Low-viscosity, environmentally friendly insulating coating for silicon steel, silicon steel sheet and its manufacturing method
A novel insulating coating for silicon steel addresses cost, heat resistance, and weldability issues, enhancing bond strength and reducing noise in motors, suitable for high-performance applications.
Patent Information
- Application Number
- JP2024529718
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-22
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024541430000001_ABST
Abstract
Description
[Technical field]
[0001] Technical Field The present disclosure relates to a silicon steel sheet and a manufacturing method thereof, in particular to an insulating coating, a silicon steel sheet and a manufacturing method thereof. [Background technology]
[0002] background In recent years, China has been vigorously promoting the development of new energy vehicles, so that more and more automobile manufacturers and researchers join research and development teams in the field of new energy vehicles. During the research and development of new energy vehicles, it is found that new energy vehicles usually have high performance requirements for their high-performance motors. Compared with the performance requirements for traditional motors, high-performance motors such as those used in new energy vehicles usually require motor cores with the characteristics of high fixing strength, high core efficiency and low magnetic vibration noise.
[0003] In the prior art, silicon steel with special C-3 type coating, such as self-bonding coating, is usually adopted to manufacture iron cores that meet the above performance requirements. Many Chinese and foreign patent applications, such as CN201810275197.8, CN201810885096.2, CN202010591227.3, CN200580037004.6, CN 200410017997.8, US 2007 / 0087201, WO 2004 / 070080, and JPH 621274 A, disclose the composition and application of such C-3 type self-bonding coating products.
[0004] However, due to the following reasons, such C-3 type self-bonding coating products can only be used for certain users or machine types and cannot be widely applied. (1) Self-bonding coating products are expensive, resulting in high costs of use. (2) The single-sided film thickness of the self-bonding coating is usually ≥ 3 μm. As the film thickness increases or the substrate becomes thinner, the lamination factor of the iron core becomes lower, which affects the motor efficiency. (3) The main component of self-bonding coating is organic resin, which cannot withstand stress-relief annealing temperatures above 750°C and / or blue-tempering processes at temperatures above 400°C. There are even few coating products that can withstand temperatures of 210°C for long periods of time. Self-bonding coating products have poor weldability. (4) Self-bonding coatings on iron cores can have problems squeezing out at the edges under hot pressing during final cure.
[0005] Therefore, the practical application effect of the above C-3 type self-bonding coating product is poor.
[0006] Up to now, C-5 type phosphate-based environmentally friendly thin-layer coating (film thickness: 0.5 μm-1.5 μm) products are still widely used as the mainstream coating for high-performance motors represented by new energy vehicles. C-5 type phosphate-based environmentally friendly thin-layer coating products are the most widely used and most carefully developed, and have a relatively low manufacturing cost.
[0007] In the prior art, silicon steel sheets with conventional C-5 type phosphate-based environmentally friendly thin-layer coating have an insulation resistivity (≧5 Ω.cm 2 It has excellent fundamental properties including excellent adhesion (Grade A, GB / T 2522), heat resistance (resistance to stress relief annealing temperatures above 750°C, IEC 60404-12), and weldability (≧40 cm / min, SEP 1210).
[0008] However, in pursuit of higher efficiency of motor, some users use a dedicated device to perform array adhesive dispensing of adhesive on the surface of silicon steel sheet, so as to bond and combine two adjacent silicon steel sheets. This process not only raises the requirement of high bonding strength for the compatibility of coating material and adhesive on the surface of silicon steel sheet, but also presents challenges to the adaptability of dispensing device and process and the stability of large-scale mass production, and the manufacturing cost is high.
[0009] Therefore, in the prior art, the traditional silicon steel sheets coated with C-5 type coating or C-3 type self-bonding coating have some defects and shortcomings, and cannot meet the further requirements for motor cores in the industry.
[0010] Therefore, the traction motor core industry, which has higher requirements for the fixing strength, magnetic vibration noise and efficiency of iron cores, is in need of silicon steel products with functional coatings that are low in cost, highly manufacturable and environmentally friendly.
[0011] In view of this, it is desirable in the art to obtain a novel low-viscosity, environmentally friendly insulating coating for silicon steel, which can be coated on the substrate of silicon steel sheet and form a coating on the substrate. In addition to the properties of the conventional C-5 type coating, such a coating also has the same layering bonding effect as the C-3 type self-bonding coating (but usually has a strength of 7 N / mm 2 It is desirable to have a bond strength of at least 100% by weight, which requires a bond strength of at least 100% by weight, according to ISO 4587 tensile shear test, but does not necessarily achieve the high bond strength of C-3 type self-bonding coatings, and does not have the disadvantage of being unable to withstand heat treatment. Summary of the Invention [Means for solving the problem]
[0012] summary One objective of the present disclosure is to develop a self-bonding coating that not only has the basic performance such as good insulation, adhesion, heat resistance and weldability of the conventional C-5 type coating, but also has a lamination bonding effect similar to that of the C-3 type self-bonding coating, and still has some bonding properties (e.g., bonding strength ≥ 2 N / mm) after the secondary heat / press treatment. 2 The object of the present invention is to provide an insulating coating that forms a coating having a strength in accordance with ISO 4587 tensile shear method. Therefore, some bonding force can be generated between the iron core sheets, so that the iron core structure is strengthened as a whole, and the problems of low fixing strength, low natural frequency and high vibration noise of the iron core can be effectively solved, and a motor with higher efficiency and lower vibration noise can be obtained.
