Ultra-high strength hot-rolled steel sheet with excellent formability and manufacturing method thereof
A hot-rolled steel sheet with specific alloy composition and controlled cooling process addresses the challenge of high strength and formability in automobile chassis components by ensuring uniform material distribution and improved fatigue performance, achieving ultra-high tensile strength and formability.
Patent Information
- Application Number
- JP2024531042
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-25
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-22
AI Technical Summary
Existing hot-rolled steel sheets used in automobile chassis components face challenges in achieving high strength, excellent fatigue performance, and uniform material distribution while maintaining formability, particularly for electric vehicles, due to issues like non-uniform microstructure and rapid cooling-induced phase transformations.
A hot-rolled steel sheet composition with specific alloy elements (C, Si, Mn, Al, Cr, Mo, Ti, B, P, S, N) and a controlled cooling process involving primary, secondary, and tertiary cooling stages to achieve a microstructure of 75-90% low-temperature bainite and martensite, with 10-25% acicular ferrite and bainitic ferrite, ensuring uniform material quality and improved formability.
The solution results in a steel sheet with ultra-high tensile strength, excellent formability, and uniform material distribution, suitable for automobile chassis structural members, with yield strength of 900 MPa or more, tensile strength of 1180 MPa or more, and elongation rate of 7% or more, while maintaining uniform material quality.
Smart Images

Figure 2024543130000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet suitable for use in automobile chassis structural members and the like, and more particularly to an ultra-high strength hot-rolled steel sheet having excellent formability and uniform material distribution within the steel sheet, and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art In recent years, there has been a rapid shift in the automobile market from internal combustion engine vehicles, which are the mainstream, to environmentally friendly vehicles such as electric vehicles in order to reduce global warming.
[0003] As internal combustion engine vehicles are replaced by electric vehicles, the types of parts that make up the vehicles are changing, and the weight of the vehicles is also changing. For example, it is known that when comparing the weight of an internal combustion engine vehicle and an electric vehicle released as the same model, the weight of the electric vehicle is increased by almost the weight of the battery compared to the internal combustion engine vehicle.
[0004] Meanwhile, chassis parts of an automobile play a role of supporting the vehicle body and are important parts for ensuring ride comfort and driving stability by absorbing vibrations and shocks from the road surface while driving. As the weight of an automobile increases, the fatigue load applied to the chassis parts increases, so steel materials used in chassis parts of electric automobiles and the like are required to have excellent fatigue strength.
[0005] Since the fatigue strength of steel is proportional to its tensile strength and yield strength, steel used in chassis parts for electric vehicles and the like needs to have improved tensile strength and yield strength.
[0006] In addition, since chassis parts are manufactured by press molding, it is required to ensure formability such as elongation and hole expandability suitable for press molding, as well as improving tensile strength and yield strength to improve fatigue strength. On the other hand, if there is a region in the steel plate with uneven microstructure and poor formability locally, processing cracks may occur during press molding, which may cause a decrease in productivity. Therefore, it is important to manufacture the steel plate so that formability such as elongation and hole expandability is uniformly distributed in the steel plate. In the case of hot-rolled steel plates used as chassis members, the temperature of the steel plate is controlled by cooling water after hot rolling, so that local temperature deviations may induce shape defects during cooling, and shape defects may again induce temperature deviations, resulting in an increase in material variation. Therefore, it is important to prevent temperature deviations in the steel plate during the manufacture of the steel plate. In particular, in the case of ultra-high strength steel plates that use a large amount of low-temperature bainite and martensite as the microstructure, it can be said that special care is required because the possibility of shape defects increasing due to rapid cooling and rapid phase transformation speed.
[0007] Various techniques have been proposed to improve the strength and formability of hot-rolled steel sheets.
[0008] As an example, Patent Document 1 discloses a method in which after hot rolling, the steel is cooled to a temperature of 200°C or higher, which is lower than the Ms temperature, and then coiled, to form a lower bainite phase and / or tempered martensite in a microstructure of the steel with a total area ratio of 90% or more. According to Patent Document 1, the hot-rolled steel sheet has a tensile strength of 1180 MPa or more, and excellent stretch flange formability and bendability can be ensured, but since the steel sheet is cooled by water cooling to a temperature of Ms or lower, there are concerns about shape defects due to the rapid phase transformation behavior of martensite and the associated material variations within the steel sheet.
[0009] Therefore, in order to ensure the running stability of chassis parts of environmentally friendly vehicles such as electric vehicles, it is necessary to develop a steel material that not only has high tensile strength and yield strength and excellent fatigue life, but also has excellent formability such as elongation and hole expandability so that press forming is easy, and at the same time, has a uniform material quality within the steel plate. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application No. 2019-553584 Summary of the Invention [Problem to be solved by the invention]
[0011] According to one aspect of the present invention, there is provided a hot-rolled steel sheet that not only has high strength and excellent fatigue performance, but also has excellent formability and is suitable for press forming, and has a uniform material distribution within the steel sheet, and a manufacturing method thereof.
[0012] The object of the present invention is not limited to the above. Anyone having ordinary knowledge in the technical field to which the present invention pertains will have no difficulty in understanding further object of the present invention from the entire contents of the specification of the present invention. [Means for solving the problem]
[0013] One aspect of the present invention is In weight percent, carbon (C): 0.06-0.18%, silicon (Si): 0.01-1.8%, manganese (Mn): 1.6-3.5%, aluminum (Al): 0.001-0.1%, chromium (Cr): 2.5% or less (including 0%), molybdenum (Mo): 2.0% or less (including 0%), titanium (Ti): 0.01-0.15%, boron (B): 0.0005-0.003%, phosphorus (P): 0.0001-0.05%, sulfur (S): 0.0001-0.05%, nitrogen (N): 0.0001-0.02%, the balance being Fe and other unavoidable impurities. The present invention provides an ultra-high strength hot-rolled steel sheet having a microstructure that contains, in terms of area fraction, one or more types selected from low-temperature bainite and martensite: 75 to 90%, one or more types selected from acicular ferrite and bainitic ferrite: 10 to 25%, and other phases: 5% or less (including 0%).
[0014] Yet another aspect of the present invention is reheating a steel slab containing, by weight, 0.06-0.18% carbon (C), 0.01-1.8% silicon (Si), 1.6-3.5% manganese (Mn), 0.001-0.1% aluminum (Al), 2.5% or less (including 0%) chromium (Cr), 2.0% or less (including 0%) molybdenum (Mo), 0.01-0.15% titanium (Ti), 0.0005-0.003% boron (B), 0.0001-0.05% phosphorus (P), 0.0001-0.05% sulfur (S), 0.0001-0.02% nitrogen (N), the balance being Fe and other unavoidable impurities, in a temperature range of 1100-1350°C; hot rolling the reheated steel slab to produce a hot rolled steel sheet; a step of primarily cooling the hot-rolled steel sheet to a temperature of Bs or less at an average cooling rate of 50°C / s or more; After the first cooling, a second cooling step is performed at an average cooling rate of 25° C. / s or less to a temperature of (Bs+Ms) / 2 or more for a time (ts) (seconds); After the second cooling, a third cooling step is performed at an average cooling rate of 30°C / s or more to a temperature range of Ms°C to 500°C. and winding the third cooled temperature range. The present invention provides a method for producing an ultra-high strength hot rolled steel sheet, in which finish hot rolling is performed within a temperature range of 750 to 1150°C so that the value of Du defined by the following relational expression 1 satisfies the range of 2 to 10 during the hot rolling.
