CATALYST COMPOSITIONS AND PROCESSES FOR MAKING AND USING SAME - Patent application
Catalyst compositions with reduced Pt content and promoter elements on a Group 2 element support address the high cost issue of precious metal catalysts, achieving stable and efficient alkane and alkyl aromatic hydrocarbons reforming processes.
Patent Information
- Application Number
- JP2024533850
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-04-08
- Filing Date
- 2022-11-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-14
Smart Images

Figure 2024542826000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Application No. 63 / 286,312, having a filing date of December 06, 2021, and U.S. Provisional Application No. 63 / 329,042, having a filing date of April 08, 2022, the disclosures of both of which are incorporated herein by reference in their entireties.
[0002] Field The present disclosure relates to catalyst compositions and processes for making and using same. [Background technology]
[0003] background Catalytic reforming or dehydrogenation, dehydroaromatization, and / or dehydrocyclization of alkanes and / or alkylaromatic hydrocarbons are endothermic, equilibrium-limited, industrially important chemical conversion processes. Alkanes, e.g., C1-C 12 Reforming or dehydrogenation, dehydroaromatization, and / or dehydrocyclization of alkanes and / or alkyl aromatic hydrocarbons, such as ethylbenzene, can be carried out over a variety of different catalyst compositions, such as Pt-based, Ni-based, Pd-based, Ru-based, Re-based, Cr-based, Ga-based, V-based, Zr-based, In-based, W-based, Mo-based, Zn-based, and Fe-based systems. Precious metals used in catalysts are expensive and can contribute significantly to the capital and / or operating costs of a chemical plant. Thus, there is a need to reduce the concentrations of precious metals used in catalyst manufacture. The present disclosure meets this need and other demands. Summary of the Invention
[0004] summary Catalyst compositions and processes for making and using the same are provided. In some embodiments, the catalyst composition may include up to 0.025 wt% Pt and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof, disposed on a support. The support may include at least 0.5 wt% Group 2 element. All weight percentages are based on the weight of the support.
[0005] In some embodiments, a process for making a catalyst composition may include (I) preparing a slurry or gel that may include a Group 2 element-containing compound and a liquid medium. The process may also include (II) spray drying the slurry or gel to produce spray-dried particles that include the Group 2 element. The process may also include (III) calcining the spray-dried particles under an oxidizing atmosphere to produce calcined support particles that include the Group 2 element. The process may also include at least one of the following (i), (ii), and (iii): (i) the Pt is present in the slurry or gel in the form of a Pt-containing compound, and the catalyst composition may include catalyst particles comprising calcined support particles having Pt disposed thereon; (ii) the Pt can be deposited on the spray-dried particles by contacting the spray-dried particles with a Pt-containing compound to produce Pt-containing spray-dried particles, and the catalyst composition may include catalyst particles comprising calcined support particles having Pt disposed thereon; and (iii) the Pt can be deposited on the calcined support particles by contacting the calcined support particles with a Pt-containing compound to produce Pt-containing calcined support particles, and the process may further include the step of (IV) calcining the Pt-containing calcined support particles to produce re-calcined support particles having Pt disposed thereon, and the catalyst composition includes the re-calcined support particles. The process may also include at least one of the following (iv), (v), and (vi): (iv) the compound comprising the promoter element is present in the slurry or gel, and the catalyst composition may include catalyst particles comprising calcined support particles having the promoter element disposed thereon; (v) the compound comprising the promoter element may be deposited on spray-dried particles to produce promoter-containing spray-dried particles, and the catalyst composition may include catalyst particles comprising calcined support particles having the promoter element disposed thereon; and (vi) the compound comprising the promoter element may be deposited on calcined support particles to produce promoter-containing calcined support particles, and the process may further include (V) calcining the promoter-containing calcined support particles to produce recalcined support particles having the promoter element disposed thereon, and the catalyst composition includes the recalcined support particles. The promoter element may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof.The catalyst particles may include Pt in an amount of up to 0.025 wt% and a promoter element in an amount of up to 10 wt% based on the weight of the calcined or recalcined support particle. The catalyst particles may include at least 0.5 wt% of a Group 2 element based on the weight of the calcined or recalcined support particle.
[0006] In some embodiments, the hydrocarbon upgrading process may include (I) contacting a hydrocarbon-containing feed with a catalyst composition that may include Pt and a promoter disposed on a support to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that may include one or more upgraded hydrocarbons and molecular hydrogen. The hydrocarbon-containing feed may be one or more C2-C 16 Linear or branched alkanes, or one or more C4-C 16 Cyclic alkanes or one or more C8-C 16 The hydrocarbon-containing feed may include any C2-C4 alkyl aromatic hydrocarbons, or mixtures thereof. The hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature in the range of 300° C. to 900° C. for a time period of ≦3 hours under a hydrocarbon partial pressure of at least 20 kPa absolute. The hydrocarbon partial pressure is in the range of ≦20 kPa absolute for any C2-C4 alkyl aromatic hydrocarbons, or mixtures thereof. 16 Alkanes and any C8-C 16 is the total partial pressure of alkylaromatic hydrocarbons. The support may include at least 0.5 wt% of a Group 2 element based on the weight of the support. The catalyst composition may include up to 0.025 wt% Pt and up to 10 wt% promoter based on the weight of the support. The promoter may include Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof. The one or more upgraded hydrocarbons may include at least one of dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, and dehydrogenated cyclized hydrocarbons. [Brief description of the drawings]
[0007] [Figure 1] A catalyst composition (Catalyst 6) is shown that maintained its performance over 204 cycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Detailed Description Below, various specific embodiments, versions and examples of the present invention are described, including preferred embodiments and definitions adopted herein for the purpose of understanding the claimed invention. The detailed description below provides certain preferred embodiments, but those skilled in the art will recognize that these embodiments are merely exemplary and that the present invention can be practiced in other ways. For purposes of determining infringement, the scope of the present invention refers to any one or more of the appended claims, including their equivalents and elements or limitations that are equivalent to those recited. Any reference to the "invention" may refer to one or more, but not necessarily all, of the invention defined by the claims. In this disclosure, a process is described as including at least one "step." Each step should be understood to be an act or operation that may be performed once or multiple times in the process in a continuous or discontinuous manner. Unless otherwise specified or the context clearly indicates otherwise, the steps of the process may be performed consecutively in the order as described, with or without overlap with one or more other steps, or, in some cases, in any other order. Furthermore, one or more or even all steps may be performed simultaneously on the same or different batches of material. For example, in a continuous process, a first step of the process may be performed on raw material just fed at the beginning of the process, while a second step may be performed simultaneously on intermediate material resulting from processing of raw material fed to the process at an earlier point in the first step. Preferably, the steps are performed in the order described.
[0009] Unless otherwise indicated, all numbers indicating quantities in this disclosure should be understood to be modified in all cases by the term "about". It should also be understood that the exact numerical values used in the specification and claims constitute specific embodiments. Efforts have been made to ensure the accuracy of the data in the examples. However, it should be understood that any measured data inherently contains a certain level of error due to the limitations of the techniques and / or instruments utilized to make the measurements. Certain embodiments and features are described herein with a series of upper numerical limits and a series of lower numerical limits, and it should be understood that unless otherwise indicated, ranges including any combination of two values are contemplated, for example, any combination of a lower limit with any upper limit, any combination of two lower limits, and / or any combination of two upper limits. As used herein, the indefinite article "a" or "an" means "at least one" unless otherwise specified or the context clearly dictates otherwise. Thus, embodiments using "a reactor" or "a conversion zone" include embodiments using one, two, or more than two reactors or conversion zones, unless otherwise specified or the context clearly dictates that only one reactor or conversion zone is used.
[0010] The term "hydrocarbon" means (i) any compound consisting of hydrogen atoms and carbon atoms or (ii) any mixture of two or more of such compounds of (i). The term "Cn hydrocarbon" (where n is a positive integer) means (i) any hydrocarbon compound containing a total of n carbon atoms in its molecule or (ii) any mixture of two or more of such hydrocarbon compounds of (i). Thus, C2 hydrocarbons can be ethane, ethylene, acetylene, or any mixture in any ratio of at least two of these compounds. "Cm~Cn hydrocarbon" or "Cm-Cn hydrocarbon" (where m and n are positive integers and m < n) means any one of Cm, Cm+1, Cm+2,..., Cn-1, Cn hydrocarbons or any mixture of two or more of these. Thus, "C2~C3 hydrocarbon" or "C2-C3 hydrocarbon" can be any one of ethane, ethylene, acetylene, propane, propene, propyne, propadiene, cyclopropane, and any mixture in any ratio between any two or more of these components. "Saturated C2-C3 hydrocarbon" can be ethane, propane, cyclopropane, or any mixture in any ratio of two or more of these. "Cn+ hydrocarbon" means (i) any hydrocarbon compound containing at least n carbon atoms in total in its molecule or (ii) any mixture of two or more of such hydrocarbon compounds of (i). "Cn- hydrocarbon" means (i) any hydrocarbon compound containing a maximum of n carbon atoms in total in its molecule or (ii) any mixture of two or more of such hydrocarbon compounds of (i). "Cm hydrocarbon stream" means a hydrocarbon stream consisting essentially of Cm hydrocarbons. "Cm-Cn hydrocarbon stream" means a hydrocarbon stream consisting essentially of Cm-Cn hydrocarbons.
[0011] For the purposes of this disclosure, the nomenclature of the elements is that of Hawley's Condensed Chemical Dictionary, 16 thThe version of the Periodic Table of Elements (under the new notation) provided in Ed., John Wiley & Sons, Inc., (2016), Appendix V is based on the new notation. For example, Group 2 elements include Mg, Group 8 elements include Fe, Group 9 elements include Co, Group 10 elements include Ni, and Group 13 elements include Al. As used herein, the term "metalloid" refers to the following elements: B, Si, Ge, As, Sb, Te, and At. In this disclosure, when a given element is indicated as being present, it may be present in the elemental state or as any compound thereof, unless otherwise stated or the context clearly indicates otherwise. The term "alkane" means a saturated hydrocarbon. The term "cyclic alkane" means a saturated hydrocarbon that contains a cyclic carbon ring in its molecular structure. Alkanes can be straight-chained, branched, or cyclic. The term "aromatic" is to be understood in accordance with its art-recognized scope and includes alkyl substituted and unsubstituted mononuclear and polynuclear compounds. When used in expressions such as "X-rich" or "rich in X" with respect to an exit stream obtained from an apparatus, e.g., a conversion zone, the term "rich" means that the material X is present at a higher concentration than in the feed material supplied to the same apparatus from which the stream is withdrawn. When used in expressions such as "X-lean" or "lean in X" with respect to an exit stream obtained from an apparatus, e.g., a conversion zone, the term "lean" means that the material X is present at a lower concentration than in the feed material supplied to the same apparatus from which the stream is withdrawn.
[0012] The term "mixed metal oxide" refers to a composition that contains oxygen atoms and at least two different metal atoms that are intermixed on an atomic scale. For example, a "mixed Mg / Al metal oxide" has O, Mg, and Al atoms intermixed on an atomic scale and is substantially identical to the composition obtained by calcining Mg / Al hydrotalcite having the general chemical formula: [ka] where A is the counter anion of the negative charge n, x is in the range >0 to <1, and m is ≧0. A material consisting of nm-sized MgO particles and nm-sized Al2O3 particles mixed together is not a mixed metal oxide because the Mg and Al atoms are not mixed on the atomic scale, but on the nm scale.
[0013] The term "selectivity" refers to the production rate (in terms of moles of carbon) of a particular compound in a catalytic reaction. For example, the phrase "alkane hydrocarbon conversion reaction has 100% selectivity to olefinic hydrocarbons" means that 100% (in terms of moles of carbon) of the alkane hydrocarbons converted in the reaction are converted to olefinic hydrocarbons. When used in relation to a particular reactant, the term "conversion" refers to the amount of reactant consumed in the reaction. For example, when the particular reactant is propane, a conversion of 100% means that 100% of the propane is consumed in the reaction. In another example, when the particular reactant is propane, if 1 mole of propane is converted to 1 mole of methane and 1 mole of ethylene, the selectivity to methane is 33.3% and the selectivity to ethylene is 66.7%. The yield (in terms of moles of carbon) is the conversion x selectivity. In this disclosure, "A, B, ... or combinations thereof" means "A, B, ... or any combination of any two or more of A, B, ...", and "A, B, ... or mixtures thereof" means "A, B, ... or any mixture of any two or more of A, B, ...".
[0014] catalyst composition In some embodiments, the catalyst composition may include up to 0.025 wt% Pt disposed on the support, based on the weight of the support. In some embodiments, the catalyst composition may include from 0.001 wt%, 0.002 wt%, 0.003 wt%, 0.004 wt%, 0.005 wt%, 0.006 wt%, 0.007 wt%, 0.008 wt%, or 0.009 wt% to 0.01 wt%, 0.011 wt%, 0.012 wt%, 0.013 wt%, 0.014 wt%, 0.015 wt%, 0.016 wt%, 0.017 wt%, 0.018 wt%, 0.19 wt%, 0.02 wt%, 0.021 wt%, 0.022 wt%, 0.023 wt%, 0.024 wt%, or 0.025 wt% Pt disposed on the support based on the weight of the support. In some embodiments, the catalyst composition may also optionally include Ni, Pd, or a combination or mixture thereof disposed on a support. When Ni, Pd, a combination or mixture thereof is also disposed on a support, the catalyst composition may include from 0.001 wt%, 0.002 wt%, 0.003 wt%, 0.004 wt%, 0.005 wt%, 0.006 wt%, 0.007 wt%, 0.008 wt%, or 0.009 wt% to 0.01 wt%, 0.011 wt%, 0.012 wt%, 0.013 wt%, 0.014 wt%, 0.015 wt%, 0.016 wt%, 0.017 wt%, 0.018 wt%, 0.019 wt%, 0.020 wt%, 0.021 wt%, 0.022 wt%, 0.023 wt%, 0.024 wt%, 0.025 wt%, 0.026 wt%, 0.027 wt%, 0.028 wt%, 0.029 wt%, 0.030 wt%, 0.031 wt%, 0.032 wt%, 0.033 wt%, 0.034 wt%, 0.035 wt%, 0.036 wt%, 0.037 wt%, 0.038 wt%, 0.039 wt%, 0.040 wt%, 0.041 wt%, 0.042 wt%, 0.043 wt%, 0.044 wt%, 0.045 wt%, 0.046 wt%, 0.047 wt%, 0.048 wt%, 0.049 wt%, 0.050 wt%, 0.050 wt%, The catalyst composition may comprise a total amount of Pt and any Ni and / or any Pd disposed on the support of up to 0.013 wt%, 0.014 wt%, 0.015 wt%, 0.016 wt%, 0.017 wt%, 0.018 wt%, 0.019 wt%, 0.02 wt%, 0.021 wt%, 0.022 wt%, 0.023 wt%, 0.024 wt%, or 0.025 wt%. In some embodiments, the active component of the catalyst composition, which may be capable of effecting one or more of reforming or dehydrogenation, dehydroaromatization, and dehydrocyclization of a hydrocarbon-containing feed, may comprise Pt, or Pt and Ni and / or Pd.
[0015] In some embodiments, the catalyst composition may also include a promoter disposed on the support in an amount up to 10 wt%, based on the weight of the support. In some embodiments, the catalyst composition may include 0.01 wt%, 0.1 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, or 1 wt% to 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, or 10 wt%, based on the weight of the support, of a promoter disposed on the support. The promoter may be or include, but is not limited to, Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof. In some embodiments, the promoter may be associated with Pt and / or, if present, Ni and / or Pd. For example, the promoter and Pt disposed on the support may form Pt-promoter clusters that may be dispersed on the support. The promoter may improve the selectivity / activity / lifetime of the catalyst composition for a given upgraded hydrocarbon. In some embodiments, the promoter may improve the propylene selectivity of the catalyst composition when the hydrocarbon-containing feed includes propane.
[0016] In some embodiments, the catalyst composition may optionally include one or more alkali metal elements disposed on the support in an amount of up to 5 wt%, based on the weight of the support. In some embodiments, the catalyst composition may include 0.01 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, or 1 wt% to 2 wt%, 3 wt%, 4 wt%, or 5 wt% of the alkali metal elements disposed on the support, based on the weight of the support. The alkali metal elements, if present, may be or include, but are not limited to, Li, Na, K, Rb, Cs, or combinations or mixtures thereof. In at least some embodiments, the alkali metal elements may be or include K and / or Cs. In some embodiments, the alkali metal elements, if present, may improve the selectivity of the catalyst composition for a given upgraded hydrocarbon.
[0017] The carrier may be or include, but is not limited to, one or more group 2 elements, combinations thereof, or mixtures thereof. In some embodiments, the group 2 element may be present in its elemental form. In other embodiments, the group 2 element may be present in the form of a compound. For example, the group 2 element may be present as an oxide, phosphate, halide, halate, sulfate, sulfide, borate, nitride, carbide, aluminate, aluminosilicate, silicate, carbonate, metaphosphate, selenide, tungstate, molybdate, chromate, chromate, dichromate, or silicide. In some embodiments, a mixture of any two or more compounds containing a group 2 element may be present in different forms. For example, the first compound may be an oxide and the second compound may be an aluminate, and the first compound and the second compound contain the same or different group 2 elements from each other.