[0013] In order to achieve the above object, in a first aspect, the present disclosure provides an insulating coating comprising the following components (preferably comprising the following components as active ingredients): a water-soluble metal inorganic salt A comprising a water-soluble phosphate A1, wherein the water-soluble phosphate A1 comprises at least one water-soluble phosphate of aluminum, zinc, magnesium, and manganese; a water-dispersible organic emulsion B comprising an epoxy emulsion and its curing agent, at least one of polyester, polyurethane, polyacrylate and ethylene-vinyl acetate copolymer; an additive C comprising at least one of a structural reinforcing additive C1 and a heat resistance reinforcing additive C2, wherein the structural reinforcing additive C1 comprises inorganic nanoparticles, and wherein the heat resistance reinforcing additive C2 is selected from at least one of boric acid and a water-soluble salt of molybdenum, tungsten, vanadium, or titanium; Adjuvant D1; and Solvent D2; Here, the solid content ratio of the water-soluble metal inorganic salt A to the water-dispersible organic emulsion B is (35-85):(15-65) in parts by mass.
[0014] The coating formed by the insulating coating of the present disclosure can be classified as a C-5 or EC-5 type coating according to the ASTM A976 or DIN EN 10342 standards. The coating formed by the insulating coating of the present disclosure not only has the basic performance of the conventional C-5 type coating, such as good insulation, adhesion, heat resistance and weldability, but also has the same layer bonding effect as the C-3 type self-bonding coating (but usually has a strength of 7 N / mm 2 or higher bond strength, ISO 4587 tensile shear test, (does not necessarily achieve the high bond strength of C-3 type self-bonding coatings), and does not have the disadvantage of being unable to withstand heat treatment of C-3 type self-bonding coatings.
[0015] Preferably, in the insulating coating of the present disclosure, the solid content ratio of the water-soluble metal inorganic salt A to the water-dispersible organic emulsion B is (40-75):(25-60) in parts by weight.
[0016] Preferably, in the insulating coating of the present disclosure, the water-soluble metal inorganic salt A further comprises a water-soluble silicate A2. The hardness of the coating formed by the insulating coating can be improved to a certain extent by adding an appropriate amount of the water-soluble silicate A2 to the insulating coating of the present disclosure. However, it is not considered that the water-soluble silicate A2 is added in excess, because if there is an excess of the water-soluble silicate A2, problems of poor compatibility and stability of the coating system are likely to occur. Therefore, in the insulating coating of the present disclosure, the water-soluble silicate A2 constitutes 0-5% of the solid content of the water-soluble metal inorganic salt A, in terms of mass percentage.
[0017] Preferably, in the insulating coating of the present disclosure, the water-soluble silicate A2 has a modulus of less than 4.
[0018] Preferably, in the insulating coating of the present disclosure, the water-soluble silicate A2 comprises sodium silicate and / or potassium silicate.
[0019] Preferably, in the insulating coating of the present disclosure, the water-soluble phosphate A1 constitutes 95% to 100% of the solid content of the water-soluble metal inorganic salt A, and the water-soluble silicate A2 constitutes 0 to 5% of the solid content of the water-soluble metal inorganic salt A, expressed in mass percentage.
[0020] Preferably, in the insulating coating of the present disclosure, the water-soluble metal inorganic salt A comprises at least a water-soluble phosphate of aluminum.
[0021] Preferably, in the insulating coating of the present disclosure, the water-soluble phosphate of aluminum constitutes 70% to 100% of the solid content of the water-soluble phosphate A1, expressed as a percentage by mass.
[0022] Preferably, the water-soluble phosphates of zinc, magnesium and manganese are zinc dihydrogen phosphate, magnesium dihydrogen phosphate and manganese dihydrogen phosphate, respectively, and the total content thereof is 0 to 30% by mass of the water-soluble phosphate A1.
[0023] Preferably, in the insulating coating of the present disclosure, the water-dispersible organic emulsion B has an average particle size D of 2 μm or less. 50 , Average particle size D of 5 μm or less 90 , and has a maximum particle size of 10 μm or less.
[0024] Preferably, in the insulating coating of the present disclosure, the water-dispersible organic emulsion B has an average particle size D of 1 μm or less. 50 and average particle size D of 3 μm or less 90 has.
[0025] Preferably, in the insulating coating of the present disclosure, the water-dispersible organic emulsion B includes an epoxy emulsion and its curing agent. The epoxy emulsion and its curing agent can play a major role in the bonding in the coating formed by the insulating coating of the present disclosure, and at the same time, improve the mechanical protection property, insulation resistivity and heat resistance of the final coating.
[0026] Preferably, in the insulating coating of the present disclosure, the curing agent of the epoxy emulsion is selected from at least one of dicyandiamide, amino resin, imidazole, and polyisocyanate.
[0027] Preferably, in the insulating coating of the present disclosure, the curing agent of the epoxy emulsion has an average particle size D of 5 μm or less. 50 and average particle size D of 10 μm or less 90 is a micronized dicyandiamide having the formula:
[0028] Preferably, in the insulating coating of the present disclosure, the water-dispersible organic emulsion B includes an epoxy emulsion and a curing agent thereof, and the epoxy emulsion constitutes 90%-99% of the total solid content of the epoxy emulsion and the curing agent thereof, in mass percentage. More preferably, the epoxy emulsion constitutes 95%-98% of the total solid content of the epoxy emulsion and the curing agent thereof, in mass percentage.
[0029] Preferably, in the insulating coating of the present disclosure, the epoxy emulsion has an epoxy equivalent weight in the range of 100 g / eq to 2000 g / eq, preferably 200 g / eq to 1000 g / eq; a weight average molecular weight Mw in the range of 200 to 4000, preferably 300 to 3000; and a degree of functionality in the range of 2 to 3.
