Improved catalysts for MWCNT production
A carbon nanotube dispersion with iron-free catalyst residues, using an amide solvent and amine compounds, addresses the agglomeration issues of MWCNTs, resulting in stable, low-viscosity dispersions suitable for lithium ion battery electrodes.
Patent Information
- Application Number
- JP2024531356
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-26
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods fail to produce stable dispersions of multi-walled carbon nanotubes (MWCNTs) using iron-free catalysts, leading to agglomeration and high viscosity, making their application in lithium ion batteries challenging due to the risk of dendrite formation and electrode failure.
A carbon nanotube dispersion comprising multi-walled carbon nanotubes with iron-free catalyst residues, an amide solvent, polyvinylpyrrolidone, and amine compounds is developed, using a specific mixing process to achieve a homogeneous dispersion with low viscosity and improved dispersibility.
The dispersion achieves stable, low-viscosity MWCNTs with particle sizes below 15 μm, enhancing their application in battery electrodes by reducing electrode resistance and preventing dendrite formation.
Smart Images

Figure 2024541516000001 
Figure 2024541516000002 
Figure 2024541516000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon nanotube dispersion, more particularly a stable multi-walled carbon nanotube dispersion, with excellent dispersibility and storage of carbon nanotubes. The present invention also relates to a method for producing said dispersion and a battery electrode mixture layer for a lithium ion secondary battery comprising said battery electrode mixture layer. [Background technology]
[0002] Carbon nanostructures (CNS) collectively refer to nano-sized carbon structures with various shapes such as nanotubes, nanohairs, fullerenes, nanocones, nanohorns, and nanorods. Carbon nanostructures have excellent properties and can be widely used in various technological applications.
[0003] Carbon nanotubes (CNTs) are cylindrical materials consisting of carbon atoms arranged in a hexagonal pattern and with a diameter of about 1-100 nm. Depending on their inherent chirality, carbon nanotubes can exhibit insulating, conductive or semiconductive properties. Carbon nanotubes have a structure in which the carbon atoms are strongly covalently bonded to each other. Due to this structure, carbon nanotubes have a tensile strength about 100 times higher than steel, are highly flexible and elastic, and are chemically stable.
[0004] Carbon nanotubes are divided into three types: single-walled carbon nanotubes (SWCNTs), which consist of a single sheet and have a diameter of about 1 nm; double-walled carbon nanotubes (DWCNTs), which consist of two sheets and have a diameter of about 1.4 to 3 nm; and multi-walled carbon nanotubes (MWCNTs), which consist of three or more sheets and have a diameter of about 5 to about 100 nm.
[0005] Depending on their diameter, length, and chirality, carbon nanotubes can exhibit unique optical, electrical, thermal, and mechanical properties.
[0006] However, the advantageous properties of carbon nanotubes are often not realized at the macroscopic level due to several reasons. The first reason is the tendency of carbon nanotubes to crystallize in rope-like structures and become entangled in a network. Strong van der Waals interactions between two carbon nanotubes lead to their alignment and consequent roping. This aggregation of carbon nanotubes often has adverse effects on both electrical and mechanical behavior. The second reason is the insolubility or poor dispersibility of carbon nanotubes in common organic solvents and polymer matrices.
[0007] To address these issues, researchers have developed many methods to produce uniform and stable carbon nanotube dispersions.
[0008] JP2016514080A relates to a dispersion containing a dispersing liquid medium, a polymeric dispersing aid, and carbon nanotubes dispersed in the dispersing liquid medium. The dispersing liquid is selected from the group of water, acetone, nitriles, alcohols, dimethylformamide, N-methylpyrrolidone, pyrrolidone derivatives, butyl acetate, methoxypropyl acetate, alkylbenzenes, cyclohexane derivatives, and mixtures thereof, and poly(vinylpyrrolidone) is disclosed as a dispersing aid between various different polymers.
[0009] CN104795570A relates to a composite conductive paste comprising 4.0-5.0 parts of carbon nanotubes, 0.5-5.0 parts of low expansion graphite, 0.3-1.2 parts of polyvinylpyrrolidone, 88-93 parts of N-methylpyrrolidone, and 0.001-0.01 parts of a complexing agent, wherein the complexing agent is at least one of ethylenediaminetetraacetic acid, sulfosalicylic acid, and acetylacetone.
[0010] EP3816103A1 relates to a carbon nanotube dispersion comprising carbon nanotubes, a solvent such as an amide-based organic solvent such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, and a dispersant such as polyvinylpyrrolidone.
[0011] US7682590A1 relates to a mixture of amide-based organic solvents and polyvinylpyrrolidone for dispersing carbon nanotubes.
