Polyamide-based products

A combination of secondary aromatic amine, phosphinic acid derivative, and bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite in glass fiber reinforced polyamides addresses appearance deterioration and mechanical property loss in high-voltage automotive applications, enhancing UV stability and color retention.

JP2024542732AActive Publication Date: 2024-11-15ENVALIOR DEUTSCHLAND GMBH

Patent Information

Application Number
JP2024532722
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-01
Filing Date
2022-11-07
Publication Date
2024-11-15
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

Polyamide-based products used in high-voltage automotive applications suffer from deterioration in appearance due to external influences such as light, heat, and adverse weather conditions, leading to loss of mechanical properties like impact resistance and elongation at break, as well as discoloration, which prior art solutions for improving impact resistance often exacerbate.

Method used

Incorporating a mixture of at least one secondary aromatic amine, at least one phosphinic acid derivative, and bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite into glass fiber reinforced polyamides to enhance UV stability, color retention, and mechanical properties during thermal aging.

Benefits of technology

The composition maintains improved impact resistance, elongation at break, and reduced color change under thermal and UV stress, ensuring long-term performance in high-voltage automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542732000001
    Figure 2024542732000001
  • Figure 2024542732000002
    Figure 2024542732000002
  • Figure 2024542732000003
    Figure 2024542732000003
Patent Text Reader

Abstract

The present invention relates to products based on glass fiber reinforced polyamide and to the use of a mixture comprising at least one secondary aromatic amine, at least one phosphinic acid derivative and bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, as well as to the use of said mixture as an additive for improving the aging behavior in the form of improved retention of elongation at break and impact toughness after thermal aging, improved color retention or improved color stability, and at the same time improved UV stability, compared to products based on glass fiber reinforced polyamide not containing this mixture.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a product based on glass fiber reinforced polyamide and to the use of a mixture comprising at least one secondary aromatic amine, at least one phosphinic acid derivative and bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, as well as to the use of said mixture as an additive for improving the aging behavior in the form of improved retention of elongation at break and impact resistance after thermal aging, improved color retention or improved color stability, and at the same time improved UV stability, compared to a glass fiber reinforced polyamide based product not containing this mixture. [Background technology]

[0002] Elasticity and crack resistance are the reasons for the wide use of polyamides.Polyamides are also of interest to other industrial sectors, especially the automotive sector, due to their strength and rigidity, as well as their resistance to organic solvents such as alcohol, acetone, benzene and fuel.Fuel hoses made of polyamide are now indispensable for automotive structures, as are many components made of polyamide, which replace metals such as aluminum or steel, thus allowing significant weight reduction with uniform properties.

[0003] According to https: / / de.wikipedia.org / wiki / Polyamide, polyamides have a relatively low glass temperature. The glass temperatures of polyamide 6, polyamide 6.6, polyamide 6.10, polyamide 6.12, polyamide 11 or polyamide 12 are all in the range of 37-60°C. To achieve higher stiffness and hardness, as well as better chemical and hydrolysis resistance, reinforcing materials, especially glass fibers, are used in polyamides. Furthermore, by adding glass fibers, one of the disadvantages of polyamides, the relatively high water absorption, can be significantly reduced. In addition to increasing the strength and modulus, the continuous use temperature is also significantly improved due to the use of glass fibers, which significantly expands the possible uses of polyamides, especially in the automotive field. The usage limits extend depending on the chemical structure of the polyamide, from approximately -30°C to over +100°C for polyamide 11, or from -70°C to over +100°C for polyamide 12, with short-term temperatures of approximately 140 to 180°C and even higher being possible, up to 280°C for polyamide 46.

[0004] Although the internal combustion engine has been the main drive concept for many years, new requirements regarding material selection have also led to a research process regarding alternative drive concepts. Here, an essential role is played by electromobility, where the internal combustion engine is replaced partly in hybrid vehicles or completely in electric vehicles by one or more electric motors, which usually get their electrical energy from batteries or fuel cells. While conventional automobiles with an internal combustion engine as the sole drive usually operate with a 12V automotive electrical system, hybrid and electric automobiles with an electric motor as drive unit require significantly higher voltages. This represents further potential dangers that need to be seriously considered for the direct area and surroundings of such voltage-conducting components, and plays an increasingly important role in technical specifications or also in standards. The clear identification of these high-voltage danger areas thus plays an essential role to avoid inadvertent contact with humans, especially drivers or mechanics, and thus the clear color identification of polyamide-based products, especially the orange color, plays a particularly important role in high-voltage applications. The German statutory accident insurance DGUV, in its information document BGI / GUV-I 8686 on "Qualifizierung fur Arbeiten an Fahrzeugen mit Hochvoltsystemen [Qualification for work on vehicles having high-voltage systems]", explains the term high voltage in hybrid and fuel cell technology and electric vehicles, in particular to include voltages > 60 V and < 1500 V in the case of DC voltages, and > 30 V and 1000 V in the case of AC voltages.

[0005] However, polyamide-based products are subject to deterioration of appearance under the influence of external influences, in particular light, UV light, heat or adverse weather conditions. As a result of the influence of high temperatures in particular, deterioration of appearance occurs. The result of such deterioration of appearance is generally recognized in the form of loss of mechanical properties, preferably impact resistance and elongation at break, and in particular discoloration. However, in the case of reinforced and colored polyamide-based products, especially orange polyamide-based products in the high voltage area, for example in automobiles, deterioration processes are not desirable, especially in the form of undesirable discoloration, since a clear and uniform color identification over the period of use is not guaranteed.

[0006] The application of polyamide-based products in the automotive field, preferably electromobility, especially in high voltage areas such as charging plugs, also requires good impact resistance in addition to requirements such as stiffness in the form of elastic modulus.Therefore, polyamide-based products used in high voltage areas may be subjected to large mechanical forces during installation and removal and during use in automobiles, and in this case cannot be damaged.The retention of impact resistance over the service life of the automobile must also be guaranteed.

[0007] A prior art solution to improve the impact resistance of polyamide-based compositions according to Kunststoffhandbuch 3 / 4, Technische Thermoplaste, Polyamide [Plastic handbook 3 / 4, technical thermoplastics, polyamides], Karl Hansen Verlag, Munich, Vienna, 1998, pages 16 and 148-150, is to use amorphous plastics such as ABS or elastomers in polyamide-based blends. Polymers used in other polymers such as polyamides to increase their impact resistance are called modifiers or impact modifiers in technical terms and according to the present invention are called impact modifiers. Suitable impact modifiers for polyamides are ethylene-propylene rubbers (EPM, EPR) or ethylene-propylene-diene rubbers (EPDM), styrene-containing elastomers such as SEBS, SBS, SEPS or acrylate rubbers. However, nitrile rubber (NBR, H-NBR), silicone rubber, EVA and microgels are also suitable as impact modifiers, as described in WO2005 / 033185A1. However, studies in the context of the 2016 paper "Untersuchung der Auswirkungen einer thermisch-oxidativen Beanspruchung auf das Emissionsverhalten von ABS und PP und der Korrelation mit dem Alterungsgrad [Study of the effects of a thermal-oxidative stress on the emission behavior of ABS and PP and the correlation with the degree of aging]" by S. Moll have shown that poly-(acrylonitrile-butadiene-styrene) "ABS" discolors under thermal-oxidative stress.Moreover, it is known to those skilled in the art that the stiffness in the form of the elastic modulus, sometimes also known as the tensile modulus, decreases due to the addition of impact modifiers (Kunststoffhandbuch 3 / 4, Technische Thermoplaste, Polyamide, [Plastic handbook 3 / 4, technical thermoplastics, polyamides], Karl Hansen Verlag, Munich, Vienna, 1998, pages 16 and 157). Therefore, the impact modifiers described in the prior art and typically used for polyamides usually appear to be inappropriate, especially when polyamide-based parts identified by color are considered not prone to discoloration.

[0008] Impact resistance is calculated as the ratio of the impact work to the cross-sectional area of ​​the test piece (unit: kJ / m 2 ) The impact resistance can be determined by various types of impact bending tests, whether according to Charpy to DIN EN ISO 179 or Izod to DIN EN ISO 180. The impact resistance is determined within the scope of the present invention on injection-molded test specimens in the as-molded state (80·10·4 mm 3 ) at 23°C and in accordance with ISO180-1U.

[0009] It is known to those skilled in the art that the glass fiber content affects the impact resistance of polyamide compositions or products produced therefrom (Glasfaserverstarkte Kunststoffe [Glass-fiber-reinforced plastics], PH Selden, Springer-Verlag Berlin, Heidelberg, New York, 1967, pp. 324-325). Therefore, the impact-improving effect of impact modifiers or impact-improving additives can only be compared at the same glass fiber content.

[0010] The elongation at break (in %) represents an index of the deformability of a plastic and is the last elongation value recorded before the tensile strength falls below 10% of the strength value in a tensile test according to DIN EN ISO 527. In the context of the present invention, the elongation at break is measured according to DIN EN ISO 527 on injection-molded test specimens (170·10·4 mm 3 , tension rod type 1A) in the freshly molded state at 23°C.

[0011] In summary, the requirements for polyamide-based products in electromobility applications, especially in the high voltage range, are manifold. In addition to improved impact resistance, both color differentiation and mechanical properties such as impact resistance and elongation at break must be ensured over the life of the vehicle. Conventional techniques for improving impact resistance by using impact modifiers are not suitable, since they lead to discoloration of the polyamide composition or products produced therefrom under thermo-oxidative stress.

[0012] The compositions according to EP 3919562 A1, which contain at least one secondary aromatic amine and at least one phosphinic acid derivative, are suitable for producing polyamide-based products with improved color stability and improved impact resistance retention after thermal aging. However, these products have insufficient UV stability and the retention of elongation at break after thermal aging for 500 hours at 150°C is insufficient for applications in the automotive field. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] WO2005 / 033185A1 [Patent Document 2] EP3919562A1 [Patent Document 3] DE102011084519A1 [Patent Document 4] DE-A4236122 [Patent Document 5] WO2013 / 083247A1 [Patent Document 6] EP0113229B1 [Patent Document 7] WO2009 / 003976A1 [Non-patent literature]

[0014] [Non-Patent Document 1] https: / / de.wikipedia.org / wiki / Polyamide [Non-Patent Document 2] [Qualification for work on vehicles having high-voltage systems] [Non-Patent Document 3] Kunststoffhandbuch 3 / 4, Technische Thermoplaste, Polyamide [Plastic handbook 3 / 4, technical thermoplastics, polyamides], Karl Hansen Verlag, Munich, Vienna, 1998, pp. 16 and 148-150 [Non-Patent Document 4] S. Moll, "Study of the effects of a thermal-oxidative stress on the emission behavior of ABS and PP and the correlation with the degree of aging]" [Non-Patent Document 5] Kunststoffhandbuch 3 / 4, Technische Thermoplaste, Polyamide, [Plastic handbook 3 / 4, technical thermoplastics, polyamides], Karl Hansen Verlag, Munich, Vienna, 1998, pp. 16 and 157

Non-patent document 6

Non-patent document 7

Non-patent document 8

Non-patent document 9

Non-patent document 10

Non-patent document 11

Non-patent document 12

Non-patent document 13

[0015] It was therefore an object of the present invention to provide glass fibre reinforced polyamide based compositions or products produced therefrom which have good ageing behaviour in the form of improved colour retention or improved colour stability after hot air ageing and at the same time improved UV stability and further good ageing behaviour in the form of sufficient retention of impact resistance and especially elongation at break after hot air ageing. [Means for solving the problem]

[0016] Good aging behavior in the form of improved color retention after hot air aging or improved color stability is understood according to the invention to mean a small color difference ΔE calculated according to DIN EN ISO11664-4 after hot air aging at 150° C. for 500 hours, preferably a color difference ΔE in the range from 0 to 20, particularly preferably a color difference ΔE in the range from 0 to 15. In the context of the present invention, therefore, a smaller ΔE value compared to the prior art means a smaller color change. If the color does not change at all after storage, this corresponds to ΔE=0.

