Ferritic stainless steel and its manufacturing method
A ferritic stainless steel with controlled alloying and annealing temperatures addresses the challenge of high elongation and productivity in continuous annealing, reducing costs and energy consumption.
Patent Information
- Application Number
- JP2024524740
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Ferritic stainless steel manufacturing processes face challenges in achieving high elongation rates while omitting energy-intensive box annealing, leading to reduced productivity and increased costs.
A ferritic stainless steel composition with controlled alloying elements and annealing heat treatment temperatures, defined by specific formulas, allowing for continuous annealing without box annealing, ensuring an elongation rate of 27% or more.
The solution achieves improved elongation rates and reduced manufacturing costs by optimizing alloy composition and annealing processes, thereby enhancing productivity and energy efficiency.
Smart Images

Figure 2024541928000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel and a manufacturing method thereof, and more particularly to a ferritic stainless steel having improved elongation even without box annealing, and a manufacturing method thereof. [Background technology]
[0002] Ferritic stainless steel contains fewer expensive alloying elements and is more cost-competitive than austenitic stainless steel. Ferritic stainless steel has excellent corrosion resistance and is widely used in construction materials, transportation equipment, home appliances, kitchen appliances, etc. Generally, 430 series hot rolled steel undergoes a box annealing process, which is performed at 800 to 850°C, a temperature at which the austenite phase transforms into the ferrite phase, for 35 to 50 hours. The purpose of the box annealing is to recrystallize the deformation structure formed during hot rolling and to decompose the austenite phase into the ferrite phase and carbides. However, the box annealing process has problems in that it consumes a lot of energy and reduces productivity due to long-term heat treatment. Therefore, the development of a continuous annealing type manufacturing technology that can reduce manufacturing costs by reducing energy and improving productivity has been promoted.
[0003] Patent Document 1 discloses that 430 steel, whose alloy is designed to enable continuous annealing, is hot-rolled at least once with a rough rolling pass at a reduction rate of 20% or more. Patent Document 2 discloses that when finish rolling is performed at a start temperature of 950°C or more and a coiling temperature of 650°C or less, no sticking defects occur and the quality characteristics are good. If 430 series stainless steel is subjected to continuous annealing without box annealing and then heat treated under normal annealing conditions, there is a risk that the elongation will be reduced due to the formation of fine Cr carbides that precipitate during cooling after hot rolling. To solve this problem, there are currently few attempts to improve elongation by controlling the annealing heat treatment temperature of hot-rolled steel and cold-rolled steel, which is related to Ac1, a phase transformation temperature calculated based on the alloy components. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-70230 [Patent Document 2] Japanese Patent Publication No. 57-155326 Summary of the Invention [Problem to be solved by the invention]
[0005] In order to solve the above-mentioned problems, an object of the present invention is to provide a ferritic stainless steel having improved elongation even when continuous annealing is performed without box annealing, and a manufacturing method thereof. [Means for solving the problem]
[0006] The ferritic stainless steel of the present invention contains, by weight, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the balance being Fe (iron) and other unavoidable impurities, and has an Ac1 value defined by the following formula (1) of 920 or more and less than 990. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element. Moreover, the ferritic stainless steel of the present invention has an elongation percentage of 27% or more.
