NAND cell structure with charge trap cut

A discontinuous charge trapping layer in 3D-NAND devices, formed using atomic layer deposition and cluster processing, addresses cell-to-cell interference and lateral charge diffusion, facilitating the scaling of 3D-NAND devices by enhancing fabrication precision and reducing interference.

JP2024541413AActive Publication Date: 2024-11-08APPLIED MATERIALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024529485
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-14
Filing Date
2022-11-18
Publication Date
2024-11-08
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

Current 3D-NAND devices face challenges with cell-to-cell interference and lateral charge diffusion due to continuous charge trapping layers, which hinder scaling down from the word line to the WL insulator, and trap-cut structures require consistent shape and thickness, limiting their effectiveness.

Method used

Implementing a discontinuous charge trapping layer confined between tunnel oxide and word lines, using atomic layer deposition for silicon nitride, and employing a cluster processing tool for precise fabrication, including methods to form memory devices with alternating dielectric and nitride layers and trap cuts.

Benefits of technology

This approach reduces intercell interference and lateral diffusion, enabling effective scaling of 3D-NAND devices by ensuring consistent charge trapping layer formation and precise fabrication processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541413000001_ABST
    Figure 2024541413000001_ABST
Patent Text Reader

Abstract

A memory device is described that includes a plurality of memory cells formed around a memory hole that extends through a memory stack on a substrate. Each of the plurality of memory cells includes a discontinuous blocking oxide layer, a charge trapping layer, and a tunnel oxide layer. The blocking oxide layer is discontinuous between each of the plurality of memory cells. The tunnel oxide layer is continuous between each of the plurality of memory cells, and the charge trapping layer is discontinuous between each of the plurality of memory cells. The charge trapping layer has a first thickness at a top portion and a second thickness at a center portion, the first thickness being different from the second thickness.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001]

[0001] Embodiments of the present disclosure relate to the field of electronic devices and methods and apparatus for manufacturing electronic devices. More particularly, embodiments of the present disclosure provide a 3D-NAND having a discontinuous charge trapping layer and a method of formation. [Background technology]

[0002]

[0002] Semiconductor technology is advancing at a rapid pace, and device dimensions are shrinking with the advancement of technology to achieve faster processing and storage per unit space. In NAND devices, the string current needs to be high enough to get enough current to distinguish between ON and OFF cells. The string current depends on the carrier mobility, which is improved by increasing the grain size of the silicon channel.

[0003]

[0003] Current 3D-NAND stacks based on charge traps as storage layers contain a continuous charge trapping layer. The continuous charge trapping layer causes two major problems that hinder scaling down from word line (WL) to WL insulator: cell-cell interference and lateral charge diffusion. To suppress these problems, the charge trapping layer under the source and drain (S / D) of each cell needs to be eliminated with a trap-cut structure or confinement structure. However, problems arise in the trap-cut structure due to partial use of the gate area and the variation in the shape and thickness of the trapping layer caused by the deposition and removal process.

[0004]

[0004] Accordingly, there is a need in the art for 3D-NAND devices with improved charge trapping layers and methods for fabricating 3D-NAND devices. Summary of the Invention

[0005]

[0005] One or more embodiments of the present disclosure are directed to a semiconductor memory device comprising: a plurality of memory cells formed around a memory hole extending through a memory stack on a substrate, the memory stack including alternating word lines and a dielectric material, each of the plurality of memory cells including a discontinuous blocking oxide layer, a charge trapping layer, and a tunnel oxide layer, the blocking oxide layer being discontinuous between each of the plurality of memory cells, the tunnel oxide layer being continuous between each of the plurality of memory cells, and the charge trapping layer being discontinuous between each of the plurality of memory cells; and a filled slit extending through the memory stack adjacent the memory hole.

[0006]

[0006] Further embodiments of the present disclosure are directed to a method of forming a semiconductor memory device. In one or more embodiments, the method of forming the semiconductor device includes forming a memory hole in a memory stack including alternating layers of a first material and a second material on a substrate, recessing a second material through the memory hole to form a first recessed region, oxidizing a portion of the second material adjacent to the memory hole to form a blocking oxide layer, depositing a charge trapping layer on the blocking oxide layer, conformally depositing a sacrificial layer on the charge trapping layer, selectively removing the charge trapping layer from the sacrificial layer, removing the sacrificial layer, forming a bit line in the memory hole, patterning a slit, forming a plurality of word lines, and filling the slit.

[0007]

[0007] Further embodiments of the present disclosure are directed to a non-transitory computer readable medium. In one or more embodiments, the non-transitory computer readable medium includes instructions that, when executed by a controller of a process chamber, cause the process chamber to perform steps of forming a memory hole in a memory stack including alternating layers of a first material and a second material on a substrate, recessing a second material through the memory hole to form a first recessed region, oxidizing a portion of the second material adjacent to the memory hole to form a blocking oxide layer, depositing a charge trapping layer on the blocking oxide layer, conformally depositing a sacrificial layer on the charge trapping layer, selectively removing the charge trapping layer from the sacrificial layer, removing the sacrificial layer, forming a bit line in the memory hole, patterning a slit, forming a plurality of word lines, and filling the slit.

[0008]

[0008] In order that the above-mentioned features of the present disclosure may be understood in detail, the present disclosure summarized above will now be more particularly described with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings are merely representative of the present disclosure and therefore should not be considered as limiting the scope of the present disclosure, which may admit of other equally effective embodiments. The embodiments described herein are presented by way of example and are not limited to the figures of the accompanying drawings in which like references indicate similar elements. [Brief description of the drawings]