[0015] [Equation 1] Du={FDT+(7.4×[C])-(24.7×[Si])-(4.7×[Mn])-(3.9×[Cr])-(5.2×[Mo])-(560×[Ti])-(1110×[Nb])}×0.049-34.2 (In the above Relational Formula 1, FDT means the rolling finish temperature (°C), and [C], [Si], [Mn], [Cr], [Mo], [Ti] and [Nb] each represent the weight percent content of the element in parentheses.) Effect of the Invention
[0016] According to the present invention, it is possible to provide a hot-rolled steel sheet having an ultra-high strength of 1180 MPa or more, excellent formability, and uniform material properties within the steel sheet, and a manufacturing method thereof, which can be suitably applied to chassis structural members of automobiles, etc.
[0017] The various and beneficial advantages and effects of the present invention are not limited to the above-mentioned contents, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0018] [Figure 1] 1 is a graph showing the relationship between the boron content and Du that simultaneously satisfies Relational Formula 1 and Relational Formula 2, and the microstructure intended in the present invention can be secured within the solid line connecting ABCDEF. [Diagram 2] Photographs of the microstructures of Example 1 (a) and Comparative Example 5 (b) observed with a scanning electron microscope (SEM) are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0020] On the other hand, the terms used in this specification are intended to describe specific embodiments and are not intended to limit the present invention. For example, the singular form used in this specification includes the plural form unless the relevant definition clearly indicates otherwise. Furthermore, the meaning of "comprise" used in this specification embodies a configuration and does not exclude the presence or addition of other configurations.
[0021] In the conventional manufacturing method of hot-rolled steel sheets to obtain ultra-high strength of tensile strength of 1180 MPa or more, a method has been widely applied in which after hot rolling, a large amount of cooling water is sprayed to cool the steel sheet to below the Ms temperature to make martensite the main phase. However, when martensite is the main phase, there is a problem that the elongation, bendability, and hole expandability are deteriorated. In addition, there is a problem that the shape is defective due to the sudden lattice expansion during cooling and the temperature unevenness in the steel sheet creates areas in the sheet where residual stress from phase transformation is concentrated, and forming cracks are generated during forming for part processing.
[0022] The present inventors have found that ultra-high strength can be ensured by utilizing bainite and martensite, and that acicular ferrite or bainitic ferrite can be uniformly dispersed in the structure to prevent excessive concentration of stress at a specific position during deformation, thereby ensuring formability. In addition, the present inventors have confirmed that an ultra-high strength hot-rolled steel sheet with uniform material properties can be provided by coiling at or above the Ms temperature to avoid rapid formation of martensite, and have thus completed the present invention. The present invention will be described in more detail below.
[0023] An ultra-high strength hot rolled steel sheet according to one aspect of the present invention, which has excellent formability and uniform material properties within the steel sheet, can contain, by weight, carbon (C): 0.06 to 0.18%, silicon (Si): 0.01 to 1.8%, manganese (Mn): 1.6 to 3.5%, aluminum (Al): 0.001 to 0.1%, chromium (Cr): 2.5% or less (including 0%), molybdenum (Mo): 2.0% or less (including 0%), titanium (Ti): 0.01 to 0.15%, boron (B): 0.0005 to 0.003%, phosphorus (P): 0.0001 to 0.05%, sulfur (S): 0.0001 to 0.05%, and nitrogen (N): 0.0001 to 0.02%.
[0024] The reasons for adding the components of the hot-rolled steel sheet and the reasons for limiting the content thereof in the present invention will be specifically described below. Meanwhile, unless otherwise specified in the present invention, the content of each element is based on weight, and the proportion of the structure is based on area.
[0025] Carbon (C): 0.06~0.18% Carbon (C) is the most economical and effective element for strengthening steel, and the strength of the steel sheet increases as the C content increases. In the present invention, C exists in the form of fine carbides or in a solid solution state in lower bainite and martensite, and plays a role in improving the yield strength and tensile strength of the steel.
[0026] If the C content is less than 0.06%, it is difficult to ensure a tensile strength of 1180 MPa or more, while if the C content exceeds 0.18%, there is a problem that weldability deteriorates. Therefore, in the present invention, the C content can be contained in an amount of 0.06 to 0.18%, and more advantageously, the lower limit of the C content can be 0.07%, and more preferably, the upper limit of the C content can be 0.15%.
[0027] Silicon (Si): 0.01 to 1.8% Silicon (Si) is an element that improves the hardenability of steel and plays a role in improving strength through the solid solution strengthening effect. It also improves strength by preventing the formation of ferrite during cooling and forming lower bainite and / or martensite phases.
[0028] If the Si content is less than 0.01%, the effect of solid solution strengthening and the effect of delaying ferrite transformation are reduced, making it difficult to ensure tensile strength, whereas if the Si content exceeds 1.8%, Fe-Si composite oxide is formed on the surface of the slab during reheating, resulting in not only deterioration of the surface quality of the steel sheet but also deterioration of weldability.
[0029] Therefore, in the present invention, the Si content may be 0.01 to 1.8%, more preferably 0.1% or more, and even more preferably the lower limit of the Si content may be 0.2%. The upper limit of the Si content may be 1.5%, more preferably 1.3%.
[0030] Manganese (Mn): 1.6-3.5% Manganese (Mn) is an element that improves the hardenability of steel, and prevents the formation of ferrite during cooling after finish rolling, facilitating the formation of low-temperature transformation structures. If the Mn content is less than 1.6%, there is a problem that the hardenability is insufficient and the fraction of ferrite increases excessively. On the other hand, if the Mn content exceeds 3.5%, the hardenability increases significantly, and the holding time for sufficiently forming the acicular ferrite or bainitic ferrite to be obtained in the present invention increases excessively, resulting in a decrease in elongation. Therefore, in the present invention, the Mn content may be 1.6 to 3.5%, and more preferably, the lower limit of the Mn content may be 1.8%, or the upper limit of the Mn content may be 2.5%.
[0031] Aluminum (Al): 0.001 to 0.1% Aluminum (Al) is an element added for deoxidizing molten steel, and a part of it is present in steel after deoxidization. If the content of Al exceeds 0.1%, it increases oxide and nitride inclusions in the steel, deteriorating the formability of the steel sheet. On the other hand, if the content of Al is less than 0.001%, it increases unnecessary refining costs due to excessive reduction of Al, which is economically disadvantageous. Therefore, in the present invention, the content of Al may be 0.001 to 0.1%, and more preferably, the lower limit of the Al content may be 0.005% or 0.02%. Alternatively, more preferably, the upper limit of the Al content may be 0.05% or 0.025%.