[0012] US2011301251A1 relates to dispersible single-walled and multi-walled carbon nanotubes produced by dissolving a surfactant in a solvent to form a solution and adding carbon nanotubes to the solution to form a mixture, where the surfactant includes polyvinylpyrrolidone and the solvent may be N-methylpyrrolidone.
[0013] JP2005162877A discloses a carbon nanotube dispersion solution comprising carbon nanotubes, an amide-based polar organic solvent, and polyvinylpyrrolidone, in which the amide-based polar organic solvent is N-methylpyrrolidone (NMP).
[0014] JP2008138039 discloses a carbon nanofiber dispersion containing an amide-based organic solvent, an amine compound, and a polymer selected from polyvinylpyrrolidone, a copolymer of vinylpyrrolidone and vinyl acetate, a copolymer of vinylpyrrolidone and vinylimidazole, or a copolymer of vinylpyrrolidone and vinylcaprolactam, or a combination thereof. The amide-based organic solvent is selected from dimethylformamide, diethylformamide, dimethylacetamide, N-methylpyrrolidone, etc., while the amine-based compound is selected from 2-methylaminoethanol, 2-aminoethanol, isopropanolamine, n-propylamine, 2-ethoxyethylamine, ethanolamine, etc.
[0015] JP2015072899(A) discloses a carbon fiber dispersion containing a polymeric dispersant, the polymer being selected from cellulose derivatives, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetal, and polyamic acid salts, or a mixture of two or more thereof. The dispersion may further include an amine compound such as N-methyl-2-pyrrolidone and trimethylamine.
[0016] EP3786110(A1) discloses a carbon nanotube dispersion having N-methyl-2-pyrrolidone as a solvent, which has excellent viscosity, dispersibility, and storage stability despite having a high concentration of carbon nanotubes, and provides a cell electrode composite layer having uniform and satisfactory coating film properties and low electrode plate resistance. The carbon nanotube dispersion is characterized by containing carbon nanotubes, polyvinylpyrrolidone, N-methyl-2-pyrrolidone, and an amine compound as a dispersing aid. The carbon nanotube dispersion contains 10 to less than 25 parts by weight of polyvinylpyrrolidone and 2 to 10 parts by weight of an amine-based compound per 100 parts by weight of carbon nanotubes. The amine-based compound is selected from the group consisting of aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, amino acids, alkanolamines, polyoxyalkylene alkylamines, polyamines, and nitrogen-containing alicyclic heterocyclic compounds. The alkanolamines disclosed herein are dimethylaminoethanol, monoethanolamine, diethanolamine, methyldiethanolamine, and triethanolamine. The effect of non-iron-containing catalyst residues on the dispersion process of MWCNTs containing said residues and on the final viscosity of the MWCNT dispersions is not addressed.
[0017] Carbon nanotubes have been attracting attention as a promising electrode backbone or buffer material for lithium batteries.
[0018] A typical lithium-ion battery utilizes a carbon anode (negative electrode) and a lithiated transition metal oxide cathode (positive electrode) positioned on either side of a microporous polymer separator.
[0019] Lithium-ion battery cells start with all the lithium in the cathode, and upon charging, a fraction of this lithium migrates to the anode and becomes intercalated into the carbon anode.
[0020] Failures in lithium-ion batteries are the result of dendrite formation within the battery. Dendrites are tiny deposits of metal that can form in the cell. Dendrite formation typically begins in the anode and creates an internal shortcut as it extends through the separator to the cathode.
[0021] If iron impurities from any electrode dissolve in the electrolyte, there is a significant risk that these impurities will migrate to the anode side and initiate dendrite growth by precipitation, which is why iron-free materials are needed as electrode materials.
[0022] The use of MWCNTs as an electrode material increases the risk of battery failure caused by the dendrites.
[0023] As a result, MWCNTs containing interstitial iron components obtained by processes using catalytic systems that include iron-based graphitization catalysts should be avoided.
[0024] Thus, the inventors have concluded that while they have successfully produced non-iron-containing supported catalysts and MWCNTs using said non-iron-containing supported catalysts, the dispersion media disclosed in the prior art are not sufficient to effectively disperse MWCNTs produced from said non-iron-containing catalysts, including non-iron-containing catalyst residues.