[0018] The carrier may be selected from the group consisting of ≧0.5wt%, ≧1wt%, ≧2wt%, ≧3wt%, ≧4wt%, ≧5wt%, ≧6wt%, ≧7wt%, ≧8wt%, ≧9wt%, ≧10wt%, ≧11wt%, ≧12wt%, ≧13wt%, ≧14wt%, ≧15wt%, ≧16wt%, ≧17wt%, ≧18wt%, ≧19wt%, ≧20wt%, ≧21wt%, based on the weight of the carrier. , ≧22wt%, ≧23wt%, ≧24wt%, ≧25wt%, ≧26wt%, ≧27wt%, ≧28wt%, ≧29wt%, ≧30wt%, ≧35wt%, ≧40wt%, ≧45wt%, ≧50wt%, ≧55wt%, ≧60wt%, ≧65wt%, ≧70wt%, ≧75wt%, ≧80wt%, ≧85wt%, or ≧90wt% of a Group 2 element. In some embodiments, the support may include a Group 2 element in a range from 0.5 wt%, 1 wt%, 2 wt%, 2.5 wt%, 3 wt%, 5 wt%, 7 wt%, 10 wt%, 11 wt%, 13 wt%, 15 wt%, 17 wt%, 19 wt%, 21 wt%, 23 wt%, or 25 wt% to 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or 92.34 wt%, based on the weight of the support. In some embodiments, the molar ratio of Group 2 element to Pt or Pt and any Ni and / or Pd present is 0.24, 0.5, 1, 10, 50, 100, 300, 450, 600, 800, 1,000, 1,200, 1,500, 1,700, or 2,000 to 3,000, 3,500, 4,000, 4,500, 5,000, 5,500, 6,000, 6,500, 7,000, 7,500, 8,000, 8,500, 9,000, 9,500, 10 The range may be up to 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, or 900,000.
[0019] In some embodiments, the support may include a group 2 element and Al, and may be in the form of a mixed group 2 element / Al metal oxide with O, Mg, and Al atoms mixed on an atomic scale. In some embodiments, the support may be or include a group 2 element and Al in the form of an oxide, or one or more oxides of group 2 elements and Al2O3 that may be mixed on a nm scale. In some embodiments, the support may be or include an oxide of a group 2 element, for example, MgO, and Al2O3 mixed on a nm scale. In some embodiments, the support may be or include a first amount of Group 2 element and Al in the form of a mixed Group 2 element / Al metal oxide and a second amount of Group 2 element in the form of an oxide of the Group 2 element, in which the mixed Group 2 element / Al metal oxide and the oxide of the Group 2 element may be mixed on the nm scale, and the Group 2 element and Al in the mixed Group 2 element / Al metal oxide may be mixed on an atomic scale. In other embodiments, the support may be or include a first amount of Group 2 element and a first amount of Al in the form of a mixed Group 2 element / Al metal oxide, a second amount of Group 2 element in the form of an oxide of the Group 2 element, and a second amount of Al in the form of Al2O3, in which the mixed Group 2 element / Al metal oxide, the oxide of the Group 2 element, and Al2O3 may be mixed on the nm scale, and the Group 2 element and Al in the mixed Group 2 element / Al metal oxide may be mixed on an atomic scale.
[0020] In some embodiments, when the support comprises a Group 2 element and Al, the mass ratio of the Group 2 element to Al in the support can be in the range from 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.2, 0.3, 0.5, 0.7, or 1 to 3, 6, 12.5, 25, 50, 75, 100, 200, 300, 400, 500, 600, 700, 800, 900, or 1,000. In some embodiments, when the support comprises Al, the inorganic support may comprise Al in the range of 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.1 wt%, 2.3 wt%, 2.5 wt%, 2.7 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, or 11 wt% to 15 wt%, 20 wt%, 25 wt%, 30 wt%, 40 wt%, 45 wt%, or 50 wt% based on the weight of the support. In some embodiments, the group 2 element may include Mg, and at least a portion of the group 2 element may be in the form of MgO or in the form of a mixed metal oxide including Mg. In some embodiments, the support may be or include, but is not limited to, a mixed Mg / Al metal oxide. In some embodiments, the support may be or include a mixed Mg / Al metal oxide produced or obtained by calcining hydrotalcite. In some embodiments, the support may be or include a mixed Mg / Al metal oxide produced or obtained by calcining hydrotalcite, but having the same or similar structure as the compound produced via other alternative processes. In some embodiments, when the support is a mixed Mg / Al metal oxide, the support may have a mass ratio of Mg to Al ranging from 0.001, 0.005, 0.01, 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5 to 6, 10, 12.5, 25, 50, 75, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, or 1,000.
[0021] In some embodiments, the carrier may be or include, but is not limited to, one or more of the following compounds: Mg w AlO3+w (w is a positive number), Ca x AlO 3+x (x is a positive number), Sr y AlO 3+y (y is a positive number), Ba z AlO 3+z (z is a positive number), BeO, MgO, CaO, BaO, SrO, BeCO3, MgCO3, CaCO3, SrCO3, BaCO3, CaZrO3, Ca7ZrAl6O 18 , CaTiO3, Ca7Al6O 18 , Ca7HfAl6O 18 , BaCeO3, one or more magnesium chromates, one or more magnesium tungstates, one or more magnesium molybdates, combinations thereof, and / or mixtures thereof.
[0022] Mg w AlO 3+w (w is a positive number), when present as a support or as a component of a support, may have a molar ratio of Mg to Al ranging from 0.5, 1, 2, 3, 4, or 5 to 6, 7, 8, 9, or 10. In some embodiments, Mg w AlO 3+w may include MgAl2O4, Mg2Al2O5, or a mixture thereof. x AlO 3+x (x is a positive number), when present as a support or as a component of a support, may have a molar ratio of Ca to Al in the range of 1:12, 1:4, 1:2, 2:3, 5:6, 1:1, 12:14, or 1.5:1. x AlO 3+x may include tricalcium aluminate, dodecalcium heptaaluminate, monocalcium aluminate, monocalcium dialuminate, monocalcium hexaaluminate, dicalcium aluminate, pentacalcium trialuminate, tetracalcium trialuminate, or any mixture thereof. y AlO 3+y (y is a positive number), when present as a support or as a component of a support, may have a molar ratio of Sr to Al ranging from 0.05, 0.3, or 0.6 to 0.9, 1.5, or 3. z AlO3+z (z is a positive number) may have a molar ratio of Ba to Al ranging from 0.05, 0.3, or 0.6 to 0.9, 1.5, or 3 when present as a support or as a component of a support.
[0023] In some embodiments, the support may also include at least one metal element and / or at least one metalloid element selected from a group other than, but not limited to, Group 2 and Group 10, and / or at least one compound thereof, where the at least one metal element and / or at least one metalloid element is not Li, Na, K, Rb, Cs, Sn, Cu, Au, Ag, or Ga. When the support also comprises a compound comprising a metal element and / or a metalloid element selected from a group other than Groups 2 and 10 (wherein the at least one metal element and / or the at least one metalloid element is not Li, Na, K, Rb, Cs, Sn, Cu, Au, Ag, or Ga), the compound may be present in the support as an oxide, phosphate, halide, halate, sulfate, sulfide, borate, nitride, carbide, aluminate, aluminosilicate, silicate, carbonate, metaphosphate, selenide, tungstate, molybdate, chromate, chromate, dichromate, or silicide. In some embodiments, the at least one metallic element and / or at least one metalloid element selected from a group other than Group 2 and Group 10 (wherein the at least one metallic element and / or at least one metalloid element is not Li, Na, K, Rb, Cs, Sn, Cu, Au, Ag, or Ga) can be or include, without limitation, one or more rare earth elements, i.e., elements having an atomic number of 21, 39, or 57-71.
[0024] When the support comprises at least one metal element and / or at least one metalloid element selected from a group other than Group 2 and Group 10 and / or at least one compound thereof (wherein the at least one metal element and / or at least one metalloid element is not Li, Na, K, Rb, Cs, Sn, Cu, Au, Ag, or Ga), the at least one metal element and / or at least one metalloid element may function as a binder in some embodiments and may be referred to as a "binder." Furthermore, for clarity and ease of explanation, the at least one metal element and / or at least one metalloid element selected from a group other than Group 2 and Group 10 will be described herein as a "binder," regardless of whether the at least one metal element and / or at least one metalloid element selected from a group other than Group 2 and Group 10 and / or at least one compound thereof (wherein the at least one metal element and / or at least one metalloid element is not Li, Na, K, Rb, Cs, Sn, Cu, Au, Ag, or Ga). In some embodiments, the support may comprise from 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.5 wt%, 1 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or 40 wt% to 50 wt%, 60 wt%, 70 wt%, 80 wt%, or 90 wt% of a binder based on the weight of the support.
[0025] In some embodiments, suitable compounds that can be used as binders include, but are not limited to, the following: B2O3, AlBO3, Al2O3, SiO2, ZrO2, TiO2, SiC, Si3N4, aluminosilicates, zinc aluminate, ZnO, VO, V2O3, VO2, V2O5, Ga s O t , In u O v, Mn2O3, Mn3O4, MnO, one or more molybdenum oxides, one or more tungsten oxides, one or more zeolites (s, t, u, and v are positive numbers), and mixtures and combinations thereof. When the Group 2 element is in the form of a mixed metal oxide, e.g., a mixed Mg / Al metal oxide, the additional metal(s) in the mixed metal oxide are not considered part of the binder. For example, the support may include a mixed Mg / Al metal oxide, such as that obtained by calcining Mg / Al hydrotalcite, and a binder that is Al2O3.
[0026] Surprisingly and unexpectedly, it has been found that the amount of Pt or the amount of Pt and Ni and / or Pd disposed on a support can be significantly reduced from the amount thought to be necessary to produce a catalyst composition with sufficient activity. More specifically, it has been surprisingly and unexpectedly found that the amount of Pt or the amount of Pt and Ni and / or Pd disposed on a support containing at least 0.5 wt% of a Group 2 element can be ≦0.025 wt% and still maintain a sufficient level of activity. This was not thought to be possible. The conventional view was that the amount of Pt or the amount of Pt and Ni and / or Pd needed to be at least 0.05 wt% based on the weight of the support. See, for example, U.S. Patent Nos. 6,967,182; 5,922,925; 6,582,589; 6,313,063 and 5,817,596; U.S. Patent Application Publication Nos. 2003 / 0139637; 2004 / 0029729; 2005 / 0003960; and European Patent Application Nos. EP1016641 and EP1073516.
[0027] In some embodiments, the catalyst composition may include 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.015 wt%, 0.02 wt%, 0.025 wt%, 0.03 wt%, 0.06 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, or 1 wt% to 2 wt%, 3 wt%, 4 wt%, 5 wt%, or 6 wt% Pt or Pt and Ni and / or Pd disposed on a support containing at least 0.5 wt% Group 2 element, where all weight percentages are based on the weight of the support and the promoter is optional. In such embodiments, at least a portion of the Group 2 element in the support may be in the form of a mixed Group 2 element / Al metal oxide. It has been surprisingly and unexpectedly found that when at least a portion of the Group 2 element in the support is in the form of a mixed Group 2 / Al metal oxide, the presence of Si in the catalyst composition in an amount of 0.1 wt% or more adversely affects the stability of the catalyst performance. For example, when the support comprises a mixed Mg / Al metal oxide, the presence of Si in an amount of 0.1 wt% or more adversely affects the stability of the catalyst performance. Thus, when at least a portion of the Group 2 element in the support is in the form of a mixed Group 2 / Al metal oxide when the promoter is optional, the catalyst composition may contain <0.1 wt%, <0.09 wt%, <0.08 wt%, <0.07 wt%, <0.06 wt%, <0.05 wt%, <0.04 wt%, <0.03 wt%, <0.02 wt%, <0.01 wt%, <0.007 wt%, <0.005 wt%, or <0.001 wt% Si. In other embodiments, when at least a portion of the Group 2 element in the support is in the form of a mixed Group 2 / Al metal oxide when the promoter is optional, the catalyst composition may not contain any Si. However, in other embodiments, where the promoter is optional, at least a portion of the Group 2 element in the support may be in the form of a mixed Group 2 element / Al metal oxide, and the catalyst composition may contain <0.1 wt%, <0.09 wt%, <0.08 wt%, <0.07 wt%, <0.06 wt%, <0.05 wt%, <0.04 wt%, <0.03 wt%, <0.02 wt%, <0.01 wt%, <0.007 wt%, <0.005 wt%, or <0.001 wt% Al.
[0028] In some embodiments, the catalyst composition may be in the form of catalyst particles or a monolithic structure. When the catalyst composition is in the form of catalyst particles, the catalyst particles may have a median particle size ranging from 1 μm, 5 μm, 10 μm, 20 μm, 40 μm, or 60 μm to 80 μm, 100 μm, 115 μm, 130 μm, 150 μm, 200 μm, 300 μm, or 400, or 500 μm. The catalyst particles may have a median particle size of 0.3 g / cm, as measured according to ASTM D7481-18, modified using 10, 25, or 50 mL graduated cylinders instead of 100 or 250 mL graduated cylinders. 3 , 0.4g / cm 3 , 0.5g / cm 3 , 0.6g / cm 3 , 0.7g / cm 3 , 0.8g / cm 3 , 0.9g / cm 3 , or 1g / cm 3 from 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , or 2 g / cm 3 In some embodiments, the catalyst composition may have an apparent loose bulk density ranging from ≦5 wt%, ≦4 wt%, ≦3 wt%, ≦2 wt%, ≦1 wt%, ≦0.7 wt%, ≦0.5 wt%, ≦0.4 wt%, ≦0.3 wt%, ≦0.2 wt%, ≦0.1 wt%, ≦0.07 wt%, or ≦0.05 wt% attrition loss after 1 hour, measured according to ASTM D5757-11(2017). The morphology of the particles may be predominantly spherical, making them suitable for moving around in a fluidized bed reactor. In some embodiments, the catalyst composition may have a size and density consistent with the Geldart A or Geldart B definition of a flowable solid.
[0029] In some embodiments, the catalyst composition is 2 / g, 1m 2 / g, 10m 2 / g, or 100m 2 / g to 500m 2 / g, 800m 2 / g, 1,000m 2 / g, or 1,500m 2 The surface area of the catalyst composition can be measured according to the Brunauer-Emmett-Teller (BET) method using nitrogen adsorption-desorption (temperature of liquid nitrogen, -196°C (77K)) on a Micromeritics 3flex instrument after degassing the powder at 350°C for 4 hours. More information on this method can be found, for example, in "Characterization of Porous Solids and Powders: Surface Area, Pore Size and Density," S. Lowell et al., Springer, 2004.
[0030] First manufacturing process of catalyst particles The process for preparing the catalyst composition may include a step of preparing a slurry or gel, which may include, but is not limited to, milling, mixing, blending, mixing, or otherwise contacting a group 2 element-containing compound and a liquid medium. In some embodiments, the preparation of the slurry or gel may also include, but is not limited to, contacting a group 2 element-containing compound, a liquid medium, and one or more additives. In other embodiments, the preparation of the slurry or gel may include, but is not limited to, contacting a group 2 element-containing compound, a liquid medium, a binder or binder precursor, and, optionally, one or more additives. The Group 2 element-containing compound may be in the form of an oxide, hydroxide, hydrated carbonate, salt, Group 2 element-containing clay, layered double hydroxide, phosphate, halide, halate, sulfate, sulfide, borate, nitride, carbide, aluminate, aluminosilicate, silicate, carbonate, metaphosphate, selenide, tungstate, molybdate, chromate, chromate, dichromate, silicide, or mixtures thereof. In some embodiments, the Group 2 element may be or include Mg, and the Group 2 element-containing compound may be in the form of magnesium oxide, magnesium hydroxide, hydromagnesite (hydrated magnesium carbonate mineral, Mg5(CO3)4(OH)2·4H2O), magnesium salt, magnesium-containing clay, hydrotalcite (layered double hydroxide), organomagnesium compound, or mixtures thereof.
[0031] The liquid medium may be or include, but is not limited to, water, alcohol, acetone, chloroform, methylene chloride, dimethylformamide, dimethylsulfoxide, glycerin, ethyl acetate, or any mixture thereof. Illustrative alcohols may be or include, but are not limited to, methanol, ethanol, isopropanol, or any mixture thereof. The binder, if present, may be or include the binders described above. The binder precursor, if present, may be or include, but is not limited to, Al2Si2O5(OH)4 (kaolin clay), aluminum chlorohydrol, boehmite, pseudoboehmite, gibbsite, bayerite, aluminum nitrate, aluminum chloride, sodium aluminate, alumina sol, silica sol, or any mixture thereof. In the literature, it is known that compounds referred to herein as "binders" may also be referred to as fillers, matrices, additives, etc. The one or more additives, if present, may be or include, but are not limited to, acids such as formic acid, lactic acid, citric acid, acetic acid, HNO3, HCl, oxalic acid, stearic acid, carbonic acid, etc.; bases such as ammonia solution, NaOH, KOH, etc.; inorganic salts such as nitrates, carbonates, bicarbonates, chlorides, etc.; organic salts such as acetates, oxalates, formates, citrates, etc.; polymers such as polyvinyl alcohol, polysaccharides, etc., or any mixture thereof. The additives may help to improve the chemical / physical properties of the spray dried material and / or help to improve the rheological properties of the slurry / gel to facilitate spray drying.
