Hardening composition

A curable composition with a resin and non-encapsulated PCM forms a stable, semi-IPN structure to manage heat in battery modules, addressing temperature uniformity and preventing heat-related issues, with long-term effectiveness and flame retardancy.

JP2024542794APending Publication Date: 2024-11-15LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024533082
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-10
Filing Date
2023-01-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies face challenges in managing heat generation from products like battery modules due to the proximity of battery cells, leading to difficulties in maintaining uniform temperature, preventing abnormal heat generation, ignition, and explosion, and the instability of phase change materials (PCMs) used for heat absorption.

Method used

A curable composition comprising a resin component and a non-encapsulated phase change material (PCM) that forms a cured product with latent heat properties, maintaining stability and effectiveness over time, and includes a semi-IPN structure to prevent leakage and ensure uniform temperature control.

Benefits of technology

The curable composition effectively manages heat generation, preventing abnormal heat, ignition, and explosion by maintaining uniform temperature and ensuring long-term stability, while providing excellent handling properties, storage stability, and flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542794000001_ABST
    Figure 2024542794000001_ABST
Patent Text Reader

Abstract

The present invention can provide a curable composition and its use. The present invention can provide a curable composition that is applied to a product or element that may generate heat, ignite, or explode during operation, storage, and / or maintenance, and can effectively respond to the heat, ignition, and explosion. For example, the composition of the present invention can be applied to an article including a plurality of such products or elements, and can respond to abnormal heat, explosion, and ignition generated from any one element or product, and can prevent or minimize the spread of such heat, explosion, and ignition to other adjacent elements or products. The present invention can also provide the curable composition such that excellent handling, storage stability, and flame retardancy are ensured. The curable composition or cured product of the present invention can also achieve the above properties by using a phase transition material that is not encapsulated, and can stably maintain the above properties for a long period of time.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0003582, dated January 10, 2022, and all contents disclosed in the documents of that patent application are incorporated herein by reference.

[0002] The present invention relates to a curable composition and its use. [Background technology]

[0003] The importance of technology for managing heat generated by products is increasing, but it is not easy to properly manage heat depending on the heat generation behavior of related products.

[0004] For example, a device such as a battery module or a battery pack includes a plurality of battery cells or a plurality of battery modules that are located relatively adjacent to each other. In such a device, it is necessary to maintain the temperature of a plurality of components as constant as possible under normal conditions, and it is necessary to prevent abnormal heat generation, fire, and / or explosion occurring in any one component from affecting other components as much as possible. However, since the components are located very close to each other, such control is very difficult.

[0005] In order to manage heat generated from components, a technique is known in which a so-called phase change material (PCM) is used to absorb heat due to abnormal heat generation (for example, Patent Document 1).

[0006] However, since the heat absorption patterns are all different depending on the type of phase transition material, it is difficult to achieve the necessary heat absorption properties for the applicable product, i.e., to absorb only the heat generated by abnormal heating without disturbing the normal state of the applicable product.

[0007] In addition, since phase transition materials usually change into a liquid phase when they absorb heat, it is quite difficult to maintain the heat absorption characteristics stably for a long period of time because the phase transition material disappears during use. To solve this problem, a technology is known in which the phase transition material is encapsulated to prevent leakage even when it changes into a liquid phase.

[0008] However, encapsulating the phase change material requires an additional step.

[0009] In addition, since the properties of the phase transition material change upon encapsulation, it is very difficult to precisely match the endothermic properties required by a product using the encapsulated phase transition material. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Korean Patent Publication No. 10-2020-0135105 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention relates to a curable composition and its use. The present invention aims to provide a curable composition that is applied to a product or element that may generate heat, ignite, or explode during operation, storage, and / or maintenance, and can effectively respond to the heat, ignition, and explosion. For example, the composition of the present invention is applied to an article including a plurality of such products or elements, and can respond to abnormal heat, explosion, and ignition generated from any one element or product, and can prevent or minimize the spread of such heat, explosion, and ignition to other adjacent elements or products. Another object of the present invention is to provide the curable composition in such a way that excellent handling, storage stability, and flame retardancy are ensured.

[0012] It is another object of the present invention to achieve the above properties using a non-encapsulated phase change material while still being able to stably maintain the above properties for an extended period of time. [Means for solving the problem]

[0013] Of the physical properties referred to in this specification, those that are affected by temperature are those measured at room temperature, unless otherwise specified.

[0014] In the present specification, the term "room temperature" refers to a natural temperature without heating or cooling, and means, for example, any one temperature within a range of about 10° C. to 30° C., such as about 15° C., about 18° C., about 20° C., about 23° C., or about 25° C. Unless otherwise specified in the present specification, the unit of temperature is ° C.

[0015] In the present specification, when pressure affects the results of physical properties, the physical properties are measured at normal pressure unless otherwise specified. The term "normal pressure" refers to the natural pressure without pressure increase or decrease, and is usually within the range of about 700 to 800 mmHg.

[0016] In the present specification, when humidity affects the results of physical properties, the physical properties are measured at room temperature and pressure with no particular adjustment of humidity, unless otherwise specified.

[0017] The present specification discloses a curable composition.

[0018] The curable composition may include at least a resin component and a Phase Change Material (PCM).

[0019] The term "curable composition" refers to a composition that can be cured. Curing refers to the phenomenon in which the composition hardens or the viscosity of the composition increases due to a chemical and / or physical reaction. As used herein, the term "cured product" refers to the cured state of the curable composition.

[0020] The curable composition may be a composition that can be cured by a known method. In one example, the curable composition may be an energy ray curable type, a moisture curable type, a heat curable type, or a room temperature curable type, or may be a hybrid curable type in which two or more of the above curing methods are applied.

[0021] If the curable composition is an energy ray curable type, the curing of the curable composition may be performed by irradiating the curable composition with energy rays such as ultraviolet rays. If the curable composition is a moisture curable type, the curing of the curable composition may be performed by maintaining the curable composition under appropriate humidity. If the curable composition is a heat curable type, the curing of the curable composition may be performed by applying appropriate heat. If the curable composition is a room temperature curable type, the curing of the curable composition may be performed by maintaining the curable composition at room temperature.

[0022] In one example, the curable composition may be a room temperature curable composition that can be cured by maintaining at room temperature without irradiation of special energy rays or application of heat. Even when the curable composition is a room temperature curable composition, the curing of the curable composition may be performed within an appropriate temperature range, not at room temperature, in consideration of the phase of the phase transition material contained in the curable composition. The appropriate temperature range is not particularly limited, and may be, for example, within a temperature range of about 40°C to 80°C or 50°C to 70°C.

[0023] The curable composition may be a one-part curable composition or a two-part curable composition. The one-part curable composition is a composition in which all components necessary for curing are mixed and stored, and the two-part curable composition is a composition in which the components necessary for curing are physically separated and stored. The two-part curable composition usually includes a so-called base part and a hardener part, and the base part and the hardener part are mixed for curing. When the curable composition according to an embodiment of the present invention is a two-part curable composition, the curable composition may be the base part or the hardener part of the two-part curable composition, or may be a mixture of the base part and the hardener part.

[0024] The cured product formed by the curable composition of the present invention may exhibit latent heat in a certain temperature range. The term "latent heat" is generally defined as the amount of heat required for any substance to undergo a phase transition without a temperature change. However, when the cured product of the present invention exhibits the latent heat, it does not necessarily have to undergo a phase transition as a whole. The latent heat for the cured product of the curable composition according to one embodiment of the present invention may be generated during the process of a state change of at least a part of the cured product or a component contained in the cured product.

[0025] The fact that the cured product of the curable composition of the present invention exhibits latent heat in a predetermined temperature range means that the cured product exhibits an endothermic peak in a predetermined temperature range in a DSC (Differential Scanning Calorimeter) analysis according to the method described in the Examples (Latent Heat Measurement Items in the Examples). The process in which the cured product of the curable composition according to one embodiment of the present invention exhibits the latent heat may be an isothermal process. Therefore, the cured product is applied to a heat-generating product, and can control the heat while maintaining the temperature of the product uniform, thereby minimizing or preventing the influence of abnormal heat generation, explosion, and / or fire generated from one product on other adjacent products.

[0026] The lower limit of the latent heat exhibited by the cured product of the curable composition of the present invention may be about 30 J / g, 32.5 J / g, 35 J / g, 37.5 J / g, 40 J / g, 42.5 J / g, 45 J / g, 47.5 J / g, 50 J / g, 52.5 J / g, 55 J / g, 57.5 J / g, 60 J / g, 61 J / g, or 62 J / g, and the upper limit may be about 200 J / g, 195 J / g, 190 J / g, 185 J / g, 180 J / g, 175 J / g, 180 J / g, 195 J / g, 200 J / g, 215 J / g, 220 J / g, 230 J / g, 240 J / g, 250 J / g, 260 J / g, 270 J / g, 280 J / g, 290 J / g, 300 J / g, 310 J / g, 320 J / g, 330 J / g, 340 J / g, 350 J / g, 360 J / g, 370 J / g, 380 J / g, 390 J / g, 400 J / g, 410 J / g, 420 J / g, 450 J / g, 47.5 J / g, 50 J / g, 52.5 J / g, 55 J / g, 57.5 J / g, 60 J / g, 61 J / g, or 62 J / g. The latent heat may be about 70 J / g, 165 J / g, 160 J / g, 155 J / g, 150 J / g, 145 J / g, 140 J / g, 135 J / g, 130 J / g, 125 J / g, 120 J / g, 115 J / g, 110 J / g, 105 J / g, 100 J / g, 95 J / g, 90 J / g, 85 J / g, 80 J / g, 75 J / g, 70 J / g, 65 J / g, 60 J / g, 55 J / g, 50 J / g, 45 J / g, or 40 J / g. The latent heat may be greater than or exceeding any one of the lower limits described above, or greater than or exceeding any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0027] The hardened body can exhibit the latent heat in a predetermined temperature range. A temperature section in which the hardened body exhibits latent heat can be referred to as a latent heat section in this specification. The latent heat section may be within a range obtained by subtracting the latent heat section start temperature from the latent heat section end temperature.

[0028] The latent heat interval start temperature is the temperature at the start of an endothermic peak in the DSC analysis, specifically, the temperature at the inflection point of the left onset of the endothermic peak. The latent heat interval end temperature is the temperature at the end of an endothermic peak in the DSC analysis, specifically, the temperature at the inflection point of the right onset of the endothermic peak. In the case where two or more endothermic peaks are observed in the DSC analysis, the latent heat interval start temperature is the temperature at the start of the first endothermic peak observed among the multiple endothermic peaks (the temperature at the inflection point of the left onset of the first endothermic peak), and the latent heat interval end temperature is the temperature at the end of the last endothermic peak observed among the multiple endothermic peaks (the temperature at the inflection point of the right onset of the last endothermic peak).