[0009] [Figure 1-1] FIG. 1 is a process flow diagram of a method for forming a memory device according to embodiments described herein. [Figure 1-2] FIG. 1 is a process flow diagram of a method for forming a memory device according to embodiments described herein. [Diagram 2] FIG. 1 illustrates a cross-sectional view of an electronic device including a memory stack according to one or more embodiments. [Diagram 3] FIG. 2 illustrates a cross-sectional view of an electronic device after forming a stepped pattern of a memory stack according to one or more embodiments. [Figure 4]FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 5A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 5B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 6A] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 6B] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 7A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 7B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 8A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 8B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 9A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 9B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 10A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 10B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 11A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 11B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 11C] 1 is an enlarged view of region 120 according to one or more alternative embodiments. [Figure 12A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 12B] 1 is an enlarged view of region 120 according to one or more embodiments. [Figure 13]FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 14] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 15] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 16] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 17] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 18] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 19] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 20] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 21A] FIG. 1 is a cross-sectional view illustrating an electronic device according to one or more embodiments. [Figure 21B] 1 is an enlarged view of region 170 according to one or more embodiments. [Figure 22-1] FIG. 1 is a process flow diagram illustrating a method of forming a memory device according to embodiments described herein. [Figure 22-2] FIG. 1 is a process flow diagram illustrating a method of forming a memory device according to embodiments described herein. [Figure 23A] FIG. 1 is a perspective view of an electronic device according to one or more embodiments. [Figure 23B] 1 is an enlarged view of region 180 according to one or more embodiments. [Figure 24A] FIG. 1 is a perspective view of an electronic device according to one or more embodiments. [Figure 24B] 1 is an enlarged view of region 180 according to one or more embodiments. [Figure 25A] FIG. 1 is a perspective view of an electronic device according to one or more embodiments. [Figure 25B] 1 is an enlarged view of region 180 according to one or more embodiments. [Figure 26A] FIG. 1 is a perspective view of an electronic device according to one or more embodiments. [Figure 26B] 1 is an enlarged view of region 180 according to one or more embodiments. [Figure 27] FIG. 1 illustrates a cluster tool according to one or more embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010]

[0050] Before describing several example embodiments of the present disclosure, it is to be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following description as being capable of other embodiments and of being practiced or carried out in various ways.

[0011]

[0051] As used herein and in the appended claims, the terms "precursor," "reactant," "reactive gas," and the like are used interchangeably to refer to any gas species capable of reacting with the substrate surface.

[0012]

[0052] As used herein, "atomic layer deposition" or "cyclic deposition" refers to the sequential exposure of two or more reactive compounds to deposit layers of material on a substrate surface. As used herein and in the appended claims, the terms "reactive compound", "reactive gas", "reactive species", "precursor", "process gas", and the like are used interchangeably to mean a substance having a species capable of reacting with a substrate surface or a material on the substrate surface in a surface reaction (e.g., chemisorption, oxidation, reduction). The substrate or a portion of the substrate is exposed to the precursors (or reactive gases) sequentially or substantially sequentially. As used throughout this specification, "substantially sequential" means that the majority of the duration of the precursor exposure does not overlap with the exposure to the co-reagent, although there may be some overlap.

[0013]

[0053] As used herein, the term "over" does not refer to the physical orientation of one surface over another, but rather to the relationship of the thermodynamic or kinetic properties of a chemical reaction relative to one surface over another. For example, selectively depositing a film on a damaged dielectric material over an oxide material means that the film deposits on the damaged dielectric material and less or no film deposits on the oxide material, or that the formation of a film on the damaged dielectric material is thermodynamically or kinetically favored relative to the formation of a film on the oxide material.

[0014]

[0054] In the following description, numerous specific details are set forth, such as specific materials, chemicals, element dimensions, etc., to provide a thorough understanding of one or more embodiments of the present disclosure. However, it will be apparent to one of ordinary skill in the art that one or more embodiments of the present disclosure may be practiced without these specific details. In other instances, semiconductor manufacturing processes, techniques, materials, equipment, etc. have not been described in detail to avoid unnecessarily obscuring the present specification. One of ordinary skill in the art will be able to achieve the appropriate functionality without undue experimentation, given the description contained herein.

[0015]

[0055] Although certain exemplary embodiments of the present disclosure have been described and illustrated in the accompanying drawings, it is to be understood that the above embodiments are illustrative only and do not limit the present disclosure, and that the present disclosure is not limited to the specific constructions and arrangements shown and described, as modifications may be made by those skilled in the art.

[0016]

[0056] In existing 3D NAND devices based on a memory stack of alternating layers of oxide and nitride materials and with charge traps as storage layers, the charge traps are a continuous layer. This continuous charge trap layer causes cell-to-cell interference and lateral charge diffusion, which hinders scaling down from the word line (WL) to the WL insulator. To address cell-to-cell interference and lateral charge diffusion, a trap cut or confinement structure must be used to eliminate the trap layer under the source and drain (S / D) of each cell. However, the trap cut cannot use the gate region, and the trap layer must have a consistent shape and thickness. Thus, one or more embodiments provide a 3D NAND structure and a method for fabricating a charge trap layer using a trap cut.

[0017]

[0057] One or more embodiments provide a structure and method for fabricating a 3-NAND device using atomic layer deposition silicon nitride for the formation of a discontinuous charge trapping layer. The charge trapping layer of one or more embodiments is confined only between the tunnel oxide and the word line so that cell-to-cell interference and lateral diffusion are not inhibited. In one or more embodiments, non-selective silicon nitride (SiN) can be used as the charge trapping layer.

[0018]

[0058] In one or more embodiments, the metal deposition and other processes can be performed in an isolated environment (e.g., a cluster processing tool). Accordingly, some embodiments of the present disclosure provide an integrated tool system with associated process modules for performing the methods.

[0019]

[0059] FIG. 1 is a flow diagram illustrating an exemplary method 10 for forming a memory device. Those skilled in the art will recognize that the method 10 may include any or all of the illustrated processes. Furthermore, the order of the individual processes may be changed in some parts. The method 10 may start with any of the listed processes without departing from the present disclosure. With reference to FIG. 1, in step 12, a memory stack is formed. In step 14, a word line staircase is formed in the memory stack. In step 16, a memory hole is patterned. In step 18, a nitride layer is recessed. In step 20, a blocking oxide is formed in the recess. In step 22, a charge trapping layer is deposited, followed by a sacrificial layer. In step 24, the sacrificial layer is partially removed. In step 26, the charge trapping layer is unmasked and the sacrificial layer is removed. In step 28, a transistor layer is deposited in the memory hole. In step 30, a bit line pad is formed. In step 32, a slit pattern is formed in the device. In step 34, the common source line sacrificial layer is removed and replaced. In step 36, the nitride layer of the memory stack is removed (mold pullback). In step 38, the word lines are formed. In step 40, the slits are filled. In step 42, the bit line pad studs are formed. In step 44, the back end (BEOL) contacts are formed.

[0020]

[0060] 2-21 are diagrams illustrating a portion of a memory device 100 following the process flow illustrated in method 10 of FIG.