[0032] Chromium (Cr): 2.5% or less (including 0%) Chromium (Cr) is an element that improves the hardenability of steel and suppresses the formation of ferrite during cooling after finish rolling. If the Cr content exceeds 2.5%, the hardenability increases significantly, bainite transformation does not occur smoothly in the cooling zone, and the holding time for securing the fraction of acicular ferrite or bainitic ferrite increases excessively, deteriorating the elongation rate. Therefore, in the present invention, the Cr content may be 2.5% or less, and more preferably 1.5% or less. Meanwhile, according to one embodiment of the present invention, the upper limit of the Cr content may be more preferably 0.9%.
[0033] On the other hand, the present invention includes the case where the Cr content is 0%, since the intended physical properties can be secured without the inclusion of the Cr. However, when the Cr is intentionally added, it is effective to add a minimum of 0.01%.
[0034] Molybdenum (Mo): 2.0% or less (including 0%) Molybdenum (Mo) is an element that improves the hardenability of steel, and plays a role in improving strength through the solid solution strengthening effect and suppressing the formation of ferrite during cooling after finish rolling. If the Mo content exceeds 2.0%, the hardenability increases significantly and bainite transformation does not occur smoothly in the cooling zone. As a result, the holding time required to secure the fraction of acicular ferrite or bainitic ferrite increases excessively, resulting in a decrease in elongation.
[0035] Therefore, in the present invention, the Mo content can be 2.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.
[0036] On the other hand, the present invention includes the case where the Mo content is 0%, since the intended physical properties can be secured without containing Mo. However, it is clear that when Mo is added, it is effective to add a minimum of 0.01%.
[0037] Titanium (Ti): 0.01-0.15% Titanium (Ti) is an element that forms carbonitrides in steel and is widely used to induce the formation of precipitates in order to ensure the strength of steel. In the present invention, however, titanium is used to remove nitrogen (N) from steel and suppress the formation of BN, thereby allowing boron (B) to concentrate at the austenite grain boundaries, as well as to control the grain size of austenite before rolling.
[0038] In order to fully obtain the intended effect of the present invention, it is preferable that the Ti content is 0.01% or more, and it is preferable that the Ti content is 2.9 times or more the nitrogen (N) content in order to remove nitrogen (N) from the steel. However, if the Ti content exceeds 0.15%, oxides may be formed during continuous casting, which may cause problems such as clogging of the casting nozzle.
[0039] Therefore, in the present invention, the Ti content can be 0.01 to 0.15%, and more advantageously, the lower limit of the Ti content may be 0.02%, or the upper limit of the Ti content may be 0.12%.
[0040] Boron (B): 0.0005 to 0.003% Boron is an element that enhances the hardening ability of steel by concentrating at austenite grain boundaries and reducing grain boundary energy. In the present invention, boron plays a role in suppressing the phase transformation of ferrite and upper bainite, which occurs at the austenite grain boundaries due to diffusion transformation and nucleation of the phase transformation, and ensuring lower bainite and martensite as the main phases.
[0041] In order to fully obtain the intended effects of the present invention, the concentration of B is preferably 0.0005% or more. However, if the content exceeds 0.003%, the hardenability increases significantly, the holding time for fully forming the acicular ferrite or bainitic ferrite to be obtained in the present invention increases excessively, and the elongation decreases.
[0042] Therefore, in the present invention, the B content may be 0.0005 to 0.003%, and more advantageously, the lower limit of the B content may be 0.001%, or the upper limit of the B content may be 0.0025%.
[0043] Phosphorus (P): 0.0001 to 0.05% Phosphorus (P) is an impurity that is inevitably contained in steel and is the main cause of impairing the workability of steel due to segregation, so it is preferable to control its content as low as possible.
[0044] Theoretically, it is advantageous to limit the P content to 0%, but controlling the P content to less than 0.0001% requires excessive manufacturing costs, so the lower limit can be set to 0.0001%. However, if the P content exceeds 0.05%, there is a risk of reduced workability, so the upper limit of the P content can be limited to 0.05%. However, more advantageously, the lower limit of the P content may be 0.0005%, or the upper limit of the P content may be 0.013%.
[0045] Sulfur (S): 0.0001-0.05% Sulfur (S) is an impurity that is inevitably contained in steel, and it has the problem that it combines with Mn and other elements to form nonmetallic inclusions, which reduces the workability of the steel. Therefore, it is preferable to control the S content as low as possible.
[0046] Theoretically, it is advantageous to limit the S content to 0%, but controlling the S content to less than 0.0001% requires excessive manufacturing costs, so the lower limit can be set to 0.0001%. However, if the S content exceeds 0.05%, there is a risk of reduced workability, so the upper limit of the S content can be limited to 0.05%. However, more advantageously, the lower limit of the S content may be 0.0003%, or the upper limit of the S content may be 0.0012%.
[0047] Nitrogen (N): 0.0001-0.02% Nitrogen (N) is an impurity that is inevitably contained in steel, and has the problem of combining with Al and other elements to form nitrides that impair the workability of steel. Therefore, it is preferable to control the N content as low as possible.
[0048] Theoretically, it is advantageous to limit the N content to 0%, but controlling the N content to less than 0.0001% requires excessive manufacturing costs, so the lower limit can be set to 0.0001%. However, if the content exceeds 0.02%, there is a risk of reduced workability, so the upper limit of the N content can be limited to 0.02%. However, more advantageously, the lower limit of the N content may be 0.001%, or the upper limit of the N content may be 0.006%.
[0049] The hot-rolled steel sheet of the present invention may selectively further contain niobium (Nb) in addition to the above-mentioned alloy composition.
[0050] Niobium (Nb): 0.01-0.2% Niobium (Nb) is an element that forms carbonitrides in steel and is widely used to induce the formation of precipitates to ensure the strength of steel, but in the present invention, it plays a role in controlling the grain size of austenite by delaying recrystallization during hot rolling. If the Nb content is less than 0.01%, the effect of controlling the grain size is low, and if the Nb content exceeds 0.2%, the grain size of austenite becomes excessively fine, which may deteriorate the formability. Therefore, in the present invention, the Nb content may include 0.01 to 0.2%.
[0051] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities may be inevitably mixed in from the raw materials or the surrounding environment, and this cannot be excluded. These impurities are known to any technician in a normal manufacturing process, so the entire contents of these impurities are not specifically mentioned in this specification.
[0052] The hot-rolled steel sheet of the present invention, which satisfies the above-mentioned alloy composition, contains at least one selected from low-temperature bainite and martensite, which are low-temperature transformation structures, as a base structure in order to ensure a yield strength of 900 MPa or more and a tensile strength of 1180 MPa or more. Therefore, according to one embodiment of the present invention, the at least one selected from the low-temperature bainite and martensite may be contained in an area fraction of 75 to 90%.