[0030] In order to obtain a good balance between the bonding performance and heat resistance of the coating, preferably, in the insulating coating of the present disclosure, the water-dispersible organic emulsion B comprises an ethylene-vinyl acetate copolymer, where, in terms of mass percentage, the ethylene-vinyl acetate copolymer constitutes 0-20% of the solid content of the water-dispersible organic emulsion B.
[0031] Preferably, in the insulating coating of the present disclosure, the content of vinyl acetate in the ethylene-vinyl acetate copolymer is in the range of 10% by mass to 40% by mass, and more preferably 15% by mass to 30% by mass.
[0032] Preferably, in the insulating coating of the present disclosure, each of the polyurethane and polyacrylate is an anionic water-dispersible emulsion having a high molecular weight.
[0033] Preferably, in the insulating coating of the present disclosure, the mass of additive C relative to the total mass of water-soluble metal inorganic salt A and water-dispersible organic emulsion B is in the range of 0.1%-10%. If the content of additive C is lower than the lower limit of the above range, the performance characteristics of additive C cannot be obtained; and if the content of additive C is higher than the upper limit of the above range, it easily causes poor stability of the coating, and the lamination bond strength of the coating is reduced. In order to obtain a better effect, the mass of additive C relative to the total mass of water-soluble metal inorganic salt A and water-dispersible organic emulsion B is more preferably in the range of 0.5%-5%.
[0034] Preferably, in the insulating coating of the present disclosure, the aggregates of inorganic nanoparticles have an average particle size in the range of 50 nm to 800 nm, more preferably 80 nm to 500 nm.
[0035] Preferably, in the insulating coating of the present disclosure, the inorganic nanoparticles are metal oxides selected from at least one of SiO2, Al2O3, TiO2, ZnO, ZrO2, Fe3O4, and CaCO3.
[0036] Preferably, in the insulating coating of the present disclosure, the inorganic nanoparticles are SiO2, Al2O3, TiO2, ZnO or composite oxides thereof.
[0037] Preferably, in the insulating coating of the present disclosure, the heat resistance enhancing additive C2 is selected from at least one of boric acid, ammonium molybdate, and sodium tungstate.
[0038] Preferably, the heat-resistance enhancing additive C2 is a water-soluble salt of boric acid (H3BO3) or a variable valence metal, such as molybdenum, tungsten, vanadium, and titanium.
[0039] In the insulating coating of the present disclosure, the total mass of the auxiliary agent D1 and the solvent D2 relative to the total mass of the water-soluble inorganic metal salt A and the water-dispersible organic emulsion B is preferably in the range of 5% to 35%.
[0040] Preferably, in the insulating coating of the present disclosure, the adjuvant D1 is selected from at least one of a defoamer, a wetting agent, a leveling agent, a thickening agent, an anti-settling agent and a flash rust inhibitor, in order to ensure the coating's controllability against defects in the coating rolled at high speed.
[0041] Preferably, in the insulating coating of the present disclosure, the solvent D2 comprises at least two of ethylene glycol, glycerol, n-butyl alcohol, isobutyl alcohol, isopropyl alcohol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, and propylene glycol methyl ether acetate.
[0042] Preferably, the solids content of the insulating coating of the present disclosure ranges from 15% to 40%.
[0043] The insulating coating of the present disclosure is suitable for coating on the surface of the substrate of silicon steel plate of various motors and generator cores, and can form a coating on the substrate, and is particularly suitable for coating non-oriented silicon steel plate used in fields such as new energy vehicle motors, servo motors, and small and special electric machines.
[0044] In a second aspect, the present disclosure provides a silicon steel sheet including a substrate, wherein the substrate has a coating on a surface thereof formed from the insulating coating of the present disclosure.
[0045] Preferably, in the silicon steel sheet of the present disclosure, the coating has a single-side dry film thickness in the range of 0.3 μm to 2 μm, preferably 0.5 μm to 1.5 μm.
[0046] The silicon steel sheet of the present disclosure is coated with the insulating coating of the present disclosure, so that a layer of the coating is formed on the substrate of the silicon steel sheet. The silicon steel sheet of the present disclosure can be used to manufacture the iron core of a driving motor, and the coating still has some bonding properties (e.g., the bonding strength is ≧2 N / mm) after the secondary heat / press treatment. 2 The silicon steel sheet of the present disclosure can be widely used in new energy vehicle motors, servo motors and electric machines, and has good popularization prospects and application value.
[0047] In a third aspect, the present disclosure provides a method for producing a silicon steel sheet, the method comprising the steps of: applying the insulating coating of the present disclosure onto a surface of a substrate of a silicon steel sheet; and drying the insulating coating at a sheet baking temperature of 150°C to 250°C to form a coating.
[0048] Compared with the prior art, the insulating coating, silicon steel sheet and its manufacturing method of the present disclosure have the following advantages and beneficial effects: The components of the insulating coating of the present disclosure are rationally manufactured by optimization design, in which water-soluble phosphate and film-forming emulsion are used as the basic raw materials, and solvents with low toxicity and low harm are selected, so that the resulting insulating coating is a harmless chemical with low volatile organic compound (VOC) emissions, and is completely environmentally friendly.
[0049] The insulating coating of the present disclosure can be coated on the surface of the substrate of silicon steel plate of various motors and generator cores, and can form a coating on the substrate, and is particularly suitable for non-oriented silicon steel used in fields such as new energy vehicle motors, servo motors, and small and special electric machines.
[0050] The coating formed by the insulating coating of the present disclosure not only has the properties of the conventional C-5 type coating, but also has the same layer bonding effect as the C-3 type self-bonding coating (but usually has a bond strength of 7 N / mm 2 or higher bond strength, ISO 4587 tensile shear test, (which does not necessarily achieve the high bond strength of C-3 type self-bonding coatings), and completely avoids the poor heat resistance, poor weldability, low stacking factor and hot press extrusion problems of C-3 type self-bonding coatings.