[0021]

[0061] Figure 2 illustrates an initial or starting memory stack for an electronic device 100 in accordance with one or more embodiments of the present disclosure. In some embodiments, the electronic device 100 illustrated in Figure 2 is layered on a bare substrate 102, as shown. The electronic device of Figure 2 is comprised of a substrate 102, a common source line 103, and a memory stack 130.

[0022]

[0062] The substrate 102 may be any suitable material known to those of skill in the art. As used herein and in the appended claims, the term "substrate" refers to a surface, or a portion of a surface, upon which a process acts. Additionally, those of skill in the art will understand that a reference to a substrate may refer to only a portion of a substrate, unless the context clearly indicates otherwise. Furthermore, a reference to depositing on a substrate may refer to both a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0023]

[0063] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment may be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and the like, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, and / or bake the substrate surface. In addition to performing film treatments directly on the surface of the substrate itself, in the present disclosure, any of the disclosed film treatment steps may be performed on an underlying layer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include such underlying layers as the context indicates. Thus, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0024]

[0064] In one or more embodiments, a common source line 103 is on the substrate 102. The common source line 103 may also be referred to as a semiconductor layer. The common source line 103 may be formed by any suitable technique known to those skilled in the art and may be made of any suitable material, including but not limited to polysilicon (poly-Si). In some embodiments, the common source line 103 includes multiple different conductive or semiconductor materials. For example, in one or more embodiments, as shown in FIG. 2, the common source line 103 includes a polysilicon layer 104 on the substrate 102, a common source sacrificial layer 106 on the polysilicon layer, and a second polysilicon layer 104 on the common source sacrificial layer 106.

[0025]

[0065] In one or more embodiments, the sacrificial layer 106 may be formed on the polysilicon layer 104 and may be made of any suitable material. The sacrificial layer 106 in some embodiments is removed and replaced in a later process. In some embodiments, the sacrificial layer 106 is not removed and remains in the memory device 100. In this case, the term "sacrificial" has an expanded meaning to include a permanent layer, which may be referred to as a conductive layer. In the illustrated embodiment, the sacrificial layer 106 is removed in step 34, as described further below. In one or more embodiments, the sacrificial layer 106 comprises a material that can be selectively removed relative to the adjacent polysilicon layer 104. In one or more embodiments, the sacrificial layer is a nitride material, such as silicon nitride (SiN), or an oxide material, such as silicon oxide (SiO x ).

[0026]

[0066] In one or more embodiments, the memory stack 130 is formed on the common source line 103. The memory stack 130 in the illustrated embodiment includes a plurality of alternating first layers 108 and second layers 110. The memory stack 130 illustrated in FIG. 2 includes five pairs of alternating first layers 108 and second layers 110, but one of ordinary skill in the art will recognize that this is for illustrative purposes only. The memory stack 130 may include any number of alternating first layers 108 and second layers 110. For example, in some embodiments, the memory stack 130 includes 192 pairs of alternating first layers 108 and second layers 110. In other embodiments, the memory stack 130 includes more than 50 pairs of alternating first layers 108 and second layers 110, or more than 100 pairs of alternating first layers 108 and second layers 110, or more than 300 pairs of alternating first layers 108 and second layers 110.

[0027]

[0067] In one or more embodiments, the first layer 108 and the second layer 110 independently comprise a dielectric material. In one or more embodiments, the dielectric material may comprise any suitable dielectric material known to one of skill in the art. As used herein, the term "dielectric material" refers to an electrical insulator that can be polarized in an electric field. In some embodiments, the dielectric material comprises one or more of an oxide, a carbon-doped oxide, a porous silicon dioxide (SiO2), a silicon nitride (SiN), a silicon dioxide / silicon nitride, a carbide, an oxycarbide, a nitride, an oxynitride, an oxycarbonitride, a polymer, a phosphosilicate glass, a fluorosilicate (SiOF) glass, or an organosilicate glass (SiOCH).

[0028]

[0068] In one or more embodiments, the first layer 108 comprises an oxide layer and the second layer 110 comprises a nitride layer. In one or more embodiments, the second layer 110 comprises a material that has etch selectivity with respect to the first layer 108 such that the second layer 110 can be removed without substantially affecting the first layer 108. In one or more embodiments, the first layer 108 comprises a silicon oxide (SiO xIn one or more embodiments, the second layer 110 comprises silicon nitride (SiN). In one or more embodiments, the first layer 108 and the second layer 110 are deposited by chemical vapor deposition (CVD) or physical vapor deposition (PVD).

[0029]

[0069] The individual alternating layers may be formed to any suitable thickness. In some embodiments, the thickness of each second layer 110 is approximately equal. In one or more embodiments, each second layer 110 has a second layer thickness. In some embodiments, the thickness of each first layer 108 is approximately equal. Approximately equal thicknesses, as used in this regard, are within ±5% of each other. In some embodiments, a silicon layer (not shown) is formed between the second layer 110 and the first layer 108. The thickness of the silicon layer may be relatively thin compared to the layer thickness of the second layer 110 or the first layer 108. In one or more embodiments, the first layer 108 has a thickness in the range of about 0.5 nm to about 30 nm, including about 1 nm, about 3 nm, about 5 nm, about 7 nm, about 10 nm, about 12 nm, about 15 nm, about 17 nm, about 20 nm, about 22 nm, about 25 nm, about 27 nm, and about 30 nm. In one or more embodiments, the first layer 108 has a thickness in the range of about 0.5 to about 40 nm. In one or more embodiments, the second layer 110 has a thickness in the range of about 0.5 to about 30 nm, including about 1 nm, about 3 nm, about 5 nm, about 7 nm, about 10 nm, about 12 nm, about 15 nm, about 17 nm, about 20 nm, about 22 nm, about 25 nm, about 27 nm, and about 30 nm. In one or more embodiments, the second layer 110 has a thickness in the range of about 0.5 to about 40 nm.