[0053] In the present invention, after the tertiary cooling performed after hot rolling, austenite is transformed into low-temperature bainite or martensite. Since low-temperature bainite and martensite are generated by shear transformation (displacive phase transformation), a high level of dislocation density exists in the structure due to screw dislocations generated in the structure to reduce the shear deformation generated during transformation and edge dislocations generated to accommodate the volume expansion due to phase transformation. Therefore, it is suitable for improving the yield strength and tensile strength of steel due to the carbon and fine carbides solid-solubilized in the structure. On the other hand, the high level of dislocation density and the solid-solubilized carbon and fine carbides prevent the movement of dislocations in the structure, which is characterized by a decrease in elongation.
[0054] Therefore, in the present invention, from the viewpoint of ensuring yield strength and tensile strength, it is preferable that the low-temperature transformation structure of one or more selected from low-temperature bainite (LB) and martensite (M) is contained in an amount of 75% or more by area percent, and in order to simultaneously ensure elongation, it is preferable to limit it to 90% or less. On the other hand, according to one embodiment of the present invention, more preferably, the lower limit of the fraction of the one or more selected from low-temperature bainite and martensite may be 76.9%, or the upper limit of the fraction of the one or more selected from low-temperature bainite and martensite may be 86.6%.
[0055] In the present invention, the low-temperature bainite and martensite both contain iron carbides at grain boundaries and within grains in a lath structure, and therefore must be controlled as a total fraction, and therefore the fraction of at least one selected from the low-temperature bainite and martensite is controlled in the present invention.
[0056] On the other hand, the hot-rolled steel sheet according to the present invention preferably contains at least one selected from acicular ferrite (AC) and bainitic ferrite (BF) in an area fraction of 10 to 25%.
[0057] The steel of the present invention is cooled to a temperature below Bs (bainite transformation start temperature) during the first cooling to avoid ferrite phase transformation after hot rolling, and then slowly cooled during the subsequent second cooling, whereby bainite transformation proceeds. The bainite transformation at this time occurs in the high-temperature bainite transformation region. Therefore, the formation of bainitic ferrite and the diffusion phenomenon of carbon into untransformed austenite occur, and carbides are not formed inside the bainitic ferrite. On the other hand, although a large number of dislocations exist inside the bainitic ferrite formed by shear transformation, the dislocation density is reduced to an appropriate level by the above-mentioned secondary cooling and the subsequent recovery phenomenon after coiling, which has the effect of improving the elongation of the steel sheet.
[0058] The bainitic ferrite formed at or below the Bs temperature is similar in shape and properties to the acicular ferrite formed during supercooling in ultra-low carbon steel, and therefore, in the present invention, the total fraction of the bainitic ferrite and acicular ferrite is controlled. Therefore, in the present invention, the fraction of one or more selected from the acicular ferrite and the bainitic ferrite is controlled.
[0059] If the content of one or more selected from the acicular ferrite and bainitic ferrite is less than 10%, there is a problem that it is difficult to ensure elongation. On the other hand, if the content of one or more selected from the acicular ferrite and bainitic ferrite exceeds 25%, there is a problem that it is difficult to ensure a low-temperature transformation structure that plays a role in improving strength. On the other hand, according to one embodiment of the present invention, the lower limit of the fraction of one or more selected from the acicular ferrite and bainitic ferrite may be 12.4%, or the upper limit of the fraction of one or more selected from the acicular ferrite and bainitic ferrite may be 21.0%.
[0060] In this case, according to an embodiment of the present invention, the average size of at least one selected from acicular ferrite and bainitic ferrite may be 2.0 μm or more.
[0061] On the other hand, according to one embodiment of the present invention, more preferably, the lower limit of the average size of one or more selected from among the acicular ferrite and bainitic ferrite may be 3.9 μm, or the upper limit of the average size of the one or more selected from the acicular ferrite and bainitic ferrite may be 6.2 μm.
[0062] Furthermore, according to one embodiment of the present invention, the average spacing of one or more selected from among acicular ferrite and bainitic ferrite may be 3 μm or more. More preferably, according to one embodiment of the present invention, the lower limit of the average spacing of one or more selected from among acicular ferrite and bainitic ferrite may be 6.2 μm, or the upper limit of the average spacing of one or more selected from among acicular ferrite and bainitic ferrite may be 13.2 μm.
[0063] In this case, the average size of one or more selected from the acicular ferrite and bainitic ferrite means a circle equivalent diameter, and the average spacing of one or more selected from the acicular ferrite and bainitic ferrite means an average of the distances between the five most adjacent structures for each microstructure.
[0064] The low-temperature bainite and martensite formed after the tertiary cooling start to transform first at the point where nucleation is easy inside the austenite. As the phase transformation continues, the dislocation density inside the final transformation point becomes excessively high locally, and stress easily concentrates during the forming process, which causes fine cracks to form in the structure and deteriorates hole expandability. On the other hand, if soft acicular ferrite or bainitic ferrite is uniformly distributed in the low-temperature transformation structure, which is the base structure, it has the effect of uniformly accommodating deformation during forming, preventing localized stress concentration and improving hole expandability.
[0065] Therefore, when the average size of one or more selected from acicular ferrite and bainitic ferrite, which are soft structures, is less than 2.0 μm, the effect of deformation acceptance is low and improvement in hole expandability cannot be expected. In addition, when the average interval of one or more selected from acicular ferrite and bainitic ferrite is less than 3.0 μm, the fraction of soft steel increases excessively, so that the yield strength and tensile strength may decrease. Although the upper limit of the average size and the upper limit of the average interval of the soft structure are not separately regulated, under the condition that the total fraction of the soft structure satisfies the range of 10 to 25%, the average size of the soft structure is preferably 20 μm or less, and the average interval of the soft structure is preferably 20 μm or less.
[0066] The hot-rolled steel sheet of the present invention may contain, in addition to the above-mentioned structure, other phases such as ferrite, carbides, and retained austenite, but these are preferably controlled to an area fraction of 5% or less. Here, the above-mentioned ferrite means granular ferrite.
[0067] In particular, ferrite formed during cooling after hot rolling is usually characterized by low strength because it is formed by diffusion transformation. By controlling such ferrite to 5% or less (including 0%), the previously formed ferrite undergoes shear deformation to accommodate the lattice deformation generated when the retained austenite transforms into bainite and martensite after ferrite formation. Therefore, it was confirmed that the dislocation density inside the ferrite is maintained at a high level, and the strength of the steel does not decrease significantly even if it contains other phases such as ferrite at 5% or less. However, if the fraction of ferrite exceeds 5%, the strength of the steel decreases, which is not preferable.
[0068] On the other hand, carbides may be generated during the manufacturing process of the present product. Since the present invention utilizes a low-temperature transformation structure as the second phase to improve strength, the generation of carbides may cause a decrease in the second phase fraction. In other words, excessive generation of carbides hinders the strengthening effect targeted in the present invention. However, when Ti and Nb are present in the phase, alloy carbonitrides can be formed, and in this case, further strengthening effects due to grain refinement can be expected, but since coarse carbides hinder the toughness of the steel, it is preferable that the carbides present in the hot-rolled steel sheet of the present invention are less than 5%.