[0029] In one example, the lower limit of the latent heat section start temperature of the cured body may be about 0 ° C., 5 ° C., 10 ° C., 15 ° C., 20 ° C., 25 ° C., 30 ° C., 35 ° C., 40 ° C., 45 ° C., 50 ° C. or 55 ° C., and the upper limit may be about 80 ° C., 75 ° C., 70 ° C., 65 ° C., 60 ° C., 55 ° C., 50 ° C., 45 ° C., 40 ° C., 35 ° C., 30 ° C. or 25 ° C. The latent heat section start temperature may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the upper limits described above, and equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0030] In one example, the lower limit of the latent heat interval end temperature of the cured body may be about 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., or 60° C., and the upper limit may be about 100° C., 95° C., 90° C., 85° C., 80° C., 75° C., 70° C., 65° C., or 60° C. The latent heat interval end temperature may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0031] The lower limit of the width of the latent heat section of such a hardened body (latent heat section end temperature-latent heat section start temperature) may be about 5°C, 5.5°C, 6°C, 6.5°C, 7°C, 7.5°C, 8°C, 8.5°C, 9°C, 9.5°C, 10°C, 12°C, 14°C, 15°C, 16°C, 18°C, 19°C, 20°C, 25°C, 30°C or 35°C, and the upper limit may be about 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C or 20°C. The width of the latent heat interval may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or may be within a range of equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0032] The cured body having the latent heat property can be applied to various heat generating products and can operate the products in a stable and uniform temperature range. In addition, the cured body can be applied to a product including a plurality of heat generating elements arranged relatively adjacent to each other and can maintain the temperature of the entire product uniform, and can minimize or prevent the influence of abnormal heat generation, fire and / or explosion in any one element on the other elements. In particular, the cured body of the curable composition exhibiting the latent heat property can be applied to a product whose operating temperature should be maintained within a range of about 15°C to 60°C (e.g., a secondary battery or a battery module or battery pack including a plurality of secondary batteries) and can efficiently control heat.

[0033] The cured product of the curable composition of the present invention can stably maintain the latent heat property for a long period of time. The curable composition may contain a phase change material (PCM) so that the cured product exhibits the latent heat property. The phase change material may be a material that absorbs heat during a phase change from solid to liquid, a phase change from liquid to vapor, and / or a phase change from solid to vapor.

[0034] In one example, the phase transition material may be a material that absorbs heat during a phase transition from solid to liquid. Since such a material transitions to a liquid phase after absorbing heat, it may disappear in the cured body due to leakage, etc., and as a result, the heat absorbing property of the cured body may also disappear over time. In the present invention, the phase transition material in the cured body may not disappear in the cured body even after transitioning to a liquid phase by selecting a resin component contained in the curable composition that forms the cured body, adjusting the degree of crosslinking, adjusting the type and ratio of the phase transition material, and / or adjusting the method for producing the curable composition, and therefore the latent heat property may be stably maintained for a long period of time.

[0035] The cured product of the curable composition according to one embodiment of the present invention is a compound represented by the following formula 1:R For example, the L R The upper limit of L may be about 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1.4%, 1.3%, 1.2%, 1.1%, 1% or 0.5%, and the lower limit may be about 0% or 0.01%. R may be in the range of less than or equal to any one of the upper limits set forth above, or greater than or equal to any one of the lower limits set forth above, and less than or equal to any one of the upper limits set forth above.

[0036] [Formula 1] L R =100×(m1-m2) / m1

[0037] In formula 1, m1 is the initial weight of the cured body. This initial weight is the weight of the cured body before measuring m2. In formula 1, m2 is the weight of the cured body (the cured body with the initial weight m1) after maintaining the cured body at 80°C for 24 hours. The maintenance at 80°C for 24 hours may be performed, for example, with the cured body placed on filter paper. The units of m1 and m2 may be the same as each other, for example, g.

[0038] Generally, a phase transition material transitions to a liquid in an endothermic process. Since the endothermic start temperature of a general phase transition material is less than 80° C., if the material is maintained at 80° C. for 24 hours, a considerable amount of the phase transition material is expected to disappear. However, in the present invention, the phase transition material can be stably maintained in the cured body for a long period of time, and therefore, the L in the above range can be used. R It can be shown that

[0039] In particular, in the present invention, the above-mentioned properties can be exhibited even when the phase transition material contains a non-encapsulated phase transition material as a main component.

[0040] For example, the lower limit of the proportion of the non-encapsulated phase transition material based on the total weight of the phase transition material contained in the hardened body may be about 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or 95 wt%, and the upper limit may be about 100 wt%. The proportion may be equal to or greater than any one of the lower limits described above, or may be equal to or greater than any one of the lower limits described above and less than or equal to any one of the upper limits described above. The above properties can be ensured when the non-encapsulated phase transition material is contained in such a proportion.

[0041] The cured product of the curable composition according to one embodiment of the present invention is a compound represented by the following formula 2: L can be within a predetermined range. L The upper limit of M may be about 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.8% or 0.6%, and the lower limit may be about 0% or 0.01%. L may be in the range of less than or equal to any one of the upper limits set forth above, or greater than or equal to any one of the lower limits set forth above, and less than or equal to any one of the upper limits set forth above.

[0042] [Formula 2] M L =100×(m3-m4) / (m3×m5)

[0043] In formula 2, m3 means the initial weight of the hardened body, which is the weight before the hardened body is kept in water (e.g., distilled water) at room temperature for 96 hours as described below. In formula 2, m4 is the weight measured after the hardened body of the initial weight m3 is immersed in water (e.g., distilled water) at room temperature for 96 hours, and m5 is the weight ratio of the phase transition material contained in the hardened body. The units of m3 and m4 may be the same, for example, g. Also, the unit of m5 is % by weight, which is the percentage of the weight of the phase transition material contained in the hardened body with respect to the total weight of the hardened body. In this case, the hardened body for measuring m5 may be the hardened body of the weight m3 (i.e., the hardened body before being immersed in water (e.g., distilled water) at room temperature for 96 hours). In addition, the weight of the phase transition material applied to the calculation of m5 is the weight of the entire phase transition material present in the hardened body, and therefore, when the hardened body contains only the polar crystalline phase transition material, m5 may be determined based on the weight of only the polar crystalline phase transition material, and when the hardened body contains both the polar crystalline phase transition material and other phase transition materials, m5 may be determined based on the total weight of the polar crystalline phase transition material and other phase transition materials. In addition, m4 may be the weight measured after removing the hardened body from water and removing the moisture.

[0044] The cured product of the present invention has the M of the above formula 2 even when a polar crystalline phase transition material described later is used as the phase transition material. L can be set to be within the above range. Polar crystalline phase transition materials are advantageous in exhibiting the preferred endothermic properties required in the present invention, but because they have polarity, they are compatible with water and therefore can be easily lost when in contact with water. However, in the present invention, when a polar crystalline phase transition material is applied, particularly when a non-encapsulated polar crystalline phase transition material is applied, the above properties can be exhibited.

[0045] For example, the lower limit of the ratio of the polar crystalline phase transition material or the non-encapsulated polar crystalline phase transition material based on the total weight of the phase transition material contained in the cured body may be about 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or 95 wt%, and the upper limit may be about 100 wt%, 95 wt%, 90 wt%, 85 wt%, 80 wt%, 75 wt%, or 70 wt%. The ratio may be equal to or greater than any one of the lower limits described above, or may be equal to or greater than any one of the lower limits described above and less than or equal to any one of the upper limits described above. The above properties can be ensured when the polar crystalline phase transition material or the non-encapsulated polar crystalline phase transition material is contained in such a ratio.

[0046] Such properties can be achieved by adjusting the crosslinked network of the cured product and / or the molecular weight properties of the resin components constituting the network. In general, when the crosslinking degree of the crosslinked network is high and / or the molecular weight of the resin components is high, the property of maintaining the phase transition material is high, and as a result, even when the phase transition material becomes liquid and / or comes into contact with water, the loss of the material can be effectively suppressed. However, when the crosslinking degree of the crosslinked network is too high or the molecular weight of the resin components is too high, the flexibility and elasticity of the cured product are relatively poor, and therefore it is not suitable for cases where impact resistance or vibration resistance is required.

[0047] In the present invention, all of the above characteristics can be satisfied by controlling the degree of crosslinking of the cured product so as to have the hardness and / or elasticity characteristics described below.

[0048] The Shore A hardness of the cured product of the curable composition according to one embodiment of the present invention can be adjusted. For example, the upper limit of the Shore A hardness may be about 10, 9.9, 9.8, 9.7, 9.6, 9.5, 9.4, 9.3, 9.2, 9.1, 9.0, 8.5, 8, 7.5, 7, 6.5, or 6, and the lower limit may be about 0.01, 0.1, 0.5, 1, 1.2, 1.4, 1.6, 1.8, 2, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, or 9. The Shore A hardness may be less than or equal to any one of the upper limits described above, or may be greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0049] The hardness of the cured body is determined by the type of resin component constituting the cured body and / or the degree of crosslinking. In the present invention, a crosslinked network is formed so that the cured body can exhibit a hardness within the above range, and thus a network capable of stably maintaining the phase transition material can be provided. In addition, a hardness within the above range allows the cured body of the curable composition to stably fill spaces of complex shapes, and also improves vibration resistance and impact resistance.

[0050] In the cured product of the curable composition according to one embodiment of the present invention, Tan δ in the following formula 3 may be within a predetermined range. For example, the lower limit of Tan δ may be about 0.01, 0.05, 0.1, 0.15, 0.16, 0.18, 0.2, 0.22, 0.25, 0.3, 0.35, or 0.4, and the upper limit may be about 5, 4.5, 4, 3.5, 3, 2.5, 2, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.25, or 0.25. The Tan δ may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0051] [Formula 3] Tanδ = G” / G'

[0052] In Equation 3, G' is the storage modulus of the cured body at room temperature, and G" is the loss modulus of the cured body at room temperature. Methods for measuring the storage modulus and loss modulus are described in the Examples.

[0053] As can be seen from Equation 3, Tan δ is the ratio of the loss modulus G" to the storage modulus G'. Generally, the higher the storage modulus, the more the cured body behaves like an elastic body, and the higher the loss modulus, the more the cured body behaves like a viscous body or liquid. A cured body having the above ratio of G' and G" can exhibit the properties targeted in the present invention.

[0054] The lower limit of the storage modulus of the cured body at room temperature (i.e., G' in Formula 3) may be about 0.2 MPa, 0.21 MPa, 0.22 MPa, 0.23 MPa, 0.24 MPa, 0.25 MPa, 0.26 MPa, 0.27 MPa, 0.28 MPa, 0.29 MPa, 0.3 MPa, or 0.31 MPa, and the upper limit may be about 10 MPa, 9 MPa, 8 MPa, 7 MPa, 6 MPa, 5 MPa, 4 MPa, 3 MPa, 2 MPa, 1 MPa, 0.9 MPa, 0.8 MPa, 0.7 MPa, 0.6 MPa, 0.5 MPa, 0.4 MPa, 0.3 MPa, 0.29 MPa, 0.28 MPa, or 0.27 MPa. The storage modulus may be equal to or greater than any one of the lower limits described above, or may be equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. A cured material having the G' may exhibit the properties desired in the present invention.