[0025] Due to the longer length of MWCNTs produced from non-iron containing catalysts and the resulting nano- and microstructures formed, dispersion in N-methylpyrrolidone with polyvinylpyrrolidone produces gel-like highly viscous dispersions that are very difficult to process, i.e., good uniformity is difficult to obtain and application on electrode surfaces for lithium battery applications is almost unfeasible. [Prior art documents] [Patent documents]
[0026] [Patent Document 1] JP2016514080A [Patent Document 2] CN104795570A [Patent Document 3] EP3816103A1 [Patent Document 4] US7682590A1 [Patent Document 5] US2011301251A1 [Patent Document 6] JP2005162877A [Patent Document 7] JP2008138039 [Patent Document 8] JP2015072899(A) [Patent Document 9] EP3786110(A1) Summary of the Invention [Problem to be solved by the invention]
[0027] The object of the present invention is to disclose a dispersing medium for the preparation of MWCNT dispersions, to facilitate the dispersion of MWCNTs produced in a process involving a non-iron containing catalyst, and its use in batteries. [Means for solving the problem]
[0028] The present invention provides a carbon nanotube dispersion, - multi-walled carbon nanotubes comprising 0.1-13 wt. % of iron-free catalyst residue, the residue comprising one or more iron-free metal oxide compounds of at least three metals selected from the group consisting of aluminum, vanadium, cobalt and molybdenum; an amide solvent; - polyvinylpyrrolidone, - Amine compounds and A carbon nanotube dispersion is disclosed, comprising:
[0029] Preferred embodiments of the present invention disclose one or more of the following features: the amine-based compound is selected from the group consisting of aliphatic amines, amino acids, alkanolamines, and mixtures thereof; The amine compound has the following formula: NH2-CR1, R2-CH, R2-(CH2) n -OH (In the formula, R1 is methyl, ethyl, propyl or butyl; R2 is a hydrogen, a methyl, ethyl, propyl or butyl group; - n is an integer from 0 to 3. is at least one alkanolamine of the alkanolamine is selected from the group consisting of 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1-butanol, 3-amino-3-methyl-1-butanol, 3-amino-2-methyl-1-butanol, 4-amino-4-methyl-1-pentanol and mixtures thereof; the alkanolamine is 2-amino-2-methyl-1-propanol; the amide solvent is selected from the group consisting of dimethylformamide, diethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone and mixtures thereof; - the amide solvent is N-methyl-2-pyrrolidone; The carbon nanotube dispersion contains, based on the total mass of the amide-based solvent, the iron-free catalyst residue-containing multi-walled carbon nanotubes, the amine-based compound, and the polyvinylpyrrolidone, - multi-walled carbon nanotubes containing 2 to 6% by weight of iron-free catalyst residue, - 0.01 to 2% by weight of polyvinylpyrrolidone, - 0.1 to 2% by mass of amine compounds wherein the sum of the mass percentages of the amide-based solvent, the iron-free catalyst residue-containing multi-walled carbon nanotubes, the amine-based compound and the polyvinylpyrrolidone is equal to 100 mass%; - the carbon nanotube dispersion is The mass ratio of polyvinylpyrrolidone to multi-walled carbon nanotubes containing iron-free catalyst residue is 2.5×10 -4 ~4×10 -1 Included in The mass ratio of the amine-based compound to the multi-walled carbon nanotubes containing the non-iron-containing catalyst residue is 2.5×10 -4 ~4×10 -1 Included in - The mass ratio of the amine compound to polyvinylpyrrolidone is 1×10 -3 Included in ~1,320 Characterized in that the carbon nanotube dispersion is characterized by a complex viscosity comprised between 10 and 1500 Pa.s at 0.2% deformation when obtained from an amplitude oscillatory sweep test with a deformation between 0.1 and 100% at a fixed frequency of 1 Hz at 25°C; The carbon nanotube dispersion is characterized in that the dispersed iron-free catalyst residue-containing multi-walled carbon nanotube aggregates have a D90 of 15 μm or less as measured by a Malvern Mastersizer M3000 (D90 represents the equivalent spherical diameter below which 90% by volume of the aggregates lie).
[0030] The present invention further comprises: - forming a mixture of an amide-based solvent, an amine-based compound and polyvinylpyrrolidone by mixing in a dispersing device for at least 10 minutes; - slowly adding a first portion comprising 20-70% of the total amount of multi-walled carbon nanotubes containing non-iron-containing catalyst residues while mixing for at least 20 minutes; - stopping the mixing to allow trapped air to be removed; - slowly adding a second portion comprising 70-20% of the total amount of iron-free catalyst residue-containing multi-walled carbon nanotubes while dispersing for at least 20 minutes until the dispersion becomes shiny, no aggregates are visible to the naked eye, and a D90 of 15 μm or less is obtained as measured by a Malvern Mastersizer M3000; - stopping the mixing; A method for producing a MWCNT dispersion is disclosed, comprising:
[0031] A preferred embodiment of the method relates to a dispersion device comprising a bead mill having spherical beads with a spherical diameter comprised between 0.7 and 1.0 mm, preferably between 0.7 and 0.9 mm.