[0030]

[0070] In one or more embodiments, the first layer 108 and the second layer 110 are deposited by chemical vapor deposition (CVD) or physical vapor deposition (PVD). The individual alternating layers may be formed to any suitable thickness. In some embodiments, the thickness of each second layer 112 is approximately equal. In one or more embodiments, each second layer 112 has a thickness of the first second layer. In some embodiments, the thickness of each first layer 110 is approximately equal. Approximately equal thicknesses, as used in this regard, are within ±5% of each other. In one or more embodiments, the first layer 108 has a thickness in the range of about 0.5 nm to about 30 nm, including about 1 nm, about 3 nm, about 5 nm, about 7 nm, about 10 nm, about 12 nm, about 15 nm, about 17 nm, about 20 nm, about 22 nm, about 25 nm, about 27 nm, and about 30 nm. In one or more embodiments, the second layer 110 has a thickness in the range of about 0.5 nm to about 30 nm, including about 1 nm, about 3 nm, about 5 nm, about 7 nm, about 10 nm, about 12 nm, about 15 nm, about 17 nm, about 20 nm, about 22 nm, about 25 nm, about 27 nm, and about 30 nm.

[0031]

[0071] Referring to FIG. 3, in step 14 of method 10, a staircase structure 131 is created. In one or more embodiments, the staircase structure 131 exposes a top surface 134 of the first layer 108. The top surface 134 can be used to provide a space for forming a word line contact, as described below. A suitable filler material 135 can be deposited to fill the space outside of the staircase structure 131. The suitable filler material 135 can be any material that prevents electrical shorting between adjacent word lines, as will be understood by those skilled in the art. The staircase structure 131 has a width (shown from left to right in the figure) where each word line is smaller than the word line below. The use of relative terms such as "above" and "below" should not be taken as limiting the scope of the present disclosure to physical orientations in space.

[0032]

[0072] 4, in step 16, the memory hole channel 116 is opened / patterned through the memory stack 130. In some embodiments, opening the memory hole channel 116 includes etching through the mask layer 137, the memory stack 130, the common source line 103, and the substrate 102. The memory hole channel 116 has sidewalls that extend through the memory stack 130, exposing the surface 111 of the second layer 110 and the surface 109 of the first layer 108.

[0033]

[0073] The memory hole channel 116 extends a distance into the substrate 102 such that the sidewall surfaces 109, 111, 113 and the bottom surface 115 of the memory hole channel 116 are formed in the substrate 102. The bottom 114 of the memory hole channel 116 may be formed at any point within the thickness of the substrate 102. In some embodiments, the memory hole channel 116 extends into the substrate 102 a thickness in the range of about 1% to about 90%, or in the range of about 5% to about 90%, or in the range of about 20% to about 80%, or in the range of about 30% to about 70%, or in the range of about 40% to about 60% of the thickness of the substrate 102. In some embodiments, the memory hole channel 116 extends into the substrate 102 a distance of 10 nm or more.

[0034]

[0074] 5A and 5B illustrate step 18 in which the second layer 110 is recessed partially through the memory hole 116 to form a recessed region 118. In one or more embodiments, the second layer 110 is recessed by a recessed distance r1 in the range of 1 nm to 30 nm, or in the range of 5 nm to 20 nm. Thus, in one or more embodiments, the recessed region 118 has a size in the range of 1 nm to 30 nm, or in the range of 5 nm to 20 nm. The second layer 110 can be recessed by any method known to those skilled in the art. In one or more embodiments, a portion of the second layer 110 is recessed through the memory hole 116 by selective removal by reactive species formed via a remote plasma from a process gas including oxygen (O2) and nitrogen trifluoride (NF3). In another embodiment, a portion of the second layer 110 is recessed through the memory hole 116 by selective removal by hot phosphorus (HP).

[0035]

[0075] 6A and 6B illustrate a step 20 in which a blocking oxide layer 122 is formed in the recessed region 118 adjacent to the second layer 110. In one or more embodiments, the blocking oxide layer 122 is formed by oxidizing a portion of the second layer 110. Thus, in one or more embodiments, the blocking oxide layer comprises silicon oxynitride (SiON). The blocking oxide layer 122 may have any suitable thickness. In some embodiments, the blocking oxide layer 122 has a thickness in the range of 1 nm to 15 nm, or in the range of 3 nm to 10 nm.

[0036]

[0076] 7A and 7B illustrate step 22, in which a charge trapping layer 124 is formed adjacent to the blocking oxide layer 122. In some embodiments, the sides of the charge trapping layer 124 are exposed to the memory hole channel 116. The charge trapping layer 124 may include any suitable material known to those of skill in the art. In one or more embodiments, the charge trapping layer 124 includes a nitride, such as silicon nitride (SiN). The charge trapping layer 124 may be formed by any suitable means known to those of skill in the art. In one or more embodiments, the charge trapping layer 124 is deposited by atomic layer deposition (ALD). In some embodiments, the charge trapping layer 124 has a thickness in the range of 1 nm to 15 nm, or in the range of 3 nm to 10 nm.

[0037]

[0077] 8A and 8B illustrate step 22 in which a sacrificial layer 128 is formed adjacent to the charge trapping layer 124 and through the memory hole channel 116 in the recessed region 118. The sacrificial layer 128 may comprise any suitable material known to those of skill in the art. In one or more embodiments, the sacrificial layer 128 is an oxide layer, such as silicon oxide (SiO x ). The sacrificial layer 128 may be formed by any suitable means known to one of ordinary skill in the art. In one or more embodiments, the sacrificial layer is formed by atomic layer deposition (ALD). In one or more embodiments, the sacrificial layer 128 is a conformal layer. In other embodiments, the sacrificial layer 128 is a conformal layer, where the sacrificial layer 128 is substantially conformal to the underlying charge trapping layer 124. As used herein, a "substantially conformal" layer refers to a layer that is about the same in thickness throughout (e.g., over the charge trapping layer 124). A substantially conformal layer has a thickness variation of about 5% or less, 2% or less, 1% or less, or 0.5% or less.

[0038]

[0078] 8B, the sacrificial layer 128 is thicker in the center of the recessed region 118 compared to the top and bottom of the recessed region 118. In one or more embodiments, the center of the sacrificial layer 128 has a thickness in the range of 1 nm to 50 nm, or in the range of 5 nm to 30 nm, and the top / bottom of the sacrificial layer 128 has a thickness in the range of >0% to 50% of the thickness of the center of the sacrificial layer 128.

[0039]

[0079] 9A and 9B, in step 24, a portion of the sacrificial layer 128 is removed. In one or more embodiments, the sacrificial layer 128 is removed from the sidewalls of the memory hole channel 116, while leaving portions 129 of the sacrificial layer 128 in the recessed region 118. The sacrificial layer 128 may be removed by any suitable means known to those of skill in the art. In one or more embodiments, the portion of the sacrificial layer 128 is removed by selective etching, for example, with a dilute hydrofluoric acid (HF) solution or HF gas.