[0055] The hardness and / or elasticity of the cured product can be achieved by adjusting the crosslinked network of the cured product. However, it is difficult to achieve a cured product with the above properties by curing only a general resin component. In the present invention, the desired crosslinked network can be achieved by adjusting the type of resin component that forms the crosslinked network, the type of the phase transition material, the method for producing the curable composition, and / or the method for curing the curable composition.

[0056] Such a crosslinked network of the present invention may be called a semi-IPN (Interpenetrating Polymer Network). Semi-IPN means that the crosslinked network includes a crosslinked structure of the resin component and further includes a structure formed by an interaction between the phase transition materials and / or an interaction between the phase transition material and the crosslinked structure of the resin component. Such a semi-IPN structure may be achieved by adjusting the type of resin component, the type of the phase transition material, the method for producing the curable composition, and / or the method for curing the curable composition.

[0057] In addition, the cured product according to one embodiment of the present invention may have a flame retardancy evaluation result of V-0 or V-1 grade measured according to the UL94V measurement standard, thereby ensuring excellent flame retardancy so that even if abnormal heat generation, explosion, or fire occurs in one of the multiple elements, the influence of such heat generation, explosion, or fire on the other adjacent elements can be prevented or minimized.

[0058] The curable composition may include a resin component. Such a resin component may be a curable resin component that can be cured. The term "curable resin component" includes not only a so-called resin component itself, but also a component that can form a resin component after a curing reaction. Thus, the curable resin component may be a monomolecular, oligomeric, or polymeric compound.

[0059] In the present invention, a component having a predetermined weight average molecular weight (Mw) can be used as the resin component. For example, the lower limit of the weight average molecular weight of the resin component may be about 9000 g / mol, 10000 g / mol, 15000 g / mol, 20000 g / mol, or 25000 g / mol, and the upper limit may be about 100000 g / mol, 90000 g / mol, 80000 g / mol, 70000 g / mol, 60000 g / mol, 50000 g / mol, 40000 g / mol, or 30000 g / mol. The weight average molecular weight may be less than or equal to any one of the upper limits described above, or greater than or equal to any one of the lower limits described above, or greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above. A resin component having such molecular weight characteristics is advantageous for components in the composition, for example, for forming a cured body with a desired crosslinked network.

[0060] There is no particular limit to the type of resin component. In one example, the resin component may be a urethane resin component, a silicone resin component, an acrylic resin component, or an epoxy resin component. The urethane resin component, the silicone resin component, the acrylic resin component, or the epoxy resin component may be a polyurethane, a silicone resin, an acrylic resin, or an epoxy resin, or may be a component that forms the polyurethane, the silicone resin, the acrylic resin, or the epoxy resin through a curing reaction. There is no particular limit to the specific type of applicable resin component, and one that exhibits the above-mentioned molecular weight characteristics can be selected and used from among known urethane resin components, silicone resin components, acrylic resin components, or epoxy resin components, and the crosslinking network of the final cured body can be controlled by controlling the crosslinking degree of such resin components. In particular, a silicone resin component or a urethane resin component can be used from the viewpoint of effectively forming the semi-IPN structure together with a phase transition material, particularly a crystalline polar phase transition material, described later.

[0061] For example, when the resin component is a silicone resin component, the component may include, as an addition-curable silicone resin component, (1) a polyorganosiloxane containing two or more alkenyl groups in the molecule and (2) a polyorganosiloxane containing two or more silicon-bonded hydrogen atoms in the molecule. The compound can form a cured product by addition reaction in the presence of a catalyst such as a platinum catalyst.

[0062] The (1) polyorganosiloxane contains at least two alkenyl groups. Specific examples of the alkenyl groups include vinyl, allyl, butenyl, pentenyl, hexenyl, and heptenyl groups, among which vinyl groups are usually used, but are not limited thereto. In the (1) polyorganosiloxane, the bonding position of the alkenyl groups is not particularly limited. For example, the alkenyl groups may be bonded to the ends of the molecular chain and / or to the side chains of the molecular chain. In the (1) polyorganosiloxane, examples of the substituents that may be included in addition to the alkenyl include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl and phenethyl; and halogen-substituted alkyl groups such as chloromethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl. Of these, methyl and phenyl groups are usually used, but the present invention is not limited thereto.

[0063] The molecular structure of the (1) polyorganosiloxane is not particularly limited, and may have any shape, such as linear, branched, cyclic, network, or partially branched linear. Usually, among the molecular structures described above, those having a linear molecular structure are particularly used, but are not limited thereto.

[0064] More specific examples of the (1) polyorganosiloxane include dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with trimethylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, R 1 2SiO 2 / 2 The siloxane unit represented by R 1 2R 2 SiO 1 / 2 The siloxane unit represented by and SiO 4 / 2 Polyorganosiloxane copolymers containing siloxane units represented by R 1 2R 2 SiO 1 / 2 The siloxane unit represented by and SiO 4 / 2 Polyorganosiloxane copolymers containing siloxane units represented by R 1 R 2 SiO 2 / 2 The siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by R 2 SiO 3 / 2 and mixtures of two or more of the above. 1is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenethyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group. 2 is an alkenyl group, and specifically may be a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, or the like.

[0065] In the addition curable silicone composition, the (2) polyorganosiloxane can crosslink the (1) polyorganosiloxane. In the (2) polyorganosiloxane, the bond position of the hydrogen atom is not particularly limited, and may be bonded to, for example, the end of the molecular chain and / or the side chain. In the (2) polyorganosiloxane, the type of the substituent that can be contained other than the silicon-bonded hydrogen atom is not particularly limited, and examples thereof include alkyl groups, aryl groups, aralkyl groups, and halogen-substituted alkyl groups, as mentioned in the (1) polyorganosiloxane, and among these, methyl groups or phenyl groups are usually used, but are not limited thereto.

[0066] The molecular structure of the (2) polyorganosiloxane is not particularly limited, and may have any shape, such as linear, branched, cyclic, network, or partially branched linear, etc. Among the molecular structures described above, those having a linear molecular structure are usually used, but are not limited thereto.

[0067] More specific examples of the (2) polyorganosiloxane include methylhydrogenpolysiloxanes capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogen copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, dimethylsiloxane-methylphenylsiloxane copolymers capped with dimethylhydrogensiloxane groups at both molecular chain terminals, methylphenylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, R 1 3SiO 1 / 2 The siloxane unit represented by R 1 2HSiO 1 / 2 The siloxane unit represented by and SiO 4 / 2 Polyorganosiloxane copolymers containing siloxane units represented by R 1 2HSiO 1 / 2 The siloxane unit represented by and SiO 4 / 2 Polyorganosiloxane copolymers containing siloxane units represented by R 1 HSiO 2 / 2 The siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by HSiO 3 / 2 and mixtures of two or more of the above. 1 is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenethyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group.

[0068] The content of the (2) polyorganosiloxane is not particularly limited as long as it is contained to an extent that suitable curing can be performed. For example, the (2) polyorganosiloxane may be contained in an amount such that the number of silicon-bonded hydrogen atoms is 0.5 to 10 per one alkenyl group contained in the (1) polyorganosiloxane. Within such a range, curing can be sufficiently promoted and heat resistance can be ensured.

[0069] The addition curable silicone resin component may further contain platinum or a platinum compound as a catalyst for curing. The specific type of platinum or platinum compound is not particularly limited. The proportion of the catalyst may be adjusted to a level at which suitable curing can be performed.

[0070] In another example, the silicone resin component may include, as a condensation-curable silicone resin component, for example, (a) an alkoxy group-containing siloxane polymer and (b) a hydroxyl group-containing siloxane polymer.

[0071] The (a) siloxane polymer may be, for example, a compound represented by the following chemical formula 1.

[0072] [Chemical formula 1] R 1 a R 2 b SiO c (OR 3 ) d

[0073] In chemical formula 1, R 1 and R 2 each independently represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group; R 3 represents an alkyl group, R 1 , R 2 and R 3When there are multiple of each, they may be the same or different, a and b each independently represent a number greater than or equal to 0 and less than 1, a+b represents a number greater than 0 and less than 2, c represents a number greater than 0 and less than 2, d represents a number greater than 0 and less than 4, and a+b+c×2+d is 4.

[0074] In the definition of Chemical Formula 1, the monovalent hydrocarbon group may be, for example, an alkyl group having 1 to 8 carbon atoms, a phenyl group, a benzyl group, or a tolyl group, and in this case, the alkyl group having 1 to 8 carbon atoms may be a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, or an octyl group. In addition, in the definition of Chemical Formula 1, the monovalent hydrocarbon group may be substituted with a known substituent such as a halogen, an amino group, a mercapto group, an isocyanate group, a glycidyl group, a glycidoxy group, or a ureido group.

[0075] In the definition of Chemical Formula 1, R 3 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, and a butyl group. Among the alkyl groups, a methyl group or an ethyl group is usually applied, but the alkyl group is not limited thereto.

[0076] A branched or tertiary crosslinked siloxane polymer can be used in the polymer of Chemical Formula 1. In addition, the (a) siloxane polymer may have residual hydroxyl groups within a range that does not impair the purpose, specifically, within a range that does not inhibit the dealcoholization reaction.

[0077] Said (a) siloxane polymer can be produced, for example, by hydrolysis and condensation of polyfunctional alkoxysilane or polyfunctional chlorosilane. An average technician in this field can easily select an appropriate polyfunctional alkoxysilane or chlorosilane according to the desired (a) siloxane polymer, and can easily control the conditions of hydrolysis and condensation reaction using it. In addition, when producing said (a) siloxane polymer, an appropriate monofunctional alkoxysilane can also be used in combination depending on the purpose.

[0078] As the (a) siloxane polymer, for example, commercially available organosiloxane polymers such as X40-9220 or X40-9225 manufactured by Shin-Etsu Silicones, and XR31-B1410, XR31-B0270 or XR31-B2733 manufactured by GE Toray Silicones can be used.

[0079] As the (b) hydroxyl group-containing siloxane polymer contained in the condensation-curable silicone composition, for example, a compound represented by the following chemical formula 2 can be used.

[0080] [ka]

[0081] In Chemical Formula 2, R4 and R5 each independently represent a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group, and when there are multiple R4 and multiple R5, they may be the same or different, and n represents an integer of 5 to 2,000.

[0082] In the definition of Chemical Formula 2, specific examples of the monovalent hydrocarbon group include the same hydrocarbon groups as those in Chemical Formula 1 above.

[0083] The (b) siloxane polymer can be produced, for example, by hydrolysis and condensation of dialkoxysilane and / or dichlorosilane. An average technician in this field can easily select an appropriate dialkoxysilane or dichlorosilane depending on the desired (b) siloxane polymer, and can easily control the conditions of the hydrolysis and condensation reaction using the dialkoxysilane or dichlorosilane. As the (b) siloxane polymer, for example, commercially available bifunctional organosiloxane polymers such as XC96-723, YF-3800, and YF-3804 from GE Toray Silicone Co., Ltd. can be used.