[0007] The method for producing a ferritic stainless steel of the present invention comprises, by weight, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the balance being Fe (iron) and other unavoidable impurities, and the Ac1 value defined by the following formula (1) being 920 The method includes the steps of producing a slab having a hardness of 990 or more and less than 990, reheating the slab, hot rolling the reheated slab and coiling it to produce a hot-rolled steel material, hot-rolling the hot-rolled steel material at a hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.) that satisfies the following formula (2), and then cooling and pickling the hot-rolled and pickled hot-rolled sheet, cold-rolling the hot-rolled and pickled hot-rolled sheet to produce a cold-rolled sheet, and cold-rolling the cold-rolled sheet at a cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.) that satisfies the following formula (3), and then cooling and pickling the cold-rolled sheet. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element. Formula (2): 840≦T(HRA,℃)≦Ac1-20 Formula (3): 870≦T(CRA,℃)≦Ac1-20
[0008] In the method for producing a ferritic stainless steel of the present invention, the reheating step is carried out at a temperature of 1100 to 1250°C. The hot rolling is carried out at a finish rolling completion temperature of 800 to 950°C. The coiling is carried out at a temperature of 750 to 850°C. The hot-rolled sheet annealing and pickling and the cold-rolled sheet annealing and pickling are performed for 30 seconds or more and 10 minutes or less. After the hot-rolled sheet annealing, the sheet is cooled, and after the cold-rolled sheet annealing, the sheet is cooled at a cooling rate of 10 to 50° C. / s. The cold rolling is carried out at a reduction ratio of 60 to 90%. Effect of the Invention
[0009] It is also possible to provide a ferritic stainless steel having improved elongation and a method for producing the same by omitting box annealing and performing continuous annealing while controlling the annealing heat treatment temperature. Also, by eliminating the time-consuming box annealing process, manufacturing costs can be reduced. [Brief description of the drawings]
[0010] [Figure 1] 1 is a graph showing the range of annealing heat treatment temperatures that can ensure an elongation of 27% or more. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The ferritic stainless steel of the present invention contains, by weight, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the balance being Fe (iron) and other unavoidable impurities, and has an Ac1 value defined by the following formula (1) of 920 or more and less than 990. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element.
[0012] Hereinafter, the present invention will be described in detail with reference to the drawings. The following embodiments are presented to fully convey the concept of the present invention to those skilled in the art to which the present invention pertains. The present invention is not limited to the embodiments presented herein and may be embodied in other forms. In the drawings, parts that are not relevant to the description may be omitted in order to clarify the present invention, and the sizes of components may be somewhat exaggerated in order to facilitate understanding. Throughout the specification, when any part is said to "comprise" a certain element, this does not mean to exclude other elements, but that it may further include other elements, unless specifically stated to the contrary. The singular expression includes the plural expression unless the context clearly dictates otherwise.
[0013] The reasons for limiting the numerical values of the alloy component contents in the present invention will be explained below. In the following, the unit is weight percent unless otherwise specified. The ferritic stainless steel of the present invention contains, by weight, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the remainder being Fe (iron) and other unavoidable impurities.
[0014] The C (carbon) content is 0.01% or more and 0.1% or less. C is a strong austenite phase stabilizing element and is effective in increasing material strength through solid solution strengthening. Taking this into consideration, C is added in an amount of 0.01% or more. However, if the C content is excessive, the strength increases excessively, reducing the elongation rate and toughness of the steel. Taking this into consideration, the upper limit of the C content is set to 0.1%.
[0015] The content of Si (silicon) is 0.01% or more and 1.0% or less. Silicon is an element added as a deoxidizer during steelmaking, and is effective in improving yield strength and corrosion resistance. Silicon is also an element that can increase the stability of the ferrite phase. Taking this into consideration, silicon is added in an amount of 0.01% or more. However, if the silicon content is excessive, it may cause hardening of the material, resulting in poor elongation and toughness. Taking this into consideration, the upper limit of silicon content is set to 1.0%.
[0016] The Mn (manganese) content is 0.01% or more and 1.5% or less. Mn is an element effective in improving corrosion resistance. In consideration of this, Mn can be added in an amount of 0.01% or more, and preferably 0.2% or more. However, if the Mn content is excessive, inclusions (MnS) are formed, which deteriorates the hot workability, softness, and toughness of the steel material. In consideration of this, the upper limit of the Mn content is limited to 1.5%, and more preferably 1.0%.
[0017] The P (phosphorus) content is more than 0% and not more than 0.05%. P is an unavoidable impurity contained in steel, and is an element that causes intergranular corrosion during pickling or impairs hot workability. Therefore, it is preferable to control the P content as low as possible. Taking this into consideration, the upper limit of the P content is limited to 0.05%.