[0032] The present invention further discloses an electrode comprising the carbon nanotube dispersion and an electrode active material.
[0033] The present invention further discloses a battery electrode mixture layer comprising a carbon nanotube dispersion formed into a layer and characterized by a surface resistivity of less than 1000 ohms / square as measured by a Keithley 2700 Multimeter in a 250 μm film, obtained by coating the dispersion onto a polyethylene terephthalate film and evaporating the solvent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The present invention provides a multi-walled carbon nanotube dispersion having excellent viscosity, dispersibility, and storage stability, and providing a cell electrode composite layer having uniform and satisfactory coating film properties and low electrode plate resistance, - multi-walled carbon nanotubes; an amide solvent; - polyvinylpyrrolidone, - Amine compounds and A multi-walled carbon nanotube dispersion is disclosed, comprising:
[0035] The multi-walled carbon nanotubes (MWCNTs) of the present invention are obtained from a process that uses a non-iron-containing supported catalyst and, as a result, further comprises catalyst residues (also referred to as catalyst residues).
[0036] The MWCNTs contain 0.1-13 wt %, preferably less than 10 wt %, of catalyst residues, said residues comprising metal compounds of at least two metals selected from IUPAC Groups 4, 5, 6, 7, 9, 10, 11 and 13.
[0037] More specifically, the multi-walled carbon nanotubes include a catalyst residue, said residue including a metal compound of at least three metals selected from the group consisting of aluminum, cobalt, molybdenum, and vanadium.
[0038] The MWCNTs of the present invention are substantially free of iron, whereby substantially free means less than 150 ppm, preferably less than 100 ppm, more preferably less than 50 ppm, and most preferably less than 10 ppm.
[0039] The inventors have observed that MWCNTs produced from non-iron-containing supported catalysts are longer and exhibit different aspect ratios and specific nano- and microstructures compared to MWCNTs produced from iron-containing supported catalysts.
[0040] These differences result in a more difficult dispersion process and dispersions with higher viscosities when the dispersions are made from current dispersion media.
[0041] The dispersion medium of the present invention comprises a polar amide solvent selected from the group consisting of dimethylformamide, diethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, and mixtures thereof.
[0042] Preferably, the polar amide solvent of the dispersion medium of the present invention is N-methyl-2-pyrrolidone.
[0043] Polyvinylpyrrolidone for use in the dispersion medium of the present invention is characterized by a K value comprised between K-12 and K-90, more preferably between K-15 and K-80.
[0044] The amine-based compounds for use in the dispersion medium of the present invention are selected from the group consisting of aliphatic primary amines, aliphatic secondary amines, aliphatic tertiary amines, amino acids, alkanolamines, and mixtures thereof.
[0045] Examples of aliphatic primary amines for use in the dispersion media of the present invention include ethylamine, octylamine, laurylamine, myristylamine, stearylamine, and oleylamine.
[0046] Examples of aliphatic secondary amines for use in the dispersion media of the present invention include diethylamine, dibutylamine, and distearylamine.
[0047] Examples of aliphatic tertiary amines for use in the dispersion media of the present invention include triethylamine, dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dimethylbehenylamine, dilaurylmonomethylamine, and trioctylamine.
[0048] Exemplary amino acids for use in the dispersion media of the present invention include alanine, methionine, proline, serine, asparagine, glutamine, lysine, arginine, histidine, aspartic acid, glutamic acid, and cysteine.
[0049] Preferably, the dispersion medium of the present invention has the formula: NH2-CR1, R2-CH, R2-(CH2) n -OH (In the formula, R1 is a methyl, ethyl, propyl or butyl group; R2 is a hydrogen, a methyl, ethyl, propyl or butyl group; - n is an integer from 0 to 3. Contains alkanolamines.
[0050] More preferably, the dispersion medium of the present invention comprises an alkanolamine selected from the group consisting of 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1-butanol, 3-amino-3-methyl-1-butanol, 3-amino-2-methyl-1-butanol, 4-amino-4-methyl-1-pentanol and mixtures thereof.
[0051] Most preferably, the dispersion medium of the present invention comprises 2-amino-2-methyl-1-propanol.
[0052] Preferably, the dispersion medium of the present invention comprises N-methyl-2-pyrrolidone, polyvinylpyrrolidone K30 and 2-amino-2-methyl-1-propanol.