[0051] The silicon steel sheet of the present disclosure can be used to manufacture the iron core of a drive motor, and the coating still has some bonding properties (e.g., bonding strength ≥ 2 N / mm) after the secondary heat / press treatment. 2 , ISO 4587 tensile shear method). Therefore, some bonding force can be generated between the iron core sheets, so that the iron core structure is strengthened as a whole, and the problems of low fixing strength, low natural frequency and high vibration noise of the iron core can be effectively solved, and a motor with higher efficiency and lower vibration noise can be obtained.
[0052] The manufacturing method of the disclosed silicon steel sheet is environmentally friendly and efficient.
[0053] Furthermore, silicon steel sheets with the coating of the present disclosure can be laminated to form an iron core after a shearing and punching process. Then, magnetic steel can be inserted into the iron core slot with adhesive and subjected to a secondary heating / hardening treatment. After hardening, the fixing of the magnetic steel and the assembly of the iron core are completed. The resulting iron core has high overall strength and significantly improved natural frequency.
[0054] The above secondary curing process can be carried out as follows: the iron core is held at a pressure load of 1 MPa to 5 MPa and an iron core temperature of 150°C to 300°C for 1 minute to 4 hours, preferably the iron core is held at a pressure load of 1 MPa to 5 MPa and an iron core temperature of 150°C to 250°C for 10 minutes to 2 hours. The purpose of the secondary curing process is to cure the adhesive, but in fact the entire iron core is also subjected to a secondary heating process treatment. Therefore, such a heat process can be fully utilized to perform hot pressing on the silicon steel coating of the laminated core, thereby producing a laminated bonding effect. [Brief description of the drawings]
[0055] [Figure 1] FIG. 1 graphically illustrates a plot of bond strength and hardening as a function of sheet bake temperature during the manufacture of silicon steel sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0056] Detailed Description Unless otherwise defined, all technical or scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.
[0057] As used herein, the term "and / or" refers to and includes any and all possible combinations of one or more of the listed items.
[0058] "Solid content" herein refers to the mass percentage of the remaining part of the emulsion or coating material after drying under specified conditions relative to the total amount of the emulsion or coating material. The measurement standard for solid content is EN ISO 3251, and the measurement conditions are 1g / 2h / 130°C (i.e., 1g of coating material is held at a temperature of 130°C for 2 hours).
[0059] As used herein, "modulus" refers to a molar ratio. For example: in the formula R2O·nSiO2, n is the ratio of moles of SiO2 to moles of R2O, and is referred to as the modulus of R2O·nSiO2.
[0060] In this specification, D 50 represents the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 50%, and D 90 represents the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 90%. "Particle size distribution" refers to the percentage of particles with different particle sizes in the total amount of particles in a powder sample reflected by using a specific instrument and method. Laser diffraction method can be used for the measurement. The measurement standard can refer to ISO 13320 Particle size analysis-Laser diffraction method. The measurement device that can be used is, for example, Mastersizer-series laser diffraction particle size analyzer.
[0061] As used herein, "epoxy equivalent weight" refers to the number of grams of epoxy resin containing one equivalent of epoxy groups in units of g / eq, i.e., [grams / equivalent].
[0062] "Functionality" is defined as the number of epoxy groups contained in an epoxy resin molecule. In this specification, "functionality" refers to the average functionality of an epoxy compound and is the average number of groups in one molecule, i.e., the total equivalent number of epoxy functional groups participating in the polycondensation reaction during the epoxy curing process. It can be determined by gel permeation chromatography (according to ISO 13885-1 standard) and nuclear magnetic resonance spectroscopy. In this specification, "functionality" is calculated as the quotient of the weight average molecular weight Mw of the epoxy resin and the epoxy equivalent weight.
[0063] In this specification, the weight average molecular weight Mw is measured by gel chromatography, the reference standard for which is ISO 13885-1 (Binders for coatings and varnishes - Gel permeation chromatography (GPC) - Part 1: Tetrahydrofuran (THF) as eluent).
[0064] In this specification, the structure-reinforcing additive C1 refers to inorganic nanoparticles having reaction activity, and can form physical / chemical crosslinking points with the functional groups of film-forming resins to introduce ROR and / or ROC bonds (R represents metal elements such as Si / Al / Ti / Zr / Zn) into the molecular chains to form a network structure. Inorganic nanoparticles that satisfy the above characteristics can be prepared by using gas phase methods, gas phase deposition methods or related hydrolysis and condensation methods, but they cannot be sol-type products.
[0065] In a preferred embodiment of the insulating coating of the present disclosure, the water-soluble metal inorganic salt A comprises at least a water-soluble phosphate of aluminum.
[0066] The water-soluble phosphate salt of aluminum can be prepared by adding phosphoric acid (H3PO4) and aluminum hydroxide (Al(OH)3) in a molar ratio of (2.3-3.5):1 to a reactor, reacting at a reaction temperature of 70°C to 135°C for 30 to 120 minutes, then cooling, filtering, and discharging the reaction mixture. In some preferred embodiments, the water-soluble phosphate salt of aluminum can be prepared by adding phosphoric acid (H3PO4) and aluminum hydroxide (Al(OH)3) in a molar ratio of (3.0-3.4):1 to a reactor, reacting at a reaction temperature of 70°C to 135°C for 60 to 90 minutes, then cooling, filtering, and discharging the reaction mixture.