[0032] The slurry or gel can be spray dried to produce spray-dried particles containing group 2 elements. Spray drying refers to the process of producing a dry particulate solid product from the slurry or gel. The process can include spraying or atomizing the slurry or gel, for example, forming small droplets in a temperature-controlled gas stream to evaporate the liquid medium from the atomized droplets and produce the particulate solid product. For example, in a spray drying process, the slurry or gel can be atomized into small droplets and mixed with hot air or a hot inert gas, for example, nitrogen, to evaporate the liquid from the droplets. The temperature of the slurry or gel during the spray drying process can usually be close to or higher than the boiling temperature of the liquid. An outlet air temperature of about 60°C to about 120°C can be typical. The slurry or gel may be atomized with one or more pressure nozzles (e.g., fluid nozzle atomizers), one or more pulse atomizers, one or more high speed rotating disks (e.g., centrifugal or rotary atomizers), or any other known process. The median particle size, liquid (e.g., water) concentration, apparent loose bulk density, or any combination thereof, of the particulate solid product prepared by spray drying may be controlled, adjusted, or otherwise influenced by one or more operating conditions and / or parameters of the spray dryer. Illustrative operating conditions include, but are not limited to, the feed rate and temperature of the gas stream, the atomizer speed, the feed rate of the slurry or gel through the atomizer, the temperature of the slurry or gel, the droplet size and solids concentration, the dimensions of the spray dryer, or any combination thereof. It is well known in the art that the various operating conditions vary depending on the particular spray drying equipment used and can be readily determined by one of ordinary skill in the art.
[0033] The spray-dried particles can optionally be calcined under an oxidizing atmosphere, e.g., air, to produce calcined support particles comprising a Group 2 element. In some embodiments, the spray-dried particles can be calcined at a temperature ranging from 450°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, or 675°C to 700°C, 725°C, 750°C, 775°C, 800°C, 850°C, 900°C, or 950°C. In some embodiments, the spray-dried particles can be calcined at a temperature of ≦950°C, ≦900°C, ≦850°C, ≦800°C, ≦750°C, ≦700°C, ≦650°C, ≦600°C, or ≦550°C, ≦525°C, ≦500°C, ≦475°C, or ≦460°C. In some embodiments, the spray-dried particles may be calcined for a time period of ≦240 min, ≦180 min, ≦120 min, ≦90 min, ≦60 min, ≦45 min, ≦30 min, ≦25 min, ≦20 min, or ≦15 min. In some embodiments, the spray-dried particles may be calcined in the presence of oxygen, e.g., air. In some embodiments, the spray-dried particles may be calcined at a temperature ranging from 550° C. to 900° C. or 550° C. to 850° C. for a time period of ≦240 min, ≦180 min, ≦120 min, ≦90 min, ≦60 min, ≦45 min, ≦30 min, ≦25 min, ≦20 min, or ≦15 min. In other embodiments, the spray-dried particles may be calcined at temperatures of ≦550° C., ≦540° C., ≦530° C., ≦520° C., ≦510° C., or ≦500° C. for times of ≦240 minutes, ≦180 minutes, ≦120 minutes, ≦90 minutes, ≦60 minutes, ≦45 minutes, ≦30 minutes, ≦25 minutes, ≦20 minutes, or ≦15 minutes.
[0034] The Pt present in the catalyst particles can be introduced by one or more methods. In some embodiments, the process for making the catalyst composition can include (i) contacting at least a Group 2 element-containing compound and a liquid medium with a Pt-containing compound such that the Pt can be present in a slurry or gel, in which case the catalyst composition can include catalyst particles including calcined support particles having Pt disposed thereon. In other embodiments, the process for making the catalyst composition can include (ii) depositing Pt on the spray-dried particles by contacting the spray-dried particles with a Pt-containing compound to produce Pt-containing spray-dried particles, in which case the catalyst composition can include catalyst particles including calcined support particles having Pt disposed thereon. In other embodiments, the process for making the catalyst composition can include (iii) depositing Pt on the calcined support particles to produce Pt-containing calcined support particles if the spray-dried particles are optionally calcined by contacting the calcined support particles with a Pt-containing compound, in which case the process can further include optionally calcining the Pt-containing calcined support particles to produce re-calcined support particles having Pt disposed thereon, in which case the catalyst composition can include re-calcined support particles. In some embodiments, the catalyst composition can include Pt-containing calcined support particles without an optional additional calcination step. In other embodiments, the process for preparing the catalyst composition can include options (i), (ii), (iii), (i) and (ii), (i) and (iii), (ii) and (iii), or (i), (ii), and (iii). The Pt-containing compound can be or include, but is not limited to, chloroplatinic acid hexahydrate, tetraammineplatinum(II) nitrate, platinum(II) acetylacetonate, platinum(II) bromide, platinum(II) iodide, platinum(II) chloride, platinum(IV) chloride, platinum(II) diammine dichloride, ammonium tetrachloroplatinate(II), tetraammineplatinum(II) chloride hydrate, tetraammineplatinum(II) hydroxide hydrate, or any mixture thereof.
[0035] The promoter present in the catalyst particle can be introduced by one or more methods. In some embodiments, the process for making the catalyst composition can include (iv) contacting at least a Group 2 element-containing compound and a liquid medium with a compound containing a promoter element such that the promoter element is present in a slurry or gel, in which case the catalyst composition can include catalyst particles including calcined support particles having a promoter element disposed thereon. In other embodiments, the process for making the catalyst composition can include (v) depositing a compound containing a promoter element onto a spray-dried particle to produce a promoter-containing spray-dried particle, in which case the catalyst composition can include catalyst particles including calcined support particles having a promoter element disposed thereon. In other embodiments, the process for making the catalyst composition can include (vi) depositing a compound containing a promoter element onto a calcined support particle to produce a promoter-containing calcined support particle if the spray-dried particle is optionally calcined, in which case the process can further include calcining the promoter-containing calcined support particle to produce a re-calcined support particle having a promoter element disposed thereon, in which case the catalyst composition includes a re-calcined support particle. In some embodiments, the catalyst composition can include promoter-containing calcined support particles without the optional additional calcination step. In other embodiments, the process for making the catalyst composition may include options (iv), (v), (vi), (iv) and (v), (iv) and (vi), (v) and (vi), or (iv), (v), and (vi). In other embodiments, the process may include any one or more of options (i), (ii), and (iii) and any one or more of options (iv), (v), and (iv). The compound containing the promoter element may be or include, but is not limited to, tin(II) oxide, tin(IV) oxide, tin(IV) chloride pentahydrate, tin(II) chloride dihydrate, tin(II) bromide, tin(IV) bromide, tin(II) acetylacetonate, tin(II) acetate, tin(IV) acetate, tin(IV) oxalate, silver(I) nitrate, gold(III) nitrate, copper(II) nitrate, gallium(III) nitrate, or any mixture thereof.
[0036] The alkali metal element, if present in the catalyst particles, can be introduced by one or more methods. In some embodiments, the process for making the catalyst composition can include (vii) contacting at least a Group 2 element-containing compound and a liquid medium with a compound containing an alkali metal element such that the alkali metal element is present in a slurry or gel, in which case the catalyst composition can include catalyst particles including calcined support particles having an alkali metal element disposed thereon. In other embodiments, the process for making the catalyst composition can include (viii) depositing a compound containing an alkali metal element onto a spray-dried particle to produce an alkali metal element-containing spray-dried particle, in which case the catalyst composition can include catalyst particles including calcined support particles having an alkali metal element disposed thereon. In other embodiments, the process for making the catalyst composition can include (ix) depositing a compound containing an alkali metal element onto a calcined support particle to produce an alkali metal element-containing calcined support particle, in which case the spray-dried particle is optionally calcined, in which case the process can further include calcining the alkali metal element-containing calcined support particle to produce a re-calcined support particle having an alkali metal element disposed thereon, in which case the catalyst composition includes a re-calcined support particle. In other embodiments, the process for preparing the catalyst composition may include options (vii), (viii), (ix), (vii) and (viii), (vi) and (ix), (viii) and (ix), or (vii), (viii), and (iv). In other embodiments, the process may include any one or more of options (i), (ii), and (iii), any one or more of options (iv), (v), and (iv), and any one or more of options (vii), (viii), and (ix). The compound containing an alkali metal element may be or include, but is not limited to, lithium nitrate, sodium nitrate, potassium nitrate, rubidium nitrate, cesium nitrate, or any mixture thereof.
[0037] In some embodiments, the process for making the catalyst composition may optionally include hydrating the calcined support particles to produce hydrated support particles. For example, the calcined support particles may be contacted with water to produce hydrated support particles. In such embodiments, the process may also include calcining the hydrated support particles to produce the catalyst composition comprising the recalcined support particles. The hydration of the calcined support may be performed at a temperature ranging from 20° C., 40° C., or 60° C. to 80° C., 120° C., 140° C., 160° C., 180° C., or 200° C. The calcined support may be contacted with water for a time ranging from 1 minute, 5 minutes, or 10 minutes to 20 minutes, 40 minutes, 80 minutes, 160 minutes, 6 hours, 12 hours, 24 hours, or 48 hours. In some embodiments, anions, such as chloride, nitrate, carbonate, bicarbonate, acetate, oxalate, formate, and / or citrate ions, may be present during hydration. In some embodiments, the process for making the catalyst composition may optionally include hydrating the spray-dried particles to produce hydrated spray-dried particles. For example, the spray-dried particles may be contacted with water to produce hydrated spray-dried particles. In such embodiments, the process may also include calcining the hydrated spray-dried particles to produce the catalyst composition comprising the calcined support particles. The hydration of the spray-dried particles may be carried out at a temperature ranging from 20° C., 40° C., or 60° C. to 80° C., 120° C., 140° C., 160° C., 180° C., or 200° C. The spray-dried particles may be contacted with water for a time ranging from 1 minute, 5 minutes, or 10 minutes to 20 minutes, 40 minutes, 80 minutes, 160 minutes, 6 hours, 12 hours, 24 hours, or 48 hours. In some embodiments, anions such as chloride, nitrate, carbonate, bicarbonate, acetate, oxalate, formate, and / or citrate ions may be present during hydration.
[0038] In some embodiments, the process for making the catalyst composition may optionally include hydrating spray-dried particles to produce hydrated spray-dried particles, calcining the hydrated spray-dried particles to produce calcined support particles, hydrating the calcined support particles to produce hydrated calcined support particles, and calcining the hydrated calcined support particles to produce re-calcined support particles. As a result, the catalyst composition may include spray-dried particles, calcined support particles, hydrated spray-dried particles, hydrated spray-dried particles that can be calcined, hydrated calcined support particles, hydrated calcined support particles that can be re-calcined, or any mixture thereof. In some embodiments, particles of catalyst produced by hydrating the calcined support particles or spray-dried particles and then calcining the hydrated calcined support particles or hydrated spray-dried particles can result in catalyst particles having an attrition loss after 1 hour, measured according to ASTM D5757-11(2017), that is less than the attrition loss after 1 hour of the initial calcined particles or spray-dried particles produced before the hydration step. In some embodiments, particles of catalyst produced by hydrating the calcined support particles or spray-dried particles and then calcining the hydrated support particles or hydrated support particles can result in catalyst particles having an attrition loss after 1 hour, measured according to ASTM D5757-11(2017), that is 10% less, 30% less, 50% less, 70% less, 90% less, or 100% less than the attrition loss after 1 hour of the initial calcined particles produced before the hydration step.
[0039] Second manufacturing process for catalyst particles In some embodiments, the catalyst composition may be a catalyst particle, a spray-dried particle, or a combination thereof, produced only through a spray-drying step, such that a slurry is prepared and the spray-dried particle is produced from the slurry with Pt and a promoter added to the slurry. Thus, in some embodiments, the process for producing the catalyst composition may include a step of preparing a slurry or gel that may include a Group 2 element-containing compound and a liquid medium and optionally one or more of the above-mentioned additives, and spray-drying the slurry or gel to produce a spray-dried support particle containing a Group 2 element. At least one of the following (i) and (ii) may be satisfied: (i) Pt may be present in the slurry or gel in the form of a Pt-containing compound, and the catalyst composition may include catalyst particles that include spray-dried support particles having Pt disposed thereon; and (ii) Pt may be deposited on the spray-dried support particles by contacting the spray-dried support particles with a Pt-containing compound to produce a Pt-containing spray-dried support particle, and the catalyst composition may include catalyst particles that may include spray-dried support particles having Pt disposed thereon; Also, at least one of the following (iii) and (iv) may be satisfied: (iii) the compound containing the promoter element may be present in a slurry or gel, and the catalyst composition may include catalyst particles including spray-dried support particles having a promoter element disposed thereon; and (iv) the compound that may include the promoter element may be deposited on a spray-dried support particle to produce a promoter-containing spray-dried support particle, and the catalyst composition may include catalyst particles including spray-dried support particles having a promoter element disposed thereon, the promoter element including Sn, Cu, Au, Ag, Ga, or a combination or mixture thereof. In some embodiments, an optional alkali metal element(s) and / or binder may be added during synthesis of the catalyst particles.
[0040] In some embodiments, the catalyst particles can be further processed or activated in situ by adding the catalyst particles to a hydrocarbon upgrading process that exposes the catalyst particles to more severe conditions to produce catalyst particles with a higher activation level than the spray-dried particles had at the very time of their preparation. In some embodiments, when the catalyst particles comprise catalyst particles, spray-dried support particles, or combinations thereof that have undergone only a spray drying step such that a slurry is prepared and the spray-dried support particles are produced from the slurry with Pt and promoter added to the slurry, the catalyst particles can be introduced into a reaction zone, a combustion zone, a reduction zone, or any other location within a fluid hydrocarbon upgrading process, some of which are described further below. The preparation of the catalyst composition and the process for adding Pt, promoter(s), such as Sn, optional alkali metal element(s), and optional rare earth metal element(s) to the catalyst composition are described above. In some embodiments, the preparation of the slurry or gel, the spray drying of the slurry, the calcination of the spray dried particles and / or the hydrated calcined particles, and / or the hydration of the Group 2 metal-containing calcined support particles or spray dried particles can be carried out in a manner similar to that described in the literature, e.g., U.S. Pat. Nos. 4,866,019; 6,028,023; 6,589,902; 6,593,265; 6,800,578; 7,361,264; and 7,417,005; U.S. Patent Application Publication Nos. 2004 / 0029729; 2005 / 000396; and 2016 / 0082424; International Publication No. WO2008083563A1; and journal publications Wang et al., Ind. Eng. Chem. Res. 2008, 47, This can also be done using one of the known methods reported in: Chubar et al., Chem. Eng. J. 2013, 234, 284-299; Valente et al., Energy Environ. Sci., 2011, 4, 4096-4107; and Julklang et al., Mater. Lett. 2017, 209, 429-432.
[0041] The first upgrading process of hydrocarbons The first upgrading process of hydrocarbons may include contacting a hydrocarbon-containing feed (first hydrocarbon-containing feed) with a catalyst composition comprising Pt and a promoter disposed on a support to cause one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and an effluent comprising one or more upgraded hydrocarbons and molecular hydrogen. The catalyst composition and the first hydrocarbon-containing feed may be contacted with each other in any suitable environment, such as one or more reaction zones or conversion zones disposed within one or more reactors to produce an effluent and a coked catalyst composition. The reaction zone or conversion zone may be disposed or otherwise located within one or more fixed bed reactors, one or more fluidized or moving bed reactors, one or more countercurrent reactors, or any combination thereof.
[0042] The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature ranging from 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 620° C., 650° C., 660° C., 670° C., 680° C., 690° C., or 700° C. to 725° C., 750° C., 760° C., 780° C., 800° C., 825° C., 850° C., 875° C., or 900° C. In some embodiments, the first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature of at least 620° C., at least 650° C., at least 660° C., at least 670° C., at least 680° C., at least 690° C., or at least 700° C. to 725° C., 750° C., 760° C., 780° C., 800° C., 825° C., 850° C., 875° C., or 900° C. The first hydrocarbon-containing feed may be introduced into the reaction or conversion zone and contacted with the catalyst composition therein for a time of ≦3 hours, ≦2.5 hours, ≦2 hours, ≦1.5 hours, ≦1 hour, ≦45 minutes, ≦30 minutes, ≦20 minutes, ≦10 minutes, ≦5 minutes, ≦1 minute, ≦30 seconds, ≦10 seconds, ≦5 seconds, or ≦1 second or ≦0.5 seconds. In some embodiments, the first hydrocarbon-containing feed may be contacted with the catalyst composition for a time ranging from 0.1 seconds, 0.5 seconds, 0.7 seconds, 1 second, 30 seconds, 1 minute, 5 minutes, or 10 minutes to 30 minutes, 50 minutes, 70 minutes, 1.5 hours, 2 hours, or 3 hours.
[0043] The first hydrocarbon-containing feed and the catalyst composition may be contacted under a hydrocarbon partial pressure of at least 20 kPa absolute, where the hydrocarbon partial pressure is at least 20 kPa absolute, and ... 16 Alkanes and any C8-C 16The total partial pressure of alkyl aromatic hydrocarbons. In some embodiments, the hydrocarbon partial pressure during contact of the first hydrocarbon-containing feed with the catalyst composition can be in the range of 20 kPa absolute, 50 kPa absolute, 100 kPa absolute, at least 150 kPa absolute, at least 200 kPa absolute, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute. Here, the hydrocarbon partial pressure is the total partial pressure of any C2-C4 alkyl aromatic hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 is the total partial pressure of alkyl aromatic hydrocarbons. In other embodiments, the hydrocarbon partial pressure during contact of the hydrocarbon-containing feed with the catalyst composition can be in the range of 20 kPa absolute, 50 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute. Here, the hydrocarbon partial pressure is the total partial pressure of any C2-C4 alkyl aromatic hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 is the total partial pressure of alkyl aromatic hydrocarbons.