[0053] Preferably, the dispersion medium of the present invention is - at least 92% by weight, more preferably at least 94% by weight, most preferably at least 95% by weight, and not more than 99.9% by weight, preferably not more than 99% by weight, most preferably not more than 98.5% by weight of N-methyl-2-pyrrolidone, - at least 0.01%, more preferably at least 0.05%, most preferably at least 0.1% by weight of polyvinylpyrrolidone, and not more than 2%, preferably not more than 1.7%, most preferably not more than 1.4% by weight, at least 0.1% by weight, more preferably at least 0.15% by weight, most preferably at least 0.2% by weight, and not more than 2% by weight, preferably not more than 1.8% by weight, most preferably not more than 1.5% by weight of amine-based compounds; Includes.
[0054] The MWCNTs of the present invention are produced using a non-iron containing catalyst.
[0055] Preferably, the non-iron containing supported catalyst is a non-iron containing two-component or three-component supported catalyst, the support comprising aluminum oxide (Al2O3) and / or aluminum hydroxide (Al(OH)3) and aluminum oxide hydroxide (AlO(OH)), as confirmed by X-ray diffraction.
[0056] Preferably, the iron-free dual catalyst comprises a first cobalt-based catalytic component and a second vanadium-based catalytic component, both of which are preferably in the form of oxides.
[0057] Preferably, the iron-free ternary graphitization catalyst comprises a first cobalt-based catalytic component, a second vanadium-based catalytic component and a third molybdenum-based catalytic component, all preferably in the form of oxides.
[0058] The aluminum-based supports of both the bicomponent and ternary supported catalysts contain at least 30 wt. % aluminum oxide hydroxide.
[0059] The bicomponent and ternary supported catalysts have a purity of at least 95%.
[0060] In the production of MWCNTs, a non-iron-containing supported catalyst is contacted with a carbon source in the gas phase.
[0061] The use of supported catalysts allows for the growth of carbon nanotubes by chemical vapor deposition synthesis via the decomposition of a carbon source, resulting in the production of carbon nanotube aggregates.
[0062] Any carbon source capable of providing carbon and being present in the gas phase at a temperature of 300° C. or greater can be used in the chemical vapor deposition synthesis, without particular limitation. The gas phase carbonaceous material is preferably a compound consisting of up to 6 carbon atoms, more preferably a compound consisting of up to 4 carbon atoms.
[0063] The iron-free catalyst according to the invention allows the production of MWCNTs with a carbon yield comprised between 800 and 2500% by weight, preferably between 1000 and 2400% by weight, more preferably between 1100 and 2300% by weight.
[0064] The carbon yield (mass%) is 100(m 総 -m 触媒 ) / m 触媒 (In the formula, m 総 is the total mass of the product after the reaction, m 触媒 is the mass of catalyst used in the reaction) It is defined as:
[0065] The MWCNT obtained by the above method contains 0.1 to 13 mass %, preferably 1 to 10 mass %, of catalyst residue.
[0066] The mass percentage of catalyst residue is determined by thermogravimetric analysis or by calcination in air.
[0067] The MWCNT dispersion is produced in a dispersing device generally used for dispersing pigments and the like.
[0068] Examples of the dispersion device include a homomixer, a planetary mixer, a colloid mill, a cone mill, a ball mill, a sand mill, a pearl mill, a wet jet mill, a roll mill, and a bead mill.
[0069] Preferably, the dispersion device comprises a bead mill having spherical beads with a spherical diameter comprised between 0.7 and 1.0 mm, preferably between 0.7 and 0.9 mm.
[0070] In the method of producing a MWCNT dispersion, the amount (or mass percentage) of MWCNT is the amount (or mass percentage) of MWCNT containing 0.1-13 mass% of non-iron-containing catalyst residue (further referred to as non-iron-containing catalyst residue-containing MWCNT). The catalyst residue is inherently present in the MWCNT as a result of the production of the MWCNT. Thus, for a dispersion of MWCNT containing 2 mass% non-iron-containing catalyst residue with 0.1-13 mass% non-iron-containing catalyst residue, the dispersion will contain 1.998-1.74 mass% pure MWCNT.
[0071] First, a dispersion medium is prepared by mixing an amide-based solvent, an amine-based compound, and polyvinylpyrrolidone in a dispersing device for at least 10 minutes, preferably at least 20 minutes, and the mixture is - at least 92% by weight, more preferably at least 94% by weight, most preferably at least 95% by weight, and not more than 99.9% by weight, preferably not more than 99% by weight, most preferably not more than 98.5% by weight of an amide-based solvent, - at least 0.01%, more preferably at least 0.05%, most preferably at least 0.1% by weight of polyvinylpyrrolidone, and not more than 2%, preferably not more than 1.7%, most preferably not more than 1.4% by weight, at least 0.1%, more preferably at least 0.15%, most preferably at least 0.2%, and not more than 2%, preferably not more than 1.8%, most preferably not more than 1.5%, by weight of amino compounds; The total of the amide-based solvent, polyvinylpyrrolidone and amine-based component is 100 mass %.