[0069] According to one embodiment of the present invention, the hot-rolled steel sheet may contain only retained austenite as the other phase as the microstructure. Therefore, the hot-rolled steel sheet may contain 5% or less (including 0%) of retained austenite as the microstructure in terms of area percent. During the secondary cooling of the present invention, when bainitic ferrite is generated, isolated island-like austenite in the growing bainitic ferrite does not transform into bainite and martensite in the subsequent cooling process due to carbon concentration, and can remain until room temperature. When the fraction of the retained austenite is low, the effect on physical properties may be slight, but when the fraction exceeds 5%, the hole expandability may deteriorate and hydrogen delayed fracture may occur. Therefore, the fraction of the retained austenite in the present invention is preferably 5% or less, and more preferably 3% or less. Meanwhile, according to one embodiment of the present invention, more preferably, the lower limit of the fraction of the retained austenite may be 0.9%, or the upper limit of the fraction of the retained austenite may be 2.1%.
[0070] The hot-rolled steel sheet of the present invention having the above-mentioned alloy composition and microstructure has high strength, such as a yield strength (YS) of 900 MPa or more (or 948 to 1064 MPa) and a tensile strength (TS) of 1180 MPa or more (or 1204 to 1343 MPa), while having excellent formability, such as an elongation (El) (i.e., El average) of 7% or more (or 8.4 to 12.6%), a standard deviation of the elongation of 2% or less (0.3 to 1.1%), and a hole expansion ratio (HER) of 25% or more (or 27 to 36%), and is characterized by a uniform material distribution within the steel sheet.
[0071] Next, a manufacturing method of an ultra-high strength steel sheet having excellent formability and uniform material properties within the steel sheet, which is yet another aspect of the present invention, will be described in detail below. However, this does not necessarily mean that the ultra-high strength steel sheet of the present invention should be manufactured by the manufacturing method described below.
[0072] The hot-rolled steel sheet according to the present invention can be manufactured by subjecting a steel slab having the alloy composition proposed in the present invention to a series of steps of [reheating - hot rolling - cooling - coiling]. The conditions of each of the above steps will be described in detail below.
[0073] [Steel slab reheating] In the present invention, it is preferable to carry out a step of reheating the steel slab and homogenizing it before carrying out the rolling step, and this can be carried out in a temperature range of 1100 to 1350°C.
[0074] If the temperature during reheating of the steel slab is less than 1100°C, there is a problem that the homogenization of the alloy elements is insufficient, while if the temperature exceeds 1350°C, excessive oxides are formed on the surface of the slab, which may deteriorate the surface quality of the steel sheet.
[0075] [Hot rolling] The reheated steel slab can be hot-rolled to produce a hot-rolled steel sheet. In this case, the hot rolling is preferably carried out in a temperature range of 750 to 1150°C, and the total reduction in the final two passes is preferably controlled to 10 to 40%.
[0076] If hot rolling is started at a temperature exceeding 1150°C, oxides are excessively formed on the surface of the steel sheet after rolling, and even if a pickling process is performed, they are not effectively controlled, resulting in poor surface quality. On the other hand, if hot rolling is performed at a temperature lower than 750°C, the rolling load increases excessively, resulting in poor workability, and ferrite is generated during rolling, resulting in poor anisotropy.
[0077] Usually, the reason for performing multi-stage rolling during hot rolling is to reduce the rolling load and precisely control the thickness. When performing hot rolling by such multi-stage rolling, if the sum of the rolling reductions (or the total rolling reduction) of the final two passes (the latter two passes) exceeds 40%, there is a problem that the rolling load of the final two passes becomes excessive and workability decreases. On the other hand, if the sum of the rolling reductions of the final two passes is less than 10%, there is a problem that the temperature of the steel sheet drops rapidly, inducing shape defects. On the other hand, according to one embodiment of the present invention, during the above hot rolling, the lower limit of the total rolling reduction of the final two passes may more preferably be 25%, or the upper limit of the total rolling reduction of the final two passes may more preferably be 38%.
[0078] On the other hand, the grain size of austenite after hot rolling is affected by the alloying composition, the rolling end temperature and the rolling reduction, which affect the formation behavior of ferrite and bainite in the subsequent cooling process and the final microstructure. In addition, the fraction and size of acicular ferrite or bainitic ferrite, which are the main constituent phases in the present invention, are greatly affected by the austenite grain size after hot rolling.
[0079] The size of the structure after phase transformation is affected by the phase transformation temperature and holding time because the grains of equiaxed ferrite and pearlite grow due to the diffusion of elements during phase transformation. On the other hand, acicular ferrite and bainitic ferrite generated by shear transformation such as bainite grow only within the austenite grains and cannot become larger than the size of the austenite before transformation. Therefore, in order to control the size of acicular ferrite and bainitic ferrite, it is advantageous to control the grain size of austenite after hot rolling.
[0080] Therefore, in the present invention, after hot rolling, the effective grain size of austenite is derived as a relationship between the rolling finish temperature (FDT) and a specific alloy composition, and specifically, is defined by the following Relation 1. That is, during hot rolling, finish hot rolling is performed within a temperature range of 750 to 1150°C so that the value of Du defined by the following Relation 1 satisfies the range of 2 to 10.
[0081] [Equation 1] Du=FDT+(7.4×[C])-(24.7×[Si])-(4.7×[Mn])-(3.9×[Cr])-(5.2×[Mo])-(560×[Ti])-(1110×[Nb])}×0.049-34.2 (In the above Relational Formula 1, FDT means the rolling finish temperature (°C), and [C], [Si], [Mn], [Cr], [Mo], [Ti] and [Nb] each represent the weight percent content of the element in parentheses.)
[0082] The above Du is an index indicating the effective grain size of austenite immediately before the primary cooling after hot rolling. When the value of Du defined in the above Relational Formula 1 is 2 or more, the average grain size of acicular ferrite and / or bainitic ferrite is 2.0 μm or more, and the hole expansion ratio can be secured to 25% or more. On the other hand, when the value of Du defined in the above Relational Formula 1 exceeds 10, the grain size of austenite before transformation becomes excessively coarse, the impact resistance decreases, and the grain boundary concentration of boron element increases, delaying the phase transformation during the secondary cooling, resulting in a problem of a decrease in elongation. On the other hand, according to one embodiment of the present invention, the lower limit of the value of Du defined in the above Relational Formula 1 may more preferably be 4.4, or the upper limit of the value of Du defined in the above Relational Formula 1 may more preferably be 7.8.
[0083] Meanwhile, according to one embodiment of the present invention, boron segregates to the grain boundaries of austenite to stabilize the austenite grain boundaries, thereby delaying the nucleation of ferrite and upper bainite and slowing down the phase transformation rate. In order to ensure the area fraction and average spacing of acicular ferrite or bainitic ferrite intended in the present invention, it is important to control the concentration of boron segregated to the grain boundaries of austenite. The concentration of boron segregated to the austenite grain boundaries shows different values for each grain boundary due to the influence of microsegregation during casting and the grain size of austenite. Among them, nucleation of acicular ferrite or bainitic ferrite occurs selectively in the second cooling stage in the austenite grain boundaries where the concentration of boron element is low. In general, when the austenite grain size is small, the concentration of boron segregated to each grain boundary is low and nucleation is smooth, and when the grain size is large, the concentration of boron segregated to the grain boundaries is high, so it can be expected that nucleation will be delayed. Therefore, the concentration of boron present at the grain boundary and the phase transformation behavior during secondary cooling are affected by the amount of boron added to the steel and the grain size of austenite, as shown in Relation 2.