[0018] The S (sulfur) content is more than 0% and not more than 0.005%. S is an impurity that is inevitably contained in steel and is an element that segregates at grain boundaries and causes deterioration of hot workability. Therefore, it is preferable to control the S content as low as possible. Taking this into consideration, the upper limit of the S content is limited to 0.005%.
[0019] The Cr (chromium) content is equal to or greater than 13.0% and equal to or less than 18.0%. Cr is an element that forms a passive film in an oxidizing environment and improves corrosion resistance. Taking this into consideration, Cr is added in an amount of 13.0% or more. However, if the Cr content is excessive, it promotes the formation of delta (δ) ferrite in the slab, reducing the elongation and impact toughness and increasing the manufacturing cost. Taking this into consideration, the upper limit of the Cr content is set to 18.0%.
[0020] The N (nitrogen) content is 0.005% or more and 0.1% or less. N, like C, is an interstitial element and is an effective element for improving the yield strength of steel materials by the solid solution strengthening effect. Taking this into consideration, N is added in an amount of 0.005% or more. However, if the N content is excessive, there is a risk of the impact toughness and formability being deteriorated, and in consideration of this, the upper limit of the N content is set to 0.1%.
[0021] The content of Al (aluminum) is 0.005% or more and 0.2% or less. Al is a strong deoxidizer and an element that plays a role in reducing the oxygen content in molten steel. Taking this into consideration, Al is added in an amount of 0.005% or more. However, if the Al content is excessive, nonmetallic inclusions increase, causing sliver defects in the cold rolled strip and deteriorating weldability. Taking this into consideration, the upper limit of the Al content is limited to 0.2%, more preferably to 0.15% or less.
[0022] The Ni (nickel) content is 0.05% or more and 0.25% or less. Ni has the effect of softening steel. Taking this into consideration, Ni is added in an amount of 0.05% or more. However, if the Ni content is excessive, there is a problem of increased costs. Taking this into consideration, the upper limit of the Ni content is limited to 0.25%.
[0023] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities may be inevitably mixed in from the raw materials or the surrounding environment, and it is not possible to exclude them. Since any engineer of a normal manufacturing process would know about these impurities, the contents of all of them will not be mentioned in this specification. The ferritic stainless steel of the present invention has an Ac1 value defined by the following formula (1) of 920 or more and less than 990. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element.
[0024] Ac1 is the temperature at which the austenite phase transforms into the ferrite phase. One of the features of the present invention is that the elongation is improved by controlling the annealing temperature based on the Ac1 value calculated through the design of the alloy composition and the range of components. If the calculated Ac1 value is low, heat treatment is performed at a low temperature and recrystallization does not occur sufficiently during hot-rolled continuous annealing. Taking this into consideration, the alloy composition and component range are designed so that the calculated Ac1 value is 920 or more. However, if the calculated Ac1 value is too high, the content of austenite-forming elements such as C and N is reduced and the formation of carbides and nitrides is insufficient, which may result in poor strength. Taking this into consideration, the alloy composition and component range are designed so that the calculated Ac1 value is less than 990. By controlling the annealing heat treatment temperature based on the calculated Ac1 value, the ferritic stainless steel of the present invention has an elongation of 27% or more.