[0072] Then, 2 wt. % of the non-iron containing catalyst residue containing MWCNTs is slowly added while mixing for at least 20 minutes, preferably at least 30 minutes.
[0073] Mixing is then stopped to allow trapped air to be removed.
[0074] An additional amount of the non-iron containing catalyst residue containing MWCNTs, up to 6% by weight, is slowly added with continued mixing for at least 20 minutes, preferably at least 30 minutes, until a glossy, uniform dispersion with no visible agglomerates is obtained.
[0075] The amounts of the amide-based solvent, polyvinylpyrrolidone, amine-based compound, and non-iron-containing catalyst residue-containing MWCNTs are determined so that the dispersion of non-iron-containing catalyst residue-containing MWCNTs is - the mass ratio of polyvinylpyrrolidone to MWCNTs containing iron-free catalyst residues is 2.5×10 -4 ~4×10 -1 , preferably 6.5 x 10 -3 ~3.5×10 -1 , more preferably 1.2×10 -1 ~3×10 -1 Included in - The mass ratio of the amine-based compound to the MWCNT containing the iron-free catalyst residue is 2.5×10 -4 ~4×10 -1 , preferably 6.5 x 10 -3 ~3.5×10 -1 , more preferably 1.2×10 -1 ~3×10 -1 Included in - The mass ratio of the amine compound to polyvinylpyrrolidone is 1×10 -3 ~1,320, preferably 1 × 10 -2 ~500, more preferably 5×10 -1 Included in ~2 The method is selected so as to be characterized in that
[0076] In the present invention, mixing means dispersing and homogenizing.
[0077] Dispersion of non-iron containing catalyst residue-containing MWCNTs is considered complete when the dispersed non-iron containing catalyst residue-containing MWCNT agglomerates are characterized by a D90 of 15 μm or less (D90 represents the equivalent spherical diameter below which 90% by volume of the agglomerates lie) as measured by a Malvern Mastersizer M3000.
[0078] The particle size distribution of the dispersion is measured by laser diffraction technique using a Malvern Mastersizer M3000. After automated cleaning and validation of the background of the particle analysis software, the sample is diluted in an aqueous fluid carrier. Once the obscuration is within limits, five measurements are recorded and averaged. Each measurement is performed at room temperature.
[0079] The dispersion of MWCNTs containing iron-free catalyst residue is characterized by a complex viscosity of 10 Pa.s or more at 0.2% deformation when obtained from an amplitude oscillatory sweep test with deformations of 0.1-100% at a fixed frequency of 1 Hz. Preferably, the complex viscosity at 2% deformation is less than 1,500 Pa.s, more preferably less than 1,000 Pa.s, and most preferably less than 500 Pa.s when measured on an Anton Paar MCR-301 controlled stress rheometer at 25°C.
[0080] To evaluate the performance of the iron-free catalytic residue-containing MWCNT dispersion of the present invention in either the cathode or anode of a battery, particularly a lithium-ion battery, the resistivity is measured as the surface resistivity in a 250 micron film. The iron-free catalytic residue-containing MWCNT dispersion is coated on PET (polyethylene terephthalate) and the solvent is evaporated in an oven at 80°C before measurement. Then, 6 points on the surface of the film are measured and averaged using a Keithley 2700 Multimeter. EXAMPLES
[0081] The following illustrative examples are meant only to be illustrative of the invention and are not intended to limit or otherwise define the scope of the invention.
[0082] Example 1 Synthesis of iron-free ternary graphitization catalysts. At 60° C., 5000 parts by weight of water containing 277 parts by weight of citric acid and 387 parts by weight of malic acid were added to 340 parts by weight of ammonium metavanadate and 64 parts by weight of ammonium molybdate tetrahydrate and mixed for 15 minutes using a paddle mixer, resulting in a first aqueous solution.
[0083] Similarly, 5000 parts by weight of water was added to 4931 parts by weight of cobalt (II) acetate tetrahydrate at 60° C. and mixed for 15 minutes using a paddle mixer, resulting in a second aqueous solution.
[0084] The second aqueous solution was added to the first aqueous solution and mixed for 15 minutes using a paddle mixer.
[0085] The mixture of the first and second aqueous solutions was treated with a solution having a specific surface area (BET) of 15 m 2 / g, 13333 parts by weight of aluminum hydroxide (Apyral® 200SM - Nabaltec AG) was added and mixed for 15 minutes using a paddle mixer.