[0040]

[0080] 10A and 10B, in step 26, the portions 130 of the sacrificial layer 128 are unmasked, e.g., trap cut, by selectively removing the charge trapping layer 124 around the portions 130 of the sacrificial layer 128. The portions 130 of the sacrificial layer 128 may be unmasked by any suitable means. In one or more embodiments, the charge trapping layer 124 is selectively removed from the portions 130 of the sacrificial layer 128 using a wet or dry process with a phosphoric acid solution or gas.

[0041]

[0081] 11A and 11B, after the trap cut of step 26, the remaining portions 130 of the sacrificial layer 128 are removed to form openings 132. The remaining portions 130 of the sacrificial layer 128 may be removed by any suitable means. In one or more embodiments, the remaining portions 130 of the sacrificial layer 128 are removed by selective etching. In some specific embodiments, the remaining portions 130 of the sacrificial layer 128 are removed using a dilute hydrofluoric acid (HF) solution or gas.

[0042]

[0082] In one or more embodiments, the charge trapping layer 124 has a first thickness t t and a second thickness t c In one or more embodiments, the first thickness t t and the second thickness t c In one or more embodiments, the top (and bottom) first thickness t t is the second thickness t c In one or more embodiments, the first thickness t t is the second thickness t c In one or more embodiments, the first thickness t t is the second thickness t c In another embodiment, the top (and bottom) first thickness t t is the second thickness t c In one or more embodiments, the first thickness t t is the second thickness t c In one or more embodiments, the first thickness t t is the second thickness t c It ranges from 1% to 50% thinner.

[0043]

[0083] 12A and 12B, at step 28, a transistor layer 136 is formed in the memory hole channel 116. The transistor layer 136 may be formed by any suitable technique known to those of skill in the art. In some embodiments, the transistor layer is formed by a conformal deposition process. In some embodiments, the transistor layer is formed by one or more of atomic layer deposition or chemical vapor deposition.

[0044]

[0084] In one or more embodiments, the deposition of the transistor layer 136 is substantially conformal. As used herein, a "substantially conformal" layer refers to a layer that is about the same thickness throughout (e.g., the top, middle, and bottom of the sidewalls, and the bottom of the memory hole channel 116). The thickness variation of a substantially conformal layer is about 5% or less, 2% or less, 1% or less, or 0.5% or less. The transistor layer 136 in the memory hole may include one or more of an aluminum oxide (AlO) layer, a blocking oxide layer, a trapping layer, a tunnel oxide layer, and a channel layer.

[0045]

[0085] 12B, which is an expanded view of region 120 of FIG. 12A, in one or more embodiments, the transistor layers 136 include a blocking oxide layer 122, a nitride trapping layer 124, a tunnel oxide layer 136a, a channel material 136b, and a core oxide material 136c in the memory hole channel 116. In one or more embodiments, the channel material 136b includes polysilicon.

[0046]

[0086] The transistor layer 136 may have any suitable thickness depending, for example, on the dimensions of the memory hole channel 116. In some embodiments, the transistor layer 136 has a thickness in the range of about 0.5 nm to about 50 nm, or in the range of about 0.75 nm to about 35 nm, or in the range of about 1 nm to about 20 nm.

[0047]

[0087] 13 illustrates step 30 of method 10 in which bitline pad 138 is formed on the top surface of transistor layer 136 and mask layer 137. In one or more embodiments, core oxide 136c is recessed and then the recessed area is filled with doped polysilicon to form bitline pad 138. Bitline pad 138 may be any suitable material known to those of skill in the art, including but not limited to polysilicon.

[0048]

[0088] 14, in step 32 of method 10, memory stack 130 is slit patterned to form slit pattern openings 142 extending from the top surface of layer 140 to sacrificial layer 106 of common source line 103.

[0049]

[0089] 15 and 16, in step 34 of method 10, the sacrificial layer 106 of the common source line 103 is removed and replaced with a polysilicon layer 146 to form an opening 144. The sacrificial layer 106 may be removed by any suitable technique known to those skilled in the art, including but not limited to selective etching, hot phosphoric acid, etc. The polysilicon layer 186 may be doped or undoped.

[0050]

[0090] 17 illustrates step 36, mold pullback, where second layer 110 is removed to form opening 148. Second layer 110 may be removed by any suitable means known to those of skill in the art. In one or more embodiments, second layer 110 is removed by selective etching, for example, a selective wet etch or a selective dry etch. Removal of second layer 110 forms opening 148.

[0051]

[0091] 18 illustrates step 38 of method 10 in which wordline 150 is formed. Wordline 150 includes one or more of oxide layer 150a, barrier layer 150b, and wordline metal 150c. Oxide layer 150a may include any suitable material known to those of skill in the art. In one or more embodiments, oxide layer 150a is an aluminum oxide layer. Barrier layer 150b may include any suitable material known to those of skill in the art. In one or more embodiments, barrier layer 150b includes one or more of titanium nitride (TiN), tantalum nitride (TaN), and the like. In one or more embodiments, wordline metal 150c includes a bulk metal including one or more of copper (Cu), cobalt (Co), tungsten (W), aluminum (Al), ruthenium (Ru), iridium (Ir), molybdenum (Mo), platinum (Pt), tantalum (Ta), titanium (Ti), or rhodium (Rh). In one or more embodiments, the wordline metal 150c includes tungsten (W). In other embodiments, the wordline metal 150c includes ruthenium (Ru). In one or more embodiments, the wordline 150 includes one or more of a metal, a metal nitride, a conductive metal compound, and a semiconductor material. The metal may be selected from one or more of tungsten (W), molybdenum (Mo), tantalum (Ta), niobium (Nb), osmium (Os), zirconium (Zr), iridium (Ir), rhenium (Re), or titanium (Ti). The metal nitride may be selected from one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), molybdenum nitride (MoN), and zirconium nitride (ZrN). The conductive metal compound may be selected from one or more of tungsten oxide (WOx), ruthenium oxide (RuOx), and iridium oxide (IrOx). The semiconductor material may be selected from one or more of silicon (Si), silicon germanium (SiGe), and germanium (Ge).