[0044] In some embodiments, the first hydrocarbon-containing feed comprises at least 60 vol.%, at least 65 vol.%, at least 70 vol.%, at least 75 vol.%, at least 80 vol.%, at least 85 vol.%, at least 90 vol.%, at least 95 vol.%, or at least 99 vol.% of a single C2-C 16 The first hydrocarbon-containing feed and the catalyst composition may comprise a single C2-C 16The alkane, for example, propane, may be contacted under a pressure of at least 20 kPa absolute, at least 50 kPa absolute, at least 100 kPa absolute, at least 150 kPa absolute, at least 250 kPa absolute, at least 300 kPa absolute, at least 400 kPa absolute, at least 500 kPa absolute, or at least 1,000 kPa absolute.
[0045] The first hydrocarbon-containing feed may be contacted with the catalyst composition in the reaction zone or conversion zone at any mass hourly space velocity (WHSV) effective to carry out the upgrading process. In some embodiments, the WHSV is 0.01 h -1 , 0.1 hours -1 , 1 hour -1 , 2 hours -1 , 5 hours -1 , 10 hours -1 , 20 hours -1 , 30 hours -1 or 50 hours -1 100 hours from -1 , 250 hours -1 , 500 hours -1 or 1,000 hours -1 In some embodiments, when the hydrocarbon upgrading process includes a fluidized or otherwise moving catalyst composition, the catalyst composition circulation mass flow rate and any C2-C 16 Alkanes and any C8-C 16 The ratio of the total amount of mass flow of alkyl aromatic hydrocarbons can range from 1, 3, 5, 10, 15, 20, 25, 30, or 40 to 50, 60, 70, 80, 90, 100, 110, 125, or 150 on a mass to mass basis. When the activity of the coked catalyst composition falls below a desired minimum amount, the coked catalyst composition, or at least a portion thereof, may undergo a regeneration process to produce a regenerated catalyst composition. More specifically, the coked catalyst composition may be contacted with one or more oxidants to cause combustion of at least a portion of the coke to produce a regenerated catalyst composition and combustion gases that are less coke. Depending on the particular reactor configuration, regeneration of the coked catalyst composition may occur within the reaction zone or conversion zone or in a separate combustion zone separate from the reaction zone or conversion zone to produce a regenerated catalyst composition. For example, regeneration of the coked catalyst composition may occur within the reaction zone or conversion zone when using a fixed bed or upflow reactor, or in a separate combustion zone separate from the reaction zone or conversion zone when using a fluidized bed reactor or other circulating or fluidized type reactor.
[0046] In some embodiments, the process may optionally contact at least a portion of the regenerated catalyst composition with a reducing gas to produce a regenerated and reduced catalyst composition. An additional amount of a hydrocarbon-containing feed may be contacted with at least a portion of the regenerated catalyst composition and / or at least a portion of any regenerated and reduced catalyst composition to produce a recoked catalyst composition and additional effluents. In some embodiments, the cycle time from contacting the hydrocarbon-containing feed with the catalyst composition to contacting the additional amount of the hydrocarbon-containing feed with the regenerated catalyst composition can be ≦5 hours. The first cycle begins when the catalyst composition is contacted with the first hydrocarbon-containing feed, and then contacted with at least an oxidizing gas to produce a regenerated catalyst composition or at least an oxidizing gas and an optional reducing gas to produce a regenerated catalyst composition, and the first cycle ends when the regenerated catalyst composition is contacted with an additional amount of the first hydrocarbon-containing feed. If one or more additional feeds (described in more detail below) are utilized between the flow of the first hydrocarbon-containing feed and the oxidizing gas, between the flow of the oxidizing gas and the reducing gas (if used), between the flow of the oxidizing gas and the additional amount of the first hydrocarbon-containing feed, and / or between the flow of the reducing gas (if used) and the additional amount of the first hydrocarbon-containing feed, the time during which the stripping gas is utilized will be included in the time included in the cycle time. Thus, the cycle time from the contacting step of the first hydrocarbon-containing feed with the catalyst composition to the contacting step of the additional amount of the hydrocarbon-containing feed with the regenerated catalyst composition can be ≦5 hours in some embodiments.
[0047] The oxidant may be or include, but is not limited to, O2, O3, CO2, H2O, or mixtures thereof. In some embodiments, an amount of oxidant greater than that required to combust 100% of the coke on the catalyst composition may be used to increase the rate of coke removal from the catalyst composition, which may result in a decrease in the time required for coke removal and an increase in the yield of upgraded products produced in a given time. The use of pure O2 as an oxidant may facilitate the capture and sequestration of CO2 generated during combustion in one or more downstream CO2 capture systems. The coked catalyst composition and the oxidant may be contacted with each other at a temperature ranging from 500° C., 550° C., 600° C., 650° C., 700° C., 750° C., or 800° C. to 900° C., 950° C., 1,000° C., 1,050° C., or 1,100° C. to produce the regenerated catalyst composition. In some embodiments, the coked catalyst composition and the oxidant may be contacted with each other at a temperature ranging from 500° C. to 1,100° C., 600° C. to 1,000° C., 650° C. to 950° C., 700° C. to 900° C., or 750° C. to 850° C. to produce the regenerated catalyst composition. The coked catalyst composition and the oxidant may be contacted with each other for a time period of ≦2 hours, ≦1 hour, ≦30 minutes, ≦10 minutes, ≦5 minutes, ≦1 minute, ≦30 seconds, ≦10 seconds, ≦5 seconds, or ≦1 second. For example, the coked catalyst composition and the oxidant may be contacted with each other for a time period ranging from 2 seconds to 2 hours. In some embodiments, the coked catalyst composition and the oxidant may be contacted with each other for a time period sufficient to remove ≧50 wt%, ≧75 wt%, or ≧90 wt%, or >99% of any coke disposed on the catalyst composition.
[0048] In some embodiments, the time that the coked catalyst composition and the oxidant are in contact with each other can be less than the time that the catalyst composition is in contact with the hydrocarbon-containing feed to produce an effluent and a coked catalyst composition. For example, the time that the coked catalyst composition and the oxidant are in contact with each other can be at least 90%, at least 60%, at least 30%, or at least 10% less than the time that the catalyst composition is in contact with the hydrocarbon-containing feed to produce an effluent. In other embodiments, the time that the coked catalyst composition and the oxidant are in contact with each other can be greater than the time that the catalyst composition is in contact with the hydrocarbon-containing feed to produce an effluent and a coked catalyst composition. For example, in some embodiments, the coking catalyst composition and the oxidant may be in contact with each other for a time that may be at least 50%, at least 100%, at least 300%, at least 500%, at least 1,000%, at least 10,000%, at least 30,000%, at least 50,000%, at least 75,000%, at least 100,000%, at least 250,000%, at least 500,000%, at least 750,000%, at least 1,000,000%, at least 1,250,000%, at least 1,500,000%, or at least 1,800,000% longer than the time the catalyst composition is in contact with the hydrocarbon-containing feed to produce an effluent. The coked catalyst composition and the oxidant may be contacted with each other under an oxidant partial pressure ranging from 20 kPa absolute, 50 kPa absolute, 100 kPa absolute, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute. In other embodiments, the oxidant partial pressure during contact with the coked catalyst composition to produce the regenerated catalyst composition can range from 20 kPa absolute, 50 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute.
[0049] Without wishing to be bound by theory, it is believed that at least a portion of the Pt and, if present, Ni and / or Pd disposed on the coked catalyst composition may be agglomerated compared to the catalyst composition prior to contact with the first hydrocarbon-containing feed. It is believed that during combustion of at least a portion of the coke on the coked catalyst composition, at least a portion of the Pt and, if present, Ni and / or Pd may be redispersed around the support. Redispersion of at least a portion of any agglomerated Pt and, if present, Ni and / or Pd may improve the stability of the catalyst composition over multiple cycles. In some embodiments, at least a portion of the Pt, Ni and / or Pd, if present, in the regenerated catalyst composition may be in a higher oxidation state than the Pt, Ni and / or Pd, if present, in the catalyst composition contacted with the first hydrocarbon-containing feed and than the Pt, Ni and / or Pd, if present, in the coked catalyst composition. As a result, as described above, in some embodiments, the process may optionally include a step of contacting at least a portion of the regenerated catalyst composition with a reducing gas to produce a regenerated reduced catalyst composition. Suitable reducing gases (reducing agents) may be or include, but are not limited to, H2, CO, CH4, C2H6, C3H8, C2H4, C3H6, steam, or mixtures thereof. In some embodiments, the reducing agent may be mixed with an inert gas, such as Ar, Ne, He, N2, CO2, HO, or mixtures thereof. In this embodiment, at least a portion of the Pt, and if present, Ni and / or Pd, in the regenerated and reduced catalyst composition may be reduced to a lower oxidation state, e.g., an elemental state, relative to the Pt, and if present, Ni and / or Pd, in the regenerated catalyst composition. In this embodiment, an additional amount of a hydrocarbon-containing feed may be contacted with at least a portion of the regenerated catalyst composition and / or at least a portion of the regenerated and reduced catalyst composition.
[0050] In some embodiments, the regenerated catalyst composition and the reducing gas may be contacted at a temperature ranging from 400° C., 450° C., 500° C., 550° C., 600° C., 620° C., 650° C., or 670° C. to 720° C., 750° C., 800° C., or 900° C. The regenerated catalyst composition and the reducing gas may be contacted for a time ranging from 1 second, 5 seconds, 10 seconds, 20 seconds, 30 seconds, or 1 minute to 10 minutes, 30 minutes, or 60 minutes. The regenerated catalyst composition and reducing gas may be contacted at a reducing agent partial pressure of from 20 kPa absolute, 50 kPa absolute, or 100 kPa absolute, 300 kPa absolute, 500 kPa absolute, 750 kPa absolute, or 1,000 kPa absolute to 1,500 kPa absolute, 2,500 kPa absolute, 4,000 kPa absolute, 5,000 kPa absolute, 7,000 kPa absolute, 8,500 kPa absolute, or 10,000 kPa absolute. In other embodiments, the reducing agent partial pressure during contact with the regenerated catalyst composition to produce the regenerated catalyst composition may range from 20 kPa absolute, 50 kPa absolute, 100 kPa absolute, 150 kPa absolute, 200 kPa absolute, 250 kPa absolute, or 300 kPa absolute to 500 kPa absolute, 600 kPa absolute, 700 kPa absolute, 800 kPa absolute, 900 kPa absolute, or 1,000 kPa absolute. Within the reaction or conversion zone, at least a portion of the regenerated catalyst composition, the regenerated reduced catalyst composition, the fresh or unused catalyst composition, or a mixture thereof may be contacted with an additional amount of the first hydrocarbon-containing feed to produce additional effluent and additional coked catalyst composition. As noted above, in some embodiments, the cycle time from contacting the hydrocarbon-containing feed with the catalyst composition to contacting the additional amount of the hydrocarbon-containing feed with the regenerated catalyst composition, and / or at least a portion of the regenerated reduced catalyst composition, and optionally with the fresh or unused catalyst composition, may be ≦5 hours.
[0051] In some embodiments, as described above, one or more additional feeds, e.g., one or more sweep fluids, may be utilized between the flow of the first hydrocarbon-containing feed and the oxidant, between the flow of the oxidant and the optional reducing gas, if used, between the flow of the oxidant and the additional first hydrocarbon-containing feed, and / or between the flow of the reducing gas and the additional first hydrocarbon-containing feed. The sweep fluid may, among other things, purge or otherwise remove undesirable materials, e.g., non-combustible particulates, including soot, from the reactor. In some embodiments, the additional feed may be inert under the dehydrogenation, dehydroaromatization, and dehydrocyclization, combustion, and / or reduction conditions. Suitable sweep fluids may be or include, but are not limited to, N2, He, Ar, CO2, H2O, CO2, CH4, or mixtures thereof. In some embodiments, when the process utilizes a sweep fluid, the duration for which the sweep fluid is utilized may range from 1 second, 5 seconds, 10 seconds, 20 seconds, 30 seconds, or 1 minute to 10 minutes, 30 minutes, or 60 minutes.
[0052] In some embodiments, the catalyst composition may remain sufficiently active and stable after multiple cycles, for example, at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100 cycles, at least 125 cycles, at least 150 cycles, at least 175 cycles, or at least 200 cycles, with each cycle time lasting < 5 hours, < 4 hours, < 3 hours, < 2 hours, < 1 hour, < 50 minutes, < 45 minutes, < 30 minutes, < 15 minutes, < 10 minutes, < 5 minutes, < 1 minute, < 30 seconds, or < 10 seconds. In some embodiments, the cycle time may be from 5 seconds, 30 seconds, 1 minute, or 5 minutes to 10 minutes, 20 minutes, 30 minutes, 45 minutes, 50 minutes, 70 minutes, 2 hours, 3 hours, 4 hours, or 5 hours. In some embodiments, after stabilization of catalyst performance (the first few cycles may have relatively poor or relatively good performance, but performance may eventually stabilize), the process may provide a first upgraded hydrocarbon product yield, e.g., a propylene yield when the hydrocarbon-containing feed comprises propane, at an upgraded hydrocarbon selectivity, e.g., a propylene selectivity, of ≧75%, ≧80%, ≧85%, or ≧90%, or ≧95% upon initial contact with the first hydrocarbon-containing feed, and may have a second upgraded hydrocarbon yield, which may be at least 90%, at least 93%, at least 95%, at least 97%, at least 98%, at least 99%, at least 99.5%, or at least 100% of the first upgraded hydrocarbon product yield, at an upgraded hydrocarbon selectivity, e.g., a propylene selectivity, of ≧75%, ≧80%, ≧85%, or ≧90%, or ≧95% upon completion of the last cycle (at least 15 cycles in total).
[0053] In some embodiments, when the first hydrocarbon-containing feed comprises propane and the upgraded hydrocarbon comprises propylene, contacting the hydrocarbon-containing feed with the catalyst composition can result in a propylene yield of ≧52%, ≧53%, ≧54%, ≧55%, ≧56%, ≧57%, ≧58%, ≧59%, ≧60%, ≧61%, ≧62%, ≧63%, ≧64%, ≧65%, or ≧66% with a propylene selectivity of ≧75%, ≧80%, ≧85%, ≧90%, ≧93%, or ≧95% for at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100 cycles, at least 125 cycles, at least 150 cycles, at least 175 cycles, or at least 200 cycles. In other embodiments, when the hydrocarbon-containing feed comprises at least 70 vol.% propane based on the total volume of the first hydrocarbon-containing feed and is contacted under a propane partial pressure of at least 20 kPa absolute pressure, a propylene yield of ≥ 52%, ≥ 53%, ≥ 55%, ≥ 57%, ≥ 60%, ≥ 62%, ≥ 63%, ≥ 64%, ≥ 65%, or ≥ 66% can be obtained with a propylene selectivity of ≥ 75%, ≥ 80%, ≥ 85%, ≥ 90%, ≥ 93%, or ≥ 95% for at least 15, at least 20, at least 30, at least 40, at least 50, at least 60, at least 70, at least 100 cycles, at least 125 cycles, at least 150 cycles, at least 175 cycles, or at least 200 cycles. It is believed that the propylene yield may be further increased to ≧67%, ≧68%, ≧70%, ≧72%, ≧75%, ≧77%, ≧80%, or ≧82% with a propylene selectivity of ≧75%, ≧80%, ≧85%, ≧90%, ≧93%, or ≧95% over ≧15 cycles, ≧20 cycles, ≧30 cycles, ≧40 cycles, ≧50 cycles, ≧60 cycles, ≧70 cycles, ≧100 cycles, ≧125 cycles, ≧150 cycles, ≧175 cycles, or ≧200 cycles by further optimizing the composition of the support and / or adjusting one or more process conditions.In some embodiments, this propylene yield may be obtained over ≧15 cycles, ≧20 cycles, ≧30 cycles, ≧40 cycles, ≧50 cycles, ≧60 cycles, ≧70 cycles, ≧100 cycles, ≧125 cycles, ≧150 cycles, ≧175 cycles, or ≧200 cycles when the catalyst composition is contacted with the catalyst composition at a temperature of ≧620°C, ≧630°C, ≧640°C, ≧650°C, ≧655°C, ≧660°C, ≧670°C, ≧680°C, ≧690°C, ≧700°C, or ≧750°C.
[0054] Systems suitable for carrying out the processes disclosed herein can include systems known in the art, such as fixed bed reactors as disclosed in International Publication No. WO2017078894; fluidized riser and / or downer reactors as disclosed in U.S. Pat. Nos. 3,888,762; 7,102,050; 7,195,741; 7,122,160; and 8,653,317; and U.S. Patent Application Publication Nos. 2004 / 0082824; 2008 / 0194891; and countercurrent reactors as disclosed in U.S. Pat. No. 8,754,276; U.S. Patent Application Publication No. 2015 / 0065767; and WO2013169461.
[0055] The first hydrocarbon-containing feed may include, but is not limited to, one or more alkane hydrocarbons, such as C2-C 16 Linear or branched alkanes and / or C4-C 16 Cyclic alkanes, and / or one or more alkyl aromatic hydrocarbons, e.g., C8-C 16 In some embodiments, the first hydrocarbon-containing feed may be or may include alkyl aromatic hydrocarbons. In some embodiments, the first hydrocarbon-containing feed may be or may include any C2-C alkyl aromatic hydrocarbons in the hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 The first hydrocarbon-containing feed may contain from 0.1 vol.% to 50 vol.% water vapor based on the total volume of the alkylaromatic hydrocarbon. In another embodiment, the ... 16 Alkanes and any C8-C 16May contain no or <0.1 vol.% water vapor based on the total volume of alkylaromatic hydrocarbons.