[0067] In the insulating coating of the present disclosure, the water-dispersible organic emulsion B is a water-dispersible organic emulsion rather than a water-soluble resin solution. The water-dispersible organic emulsion B can be further classified into the following two categories according to the type of film formation: I. Water-dispersible organic emulsions, such as epoxy emulsions and their hardeners, whose primary film-forming mechanism is crosslinking and curing. II. Water-dispersible organic emulsions, such as polyester, polyurethane, polyacrylate, ethylene-vinyl acetate copolymer emulsions, whose main film-forming mechanism is particle aggregation type film formation. Among them, polyurethane and polyacrylate are preferably anionic water-dispersible emulsions with high molecular weight, whose main film-forming mode is particle aggregation, and the auxiliary film-forming mode can also be self-crosslinking and curing under heating. It can affect the structural performance of the coating, such as hardness, scratch resistance, heat resistance, chemical resistance, etc.
[0068] In a preferred embodiment of the insulating coating of the present disclosure, a compound organic film-forming emulsion formed from at least two of an epoxy emulsion and its curing agent, a polyacrylate emulsion, a polyester, a polyurethane emulsion, and an ethylene-vinyl acetate copolymer is used as a component of the water-dispersible organic emulsion B, so that the coating formed by the insulating coating has good basic performance.
[0069] In the insulating coating of the present disclosure, the solvent D2 is mainly used to increase the solubility of the organic resin and the auxiliary agent D1 in water, and at the same time to reduce the surface tension of the solution to prevent the occurrence of defects such as shrinkage cavities, absent areas, etc. in the coating during the baking process, and also has a defoaming effect.
[0070] For the preparation of the insulating coating of the present disclosure, the water-soluble metal inorganic salt A, the water-dispersible organic emulsion B, the additive C, the auxiliary D1 and the solvent D2 can be added and mixed, and then an appropriate amount of pure water can be added and mixed uniformly by stirring.
[0071] In a preferred embodiment of the insulating coating of the present disclosure, the final insulating coating has a solids content in the range of 15% to 40%, a Tu-4 cup viscosity in the range of 10 seconds to 40 seconds, and therefore good precise control over the film thickness of the coating and high speed roll coating operability can be achieved.
[0072] In the present disclosure, there is no specific limitation on the composition of the substrate of the silicon steel plate, and any composition that can achieve the technical effects of the present disclosure in the prior art may be adopted.
[0073] The insulating coating, silicon steel sheet and its manufacturing method of the present disclosure will be further explained and described below with reference to the accompanying drawings and examples, but the explanations and descriptions do not constitute undue limitations on the technical solutions of the present disclosure.
[0074] Examples 1 to 6 and Comparative Examples 1 to 2 The insulating coatings of Examples 1 to 6 include the following components: water-soluble metal inorganic salt A, water-dispersible organic emulsion B, additive C, auxiliary agent D1 and solvent D2. According to the components and ratios shown in Tables 1 to 8 below, the above water-soluble metal inorganic salt A, water-dispersible organic emulsion B, additive C, auxiliary agent D1 and solvent D2 were mixed and added, and then an appropriate amount of pure water was added and mixed uniformly by stirring to obtain the insulating coatings of Examples 1 to 6.
[0075] In a specific design, it should be noted that the specific requirements for the water-soluble metal inorganic salt A, the water-dispersible organic emulsion B, the additive C, the auxiliary D1 and the solvent D2 are as follows (1) to (4). (1) The water-soluble metal inorganic salt A employed in Examples 1 to 6 must contain at least one water-soluble phosphate A1 of aluminum, zinc, magnesium, and manganese. (2) The water-dispersible organic emulsion B employed in Examples 1 to 6 contains an epoxy emulsion and at least one of its curing agent, polyester, polyurethane, polyacrylate, and ethylene-vinyl acetate copolymer. (3) The additive C employed in Examples 1 to 6 includes a structural strengthening additive C1 and a heat resistance strengthening additive C2. The structural strengthening additive C1 may include inorganic nanoparticles; and the heat resistance strengthening additive C2 is selected from at least one of boric acid and water-soluble salts of molybdenum, tungsten, vanadium, or titanium. (4) In some of Examples 1 to 6, the auxiliary D1 employed includes at least one of: an antifoaming agent, a wetting agent, a leveling agent, a thickening agent, an anti-settling agent and a flash rust inhibitor; and the solvent D2 employed includes at least two of: ethylene glycol, glycerol, n-butyl alcohol, isobutyl alcohol, isopropyl alcohol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether and propylene glycol methyl ether acetate.
[0076] It should be noted that in some of Examples 1 to 6, the water-soluble metal inorganic salt A further contains a water-soluble silicate A2 in addition to the water-soluble phosphate A1. The water-soluble silicate A2 contains sodium silicate and / or potassium silicate. The water-soluble silicate A2 has a ratio of less than 4.
[0077] Table 1 lists the specific components of the insulating coatings of Examples 1-6.
[0078] [Table 1]
[0079] Note: In the above Table 1, Aerodisp® W 640 ZX, HDK® A3017, Aerosil® 300, HDK® A3017, Aerosil® 380 and CAB-O-SIL EH-5 are inorganic nanoparticles and contain at least one of SiO2, Al2O3, TiO2, ZnO, ZrO2, Fe3O4 and CaCO3. In the supplement D1, the added BYK-348 can be used as a wetting agent and defoamer, BYK-346 can be used as a leveling agent and / or wetting agent, BYK-025 is a defoamer, Tego 245 can be used as a wetting agent, leveling agent and defoamer, ZT-709 is a flash rust inhibitor, and Cellosize QP-100MH is an anti-settling agent or thickener.