[0052]

[0092] 19 illustrates step 40 of method 10, in which slits 142 are filled with one or more of a spacer material 152 and a filler material 154. Spacer material 152 may include any suitable material known to those of skill in the art. In one or more embodiments, spacer material 152 is silicon oxide (SiO x ). The insulator material 154 may be any suitable material known to one of ordinary skill in the art. In one or more embodiments, the fill material 154 includes polysilicon. The polysilicon may be doped or undoped. In one or more embodiments, the polysilicon may be N + It is doped polysilicon.

[0053]

[0093] 20 illustrates a cap formed on top of the filled slit. In one or more embodiments, the cap includes a barrier layer 156 and a metal layer 158. Barrier layer 156 may include any suitable material known to one of ordinary skill in the art. In one or more embodiments, barrier layer 156 includes titanium nitride (TiN). Metal layer 158 may include any suitable metal known to one of ordinary skill in the art. In some embodiments, metal 158 includes tungsten (W).

[0054]

[0094] 21A and 21B are diagrams illustrating steps 42 and 44 in which bit line pad studs 162 and word line (W / L) contacts 160 are formed. Bit line studs 162 may be formed by any suitable means known to those skilled in the art.

[0055]

[0095] The word line contact 160 extends a sufficient distance through the memory stack 130 to terminate at one of the word lines 150. In one or more embodiments, the word line contact 160 may comprise any suitable material known to one of ordinary skill in the art. In one or more embodiments, the word line contact 160 comprises one or more of a metal, a metal silicide, polysilicon, amorphous silicon, or EPI silicon. In one or more embodiments, the word line contact 160 is doped with either an N-type dopant or a P-type dopant to reduce contact resistance. In one or more embodiments, the metal of the word line contact 160 is selected from one or more of copper (Cu), cobalt (Co), tungsten (W), titanium (Ti), molybdenum (Mo), nickel (Ni), ruthenium (Ru), silver (Ag), gold (Au), iridium (Ir), tantalum (Ta), or platinum (Pt).

[0056]

[0096] FIG. 22 is a flow diagram illustrating an exemplary alternative method 11 for forming a memory device. Those skilled in the art will recognize that method 11 may include any or all of the illustrated processes. Furthermore, the order of the individual processes may be changed for some parts. Method 11 may start with any of the listed processes without departing from the present disclosure. With reference to FIG. 22, in step 12, a memory stack is formed. In step 14, a word line staircase is formed in the memory stack. In step 16, a memory hole is patterned. In step 18, a nitride layer is recessed. In step 20, a blocking oxide is formed in the recess. In step 22, a charge trapping layer is deposited, followed by a sacrificial layer. In step 24, the sacrificial layer is partially removed. In step 26, the charge trapping layer is unmasked and the sacrificial layer is removed. In step 28, a transistor layer is deposited in the memory hole. In step 30, a bit line pad is formed. In step 32, a slit pattern is formed in the device. In step 34, the common source line sacrificial layer is removed and replaced. In step 36, the nitride layer of the memory stack is removed (mold pullback). In step 37A, the blocking oxide is removed. In step 37B, a portion of the charge trapping layer is oxidized. Method 11 then continues in the same manner as method 10 of FIG. 1. In step 38, the word lines are formed. In step 40, the slits are filled with a dielectric material. In step 42, the bit line pad studs are formed. In step 44, the back-end (BEOL) contacts are formed.

[0057]

[0097] Figures 23A to 26B show alternative method 11. Referring to Figure 22, steps 12 to 36 are identical to those of method 10 described above.

[0058]

[0098] 23A and 23B show the device 100 after the mold pullback step 36, in which the second layer 110 is removed to form an opening 148. The second layer 110 may be removed by any suitable means known to those of skill in the art. In one or more embodiments, the second layer 110 is removed by a selective etch, for example, a selective wet etch or a selective dry etch. Removal of the second layer 110 forms the opening 148.

[0059]

[0099] 24A and 24B, in step 37A, blocking oxide 122 is removed through opening 148. Blocking oxide 122 may be removed by any suitable means known to those skilled in the art.

[0060]

[0100] 25A and 25B illustrate step 37B of method 11, in which a portion of charge trapping layer 124 is oxidized to form oxide layer 182. Charge trapping layer 124 may be partially oxidized by any means known to one of skill in the art. In one or more embodiments, oxide layer 182 may be silicon oxynitride (SiON) or silicon oxide (SiO x ) including one or more of the following:

[0061]

[0101] 26A and 26B illustrate step 38 of method 11 in which word lines 150 are formed. Word lines 150 include one or more of an oxide layer 150a, a barrier layer 150b, and a word line metal 150c. Oxide layer 150a may include any suitable material known to those of skill in the art. In one or more embodiments, oxide layer 150a is an aluminum oxide layer. Barrier layer 150b may include any suitable material known to those of skill in the art. In one or more embodiments, barrier layer 150b includes one or more of titanium nitride (TiN), tantalum nitride (TaN), or the like. In one or more embodiments, the wordline metal 150c comprises a bulk metal including one or more of copper (Cu), cobalt (Co), tungsten (W), aluminum (Al), ruthenium (Ru), iridium (Ir), molybdenum (Mo), platinum (Pt), tantalum (Ta), titanium (Ti), or rhodium (Rh). In one or more embodiments, the wordline metal 150c comprises tungsten (W). In other embodiments, the wordline metal 150c comprises ruthenium (Ru). In one or more embodiments, the wordline 150 comprises one or more of a metal, a metal nitride, a conductive metal compound, and a semiconductor material. The metal may be selected from one or more of tungsten (W), molybdenum (Mo), tantalum (Ta), niobium (Nb), osmium (Os), zirconium (Zr), iridium (Ir), rhenium (Re), or titanium (Ti). The metal nitride may be selected from one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), molybdenum nitride (MoN), and zirconium nitride (ZrN). The conductive metal compound may be selected from one or more of tungsten oxide (WOx), ruthenium oxide (RuOx), and iridium oxide (IrOx). The semiconductor material may be selected from one or more of silicon (Si), silicon germanium (SiGe), and germanium (Ge).

[0062]

[0102] Method 11 then proceeds in the same manner as described above with respect to method 10 of Figures 1 and 19-21B. At step 40, slits 142 are filled. At step 42, bitline pad studs are formed. At step 44, back-end (BEOL) contacts are formed.