[0084] The addition-curable or condensation-curable silicone composition described above is one example of the silicone resin component that can be used in the present invention.

[0085] In another example, if the resin component is a urethane resin component, the component may include at least a polyol and a polyisocyanate. In the above, the polyol is a compound containing at least two hydroxyl groups, and the polyisocyanate is a compound containing at least two isocyanate groups. Each of these compounds may be a monomolecular, oligomeric, or polymeric compound.

[0086] The type of polyol is not particularly limited, and for example, known polyether polyols or polyester polyols can be applied. As the polyether polyols, polyalkylene glycols having 1 to 20, 1 to 16, 1 to 12, 1 to 8, or 1 to 4 carbon atoms in the alkylene glycol portion, such as polypropylene glycol or polyethylene glycol, ethylene oxide / propylene oxide copolymer polyols, PTME (poly(tetramethylene glycol)), PHMG (poly(hexamethylene ether glycol)), etc. are known. As the polyester polyols, there are known polyols synthesized from dibasic acids and glycols, such as polyester polyols or polycaprolactone polyols (obtained by ring-opening polymerization of cyclic lactones) containing the dibasic acid units and glycol units. In addition to the above-mentioned polyols, there are also known hydrocarbon polyols such as carbonate polyols, vegetable polyol castor oil, HTPB (hydroxyl-terminated polybutadiene), and HTPIB (hydroxyl-terminated polyisobutylene). An appropriate type of polyol can be selected and used from among the known polyols as described above. In addition, an appropriate type of polyisocyanate can be selected and used from among known aromatic or aliphatic polyisocyanate compounds as the polyisocyanate.

[0087] The lower limit of the ratio of the resin component based on the total weight of the curable composition may be about 10% by weight, 15% by weight, 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, 55% by weight, 60% by weight, 65% by weight, 70% by weight, 75% by weight, or 80% by weight, and the upper limit may be about 95% by weight, 90% by weight, 85% by weight, 80% by weight, 75% by weight, 70% by weight, 65% by weight, 60% by weight, 55% by weight, 50% by weight, 45% by weight, 40% by weight, 35% by weight, or 30% by weight. Such a ratio is based on the total weight of the curable composition, provided that, in the case where the curable composition contains a solvent, the ratio is based on the total weight of the curable composition excluding the solvent. The ratio may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0088] The curable composition may further include a so-called phase change material (PCM) in order to ensure the above-mentioned latent heat property. As is well known, a phase change material is a material that absorbs or generates heat during a phase transition. The phase transition process is generally an isothermal process.

[0089] The phase transition in which the phase transition material absorbs or generates heat may be a solid-to-solid phase transition, a solid-to-liquid phase transition, a solid-to-gas phase transition, or a liquid-to-gas phase transition. The above-described phase transition reactions (solid-to-solid, solid-to-liquid, solid-to-gas, liquid-to-gas) may be endothermic reactions. From the viewpoint of efficiency, a substance that undergoes a phase transition from solid to liquid is advantageous, but such a substance is difficult to maintain in the hardened body because it becomes a liquid phase after the phase transition. However, the hardened body of the present invention shows the above-mentioned weight change rate, and therefore a substance that undergoes a phase transition from solid to liquid can be applied. Thereby, the phase transition material applied in the present invention may be a substance in which a phase transition occurs between a solid phase and a liquid phase, or a substance in which the phase transition reaction from the solid phase to the liquid phase is an endothermic reaction.

[0090] In the curable composition, the weight ratio of the phase transition material relative to 100 parts by weight of the resin component may be about 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, or 95 parts by weight, and the upper limit may be about 200 parts by weight, 190 parts by weight, 180 parts by weight, 170 parts by weight, 160 parts by weight, 150 parts by weight, 140 parts by weight, 130 parts by weight, 120 parts by weight, 110 parts by weight, 100 parts by weight, 90 parts by weight, 80 parts by weight, 70 parts by weight, or 65 parts by weight. The ratio may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0091] In order to achieve the semi-IPN structure, a crystalline polar phase transition material can be used as the phase transition material. The phase transition material being polar means that the phase transition material contains a polar functional group, and the types of such polar functional groups include hydroxyl groups, alkylene oxide residues (e.g., alkylene oxide residues having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms), and / or carboxyl groups. In particular, phase transition materials containing the hydroxyl groups and / or alkylene oxide residues (e.g., alkylene oxide residues having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms) can be used. Due to such polar functional groups, the phase transition material can physically or chemically interact with the resin component or its crosslinked structure and / or other phase transition materials, thereby realizing the semi-IPN. The lower limit of the number of polar functional groups contained in the phase transition material may be about 1 or 2, and the upper limit may be about 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, or 2. The number of polar functional groups may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0092] The phase transition material being crystalline means that the phase transition material exhibits a melting point within a certain range in the DSC analysis in the examples described below, whereas a non-crystalline material does not have the melting point.

[0093] As used herein, the terms "crystalline polar phase change material" and "polar crystalline phase change material" are synonymous.

[0094] The lower limit of the melting point (Tm) of such a crystalline polar phase transition material may be about 1°C, 1.5°C, 2°C, 2.5°C, 3°C, 3.5°C, 4°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, and the upper limit may be about 95°C, 90°C, 85°C, 80°C, 79°C, 78°C, 77°C, 76°C, 75°C, 74°C, 73°C, 72°C, 71°C or 70°C, 65°C, 60°C, 55°C, 50°C, 45°C or 40°C. The melting point may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0095] In order to efficiently form the semi-IPN, the polar crystalline phase transition material may have a molecular weight above a certain level. For example, the number average molecular weight (Mn) of the polar crystalline phase transition material may be 100% or more. The lower limit of the molecular weight may be about 1,000 g / mol, 1,200 g / mol, 1,400 g / mol, 1,600 g / mol, 1,800 g / mol, 2,000 g / mol, 2,500 g / mol, 3,000 g / mol, 3,500 g / mol, 3,800 g / mol, or 4,000 g / mol, and the upper limit may be about 10,000 g / mol, 9,500 g / mol, 9,000 g / mol, 8,500 g / mol, 8,000 g / mol, 7,500 g / mol, 7,000 g / mol, 6,500 g / mol, 6,000 g / mol, 5,500 g / mol, 5,000 g / mol, 4,500 g / mol, or 4,000 g / mol. The number average molecular weight may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above. A material having such a number average molecular weight level can effectively form a semi-IPN structure through the physical or chemical interaction, and such a structure can exhibit a desired level of hardness and elasticity. In addition, when the number average molecular weight is within the above range, the melting point of the material can be formed at a suitable level in relation to the normal operating temperature range of a heat-generating product, and therefore, when applied to a heat-generating product, the problem of a shortened life span of the product due to heat generation can be effectively prevented.

[0096] In order to effectively form a semi-IPN structure, a material having a linear structure can be used as the material.

[0097] The type of the polar crystalline phase transition material is not particularly limited, and for example, polyalcohol can be used. The term "polyalcohol" refers to a compound having two or more hydroxyl groups. The lower limit of the number of hydroxyl groups contained in the polyalcohol may be about 2, and the upper limit may be about 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, or 2. The number of hydroxy groups may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0098] Such polyalcohols, particularly linear polyalcohols having the number-average molecular weight, can effectively form the semi-IPN while exhibiting the desired latent heat characteristics. Specific examples of polyalcohols include one or more selected from the group consisting of glycerin, polyalkylene glycols such as polyethylene glycol (PEG) (for example, polyalkylene glycols having an alkylene glycol moiety with a carbon number of 1 to 20, 1 to 16, 1 to 12, 1 to 8, or 1 to 4), xylitol, and erythritol. From the viewpoint of easily securing a number-average molecular weight in the above-mentioned range, the polyalkylene glycols can be applied, and in particular, the polyalkylene glycols having a linear structure can be applied.

[0099] The lower limit of the latent heat exhibited by such a crystalline polar phase transition material may be about 100 J / g, 110 J / g, 120 J / g, 130 J / g, 140 J / g, 150 J / g, 155 J / g, 160 J / g, 165 J / g, 170 J / g, 175 J / g, or 180 J / g, and the upper limit may be about 300 J / g, 280 J / g, 260 J / g, 240 J / g, 220 J / g, 200 J / g, 190 J / g, 180 J / g, 170 J / g, or 165 J / g. The latent heat may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0100] The lower limit of the latent heat interval start temperature of the crystalline polar phase transition material may be about 20°C, 30°C, 40°C, 45°C, 50°C or 55°C, and the upper limit may be about 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C or 60°C. The temperature may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. The definition of the latent heat interval start temperature is the same as that of the latent heat interval start temperature of the hardened body.

[0101] The upper limit of the latent heat interval end temperature of the crystalline polar phase transition material may be about 200°C, 150°C, 100°C, 95°C, 90°C, 85°C, 80°C, 75°C or 70°C, and the lower limit may be about 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C or 65°C. The temperature may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. The definition of the latent heat interval end temperature is the same as the latent heat interval end temperature of the hardened body.

[0102] The lower limit of the width of the latent heat interval (latent heat interval end temperature-latent heat interval start temperature) of the crystalline polar phase transition material may be about 1° C., 2° C., 3° ​​C., 4° C., 5° C., 6° C., 7° C., 8° C., 9° C., or 9.5° C., and the upper limit may be about 100° C., 90° C., 80° C., 70° C., 60° C., 50° C., 40° C., 30° C., 20° C., or 10° C. The width may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0103] Among the materials known to be polar crystalline phase transition materials described above, materials having the above number average molecular weight, linear structure and / or latent heat characteristics can be selected.

[0104] The content of the polar crystalline phase transition material can be controlled to form the semi-IPN. For example, the lower limit of the ratio of the polar crystalline phase transition material based on the total weight of the phase transition material contained in the curable composition or the cured body may be about 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or 95 wt%, and the upper limit may be about 100 wt%, 99 wt%, 98 wt%, 95 wt%, 90 wt%, 85 wt%, 80 wt%, 75 wt%, or 70 wt%. The ratio may be equal to or greater than any one of the lower limits described above, or may be equal to or greater than any one of the lower limits described above and less than or equal to any one of the upper limits described above. The polar crystalline phase transition material contained in such a ratio effectively forms the semi-IPN described above. For the formation of the semi-IPN, the crystalline polar phase transition material may be a non-encapsulated material.

[0105] The curable composition may further include a phase transition material different from the crystalline polar phase transition material. For convenience, such a phase transition material is called a second phase transition material. Examples of the second phase transition material include, but are not limited to, one or more selected from the group consisting of fatty acids, ketone compounds, D-lactic acid, and paraffin compounds.