[0056] C2-C 16 The alkane may be or include, but is not limited to, ethane, propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane, n-heptane, 2-methylhexane, 2,2,3-trimethylbutane, cyclopentane, cyclohexane, methylcyclopentane, ethylcyclopentane, n-propylcyclopentane, 1,3-dimethylcyclohexane, or mixtures thereof. For example, the first hydrocarbon-containing feed may include propane, which may be dehydrogenated to produce propylene, and / or isobutane, which may be dehydrogenated to produce isobutylene. In another example, the first hydrocarbon-containing feed may include liquefied petroleum gas (LP gas), which may be in the gas phase upon contact with the catalyst composition. In some embodiments, the first hydrocarbon in the hydrocarbon-containing feed may be substantially composed of a single alkane, such as propane. In some embodiments, the hydrocarbon-containing feed comprises ≥ 50 mol%, ≥ 75 mol%, ≥ 95 mol%, ≥ 98 mol%, or ≥ 99 mol% of a single C-C hydrocarbon, based on the total moles of all hydrocarbons in the first hydrocarbon-containing feed. 16 In some embodiments, the first hydrocarbon-containing feed is at least 50 vol%, at least 55 vol%, at least 60 vol%, at least 65 vol%, at least 70 vol%, at least 75 vol%, at least 80 vol%, at least 85 vol%, at least 90 vol%, at least 95 vol%, at least 97 vol%, or at least 99 vol% of a single C2-C3 hydrocarbon, based on the total volume of the first hydrocarbon-containing feed. 16 It may include alkanes such as propane.
[0057] C8-C 16The alkyl aromatic hydrocarbon may be or include, but is not limited to, ethylbenzene, propylbenzene, butylbenzene, one or more ethyltoluenes, or mixtures thereof. In some embodiments, the hydrocarbon-containing feed is ≧50 mol%, ≧75 mol%, ≧95 mol%, ≧98 mol%, or ≧99 mol% of a single C8-C8 hydrocarbon, based on the total mass of all hydrocarbons in the first hydrocarbon-containing feed. 16 The first upgrading process of the hydrocarbons disclosed herein may include alkyl aromatic hydrocarbons such as ethylbenzene. In some embodiments, ethylbenzene may be dehydrogenated to produce styrene. As a result, in some embodiments, the first upgrading process of the hydrocarbons disclosed herein may include dehydrogenation of propane, dehydrogenation of butane, dehydrogenation of isobutane, dehydrogenation of pentane, dehydrocyclization of pentane to cyclopentadiene, naphtha reforming, dehydrogenation of ethylbenzene, dehydrogenation of ethyltoluene, etc. In some embodiments, the first hydrocarbon-containing feed may be diluted, for example, with one or more diluents, such as one or more inert gases. Suitable inert gases may be or include, but are not limited to, Ar, Ne, He, N2, CO2, CH4, or mixtures thereof. When the hydrocarbon-containing feed includes a diluent, the hydrocarbon-containing feed may be diluted with any C2-C4 in the hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 It may contain from 0.1 vol%, 0.5 vol%, 1 vol%, or 2 vol% to 3 vol%, 8 vol%, 16 vol%, or 32 vol% of the diluent, based on the total volume of the alkyl aromatic hydrocarbon.
[0058] In some embodiments, the first hydrocarbon-containing feed may also contain H2. In some embodiments, when the first hydrocarbon-containing feed contains H2, H2 and any C2-C 16 Alkanes and any C8-C 16 The molar ratio to the total amount of alkyl aromatic hydrocarbons can range from 0.1, 0.3, 0.5, 0.7, or 1 to 2, 3, 4, 5, 6, 7, 8, 9, or 10. In some embodiments, the first hydrocarbon-containing feed is substantially free of any water vapor, e.g., any C2-C4 in the hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 There may be <0.1 vol.% water vapor based on the total volume of alkylaromatic hydrocarbons. In other embodiments, the first hydrocarbon-containing feed may contain water vapor. For example, the first hydrocarbon-containing feed may contain any C2-C ... 16 Alkanes and any C8-C 16 The first hydrocarbon-containing feed may contain from 0.1 vol%, 0.3 vol%, 0.5 vol%, 0.7 vol%, 1 vol%, 3 vol%, or 5 vol% to 10 vol%, 15 vol%, 20 vol%, 25 vol%, 30 vol%, 35 vol%, 40 vol%, 45 vol%, or 50 vol% water vapor based on the total volume of alkylaromatic hydrocarbons. In other embodiments, the first hydrocarbon-containing feed may contain any C2-C 16 Alkanes and any C8-C 16 Based on the total volume of alkylaromatic hydrocarbons, the first hydrocarbon-containing feed may contain ≦50 vol%, ≦45 vol%, ≦40 vol%, ≦35 vol%, ≦30 vol%, ≦25 vol%, ≦20 vol%, or ≦15 vol% water vapor. In other embodiments, the first hydrocarbon-containing feed may contain ≦50 vol%, ≦45 vol%, ≦40 vol%, ≦35 vol%, ≦30 vol%, ≦25 vol%, ≦20 vol%, or ≦15 vol% water vapor. 16 Alkanes and any C8-C 16 Based on the total volume of the alkylaromatic hydrocarbon, it may contain at least 1 vol.%, at least 3 vol.%, at least 5 vol.%, at least 10 vol.%, at least 15 vol.%, at least 20 vol.%, at least 25 vol.%, or at least 30 vol.% water vapor.
[0059] In some embodiments, the first hydrocarbon-containing feed may contain sulfur. For example, the first hydrocarbon-containing feed may contain sulfur in the range of 0.5 ppm, 1 ppm, 5 ppm, 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, or 80 ppm to 100 ppm, 150 ppm, 200 ppm, 300 ppm, 400 ppm, or 500 ppm. In other embodiments, the first hydrocarbon-containing feed may contain sulfur in the range of 1 ppm to 10 ppm, 10 ppm to 20 ppm, 20 ppm to 50 ppm, 50 ppm to 100 ppm, or 100 ppm to 500 ppm. When sulfur is present in the first hydrocarbon-containing feed, the sulfur may be or include, but is not limited to, H2S, dimethyl disulfide, one or more mercaptans, or mixtures thereof. In some embodiments, the first hydrocarbon-containing feed may be substantially free or free of molecular oxygen. In some embodiments, the first hydrocarbon-containing feed may contain ≦5 mol%, ≦3 mol%, or ≦1 mol% molecular oxygen (O2). Providing a first hydrocarbon-containing feed that is substantially free of molecular oxygen is believed to substantially prevent oxidation reactions that would otherwise consume at least a portion of the alkanes and / or alkyl aromatic hydrocarbons in the first hydrocarbon-containing feed.
[0060] The second upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the upgrading process disclosed in U.S. Patent Application Publication No. 2021 / 0276932. For example, the hydrocarbon upgrading process may include (I) contacting a first hydrocarbon-containing feed with a catalyst composition comprising Pt and a promoter disposed on a support to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that may include one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed may be one or more C2-C 16 Linear or branched alkanes, or one or more C4-C16 Cyclic alkanes or one or more C8-C 16 The first hydrocarbon-containing feed and the catalyst composition may comprise an alkylaromatic hydrocarbon, an alkyl aromatic hydrocarbon, or a mixture thereof. The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature in the range of 300° C. to 900° C. for a time period of ≦3 hours under a hydrocarbon partial pressure of at least 20 kPa absolute, where the hydrocarbon partial pressure is less than or equal to the total hydrocarbon partial pressure of any C2-C4 in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 is the total partial pressure of alkylaromatic hydrocarbons. The catalyst composition may include up to 0.025 wt% Pt and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof, disposed on a support, the support including at least 0.5 wt% Group 2 element, all weight percentages being based on the weight of the support. The one or more upgraded hydrocarbons may include at least one of dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, and dehydrogenated cyclized hydrocarbons. The process may also include (II) contacting at least a portion of the coked catalyst composition with an oxidizing agent to cause combustion of at least a portion of the coke to produce a regenerated catalyst composition and combustion gases having less coke. The process may also include (III) contacting an additional amount of the first hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce a recoked catalyst composition and additional effluent. The cycle time from contacting the first hydrocarbon-containing feed with the catalyst composition in step (I) to contacting an additional amount of the first hydrocarbon-containing feed with the regenerated catalyst composition in step (III) may be ≦5 hours. In some embodiments, at least a portion of the Pt in the regenerated catalyst may be in a higher oxidation state than the Pt in the catalyst contacted with the first hydrocarbon-containing feed, and the process may further include, after step (II) and before step (III), contacting at least a portion of the regenerated catalyst with a reducing gas to produce a regenerated reduced catalyst, as described below in step (IIa). In this case, at least a portion of the Pt in the regenerated reduced catalyst is reduced to a lower oxidation state than the Pt in the regenerated catalyst, and an additional amount of the hydrocarbon-containing feed may be contacted with at least a portion of the regenerated reduced catalyst.
[0061] The third upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the upgrading process disclosed in U.S. Patent Application Publication No. 2021 / 0276002. For example, the hydrocarbon upgrading process may include (I) contacting a first hydrocarbon-containing feed in a conversion zone with fluidized catalyst particles that may include Pt and a promoter disposed on a support to cause one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a conversion effluent that may include coked catalyst particles, one or more upgraded hydrocarbons, and molecular hydrogen. The first hydrocarbon-containing feed may be one or more C2-C 16 Linear or branched alkanes, at least one C4-C 16 Cyclic alkanes, one or more of C8-C 16 The first hydrocarbon-containing feed may comprise any C2-C4 alkyl aromatic hydrocarbons, or mixtures thereof. The first hydrocarbon-containing feed and the fluidized catalyst particles may be contacted at a temperature ranging from 300° C. to 900° C. for a time ranging from 0.1 seconds to 2 minutes under a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is at least 20 kPa absolute pressure, and the first hydrocarbon-containing feed may comprise any C2-C4 alkyl aromatic hydrocarbons, or mixtures thereof. 16 Alkanes and any C8-C 16is the total partial pressure of alkyl aromatic hydrocarbons. The catalyst particles may include up to 0.025 wt% Pt and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof, disposed on a support, the support including at least 0.5 wt% Group 2 element, all mass percentages being based on the weight of the support. The one or more upgraded hydrocarbons may include dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, dehydrogenated cyclized hydrocarbons, or mixtures thereof. The process may also include (II) obtaining from the conversion effluent a first gas stream rich in the one or more upgraded hydrocarbons and molecular hydrogen, and a first particle stream rich in coked catalyst particles. The process may also include (III) contacting in a combustion zone at least a portion of the coked catalyst particles in the first particle stream with an oxidant to cause combustion of at least a portion of the coke to produce a combustion effluent, which may include regenerated catalyst particles low in coke and combustion gases. The process may also include (IV) obtaining a second gas stream rich in combustion gases and a second particulate stream rich in regenerated catalyst particles from the combustion effluent. The process may also include (V) contacting an additional amount of the first hydrocarbon-containing feed with the fluidized regenerated catalyst particles to produce an additional converted effluent comprising recoked catalyst particles, additional one or more upgraded hydrocarbons, and additional molecular hydrogen. In some embodiments, the process may further include, after step (IV) and before step (V), contacting at least a portion of the regenerated catalyst particles with a reducing gas as described below in step (IVa) to produce regenerated and reduced catalyst particles, in which case an additional amount of a hydrocarbon-containing feed may be contacted with the fluidized regenerated and reduced catalyst particles in step (V).
[0062] The fourth upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the first multi-stage upgrading process disclosed in WO 2021 / 225747. For example, the upgrading process may be a multi-stage hydrocarbon upgrading process that may include (I) contacting a first hydrocarbon-containing feed with a first catalyst composition that may include Pt and a promoter disposed on a support in a first conversion zone to cause one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of a portion of the first hydrocarbon-containing feed to produce a first conversion zone effluent that may include one or more upgraded hydrocarbons, molecular hydrogen, and the first unconverted hydrocarbon-containing feed. The process may also include (II) contacting the first conversion zone effluent with a second catalyst composition that may include Pt and a promoter disposed on a support in a second conversion zone to cause one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first unconverted hydrocarbon-containing feed to produce a second conversion zone effluent that may include an additional amount of one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed is one or more C-C 16 Linear or branched alkanes, at least one C4-C 16 Cyclic alkanes, one or more of C8-C 16 The first hydrocarbon-containing feed and the first catalyst composition may comprise an alkylaromatic hydrocarbon, an alkyl aromatic hydrocarbon, or a mixture thereof. The first hydrocarbon-containing feed and the first catalyst composition may be contacted under a hydrocarbon partial pressure of at least 20 kPa absolute for a time period ranging from 0.1 seconds to 3 hours, wherein the hydrocarbon partial pressure is at least 20 kPa absolute pressure, and ... 16 Alkanes and any C8-C 16 The first conversion zone effluent and the second catalyst composition may be contacted under a hydrocarbon partial pressure of at least 20 kPa absolute for a time period ranging from 0.1 seconds to 3 hours, where the hydrocarbon partial pressure is the total partial pressure of any C2-C alkylaromatic hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16is the total partial pressure of the alkylaromatic hydrocarbons. The first conversion zone effluent may have a temperature in the range of 300°C to 850°C. The second conversion zone effluent may have a temperature in the range of 350°C to 900°C. The temperature of the second conversion zone effluent may be higher than the temperature of the first conversion zone effluent. The first catalyst composition and the second catalyst composition may have the same composition or different compositions. The first catalyst composition and the second catalyst composition each include up to 0.025 wt% Pt and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof, disposed on a support, the support including at least 0.5 wt% Group 2 element, and all mass percentages are based on the weight of the support. The one or more upgraded hydrocarbons may include dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, dehydrogenated cyclized hydrocarbons, or mixtures thereof.
[0063] In some embodiments, at least one of the first catalyst composition and the second catalyst composition may be disposed in a fixed bed. In some embodiments, the first conversion zone and the second conversion zone may be disposed in a fixed bed reactor. In some embodiments, the first conversion zone and the second conversion zone may be disposed in a counter-flow reactor. In some embodiments, at least one of the first catalyst and the second catalyst may be in the form of fluidized catalyst particles. In some embodiments, the first catalyst and the second catalyst may be in the form of fluidized catalyst particles. In some embodiments, the first conversion zone and the second conversion zone may be substantially adiabatic. In some embodiments, the process may further comprise, after step (I) and prior to step (II), the following step: (Ia) contacting the first conversion zone effluent with one or more intermediate catalyst compositions, which may comprise Pt and a promoter disposed on a support, in one or more intermediate conversion zones to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of a portion of the unconverted hydrocarbon-containing feed in the first conversion zone effluent to produce one or more coked intermediate catalysts and one or more intermediate conversion zone effluents having one or more intermediate temperatures and which may comprise the unconverted hydrocarbon-containing feed and an additional amount of one or more upgraded hydrocarbons and molecular hydrogen, the final intermediate conversion zone effluent being contacted with a second catalyst in step (II) in a second conversion zone. In some embodiments, when the process comprises the optional step (Ia), one or more intermediate temperatures of the one or more intermediate conversion zone effluents may be higher than the temperature of the first conversion zone effluent, and the temperature of the second conversion zone effluent may be higher than the one or more intermediate temperatures of the one or more intermediate conversion zone effluents.
[0064] In some embodiments, contacting the hydrocarbon-containing feed with the first catalyst can provide a first coking catalyst, contacting the first conversion zone effluent with the second catalyst can provide a second coking catalyst, and the process can further include step (III) which can include contacting the first coking catalyst, the second coking catalyst, or the first coking catalyst and the second coking catalyst with an oxidant to cause combustion of at least a portion of the coke to produce combustion gas and the first regenerated catalyst, the second regenerated catalyst, or the first regenerated catalyst and the second regenerated catalyst. In some embodiments, in step (III), the first coking catalyst particles, the second coking catalyst particles, or the first coking catalyst particles and the second coking catalyst particles can be contacted with the oxidant at a temperature in the range of 580°C to 1,100°C, preferably 650°C to 1,000°C, more preferably 700°C to 900°C, more preferably 750°C to 850°C. In some embodiments, the process may also include the step of (IV) contacting at least a portion of any of the first regenerated catalyst, at least a portion of any of the second regenerated catalyst, or at least a portion of any of the first regenerated catalyst and at least a portion of any of the second regenerated catalyst with a reduction gas to produce a first regenerated reduction catalyst, a second regenerated reduction catalyst, or a first regenerated reduction catalyst and a second regenerated reduction catalyst.