[0017] The good aging behavior in the form of improved UV stability is achieved according to the invention at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 This is understood to mean that the color difference ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A at 400 °C for 200 h is small, preferably a color difference ΔE in the range of 0 to 30, particularly preferably a color difference ΔE in the range of 0 to 20. In the context of the present invention, therefore, a smaller ΔE value compared to the prior art means a smaller color change. If the color does not change at all after storage, this corresponds to ΔE=0.

[0018] Good ageing behavior in the form of sufficient retention of impact resistance after hot air ageing is understood according to the invention to mean that the impact resistance of the sample after hot air ageing at 150° C. for 500 hours, measured according to ISO 180-1U, does not decrease by more than 50% compared to the time at 0 hours.

[0019] Good ageing behavior in the form of sufficient retention of the breaking elongation after hot air ageing is understood according to the invention to mean that the breaking elongation, measured according to DIN EN ISO 527 after hot air ageing at 150° C. for 500 hours, does not decrease by more than 30% compared to the time at 0 hours.

[0020] The achievement of this complex objective in the case of glass fiber reinforced polyamide is the use of a mixture comprising at least one secondary aromatic amine, at least one phosphinic acid derivative and bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite.

[0021] The present invention relates to a) at least one polyamide, preferably polyamide 6 or polyamide 66 b) at least one secondary aromatic amine c) General formula (I)

[0022] [ka]

[0023] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' is an alkali metal, an alkaline earth metal, a metal of Groups 12 and 13 of the Periodic Table of the Elements, an ammonium ion, or a C1-C 10 At least one phosphinic acid derivative of d) bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, and e) Glass fiber Compositions and products comprising: However, for 100 parts by mass of component a), 0.1 to 3 parts by weight, preferably 0.3 to 2 parts by weight, particularly preferably 0.35 to 1.5 parts by weight of component b) 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of component c) 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of component d), and With the proviso that from 5 to 200 parts by weight, preferably from 15 to 160 parts by weight, particularly preferably from 30 to 150 parts by weight, of component e) are used.

[0024] Ammonium ion NH4 for R' in formula (I) + is a cation and forms salts with anions, as do alkali metal ions. The ammonium ion is the conjugate acid of the base ammonia (NH3).

[0025] Surprisingly, the glass fiber reinforced polyamide compositions or products based thereon containing components b), c) and d) according to the invention also show good aging behavior in the form of improved UV stability and improved color retention or improved color stability after hot air aging, as well as improved impact resistance and retention of elongation at break after hot air aging, compared to glass fiber reinforced polyamide compositions or products based thereon containing components b) and c) but not d).The various above-mentioned requirements for glass fiber reinforced polyamide-based products for applications in electromobility are thus achieved by combining components b) and c) with the addition of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite.

[0026] It is known to the skilled artisan from PH Selden, Glasfaserverstarkte Kunststoffe [Glass-fiber-reinforced plastics], pages 324-325, chapter "Glasfaserverstarkte Thermoplaste" ["glass-fiber-reinforced thermoplastics"], K. Schlichting, Springer Verlag, Berlin, 1967, that the glass fiber content influences the impact resistance of polyamide compositions. Since the reinforcing material, in particular the glass fiber, itself therefore influences the impact resistance of polyamides, comparative statements within the scope of the present invention always refer to compositions or products with the same content of reinforcing material, in particular glass fiber. This statement also applies to the method and use according to the invention.

[0027] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2for producing glass fibre reinforced polyamide based products having a small colour change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A for 200 hours at 150° C. and / or a retention of impact resistance measured according to ISO 180-1U and / or a retention of elongation at break measured according to ISO 527 after hot air aging for 500 hours at 150° C. b) at least one secondary aromatic amine c) General formula (I)

[0028] [ka]

[0029] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10 At least one phosphinic acid derivative of 5 to 200 parts by weight, preferably 15 to 160 parts by weight, particularly preferably 30 to 150 parts by weight, of at least one polyamide reinforced with glass fibers used as component e), per 100 parts by weight of at least one polyamide used as component a), which is preferably polyamide 6 or polyamide 66, 0.1 to 3 parts by weight, preferably 0.3 to 2 parts by weight, particularly preferably 0.35 to 1.5 parts by weight of component b) 0.01 to 3 parts by weight, preferably 0.05 to 2 parts by weight, particularly preferably 0.1 to 1.7 parts by weight of component c), and It further relates to the use, provided that 0.01 to 3 parts by weight, preferably 0.05 to 1 parts by weight, of component d) are used.

[0030] Finally, the present invention provides a method for reducing the color change ΔE calculated according to DIN EN ISO 11664-4 over 500 hours at 150° C. and / or at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 1. A method for reducing the color change ΔE calculated according to DIN EN ISO 11664-4 after UV irradiation according to DIN ISO 4892-2A at 100° C. for 200 hours and / or for retaining the impact resistance determined according to ISO 180-1U and / or for retaining the elongation at break determined according to ISO 527 after hot air aging at 140° C. for 500 hours, b) at least one secondary aromatic amine c) General formula (I)

[0031] [ka]

[0032] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10 At least one phosphinic acid derivative of d) Bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite is used in glass fiber reinforced polyamide based products, with the proviso that per 100 parts by weight of at least one polyamide, used as component a), preferably polyamide 6 or polyamide 66, and from 5 to 200 parts by weight, preferably from 15 to 160 parts by weight, particularly preferably from 30 to 150 parts by weight, of glass fibers, used as component e), 0.1 to 3 parts by weight, preferably 0.3 to 2 parts by weight, particularly preferably 0.35 to 1.5 parts by weight of component b) 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of component c) with the proviso that 0.01 to 3 parts by weight, preferably 0.05 to 1 parts by weight, of component d) are used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] In the use and method according to the invention, the ammonium ion NH4 + is a cation and forms salts with anions, as do alkali metal ions. The ammonium ion is the conjugate acid of the base ammonia (NH3).

[0034] For the sake of clarity, it is noted that within the scope of the present invention, for the composition according to the invention, the product according to the invention, the use according to the invention and the method according to the invention, the tests for impact resistance according to ISO 180-1U (Izod) and for elongation at break according to ISO 527 are carried out at 23° C. on injection-molded test specimens in the freshly molded state as specified in accordance with DIN EN ISO 1874-2. The freshly molded state, i.e. "dry as molded", is specified in DIN EN ISO 1874-2.

[0035] For the sake of clarity, it is further noted that within the scope of the present invention, the tests of the aging behavior of the compositions according to the invention, the products according to the invention, the uses according to the invention and the methods according to the invention in impact-resistant form were carried out by storing injection-molded test specimens as specified in accordance with DIN EN ISO 1874-2 in a material testing cabinet of the model binder FP115 with circulating air at a temperature of 150° C. for 500 hours. The impact resistance was therefore determined within the scope of the present invention on test specimens produced within the scope of the present invention both before (freshly molded state) and after storage according to ISO 180-1U at 23° C., and the difference in values ​​was noted. The elongation at break was therefore determined within the scope of the present invention on these test specimens both before (freshly molded state) and after thermal aging according to ISO 527, and the difference in values ​​was noted.

[0036] Lab color space (also known as CIELAB, CIEL * a * b * The Lab color space describes all perceptible colors. * uses a three-dimensional color space perpendicular to the color plane (a,b). * The axis describes the brightness (luminance) of the color, with values ​​from 0 to 100. In the example shown, this is * b * All achromatic colors (grayscale) lie at the black end point (L * =0) and the white end point (L * = 100), so L * The axis may also be referred to as the neutral gray axis. Similar to Ewald Hering's complementary color theory, the a coordinate specifies the type and intensity of the color between green and red, and the b coordinate specifies the type and intensity of the color between blue and yellow. The more positive the values ​​of a and b, and the less negative the values ​​of a and b, the stronger the color tone. When a=0 and b=0, there is an achromatic tone on the lightness axis. In a typical software implementation, the L * assumes values ​​between 0 and 100, while a and b can vary between -128 and 127. Discoloration of polymer-based products due to oxidative damage of the polymer matrix can be determined by measuring the color difference ΔE over storage time at elevated temperatures. The color difference ΔE between two color stimuli is calculated according to the formula ΔE = [(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2For the sake of clarity, it is therefore noted that within the scope of the present invention, the tests of the aging behavior of the compositions according to the invention, the products according to the invention, the uses according to the invention and the methods according to the invention in improved color retention / improved color stability form were carried out by storing injection-molded slabs of 60 mm·40 mm·4 mm in a material testing cabinet of the model binder FP115 with circulating air at a temperature of 150° C., referred to hereafter as hot air aging. As a measure of discoloration, within the scope of the present invention, the color difference ΔE of injection-molded products based on the polymer compositions according to the invention is calculated according to the color value L * a * b * is determined before or after hot air aging by measuring ΔE = [(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2

[0037] Thus, according to the invention, good aging behavior in the form of improved color retention after hot air aging or improved color stability is distinguished by the small color change ΔE that occurs. * a * b * is determined in the scope of the present invention on a panel with a size of 60 mm·40 mm·4 mm, from which the color difference ΔE is calculated in accordance with DIN EN ISO11664-4. Small also means that in relation to the use or method, the color difference ΔE is preferably in the range of 0 to 20, in particular in the range of 0 to 15. A small ΔE value means in the scope of the present invention that the color change is small. If the color does not change at all after storage, ΔE=0 results.

[0038] For the sake of clarity, within the scope of the present invention, the tests of the ageing behavior of the compositions according to the invention, the products according to the invention, the uses according to the invention and the methods according to the invention in a form with improved UV stability compared to a glass-fiber-reinforced polyamide-based product containing components b) and c) but not component d) are carried out at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain, referred to hereafter in the abbreviated form as UV storage. 2 The test was carried out by storing injection-molded slabs of 60 mm × 40 mm × 4 mm in a QUV fast weathering tester from Q-Lab in accordance with DIN ISO 4892-2A at 200 °C for 200 h. As a measure of discoloration, in the context of the present invention, the color difference ΔE of the injection-molded products based on the polymer composition according to the invention is calculated by the color value L * a * b * is determined before and after 200 hours of UV storage by measurement of ΔE = [(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2

[0039] Thus, according to the invention, the good ageing behavior in the form of improved UV stability after UV storage in a QUV fast weathering tester is distinguished by the small color change ΔE that occurs compared to polyamide-based products not comprising component d), the color difference ΔE being in the range from 0 to 30, particularly preferably in the range from 0 to 20. Small also means, in relation to the use or method, that the color difference ΔE is preferably in the range from 0 to 30, in particular in the range from 0 to 20.

[0040] Good ageing behavior in the form of sufficient retention of impact resistance after hot air ageing also means, with respect to the use or method, that the impact resistance of a sample measured in accordance with ISO 180-1U after 500 hours of hot air ageing at 150°C does not decrease by more than 50% compared to the time at 0 hours.