[0086] The paste thus obtained was then transferred to a ceramic crucible with a large opening and subjected to a heating process in which a heating gradient of 2°C / min and a heating rate of 0.5 m were applied. 3 The paste was heated to 120°C by airflow at 10000 / h and maintained at 120°C for 5 h.
[0087] After 5 hours at 120°C, the paste was further heated to 400°C at a heating rate of 2°C / min, and then heated for 0.5 m. 3 The temperature was maintained at 400° C. for 5 hours while maintaining an air flow of 1000 g / h.
[0088] The solid material thus obtained was cooled to room temperature and ground in a cone grinder to a volume median particle diameter (D 50 ) and ground into a powder characterized by
[0089] The non-iron-containing supported catalyst is - The mass ratio of cobalt to aluminum is 2.53 x 10 -1 , - The mass ratio of vanadium to aluminum is 3.20 x 10 -2 , - The mass ratio of molybdenum to aluminum is 7.54 x 10 -3 , - The mass ratio of cobalt to the combined mass of vanadium and molybdenum is 6.4 It is characterized by:
[0090] Example 2 Synthesis of MWCNTs 1.0 g of the non-iron-containing supported graphitized catalyst of Example 1 was spread in a quartz container, which was then placed in the center of a quartz tube reactor having an inlet and an outlet.
[0091] The centre of the quartz tube reactor in which the vessel containing the catalyst was located was heated to a temperature of 700°C.
[0092] Subsequently, ethylene gas, nitrogen and hydrogen were flowed through the quartz tube reactor at flow rates of 1.744 l / min (C2H4), 0.857 l / min (N2) and 0.286 l / min (H2) for 20 minutes.
[0093] MWCNTs were produced with a carbon yield of 2076 wt %, including 5 wt % catalyst residue.
[0094] Example 3 Preparation of MWCNT dispersions A MWCNT dispersion comprising the non-iron containing catalyst residue-containing MWCNTs of Example 2 (3 wt %) in N-methyl-2-pyrrolidone was prepared according to the formulation listed in Table 1.
[0095] [Table 1]
[0096] In Table 1, AMP stands for 2-amino-2-methyl-1-propanol.
[0097] In Table 1, the MWCNT dispersions were prepared in a pilot production line operated in circulation mode using a premixing apparatus consisting of a bead mill with beads of 0.8 mm spherical diameter and a tank with a mixer.
[0098] The iron-free catalyst residue-containing MWCNT dispersions of Examples 4, 5 and 7 were characterized by a D90 of 14.4 μm (amine-based compound: 2-amino-2-methyl-1-propanol), 22 μm (amine-based compound: n-octylamine) and 15 μm (amine-based compound: ethanolamine), respectively, as measured by a Malvern Mastersizer M3000. In comparison, MWCNT dispersions produced under the same dispersion conditions with comparable energy input but without amine-based compound are characterized by a D90 of 19.1 μm.
[0099] The MWCNT dispersions of Examples 4, 5 and 7 were tested for surface resistivity. Surface resistivity values of 855 Ω / sq (amine-based compound: n-octylamine), 983 Ω / sq (amine-based compound: 2-amino-2-methyl-1-propanol) and 890 Ω / sq (amine-based compound: ethanolamine) were measured, respectively. In comparison, the surface resistivity of the MWCNT dispersion without an amine-based compound is equal to 911.8 Ω / sq. According to the inventors, even taking into account the experimental error in the measurement of the surface resistivity, the respective values of the surface resistivity of the dispersion medium with n-octylamine, the dispersion medium with 2-amino-2-methyl-1-propanol, the dispersion medium with ethanolamine and the same dispersion medium without an amine-based compound are comparable.
[0100] As clearly shown from Example 6, increasing the polyvinylpyrrolidone (PVP content) and 2-amino-2-methyl-1-propanol (AMP content) has a large effect on the complex viscosity and D90, while the surface resistivity remains virtually unchanged within experimental error.
[0101] The benefits of the addition of amine-based compounds, particularly alkanolamines, on complex viscosity, D90 and surface resistivity as claimed in this invention have been clearly demonstrated.
Claims
1. A carbon nanotube dispersion, - multi-walled carbon nanotubes comprising 0.1 to 13 wt. % of a non-iron-containing catalyst residue, said residue comprising one or more non-iron-containing metal oxide compounds of at least three metals selected from the group consisting of aluminum, vanadium, cobalt and molybdenum; an amide solvent selected from the group consisting of dimethylformamide, diethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone and mixtures thereof; - polyvinylpyrrolidone, - an amine-based compound selected from the group consisting of aliphatic amines, amino acids, alkanolamines, and mixtures thereof; A carbon nanotube dispersion comprising:
2. The amine compound has the following formula: NH 2 -CR1, R2-CH, R2-(CH 2 ) n -OH (In the formula, R1 is a methyl, ethyl, propyl or butyl group; R2 is a hydrogen, a methyl, ethyl, propyl or butyl group; - n is an integer from 0 to 3.