[0065] The fifth upgrading process of hydrocarbons In other embodiments, the hydrocarbon upgrading process may include the second multi-stage upgrading process disclosed in WO 2021 / 225747. For example, the multi-stage hydrocarbon upgrading process may include (I) contacting, in a first conversion zone, a first hydrocarbon-containing feed with a first plurality of fluidized catalyst particles, which may include Pt and a promoter disposed on a support, to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of a first portion of the first hydrocarbon-containing feed to produce a first conversion zone effluent, which may include first coked catalyst particles, one or more upgraded hydrocarbons, molecular hydrogen, and the first unconverted hydrocarbon-containing feed. The process may also include (II) contacting, in a second conversion zone, the first conversion zone effluent with a second plurality of fluidized catalyst particles, which may include Pt and a promoter disposed on a support, to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first unconverted hydrocarbon-containing feed to produce a second conversion zone effluent, which may include second coked catalyst particles, an additional amount of upgraded hydrocarbons, and an additional amount of molecular hydrogen. The first hydrocarbon-containing feed may be one or more C2-C 16 Linear or branched alkanes, at least one C4-C 16 Cyclic alkanes, one or more of C8-C 16 The first hydrocarbon-containing feed and the first plurality of fluidized catalyst particles may be contacted for a time period ranging from 0.1 seconds to 2 minutes under a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is at least 20 kPa absolute of any C2-C4 alkyl aromatic hydrocarbons in the first hydrocarbon-containing feed. 16 Alkanes and any C8-C 16 The first conversion zone effluent and the second plurality of fluidized catalyst particles may be contacted under a hydrocarbon partial pressure of at least 20 kPa absolute for a time period ranging from 0.1 seconds to 2 minutes, wherein the hydrocarbon partial pressure is the total partial pressure of any C2-C alkyl aromatic hydrocarbons in the first conversion zone effluent. 16 Alkanes and any C8-C 16is the total partial pressure of the alkyl aromatic hydrocarbons. The first conversion zone effluent may have a temperature in the range of 300°C to 850°C. The second conversion zone effluent may have a temperature in the range of 350°C to 900°C. The temperature of the second conversion zone effluent may be higher than the temperature of the first conversion zone effluent. The first and second plurality of fluidized catalyst particles may each comprise up to 0.025 wt% Pt and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations or mixtures thereof, disposed on a support, the support comprising at least 0.5 wt% Group 2 element, all mass percentages being based on the weight of the support. The one or more upgraded hydrocarbons may include dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, dehydrogenated cyclized hydrocarbons, or mixtures thereof. The process may also include (III) obtaining from the second conversion zone effluent a first gas stream rich in upgraded hydrocarbons and molecular hydrogen and a first particulate stream rich in the first coked catalyst particles and the second coked catalyst particles. The process may also include (IV) splitting the first particulate stream into a second particulate stream and a third particulate stream. The process may also include (V) recycling the second particulate stream to the first conversion zone as a first plurality of fluidized particles. The process may also include (VI) contacting the third particulate stream with an oxidant in a combustion zone to cause combustion of at least a portion of the coke to produce a combustion effluent that may include regenerated catalyst particles that are low in coke and combustion gases. The process may also include (VII) obtaining from the combustion effluent a second gas stream rich in combustion gases and a fourth particulate stream rich in regenerated catalyst particles. The process may also include the step of (VIII) recycling the fourth particle stream to the second conversion zone as a second plurality of fluidized catalyst particles.
[0066] In some embodiments, the process may also include, after step (VII) and before step (VIII), a step (VIIa) below of contacting at least a portion of the fourth particle stream with a reducing gas to produce regenerated, reduced catalyst particles, which may be recycled to the second conversion zone as a second plurality of fluidized catalyst particles in step (VIII). In some embodiments, step (IV) may optionally include separating a fifth particle stream from the first particle stream, and the process may optionally include contacting the fourth particle stream with the fifth particle stream to produce a mixed particle stream. In some embodiments, the process may optionally include, after step (I) and prior to step (II), step (Ia) below of contacting the first conversion zone effluent with one or more intermediate fluid catalyst particles comprising Pt and a promoter disposed on a support in one or more intermediate conversion zones to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of a portion of the unconverted hydrocarbon-containing feed in the first conversion zone to produce one or more coked intermediate fluid catalyst particles and one or more intermediate conversion zone effluents which may have one or more intermediate temperatures and may comprise the unconverted hydrocarbon-containing feed and additional amounts of one or more upgraded hydrocarbons and molecular hydrogen, the final intermediate conversion zone effluent may be contacted with a second catalyst in a second conversion zone in step (II).
[0067] The sixth upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the upgrading process disclosed in U.S. Patent Application No. 63 / 062,084. For example, the upgrading process may include: (I) one or more C2-C 16 Linear or branched alkanes, at least one C4-C 16 Cyclic alkanes, one or more of C8-C 16The process may include introducing a first hydrocarbon-containing feed, which may include alkylaromatic hydrocarbons, or a mixture thereof, into the reaction zone. The process may also include (II) contacting the first hydrocarbon-containing feed with a catalyst composition disposed within the reaction zone to cause at least one of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the first hydrocarbon-containing feed to produce a coked catalyst composition and a first effluent, which may include one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature in the range of 300° C. to 900° C. for a time period of 1 minute to 90 minutes under a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is at least 20 kPa absolute, and is preferably at least 20 kPa absolute, and more ... 16 Alkanes and any C8-C 16is the total partial pressure of alkylaromatic hydrocarbons. The catalyst composition may include up to 0.025 wt% Pt disposed on a support and up to 10 wt% promoter, which may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof, the support including at least 0.5 wt% Group 2 element, all mass percentages being based on the mass of the support. The process may also include (III) ceasing the introduction of the first hydrocarbon-containing feed into the reaction zone; (IV) introducing an oxidant into the reaction zone; (V) contacting the oxidant with a coked catalyst composition to cause combustion of at least a portion of the coke to produce a regenerated catalyst composition having less coke and a second effluent including combustion gas, the oxidant and the coked catalyst composition being contacted for a time period between 1 minute and 90 minutes; and (VI) ceasing the introduction of the oxidant into the reaction zone. The process may also include the steps of (VII) introducing a reducing gas into the reaction zone; (VIII) contacting the reducing gas with a regenerated catalyst composition to produce a regenerated reduced catalyst composition and a third effluent, the reducing gas and the regenerated catalyst composition being contacted for a time period of from 0.1 seconds to 90 minutes; and (IX) ceasing the introduction of the reducing gas into the reaction zone. The process may also include the steps of (X) introducing an additional amount of a first hydrocarbon-containing feed into the reaction zone and (XI) contacting the additional amount of the first hydrocarbon-containing feed with the regenerated reduced catalyst composition to produce a recokized catalyst composition and an additional first effluent. The additional amount of the first hydrocarbon-containing feed and the regenerated reduced catalyst composition may be contacted at a temperature in the range of from 300° C. to 900° C. for a time period of from 1 minute to 90 minutes under a hydrocarbon partial pressure of at least 20 kPa absolute, wherein the hydrocarbon partial pressure is less than or equal to the total hydrocarbon partial pressure of any C2-C ... 16 Alkanes and any C8-C 16 is the total partial pressure of alkyl aromatic hydrocarbons.
[0068] In some embodiments, the process optionally comprises, after step (III) and before step (IV), a1) introducing a stripping gas into the reaction zone to remove at least a portion of any residual hydrocarbon-containing feed, the first effluent, or both from the reaction zone; (III) a2 ) removing at least a portion of any residual hydrocarbon-containing feed, effluent, or both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (III). a1 ) and Step (III a2 In some embodiments, the process may also include a combination of the following steps after step (VI) and before step (VII): a1 ) introducing a stripping gas into the reaction zone to remove at least a portion of any residual oxidant, the second effluent, or both from the reaction zone; (VI a2 ) removing at least a portion of any residual oxidant, the second effluent, or both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (VI). a1 ) and Step(VI a2 ) may also be included. In some embodiments, the process optionally comprises, after step (IX) and before step (X), a1 ) introducing a stripping gas into the reaction zone to remove at least a portion of any residual reducing gas, the third effluent, or both from the reaction zone; (IX) a2 ) removing at least a portion of any residual reducing gas, the third effluent, or both from the reaction zone by subjecting the reaction zone to a pressure less than atmospheric pressure; or step (IX). a1 ) and Step (IX a2In some embodiments, step (IV) of the process may include introducing a fuel into the reaction zone, optionally with an oxidant; and combusting at least a portion of the fuel in the reaction zone to generate heat for heating the reaction zone to a temperature of ≧580° C., ≧620° C., ≧650° C., ≧680° C., ≧710° C., ≧740° C., ≧770° C., ≧800° C., ≧850° C., ≧900° C., or ≧1,000° C.
[0069] The seventh upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the upgrading process disclosed in U.S. Patent Application Serial No. 63 / 195,966. For example, the process may include the steps of: (I) contacting a first hydrocarbon-containing feed with a catalyst composition that may include Pt and a promoter disposed on a support to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbon-containing feed to produce an at least partially deactivated catalyst composition that may include Pt, a promoter, a support, and contaminants, and an effluent that may include one or more upgraded hydrocarbons and molecular hydrogen. The first hydrocarbon-containing feed may include one or more C2-C 16 Linear or branched alkanes, or one or more C4-C 16 Cyclic alkanes, one or more of C8-C 16The catalyst composition may include up to 0.025 wt% Pt disposed on a support and up to 10 wt% promoter which may include Sn, Cu, Au, Ag, Ga, combinations or mixtures thereof, the support including at least 0.5 wt% Group 2 element, all weight percentages being based on the weight of the support. The first hydrocarbon-containing feed and the catalyst composition may be contacted at a temperature ranging from 300°C to 900°C. The one or more upgraded hydrocarbons may include at least one of dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, and dehydrogenated cyclized hydrocarbons. The process may also include (II) heating the at least partially deactivated catalyst composition with a heated gas mixture that may include H2O at a concentration greater than 5 mole % based on the total moles of the heated gas mixture to produce a precursor catalyst composition. The process may also include (III) providing an oxidizing gas that may include 5 mole % or less H2O based on the total moles of the heated gas mixture. The process may also include (IV) contacting the precursor catalyst composition with an oxidizing gas at an oxidation temperature in the range of 620° C. to 1,000° C. for a duration of at least 30 seconds to produce an oxidized precursor catalyst composition. The process may also include (V) obtaining a regenerated catalyst composition from the oxidized precursor catalyst composition. The process may also include (VI) contacting an additional amount of the first hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce an additional at least partially deactivated catalyst composition and an additional effluent. In some embodiments, the heated gas mixture may be produced by combusting a fuel with an oxidizing gas. In some embodiments, the fuel includes at least one of H2, CO, and a hydrocarbon, and the oxidizing gas may include O2. In some embodiments, the oxidizing gas may be or include, but is not limited to, O2, O3, CO2, or mixtures thereof, and may include 5 mole % or less of H2O.
[0070] The eighth upgrading process of hydrocarbons In some embodiments, the hydrocarbon upgrading process may include the upgrading process disclosed in U.S. Patent Application No. 63 / 232,959. For example, the hydrocarbon upgrading process may include the step of (I) contacting a first hydrocarbon-containing feed with fluidized dehydrogenation catalyst particles in a conversion zone to cause dehydrogenation of at least a portion of the hydrocarbon-containing feed to produce a converted effluent that may include coked catalyst particles and one or more dehydrogenated hydrocarbons. The fluidized dehydrogenation catalyst particles may include up to 0.025 wt% Pt disposed on a support and up to 10 wt% promoter that may include Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof, the support including at least 0.5 wt% Group 2 element, all mass percentages being based on the weight of the support. The first hydrocarbon-containing feed may include one or more C2-C 16 Linear or branched alkanes, at least one C4-C 16 Cyclic alkanes, one or more of C8-C 16 The first hydrocarbon-containing feed may comprise any C2-C alkyl aromatic hydrocarbons, alkyl aromatic hydrocarbons, or mixtures thereof. 16 Alkanes and any C8-C 16 Based on the mass of aromatic hydrocarbons, 0.1 hours -1 ~1,000 hours -1 The fluidized dehydrogenation catalyst particles can be contacted with any of the C2-C 16 Alkanes and any C8-C 16The mass ratio of the first hydrocarbon-containing feed to the total amount of aromatic hydrocarbons may range from 3 to 100. The first hydrocarbon-containing feed and the catalyst particles may be contacted at a temperature ranging from 600° C. to 750° C. The process may also include (II) separating from the conversion effluent a first particulate stream rich in the coked catalyst particles and a first gas stream rich in the one or more dehydrogenated hydrocarbons. The process may also include (III) contacting in a combustion zone at least a portion of the coked catalyst particles in the first particulate stream with an oxidant and a fuel to cause combustion of at least a portion of the coke to produce a combustion effluent that may include the coke-reduced catalyst particles and combustion gases. The dehydrogenation activity of the coke-reduced catalyst particles may be lower than the dehydrogenation activity of the coked catalyst particles. The process may also include (IV) separating from the combustion effluent a second particulate stream rich in the coke-reduced catalyst particles and a second gas stream rich in combustion gases. The process may also include (V) contacting at least a portion of the low-coke catalyst particles in the second particle stream with an oxidizing gas in an oxygen soak zone at an oxidation temperature in the range of 620° C. to 1,000° C. for a duration of at least 30 seconds to produce conditioned catalyst particles having activity that may be lower than the coked catalyst particles. The process may also include (VI) contacting at least a portion of the conditioned catalyst particles with a reducing gas in a reduction zone to produce regenerated catalyst particles having dehydrogenation activity that may be higher than the coked catalyst particles. The process may also include (VII) contacting an additional amount of a hydrocarbon-containing feed with at least a portion of the regenerated catalyst particles in a conversion zone to produce an additional amount of a converted effluent that may include re-coked catalyst particles and an additional amount of one or more dehydrogenated hydrocarbons. The process may also include (VIII) cooling the first gas stream to produce a cooled gas stream. The process may also include (IX) compressing at least a portion of the cooled gas stream to produce a compressed gas stream. The process may also include the step of (X) separating a plurality of products from the compressed gas stream.
[0071] In some embodiments, the first gas stream rich in one or more dehydrogenated hydrocarbons may further comprise entrained coking catalyst particles. In such embodiments, step (VIII) may include (VIIIa) contacting the first gas stream with a first quenching medium, or indirectly transferring heat from the first gas stream to a first heat transfer medium, or a combination thereof, to generate a cooling gas stream, and (VIIIb) contacting the cooling gas stream with a second quenching medium in a quenching tower, (VIIIc) recovering from the quenching tower a third gas stream that may comprise one or more dehydrogenated hydrocarbons and a slurry stream that may comprise at least a portion of the second quenching medium and entrained coking catalyst particles in the liquid phase, and step (IX) may include compressing at least a portion of the third gas stream to generate a compressed gas stream. In some embodiments, the conversion effluent may further comprise benzene, and the process may further include (XI) withdrawing a benzene product stream from the quenching tower.
[0072] The ninth upgrading process of hydrocarbons In some embodiments, the alkane and / or alkylaromatic hydrocarbon upgrading process may include the process disclosed in U.S. Patent Application No. 63 / 231,939. For example, the hydrocarbon upgrading process may include (I) contacting a first hydrocarbon-containing feed with fluidized dehydrogenation catalyst particles in a conversion zone to cause dehydrogenation of at least a portion of the first hydrocarbon-containing feed to produce a conversion effluent that may include coked catalyst particles and one or more dehydrogenated hydrocarbons. The fluidized dehydrogenation catalyst particles may include a contaminant disposed on a support, 0.025 wt% Pt, and up to 10 wt% promoter that may include Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof, the support including at least 0.5 wt% Group 2 element, and all mass percentages are based on the mass of the support. The process may also include (II) separating from the conversion effluent a first stream rich in coking catalyst particles and depleted in one or more dehydrogenated hydrocarbons and a second stream rich in one or more dehydrogenated hydrocarbons and containing entrained coking catalyst particles. The process may also include (III) contacting the second stream with a first quench medium to produce a second quenched stream. The process may also include (IV) contacting the second quenched stream with a second quench medium in a quench tower. The process may also include (V) recovering from the quench tower a gas stream that may contain one or more dehydrogenated hydrocarbons, the first concentrated quench medium stream, and a slurry stream that may contain at least a portion of the second quench medium and entrained coking catalyst particles in a liquid phase. The process may also include (VI) recycling at least a portion of the first concentrated quench medium to step (III). The process may also include (VII) separating at least a portion of the entrained coked catalyst particles from the slurry stream to provide a second recovered quench medium stream and a recovered entrained coked catalyst particle stream. The process may also include (VIII) recycling at least a portion of the second recovered quench medium stream to step (IV).
[0073] In some embodiments, the process may also include the steps of: (IX) contacting at least a portion of the coked catalyst particles in the first stream and at least a portion of the coked catalyst particles in the recovered entrained catalyst particle stream with an oxidant and optionally a fuel in a combustion zone to cause combustion of the coke and at least a portion of the fuel, if present, to produce a combustion effluent that may include regenerated catalyst particles having less coke and combustion gases; (X) separating the combustion gas stream and the regenerated catalyst particle stream; and (XI) contacting an additional amount of the first hydrocarbon-containing feed with the fluidized regenerated catalyst particles from the regenerated catalyst particle stream to produce an additional converted effluent that includes recoked catalyst particles and additional one or more dehydrogenated hydrocarbons. In some embodiments, the process may optionally further include (XII) transporting at least a portion of the recovered entrained catalyst particle stream to a metals reclamation facility; and (XIII) recovering at least a portion of the Pt and, if present, Ni and / or Pd from the coked catalyst particles in the recovered entrained coked catalyst particle stream. In some embodiments, the process may further include (XIV) cooling the slurry stream prior to step (VII) to produce a cooled slurry stream. In some embodiments, the conversion effluent may include benzene, and the process may further include (XV) removing a benzene product stream from the quench tower.