[0063]

[0103] In another embodiment, a method of forming a semiconductor device is provided. The method may include forming a memory hole in a memory stack including alternating layers of a first material and a second material on a substrate. The second material is recessed through the memory hole to form a recessed region. A portion of the second material adjacent the memory hole is oxidized to form a blocking oxide layer. A charge trapping layer is deposited on the blocking oxide layer. A sacrificial layer is conformally deposited on the charge trapping layer. The charge trapping layer is selectively removed from the sacrificial layer, and then the sacrificial layer is removed. A bit line is formed in the memory hole. A slit pattern is then formed in the memory device to form a plurality of word lines. The slits are then filled.

[0064]

[0104] An additional embodiment of the present disclosure is directed to a processing tool 900 for forming the described memory devices and methods, as shown in FIG.

[0065]

[0105] The cluster tool 900 includes at least one central transfer station 921, 931 having multiple sides. Robots 925, 935 are positioned within the central transfer stations 921, 931 and configured to move a robot blade and a wafer to each of the multiple sides.

[0066]

[0106] The cluster tool 900 comprises a number of processing chambers, also referred to as process stations, 902, 904, 906, 908, 910, 912, 914, 916, and 918, connected to a central transfer station. The various processing chambers provide separate processing areas isolated from adjacent processing stations. The processing chambers may be any suitable chamber, including, but not limited to, a pre-clean chamber, a buffer chamber, a transfer space, a wafer orienter / degassing chamber, a cryogenic cooling chamber, a deposition chamber, an annealing chamber, an etching chamber, a selective oxidation chamber, an oxide layer thinning chamber, or a word line deposition chamber. The particular arrangement of process chambers and components may vary depending on the cluster tool and should not be considered as limiting the scope of the present disclosure.

[0067]

[0107] In some embodiments, the cluster tool 900 includes a select gate for drain (SGD) patterning chamber. The select gate for drain (SGD) patterning chamber in some embodiments comprises one or more selective etch chambers.

[0068]

[0108] 27, a factory interface 950 is connected to the front of the cluster tool 900. The factory interface 950 includes a loading chamber 954 and an unloading chamber 956 at the front 951 of the factory interface 950. Although the loading chamber 954 is illustrated on the left and the unloading chamber 956 on the right, one of ordinary skill in the art will appreciate that this represents only one possible configuration.

[0069]

[0109] The size and shape of the loading chamber 954 and the unloading chamber 956 can vary depending on, for example, the substrate being processed in the cluster tool 900. In the illustrated embodiment, the loading chamber 954 and the unloading chamber 956 are sized to hold a wafer cassette having multiple wafers positioned within the cassette.

[0070]

[0110] Within the factory interface 950 is a robot 952 that can move between a loading chamber 954 and an unloading chamber 956. The robot 952 can transfer wafers from a cassette in the loading chamber 954 through the factory interface 950 to a load lock chamber 960. The robot 952 can also transfer wafers from the load lock chamber 962 through the factory interface 950 to a cassette in the unloading chamber 956. As will be appreciated by those skilled in the art, the factory interface 950 can include multiple robots 952. For example, the factory interface 950 can include a first robot that transfers wafers between the loading chamber 954 and the load lock chamber 960 and a second robot that transfers wafers between the load lock 962 and the unloading chamber 956.

[0071]

[0111] The illustrated cluster tool 900 includes a first section 920 and a second section 930. The first section 920 is connected to a factory interface 950 through load lock chambers 960, 962. The first section 920 includes a first transfer chamber 921 having at least one robot 925 positioned therein. The robot 925 is also referred to as a robotic wafer transfer mechanism. The first transfer chamber 921 is centrally located relative to the load lock chambers 960, 962, the process chambers 902, 904, 916, 918, and the buffer chambers 922, 924. The robot 925 in some embodiments is a multi-arm robot capable of independently moving multiple wafers at a time. In some embodiments, the first transfer chamber 921 includes multiple robotic wafer transfer mechanisms. The robot 925 in the first transfer chamber 921 is configured to move wafers between chambers around the first transfer chamber 921. Individual wafers are carried on a wafer transport blade located at the distal end of the first robotic mechanism.

[0072]

[0112] After processing the wafer in the first section 920, the wafer may be sent through a pass-through chamber to the second section 930. For example, the chambers 922, 924 may be one-way or two-way pass-through chambers. The pass-through chambers 922, 924 may be used, for example, to cryogenically cool the wafer before processing in the second section 930 or to allow for wafer cooling or post-processing before returning to the first section 920.

[0073]

[0113] A system controller 990 communicates with the first robot 925, the second robot 935, the first plurality of processing chambers 902, 904, 916, 918, and the second plurality of processing chambers 906, 908, 910, 912, 914. The system controller 990 may be any suitable component capable of controlling the processing chambers and robots. For example, the system controller 990 may be a computer including a central processing unit, memory, suitable circuitry, and storage.

[0074]

[0114] The processes may generally be stored in the memory of the system controller 990 as software routines that, when executed by a processor, cause the process chamber to perform the processes of the present disclosure. The software routines may also be stored and / or executed by a second processor (not shown) located remotely from the hardware controlled by the processor. Some or all of the methods of the present disclosure may also be performed in hardware. Thus, the processes may be implemented in software and executed using a computer system, or may be executed in hardware, for example, as an application specific integrated circuit or other type of hardware implementation, or as a combination of software and hardware. The software routines, when executed by a processor, transform a general-purpose computer into a special-purpose computer (controller) that controls the operation of the chamber so that the processes are performed.

[0075]

[0115] In one or more embodiments, the processing tool includes a central transfer station including a robot configured to move the wafer; a plurality of process stations, each process station connected to the central transfer station and providing a processing area isolated from the processing areas of adjacent process stations, the plurality of process stations including a select gate for drain (SGD) patterning chamber; and a controller connected to the central transfer station and the plurality of process stations, the controller configured to activate the robot to move the wafer between the process stations and to control the process performed at each of the process stations.

[0076]

[0116] One or more embodiments provide a non-transitory computer readable medium comprising instructions that, when executed by a controller of a process chamber, cause the process chamber to perform steps of forming a memory hole in a memory stack comprising alternating layers of a first material and a second material on a substrate, recessing a second material through the memory hole to form a first recessed region, oxidizing a portion of the second material adjacent to the memory hole to form a blocking oxide layer, depositing a charge trapping layer on the blocking oxide layer, conformally depositing a sacrificial layer on the charge trapping layer, selectively removing the charge trapping layer from the sacrificial layer, removing the sacrificial layer, forming a bit line in the memory hole, patterning a slit, forming a plurality of word lines, and filling the slits.