[0080] Although examples of using water-soluble salts of titanium and vanadium as the heat-resistance strengthening additive C2 are not shown in Examples 1 to 6 in Table 1 above, it should be understood that in other embodiments of the present disclosure, water-soluble salts of titanium and vanadium may be used as the heat-resistance strengthening additive C2.
[0081] As shown in Table 1 above, the water-soluble phosphate containing aluminum was added to the water-soluble metal inorganic salt A employed in Examples 1 to 6. The water-soluble phosphate containing aluminum was prepared by adding phosphoric acid (H3PO4) and aluminum hydroxide (Al(OH)3) in a molar ratio of (2.3-3.5):1 to a reactor, respectively, and reacting at a reaction temperature of 70°C to 135°C for 30 minutes to 120 minutes, then cooling, filtering, and discharging the reaction product.
[0082] Furthermore, it can be seen from Table 1 above that the curing agent of the epoxy emulsion in the water-dispersible organic emulsion B employed in Examples 1 to 6 is finely powdered dicyandiamide.
[0083] It should be understood that in another embodiment of the present disclosure, the curing agent for the epoxy emulsion can also be an amino resin, an imidazole or a polyisocyanate.
[0084] Table 2 shows the content of each component of the insulating coatings of Examples 1 to 6 relative to the total mass of the water-soluble metal inorganic salt A and the water-dispersible organic emulsion B (the total mass of the water-soluble metal inorganic salt A and the water-dispersible organic emulsion B is 100%).
[0085] [Table 2]
[0086] The average particle diameter D of the aggregates of inorganic nanoparticles C1 used in Examples 1 to 6 50 are shown in Table 3 below.
[0087] Average particle size D of water-dispersible organic emulsion B used in Examples 1 to 6 50and D. 90 The specific values are shown in Table 3 below.
[0088] Furthermore, as shown in Table 1, in Examples 1 to 6, the polyurethane and polyacrylate in the water-dispersible organic emulsion B are anionic water-dispersible emulsions having high molecular weights. The epoxy emulsion curing agent in the water-dispersible organic emulsion B used in Examples 1 to 6 is finely powdered dicyandiamide.
[0089] The specific particle sizes of the micronized dicyandiamide added in Examples 1 to 6 are listed in Table 3 below.
[0090] [Table 3]
[0091] Note: In Table 3 above, D 50 represents the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 50%, and D 90 D represents the particle size corresponding to the cumulative particle size distribution percentage of the sample reaching 90%. 50 and D. 90 represents the value of each point at which the particle size distribution is tested. However, due to errors or fluctuations in the test itself, D 50 and D. 90 are recorded in Table 3 as a range of values rather than a single value.
[0092] The epoxy equivalent weight, weight average molecular weight Mw and functionality of the epoxy emulsion in the water-dispersible organic emulsion B in Examples 1 to 6 are shown in Table 4 below.
[0093] [Table 4]
[0094] In Examples 1 to 6, the mass percentage ratio of the solid content of the epoxy emulsion in the water-dispersible organic emulsion B to the solid content of the epoxy emulsion and its curing agent is shown in Table 5 below.
[0095] In Examples 1 to 6, the ratio of the ethylene-vinyl acetate copolymer in water-dispersible organic emulsion B relative to water-dispersible organic emulsion B, and the mass percentage content of vinyl acetate in the ethylene-vinyl acetate copolymer are shown in Table 5 below.
[0096] [Table 5]
[0097] It should be noted that among Examples 1-6, only the water-dispersible organic emulsion B of Example 4 contains an ethylene-vinyl acetate copolymer, but there are many examples not shown in this disclosure that include an ethylene-vinyl acetate copolymer.
[0098] Table 6 shows the solids content ratio of water-soluble phosphate A1 to water-soluble metal inorganic salt A, the solids content ratio of aluminum salt to water-soluble phosphate A1 (in mass percentage), the solids content ratio of water-soluble metal inorganic salt A to water-dispersible organic emulsion B (in parts by mass), the ratio of additive C to the total solids content of water-soluble metal inorganic salt A and water-dispersible organic emulsion B, and the contents of auxiliary D1 and solvent D2 to the total mass of water-soluble metal inorganic salt A and water-dispersible organic emulsion B in the insulating coatings of Examples 1 to 6.
[0099] [Table 6]
[0100] Unlike the insulating coatings in Examples 1 to 6 above, Comparative Examples 1 and 2 are commercially available general coatings.
[0101] The comparative coating of Comparative Example 1 is a commercial Remisol EB 5350S type coating, which is a typical commercial coating for C-5 type coatings on non-oriented silicon steel.
[0102] The comparative coating of Comparative Example 2 is a commercial Remisol EB 549 type coating, which is a typical commercial coating for a C-3 type self-bonding coating on non-oriented silicon steel.
[0103] The insulating coatings of Examples 1-6 and the comparative coatings of Comparative Examples 1-2 were each applied onto two surfaces of a silicon steel plate substrate, then dried and cured at a plate baking temperature of 150°C-250°C to obtain a finished silicon steel plate with different coatings. The dry film thickness of the coating on one side of the plate ranges from 0.3 μm to 2 μm.
[0104] It should be noted that the silicon steel sheet substrates of Examples 1-6 and Comparative Examples 1-2 have the same mass percentage content of each chemical element. Commercially available B30A250 grade non-oriented silicon steel was used as the silicon steel sheet substrate of Examples 1-6 and Comparative Examples 1-2.
[0105] Table 7 lists the process parameters of the finished silicon steel sheets obtained by coating B30A250 grade non-oriented silicon steel with the insulating coatings of Examples 1-6 and the comparative coatings of Comparative Examples 1-2.