[0041] Good ageing behavior in the form of sufficient retention of breaking elongation after hot air ageing also means that, in relation to the use or method, the breaking elongation of a sample after hot air ageing at 150°C for 500 hours, measured according to ISO 527, does not decrease by more than 30% compared to the time at 0 hours.

[0042] For clarity, it should be further noted that the scope of the present invention, relating to the composition according to the present invention, the product according to the present invention, the use according to the present invention and the method according to the present invention, includes all the definitions and parameters listed in the general or any combination of preferred ranges. This also relates in particular to the description of the amounts of the individual components used in the methods and uses claimed in the scope of this application. The standards mentioned in the scope of this application refer to the version applicable at the filing date of the present invention. Unless otherwise indicated, the description of percentages is percent by weight.

[0043] Preferred Embodiments In a further preferred embodiment, the invention relates to compositions and / or reinforced polyamide-based products which, in addition to components a), b), c), d) and e), comprise as component f) at least one flame retardant in an amount of 3 to 100 parts by weight, preferably 5 to 80 parts by weight, particularly preferably 10 to 50 parts by weight, each based on 100 parts by weight of component a).

[0044] For the sake of clarity, it is noted that within the scope of the present invention, all statements about the flame retardants used as component f) and the amounts mentioned therein relate to both the compositions and polyamide-based products produced therefrom, in particular polyamide-based products in high voltage applications, and apply to the uses and methods according to the invention.

[0045] In a further embodiment, the present invention relates to a composition and / or a reinforced polyamide-based product which, in addition to or instead of components a), b), c), d), e) and f), also comprises from 0.01 to 80 parts by weight, preferably from 0.05 to 50 parts by weight, particularly preferably from 0.1 to 30 parts by weight, of at least one further additive g) which is different from components b), c), d), e) and f), in each case based on 100 parts by weight of component a).

[0046] For the sake of clarity, it is noted that within the scope of the present invention, all statements of the additives used as component g) and the amounts mentioned therein all relate to both the polyamide-based compositions and the polyamide-based products produced therefrom, in particular polyamide-based products in high voltage applications, and apply to the uses and methods according to the invention.

[0047] Component a) The polyamides used according to the invention as component a) can be produced according to various methods and can be synthesized from various building blocks. Various methods are known for producing polyamides, and depending on the desired end product, various monomer building blocks, various chain regulators for setting the desired molecular weight, or even monomers with reactive groups for post-treatment, can be used as intended.

[0048] Technically relevant processes for producing polyamides are usually carried out by polycondensation in the melt. The hydrolytic polymerization of lactams is also understood in this context as polycondensation.

[0049] Aliphatic and / or aromatic dicarboxylic acids such as adipic acid, 2,2,4- and 2,4,4-trimethyladipic acid, azelaic acid, sebacic acid, isophthalic acid, terephthalic acid, etc., aliphatic and / or aromatic diamines such as tetramethylenediamine, hexamethylenediamine, 1,9-nonanediamine, 2,2,4- and 2,4,4-trimethylhexamethylenediamine, diaminodicyclohexylmethane isomers, diaminodicyclohexylpropane, bisamino-methylcyclohexane, phenylenediamine, xylylenediamine, etc., aminocarboxylic acids such as aminocapronic acid, and the corresponding lactams are considered as educts. Caprolactam, especially ε-caprolactam, is particularly preferably used. Copolyamides made from some of the mentioned monomers are included.

[0050] Preferred polyamides are partially crystalline polyamides which can be produced starting from diamines and dicarboxylic acids and / or lactams having at least 5 ring members or the corresponding amino acids. The partially crystalline polyamides preferably used according to the invention are distinguished according to DE102011084519A1 by a melting enthalpy of greater than 25 J / g, measured using the DSC method according to ISO11357 during the second heating and merging of the melting peaks.

[0051] Polyamide 6, polyamide 6.6, polyamide 4.6 and / or partially aromatic copolyamides are particularly preferably used as polyamides. Preferred partially aromatic copolyamides are PA6T / 6, PA6T / 66, PA6T / 6I or PA6T / 6I / 66.

[0052] The designation of polyamides used within the scope of this application corresponds to the international standard ISO 1874-1, where the first number designates the number of C atoms of the starting diamine and the last number designates the number of C carbon atoms of the dicarboxylic acid. If only one number is designated, as in the case of PA6, this means that the synthesis started from an α,ω-aminocarboxylic acid or a lactam derived therefrom, in the case of PA6, namely ε-caprolactam.

[0053] Polyamide 6 [CAS number 25038-54-4], which is particularly preferably used as component a) according to the invention, preferably has a viscosity number in the range of 80 to 180 ml / g, particularly preferably in the range of 85 to 170 ml / g and very particularly preferably in the range of 90 to 160 ml / g in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C., determined according to ISO 307. Polyamide 6 which is preferably used according to the invention as component a) is available, for example, as Durethan® B29 from Lanxess Deutschland GmbH (Cologne).

[0054] Polyamide 66 [CAS number 32131-17-2], which is particularly preferably used as component a), preferably has a viscosity number in the range of 80 to 180 ml / g, very particularly preferably in the range of 85 to 170 ml / g and particularly preferably in the range of 90 to 160 ml / g in a 0.5% by weight solution in 96% by weight sulfuric acid at 25° C., determined according to ISO 307. The polyamide 66 used according to the invention as component a) is available, for example, as Ultramid® A27E01 from BASF SE (Ludwigshafen).

[0055] The polyamides used according to the invention as component a) can also be used in a mixture with at least one other polyamide or in the form of a copolyamide.

[0056] Typical additives known to the person skilled in the art, preferably release agents, stabilizers and / or anticaking agents, can be mixed into the polyamide used as component a) already in the melt.

[0057] Component b) According to the invention, at least one secondary aromatic amine is used as component b).

[0058] [ka]

[0059] (In the formula, m and n each independently represent 0 or 1; A and B each independently represent a tertiary C atom substituted by C1-C4-alkyl or phenyl, R 1 and R 2 each independently of the other represents hydrogen, a C1-C6-alkyl group in the ortho- and para-positions which may be substituted by one to three phenyl radicals, or a halogen, a carboxyl or a metal salt of this carboxyl group, R 3 and R 4 each independently of one another represents hydrogen or a methyl radical in the ortho- and para-position, or represents a tertiary C3-C9-alkyl group in the ortho- or para-position, which can optionally be substituted by one to three phenyl radicals), is preferred.

[0060] Preferred A or B groups in formula (II) are symmetrically substituted tertiary carbon atoms, with dimethyl-substituted tertiary carbons being particularly preferred.Tertiary carbons bearing one to two phenyl groups as substituents are also preferred.

[0061] Preferred R in formula (II) 1 and R 2The group is a tert-butyl- or trimethyl-substituted quaternary carbon atom, where the methyl group is preferably replaced by one to three phenyl groups, and particularly preferably by one phenyl- or tetramethyl-substituted n-butyl, where the methyl group may be replaced by a phenyl group. Preferred halogens are bromine and chlorine. The metal salt is preferably a compound of formula (II) where R 1 or R 2 forms a carboxyl metal salt.

[0062] Preferred R in formula (II) 3 and R 4 The group is a hydrogen and a trimethyl-substituted quaternary carbon atom in the ortho- or para-position, the methyl group being preferably replaced by one to three phenyl groups.

[0063] Particularly preferred secondary aromatic amines according to the invention are those of the following group: 4,4'-Bis(α,α'-tert-octyl)diphenylamine 4,4'-Bis(α,α'-dimethylbenzyl)diphenylamine 4-(1,1,3,3-tetramethylbutyl)4'-triphenylmethyldiphenylamine 4,4'-Bis(α,α'-p-trimethylbenzyl)diphenylamine 2,4,4'-Tris(α,α'-p-trimethylbenzyl)diphenylamine 2,2'-Dibromo,4,4'-bis(α,α'-dimethylbenzyl)diphenylamine 4,4'-Bis(α,α-dimethylbenzyl)-2-carboxydiphenylamini-nickel-4,4'-bis(α,α-dimethylbenzyl)-diphenylamine 2-sec-Butyl-4,4'-bis(α,α-dimethylbenzyl)diphenylamine 4,4'-Bis(α,α-dimethylbenzyl)-2-(α-methylheptyl)diphenylamine 2-(α-Methylpentyl)4,4'-ditrityldiphenylamine 4-α,α-Dimethylbenzyl-4'-isopropoxydiphenylamine 2-(α-methylheptyl)-4'-(α,α-dimethylbenzyl)diphenylamine 2-(α-Methylpentyl)-4'-trityldiphenylamine 4,4'-Bis(tert-butyl)diphenylamine

[0064] [ka]

[0065] [ka]

[0066] [ka]

[0067] is selected from.

[0068] According to the invention, 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine [CAS number 10081-67-1] is very particularly preferably used as component b), which can be purchased, inter alia, from the company Rialon under the name Rianox® 445.

[0069] Constituent c) General formula (I)

[0070] [ka]

[0071] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10At least one phosphinic acid derivative of the formula (I) is used as component c).

[0072] When R in formula (I) represents a hydrogen atom, formula (I) is a hypophosphorous acid.When R in formula (I) represents an alkyl, cycloalkyl or aryl group, formula (I) is a phosphinic acid, the alkyl, cycloalkyl or aryl group preferably containing up to 12 carbon atoms.

[0073] When R in formula (I) represents an alkyl, cycloalkyl or aryl group, the salts and esters of phosphinic acid are preferably used.According to the present invention, the salts of phosphinic acid are preferably used, and these can also be hydrates of salt.Alkali metal salts and alkaline earth metal salts, as well as the salts of metals of group 12 or 13 of the periodic table of phosphinic acid are very particularly preferred, and these can also be hydrates of salt.

[0074] When R in formula (I) represents a hydrogen atom, formula (I) is hypophosphorous acid, and its salt or ester is preferably used. As the cation, alkali metal salt, alkaline earth metal salt, salt with ammonium ion, and hypophosphorous acid salt of metal of group 12 or 13 of the periodic table are particularly preferably used. The alkali metal salt of hypophosphorous acid is particularly preferably used, and these may also be salt hydrates.

[0075] Sodium hypophosphite [CAS number 7681-53-0] or sodium hypophosphite monohydrate [CAS number 10039-56-2] is very particularly preferably used as component c). Sodium hypophosphite and sodium hypophosphite monohydrate can be purchased commercially, inter alia, from the company Sigma Aldrich.

[0076] Component d) According to the invention, the organic phosphite of formula (III), bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite (Antioxidant 626), having the CAS number 26741-53-7, is used as component d).

[0077] [ka]

[0078] Component d) is commercially available, inter alia, under the trade name Ultranox® 626 from the company Brenntag.

[0079] Component e) Glass fibres are used as component e). With regard to glass fibres, the skilled artisan distinguishes between cut fibres, also called short fibres according to "http: / / de.wikipedia.org / wiki / Faser-Kunststoff-Verbund", having a length in the range of 0.1-1 mm, long fibres having a length in the range of 1-50 mm and endless fibres having a length L>50 mm. All length statements refer to the state before processing to form the composition, moulding compound or product according to the invention. Short fibres are preferably used in injection moulding techniques and can be processed directly using an extruder. Long fibres can also be processed in an extruder. They are used to a great extent in fibre spraying. Long fibres are often mixed into thermosetting plastics as fillers.

[0080] Endless fibers are used in fiber-reinforced plastics as rovings or fabrics. Products with endless fibers achieve the highest stiffness and strength values. Furthermore, crushed glass fibers are provided, the length of which after crushing is usually in the range of 70 to 200 μm.