[0084] Relational formula 2 is an index showing the concentration of boron (B) distributed at the grain boundaries of austenite just before cooling, and is expressed as Du × Bat × 2.968 × 10 10 The value of Va [=Du×Bat×2.968×10 10 ] is 5.0 × 10 6 If the ratio is less than Du × Bat × 2.968 × 10, the fraction of acicular ferrite or bainitic ferrite is excessive, and the yield strength and tensile strength cannot be ensured. 10 The value is 2.0×10 7 If the value of Va exceeds 8.60×10, the secondary cooling time for ensuring the fraction of acicular ferrite or bainitic ferrite becomes excessively long, resulting in a problem of reduced elongation. 6 Alternatively, the upper limit of the Va value is more preferably 1.89×10 7 may be also possible.
[0085] [Equation 2] 5.0×10 6 ≦Du×Bat×2.968×10 10 ≦2.0×10 7 (In the above Relational Formula 2, Du is defined as in Relational Formula 1, and Bat is 55.845×[B] / (1080.6+45.04×[B]), where [B] is the weight percent content of boron (B).)
[0086] FIG. 1 is a graph showing the relationship between the boron content and Du that simultaneously satisfies the above-mentioned Relational Formula 1 and Relational Formula 2, and the microstructure intended in the present invention can be secured within the solid line connecting ABCDEF.
[0087] [Cooling and winding] The hot-rolled steel sheet produced as described above is cooled, and it is preferable to cool the sheet in stages depending on the temperature to which the sheet is cooled.
[0088] Specifically, it is preferable to perform primary cooling of the hot-rolled steel sheet to a temperature of Bs or lower at a cooling rate of 50°C / s or more, secondary cooling to a temperature of (Bs+Ms) / 2 or higher at a cooling rate of 25°C / s or less for a time ts (seconds) defined in Relation 3, and then tertiary cooling to a temperature range of Ms°C to 500°C at a cooling rate of 30°C / s or more.
[0089] The hot-rolled steel sheet manufactured as described above is rapidly cooled to a temperature (Bs) at which bainite begins to form or below, thereby suppressing the formation of ferrite (granular ferrite). Then, the steel sheet is gradually cooled for a time ts (seconds) to an intermediate temperature between the bainite start temperature (Bs) and the martensite start temperature (Ms), or to a temperature higher than the intermediate temperature, thereby ensuring an area fraction of 10 to 25% of acicular ferrite or bainitic ferrite. Meanwhile, according to one embodiment of the present invention, more preferably, the lower limit of the cooling end temperature (T1) of the primary cooling may be 500°C, or the upper limit of the cooling end temperature (T1) of the primary cooling may be 540°C.
[0090] When the first cooling is performed at a temperature below Bs after the completion of the hot rolling, if the cooling rate is less than 50°C / s, there is a problem that the ferrite phase is excessively formed during cooling. In this case, the upper limit of the first cooling rate is not particularly limited, but it can be limited to 200°C / s or less because the steel sheet may be distorted in shape if it is cooled excessively. Meanwhile, according to one embodiment of the present invention, the lower limit of the cooling rate during the first cooling may be more preferably 70°C / s, or the upper limit of the cooling rate during the first cooling may be more preferably 100°C / s.
[0091] There is no particular lower limit for the end temperature of the primary cooling. However, if it is too low, there is a risk that the cooling time of the subsequent secondary cooling will be insufficient. Therefore, it is made clear that it can be limited to Bs-100°C.
[0092] When the temperature of the hot-rolled steel sheet reaches Bs or lower through the above-mentioned primary cooling, the intensive cooling is terminated, and secondary cooling can be carried out at a cooling rate of 25° C. / s or less and a temperature of (Bs+Ms) / 2 or higher.
[0093] In the above-mentioned primarily cooled hot-rolled steel sheet, growth of bainitic ferrite occurs while the steel sheet is cooled from the primarily cooled temperature to the target temperature of the secondary cooling. In particular, in order to obtain the target fraction in the present invention, it is preferable to maintain the above-mentioned secondary cooling for a time (ts, seconds (sec)) that satisfies the following Relation 3.
[0094] In Equation 3, k(T) is an index showing the growth rate of bainitic ferrite, and is affected not only by the alloying components of the steel but also by the phase transformation temperature and the grain size after hot rolling. Therefore, the value of Equation 3, that is, the relationship between k(T) and holding time (exp(-k(T)×(ts) 2 If the ratio of acicular ferrite or bainitic ferrite is less than 0.75, the proportion of acicular ferrite or bainitic ferrite will be excessive, and although the elongation will be excellent, the target level of strength will not be ensured. On the other hand, if the ratio exceeds 0.9, there will be a problem of deterioration in elongation.
[0095] [Equation 3] 0.75≦exp(-k(T)×(ts) 2 )≦0.9 (The above k(T) represents a value defined by the following relational expression 4.)
[0096] [Equation 4]
number
[0097] During the secondary cooling according to the above conditions, the temperature of the steel sheet may increase due to transformation heat caused by the bainite phase transformation. At this time, since the dislocation density may be excessively reduced due to excessive heat generation, the cooling rate during the secondary cooling may be controlled to 25°C / s or less in order to minimize the temperature increase of the steel sheet due to the transformation heat. If the cooling rate exceeds 25°C / s, the sheet shape may be distorted. In the present invention, it is clarified that the secondary cooling also includes an air cooling process. Meanwhile, according to one embodiment of the present invention, more preferably, the lower limit of the cooling rate during the secondary cooling may be 5.0°C / s, or the upper limit of the cooling rate during the secondary cooling may be 20.0°C / s.
[0098] Alternatively, according to one embodiment of the present invention, more preferably, exp(-k(T)×(ts)) according to the above relation 3 2 The lower limit of the value of exp(-k(T)×(ts)) may be 0.79, or exp(-k(T)×(ts))) according to the above relation 3. 2 The upper limit of the value of ) may be 0.88.
[0099] Alternatively, according to one embodiment of the present invention, the cooling end temperature (T2) of the secondary cooling may be lower than the cooling end temperature of the primary cooling. Alternatively, preferably, the cooling end temperature (T2) of the secondary cooling may be a temperature that is 20° C. or more lower than the cooling end temperature (T1) of the primary cooling. More preferably, the cooling end temperature (T2) of the secondary cooling may be a temperature that is 20° C. lower than the cooling end temperature (T1) of the primary cooling.
[0100] Alternatively, according to one embodiment of the present invention, more preferably, the lower limit of the cooling end temperature (T2) of the secondary cooling may be 480°C, or the upper limit of the cooling end temperature (T2) of the secondary cooling may be 520°C.
[0101] Alternatively, according to one embodiment of the present invention, more preferably, the lower limit of the cooling time of the secondary cooling may be 1.0 seconds, or the upper limit of the cooling time of the secondary cooling may be 4.0 seconds.