[0106] [Table 7]
[0107] The resulting silicon steel sheets having the coatings of the examples and comparative examples were sampled to obtain sample steel sheets, and various tests were carried out on the sample steel sheets. The test results are shown in Table 8 below.
[0108] Table 8 shows the test results of the relevant properties of the finished silicon steel sheets in Examples 1 to 6 and Comparative Examples 1 and 2.
[0109] [Table 8]
[0110] Note: The meanings expressed by the evaluation symbols are: ◎ represents excellent;
[0111] [ka]
[0112] indicates good; ◯ indicates fair; △ indicates poor; × indicates unacceptable.
[0113] As shown in Table 8, the performance of the finished silicon steel sheets of Examples 1 to 6 is significantly better than that of Comparative Example 1 and Comparative Example 2. With reference to Table 8 in combination with Tables 1 to 7, it can be seen that in Examples 1 to 6, the higher the content of organic components in the coating, the better the bond strength, corrosion resistance and insulation resistivity of the coating formed on the silicon steel sheet, but the worse the heat resistance such as annealing resistance and weldability. On the other hand, the coating formed by the coating material containing a compound organic film-forming emulsion containing two or more types of crosslinked cured film-forming emulsion and particle agglomeration film-forming emulsion has better cold bond defect control and scratch resistance, as well as better overall performance.
[0114] As shown in Table 8, the coatings of Examples 3-5 have the performance of a C-5 type coating for non-oriented silicon steel and also have the bonding performance characteristic of a C-3 type self-bonding coating (i.e., they can have the performance of both) and are the best embodiments.
[0115] Comparative Example 1 is a typical commercial coating of C-5 type coating for non-oriented silicon steel. This coating has good general properties but no adhesion properties. Comparative Example 2 is a typical commercial coating of C-3 type self-bonding coating for non-oriented silicon steel. This self-bonding coating has good related properties but cannot withstand heat treatment above 250°C at all and requires high coating film thickness, resulting in high production costs.
[0116] Further, the finished silicon steel sheets of Examples 1 to 6 were slit into coils, punched, and laminated to form iron cores. During assembly, different types of magnetic steel were inserted into the prepared iron core slots, and adhesive was filled on the sidewall surfaces of the magnetic steel and iron core. Then, secondary curing and heat treatment were performed. After curing, the fixing of the magnetic steel and the assembly of the iron core were completed.
[0117] The secondary curing process was carried out as follows: heating for 1 min to 4 h at an iron core temperature of 150 °C to 300 °C and a pressure load of 1 MPa to 5 MPa.
[0118] Similar to the effect of steel with self-bonding coating, the higher the bonding strength of the coating of the obtained silicon steel plate, the stronger the overall bonding strength of the corresponding iron core prepared by the silicon steel plate. Then, it is more beneficial to improve the fixed strength, overall vibration frequency and efficiency of the iron core, and effectively reduce noise.
[0119] FIG. 1 graphically illustrates a plot of bond strength and hardening as a function of sheet bake temperature during the manufacture of silicon steel sheet.
[0120] As shown in Figure 1, the appropriate sheet annealing temperature (peak metal temperature PMT) is 150°C to 250°C. The higher the temperature, the shorter the annealing time required.
[0121] From Figure 1, it can be seen that the effect of annealing hardening process temperature on the performance of coated steel sheet is obvious. The lower the sheet annealing temperature, the lower the hardening degree of the coating, and the better the bonding strength of the coated steel sheet after lamination and forming and hot press hardening, but the worse the scratch resistance (protective property), weldability, corrosion resistance, adhesion and cold bonding controllability of the coating, and even the poor stability problem of continuous production of coated steel coils occurs.
[0122] It should be noted that the combination methods of the technical features in this disclosure are not limited to the combination methods described in the claims or the combination methods described in the specific embodiments of this disclosure. All technical features recorded in this disclosure can be freely combined or integrated in any manner as long as they are not mutually inconsistent.
[0123] It should also be noted that the above embodiments are merely illustrative of specific examples of the present disclosure. The present disclosure is not limited to the above embodiments. Similar modifications or variations that can be easily obtained or derived by those skilled in the art from the contents disclosed by the present disclosure are included in the scope of protection of the present disclosure.
Claims
1. Ingredients below: a water-soluble metal inorganic salt A comprising a water-soluble phosphate A1, said water-soluble phosphate A1 comprising at least one water-soluble phosphate of aluminum, zinc, magnesium and manganese; a water-dispersible organic emulsion B comprising an epoxy emulsion and its curing agent, at least one of polyester, polyurethane, polyacrylate, and ethylene-vinyl acetate copolymer; an additive C comprising at least one of a structural reinforcing additive C1 and a heat resistance reinforcing additive C2, wherein the structural reinforcing additive C1 comprises inorganic nanoparticles, and wherein the heat resistance reinforcing additive C2 is selected from at least one of boric acid and a water-soluble salt of molybdenum, tungsten, vanadium, or titanium; Adjuvant D1; and Solvent D2; wherein the solids content ratio of the water-soluble metal inorganic salt A to the water-dispersible organic emulsion B is (35-85):(15-65) in parts by weight.
2. 2. The insulating coating of claim 1, wherein the solid content ratio of the water-soluble metal inorganic salt A to the water-dispersible organic emulsion B is (40-75):(25-60) by weight.
3. 2. The insulating coating of claim 1, wherein the water-soluble metal inorganic salt A further comprises a water-soluble silicate A2.
4. 4. The insulating coating of claim 3, wherein the water-soluble silicate A2 has a ratio of less than 4.
5. 5. The insulating coating of claim 4, wherein the water-soluble silicate A2 comprises sodium silicate and / or potassium silicate.