[0081] The glass fibres preferably used according to the invention as component e) are cut-length glass fibres having an average starting length in the range from 1 to 50 mm, particularly preferably in the range from 1 to 10 mm and very particularly preferably in the range from 2 to 7 mm, determined by laser diffraction according to ISO 13320. The term starting length refers to the state of the glass fibres before any incorporation into components a), b), c) or d).

[0082] For laser diffraction particle size determination / laser diffraction method according to standard ISO13320, see https: / / de.wikipedia.org / wiki / Laserbeugungs-Partikelgr%C3%B6%C3%9Fenanalyse.

[0083] Preferred glass fibers used as component e) have an average fiber diameter, determined by laser diffraction according to ISO 13320, in the range from 7 to 18 μm, particularly preferably in the range from 9 to 15 μm.

[0084] The glass fibers used as component e) are in a preferred embodiment completed with a suitable slurry system or adhesion promoter or adhesion promoter system. Silane-based slurry systems or adhesion promoters are preferably used. Particularly preferred adhesion promoters based on silanes for the treatment of component e), in particular for the treatment of glass fibers, are those of the general formula (IV) (X-(CH2) q ) k -Si-(O-CrH 2r+1 ) 4-k (IV) (In the formula, X is NH2, carboxyl, HO or

[0085] [ka]

[0086] represents In formula (IV), q represents an integer of 2 to 10, preferably 3 to 4. In formula (IV), r represents an integer of 1 to 5, preferably 1 to 2. In the formula (IV), k represents an integer of 1 to 3, preferably 1.

[0087] Particularly preferred adhesion promoters are silane compounds from the group of aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane, aminobutyltriethoxysilane and the corresponding silanes which contain a glycidyl group or a carboxyl group as the substituent X, the carboxyl group being very particularly preferred.

[0088] For the finishing of glass fibres used as component e), adhesion promoters, preferably silane compounds according to formula (IV), are preferably used in an amount in the range of 0.05 to 2% by weight, particularly preferably in an amount in the range of 0.25 to 1.5% by weight, very particularly preferably in an amount in the range of 0.5 to 1% by weight, each based on 100% by weight of component e).

[0089] The glass fibres used as component e) may be shorter than the glass fibres originally used for processing to form the composition or the product in the composition or product. Thus, the arithmetic mean value of the glass fibre length after processing or in the polyamide-based product, determined by high-resolution X-ray computed tomography, is often still only in the range of 150 μm to 300 μm.

[0090] According to http: / / www.rg.de / wiki / Glasfasern, glass fibres are produced by melt spinning processes (nozzle drawing, bar drawing and nozzle blowing). In the nozzle drawing process, hot glass compound flows, by gravity, through hundreds of nozzle holes in a platinum spinning plate. The elementary threads can be drawn to unlimited lengths at speeds of 3-4 km / min.

[0091] A person skilled in the art distinguishes between various types of glass fibers, some of which are listed here, for example: E-glass (R&G E-glass), the most used material with the best price-performance ratio Reduced mass hollow glass fibre, H-glass (Hollow glass fibre fabric from R&G, 160g / m 2 and 216 g / m 2 ) Increased mechanical requirements for R,S glass (S2 glass from R&G) D-glass, a borosilicate glass with increased electrical requirements Increased chemical resistance of C-glass High temperature resistance, quartz glass

[0092] Further examples can be found at http: / / de.wikipedia.org / wiki / Glasfaser. E-glass fibres play a key role in strengthening plastics. The E stands for electric glass, as they were originally used, among other things, in the electrical industry.

[0093] For the production of E-glass, the glass melt is produced from pure quartz and the additives limestone, kaolin and boric acid. In addition to silicon dioxide, E-glass contains various metal oxides in different amounts. The composition determines the properties of the product. According to the invention, at least one type of glass fiber from the group of E-glass, H-glass, R,S-glass, D-glass, C-glass and quartz glass is preferably used, and particularly preferably glass fibers made from E-glass are used.

[0094] Glass fibre made from E-glass is the most widespread reinforcing material. Its strength properties correspond to those of metals (e.g. aluminium alloys) and the specific gravity of laminates containing E-glass fibre is less than that of metals. E-glass fibre is non-combustible, heat-resistant up to almost 400°C and resistant to most chemical and weathering influences.

[0095] Constituent f) In a preferred embodiment, at least one flame retardant is used as component f). Preferred flame retardants are various inorganic flame retardants, nitrogen-containing flame retardants, or phosphorus-containing flame retardants.

[0096] Among the inorganic flame retardants used as component f), magnesium hydroxide is particularly preferred. Magnesium hydroxide [CAS number 1309-42-8], due to its origin and production method, can be contaminated with impurities. Typical contaminants are, for example, species containing silicon, iron, calcium and / or aluminum, which can be intercalated, for example, in the form of oxides in magnesium hydroxide crystals. The magnesium hydroxide used as inorganic flame retardant can be either not slurried or otherwise provided in a slurry. The slurry promotes mechanical bonding between the plastic (matrix) and the components provided in the slurry in a manner that affects the quality. Preferably, the magnesium hydroxide preferably used as inorganic flame retardant is provided in a stearate or aminosiloxane-based slurry, particularly preferably aminosiloxane. Magnesium hydroxide preferably used as an inorganic flame retardant has an average particle size d50 in the range of 0.5 μm to 6 μm, determined by laser diffraction according to ISO 13320, preferably in the range of 0.7 μm to 3.8 μm, and particularly preferably in the range of 1.0 μm to 2.6 μm.

[0097] Preferred inorganic flame retardants according to the invention are of the magnesium hydroxide type, in particular Magnifin® H5IV from Martinswerk GmbH (Bergheim, Germany) or Hidromag® Q2015TC from Penoles (Mexico City, Mexico).

[0098] Preferred nitrogen-containing flame retardants for use as component e) are reaction products of trichlorotriazine, piperazine and morpholine according to CAS number 1078142-02-5, in particular MCA PPM Triazin HF from MCA Technologies GmbH (Biel-Benken, Switzerland), and also melamine cyanurate and condensation products of melamine, in particular melem, melam, melon or higher condensation compounds of this type. Preferred inorganic nitrogen-containing compounds are ammonium salts.

[0099] Furthermore, salts of aliphatic and aromatic sulfonic acids and also inorganic flame retardant additives, especially aluminium hydroxide or calcium magnesium carbonate hydrate (DE-A 4236122), can also be used.

[0100] Furthermore, flame retardant synergists from the group of the metal compounds containing oxygen, nitrogen or sulfur are considered for use as component f). Zinc-free compounds are preferred here, in particular molybdenum oxide, magnesium oxide, magnesium carbonate, calcium carbonate, calcium oxide, titanium nitride, magnesium nitride, calcium phosphate, calcium borate, magnesium borate or mixtures thereof.

[0101] However, in alternative embodiments, where necessary, zinc-containing compounds can also be used as component f), these preferably including zinc oxide, zinc borate, zinc stannate, zinc hydroxystannate, zinc sulfide and zinc nitride or mixtures thereof.

[0102] Preferred phosphorus-containing flame retardants to be used as component f) are organic metal phosphinates, aluminum salts of phosphonic acid, red phosphorus, inorganic metal hypophosphites, metal phosphonates, derivatives of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO derivatives), resorcinol-bis-(diphenylphosphate) (RDP) (including oligomers), bisphenol-A-bis-diphenylphosphate (BDP) (including oligomers), melamine pyrophosphate, melamine polyphosphate, melamine-poly(aluminum phosphate), melamine-poly(zinc phosphate) or phenoxyphosphazene oligomers and mixtures thereof.

[0103] One preferred organic metal phosphinate is aluminum tris(diethylphosphinate).One preferred inorganic metal hypophosphite is aluminum hypophosphite.

[0104] Further flame retardants used as component f) are carbon formers, particularly preferably phenol-formaldehyde resins, polycarbonates, polyimides, polysulfones, polyethersulfones or polyetherketones, and anti-drip agents, especially tetrafluoroethylene polymers.

[0105] The flame retardants used as component f) can be added in pure form and via masterbatches or compactates of component a).

[0106] However, in an alternative embodiment, halogenated flame retardants can also be used as flame retardants in component f), if such flame retardants are necessary in view of the disadvantages due to the loss of halogen-free. Preferred halogenated flame retardants are commercially available organic halogen compounds, particularly preferably ethylene-1,2-bistetrabromo-phthalimide, decabromodiphenylethane, tetrabromobisphenol-A-epoxy oligomer, tetrabromo-bisphenol-A-oligocarbonate, tetrachlorobisphenol-A-oligocarbonate, polypenta-bromobenzyl-acrylate, brominated polystyrene or brominated polyphenylene ether, which can be used alone or in combination with synergists, brominated polystyrene being particularly preferred among the halogenated flame retardants. Brominated polystyrene is preferably used here in an amount of 10 to 30% by weight, particularly preferably 15 to 25% by weight, each based on the entire composition, at least one of the other components being sufficiently reduced so that the sum of the total mass percentages is always 100.

[0107] However, in a further alternative embodiment, antimony trioxide and antimony pentoxide can also be used as flame retardant synergists, if necessary, and taking into account the disadvantages previously described with respect to hazard class H351.

[0108] Brominated polystyrene of various product qualities is commercially available, for example Firemaster® PBS64 from Lanxess, Cologne (Germany) and Saytex® HP-3010 from Albemarle, Baton (Rouge, USA).

[0109] Among the flame retardants used as component f), very particular preference is given to aluminium-tris(diethylphosphinate)][CAS number 225789-38-8] and combinations of aluminium-tris(diethylphosphinate) with melamine polyphosphate or combinations of aluminium-tris(diethylphosphinate) with at least one aluminium salt of phosphonic acid, especially combinations of aluminium-tris(diethylphosphinate) with at least one aluminium salt of phosphonic acid.

[0110] In the case of a combination of aluminum-tris(diethylphosphinate) with melamine polyphosphate or with at least one aluminum salt of phosphonic acid, the proportion of aluminum-tris(diethylphosphinate) is preferably in the range from 40 to 90 parts by weight, particularly preferably in the range from 50 to 80 parts by weight and very particularly preferably in the range from 60 to 70 parts by weight, in each case per 100 parts by weight of the combination of aluminum-tris(diethylphosphinate) with melamine polyphosphate or of the combination of aluminum-tris(diethylphosphinate) with at least one aluminum salt of phosphonic acid.

[0111] The aluminum tris(diethylphosphinate) particularly preferably used as component f) is known to those skilled in the art as Exolit® OP1230 or Exolit® OP1240 from Clariant International Ltd. (Muttenz, Switzerland). Melamine polyphosphates are commercially available in various product qualities. Examples of this are, for example, Melapur® 200 / 70 from BASF (Ludwigshafen, Germany) and Budit® 3141 from Budenheim (Budenheim, Germany).

[0112] Preferred aluminum salts of phosphonic acids to be used as component f) are selected from the following group: Aluminum primary phosphonate [Al(H2PO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Al2(HPO3)3·xAl2O3·nH2O (x is in the range of 2.27 to 1, and n is in the range of 0 to 4) Al2(HPO3)3·(H2O) of general formula (IV) q (q is in the range of 0 to 4), in particular aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O] or secondary aluminum phosphonate [Al2(HPO3)3] Al2M of general formula (V) z (HPO3) y (OH) v (H2O) w (M represents an alkali metal ion, z is in the range of 0.01 to 1.5, y is in the range of 2.63 to 3.5, v is in the range of 0 to 2, and w is in the range of 0 to 4), and Al2(HPO3) of general formula (VI) u (H2PO3) t (H2O) s (u is in the range of 2 to 2.99, t is in the range of 2 to 0.01, and s is in the range of 0 to 4) (In formula (V), z, y and v, and in formula (VI), u and t can only assume numbers such that the corresponding aluminum salt of phosphonic acid is totally uncharged).