[0077]

[0117] The use of the terms "a" and "an" and "the" and similar referents in the context of describing the materials and methods described herein (particularly in the context of the claims below) should be construed to cover both the singular and the plural, unless otherwise stated herein or clearly contradicted by context. The recitation of ranges of values ​​herein is merely intended to serve as a shorthand method of individually referring to each individual value falling within the range, unless otherwise stated herein, and each individual value is incorporated herein as if the value were individually recited herein. All methods described herein may be performed in any suitable order, unless otherwise stated herein or clearly contradicted by context. The use of any and all examples, or exemplary language (e.g., "etc.") provided herein is intended merely to better illuminate the materials and methods, and does not impose limitations on the scope unless otherwise claimed. No language in the specification should be construed as indicating any non-claimed element as essential to the practice of the disclosed materials and methods.

[0078]

[0118] As used throughout this specification, the terms "one embodiment," "particular embodiment," "one or more embodiments," or "embodiments" mean that a particular feature, structure, material, or characteristic described in connection with that embodiment is included in at least one embodiment of the present disclosure. Thus, the appearances of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0079]

[0119] Although the disclosure herein has been described with reference to particular embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the disclosure. Therefore, it is intended that the disclosure cover modifications and variations that come within the scope of the appended claims and their equivalents.

Claims

1. 1. A semiconductor memory device, comprising: a plurality of memory cells formed around a memory hole extending through a memory stack on a substrate, the memory stack including alternating word lines and a dielectric material, each of the plurality of memory cells including a discontinuous blocking oxide layer, a charge trapping layer, and a tunnel oxide layer; the blocking oxide layer is discontinuous between each of the plurality of memory cells, the tunnel oxide layer is continuous between each of the plurality of memory cells, and the charge trapping layer is discontinuous between each of the plurality of memory cells. A plurality of memory cells; a filled slit extending through the memory stack adjacent the memory hole, the filled slit including one or more of a spacer material and a filler material; A semiconductor memory device comprising:

2. 2. The semiconductor memory device of claim 1, wherein the charge trapping layer has a first thickness at a top portion and a second thickness at a center portion, the first thickness being different from the second thickness.

3. The semiconductor memory device of claim 2 , wherein the first thickness is at least 1% greater than the second thickness.

4. The semiconductor memory device of claim 2 , wherein the first thickness is at least 1% less than the second thickness.

5. The semiconductor memory device of claim 1 , wherein the charge trapping layer comprises silicon nitride (SiN).

6. The semiconductor memory device according to claim 1 , further comprising a bit line pad on an upper surface of the memory hole.

7. 10. The semiconductor memory device of claim 1, wherein the wordlines comprise one or more of a metal, a metal nitride, a conductive metal compound, and a semiconductor material.

8. 8. The semiconductor memory device of claim 7, wherein the metal is selected from one or more of tungsten (W), molybdenum (Mo), tantalum (Ta), niobium (Nb), osmium (Os), zirconium (Zr), iridium (Ir), rhenium (Re), and titanium (Ti); the metal nitride is selected from one or more of titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), molybdenum nitride (MoN), and zirconium nitride (ZrN); the conductive metal compound is selected from one or more of tungsten oxide (WOx), ruthenium oxide (RuOx), and iridium oxide (IrOx); and the semiconductor material is selected from one or more of silicon (Si), silicon germanium (SiGe), and germanium (Ge).

9. (delete)

10. 2. The semiconductor memory device of claim 1, wherein the substrate is a common source line, the common source line including a sacrificial layer, an oxide layer, and a polysilicon layer.

11. 10. The semiconductor memory device of claim 1, wherein the semiconductor memory device is a 3D-NAND.

12. 1. A method of forming a semiconductor device, comprising: forming a memory hole in a memory stack including alternating layers of a first material and a second material on a substrate; recessing the second material through the memory hole to form a first recessed region; oxidizing a portion of the second material adjacent the memory hole to form a blocking oxide layer; depositing a charge trapping layer over the blocking oxide layer; conformally depositing a sacrificial layer onto the charge trapping layer; Selectively removing the charge trapping layer from the sacrificial layer; removing the sacrificial layer; forming a bit line in the memory hole; patterning the slits; and forming a plurality of word lines; filling the slits; and The method includes:

13. The method of claim 12 , wherein the charge trapping layer is deposited by atomic layer deposition.

14. 13. The method of claim 12, wherein after the charge trapping layer is selectively removed from the sacrificial layer, the charge trapping layer has a first thickness at a top portion and a second thickness at a center portion, the first thickness being different from the second thickness.

15. The method of claim 14 , wherein the first thickness is at least 1% greater than the second thickness.

16. The method of claim 14 , wherein the first thickness is at least 1% less than the second thickness.

17. forming the bit lines depositing a transistor layer in the memory hole, the transistor layer including one or more of an aluminum oxide (AlO) layer, a trap layer, a tunnel oxide layer, and a channel layer; The method of claim 12, comprising:

18. 13. The method of claim 12, wherein the substrate is a common source line, the common source line including a common source sacrificial layer, an oxide layer, and a polysilicon layer, the method further including removing the sacrificial layer from the common source line to form a common source opening.

19. The method of claim 12 further comprising forming a word line contact.

20. A non-transitory computer readable medium containing instructions that, when executed by a controller of a process chamber, cause the process chamber to: forming a memory hole in a memory stack comprising alternating layers of a first material and a second material on a substrate; recessing the second material through the memory hole to form a first recessed region; oxidizing a portion of the second material adjacent the memory hole to form a blocking oxide layer; depositing a charge trapping layer over the blocking oxide layer; conformally depositing a sacrificial layer onto the charge trapping layer; selectively removing the charge trapping layer from the sacrificial layer; removing the sacrificial layer; forming a bit line in the memory hole; patterning the slits; forming a plurality of word lines; and Filling the slits A non-transitory computer readable medium for causing a program to be executed.

Citation Information

Patent Citations

  • Semiconductor memory device and manufacturing method thereof

    JP2019165133A

  • Three dimensional memory device containing discrete silicon nitride charge storage regions

    US20170243879A1

  • Charge-trap layer separation and word-line isolation in a 3-d NAND structure

    US20180254187A1

  • Semiconductor memory device and manufacturing method therefor

    US20190296038A1

  • Semiconductor devices including separate charge storage layers

    US20210066346A1