6. 2. The insulating coating of claim 1, wherein, in mass percentage, the water-soluble phosphate A1 constitutes 95% to 100% of the solid content of the water-soluble metal inorganic salt A.
7. 2. The insulating coating of claim 1, wherein the water-soluble metallic inorganic salt A comprises at least a water-soluble phosphate of aluminum.
8. 8. The insulating coating of claim 7, wherein the water-soluble phosphate of aluminum constitutes, in mass percentage, 70% to 100% of the solids content of the water-soluble phosphate A1.
9. The water-dispersible organic emulsion B has an average particle diameter D of 2 μm or less. 50 , Average particle size D of 5 μm or less 90 10. The insulating coating of claim 1 having a maximum particle size of 10 μm or less.
10. Water-dispersible organic emulsion B has an average particle diameter D of 1 μm or less. 50 and average particle size D of 3 μm or less 90 10. The insulating coating of claim 9, having a
11. 2. The insulating coating of claim 1, wherein the curing agent for the epoxy emulsion is selected from at least one of dicyandiamide, amino resin, imidazole, and polyisocyanate.
12. The hardener of the epoxy emulsion has an average particle size D of 5 μm or less. 50 and average particle size D of 10 μm or less 90 12. The insulating coating of claim 11, which is a finely divided dicyandiamide having the formula:
13. 2. The insulating coating of claim 1, wherein the water-dispersible organic emulsion B comprises an epoxy emulsion and its curing agent, and in terms of mass percentage, the epoxy emulsion constitutes 90% to 99%, preferably 95% to 98%, of the total solid content of the epoxy emulsion and its curing agent.
14. 2. The insulating coating of claim 1, wherein the epoxy emulsion has an epoxy equivalent weight in the range of 100 g / eq to 2000 g / eq, preferably 200 g / eq to 1000 g / eq; a weight average molecular weight Mw in the range of 200 to 4000, preferably 300 to 3000; and a functionality in the range of 2 to 3.
15. 2. The insulating coating of claim 1, wherein water-dispersible organic emulsion B comprises an ethylene-vinyl acetate copolymer, and wherein, in mass percentage, the ethylene-vinyl acetate copolymer constitutes 0-20% of the solids content of water-dispersible organic emulsion B.
16. 16. The insulating coating of claim 15, wherein the content of vinyl acetate in the ethylene-vinyl acetate copolymer is in the range of 10% to 40% by weight, preferably 15% to 30% by weight.
17. 10. The insulating coating of claim 1, wherein each of the polyurethane and polyacrylate is an anionic water-dispersible emulsion having a high molecular weight.
18. 2. The insulating coating of claim 1, wherein the mass of the additive C relative to the total mass of the water-soluble metal inorganic salt A and the water-dispersible organic emulsion B is in the range of 0.1% to 10%, preferably 0.5% to 5%.
19. 2. The insulating coating of claim 1, wherein the aggregates of inorganic nanoparticles have an average particle size in the range of 50 nm to 800 nm, preferably 80 nm to 500 nm.
20. Inorganic nanoparticles are SiO 2 , Al 2 O 3 , TiO 2 , ZnO, ZrO 2 , Fe 3 O 4 and CaCO 3 2. The insulating coating of claim 1, which is a metal oxide selected from at least one of:
21. Inorganic nanoparticles are SiO 2 , Al 2 O 3 , TiO 2 2. The insulating coating of claim 1, wherein the insulating coating is selected from the group consisting of ZnO, ZnO, and composite oxides thereof.
22. 2. The insulating coating of claim 1, wherein the heat resistance enhancing additive C2 is selected from at least one of boric acid, ammonium molybdate, and sodium tungstate.
23. 2. The insulating coating of claim 1, wherein the total mass of the auxiliary agent D1 and the solvent D2 relative to the total mass of the water-soluble metal inorganic salt A and the water-dispersible organic emulsion B is in the range of 5% to 35%.
24. 2. The insulating coating of claim 1, wherein the adjuvant D1 is selected from at least one of antifoaming agents, wetting agents, leveling agents, thickening agents, antisettling agents and flash rust inhibitors.
25. 10. The insulating coating of claim 1, wherein solvent D2 comprises at least two of ethylene glycol, glycerol, n-butyl alcohol, isobutyl alcohol, isopropyl alcohol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, and propylene glycol methyl ether acetate.
26. 10. The insulating coating of claim 1, wherein the insulating coating has a solids content in the range of 15% to 40%.
27. A silicon steel sheet comprising a substrate, wherein the substrate has a coating on a surface thereof formed from the insulating coating of any one of claims 1 to 26.
28. 28. The silicon steel sheet of claim 27, wherein the coating has a one-side dry film thickness of 0.3 μm to 2 μm, preferably 0.5 μm to 1.5 μm.
29. A method for producing a silicon steel sheet according to claim 27 or 28, comprising the steps of: applying the insulating coating according to any one of claims 1 to 26 onto a surface of a substrate of a silicon steel sheet; and drying the insulating coating at a sheet baking temperature of 150°C to 250°C to form a coating.
Citation Information
Patent Citations
Semi-inorganic environment-friendly insulating paint for non-oriented silicon steel and coating preparation method thereof
CN103013195A
Production of non-oriented electric steel sheet having extremely good film characteristic
JP1994330338A
Silicon steel sheet deposited with insulating film
JP2001107261A
Electromagnetic steel sheet with insulation film and manufacturing method therefor
JP2002294464A
Coating composition for forming an insulating film, non-oriented electrical steel sheet coated with the coating composition, and method for forming an insulating film on the steel plate
JP2003526727A