[0113] Preferred alkali metals M in formula (V) are sodium and potassium.

[0114] The stated aluminum salts of phosphonic acids can be used here individually or in mixtures.

[0115] Aluminum salts of phosphonic acids which are particularly preferably used as component f) are selected from the following group: Aluminum primary phosphonate [Al(H2PO3)3] Aluminum phosphonate [Al2(HPO3)3] Basic aluminum phosphonate [Al(OH)H2PO3)2·2H2O] Aluminum phosphonate tetrahydrate [Al2(HPO3)3·4H2O] and Al2(HPO3)3·xAl2O3·nH2O (x is in the range of 2.27 to 1, and n is in the range of 0 to 4)

[0116] Aluminum secondary phosphonate Al2(HPO3)3 [CAS number 71449-76-8] and aluminum secondary phosphonate tetrahydrate Al2(HPO3)3·4H2O [CAS number 156024-71-4] are very particularly preferred, especially aluminum secondary phosphonate Al2(HPO3)3.

[0117] The production of the aluminum salts of phosphonic acids used according to the invention as component f) is described, for example, in WO2013 / 083247A1. The production is usually carried out by reacting an aluminum source, preferably aluminum isopropoxide, aluminum nitrate, aluminum chloride or aluminum hydroxide, with a phosphorus source, preferably phosphonic acid, ammonium phosphonate, alkali phosphonate, in a solvent with a template, optionally for a period of up to 4 days, at 20-200 ° C. For this purpose, the aluminum source and the phosphorus source are mixed and heated under hydrothermal conditions or under reflux, filtered, washed and dried. Preferred templates here are hexane-1,6-diamine, guanidine carbonate or ammonia. The preferred solvent is water.

[0118] Very particularly preferably, aluminum-tris(diethylphosphinate) is used, in particular as component f).Accordingly, compositions and reinforced polyamide-based products which, in addition to components a), b), c), d) and e), also contain at least 3 to 100 parts by weight, preferably 5 to 80 parts by weight, particularly preferably 10 to 50 parts by weight, of aluminum-tris(diethylphosphinate) (each based on 100 parts by weight of component a)) are particularly preferred according to the invention.

[0119] Constituent g) At least one further additive different from components b), c), d), e) and f) is used as component g).Preferred additives used as component g) are antioxidants, heat stabilizers, UV stabilizers, gamma radiation stabilizers, components for reducing water absorption or hydrolysis stabilizers, antistatic agents, emulsifiers, nucleating agents, softeners, processing aids, lubricants and / or release agents, components for reducing water absorption, anticaking agents, additives with chain-lengthening action, colorants, coloring agents, pigments or laser absorbers.The additives can be used alone or in mixtures or in the form of masterbatches.

[0120] Preferred heat stabilizers of component g) are sterically hindered phenols, in particular those containing at least one 2,6-di-tert-butylphenyl group and / or 2-tert-butyl-6-methylphenyl group, phosphites, hydroquinones, substituted resorcinols, salicylates, benzotriazoles and benzophenones, as well as differently substituted representatives of these groups, or mixtures thereof.

[0121] In one embodiment, copper salts can also be used as heat stabilizers. Copper (I) iodide [CAS number 7681-65-4] and / or (triphenylphosphino) copper iodide [CAS number 47107-74-4] are preferably used as copper salts.

[0122] The UV stabilizers used as component g) are preferably substituted resorcinols, salicylates, benzotriazoles and benzophenones, HALS derivatives containing at least one 2,2,6,6-tetramethyl-4-piperidyl unit ("hindered amine light stabilizers"), or benzophenones. The UV stabilizers used as component g) are preferably used in amounts of 0.01 to 2 parts by weight, particularly preferably 0.1 to 1 part by weight, each relative to 100 parts by weight of component a).

[0123] In one embodiment, as colorants used as component g), inorganic pigments are preferably used, particularly preferably ultramarine blue, bismuth vanadate [CAS number 14059-33-7], iron oxide [CAS number 1309-37-1], titanium dioxide [CAS number 13463-67-7 (rutile) or CAS number 1317-70-0 (anatase)], barium sulfate [CAS number 7727-43-7], zinc sulfide [CAS number 1314-98-3] or cerium-containing sulfides. A preferred sulfide-containing cerium is cerium(III) sulfide (Ce2S3), also known as CI Pigment Orange 75 [CAS number 12014-93-6], or cerium(III) sulfide / lanthanum(III) sulfide (Ce2S3 / La2S3), also known as CI Pigment Orange 78 [CAS number 12014-93-6; CAS number 12031-49-1]. Barium sulfate is particularly preferred. Titanium dioxide, also known as Pigment White 6 or CI 77891, is also particularly preferred.

[0124] The colorants used according to the invention as component g) are preferably also pigmentary systems based on inorganic mixed oxides containing titanium dioxide, tin oxide and zinc oxide. Pigmentary systems preferably used according to the invention as component g) based on inorganic mixed oxides containing titanium dioxide, tin oxide and zinc oxide are known from EP 0113229 B1, as is their preparation. The contents of EP 0113229 B1 are hereby incorporated in their entirety. According to EP 0113229 B1, the quantitative ratios of the tin, titanium, zinc and oxygen components in the pigmentary systems used according to the invention as component g) are represented by the general formula (VII) (TiO2) c SnO(ZnO) d (SnO) e (VII) (wherein c is in the range of 0.3 to 6.2, d is in the range of 0.04 to 6.2, and e is in the range of 0 to 7).

[0125] Preferably, the pigmentary systems of general formula (VII) used as component g) contain 300 to 6000 atomic parts of alkali metal residues per million parts of atoms of the overall complex or pigmentary system. Pigmentary systems used as component g) based on inorganic mixed oxides derived from titanium dioxide, tin oxide and zinc oxide can be used according to the invention either individually or in a mixture with at least one further inorganic mixed oxide from titanium dioxide, tin oxide and zinc oxide.

[0126] The pigment system of general formula (VII) with CAS number 923954-49-8 or CI Pigment Orange 82 [CAS number 2170864-77-2] or CI Pigment Yellow 216 [CAS number 817181-98-9] are particularly preferably used. For the CI classification, see https: / / de.wikipedia.org / wiki / Colour_Index. Pigment Orange 82 can be obtained, for example, under the name Sicopal® Orange K2430 from BASF SE (Ludwigshafen, Germany). Pigment Yellow 216 can be obtained, for example, under the name Orange 10P340 from Shepherd (Gent, Belgium).

[0127] In one embodiment, organic colorants are particularly preferred, particularly preferably phthalocyanines, quinacridones, benzimidazoles, in particular Ni-2-hydroxy-naphthyl-benzimidazole [CAS number 42844-93-9] and / or pyrimidine-azo-benzimidazole [CAS number 72102-84-2] and / or Pigment Yellow 192 [CAS number 56279-27-7], furthermore perylenes, anthraquinones, in particular CI Sorbent, Yellow 163 [CAS number 13676-91-0] and the phthaloperine series, in particular 10,10'-oxy-bis-12H-phthaloperin-12-one [CAS number 203576-97-0] and 12H-phthaloperin-12-one [CAS number 6925-69-5], are preferably used as further colorants used as component g), 10,10'-oxy-bis-12H-phthaloperin-12-one being particularly preferred.

[0128] In an alternative embodiment, carbon black or nigrosine can also be used as colorants in component g), if desired.

[0129] In a particularly preferred embodiment, the colorants according to the invention are used so that the color-stable impact-resistant polyamide-based products have an "orange" color, whereby in the RAL color system "similar" shades to those of the color numbers RAL2001, RAL2003, RAL2004, RAL2007, RAL2008, RAL2009, RAL2010 and RAL2011 are preferred, with such shades "similar" to the color numbers RAL2003, RAL2008 and RAL2011 being very particularly preferred. According to the invention, "orange" is understood as a shade "similar" to a shade of the RAL color chart color number starting with "2". By "similar" shade is meant here, according to the invention, L * a * b * A color tone in a system having a color difference of ΔE<20, preferably ΔE<10, particularly preferably ΔE<5, relative to the color of the RAL color chart. For an explanation of ΔE as defined in EN ISO11664-4, see, for example, https: / / de.wikipedia.org / wiki / Delta_E.

[0130] The nucleating agent used as component g) is preferably sodium or calcium phenylphosphinate, aluminum oxide, silicon dioxide or talc. Talc [CAS number 14807-96-6], in particular microcrystalline talc, is particularly preferably used as nucleating agent. Talc, also called talc, has the chemical composition Mg3[SiO 10(OH)2], which crystallizes, depending on the modification, as talc-1A in the triclinic system or as talc-2M in the monoclinic crystal system (http: / / de.wikipedia.org / wiki / Talkum). The talc used according to the invention can be obtained, for example, as Mistron® R10 from Imerys Talc Group (Toulouse, France) (Rio Tinto Group).

[0131] Copolymers of at least one α-olefin and at least one methacrylic or acrylic ester of an aliphatic alcohol are preferably used as anticaking agents, which are used as component g). Copolymers are particularly preferred here, in which the α-olefin is synthesized from ethene and / or propene, and the methacrylic or acrylic ester contains, as the alcohol component, a linear or branched alkyl group having 6 to 20 carbon atoms. Acrylic acid 2-ethylhexyl ester is very particularly preferred. Besides the composition, copolymers suitable as anticaking agents are also distinguished by low molecular weight. Thus, in particular, copolymers are suitable for the polymer composition according to the invention, which have an MFI value of at least 100 g / 10 min, preferably at least 150 g / 10 min, particularly preferably at least 300 g / 10 min, measured at 190 ° C and a load of 2.16 kg. The melt flow index MFI is used to characterize the flow of the melt of thermoplastics and is subject to the standards ISO 1133 or ASTM D1238. A copolymer of ethene and 2-ethylhexyl acrylic acid, having an MFI of 550, known as Lotryl® 37EH550, is particularly preferably used as an anti-sticking agent.

[0132] Preferably, bi- or polyfunctional additives with branching or chain-extending action are used as chain-extending additives used as component g) and contain at least two functional groups with branching or chain-extending action per molecule. Low molecular weight or oligomeric compounds are preferred as branching or chain-extending additives, which have at least two functional groups with chain-extending action per molecule and can react with primary and / or secondary amino groups and / or amide groups and / or carboxylic acid groups. The functional groups with chain-extending action are preferably isocyanates, alcohols, blocked isocyanates, epoxides, maleic anhydrides, oxazolines, oxazines, oxazolones, preferably epoxides.

[0133] Particularly preferred bi- or polyfunctional additives with branching or chain extension action are diepoxides based on diglycidyl ethers (bisphenols and epichlorohydrin), based on aminoepoxide resins (aniline and epichlorohydrin), based on diglycidyl esters (cycloaliphatic dicarboxylic acids and epichlorohydrin), either individually or in mixtures, and 2,2-bis[p-hydroxyphenyl]propane diglycidyl ether, bis[p-(N-methyl-N-2,3-epoxypropylamino)phenyl]methane, and epoxidized aliphatic esters of glycerin containing at least two epoxide groups per molecule.