[0025] Next, a method for producing the ferritic stainless steel of the present invention will be described. The method for producing a ferritic stainless steel of the present invention comprises, by weight%, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the balance being Fe (iron) and other unavoidable impurities, and an Ac1 value defined by the following formula (1) of 920 or more The method includes the steps of producing a slab having a hardness of less than 990, reheating the slab, hot rolling the reheated slab and coiling it to produce a hot-rolled steel material, hot-rolling the hot-rolled steel material at a hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.) that satisfies the following formula (2), and then cooling and pickling the hot-rolled and pickled hot-rolled sheet, cold-rolling the hot-rolled and pickled hot-rolled sheet to produce a cold-rolled sheet, and cold-rolling the cold-rolled sheet at a cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.) that satisfies the following formula (3), and then cooling and pickling the cold-rolled sheet. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element. Formula (2): 840≦T(HRA,℃)≦Ac1-20 Formula (3): 870≦T(CRA,℃)≦Ac1-20
[0026] The component ranges of each alloy composition and the reasons for the numerical limitations of formula (1) are as described above. Each production step will be described in more detail below. First, a slab satisfying the above alloy composition and formula (1) is produced, and then undergoes a series of steps including hot rolling, hot-rolled sheet annealing and pickling, cold rolling, cold-rolled sheet annealing and pickling. The slab is hot rolled at a reheating temperature of 1100 to 1250°C. If the reheating temperature of the slab is too low, the load on the rolling rolls will increase. Taking this into consideration, the reheating temperature of the slab is set to 1100°C or higher. However, if the reheating temperature is too high, the crystal grain size of the slab will become coarse, and there is a risk of the strength being reduced. Taking this into consideration, the upper limit of the reheating temperature of the slab is limited to 1250°C.
[0027] Next, the hot rolling is carried out at a finish rolling completion temperature of 800 to 950°C. If the finish rolling completion temperature is low, the rolling load increases and there is a risk of reducing productivity. Taking this into consideration, the finish rolling completion temperature is set to 800°C or higher. However, if the finish rolling completion temperature is too high, the grain size increases and the strength decreases. Taking this into consideration, the finish rolling completion temperature is controlled to 950°C or lower. The coiling is carried out at a temperature of 750 to 850°C. If the coiling temperature is low, it is difficult to control the coil shape, and if the coiling temperature is too high, there is a risk of defects in the subsequent process due to persistent phase transformation after coiling. Taking this into consideration, the coiling temperature is set to 750 to 850°C.
[0028] Thereafter, the hot-rolled steel material is annealed at a hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.) that satisfies the following formula (2). Formula (2): 840≦T(HRA,℃)≦Ac1-20 When the hot-rolled sheet annealing heat treatment temperature T (HRA, °C) is low, recrystallization does not occur sufficiently. However, since cold-rolled sheet annealing is performed in a later process, it can be performed at a relatively low temperature. Taking this into consideration, the hot-rolled sheet annealing heat treatment temperature T (HRA, °C) is set to 840 °C or higher. However, when the hot-rolled sheet annealing heat treatment temperature T (HRA, °C) is the Ac1 temperature or higher, an austenite phase is formed, and a martensite phase is formed during quenching after heat treatment. Taking this into consideration, the upper limit of the hot-rolled sheet annealing heat treatment temperature T (HRA, °C) is limited to Ac1-20. The hot-rolled sheet annealing is carried out for 30 seconds or more and 10 minutes or less. If the hot-rolled sheet annealing time is short, the proportion of residual martensite may be high, resulting in poor elongation. In consideration of this, the hot-rolled sheet annealing is performed for 30 seconds or more. However, if the hot-rolled sheet annealing time is too long, the strength may decrease due to coarsening of crystal grains, and the thickness of the surface oxide layer may increase, which may result in a long pickling time for removing the oxide layer, leading to insufficient removal of the oxide layer. In consideration of this, the hot-rolled sheet annealing is controlled to 10 minutes or less.
[0029] After the hot-rolled sheet is annealed, the sheet is cooled at a cooling rate of 10 to 50° C. / s. If the cooling rate is low, the softening may cause the structure to become non-uniform, which may result in a decrease in elongation and formability. However, if the cooling rate is too high, the hardening may be excessive, adversely affecting the elongation. In consideration of this, the cooling rate is controlled to 10 to 50°C / s. The cold rolling is performed at a reduction rate of 60 to 90%. If the reduction is low, the stored energy due to cold working is insufficient, making it difficult to obtain a recrystallized structure. However, if the reduction is too high, cracks may occur due to rolling. Taking this into consideration, the reduction is controlled to 60-90%.