[0106] Examples of the fatty acid include formic acid, n-octanoic acid, lauric acid, palmitic acid, and stearic acid. Examples of the ketone compound include 2-pentadecanone and 4-heptadecanone. Examples of the paraffin compound include n-heptadecane, n-octadecane, n-nonadecane, n-eicosane, n-henicosane, n-docosane, and n-tricosane. osane, n-pentacosane, n-hexacosane, n-heptacosane, n-octacosane, n-nonacosane, n-triacontane, n-hentriacontane, n-dotriacontane, n-triatriacontane or other higher paraffins Examples of suitable wax include Paraffin C16 to C18, Paraffin C13 to C24, RT 35 HC, Paraffin C16 to C28, Paraffin C20 to C33, Paraffin C22 to C45, Paraffin C22 to C50, Paraffin natural wax 811, and Paraffin natural wax 106.

[0107] The second phase transition material may be, for example, a paraffin having a carbon number of 5 or more. In another example, the carbon number of the paraffin may be within a range of 5 to 40. Such a paraffin may be an alkane having the above carbon number.

[0108] When applicable, the lower limit of the melting point (Tm) of the second phase transition material may be about 1°C, 1.5°C, 2°C, 2.5°C, 3°C, 3.5°C, 4°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, and the upper limit may be about 95°C, 90°C, 85°C, 80°C, 79°C, 78°C, 77°C, 76°C, 75°C, 74°C, 73°C, 72°C, 71°C or 70°C, 65°C, 60°C, 55°C, 50°C, 45°C or 40°C. The melting point may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0109] When applicable, the lower limit of the latent heat of the second phase transition material may be about 100 J / g, 110 J / g, 120 J / g, 130 J / g, 140 J / g, 150 J / g, 155 J / g, 160 J / g, 165 J / g, 170 J / g, 175 J / g or 180 J / g, and the upper limit may be about 300 J / g, 280 J / g, 260 J / g, 240 J / g, 220 J / g, 200 J / g, 190 J / g, 180 J / g, 170 J / g, 165 J / g, 160 J / g or 155 J / g. The latent heat may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0110] The lower limit of the latent heat interval start temperature of the second phase transition material may be about 10°C, 15°C, 20°C, 30°C, 35°C or 40°C, and the upper limit may be about 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C or 45°C. The temperature may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. The definition of the latent heat interval start temperature is the same as that of the latent heat interval start temperature of the hardened body.

[0111] The upper limit of the latent heat interval end temperature of the second phase transition material may be about 200° C., 150° C., 100° C., 95° C., 90° C., 85° C., 80° C., 75° C., 70° C., 65° C., 60° C., 55° C., 50° C., 45° C., or 40° C., and the lower limit may be about 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., or 45° C. The temperature may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. The definition of the latent heat interval end temperature is the same as that of the latent heat interval end temperature of the hardened body.

[0112] The lower limit of the width of the latent heat interval (latent heat interval end temperature-latent heat interval start temperature) of the second phase transition material may be about 1° C., 2° C., 3° ​​C., 4° C., 5° C., 6° C., 7° C., 8° C., 9° C., or 9.5° C., and the upper limit may be about 100° C., 90° C., 80° C., 70° C., 60° C., 50° C., 40° C., 30° C., 20° C., 10° C., 9° C., 8° C., 7.5° C., 7° C., 6° C., or 5.5° C. The width may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0113] When applied, the second phase transition material may be a non-polar phase transition material in consideration of the efficiency of forming the semi-IPN structure described above. The term "non-polar phase transition material" refers to a phase transition material that does not have the polar functional group that the polar phase transition material has.

[0114] When included, the properties of the second phase transition material can be tailored in relation to the amorphous polar phase transition material to achieve targeted endothermic properties and effectively form the desired semi-IPN.

[0115] For example, when included, the absolute value of the difference between the melting point of the amorphous polar phase transition material and the melting point of the second phase transition material can be adjusted. The lower limit of the absolute value may be about 5° C., 7° C., 9° C., 11° C., 13° C., 15° C., 17° C., 19° C., 21° C., 23° C., or 25° C., and the upper limit may be about 60° C., 48° C., 46° C., 44° C., 42° C., 40° C., 38° C., 36° C., 34° C., 32° C., 30° C., 28° C., 26° C., 24° C., 22° C., or 20° C. The absolute value may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. When there are a plurality of the amorphous polar phase transition materials and the second phase transition materials, the absolute value may be a difference between the lowest melting point of the amorphous polar phase transition materials and the highest melting point of the second phase transition materials, or a difference between the highest melting point of the amorphous polar phase transition materials and the lowest melting point of the second phase transition materials. In the above case, the second phase transition material may have a lower or higher melting point than the amorphous polar phase transition materials.

[0116] For example, when included, the absolute value of the difference between the latent heat interval start temperature of the non-crystalline polar phase transition material and the latent heat interval start temperature of the second phase transition material can be adjusted. The lower limit of the absolute value may be about 5°C, 7°C, 9°C, 11°C, 13°C, 15°C, 17°C, 19°C, 21°C, 23°C, or 25°C, and the upper limit may be about 60°C, 48°C, 46°C, 44°C, 42°C, 40°C, 38°C, 36°C, 34°C, 32°C, 30°C, 28°C, 26°C, 24°C, 22°C, or 20°C. The absolute value may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. When there are a plurality of the amorphous polar phase transition materials and the second phase transition materials, the absolute value may be the difference between the lowest latent heat interval start temperature among the latent heat interval start temperatures of the amorphous polar phase transition materials and the highest latent heat interval start temperature among the latent heat interval start temperatures of the second phase transition material, or the difference between the highest latent heat interval start temperature among the latent heat interval start temperatures of the amorphous polar phase transition materials and the lowest latent heat interval start temperature among the latent heat interval start temperatures of the second phase transition material. In the above case, the second phase transition material may have a lower latent heat interval start temperature or a higher latent heat interval start temperature than the amorphous polar phase transition material.

[0117] The second phase transition material may not be included in the curable composition, or if included, its content may be controlled in consideration of the efficiency of forming the semi-IPN. For example, the lower limit of the content of the second phase transition material relative to 100 parts by weight of the crystalline polar phase transition material may be about 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, or 50 parts by weight, and the upper limit may be about 100 parts by weight, 90 parts by weight, 80 parts by weight, 70 parts by weight, 60 parts by weight, or 55 parts by weight. The content may be equal to or greater than any one of the lower limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. When the second phase transition material is contained within such a range, the endothermic properties of the cured product can be adjusted to a target level without inhibiting the formation of the semi-IPN.

[0118] The curable composition may optionally contain a filler, such as a thermally conductive filler, which can efficiently transfer heat generated from the part to the phase transition material and stably ensure the desired heat absorbing properties.

[0119] The thermally conductive filler is not particularly limited, and examples thereof include metal hydroxides such as aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), calcium hydroxide (Ca(OH)2), boehmite (AlOOH) and hydromagnesite, metal oxides such as zinc oxide (ZnO), beryllium oxide (BeO), magnesia and alumina (Al2O3), nitrides such as aluminum nitride (AlN, aluminum nitride), boron nitride (BN, boron nitride) and silicon nitride (Si3N4, silicon nitride), and inorganic fillers such as silicon carbide (SiC), but are not limited thereto. One or more of the above fillers can be selected. When a low-density hardened body is to be formed, a filler with a small specific gravity can be selected from the above filler components, and for example, a metal hydroxide such as aluminum hydroxide can be selected.

[0120] The shape of the filler is not particularly limited, and for example, spherical, needle-like, plate-like, and other amorphous fillers can be used.

[0121] In one example, the filler may have an average particle size in the range of 10 μm to 200 μm. The average particle size is a D50 particle size measured by the method described in the examples below. By using a filler with such a particle size, the desired effect can be more efficiently achieved.

[0122] In other examples, the average particle size of the filler may be 15 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, 35 μm or more, or 40 μm or more, or may be about 180 μm or less, 160 μm or less, 140 μm or less, 120 μm or less, 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0123] The content of the thermally conductive filler in the curable composition is adjusted according to the purpose. For example, the curable composition may contain the thermally conductive filler in the range of 50 to 200 parts by weight relative to 100 parts by weight of the resin component. In another example, the curable composition may contain the thermally conductive filler in the range of 60 parts by weight or more, 65 parts by weight or more, 70 parts by weight or more, 75 parts by weight or more, 80 parts by weight or more, 85 parts by weight or more, 90 parts by weight or more, or 95 parts by weight or more, or 190 parts by weight or less, 180 parts by weight or less, 170 parts by weight or less, 160 parts by weight or less, 150 parts by weight or less, 140 parts by weight or less, 130 parts by weight or less, 120 parts by weight or less, or 110 parts by weight or less, relative to 100 parts by weight of the resin component.

[0124] The curable composition according to one embodiment of the present invention may further include other necessary components in addition to the above components. For example, the curable composition may further include, in addition to the above components, further additives such as catalysts, pigments, dyes, dispersants, thixotropic agents, flame retardants, etc., if necessary.

[0125] Such curable compositions may be solvent-based, water-based or solventless compositions, preferably solventless compositions.

[0126] As described above, the curable composition may be a one-part composition or a two-part composition, and in some cases may be the base or hardener part of a two-part composition, or may be a mixture of the base and hardener parts.

[0127] When the curable composition is a two-liquid composition, the ratio of other components in the base and hardener parts other than the curable resin component is not particularly limited. For example, the phase transition material and / or filler may be entirely contained in the base or hardener part, or may be separately contained in the base and hardener parts.

[0128] The curable composition of the present invention is suitable for use in a variety of applications, particularly in heat-generating products, and can be used as a material for controlling the heat of said products.

[0129] The present invention also relates to a method for producing a cured product which has the semi-IPN and exhibits the endothermic properties.

[0130] The method of manufacture may include curing the curable composition described above.

[0131] In this process, the curing temperature can be controlled to effectively form the semi-IPN. For example, the curing temperature can be adjusted in relation to the melting point of the polar crystalline phase transition material contained in the curable composition. That is, the phase transition material can exhibit fluidity capable of forming the semi-IPN at the adjusted temperature. For example, the lower limit of the absolute value of the difference between the curing temperature (Tc) and the melting point (Tm) of the polar crystalline phase transition material may be about 0°C, 0.5°C, 1°C, 1.5°C, 2°C, or 2.5°C, and the upper limit may be about 20°C, 18°C, 16°C, 14°C, 12°C, 10°C, 8°C, 6°C, 5°C, or 4°C. In relation to the absolute values ​​of the curing temperature and melting points, when the curable composition contains a plurality of types of non-crystalline polar phase transition materials, the melting point may be the melting point of the phase transition material having the highest melting point among the plurality of polar phase transition materials. The absolute value of the difference between the curing temperature and the melting point may be greater than or equal to any one of the lower limits described above, or less than or equal to any one of the upper limits described above, or may be within a range of greater than or equal to any one of the lower limits described above and less than or equal to any one of the upper limits described above.

[0132] Even if the composition is not a thermosetting type, i.e., a type of curable composition that is cured by application of heat, curing can be performed at the curing temperature. For example, even if the curable composition is an energy ray curable type or a room temperature curable type, the curing temperature (Tc) can be adjusted as described above, and the semi-IPN can be formed at such a temperature.