[0134] Particularly preferred di- or polyfunctional additives with branching or chain-extending action are glycidyl ethers, very particularly preferably bisphenol A-diglycidyl ether [CAS number 98460-24-3] or epoxidized fatty acid esters of glycerin, and also very particularly preferably epoxidized soybean oil [CAS number 8013-07-8] and / or epoxidized linseed oil.

[0135] Softeners which are preferably used as component g) are dioctyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, hydrocarbon oils or N-(n-butyl)benzenesulfonamide.

[0136] The lubricants and / or release agents used as component g) are preferably long-chain fatty acids, in particular stearic acid or behenic acid, their salts, in particular calcium stearate or zinc stearate, and their ester derivatives, in particular those based on pentaerythritol, in particular fatty acid ester or amide derivatives of pentaerythritol, in particular ethylene-bis-stearylamide, montan wax, and low molecular weight polyethylene waxes or polypropylene waxes.

[0137] Montan wax within the meaning of the present invention is a mixture of linear saturated carboxylic acids having a chain length ranging from 28 to 32 carbon atoms.

[0138] According to the invention, lubricants and / or release agents from the group of esters of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms with saturated aliphatic alcohols or amides of amines having 2 to 40 carbon atoms with unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms (or in each case, instead of the carboxylic acid, metal salts of saturated or unsaturated aliphatic carboxylic acids having 8 to 40 carbon atoms) are particularly preferably used.

[0139] The lubricants and / or release agents very particularly preferably used as component g) are selected from the group of pentaerythritol tetrastearate [CAS number 115-83-3], ethylene-bis-stearylamide, calcium stearate, zinc stearate and ethylene glycol dimontanate. Zinc stearate [CAS number 557-05-1], calcium stearate [CAS number 1592-23-0] or ethylene-bis-stearylamide [CAS number 110-30-5] are particularly preferably used. In particular, ethylene-bis-stearylamide (Loxiol® EBS from Emery Oleochemicals) is particularly preferably used.

[0140] Laser absorbers preferably used as component f) are selected from the group of tin oxide, tin orthophosphate, barium titanate, aluminum oxide, copper hydroxyphosphate, copper orthophosphate, potassium copper diphosphate, copper hydroxide, bismuth trioxide, mica doped with tin oxide and / or antimony oxide, and anthraquinone. Tin oxide is particularly preferred.

[0141] In an alternative embodiment, where the disadvantages previously described for hazard class H351 need to be considered, antimony tin oxide, antimony trioxide or antimony pentoxide may instead also be used as the laser absorber.

[0142] The laser absorber can be used directly as powder or in the form of a masterbatch. Preferred masterbatches are based on polyamides and / or polyolefins, preferably polyethylene. The laser absorber is very particularly preferably used in the form of a polyamide 6-based masterbatch.

[0143] Laser absorbers can be used individually or as a mixture of multiple laser absorbers. Laser absorbers can absorb laser light of a specific wavelength. In practice, this wavelength is in the range of 157 nm to 10.6 μm. Examples of lasers of these wavelengths are described in WO2009 / 003976A1. Preferably, Nd:YAG lasers using any of the wavelengths of 1064, 532, 355 and 266 nm can be implemented, and CO2 lasers are used.

[0144] Particularly preferred compositions / products The present invention relates to a) Polyamide 6 or Polyamide 66 b) 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine c) Sodium hypophosphite or sodium hypophosphite monohydrate d) bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate, and e) Glass fiber Including, However, for 100 parts by mass of component a), 0.1 to 3 parts by weight, preferably 0.3 to 2 parts by weight, particularly preferably 0.35 to 1.5 parts by weight of component b) 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of component c) 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of component d), and It particularly relates to compositions and / or products, provided that from 5 to 200 parts by weight, preferably from 15 to 160 parts by weight, particularly preferably from 30 to 150 parts by weight, of component e) are used.

[0145] Preferred Use The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2The present invention preferably relates to the use of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate for producing glass-fiber-reinforced polyamide-based products having a low color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A at 100 °C for 200 hours and / or retention of impact resistance measured according to ISO 180-1U and / or elongation at break measured according to ISO 527 after hot air aging at 150 °C for 500 hours.

[0146] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 Particularly preferred is the use of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate for producing glass-fiber-reinforced polyamide-based products having a low color change ΔE calculated in accordance with DIN EN ISO 11664-4 after UV storage in accordance with DIN ISO 4892-2A at 100 °C for 200 hours and / or a low impact resistance, measured in accordance with ISO 180-1U, and / or retention of the breaking elongation, measured in accordance with ISO 527, after hot air aging in accordance with 150 °C for 500 hours, with the proviso that 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate are used per 100 parts by weight of polyamide, in particular polyamide 6 or polyamide 66, and 5 to 200 parts by weight, preferably 15 to 160 parts by weight, particularly preferably 30 to 150 parts by weight of glass fibers.

[0147] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2The present invention preferably relates to the use of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate in combination with at least one aromatic amine for producing glass fiber reinforced polyamide based products having a small color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A for 200 hours at 150° C. and / or impact resistance measured according to ISO 180-1U and / or retention of breaking elongation measured according to ISO 527 after hot air aging for 500 hours at 150° C. Preferably, 4,4′-bis(α,α′-dimethylbenzyl)diphenylamine is used as aromatic amine.

[0148] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 Very particularly preferably relates to the use of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate in combination with at least one aromatic amine for producing polyamide-based products having a low color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A at 100 °C for 200 hours and / or impact resistance measured according to ISO 180-1U and / or retention of elongation at break measured according to ISO 527 after hot air aging at 150 °C for 500 hours, with the proviso that 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate are used per 100 parts by weight of polyamide, in particular polyamide 6 or polyamide 66, and 5 to 200 parts by weight, preferably 15 to 160 parts by weight and particularly preferably 30 to 150 parts by weight of glass fibres. Preferably, 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine is used as the aromatic amine.

[0149] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 2. The process for producing a glass-fiber-reinforced polyamide-based product, which has a low color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A at 100° C. for 200 hours and / or a low impact resistance measured according to ISO 180-1U and / or a low retention of the elongation at break measured according to ISO 527 after hot air aging at 150° C. for 500 hours, the low color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A ...

[0150] [ka]

[0151] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10 At least one phosphinic acid derivative of Preferably, 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine is used as the aromatic amine and sodium hypophosphite or sodium hypophosphite monohydrate is used as the phosphinic acid derivative.

[0152] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 22. The process for producing a polyamide-based product, comprising at least one aromatic amine and a carboxylic acid derivative of the general formula (I)

[0153] [ka]

[0154] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10 At least one phosphinic acid derivative of Very particular preference is given to the use of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate in combination with 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate per 100 parts by weight of polyamide, in particular polyamide 6 or polyamide 66. 5 to 200 parts by mass, preferably 15 to 160 parts by mass, particularly preferably 30 to 150 parts by mass of glass fibers 0.1 to 3 parts by mass, preferably 0.3 to 2 parts by mass, particularly preferably 0.35 to 1.5 parts by mass of an aromatic amine, in particular 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine, and Provided that 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of a phosphinic acid derivative, in particular sodium hypophosphite or sodium hypophosphite monohydrate, is used.

[0155] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 Very particularly preferably relates to the use of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate in combination with 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine and sodium hypophosphite or sodium hypophosphite monohydrate for producing glass-fiber-reinforced polyamide-based products which have a small color change ΔE calculated in accordance with DIN EN ISO 11664-4 after UV storage in accordance with DIN ISO 4892-2A at 100 °C for 200 hours and / or retention of impact resistance, measured in accordance with ISO 180-1U, and / or retention of elongation at break, measured in accordance with ISO 527, after hot air aging in 500 hours at 150 °C.

[0156] The invention is characterized by a small color change ΔE calculated according to DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. and / or a color change ΔE of 1.55 W / m 2 at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain. 2 Very particularly preferably relates to the use of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate in combination with 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine and sodium hypophosphite or sodium hypophosphite monohydrate for producing glass-fiber-reinforced polyamide-based products having a small color change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A for 200 hours at 150° C. and / or retention of impact resistance measured according to ISO 180-1U and / or elongation at break measured according to ISO 527 after hot air aging for 500 hours at 150° C., with the proviso that 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate per 100 parts by weight of polyamide 6 or polyamide 66 5 to 200 parts by mass, preferably 15 to 160 parts by mass, particularly preferably 30 to 150 parts by mass of glass fibers 0.1 to 3 parts by mass, preferably 0.3 to 2 parts by mass, particularly preferably 0.35 to 1.5 parts by mass of 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine, The condition is that 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, and particularly preferably 0.1 to 1.7 parts by mass of sodium hypophosphite or sodium hypophosphite monohydrate is used.

[0157] For the sake of clarity, it is noted that the use according to the invention also encompasses all definitions and parameters listed for the composition and / or polyamide-based product as well as generally stated or in any combination of preferred ranges.

[0158] Particularly preferred methods The present invention relates to a glass fiber reinforced polyamide based product, b) 0.1 to 3 parts by mass, preferably 0.3 to 2 parts by mass, particularly preferably 0.35 to 1.5 parts by mass of at least one secondary aromatic amine, and c) 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of the compound of formula (I)

[0159] [ka]

[0160] (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of Group 12 or 13 of the Periodic Table of the Elements, an ammonium ion, or a C1 to C6 10 At least one phosphinic acid derivative of d) 0.01 to 3 parts by mass, preferably 0.05 to 1 part by mass of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate When the mixture containing the above is used for 100 parts by mass of polyamide 6 or polyamide 66 and 5 to 200 parts by mass, preferably 15 to 160 parts by mass, particularly preferably 30 to 150 parts by mass of glass fibers, To reduce the color change ΔE calculated according to DIN EN ISO 11664-4 over 500 hours at 150°C and / or at 80°C, 340 nm and 1.55 W / m2 in the absence of rain 2 and / or for retaining the impact resistance determined according to ISO 180-1U and / or for retaining the elongation at break determined according to ISO 527 after hot air aging at 140° C. for 500 hours.

[0161] Ammonium ion NH4 for R' in formula (I) + is also a cation, which in the process according to the invention forms salts with anions, as well as with alkali metal ions. The ammonium ion is the conjugate acid of the basic ammonia (NH3).

[0162] When R in formula (I) represents a hydrogen atom, formula (I) is a hypophosphorous acid, and when R represents an alkyl, cycloalkyl or aryl group, formula (I) is a phosphinic acid, the alkyl, cycloalkyl or aryl group preferably containing up to 12 carbon atoms.

[0163] When R in formula (I) represents alkyl, cycloalkyl or aryl group, the salts and esters of phosphinic acid are preferably used.The salts of phosphinic acid are preferably used, and these may also be hydrates of salt.Alkali metal salts and alkaline earth metal salts, and the salts of metals of group 12 and group 13 of the periodic table of phosphinic acid are very particularly preferred, and these may also be hydrates of salt.

[0164] When R in formula (I) is hydrogen atom, formula (I) is hypophosphorous acid.Preferably use hypophosphorous acid salts and esters.Particularly preferably use alkali metal salts and alkaline earth metal salts, and hypophosphorous acid salts of metals of group 12 and group 13 of periodic table.Particularly preferably use alkali metal salts of hypophosphorous acid, which may also be salt hydrates.