[0074] The 10th upgrading process of hydrocarbons In some embodiments, the alkane upgrading process may include the process disclosed in U.S. Patent Application No. 63 / 222,733. For example, the alkane dehydrogenation process may include introducing a first hydrocarbon-containing feed comprising one or more alkanes, e.g., propane, into a reactor that may include a catalyst composition disposed therein. The catalyst composition may include a contaminant disposed on a support, up to 0.025 wt% Pt, and up to 10 wt% promoter that may include Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof, the support including at least 0.5 wt% Group 2 element, all mass percentages being based on the weight of the support. The process may also include contacting the first hydrocarbon-containing feed with the catalyst composition in the reactor to produce a high temperature dehydrogenation product, the high temperature dehydrogenation product including at least a portion of the catalyst composition. The process may also include separating at least a portion of the catalyst composition from the hot dehydrogenation product in a primary separation unit and a secondary separation unit downstream of and in fluid communication with the primary separation unit. The process may also include combining the hot dehydrogenation product with a quench stream after it exits the secondary separation unit and cooling the hot dehydrogenation product to form an intermediate temperature dehydrogenation product, wherein the quench stream comprises hydrocarbons. The process may also include cooling the intermediate temperature dehydrogenation product to form a cooled dehydrogenation product.
[0075] In some embodiments, the quench stream may include liquid hydrocarbons and the intermediate temperature product may be entirely in the solid phase. In some embodiments, mixing of the high temperature dehydrogenation product with the quench stream may occur in the plenum section of the reactor. In some embodiments, the process may further include further cooling the cooled dehydrogenation product downstream of the reactor with a heat exchanger or a secondary quench stream, which may include at least a portion of the cooled dehydrogenation product after being further cooled by the heat exchanger or the secondary quench stream. It should be understood that the second through tenth hydrocarbon upgrading processes may include the same or similar process conditions, such as operating temperatures, pressures, time intervals for particular steps, WHSV, etc., as described for the first hydrocarbon upgrading process, as would be apparent to one skilled in the art.
[0076] Recovery and use of first upgraded hydrocarbons In some embodiments, the first upgraded hydrocarbons produced via any one of the first to tenth hydrocarbon upgrading processes may contain at least one upgraded hydrocarbon, such as olefins, water, unreacted hydrocarbons, molecular hydrogen, etc. The first upgraded hydrocarbons may be recovered or otherwise obtained via any conventional process, for example, by one or more conventional processes. One such process may include cooling and / or compressing the effluent to concentrate at least a portion of any water and any heavy hydrocarbons that may be present, leaving the olefins and any unreacted alkane or alkylaromatic hydrocarbons primarily in the gas phase. The olefins and unreacted alkane or alkylaromatic hydrocarbons may then be removed from the reaction product in one or more separator drums. For example, one or more splitters or distillation columns may be used to separate the dehydrogenation product from the first unreacted hydrocarbon-containing feed. In some embodiments, the recovered olefins, e.g., propylene, can be used to produce polymers. For example, recovered propylene can be polymerized to produce polymers having segments or units derived from the recovered propylene, e.g., polypropylene, ethylene-propylene copolymers, etc. Recovered isobutene can be used to produce, for example, the following: oxygenates, e.g., methyl tert-butyl ether, fuel additives, e.g., diisobutene, synthetic elastomeric polymers, e.g., butyl rubber, etc.
[0077] Catalyst Regeneration Process In some embodiments, the regeneration process of the catalyst composition may include the regeneration process disclosed in U.S. Patent Application No. 63 / 195,966. For example, a regeneration process usable to regenerate an at least partially deactivated catalyst composition that may include a contaminant disposed on a support and up to 0.025 wt% Pt and up to 10 wt% promoter that may include Sn, Cu, Au, Ag, Ga, combinations, or mixtures thereof. The support includes at least 0.5 wt% Group 2 element, and all weight percentages are based on the weight of the support. In some embodiments, the contaminant may be or include coke. The process may include (I) heating the at least partially deactivated catalyst composition with a heated gas mixture that may include H2O at a concentration greater than 5 mole % based on the total moles to produce a precursor catalyst composition. The process may also include (II) providing an oxidizing gas that may include 5 mole % or less H2O based on the total moles. The process may also include the step of (III) contacting the precursor catalyst composition with an oxidizing gas at an oxidation temperature in the range of 620° C. to 1,000° C. for a duration of at least 30 seconds, preferably at least 1 minute, preferably at least 5 minutes to produce an oxidized precursor catalyst composition. The process may also include the step of (IV) obtaining a regenerated catalyst composition from the oxidized precursor catalyst composition. In some embodiments, the heated gas mixture may be produced by combusting a fuel with an oxidizing gas. In some embodiments, the fuel may include at least one of H2, CO, and a hydrocarbon, and the oxidizing gas may include O2. In some embodiments, the oxidizing gas may be or include, but is not limited to, O2, O3, CO2, or mixtures thereof, and may include 5 mole % or less of H2O.
[0078] 11th upgrading process of hydrocarbons The eleventh upgrading process for hydrocarbons may include contacting a hydrocarbon-containing feed (second hydrocarbon-containing feed) with a catalyst composition comprising Pt and a promoter disposed on a support to cause reforming of at least a portion of the second hydrocarbon-containing feed to produce a coked catalyst composition and an effluent that may include carbon monoxide and molecular hydrogen. The catalyst composition and the second hydrocarbon-containing feed may be contacted with each other in any suitable environment, for example, in one or more reaction zones or conversion zones disposed in one or more reactors to produce an effluent and a coked catalyst composition. The reaction zones or conversion zones may be disposed or otherwise located in one or more fixed bed reactors, one or more fluidized or moving bed reactors, one or more countercurrent reactors, or any combination thereof. For clarity and ease of explanation, the reforming reaction is discussed in the context of a fluidized bed reactor, but it should be understood that fixed bed reactors, countercurrent or moving bed reactors, or any other reactors may be used to reform the second hydrocarbon-containing feed.
[0079] Reforming reactions can be used to produce reformed hydrocarbons by continuous or discontinuous reaction processes. In some embodiments, the reaction process can include a reforming step and a regeneration step, e.g., an exothermic reaction, which operate continuously while a fluid catalyst composition is transported between the reforming zone and the regeneration zone of the reactor. The endothermic reaction can include hydrocarbon reforming in the presence of the catalyst composition. Unused hydrocarbons and regenerated fluid catalyst particles can enter the reforming zone. After spending some time in the reforming zone, the hydrocarbons are at least partially converted to reformed products, which can exit the reforming zone together with the spent catalyst composition. The reformed products and unreacted feed can be separated from the spent catalyst by one or more separation devices. The reformed products and unreacted feed from the separation devices can proceed downstream for further purification, and the spent catalyst can be sent to the regeneration zone for regeneration. The exothermic regeneration reaction can be the reaction of an oxidant and optionally a fuel under combustion conditions to produce a regenerated catalyst and flue gas. After regeneration, the regenerated catalyst may be separated from the flue gas by one or more separators and transported back to the reforming zone to join with additional hydrocarbon feed and enter the reforming zone for further reforming reactions. The reforming step may convert CO2 and / or H2O and hydrocarbons, e.g., CH4, to synthesis gas containing H2 and CO. The regeneration step may burn reactants, e.g., coke and / or optional fuel and oxidant disposed on the spent catalyst, to generate heat to heat the regenerated catalyst, which may provide usable heat to drive the reforming reactions. In some embodiments, the catalyst may be heated to an average temperature ranging from 600°C, 700°C, or 800°C to 1,000°C, 1,300°C, or 1,600°C during the regeneration step.
[0080] Illustrative fuels may be or include, but are not limited to, hydrocarbons such as methane, ethane, propane, butane, pentane, or water vapor-containing hydrocarbons such as natural gas, molecular hydrogen, and / or other combustible compounds. The oxidant may be or include O2. In some embodiments, the oxidant may be or include air, O2-enriched air, O2-depleted air, or any other suitable O2-containing stream. Regeneration of the catalyst composition may correspond to the removal of coke from the catalyst particles. In some embodiments, during reforming, a portion of the feed introduced into the reforming zone may form coke. This coke may block access to the catalytic sites (e.g., metal sites) of the catalyst. During regeneration, at least a portion of the coke generated during reforming may be removed as CO or CO2. Regeneration of the catalyst may also correspond to the redispersion of any agglomerated active phase of the catalyst, e.g., Pt.
[0081] The second hydrocarbon-containing feed may include, but is not limited to, one or more reformable C1-C 16The second hydrocarbon-containing stream may be or include a hydrocarbon, such as an alkane, an alkene, a cycloalkane, an alkyl aromatic hydrocarbon, or any mixture thereof. In some embodiments, the second hydrocarbon-containing stream may be or include methane, ethane, propane, butane, pentane, or a mixture thereof. In some embodiments, the second hydrocarbon-containing feed may be exposed to the catalyst composition under a pressure of less than 35 kPa-a. For example, the second hydrocarbon-containing feed may be exposed to the catalyst composition under a pressure ranging from 0.7 kPa-a, 2 kPa-a, 3.5 kPa-a, 5 kPa-a, or 10 kPa-a to 15 kPa-a, 20 kPa-a, 25 kPa-a, or 30 kPa-a. In other embodiments, the second hydrocarbon-containing feed may be exposed to the catalyst composition under a pressure ranging from 35 kPa-a to 15 MPa-a. In yet other embodiments, the second hydrocarbon-containing feed may be exposed to the catalyst composition under pressures ranging from 0.7 kPa-a, 2 kPa-a, 5 kPa-a, 20 kPa-a, 35 kPa-a, 50 kPa-a, or 100 kPa-a to 200 kPa-a, 1 MPa-a, 3 MPa-a, 5 MPa-a, 10 MPa-a, or 15 MPa-a. In yet other embodiments, the second hydrocarbon-containing feed may be exposed to the catalyst composition under pressures less than 2.8 MPa-a, less than 2.5 MPa-a, less than 2.2 MPa-a, or less than 2 MPa-a.
[0082] The reforming reaction of a second hydrocarbon-containing feed, e.g., CH4, can occur in the presence of HO (steam reforming), CO2 (dry reforming), or both HO and CO2 (dual reforming). Example stoichiometries for steam reforming, dry reforming, and dual reforming of CH4 are shown in equations (1)-(3). (1) Dry reforming: CH4 + CO2 = 2CO + 2H2 (2) Steam reforming: CH4 + H2O = CO + 3H2 (3) Double reforming: 3CH4+2H2O+CO2=4CO+8H2 As shown in equations (1)-(3), dry reforming can result in a lower H2 to CO ratio than steam reforming. A reforming reaction carried out only with steam can produce a syngas having a H2:CO molar ratio of typically about 3, e.g., 2.5-3.5. In contrast, a reforming reaction carried out only with CO2 can produce a syngas having a H2:CO molar ratio of typically about 1 or less than 1. By using a combination of CO2 and H2O during reforming, the reforming reaction can be controlled to produce a wide variety of H2 to CO ratios in the resulting syngas.
[0083] The reforming reaction of the second hydrocarbon-containing feed may be carried out in the presence of O2 or may be carried out partially in the presence of O2, which is often referred to as a partial oxidation reaction. Examples of partial and complete oxidation stoichiometries are shown in equations (4) and (5). (4) Partial oxidation: CH4+0.5O2=CO+2H2 (5) Complete oxidation: CH4 + 2O2 = CO2 + 2H2O During the partial oxidation of methane, some degree of complete oxidation of methane may be unavoidable, in which the CO2 and H2O produced during the complete oxidation of methane may further reform methane via one or more of reactions (1) to (3). It should be noted that the ratio of H2 to CO in the syngas may also depend on the water-gas shift equilibrium. Although the stoichiometries of equations (1)-(4) indicate a ratio of approximately 1-3, the equilibrium amounts of H2 and CO in the syngas may differ from the reaction stoichiometry. The equilibrium amounts can be determined based on the water-gas shift equilibrium for the concentrations of H2, CO, CO2, and HO based on the reaction shown in equation (6). [ka]
[0084] In some embodiments, the catalyst composition may also serve as a water-gas shift catalyst. Thus, if the reaction environment for producing H2 and CO also includes HO and / or CO2, the initial stoichiometry from the reforming reaction may change based on the water-gas shift equilibrium. However, this equilibrium is also temperature dependent at higher temperatures that favor the production of CO and HO. As a result, the ratio of H2 to CO resulting in the formation of syngas is constrained by the water-gas shift equilibrium at the temperature in the reaction zone during syngas production. The ability to adjust the H2:CO molar ratio of the syngas provides a flexible process that can be used with a wide variety of syngas upgrading processes. Illustrative syngas upgrading processes can include, but are not limited to, Fischer-Tropsch processes, synthesis of methanol and / or other alcohols, e.g., one or more C1-C4 alcohols, fermentation processes, separation processes in which hydrogen can be separated to produce H2-rich products, dimethyl ether, and combinations thereof. These syngas upgrading processes are well known to those skilled in the art. In some embodiments, the upgraded products can include, but are not limited to, methanol, synthetic crude, diesel, lubricants, wax, olefins, dimethyl ether, other chemicals, or any combination thereof.
[0085] Suitable systems for carrying out the reforming of the second hydrocarbon-containing feed include systems known in the art, such as fixed bed reactors as disclosed in International Publication No. WO2017078894; U.S. Patent Nos. 3,888,762; 7,102,050; 7,195,741; 7,122,160; and 8,653,317; and U.S. Patent Application Publication Nos. 2004 / 0082824; 2008 / 0194891. and 10,160,708; and U.S. Patent Application Publication Nos. 2015 / 0065767 and 2017 / 0137285; and International Publication No. WO2013169461.
[0086] Feed and Energy The hydrocarbon-containing feeds described herein may be derived from either fossil fuel sources or non-fossil fuel sources. For example, propane may be a product or by-product of a process that uses biomass as a feed. The fuels described herein may also be derived from either fossil fuel sources or non-fossil fuel sources. For example, methane or H2 may be a product or by-product of a process that uses biomass as a feed. The fuels described herein may also be made from renewable energy, such as renewable electricity. For example, renewable electricity may be used to generate H2 by water electrolysis. The energy used in the processes described herein may also be provided by renewable electricity instead of fuel. EXAMPLES
[0087] Working Example: The foregoing discussion can be further illustrated with reference to the following non-limiting examples: Catalyst compositions 1-12 were prepared according to the following procedures. Catalyst compositions 1 to 14 were prepared according to the following procedure. For each catalyst composition, 80 wt% MgO and 20 wt% Al2O3 were used. 2PURALOX® MG80 / 150 (3 grams), a mixed Mg / Al metal oxide with a surface area of 1000 μg / g (Sasol), was calcined at 550° C. for 3 hours under air to form a support. A solution containing the appropriate amount of tin(IV) chloride pentahydrate, when used to make the catalyst composition (Acros Organics), and / or chloroplatinic acid, when used to make the catalyst composition (Sigma Aldrich), and 1.8 ml of deionized water was prepared in a small glass vial. The calcined PURALOX® MG80 / 150 support (2.3 grams) for each catalyst composition was impregnated with the corresponding solution. The impregnated material was equilibrated at room temperature (RT) for 24 hours in a closed vessel, dried at 110° C. for 6 hours, and calcined at 800° C. for 12 hours. Table 1 shows the nominal Pt and Sn content of each catalyst composition based on the weight of the support.
[0088] [Table 1]
[0089] Examples using the above catalysts Fixed bed experiments using catalyst compositions 1-8 (Examples 1-8, respectively) were carried out at approximately 100 kPa absolute pressure. The composition of the reactor effluent was measured using a gas chromatograph (GC). The concentrations of each component in the reactor effluent were then used to calculate the yield and selectivity to C3H6. The yields and selectivities to C3H6 reported in these examples were calculated on a moles of carbon basis. For each example, 0.3 g of catalyst composition was mixed with an appropriate amount of quartz diluent and loaded into a quartz reactor. The amount of diluent was determined so that the catalyst bed (catalyst + diluent) overlapped with the isothermal zone of the quartz reactor and the catalyst bed was mostly isothermal during operation. Quartz chips / rods filled the dead volume of the reactor. t rxn At the start of t rxn The yield and selectivity of C3H6 at the end of ini , Y end , S ini , and S end and reported as percentages in Tables 2 and 3 below.
[0090] The process steps for Examples 1-8 were as follows: 1. The system was flushed with inert gas. 2. Dry air was passed through the bypass of the reaction zone at a flow rate of 83.9 sccm while passing the inert gas through the reaction zone. The reaction zone was heated to a regeneration temperature of 800°C. 3. Dry air was then passed through the reaction zone at a flow rate of 83.9 sccm for 10 minutes to regenerate the catalyst. 4. The system was flushed with inert gas. 5. While passing the inert gas through the reaction zone, an H2-containing gas having 10 vol% H2 and 90 vol% Ar was passed through the bypass of the reaction zone at a flow rate of 46.6 sccm for a specified time. This was followed by passing the H2-containing gas through the reaction zone at 800°C for 3 seconds. 6. The system was flushed with inert gas. During this process, the temperature of the reaction zone was changed from 800°C to the reaction temperature of 670°C. 7. While passing inert gas through the reaction zone, a hydrocarbon-containing (HCgas) feed containing 81 vol% C3H8, 9 vol% inert gas (Ar or Kr) and 10 vol% water vapor was passed through the bypass of the reaction zone at a flow rate of 35.2 sccm for a specified time. The hydrocarbon-containing feed was then passed through the reaction zone at 670°C for 10 minutes. GC sampling of the reaction effluent was started immediately after the feed was switched from the reaction zone bypass to the reaction zone. The above process steps were repeated periodically until stable performance was obtained. Tables 2 and 3 show that catalyst 6, containing only 0.025 wt% Pt and 1 wt% Sn, had both similar yield and similar selectivity compared to catalyst 1, containing 0.4 wt% Pt and 1 wt% Sn, which was surprising and unexpected. Catalyst 8, which did not contain any Pt, did not show any appreciable propylene yield.