[0030] Thereafter, the cold-rolled sheet is annealed at a cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.) that satisfies the following formula (3). Formula (3): 870≦T(CRA,℃)≦Ac1-20 As with the hot-rolled sheet annealing heat treatment temperature T(HRA, °C), when the cold-rolled sheet annealing heat treatment temperature T(CRA, °C) is low, recrystallization does not occur sufficiently. Taking this into consideration, the cold-rolled sheet annealing heat treatment temperature T(CRA, °C) is set to 870°C or higher. However, when the cold-rolled sheet annealing heat treatment temperature T(CRA, °C) is set to the Ac1 temperature or higher, an austenite phase is formed, and a martensite phase may be formed during quenching after heat treatment, so the upper limit of the cold-rolled sheet annealing heat treatment temperature T(CRA, °C) is limited to Ac1-20. The cold-rolled sheet is annealed for 30 seconds or more and 10 minutes or less, and after the cold-rolled sheet is annealed, the sheet is cooled at a cooling rate of 10 to 50° C. / s. The reasons for limiting the numerical values of the cold-rolled sheet annealing time and the cooling rate are as described above.
[0031] The present invention will be described in more detail below through examples. However, the following examples are The following description is intended to illustrate and embody the present invention only, and is not intended to limit the scope of the present invention. It should be noted that the scope of the present invention is not limited to the scope of the claims. This is because it is determined based on the matters described and matters that can be reasonably inferred from them. {Example} Slabs were produced for the various alloy composition ranges shown in Table 1 below. The produced slabs were reheated at 1200°C, hot rolled at a finish rolling completion temperature of 800°C, and then coiled at 750°C to produce hot rolled steel products. Ac1 is the value defined by the following formula (1). Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] mean the content (wt %) of each element.
[0032] [Table 1]
[0033] The hot-rolled steel material thus produced was annealed for 10 minutes at a hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.), cooled at a cooling rate of 30 ° C. / s, and pickled to obtain a hot-rolled pickled hot-rolled sheet. Next, the hot-rolled steel was cold-rolled at a rolling reduction of 60%, annealed for 10 minutes at a cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.), cooled at a cooling rate of 30 ° C. / s, and pickled to produce a steel. Table 2 below shows the hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.), the cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.), the thickness and elongation of the produced steel. The elongation was measured using a Zwick Roell tensile tester.
[0034] [Table 2]
[0035] As shown in Table 2, in all of the examples, annealing was performed at an annealing heat treatment temperature that satisfied the following formulas (2) and (3). Therefore, in all of the examples, the elongation rate satisfied 27% or more. Formula (2): 840≦T(HRA,℃)≦Ac1-20 Formula (3): 870≦T(CRA,℃)≦Ac1-20 Comparative Examples A3, A5, B2 and C1 did not satisfy formula (2). In Comparative Examples A3, A5, B2 and C1, the hot-rolled sheet annealing heat treatment temperature T (HRA, °C) did not satisfy the requirement of 840°C or more, and recrystallization was not sufficiently performed, so that the elongation did not satisfy the requirement of 27% or more. Comparative Examples A1, A2, A4, A6, B1 and C2 did not satisfy formula (3). In Comparative Examples A1, A2, A4 and A6, the cold-rolled sheet annealing heat treatment temperature T (CRA, °C) did not satisfy the requirement of 870°C or more, and recrystallization was not sufficiently performed, so that the elongation did not satisfy the requirement of 27% or more. In Comparative Examples B1 and C2, the cold-rolled sheet annealing heat treatment temperature T (CRA, °C) did not satisfy Ac1-20 °C or less, and the austenite phase was formed, so that the martensite phase was formed during quenching after the heat treatment. Therefore, the elongation did not satisfy 27% or more. FIG. 1 is a graph showing the range of annealing heat treatment temperatures that can ensure an elongation of 27% or more. As shown in FIG. 1, it can be seen that when annealing is performed at an annealing heat treatment temperature that satisfies the following formulas (2) and (3), an elongation of 27% or more can be ensured. Formula (2): 840≦T(HRA,℃)≦Ac1-20 Formula (3): 870≦T(CRA,℃)≦Ac1-20 [Industrial Applicability]
[0036] According to the present invention, it is possible to provide a ferritic stainless steel having improved elongation and a manufacturing method thereof by omitting box annealing and performing continuous annealing while controlling the annealing heat treatment temperature, and by omitting the box annealing step which requires a long time, it is possible to reduce manufacturing costs, and therefore the present invention is found to have industrial applicability.