[0133] The curing temperature Tc may be higher or lower than the melting point Tm of the crystalline phase transition material, so long as it exhibits the above-mentioned difference from the melting point Tm.

[0134] In one example, the lower limit of the curing temperature Tc may be about 40° C. or 50° C., and the upper limit may be about 80° C. or 70° C. The curing temperature Tc may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or may be equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above.

[0135] Within this range, the curable composition can form a cured product having the desired properties of preventing leakage of the phase transition material, ensuring appropriate hardness, ensuring appropriate elasticity and viscosity, and having excellent flame retardancy.

[0136] The method may further include mixing the resin component and the phase change material to form the curable composition.

[0137] In this process, the temperature of the mixing can be controlled in order to effectively form the semi-IPN. For example, the mixing temperature (Tx) can be adjusted in relation to the melting point (Tm) of the polar crystalline phase transition material contained in the curable composition. That is, the phase transition material can exhibit fluidity capable of forming the semi-IPN at the adjusted temperature. For example, the lower limit of the absolute value of the difference between the mixing temperature (Tx) and the melting point (Tm) of the polar crystalline phase transition material may be about 0°C, 0.5°C, 1°C, 1.5°C, 2°C, 2.5°C, 3°C, 3.5°C, 4°C, 4.5°C, 5°C, 5.5°C, 6°C, 6.5°C, or 7°C, and the upper limit may be about 20°C, 18°C, 16°C, 14°C, 12°C, 10°C, 8°C, 6°C, 5°C, or 4°C. In relation to the absolute value of the mixing temperature and the melting point, when the curable composition contains a plurality of types of amorphous polar phase transition materials, the melting point may be the melting point of the phase transition material having the highest melting point among the plurality of polar phase transition materials. The absolute value of the difference between the mixing temperature and the melting point may be equal to or greater than any one of the lower limits described above, or equal to or less than any one of the upper limits described above, or equal to or greater than any one of the lower limits described above and equal to or less than any one of the upper limits described above. Through mixing within such a range, the phase transition material may exhibit a fluidity suitable for forming the desired semi-IPN.

[0138] The crystalline polar phase transition material having a melting point that is the basis for the difference with the curing temperature and / or mixing temperature may be a phase transition material having a linear structure and number average molecular weight as described above.

[0139] Such a phase transition material may be mixed in a molten state with the resin component. For example, the phase transition material may be maintained at a temperature equal to or higher than its melting point before being mixed with the resin component, and then mixed with the resin component. In this case, the method of melting the phase transition material is not particularly limited, and for example, the phase transition material may be maintained at a temperature equal to or higher than its melting point and melted. In one example, the temperature at which the phase transition material is maintained may be 10°C to 100°C higher than the melting point of the phase transition material. In other examples, the temperature may be 15°C or more, 20°C or more, 25°C or more, 30°C or more, 35°C or more, or 40°C or more higher than the melting point of the phase transition material, or 95°C or less, 90°C or less, 85°C or less, 80°C or less, 75°C or less, 70°C or less, 65°C or less, 60°C or less, 55°C or less, 50°C or less, 45°C or less, 40°C or less, 35°C or less, or 30°C or less lower than the melting point of the phase transition material.

[0140] By mixing the melted phase transition material and the resin component in such a temperature range to produce a curable composition, a curable composition having the desired properties can be efficiently produced. The temperature at which the melted phase transition material and the resin component are mixed may be within the same range as the temperature at which the phase transition material is melted, or may be lower than that. In one example, the mixing may be performed at a temperature 10°C to 100°C higher than the melting point of the phase transition material. In other examples, the temperature may be higher than the melting point of the phase transition material by 15°C or higher, 20°C or higher, 25°C or higher, 30°C or higher, 35°C or higher, or 40°C or higher, or may be lower than the melting point of the phase transition material by 95°C or lower, 90°C or lower, 85°C or lower, 80°C or lower, 75°C or lower, 70°C or lower, 65°C or lower, 60°C or lower, 55°C or lower, 50°C or lower, 45°C or lower, 40°C or lower, 35°C or lower, or 30°C or lower. Specifically, when the phase transition material and the resin component are mixed, the temperature during mixing may be about 40°C or more, 45°C or more, 50°C or more, 55°C or more, or 60°C or more, or 150°C or less, 140°C or less, 130°C or less, 120°C or less, 110°C or less, 100°C or less, 90°C or less, 80°C or less, or 70°C or less.

[0141] By curing the curable composition prepared as above in the above manner, a cured product having excellent flame retardancy, Shore A hardness and Tan δ within the desired range, and excellent vibration resistance and impact resistance can be prepared.

[0142] The cured body may be obtained by curing the curable composition according to one embodiment of the present invention. There is no limitation on the method of curing the curable composition to obtain a cured body, and an appropriate curing method may be applied according to the type of the curable composition. For example, in the case of an energy ray curing type, a method of irradiating the composition with energy rays such as ultraviolet rays, in the case of a moisture curing type, a method of maintaining the composition under appropriate humidity, in the case of a heat curing type, a method of applying appropriate heat to the composition, in the case of a room temperature curing type, a method of maintaining the composition at room temperature, and in the case of a hybrid curing type, a method of applying two or more curing methods may be used. As described above, in the appropriate examples, the curable composition may be a heat curing type. However, the curing may be performed at a temperature that indicates the difference between the curing temperature Tc and the melting point Tm described above.

[0143] The product according to an embodiment of the present invention may include the above-mentioned curable composition or a cured product of the curable composition. The curable composition according to an embodiment of the present invention or a cured product of the curable composition may be usefully applied as a material for controlling heat of a heat-generating part, a heat-generating element, or a heat-generating product. Thus, the product may include a heat-generating part, a heat-generating element, or a heat-generating product. The term "heat-generating part, element, or product" refers to a part, element, or product that generates heat during use, and the type thereof is not particularly limited. Representative heat-generating parts, elements, or products include various electric / electronic products including a battery cell, a battery module, or a battery pack.

[0144] The product according to one embodiment of the present invention may include, for example, the heat-generating part, element, or product, and the curable composition (or the two-liquid composition) or a cured product of the curable composition that is adjacent to the heat-generating part, etc. In such a case, as described above, the heat-generating part, element, or product may be a part, element, or product whose appropriate operating temperature is within the range of about 15°C to 60°C. That is, the curable composition of the present invention is disposed adjacent to the heat-generating part, element, or product, and is useful for maintaining the operating temperature of the product uniformly within the range.

[0145] The specific method for constructing the product according to an embodiment of the present invention is not particularly limited, and when the curable composition of the present invention or the curable composition is applied to a heat dissipation material, the product can be constructed in various known manners.

[0146] In one example, the curable composition can be used as a potting material when a battery module or a battery pack is constructed. The potting material may be a material that contacts and covers at least a part or all of a plurality of unit battery cells in a battery module or a battery pack. When the curable composition or the cured product of the curable composition of the present invention is applied to the potting material, it can control heat generated from a battery cell of a battery module or a pack, prevent chain fires or explosions, and maintain a uniform operating temperature of the module, pack, or battery cell. The present invention can also provide a curable composition that has excellent potting efficiency by controlling viscosity and thixotropy to an appropriate level before curing, and forms a stable potting structure without unnecessary air bubbles after curing. The present invention can provide a curable composition that shows low density after curing and can provide a battery module or pack that is lightweight compared to its volume but has high output. The present invention can also provide a curable composition that is excellent in required physical properties including insulation properties.

[0147] In this case, as a battery-related technology, the curable composition can be applied as a heat dissipation material of a battery module or a battery pack, or a heat dissipation material of an OBC (On Board Charger) for a vehicle. Therefore, the present invention may also relate to a battery module, a battery pack, or an on-board charger (OBC) including the curable composition or a cured body of the curable composition as a heat dissipation material. In the battery module, the battery pack, or the on-board charger, the application position or application method of the curable composition or the cured body of the curable composition is not particularly limited, and known methods can be applied. In addition, the curable composition of the present invention is not limited to the above applications, and can be effectively applied to various applications requiring excellent heat dissipation properties, storage stability, and adhesive strength.

[0148] In another embodiment of the present invention, the present invention may relate to an electronic device or apparatus having a cured product of the curable composition.

[0149] The type of electronic equipment or device is not particularly limited, and examples include audio video navigation (AVN) for vehicles, on board charger (OBC) modules for electric vehicles, LED modules, or IC chips and computers or mobile devices including the same.

[0150] The curable composition may be cured to dissipate heat within the equipment or device, and may provide impact resistance, insulation, etc. In one example, the curable composition may be used as a battery potting material.

[0151] The battery module according to an embodiment of the present invention is a battery module using the potting material described above. Such a battery module is lightweight and can exhibit high output, and the heat generated from the battery cells is appropriately controlled, so that problems such as chain fires do not occur.

[0152] In one example, the battery module may include a substrate, a plurality of battery cells disposed on the substrate, and the curable composition or a cured body of the curable composition covering at least a portion or all of the plurality of battery cells.

[0153] In the above structure, in one example, the curable composition or a cured body of the curable composition (potting material) may be in contact with the entire surfaces of the multiple battery cells (excluding the surfaces of the battery cells in contact with the substrate) and cover the battery cells (structure of Figure 1), or may be in contact with only the upper parts of the multiple battery cells (structure of Figure 2).

[0154] 1 and 2 are schematic diagrams of the structure of the battery module as described above, showing a structure including a substrate 10, a battery cell 20, and the potting material 30 (the curable composition or its cured product). The battery module may further include an adhesive material 40 that fixes the battery cell 20 to the substrate 10, and in one example, the adhesive material 40 may be configured to have thermal conductivity.

[0155] As long as the curable composition or its cured body is applied to a potting material, the specific configuration of the battery module, for example, the types of the battery cell, substrate and / or adhesive material, are not particularly limited, and known materials can be applied.

[0156] For example, the battery cell may be a known pouch-type, rectangular or cylindrical battery cell, and the substrate or adhesive material may be a known material.

[0157] The method for manufacturing the battery module is not particularly limited, and may be, for example, by pouring the curable composition onto a plurality of battery cells formed on a substrate, and curing the composition as necessary.