[0102] It is preferable that the hot-rolled steel sheet that has completed the secondary cooling as described above is tertiarily cooled to a temperature range of Ms to 500°C at a cooling rate of 30°C / s or more, and then coiled at that temperature. During the tertiary cooling, transformation of low-temperature bainite progresses, and a part of the untransformed austenite can be transformed to martensite even after coiling.
[0103] Therefore, by setting the cooling rate in the tertiary cooling to 30°C / s or more, further generation of high-temperature bainite during cooling can be avoided. On the other hand, if the cooling rate is too fast, the plate shape will be distorted by a large amount of cooling water, and the defective shape will again induce temperature deviation, increasing the material variation within the plate. Therefore, in the present invention, the cooling rate in the tertiary cooling stage accompanied by rapid phase transformation is preferably 100°C / s or less. On the other hand, according to one embodiment of the present invention, the lower limit of the cooling rate in the tertiary cooling may more preferably be 35°C / s, or the upper limit of the cooling rate in the tertiary cooling may more preferably be 80°C / s.
[0104] On the other hand, if the end temperature of the cooling, i.e., the coiling temperature, exceeds 500°C, the dislocation density inside the low-temperature bainite and martensite is excessively reduced, and the carbides become coarse, which may result in a decrease in yield strength and tensile strength. On the other hand, if the coiling temperature is Ms or lower, martensitic transformation progresses immediately before coiling, causing shape defects and temperature deviations, and increasing material quality variations within the steel sheet.
[0105] In the present invention, Bs and Ms can be calculated by the following formula, and each element means a weight content.
[0106] Bs(℃)=830-320×[C]-90×[Mn]-35×[Si]-70×[Cr]-120×[Mo] Ms(℃)=550-330×[C]-41×[Mn]-20×[Si]-20×[Cr]-10×[Mo]+30×[Al]
[0107] On the other hand, according to one embodiment of the present invention, more preferably, the lower limit of the cooling end temperature of the tertiary cooling may be 400°C, or the upper limit of the cooling end temperature of the tertiary cooling may be 430°C.
[0108] [Final cooling] After the cooling and coiling steps are completed as described above, the steel sheet is subjected to final cooling to obtain the desired hot-rolled steel sheet. At this time, the final cooling can be completed by air-cooling the steel sheet to room temperature.
[0109] On the other hand, the hot-rolled steel sheet of the present invention obtained after completing the final cooling as described above may be further pickled and oiled.
[0110] The pickled and oiled hot-rolled steel sheet can be heated to a temperature range of 420 to 740° C. to carry out a hot-dip galvanizing process.
[0111] The hot-dip galvanizing step can use a zinc-based plating bath, and there are no particular limitations on the alloy composition in the zinc-based plating bath. EXAMPLES
[0112] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for the purpose of illustrating the present invention and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0113] (Example) Steel slabs having the alloy compositions shown in Table 1 below were prepared, with the residual components of each steel slab being Fe and unavoidable impurities.
[0114] Each prepared steel slab was reheated at 1200°C, and then hot-rolled steel sheets having a thickness of 2.5 mm were manufactured through the processes of hot rolling, cooling, coiling, and final cooling (air cooling) under the conditions shown in Table 2 below. During the hot rolling, the total reduction rate of the final two passes was 25%, and the cooling rate during the first cooling was uniformly 70°C / s, and the cooling rate during the third cooling was uniformly 35°C / s.
[0115] The mechanical properties of each hot-rolled steel sheet were measured and the microstructure was observed, and the results are shown in Tables 3 and 4 below.
[0116] Among the mechanical properties, the yield strength, tensile strength and elongation were measured at room temperature using a universal tensile tester after taking JIS-5 standard test pieces at five points in the direction perpendicular to the rolling direction. At this time, the yield strength, tensile strength and elongation were expressed as the yield strength, maximum tensile strength and breaking elongation offset by 0.2%, respectively, and the elongation was shown with the standard deviation measured at five points.
[0117] The hole expandability was measured based on the ISO TS16630 standard method using the same test pieces as those used in the tensile test.
[0118] In addition, the microstructure of each hot-rolled steel sheet was observed at 10,000 magnifications using a scanning electron microscope and an image analyzer after etching the same test specimens as those used in the tensile tests using a Nital etching method, and the fraction of each phase was calculated. The average size of one or more selected from acicular ferrite and bainitic ferrite indicates the circle equivalent diameter, and the average spacing of one or more selected from acicular ferrite and bainitic ferrite indicates the average distance between the five most adjacent structures for each microstructure.
[0119] At this time, the microstructure was observed on the cross section of the test piece, that is, on the cross section perpendicular to the rolling direction.
[0120] [Table 1]
[0121] [Table 2] FDT*: Finish rolling temperature [℃] Du*={FDT+(7.4×[C])-(24.7×[Si])-(4.7×[Mn])-(3.9×[Cr])-(5.2×[Mo])-(560×[Ti)])-(1110×[Nb])}×0.049-34.2 Va*=Du×Bat×2.968×10 10
[0122] [Table 3] AC: Acicular ferrite BF: Bainitic ferrite LB: Low temperature bainite M: Martensite
[0123] [Table 4] YS: Yield strength TS: Tensile strength El: Elongation rate HER: Hole expansion ratio
[0124] As shown in Tables 1 to 3 above, Examples 1 to 12 of the present invention, which satisfy all of the alloy compositions and manufacturing conditions proposed in the present invention, were configured to satisfy the microstructure proposed in the present invention, thereby ensuring the target strength and formability.
[0125] On the other hand, in Comparative Example 1, which did not contain boron and did not satisfy the alloy composition system proposed by the present invention, excessive acicular ferrite and bainitic ferrite were generated during the secondary cooling, making it impossible to ensure the target strength, and due to this low strength, the elongation tended to be relatively high.
[0126] On the other hand, in Comparative Examples 2 to 8, although the alloy compositions satisfy the present invention, the manufacturing conditions deviate from the present invention.
[0127] Of these, Comparative Examples 2 and 3 are cases where the boron concentration at the grain boundaries was inappropriate and deviated from Relation 2. In Comparative Example 2, the boron concentration at the grain boundaries was excessive, resulting in an insufficient fraction of the soft structure, which is a secondary phase, and the elongation could not be ensured. On the other hand, in Comparative Example 3, the boron concentration at the grain boundaries was insufficient, resulting in an excessive fraction of the soft structure, which is a secondary phase, and as a result, the yield strength and tensile strength could not be ensured.
[0128] In Comparative Example 4, the value of Du defined by Relational Formula 1 did not satisfy the range of 2 to 10, and the size of the soft structure, which is the secondary phase, could not be ensured to be 2 μm or more. As a result, the stress concentration during deformation could not be effectively dispersed, and as a result, the hole expandability was reduced.
[0129] In Comparative Example 5, the secondary cooling time was insufficient, and thus Relational Expression 3 could not be satisfied. As a result, the fraction of the soft tissue, which is the secondary phase, was insufficient, and the elongation rate decreased.
