure.
Claims
1. A catalyst for the catalytic cracking of ethylene, said catalyst being in crystalline form of TiO 2 and an auxiliary agent; The TiO 2 The crystalline form of the TiO 2 The surface of TiO containing surface hydroxyl groups 2 The catalyst is covered with a disordered layer.
2. The TiO 2 2. The catalyst of claim 1, wherein the disordered layer has a thickness of 1.8 to 3 nm.
3. The TiO 2 In the disordered layer, Ti 3+ 3. The catalyst according to claim 1 or 2, wherein the molar percentage of titanium is between 2.15% and 10.37%, preferably between 5.15% and 8.66%, of elemental titanium.
4. The catalyst comprises TiO in an amount of 99.9 to 99.99 wt %, based on the total weight of the catalyst. 2 Including; Preferably, the auxiliary is K 2 O and Na 2 Contains O; Preferably, the catalyst contains 0.002 to 0.006 wt. % K, based on the total weight of the catalyst. 2 O and Na in an amount of 0.006 to 0.098% by weight 2 4. The catalyst according to claim 1 , further comprising O.
5. A method for preparing a catalyst for catalytic cracking of ethylene, comprising the steps of: (1) mixing a titanium source powder with an acid and roasting the resulting mixture; (2) leaching the product obtained by the roasting with water, followed by solid-liquid separation to obtain a Ti-containing filtrate; (3) hydrolyzing and aging the filtrate to obtain a metatitanic acid colloid containing auxiliary elements including Na and K; (4) The metatitanic acid colloid is washed with water, dried and calcined to obtain nano-TiO 2 Obtaining a powder; (5) The nano-TiO 2 hydrogenating the powder to obtain the catalyst for catalytic cracking of ethylene; Including, The titanium source powder is Na 2 O and K 2 The method for preparing the catalyst is selected from a spent SCR denitration catalyst containing O.
6. the acid is concentrated sulfuric acid, preferably the acid has a concentration of 85-92% by weight; Preferably, the mixing conditions include a temperature of 20-30° C. and a time of 2-6 hours; Preferably, the mass ratio of the titanium source powder to the acid is 1:(1.5-2); Preferably, the roasting temperature is in the range of 150-300° C., and the roasting time is 30-90 minutes; The method according to claim 5, wherein the titanium source powder preferably has an average particle size of 10 to 1,000 μm.
7. Water leaching conditions include a temperature of 60-120°C and a time of 60-180 minutes; 7. The method according to claim 5 or 6, wherein the mass ratio of the product to the water used for the water leaching is preferably 1:(2-6).
8. The hydrolysis temperature is in the range of 80-110°C, preferably 85-105°C; the hydrolysis time is in the range of 2-5 hours, preferably 2.5-4 hours; The process according to any one of claims 5 to 7, wherein the maturation time is preferably in the range of 15 to 30 hours, more preferably 16 to 26 hours, and the maturation temperature is in the range of 10 to 50°C, more preferably 20 to 35°C.
9. The drying temperature is within the range of 65-95°C, and the drying time is 60-120 minutes; The method according to any one of claims 5 to 8, wherein the calcination temperature is preferably in the range of 450-700°C, the calcination time is preferably 2-8 hours, and the heating rate is preferably 5-10°C / min.
10. 10. The method according to claim 5, wherein the hydrogenation conditions include a hydrogenation temperature of 400 to 550° C., a hydrogenation temperature increase rate of 5 to 10° C. / min, a hydrogenation time of 2 to 12 hours, a hydrogen concentration of 90 to 100 vol.%, and a hydrogen flow rate of 100 to 300 mL / min.
11. A catalyst for the catalytic cracking of ethylene made by the method according to any one of claims 5 to 10.
12. 12. Use of the catalyst according to any one of claims 1 to 4 and 11 in the catalytic cracking of ethylene.
Citation Information
Patent Citations
Hydrogenated-TiO2 catalyst for denitration and preparation method and application of hydrogenated-TiO2 catalyst
CN110743581A