[0158] The curable composition according to one embodiment of the present invention has suitable viscosity and thixotropy, and therefore can efficiently fill spaces between battery cells arranged very close to each other, and can exhibit the desired thermal insulation and heat shielding properties after forming a potting material. Effect of the Invention

[0159] The present invention can provide a curable composition and its use. The present invention can provide a curable composition that is applied to a product or element that may generate heat, ignite, or explode during operation, storage, and / or maintenance, and can effectively respond to the heat, ignition, and explosion. For example, the composition of the present invention can be applied to an article including a plurality of such products or elements, and can respond to abnormal heat, explosion, and ignition generated from any one element or product, and can prevent or minimize the spread of such heat, explosion, and ignition to other adjacent elements or products. The present invention can also provide the curable composition such that excellent handling, storage stability, and flame retardancy are ensured. The curable composition or cured product of the present invention can also achieve the above properties by using a phase transition material that is not encapsulated, and can stably maintain the above properties for a long period of time. [Brief description of the drawings]

[0160] [Figure 1] FIG. 1 is a schematic diagram of an exemplary battery module of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an exemplary battery module of the present invention. [Diagram 3] FIG. 3 shows the results of DSC analysis of the cured body of Example 1. [Figure 4] FIG. 4 shows the results of DSC analysis of the cured body of Example 2. [Diagram 5] FIG. 5 shows the results of DSC analysis of the cured body of Example 3. [Figure 6] FIG. 6 shows the results of DSC analysis of the cured body of Example 4. [Figure 7] FIG. 7 shows the results of DSC analysis of the cured body of Comparative Example 2. [Figure 8] FIG. 8 shows the results of DSC analysis of the cured body of Comparative Example 4. [Figure 9] FIG. 9 shows the results of DSC analysis of the cured body of Comparative Example 5. [Figure 10] FIG. 10 shows the results of DSC analysis of the cured body of Comparative Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0161] The present invention will be described below based on examples and comparative examples, but the scope of the present invention is not limited to the contents presented below.

[0162] 1. Measurement of latent heat The latent heat was evaluated in the following manner. Approximately 3 to 5 mg of a sample (cured body or PCM (Phase Change Material)) was loaded into a DSC (Differential Scanning Calorimeter) device (TA Instruments, Q200 model). The temperature range for evaluating the latent heat of the device was set to -20°C to 200°C, and the endothermic section was measured while increasing the temperature at a rate of approximately 10°C / min. The endothermic peak confirmed in the endothermic section was integrated to calculate the latent heat (unit: J / g). The temperature at the inflection point of the left onset of the endothermic peak was defined as the start temperature of the latent heat section (left onset temperature), and the temperature at the inflection point of the right onset was defined as the end temperature of the latent heat section (right onset temperature). The width of the latent heat section was the value obtained by subtracting the onset temperature from the offset temperature. The melting point of the PCM was defined as the temperature at the apex of the endothermic peak.

[0163] 2. Leakage rate measurement The hardened bodies obtained in the Examples or Comparative Examples were cut to a width of about 1 cm, length of about 1 cm, and thickness of about 0.8 cm to prepare test pieces. Four test pieces were prepared for each hardened body. The initial weight m1 of the test pieces was measured, and the average of the four test pieces was recorded. Then, each test piece whose initial weight was measured was placed on filter paper and left in a chamber at 80°C for about 24 hours, after which the weight m2 was measured and the average of the four test pieces was recorded. Next, the leakage rate (L R ) to calculate

[0164] [Formula A] L R =100×(m1-m2) / m1

[0165] 3. Measurement of mass loss The hardened body of each of the Examples or Comparative Examples is cut to a width of about 1 cm, length of about 1 cm, and thickness of about 0.3 cm to prepare a test piece. The initial weight m3 of the test piece is measured and recorded. Next, the test piece whose initial weight has been measured is placed in distilled water and maintained at room temperature (about 25°C) for about 4 days, and then taken out and its weight m4 is measured. The weight m4 is the weight of the test piece measured after removing the moisture from the test piece taken out of the distilled water. The moisture is removed by wiping off the moisture on the surface of the test piece with absorbent cotton. Mass loss (M L ) is measured according to the following formula B.

[0166] [Formula B] M L =100×(m3-m4) / (m3×m5)

[0167] In formula B, m5 is the weight percentage of the PCM contained in the cured body which is the test piece, which means the weight percentage of the PCM contained in the cured body relative to the total weight of the cured body.

[0168] 4.Shore A hardness The Shore A hardness of the cured body of the Examples or Comparative Examples is measured according to the ASTM D2240 standard. An ASKER Durometer is used to measure the hardness. A load of about 1.5 kg is applied to the surface of a flat cured body (test piece), and the hardness is measured by checking the value that stabilizes after 15 seconds.

[0169] 5.Method of measuring Tan δ The cured product of the examples or comparative examples is cut to a width of about 8 mm, length of about 8 mm, and thickness of about 3 mm to prepare a test specimen. The specimen is loaded into a rotational rheometer ARES G2 (TA instrument, 8 mm aluminum plate, 25°C Frequency sweep) and the storage modulus (G') at room temperature (about 25°C) is measured under conditions of 5% strain and 0.95 Hz, and the loss modulus (G") at room temperature (about 25°C) is measured under conditions of 5% strain and 0.95 Hz.

[0170] Tan δ is defined by the following formula C.

[0171] [Formula C] Tanδ=G” / G'

[0172] 6. Flame retardancy evaluation The cured product of the Example or Comparative Example is cut to a width of about 13 mm, a length of about 125 mm, and a thickness of about 2 mm to prepare a test piece, and the flame retardancy is measured according to the UL94V standard. If the measurement result is V-0 or V-1 grade, it is evaluated as P (PASS), and if it is any other grade, it is evaluated as NG.

[0173] 7.GPC(Gel Permeation Chromatography) The molecular weight characteristics are measured using GPC (Gel permeation chromatography). The material to be analyzed is placed in a 5 mL vial and diluted with toluene to a concentration of about 5 mg / mL. Then, after filtering the calibration standard sample and the material to be analyzed through a syringe filter (pore size: 0.45 μm), the measurement is carried out. The analysis program uses the ChemStation of Agilent technologies. By comparing the elution time of the sample with the calibration curve, the weight average molecular weight (Mw) or the number average molecular weight (Mn) can be determined respectively.

[0174] The measurement conditions of GPC are as follows. <GPC measurement conditions> Equipment: 1200 series of Agilent technologies Columns: Two PLgel mixed B from Polymer laboratories are used Solvent: Toluene Column temperature: 40 °C Sample concentration: 5 mg / mL, 10 μL injection Standard sample: Polystyrene (Mp: 3900000, 723000, 316500, 52200, 31400, 7200, 3940, 485)

[0175] 8. Particle size analysis of the filler The particle size of the filler is measured in accordance with ISO-13320 using a MASTERSIZER 3000 device from Marven. Ethanol is used as the solvent during the measurement. As the particle size of the filler, the D50 particle size is measured and taken as the average particle size. The D50 particle size is the particle diameter (median diameter) at the 50% volume-based cumulative of the particle size distribution, which is obtained by taking the particle size distribution on a volume basis and is the particle diameter at the point where the cumulative value becomes 50% on the cumulative curve with the total volume as 100%.

[0176] Example 1. A silicone resin component (SL3000, KCC) (weight average molecular weight: about 28,000 g / mol) was used as the curable resin component, and a base part and a curing part were prepared in the following manner to prepare a two-liquid curable composition.

[0177] Base Parts The curable resin components, base (S), PCM (P) and filler (F) were mixed in a weight ratio of 100:91.7:92.6 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a base part. PEG (poly(ethylene glycol)) (PEG4000, Sigma Aldrich) was used as the PCM, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in producing the base part. Aluminum hydroxide (Al(OH)3) with an average particle size of about 50 μm was used as the filler. The PEG had a number average molecular weight (Mn) of about 4,000 g / mol, a melting point (Tm) of about 62.77°C as determined by Differential Scanning Calorimeter (DSC) analysis, a latent heat of about 164.3 J / g, a starting temperature of the latent heat interval of about 56.47°C, an end temperature of the latent heat interval of about 66.14°C, and therefore a width of the latent heat interval of about 9.67°C.

[0178] Hardener parts The curable resin components, curing agent (C), PCM (P) and filler (F) were mixed in a weight ratio of 100:91.7:92.6 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a curing agent part. The PCM and filler were the same as those used for the base part. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0179] hardened body The base part and the hardener part were placed in a bath in a weight ratio of 1:1 and stirred at about 380 rpm at 70° C. for about 60 minutes to be uniformly mixed to prepare a hardenable composition. The hardenable composition was maintained in a chamber at 60° C. for about 1 hour, and then applied to an aluminum dish with a syringe to a thickness of about 10 mm, and maintained at about 60° C. for about 30 minutes to prepare a hardened product.

[0180] Example 2. Base Parts The same curable resin components (SL3000, KCC) as in Example 1 were mixed with the base material (S), PCM (Phase Change Material) (P) and filler (F) in a weight ratio of 100:132:106 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a base part. The PCM was kept at a temperature of about 80°C for 1 hour to completely melt it, and then used to produce the base part. The PCM used was the same mixture of PEG, docosane (D, n-docosane), and eicosane (E, n-eicosane) as in Example 1, mixed in a weight ratio of 87.5:33.4:11.1 (PEG:D:E), and the filler used was aluminum hydroxide (Al(OH)3), as in Example 1. The docosane had a melting point (Tm) of about 44° C., a latent heat of about 170 J / g, a latent heat interval start temperature of about 41.53° C., and an end temperature of about 46.99° C., as measured by DSC (Differential Scanning Calorimeter) analysis. The eicosane had a melting point (Tm) of about 36° C., a latent heat of about 152 J / g, a latent heat interval start temperature of about 31.79° C., and an end temperature of about 38.96° C., as measured by DSC (Differential Scanning Calorimeter) analysis.

[0181] Hardener parts The same curing resin components (SL3000, KCC) as in Example 1, the curing agent (C), PCM (Phase Change Material) (P) and filler (F) were mixed in a weight ratio of 100:132:106 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a curing agent part. The PCM and filler were the same as those used in the base part in Example 2. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before use.

[0182] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0183] Example 3. Base Parts The base material (S) of the curable resin component (SL3000, KCC) of Example 1 and the PCM (P) (P) were mixed in a weight ratio of 100:61.3 (S:P) and stirred at 380 rpm for 60 minutes at 70°C to produce a base material part. The PCM used was the same PEG (poly(ethylene glycol)) (PEG4000, Sigma Aldrich) as in Example 1, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in producing the base material part.

[0184] Hardener parts The hardener (C) of the hardening resin component (SL3000, KCC) and PCM (P) (P) were mixed in a weight ratio of 100:61.3 (C:P) and stirred at 380 rpm for 60 minutes at 70°C to prepare a hardener part. The PCM was the same as that used for the base part. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0185] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0186] Example 4. A urethane resin component (KC-315A / KC-315B, Kangnam Chemical) (weight average molecular weight: about 2,500 g / mol) was used as the curable resin component, and a base part and a curing part were prepared in the following manner to prepare a two-liquid curable composition.

[0187] Base Parts The curable resin components, base (S), PCM (P) and filler (F) were mixed in a weight ratio of 100:95:95 (S:P:F) and stirred at 380 rpm for 60 minutes at 70° C. to produce a base part. The same PCM and filler as in Example 1 were used, and the PCM was maintained at a temperature of about 80° C. for 1 hour to completely melt it before being used in producing the base part.

[0188] Hardener parts The curable resin components, curing agent (C), PCM (P) and filler (F) were mixed in a weight ratio of 100:95:95 (C:P:F) and stirred at 380 rpm for 60 minutes at 70° C. to produce a cured part. The same PCM and filler as those in Example 1 were used, and the PCM was maintained at a temperature of about 80° C. for 1 hour to completely melt it before being used in producing the cured part.