2. The carbon nanotube dispersion according to claim 1, wherein the at least one alkanolamine is selected from the group consisting of aryl, ...
3. 3. The carbon nanotube dispersion according to claim 1, wherein the alkanolamine is selected from the group consisting of 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1-butanol, 3-amino-3-methyl-1-butanol, 3-amino-2-methyl-1-butanol, 4-amino-4-methyl-1-pentanol, and mixtures thereof.
4. 4. The carbon nanotube dispersion according to claim 1, wherein the alkanolamine is 2-amino-2-methyl-1-propanol.
5. 5. The carbon nanotube dispersion according to claim 1, wherein the amide solvent is N-methyl-2-pyrrolidone.
6. Relative to the total mass of the amide-based solvent, the iron-free catalyst residue-containing multi-walled carbon nanotubes, the amine-based compound, and polyvinylpyrrolidone, - multi-walled carbon nanotubes containing 2 to 6% by weight of iron-free catalyst residues; - 0.01 to 2% by weight of polyvinylpyrrolidone, - 0.1 to 2% by weight of amine compounds 6. The carbon nanotube dispersion of claim 1, wherein the sum of the mass percentages of the amide-based solvent, the iron-free catalyst residue-containing multi-walled carbon nanotubes, the amine-based compound and the polyvinylpyrrolidone is equal to 100 mass%.
7. The mass ratio of polyvinylpyrrolidone to multi-walled carbon nanotubes containing iron-free catalyst residue is 2.5×10 -4 ~4×10 -1 Included in The mass ratio of the amine-based compound to the multi-walled carbon nanotubes containing the non-iron-containing catalyst residue is 2.5×10 -4 ~4×10 -1 Included in - The mass ratio of the amine compound to polyvinylpyrrolidone is 1×10 -3 Included in ~1,320 7. The carbon nanotube dispersion according to claim 1 .
8. A carbon nanotube dispersion as claimed in any one of claims 1 to 7, characterized by a complex viscosity comprised between 10 and 1500 Pa.s at 0.2% deformation when obtained from an amplitude oscillatory sweep test at 25°C and a fixed frequency of 1 Hz with a deformation of 0.1 to 100%.
9. 9. The carbon nanotube dispersion of claim 1, wherein the dispersed iron-free catalyst residue-containing multi-walled carbon nanotube aggregates are characterized by a D90 of 15 μm or less as measured by a Malvern Mastersizer M3000, where D90 represents the equivalent spherical diameter below which 90% by volume of the aggregates lie.
10. A method for producing the carbon nanotube dispersion according to any one of claims 1 to 9, comprising the steps of: a. forming a mixture of an amide-based solvent, an amine-based compound, and polyvinylpyrrolidone by mixing in a dispersing device for at least 10 minutes; b. slowly adding a first portion containing 20-70% of the total amount of multi-walled carbon nanotubes containing non-iron containing catalyst residue while mixing for at least 20 minutes; c. stopping the mixing to allow trapped air to escape; d. slowly adding a second portion containing 70-20% of the total amount of iron-free catalyst residue-containing multi-walled carbon nanotubes while dispersing for at least 20 minutes until the dispersion becomes shiny, no aggregates are visible to the naked eye, and a D90 of 15 μm or less is obtained as measured by a Malvern Mastersizer M3000; e. stopping the mixing; A method comprising:
11. The method according to claim 10, wherein the dispersion device comprises a bead mill having spherical beads with a spherical diameter comprised between 0.7 and 1.0 mm, preferably between 0.7 and 0.9 mm.
12. An electrode comprising the carbon nanotube dispersion according to claim 1 and an electrode active material.
13. A battery electrode mixture layer comprising the carbon nanotube dispersion for an electrode according to claim 12 formed in a layer, characterized by a surface resistivity of less than 1000 ohms / square as measured by a Keithley 2700 Multimeter in a 250 μm film, obtained by coating the dispersion defined in any one of claims 1 to 11 onto a polyethylene terephthalate film and evaporating the solvent.
Citation Information
Patent Citations
Carbon nanotube with high specific surface area and method for producing the same
JP2016501813A
Carbon nanotube dispersion liquid and use of the same
JP2019192537A
Carbon nanotube dispersion liquid and its use
JP2020011872A
Entangled carbon nanotubes and their manufacturing method
JP2020525385A
Composite conductive paste for anodes and cathodes of lithium ion batteries as well as preparation method for composite conductive paste
CN104795570A