[0165] Good ageing behavior in the case of the method according to the invention in the form of improved color retention after hot air ageing or improved color stability should also be understood to mean that the resulting color difference ΔE calculated in accordance with DIN EN ISO 11664-4 after 500 hours of hot air storage at 150° C. is small, preferably a color difference ΔE in the range from 0 to 20, particularly preferably a color difference ΔE in the range from 0 to 15. Good ageing behavior in the form of improved UV stability is, in the case of the method according to the invention, in the absence of rain at 80° C., 340 nm and 1.55 W / m 2 This is understood to mean that the color difference ΔE calculated in accordance with DIN EN ISO 11664-4 after UV storage in accordance with DIN ISO 4892-2A at 400 °C for 200 hours is small, preferably a color difference ΔE in the range from 0 to 30, particularly preferably a color difference ΔE in the range from 0 to 20.

[0166] Good ageing behavior in the form of sufficient retention of impact resistance after hot air ageing is understood in the case of the method according to the invention to mean that the impact resistance of the sample measured in accordance with ISO 180-1U after 500 hours of hot air ageing at 150° C. does not decrease by more than 50% compared to the time at 0 hours.

[0167] Good aging behavior in the form of sufficient retention of the breaking elongation after hot air aging is understood in the case of the method according to the invention to mean that the breaking elongation, measured according to DIN EN ISO 527 after 500 hours of hot air aging at 150° C., does not decrease by more than 30% compared to the time at 0 hours.

[0168] Finally, the present invention relates to a glass fiber reinforced polyamide based product, b) 0.1 to 3 parts by mass, preferably 0.3 to 2 parts by mass, and particularly preferably 0.35 to 1.5 parts by mass of 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine c) 0.01 to 3 parts by mass, preferably 0.05 to 2 parts by mass, particularly preferably 0.1 to 1.7 parts by mass of sodium hypophosphite or sodium hypophosphite monohydrate, and d) 0.01 to 3 parts by mass, preferably 0.05 to 1 part by mass of bis(2,4-di-t-butylphenyl)pentaerythritol diphosphate When the mixture containing the above is used for 100 parts by mass of polyamide 6 or polyamide 66 and 5 to 200 parts by mass, preferably 15 to 160 parts by mass, particularly preferably 30 to 150 parts by mass of glass fibers, To reduce the color change ΔE calculated according to DIN EN ISO 11664-4 over 500 hours at 150°C and / or at 80°C, 340 nm and 1.55 W / m2 in the absence of rain 2 Particularly preferably, the process relates to a method for reducing the color change ΔE calculated according to DIN EN ISO 11664-4 after UV irradiation according to DIN ISO 4892-2A at 100 °C for 200 h and / or for retaining the impact resistance determined according to ISO 180-1U and / or for retaining the elongation at break determined according to ISO 527 after hot air aging at 150 °C for 500 h.

[0169] For clarity, the method according to the invention also encompasses all definitions and parameters listed for the compositions and polyamide-based products and generally stated or in any combination of preferred ranges.

[0170] The subject of the present application is also the use or processing of the molding compounds produced from the components used according to the invention in extrusion processes, blow molding processes or injection molding to produce products, preferably molded parts or semi-finished products, in particular by injection molding.

[0171] The processing method according to the invention for producing products by extrusion, blow moulding or injection moulding is carried out at melt temperatures in the range from 230 to 330° C., preferably from 250 to 300° C., and optionally also at a pressure of at most 2500 bar, preferably at most 2000 bar, particularly preferably at most 1500 bar, very particularly preferably at most 750 bar.

[0172] In extrusion, also called extrusion molding, a solid to viscous curable thermoplastic molding compound is continuously forced under pressure through a molding orifice, preferably called a nozzle, die or mouthpiece. The product with the cross section of the orifice can here theoretically be of any length (http: / / de.wikipedia.org / wiki / Extrusion_(Verfahrenstechnik). The basic process steps of the profile extrusion process, which is a process form of extrusion, are: 1. Providing a plastic melt by plasticizing it in an extruder; 2. Extruding a thermoplastic molten strand from a calibrated sleeve having a cross section of the shape to be extruded. 3. The process of cooling the extruded profile on the calibration table 4. A process of further moving irregular parts using a draw-off after the calibration table 5. A process of cutting the endless irregular product to a predetermined length in a cutting facility; 6. A process of collecting irregularly shaped products cut to a specified length on a collection table It is.

[0173] Profile extrusion of polyamide 6 and polyamide 66 is described in Kunststoff-Handbuch 3 / 4, Polyamide [Plastic handbook 3 / 4, Polyamides], Carl Hanser Verlag, Munich 1998, pages 374-384.

[0174] The method of blow molding is described, for example, at http: / / www.blasformen.com / . In blow molding, in a first process step, the granular plastic is drawn in, compressed, degassed, heated, plasticized and homogenized by a heated extruder to form a plasticized plastic strand. In a next step, the plastic compound is led to the flanged tube head of the extruder. There, the plastic melt is formed into a tube and emerges vertically downwards from the nozzle. The diameter of the tube is adapted to the article to be produced using a standard mandrel and nozzles of various sizes, which are flanged to the tube head. The tube thickness of the blow molded part and the resulting mass are predetermined by selecting the various diameter differences from the mandrel to the nozzle.

[0175] Injection molding is distinguished in that the raw materials, i.e. the thermoplastic molding compound to be processed, which contains the components used according to the invention, are melted (plasticized), preferably in the form of granules, in a heated cylindrical cavity and are injected under pressure into a temperature-controlled cavity as an injection compound. After cooling (solidification) of this compound, the injection-molded part is removed from the mold.

[0176] A distinction is made between: 1.Plastification / Melting 2. Injection phase (filling process) 3. Pressure holding period (due to thermal contraction during crystallization) 4. Demolding

[0177] The injection molding machine consists of a closing unit, an injection unit, a drive and a control unit. The closing unit includes fixed and movable clamping plates, end plates and columns for the tool, and a drive (toggle joint or hydraulic closing unit) for the movable tool clamping plate.

[0178] The injection unit comprises an electrically heatable cylinder, a drive for the shaft (motor, gears) and a hydraulic system for moving the shaft and the injection unit. The role of the injection unit is to melt, meter, inject and apply holding pressure (for shrinkage) for the powder or granules. The problem of backflow of the melt in the shaft (leakage flow) is solved by an anti-backflow wall.

[0179] In the injection molding tool, the inflow melt of the molding compound to be processed, which contains the components used according to the invention, is melted and cooled, thus producing the part to be produced. For this purpose, at least two tool halves are always required. In injection molding, the following functional composite equipment is distinguished: - Gate System - Molded inserts - exhaust - Mechanical and power adjustment - Demolding system and transfer - Temperature control

[0180] In contrast to injection moulding, in extrusion moulding, an endless moulded strand made from the moulding compound used according to the invention is used in an extruder, which is a machine for producing products based on thermoplastic moulded parts. A distinction is made between single-screw and twin-screw extruders and the respective subgroups conventional single-screw extruders, active conveyor single-screw extruders, counter-rotating twin-screw extruders and synchronous twin-screw extruders.

[0181] Extrusion equipment for producing profiles consists of an extruder, profile tooling, calibration, cooling lines, draw-off caterpillars and rollers, cutting equipment, and a tipping trough.

[0182] The present invention therefore also relates to a product, preferably a molded part, a molded body or a semi-finished product, obtainable by extrusion or injection molding of a molding compound according to the invention, which contains at least the components a), b), c), d) and e), and optionally f) and optionally g).

[0183] The preparation of the composition used according to the invention for the production of molding compounds used for injection molding, extrusion molding or blow molding is carried out by mixing the individual components a), b), c), d) and e), and optionally further components, in at least one mixing assembly, preferably a compounder, particularly preferably a twin-screw extruder rotating in the same direction. This mixing process, also called compounding, gives as intermediate product a molding compound, which is in the form of powder, granules or in the form of strands for further processing. These molding compounds, also called thermoplastic molding compounds, can either be exclusively composed of components a), b), c), d) and e), or can optionally contain further components, preferably f) and / or g).

[0184] Finally, the present invention also relates to the use of products, preferably molded parts, molded bodies or semi-finished products, produced by extrusion or injection molding from molding compounds containing at least components a), b), c), d) and e), and optionally f) and optionally g), for electrical or electronic components. These products according to the invention can be preferably used in the automotive, electrical, electronic, telecommunications, solar, information technology and computer industries, in the home, in sports, in medicine or in the entertainment industry. In particular, the products according to the invention can be used in applications where long-term color stability is required. The use of molded parts in electrical engineering and vehicles is preferred for such applications, especially high-voltage parts in vehicles, especially in automobiles. EXAMPLES

[0185] To embody the property improvements described by the present invention, firstly corresponding polyamide-based polymer compositions were produced by compounding. For this purpose, the individual components were mixed in a twin-screw extruder (ZSK26 compounder from Coperion Werner & Pfleiderer, Stuttgart, Germany) at a temperature in the range of 270-300° C., discharged as strands, cooled until the strands could be granulated, and granulated. After drying (typically 2 days at 80° C. in a vacuum drying cabinet), the granules were processed at a temperature in the range of 270-290° C. to form standard test specimens for the individual tests.

[0186] The impact resistance according to ISO 180-1U (Izod) and the elongation at break according to ISO 527 were determined at 23°C on injection-molded test specimens as specified by DIN EN ISO 1874-2 in the freshly injected condition. The freshly molded condition, also "dry as molded", is specified in DIN EN ISO 1874-2.

[0187] Lab color space (also known as CIELAB, CIEL * a * b * The Lab color space (Lab color) describes all perceptible colors. The Lab color space uses a three-dimensional color space in which the luminance value L is perpendicular to the color plane (a,b). * The axis describes the brightness (luminance) of the color, with values ​​from 0 to 100. In the example shown, this is * b * All achromatic colors (grayscale) lie at the black end point (L * =0) and the white end point (L * = 100), so L *The a-axis may also be referred to as the neutral gray axis. Similar to Ewald Hering's complementary color theory, the a-coordinate specifies the color type and color intensity between green and red, and the b-coordinate specifies the color type and color intensity between blue and yellow. The more positive the values ​​of a and b, and the less negative the values ​​of a and b, the stronger the color tone. For a=0 and b=0, there is an achromatic color tone on the lightness axis. In a typical software implementation, L can be considered as a value between 0 and 100, and a and b can vary between -128 and 127. Discoloration of polymer-based products due to oxidative damage of the polymer matrix was determined in the scope of the present invention by measuring the color difference ΔE over storage time at high temperatures. The color difference ΔE between two color stimuli is calculated according to the formula ΔE=[(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2 was calculated according to

[0188] In the scope of the present invention, the ageing behavior in the form of improved color retention or improved color stability was tested by storing injection-molded polyamide-based slabs of 60 mm·40 mm·4 mm in a material testing cabinet of the binder FP115 model with circulating air at a temperature of 150° C., also referred to as hot air ageing in the scope of the present invention. As a measure of discoloration, the color difference ΔE of injection-molded products based on the composition according to the invention after 500 hours of hot air ageing was calculated as the color value L * a * b * The thermal expansion coefficient was determined before and after hot air aging by measuring ΔE = [(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2

[0189] Thus, according to the invention, the good aging behavior in the form of improved color retention or improved color stability after hot air aging is distinguished by the fact that the color change ΔE in the case of the product according to the invention is smaller than in the case of the product according to the comparative example. * a * b * was determined in the scope of the present invention on slabs with dimensions 60 mm·40 mm·4 mm and the color difference ΔE was then calculated in accordance with DIN EN ISO 11664-4. The color measurements were carried out here using a spectrophotometer CM-2600d from Konica Minolta, using CIE standard illuminant type D65, in reflection (observer angle 10°) with gloss excluded (SCE=specular light excluded).