[0189] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0190] Comparative Example 1 A cured body was prepared in the same manner as in Example 1 by mixing the base resin and curing agent of the same silicone resin component (SL3000, KCC) used in Example 1, except that no PCM or filler was used.

[0191] Comparative Example 2 Base Parts The base material (S) of the curable resin component (SL3000, KCC) of Example 1 and the PCM (P) (P) were mixed in a weight ratio of 100:62.6 (S:P) and stirred at 380 rpm for 60 minutes at 70°C to produce a base material part. The PCM used was n-docosane used in Example 2, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in producing the base material part.

[0192] Hardener parts The hardener (C) of the hardening resin component (SL3000, KCC) and PCM (P) (P) were mixed in a weight ratio of 100:62.6 (C:P) and stirred at 380 rpm for 60 minutes at 70°C to produce a hardener part. The PCM was the same n-docosane as the base part. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0193] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0194] Comparative Example 3. Base Parts The main component (S) of the curable resin component (SL3000, KCC), PCM (P) and filler (F) used in Example 1 were mixed in a weight ratio of 100:184:92.5 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C. The same PCM and filler as those used in Example 1 were used, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being applied to the mixing and stirring.

[0195] Hardener parts The curable resin components, curing agent (C), PCM (P) (P) and filler (F), were mixed in a weight ratio of 100:184:92.5 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C. The same PCM and filler as in Example 1 were used, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being mixed and stirred. However, in this case, the viscosity of the curing agent part increased excessively, causing uneven mixing of the components to a degree that could be observed with the naked eye, making mixing impossible, and therefore it was not possible to manufacture a curing agent part.

[0196] Comparative Example 4. Base Parts The same curable resin components (SL3000, KCC) as in Example 1 were mixed as the base material (S), PCM (Phase Change Material) (P), and filler (F) in a weight ratio of 100:132:106 (S:P:F) and stirred at 380 rpm for 60 minutes at room temperature (approximately 25°C) to produce a base material part. The PCM used was the same mixture of PEG, docosane (D, n-docosane), and eicosane (E, n-eicosane) as in Example 1, mixed in a weight ratio of 87.5:33.4:11.1 (PEG:D:E), and the filler used was aluminum hydroxide (Al(OH)3) as in Example 1. The docosane and eicosane used were the same as those in Example 2.

[0197] Hardener parts The same curing resin components (SL3000, KCC) as in Example 1 were mixed with the curing agent (C), PCM (Phase Change Material) (P) and filler (F) in a weight ratio of 100:132:106 (C:P:F) and stirred at 380 rpm for 60 minutes at room temperature (25°C) to produce a curing agent part. The PCM and filler were the same as those used in the base part of Example 2.

[0198] hardened body The base part and the hardener part were placed in a bath in a weight ratio of 1:1 and stirred at about 380 rpm for about 60 minutes to be uniformly mixed to prepare a hardenable composition. The hardenable composition was applied to an aluminum dish with a syringe to a thickness of about 10 mm and maintained at room temperature (about 25°C) to prepare a hardened product.

[0199] Comparative Example 5. Base Parts The base material (S) of the curable resin component (SL3000, KCC), PCM (P) and filler (F) of Example 1 were mixed in a weight ratio of 100:31.4:73.9 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C to manufacture a base material part. The PCM was a mixture of n-docosane (D) and eicosane (E) used in Example 2 in a weight ratio of 23.4:8.0 (D:E), and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in the manufacture of the base material part.

[0200] Hardener parts The curing agent (C) of the curable resin component (SL3000, KCC), PCM (P) (P) and filler (F) were mixed in a weight ratio of 100:31.4:73.9 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C to manufacture a curing agent part. The PCM was a mixture of n-docosane (D) and eicosane (E) used in Example 2 in a weight ratio of 23.4:8.0 (D:E). The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0201] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0202] Comparative Example 6. Base Parts The base material (S) of the curable resin component (SL3000, KCC) in Example 1, the PCM (P) (P) and the filler (F) were mixed in a weight ratio of 100:91.7:92.6 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a base material part. PEG (poly(ethylene glycol)) (PEG400, Sigma Aldrich) was used as the PCM, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in producing the base material part. The filler was the same aluminum hydroxide (Al(OH)3) as in Example 1. The PEG had a number average molecular weight (Mn) of about 400 g / mol, a melting point (Tm) of about 5.1°C as determined by Differential Scanning Calorimeter (DSC) analysis, a latent heat of about 116.2 J / g, a starting temperature of the latent heat interval of about -9.8°C, and an end temperature of the latent heat interval of about 6.3°C.

[0203] Hardener parts The hardener (C) of the hardening resin component (SL3000, KCC), PCM (Phase Change Material) (P) and filler (F) were mixed in a weight ratio of 100:91.7:92.6 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C to manufacture the hardener part. The PCM and filler were the same as those used for the base part. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0204] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part.

[0205] Comparative Example 7. Base Parts The base material (S) of the curable resin component (SL3000, KCC) of Example 1, the PCM (P) (P) and the filler (F) were mixed in a weight ratio of 100:91.7:92.6 (S:P:F) and stirred at 380 rpm for 60 minutes at 70°C to produce a base material part. As the PCM, PPG (poly(propylene glycol)) (PPG4000, Sigma Aldrich) was used, and the PCM was maintained at a temperature of about 80°C for 1 hour to completely melt it before being used in producing the base material part. The filler was the same aluminum hydroxide (Al(OH)3) as in Example 1. The PPG had a number average molecular weight (Mn) of about 4,000 g / mol. However, the PPG was found to be amorphous because no melting point was confirmed by DSC (Differential Scanning Calorimeter) analysis. In addition, no latent heat or latent heat interval was observed for the PPG.

[0206] Hardener parts The hardener (C) of the hardening resin component (SL3000, KCC), PCM (Phase Change Material) (P) and filler (F) were mixed in a weight ratio of 100:91.7:92.6 (C:P:F) and stirred at 380 rpm for 60 minutes at 70°C to manufacture the hardener part. The PCM and filler were the same as those used for the base part. The PCM was maintained at a temperature of about 80°C for 1 hour to completely melt before use.

[0207] hardened body A cured product was prepared in the same manner as in Example 1 using the base part and the curing agent part. The evaluation results for the Examples and Comparative Examples are summarized in the following Tables 1 and 2. Figures 3 to 10 show the DSC analysis results for the cured bodies of Examples 1 to 4, Comparative Examples 2, and 4 to 7, respectively. The DSC analysis results for Comparative Example 1, which does not contain PCM, and Comparative Example 3, in which it was impossible to produce a cured body due to incombination, were excluded.

[0208] In the following Tables 1 and 2, the Left onset temperature is the start temperature of the latent heat section, the Right onset temperature is the end temperature of the latent heat section, and G' is the storage modulus.

[0209] [Table 1]

[0210] [Table 2]

Claims

1. The resin component and the phase transition material are included. L in the following general formula 1 R A curable composition for forming a cured product having a Shore A hardness of 10 or less and a molecular weight of 5% or less: [General formula 1] L R =100×(m 1 -m 2 ) / m 1 In general formula 1, m 2 is the weight of the cured body after maintaining it at 80° C. for 24 hours, and m 1 is the weight of the cured body before being maintained at 80° C. for 24 hours.

2. The resin component and the phase transition material are included. A curable composition which forms a cured product having a Tan δ in the range of 0.15 to 2 according to the following general formula 2: [General formula 2] Tan δ=G″ / G′ In general formula 2, G' is the storage modulus of the cured material at 25°C, and G'' is the loss modulus of the cured material at 25°C.

3. The curable composition according to claim 1 or 2, wherein the cured product has a storage modulus at 25° C. of 0.2 MPa or more.

4. The curable composition according to claim 1 , wherein the resin component is a silicone resin component or a urethane resin component.

5. The curable composition according to claim 1 or 2, wherein the resin component is contained in an amount within a range of 30% by weight to 80% by weight.

6. The curable composition of claim 1 or 2, wherein the phase change material comprises a polar crystalline phase change material.

7. The curable composition of claim 1 or 2, wherein the phase change material comprises a polyalcohol.

8. The curable composition of claim 1 or 2, wherein the phase transition material comprises a polar phase transition material having a linear structure and a number average molecular weight in the range of 1,000 g / mol to 10,000 g / mol.

9. The curable composition of claim 1 or 2, wherein the phase transition material comprises a polyalkylene glycol.

10. 7. The curable composition of claim 6, comprising 40 to 180 parts by weight of the polar crystalline phase transition material per 100 parts by weight of the resin component.

11. The curable composition of claim 6 , wherein the phase transition material further comprises a non-polar phase transition material.

12. 12. The curable composition of claim 11, wherein the difference between the melting point of the polar crystalline phase transition material and the melting point of the non-polar phase transition material is in the range of 5°C to 50°C.

13. 12. The curable composition of claim 11 comprising 10 to 100 parts by weight of a non-polar phase transition material per 100 parts by weight of a polar crystalline phase transition material.

14. M in the following formula 3 L The curable composition according to claim 1 or 2, which forms a cured product having a content of 5% or less: [Formula 3] M L =100×(m 3 -m 4 ) / (m 3 ×m 5 ) In formula 3, m 4 is the weight of the cured body measured after immersing the cured body in water at 25° C. for 96 hours, and m 3 is the weight of the cured body before immersion in water at 25° C. for 96 hours, and m 5 is the weight m 3 is the weight ratio of the phase transition material contained in the hardened body.

15. curing a curable composition comprising a resin component and a phase transition material; A method for producing a cured product, wherein the curable composition is the curable composition according to claim 1 or 2.

16. The manufacturing method according to claim 15, wherein the phase transition material comprises a polar crystalline phase transition material, and the curing is carried out at a curing temperature in which the absolute value of the difference between the curing temperature Tc at the curing stage of the curable composition and the melting point Tm of the polar crystalline phase transition material is within a range of 0°C to 20°C.

17. The method for producing a curable composition according to claim 15, further comprising the step of mixing a resin component and a phase transition material to prepare a curable composition, the phase transition material including a polar crystalline phase transition material, and the mixing is carried out at a mixing temperature such that the absolute value of the difference between the mixing temperature Tx of the mixing step and the melting point Tm of the polar crystalline phase transition material is within a range of 0°C to 20°C.

18. The method for producing a cured body according to claim 17, further comprising mixing the resin component with a molten phase transition material.

19. The method for producing a hardened body according to claim 16, wherein the polar crystalline phase transition material has a linear structure and a number average molecular weight in the range of 1,000 g / mol to 10,000 g / mol.

20. A product comprising a heating element and a cured product of the curable composition according to claim 1 or 2 adjacent to the heating element.

Citation Information

Patent Citations

  • Dental curing composition

    JP2003040723A

  • Polymeric compositions incorporating polyethylene glycol as a phase change material

    US4825939A

  • Heat-storage composition

    WO2017221803A1

  • Electronic device and method of manufacturing an electronic device

    KR1020200135105A