[0130] In Comparative Example 6, the austenite grain size after hot rolling was excessively coarse, and the value of Du defined in Relational Formula 1 did not satisfy the range of 2 to 10. Therefore, the soft structure, which is a secondary phase, could not be uniformly distributed, the average interval was less than 3 μm, the secondary phase was locally dense, and stress concentration during deformation could not be effectively dispersed, resulting in a decrease in hole expandability.
[0131] In Comparative Example 7, not only was the Mn content insufficient, but the end temperature of the tertiary cooling was too low, causing martensite to form during the tertiary cooling, resulting in excessive temperature deviation within the plate and a standard deviation of the elongation of 2% or more, resulting in poor material variation within the steel plate.
[0132] 1 is a graph showing the relationship between the boron content and Du that simultaneously satisfies Relational Formula 1 and Relational Formula 2. The microstructure intended in the present invention can be secured within the solid line connecting ABCDEF.
[0133] Figure 2 shows photographs of the microstructures of Example 1 and Comparative Example 5 observed with a scanning electron microscope (SEM). As shown in Figure 2(a), Example 1 has a microstructure in which the matrix structure and secondary phase that the present invention aims to realize are appropriately formed. On the other hand, as shown in Figure 2(b), Comparative Example 5 shows that the soft structure, which is the secondary phase, is not sufficiently formed.
Claims
1. In weight percent, it contains carbon (C): 0.06-0.18%, silicon (Si): 0.01-1.8%, manganese (Mn): 1.6-3.5%, aluminum (Al): 0.001-0.1%, chromium (Cr): 2.5% or less (including 0%), molybdenum (Mo): 2.0% or less (including 0%), titanium (Ti): 0.01-0.15%, boron (B): 0.0005-0.003%, phosphorus (P): 0.0001-0.05%, sulfur (S): 0.0001-0.05%, nitrogen (N): 0.0001-0.02%, and the balance being Fe and other unavoidable impurities. The ultra-high strength hot-rolled steel sheet comprises, as a microstructure, 75 to 90% of one or more types selected from low-temperature bainite and martensite, 10 to 25% of one or more types selected from acicular ferrite and bainitic ferrite, and 5% or less (including 0%) of other phases, in terms of area fraction.
2. The ultra-high strength hot-rolled steel sheet according to claim 1, further comprising niobium (Nb): 0.01 to 0.2%.
3. The ultra-high strength hot rolled steel sheet according to claim 1, wherein the average size of the at least one selected from the group consisting of acicular ferrite and bainitic ferrite is 2.0 μm or more.
4. The ultra-high strength hot rolled steel sheet according to claim 1, wherein the average spacing of the at least one selected from the group consisting of acicular ferrite and bainitic ferrite is 3 µm or more.
5. 2. The ultra-high strength hot rolled steel sheet according to claim 1, wherein the hot rolled steel sheet has a yield strength of 900 MPa or more, a tensile strength of 1180 MPa or more, an elongation of 7% or more, and a standard deviation of elongation of 2% or less.
6. The ultra-high strength hot rolled steel sheet according to claim 1, having a hole expansion ratio of 25% or more.
7. reheating the steel slab containing, by weight, 0.06-0.18% carbon (C), 0.01-1.8% silicon (Si), 1.6-3.5% manganese (Mn), 0.001-0.1% aluminum (Al), 2.5% or less (including 0%) chromium (Cr), 2.0% or less (including 0%) molybdenum (Mo), 0.01-0.15% titanium (Ti), 0.0005-0.003% boron (B), 0.0001-0.05% phosphorus (P), 0.0001-0.05% sulfur (S), 0.0001-0.02% nitrogen (N), the balance being Fe and other unavoidable impurities, at a temperature range of 1100-1350°C; hot rolling the reheated steel slab to produce a hot rolled steel sheet; subjecting the hot-rolled steel sheet to a temperature of Bs or less at an average cooling rate of 50° C. / s or more; After the primary cooling, secondary cooling is performed at an average cooling rate of 25° C. / s or less to a temperature of (Bs+Ms) / 2 or more for a time period of ts (seconds); After the second cooling, a third cooling is performed at an average cooling rate of 30° C. / s or more to a temperature range of Ms° C. to 500° C.; and winding the tertiary cooled material in the temperature range. During the hot rolling, finish hot rolling is performed within a temperature range of 750 to 1150° C. so that the value of Du defined by the following Relation 1 satisfies the range of 2 to 10. [Relationship 1] Du={FDT+(7.4×[C])-(24.7×[Si])-(4.7×[Mn])-(3.9×[Cr])-(5.2×[Mo])-(560×[Ti])-(1110×[Nb])}×0.049-34.2 (In the above Relational Formula 1, FDT means the rolling end temperature (°C), and [C], [Si], [Mn], [Cr], [Mo], [Ti] and [Nb] each represent the weight percent content of the element in parentheses.)
8. The method for producing an ultra-high strength hot rolled steel sheet according to claim 7, further satisfying the following Relational Formula 2 during the hot rolling: [Relationship 2] 5.0×10 6 ≦Du×Bat×2.968×10 10 ≦2.0×10 7 (In the above-mentioned Relational Formula 2, Du is defined as in the Relational Formula 1, and Bat is 55.845×[B] / (1080.6+45.04×[B]), where [B] is the weight percent content of boron (B).)
9. The method for producing an ultra-high strength hot rolled steel sheet according to claim 7, wherein a total reduction in the final two passes during the hot rolling is 10 to 40%.
10. The method for producing an ultra-high strength hot rolled steel sheet according to claim 8, which satisfies the following relational expression 3. [Relationship 3] 0.75≦exp(-k(T)×(ts) 2 )≦0.9 (The above k(T) represents a value defined by the following relational expression 4.) [Relationship 4] [0010] (In the above-mentioned Relational Formula 4, Du is defined as in Relational Formula 1, and Bat is defined as in Relational Formula 2. In addition, T1 indicates the primary cooling end temperature [°C], and T2 indicates the secondary cooling end temperature [°C]. In addition, [C], [Si], [Mn], [Cr], and [Mo] each indicate the weight percent content of the element in parentheses.)
11. The method for producing an ultra-high strength hot rolled steel sheet according to claim 7, further comprising a step of final cooling to room temperature after the coiling.
12. The method for producing an ultra-high strength hot rolled steel sheet according to claim 11, further comprising pickling and oiling after the final cooling.
13. The method for producing an ultra-high strength hot rolled steel sheet according to claim 12, further comprising the step of hot dip galvanizing after the pickling and oiling.
Citation Information
Patent Citations
High strength hot rolled steel plate excellent in workability and its production
JP1994049591A
High strength steel and manufacturing method
JP2017507241A
High-strength hot-rolled steel sheet with excellent formability and manufacturing method thereof
JP2024530038A
High strength hot rolled steel sheet and manufacturing method for same
WO2017017933A1
High-strength hot-rolled steel sheet and method for manufacturing same
WO2020026593A1
Cited By
Hot-rolled steel sheet and its manufacturing method
JP2025541896A