[0190] In the scope of the present invention, the test of the ageing behavior on products based on compositions according to the invention in a UV-stabilized form is carried out at 80° C., 340 nm and 1.55 W / m 2 in the absence of rain, hereafter referred to as UV storage. 2 The test was carried out by storing injection-molded slabs with dimensions 60 mm·40 mm·4 mm in a QUV fast weathering tester from Q-Lab in accordance with DIN ISO 4892-2A at 200 °C for 200 h. As a measure of discoloration, in the context of the present invention, the color difference ΔE of an injection-molded product based on a composition according to the invention is calculated by dividing the color difference ΔE by the color value L * a * b * was determined before and after 200 hours of UV storage by measuring ΔE = [(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2

[0191] Thus, according to the invention, the good aging behavior in the form of improved UV stability after UV storage is distinguished by the fact that the color change ΔE in the case of the product according to the invention is smaller compared to the product without component d). Color value L of the test specimen * a *b * was determined in the context of the present invention on slabs with dimensions 60 mm·40 mm·4 mm and then the color difference ΔE was calculated in accordance with DIN EN ISO 11664-4.

[0192] In the context of the present invention, tests of the aging behavior in the form of impact resistance and elongation at break were carried out by storing injection-molded test specimens as specified in accordance with DIN EN ISO 1874-2 in a materials testing cabinet of the model binder FP115 with circulating air at a temperature of 150° C. The impact resistance was determined in accordance with ISO 180-1U and the elongation at break at 23° C. in accordance with ISO 527 for these test specimens before and after storage for 500 hours at 150° C.

[0193] Extract: Component a) Polyamide 6 (Durethan® B29, Lanxess Deutschland GmbH) Component b) 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, CAS number 10081-67-1 (Rianox® 445, manufactured by Rialon Cooperation) Component c) Anhydrous sodium hypophosphite CAS number 7681-53-0 (Sigma Aldrich, ultra-high purity) Component d) Ultranox® 626A, CAS number 26741-53-7 (Brenntag) Component e) Glass fiber (CS7928, Lanxess Deutschland GmbH)

[0194] [Table 1]

[0195] The results in Table 1 show that the product based on the composition according to the invention according to Example 1 has a higher optical density at 80° C., 340 nm and 1.55 W / m compared to Comparative Example 1, in which component d) was not used. 2It is shown that after 200 hours of weathering at 1000 rpm, the coating surprisingly had higher UV stability in the form of lower color change ΔE, with ΔE values ​​in the range of <20. In the context of the present invention, a smaller ΔE value means a smaller color change. If the color does not change at all after storage, ΔE=0 would be the result.

[0196] Furthermore, in the case of Example 1, an improvement in the aging behavior was surprisingly shown in the form of improved color retention or improved color stability with ΔE between ΔE=0 and 15 after 500 hours of hot air aging at 150° C. compared to Comparative Example 1 not containing component d). At the same time, the impact resistance and retention of elongation at break after 500 hours of hot air aging at 150° C. were improved compared to Comparative Example 1 not containing component d). The improvements mentioned in Example 1 also apply in comparison to Comparative Example 2 in which none of components b), c), d) and e) was used.

Claims

1. a) at least one polyamide b) at least one secondary aromatic amine c) General formula (I) 【Chemistry 1】 (wherein R represents a hydrogen atom, or an alkyl, cycloalkyl or aryl group; R' is an alkali metal, an alkaline earth metal, a metal of Groups 12 and 13 of the Periodic Table of the Elements, an ammonium ion, or C 1 ~C 10 At least one phosphinic acid derivative of d) bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, and e) Glass fiber A composition and / or product comprising: However, for 100 parts by mass of component a), 0.1 to 3 parts by weight of component b) 0.01 to 3 parts by weight of component c) 0.01 to 3 parts by weight of component d), and 5 to 200 parts by weight of component e) are used The composition and / or product provided herein is

2. 2. Compositions and / or products according to claim 1, characterized in that polyamide 6, polyamide 6.6, polyamide 4.6 and / or partially aromatic copolyamides are used as component a).

3. 3. The composition and / or product according to claim 1 or 2, characterized in that in addition to components a), b), c), d) and e), as component f) at least one flame retardant is used in an amount of 3 to 100 parts by weight, preferably 5 to 80 parts by weight, particularly preferably 10 to 50 parts by weight, each for 100 parts by weight of component a).

4. General formula (II) 【Chemistry 2】 (In the formula, m and n each independently represent 0 or 1; A and B are each independently of each other, C 1 ~C 4 represents a tertiary C atom substituted by alkyl or phenyl, R 1 and R 2 each independently of the other is hydrogen, C in the ortho and para positions which may be optionally substituted by 1 to 3 phenyl groups; 1 ~C 6 represents an alkyl group, or a halogen, a carboxyl, or a metal salt of this carboxyl group, R 3 and R 4 each independently of the other represents hydrogen or a methyl radical in the ortho- and para-positions, or a tertiary C substituted in the ortho- or para-positions, which may be optionally substituted by one to three phenyl groups; 3 ~C 9 -alkyl) 4. Compositions and / or products according to claim 1 , characterized in that as component b) is used.

5. The secondary aromatic amine used as component b) is selected from the group 4,4'-Bis(α,α'-tert-octyl)diphenylamine 4,4'-Bis(α,α'-dimethylbenzyl)diphenylamine 4-(1,1,3,3-tetramethylbutyl)4'-triphenylmethyldiphenylamine 4,4'-Bis(α,α'-p-trimethylbenzyl)diphenylamine 2,4,4'-Tris(α,α'-p-trimethylbenzyl)diphenylamine 2,2'-Dibromo,4,4'-bis(α,α'-dimethylbenzyl)diphenylamine 4,4'-Bis(α,α-dimethylbenzyl)-2-carboxydiphenylamine-nickel-4,4'-bis(α,α-dimethylbenzyl)-diphenylamine 2-sec-Butyl-4,4'-bis(α,α-dimethylbenzyl)diphenylamine 4,4'-Bis(α,α-dimethylbenzyl)-2-(α-methylheptyl)diphenylamine 2-(α-Methylpentyl)4,4'-ditrityldiphenylamine 4-α,α-Dimethylbenzyl-4'-isopropoxydiphenylamine 2-(α-methylheptyl)-4'-(α,α-dimethylbenzyl)diphenylamine 2-(α-Methylpentyl)-4'-trityldiphenylamine 4,4'-Bis(tert-butyl)diphenylamine 【Chemistry 3A】 【Chemistry 3B】 【Chemistry 3C】 4. Compositions and / or products according to any one or more of claims 1 to 3, characterized in that they are selected from:

6. 4. Composition and / or product according to claim 1, characterized in that 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine is used as component b).

7. 7. Compositions and / or products according to claim 1 , characterized in that salts of phosphinic acids are used as component c), which may also be hydrates of the salts.

8. 7. Compositions and / or products according to claim 1 , characterized in that alkali metal and alkaline earth metal salts and salts of metals of group 12 or 13 of the periodic table of phosphinic acids are used as component c), which may also be salt hydrates.

9. 7. Composition and / or product according to any one or more of the preceding claims, characterized in that sodium hypophosphite or sodium hypophosphite monohydrate is used as component c).

10. a) Polyamide 6 or Polyamide 66 b) 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine c) Sodium hypophosphite or sodium hypophosphite monohydrate d) bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, and e) Glass fiber Including, However, for 100 parts by mass of component a), 0.1 to 3 parts by weight, preferably 0.3 to 2 parts by weight, particularly preferably 0.35 to 1.5 parts by weight of component b) 0.01 to 3 parts by weight, preferably 0.05 to 2 parts by weight, particularly preferably 0.1 to 1.7 parts by weight of component c) 0.01 to 3 parts by weight, preferably 0.05 to 1 part by weight, of component d), and Compositions and / or products according to one or more of the preceding claims, characterized in that from 5 to 200 parts by weight, preferably from 15 to 160 parts by weight, particularly preferably from 30 to 150 parts by weight, of component e) are used.

11. Small color change ΔE calculated according to DIN EN ISO11664-4 after 500 hours of hot air storage at 150°C and / or at 80°C, 340 nm and 1.55 W / m2 in the absence of rain 2 for producing glass fibre reinforced polyamide based products having a small colour change ΔE calculated according to DIN EN ISO 11664-4 after UV storage according to DIN ISO 4892-2A for 200 hours at 150° C. and / or a retention of impact resistance measured according to ISO 180-1U and / or a retention of elongation at break measured according to ISO 527 after hot air aging for 500 hours at 150° C. b) at least one secondary aromatic amine, and c) General formula (I) 【Chemistry 4】 (wherein R represents a hydrogen atom or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of group 12 or 13 of the periodic table of the elements, an ammonium ion, or a C 1 ~C 10 At least one phosphinic acid derivative of Use of a mixture comprising, with the proviso that 5 to 200 parts by weight of at least one polyamide reinforced with glass fibers is used as component e), for every 100 parts by weight of the at least one polyamide used as component a), Use provided that 0.1 to 3 parts by weight of component b), 0.01 to 3 parts by weight of component c) and 0.01 to 3 parts by weight of component d) are used.

12. 12. Use according to claim 11, characterised in that polyamide 6 or polyamide 66 is used as component a), 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine is used as component b) and sodium hypophosphite or sodium hypophosphite monohydrate is used as component c).

13. To reduce the color change ΔE calculated according to DIN EN ISO 11664-4 over 500 hours at 150°C and / or at 80°C, 340 nm and 1.55 W / m2 in the absence of rain 2 for reducing the color change ΔE calculated according to DIN EN ISO 11664-4 after UV irradiation according to DIN ISO 4892-2A at 100 °C for 200 h and / or for retaining the impact resistance determined according to ISO 180-1U and / or for retaining the elongation at break determined according to ISO 527 after hot air aging at 140 °C for 500 h, b) at least one secondary aromatic amine c) General formula (I) 【Chemistry 5】 (R represents a hydrogen atom or an alkyl, cycloalkyl or aryl group; R' represents an alkali metal, an alkaline earth metal, a metal of group 12 or 13 of the periodic table of the elements, an ammonium ion, or a C 1 ~C 10 At least one phosphinic acid derivative of d) Bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite is used in glass fiber reinforced polyamide based products, with the proviso that For 100 parts by weight of at least one polyamide used as component a) and 5 to 200 parts by weight of glass fibres used as component e), 2. A process according to claim 1, characterised in that 0.1 to 3 parts by weight of component b), 0.01 to 3 parts by weight of component c) and 0.01 to 3 parts by weight of component d) are used.

14. 14. The process according to claim 13, characterized in that polyamide 6 or polyamide 66 is used as component a), 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine is used as component b) and sodium hypophosphite or sodium hypophosphite monohydrate is used as component c).

Citation Information

Patent Citations

  • Long-term high temperature thermal ageing-resistant PA6 material and preparation method thereof

    CN102618027A

  • Elevator roller dedicated PA66 composite material and its preparation method

    CN103554905A

  • Polyamide composition capable of improving color fastness after hot baking and application of the polyamide composition

    CN111117218A

  • Heat conductive resin composition

    JP2009185151A

  • Polyamide composition and molded article

    JP2014012773A

Cited By

  • Polyamide-based products

    US12398258B2