Claims
1. In weight percent, it contains C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, and the balance being Fe (iron) and other unavoidable impurities, A ferritic stainless steel having an Ac1 value defined by the following formula (1) of 920 or more and less than 990. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) (In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] represent the contents (wt%) of each element.)
2. 2. The ferritic stainless steel according to claim 1, characterized in that it has an elongation of 27% or more.
3. a step of producing a slab containing, by weight, C: 0.01% or more and 0.1% or less, Si: 0.01% or more and 1.0% or less, Mn: 0.01% or more and 1.5% or less, P: more than 0% and 0.05% or less, S: more than 0% and 0.005% or less, Cr: 13.0% or more and 18.0% or less, N: 0.005% or more and 0.1% or less, Al: 0.005% or more and 0.2% or less, Ni: 0.05% or more and 0.25% or less, with the balance being Fe (iron) and other unavoidable impurities, and having an Ac1 value defined by the following formula (1) of 920 or more and less than 990; reheating the slab; hot rolling the reheated slab and coiling it to produce a hot rolled steel material; The hot-rolled steel material is annealed at a hot-rolled sheet annealing heat treatment temperature T (HRA, ° C.) satisfying the following formula (2), and then cooled and pickled to obtain a hot-rolled pickled hot-rolled sheet; cold rolling the hot-rolled pickled hot-rolled sheet to produce a cold-rolled sheet; The cold-rolled sheet is annealed at a cold-rolled sheet annealing heat treatment temperature T (CRA, ° C.) that satisfies the following formula (3), and then cooled and pickled. Formula (1): Ac1=36*[Cr]+90*[Si]+760*[Al]+350-(800*[C]+1300*[N]+150*[Ni]+50*[Mn]) (In the formula (1), [Cr], [Si], [Al], [C], [N], [Ni], and [Mn] represent the contents (wt%) of each element.) Formula (2): 840≦T (HRA, °C)≦Ac1-20 Formula (3): 870≦T(CRA,℃)≦Ac1-20
4. 4. The method of claim 3, wherein the reheating is performed at 1100 to 1250°C.
5. 4. The method for producing a ferritic stainless steel according to claim 3, wherein the hot rolling is performed at a finish rolling completion temperature of 800 to 950°C.
6. The method for producing a ferritic stainless steel according to claim 3, characterized in that the coiling is carried out at a temperature of 750 to 850°C.
7. 4. The method for producing a ferritic stainless steel according to claim 3, wherein the hot-rolled sheet annealing and the cold-rolled sheet annealing are performed for 30 seconds or more and 10 minutes or less.
8. The method for producing ferritic stainless steel according to claim 3, characterized in that the cooling after the hot-rolled sheet annealing and the cooling after the cold-rolled sheet annealing are carried out at a cooling rate of 10 to 50 ° C. / s.
9. The method for producing a ferritic stainless steel according to claim 3, wherein the cold rolling is performed at a reduction ratio of 60 to 90%.
Citation Information
Patent Citations
Production of ferritic stainless steel sheet
JP1978040625A
Manufacture of ferrite stainless steel plate
JP1982023024A
Ferrite stainless steel with superior formability
JP1982085954A
Manufacture of sheet metal for cr stainless steel
JP1988028829A
Production of chromium stainless steel strip of double phase structure having small intra-surface anisotropy and high ductility and high strength
JP1988169333A