[0091] [Table 2]
[0092] [Table 3]
[0093] Catalysts 9-14 were also tested using the same steps 1-7 above. Table 4 shows that for catalyst compositions containing 0.1 wt% Pt based on the weight of the support, the Sn level should not be too low or too high for optimal propylene yield.
[0094] [Table 4]
[0095] Table 5 shows that for a catalyst composition containing 0.0125 wt% Pt based on the weight of the support, the Sn level should not be too high or too low for optimal propylene yield.
[0096] [Table 5]
[0097] Catalyst 6, containing only 0.025 wt% Pt and 1 wt% Sn, was also subjected to a life test using the same process steps 1-7 as above, except a flow rate of 17.6 sccm was used instead of 35.2 sccm in step 7. The figure shows that catalyst 6 maintained its performance over 204 cycles (x-axis is time, y-axis is yield of C3H6 and selectivity to C3H6, both in mole % carbon).
[0098] LIST OF EMBODIMENTS The present disclosure may further include the following non-limiting embodiments. A1. A process for upgrading a hydrocarbon, comprising: (I) contacting a hydrocarbon-containing feed with a catalyst composition comprising Pt and a promoter disposed on a support to effect reforming of at least a portion of the hydrocarbon-containing feed to produce a coked catalyst composition and a synthesis gas comprising H2 and CO, wherein the hydrocarbon-containing feed is selected from one or more C1-C 16% Group 2 element, and the catalyst composition comprises up to 0.025 wt. % Pt and up to 10 wt. % promoter, based on the weight of the support, the promoter comprising Sn, Cu, Au, Ag, Ga, combinations thereof, or mixtures thereof. A2. The process of A1, further comprising the step of (II) contacting at least a portion of the coked catalyst composition with an oxidant to cause combustion of at least a portion of the coke to produce a regenerated catalyst composition having less coke and combustion gases. A3. The process of A2, further comprising the step of (III) contacting the fuel with an oxidizer and a catalyst composition to cause combustion of at least a portion of the fuel. A4. The process of A2 or A3, further comprising (IV) contacting an additional amount of a hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce a recokized catalyst composition and an additional effluent.
[0099] A5. The process of any of A1-A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a fluidized bed reactor. A6. The process of any of A1-A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a fixed bed reactor. A7. The process of any of A1-A4, wherein the hydrocarbon-containing feed is contacted with the catalyst composition in a countercurrent reactor. A8. The process of any of A1-A7, wherein the catalyst composition comprises from 0.001 wt%, 0.005 wt%, or 0.007 wt% to 0.01 wt%, 0.015 wt%, 0.018 wt%, 0.02 wt%, 0.022 wt%, or 0.025 wt% Pt based on the weight of the support. A9. The process of any of A1-A8, wherein the catalyst composition comprises from 0.25 wt%, 0.5 wt%, or 1 wt% to 3 wt%, 5 wt%, or 10 wt% of a promoter based on the weight of the support. A10. The process of any of A1-A9, wherein the catalyst composition further comprises an alkali metal element comprising Li, Na, K, Rb, Cs, combinations thereof, or mixtures thereof disposed on the support in an amount up to 5 wt % based on the weight of the support. A11. The process of any of A1-A10, wherein the catalyst composition is in the form of particles having a size and particle density consistent with the Geldart A or Geldart B definition of a flowable solid.
[0100] A12. The process according to any one of A1 to A11, wherein the Group 2 element comprises Mg, and at least a portion of the Group 2 element is in the form of MgO or a mixed metal oxide comprising Mg. A13. The process according to any of A1-A12, wherein the Group 2 element comprises Mg, and at least a portion of the Group 2 element is in the form of a mixed Mg / Al oxide. A14. The process of any of A1-A13, wherein the support further comprises a Group 13 element, the Group 2 element comprises Mg, and the Group 13 element comprises Al, the support comprises a mixed Mg / Al metal oxide, and the mass ratio of Mg to Al in the mixed Mg / Al metal oxide is in the range of 0.001, 0.01, 0.1, or 1 to 6, 12.5, 100, or 1,000. A15. The support further comprises a Group 13 element, the promoter comprises Sn, the Group 2 element comprises Mg, the Group 13 element comprises Al, and the catalyst composition comprises from 0.001 wt%, 0.005 wt%, or 0.007 wt% to 0.01 wt%, 0.015 wt%, 0.018 wt%, 0.02 wt%, 0.022 wt%, or 0.025 wt% based on the weight of the support. The process of any of A1-A14, comprising Pt and 0.25 wt%, 0.5 wt%, or 1 wt% to 3 wt%, 5 wt%, or 10 wt% Sn, wherein the support comprises a mixed Mg / Al metal oxide, and the mass ratio of Mg to Al in the mixed Mg / Al metal oxide is in the range of 0.001 to 1,000, 0.01 to 100, 0.1 to 12.5, or 1 to 6. A16. The process of any of A1-A15, further comprising at least one of the steps of: reacting at least a portion of the syngas in the presence of a Fischer-Tropsch catalyst under effective Fischer-Tropsch conditions to produce an upgraded product, wherein the Fischer-Tropsch catalyst composition comprises a shifted Fischer-Tropsch catalyst or a non-shifted Fischer-Tropsch catalyst; exposing at least a portion of the syngas to a fermentation process to produce alcohols, organic acids, or mixtures thereof; contacting at least a portion of the syngas with a catalyst to produce at least one C1-C4 alcohol; and separating H2 from the syngas to produce an H2-rich product.
[0101] B1. A process for producing a catalyst composition, comprising: (I) preparing a slurry or gel comprising a Group 2 element-containing compound and a liquid medium; and (II) spray drying the slurry or gel to produce spray-dried support particles comprising a Group 2 element, wherein at least one of the following (i) and (ii): (i) Pt is present in the slurry or gel in the form of a Pt-containing compound, and the catalyst composition comprises catalyst particles comprising spray-dried support particles having Pt disposed thereon; and (ii) Pt is deposited on the spray-dried support particles by contacting the spray-dried particles with a Pt-containing compound to produce Pt-containing spray-dried support particles, and the catalyst composition comprises catalyst particles comprising spray-dried support particles having Pt disposed thereon; and wherein at least one of the following (iii) and (iv): (iii) process and (iv) a compound including a promoter element is deposited on a spray-dried support particle to produce a promoter-containing spray-dried support particle, and the catalyst composition includes catalyst particles including a spray-dried support particle having a promoter element disposed thereon; wherein the promoter element includes Sn, Cu, Au, Ag, Ga, or a combination or mixture thereof, and the catalyst particle includes up to 0.025 wt% Pt and up to 10 wt% promoter based on the weight of the spray-dried support particle, and the catalyst particle includes at least 0.5 wt% Group 2 element based on the weight of the spray-dried support particle.
[0102] B2. The process of B1, wherein the Pt-containing compound is present in a slurry or gel. B3. The process of B1 or B2, wherein the Pt-containing compound is deposited on a spray-dried support particle. B4. The process according to any one of B1 to B3, wherein the compound containing the promoter element is present in a slurry or gel. B5. The process according to any of B1-B4, wherein the compound containing the promoter element is deposited on a spray-dried support particle. B6. The process of any of B1-B5, wherein the Group 2 element comprises Mg, and at least a portion of the Group 2 element in the spray-dried support particles is in the form of a mixed Mg / Al metal oxide. B7. The process of any of B1-B6, further comprising (III) calcining the spray-dried support particles under an oxidizing atmosphere to produce calcined support particles, wherein the catalyst composition comprises catalyst particles comprising a Group 2 element and comprising Pt and the calcined support particles having a promoter element disposed thereon. B8. The process of B7, further comprising (IV) hydrating the calcined support particles after step (III) to produce hydrated support particles; and (V) calcining the hydrated support particles to produce a catalyst composition comprising the recalcined support particles, wherein the catalyst particles produced by steps (IV) and (V) have an attrition loss after one hour, measured according to ASTM D5757-11(2017), that is less than the attrition loss after one hour of the calcined particles produced in step (III).
[0103] Various terms have been defined above. Unless a term used in the claims is defined above, it should be given the broadest definition that one skilled in the art would give that term as reflected in at least one publication or issued patent. Furthermore, all patents, test procedures, and other documents cited in this application are incorporated by reference in their entirety to the extent that their disclosures are not inconsistent with this application, and for all authorities to which such incorporation is permitted. While the forgoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, the scope of which is determined by the claims that follow.
Claims
1. 1. A catalyst composition comprising up to 0.025 wt.% Pt and up to 10 wt.% promoter comprising Sn, Cu, Au, Ag, Ga, combinations or mixtures thereof disposed on a support, said support comprising at least 0.5 wt.% Group 2 element, and all weight percentages are based on the weight of the support.
2. 10. The catalyst composition of claim 1, wherein the catalyst composition comprises 0.001 wt% to 0.025 wt% Pt based on the weight of the support.
3. 3. The catalyst composition of claim 1 or 2, wherein the promoter comprises Sn.
4. 4. The catalyst composition of any one of claims 1 to 3, further comprising an alkali metal element comprising Li, Na, K, Rb, Cs, or a combination or mixture thereof disposed on the support in an amount up to 5 wt % based on the weight of the support.
5. 5. The catalyst composition of any one of claims 1 to 4, wherein the catalyst composition is in the form of particles having a size and particle density consistent with the Geldart A or Geldart B definition of a flowable solid.
6. The Group 2 element includes Mg, and 6. The catalytic composition according to claim 1, wherein at least a portion of said group 2 element is in the form of MgO or in the form of a mixed metal oxide containing Mg.
7. The Group 2 element includes Mg, and At least a portion of the Group 2 element is in the form of a mixed Mg / Al metal oxide; The catalyst composition according to any one of claims 1 to 6.
8. the support further comprises a Group 13 element; The Group 2 element includes Mg, and the Group 13 element includes Al, the support comprises a mixed Mg / Al metal oxide; and The mass ratio of Mg to Al in the mixed Mg / Al metal oxide is within the range of 0.001 to 1,000. The catalyst composition according to any one of claims 1 to 7.
9. the support further comprises a Group 13 element; the promoter comprises Sn, the group 2 element comprises Mg, and the group 13 element comprises Al; the catalyst composition comprising 0.001 wt. % to 0.025 wt. % Pt and 0.25 wt. % to 10 wt. % Sn based on the weight of the support; the support comprises a mixed Mg / Al metal oxide; and The mass ratio of Mg to Al in the mixed Mg / Al metal oxide is within the range of 0.001 to 1,000. The catalyst composition according to any one of claims 1 to 8.
10. 1. A process for producing a catalyst composition comprising: (I) preparing a slurry or gel comprising a Group 2 element-containing compound and a liquid medium; and (II) spray drying the slurry or gel to produce spray-dried particles comprising the Group 2 element. (III) calcining the spray-dried particles under an oxidizing atmosphere to produce calcined support particles comprising the Group 2 element; Here, the following (i), (ii), and (iii): (i) Pt is present in the slurry or gel in the form of a Pt-containing compound, and the catalyst composition comprises catalyst particles comprising calcined support particles having Pt disposed thereon; (ii) Pt is deposited on the spray-dried particles by contacting the spray-dried particles with a Pt-containing compound to produce Pt-containing spray-dried particles, and the catalyst composition comprises catalyst particles comprising the calcined support particles having Pt disposed thereon; and (iii) depositing Pt on the calcined support particles by contacting the calcined support particles with a Pt-containing compound to form Pt-containing calcined support particles, and the process further comprises the step of (IV) calcining the Pt-containing calcined support particles to form recalcined support particles having Pt disposed thereon, and the catalyst composition comprises the recalcined support particles; At least one of the following is satisfied: and the following (iv), (v), and (vi): (iv) a compound comprising a promoter element is present in the slurry or gel, and the catalyst composition comprises catalyst particles comprising the calcined support particles having the promoter element disposed thereon; (v) a compound comprising a promoter element is deposited on the spray-dried particles to produce a promoter-containing spray-dried particle, and the catalyst composition comprises catalyst particles comprising the calcined support particles having the promoter element disposed thereon; and (vi) a compound comprising a promoter element is deposited on the calcined support particle to produce a promoter-containing calcined support particle, and the process further comprises the step of (V) calcining the promoter-containing calcined support particle to produce a recalcined support particle having the promoter element disposed thereon, and the catalyst composition comprises the recalcined support particle; At least one of the following is satisfied: wherein the promoter element comprises Sn, Cu, Au, Ag, Ga, a combination thereof, or a mixture thereof; the catalyst particles comprise Pt in an amount of up to 0.025 wt. % and the promoter element in an amount of up to 10 wt. % based on the weight of the calcined or recalcined support particle; and the catalyst particles comprising at least 0.5 wt. % of the Group 2 element based on the weight of the calcined or recalcined support particles; The above process.
11. 11. The process of claim 10, wherein the spray-dried particles are calcined at a temperature in the range of 550°C to 900°C for a time period of ≦45 minutes.
12. 11. The process of claim 10, wherein the spray-dried particles are calcined at a temperature of <550°C for a time of ≦45 minutes.
13. The process of any one of claims 10 to 12, wherein the Pt-containing compound is present in the slurry or gel.
14. The process of any one of claims 10 to 13, wherein the Pt-containing compound is deposited on the spray-dried particles.
15. The process of any one of claims 10 to 14, wherein the Pt-containing compound is deposited on the calcined support particles and the process further comprises step (IV).
16. The process of any one of claims 10 to 15, wherein the compound containing the promoter element is present in the slurry or gel.
17. The process according to any one of claims 10 to 16, wherein the compound comprising the promoter element is deposited on the spray-dried particles.
18. The process according to any one of claims 10 to 17, wherein the compound comprising a promoter element is deposited on the calcined support particles and the process further comprises a step (V).
19. moreover, (VI) hydrating the calcined support particles after step (III) to form hydrated support particles; and (VII) calcining the hydrated support particles to produce a catalyst composition comprising recalcined support particles, wherein the recalcined support particles produced by steps (VI) and (VII) have an attrition loss after one hour, as measured according to ASTM D5757-11(2017), that is less than the attrition loss after one hour of the calcined support particles produced in step (III).
20. The Group 2 element includes Mg, and 20. The process according to any one of claims 11 to 19, wherein at least a portion of the group 2 element is in the form of MgO or a mixed metal oxide containing Mg.
21. 1. A hydrocarbon upgrading process comprising: (I) contacting a hydrocarbon-containing feed with a catalyst composition comprising Pt and a promoter disposed on a support to effect one or more of dehydrogenation, dehydroaromatization, and dehydrocyclization of at least a portion of the hydrocarbon-containing feed to produce a coked catalyst composition and an effluent comprising one or more upgraded hydrocarbons and molecular hydrogen; Where: The hydrocarbon-containing feed may comprise one or more C 2 -C 16 Linear or branched alkanes, or one or more C 4 -C 16 Cyclic alkanes or one or more C 8 -C 16 alkyl aromatic hydrocarbons, or mixtures thereof; The hydrocarbon-containing feed and catalyst composition are contacted at a temperature in the range of 300° C. to 900° C. for a time period of ≦3 hours under a hydrocarbon partial pressure of at least 20 kPa absolute, which hydrocarbon partial pressure is less than or equal to 100% of any C in the hydrocarbon-containing feed. 2 -C 16 Alkanes and any C 8 -C 16 is the total partial pressure of alkylaromatic hydrocarbons, the support comprises at least 0.5 wt. % of a Group 2 element based on the weight of the support; the catalyst composition comprising up to 0.025 wt. % Pt and up to 10 wt. % promoter based on the weight of the support; The promoter comprises Sn, Cu, Au, Ag, Ga, a combination thereof, or a mixture thereof; and The one or more upgraded hydrocarbons include at least one of dehydrogenated hydrocarbons, dehydrogenated aromatized hydrocarbons, and dehydrogenated cyclized hydrocarbons; The above process.
22. moreover (II) contacting at least a portion of the coked catalyst composition with an oxidant to cause combustion of at least a portion of the coke to produce a regenerated catalyst composition having less coke and combustion gases; (III) contacting an additional amount of the hydrocarbon-containing feed with at least a portion of the regenerated catalyst composition to produce a recokized catalyst composition and an additional effluent. wherein the cycle time from contacting the hydrocarbon-containing feed with the catalyst composition in step (I) to contacting the additional amount of hydrocarbon-containing feed with the regenerated catalyst composition in step (III) is ≦5 hours.
22. The process of claim 21.
23. 23. The process of claim 21 or claim 22, wherein the hydrocarbon-containing feed comprises propane, and wherein contacting the hydrocarbon-containing feed with the catalyst composition in step (I) has a propylene yield of at least 52% with a propylene selectivity of ≥ 85%.
24. The Group 2 element includes Mg, and 24. The process according to any one of claims 21 to 23, wherein at least a portion of the group 2 element is in the form of MgO or a mixed metal oxide containing Mg.
Citation Information
Patent Citations
Processes and systems for upgrading alkanes and alkyl aromatic hydrocarbons
WO2021225747A1