Ultra-high strength cold-rolled steel sheet with excellent elongation ratio and its manufacturing method

A cold-rolled steel sheet with controlled Mn and C contents and a two-stage annealing process addresses the inverse elongation-strength issue, achieving 1.5 GPa tensile strength and 10% elongation for improved cold stamping formability.

JP2024543182AActive Publication Date: 2024-11-19POHANG IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024531660
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-29
Filing Date
2022-11-29
Publication Date
2024-11-19
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing cold-rolled steel sheets with ultra-high tensile strength face a challenge of inversely proportional elongation, limiting their formability and applicability in cold stamping due to poor drawing ratio and burring properties.

Method used

A cold-rolled steel sheet with a specific composition and microstructure, including controlled Mn and C contents, and a two-stage annealing process to create a gradient Mn concentration, ensuring a microstructure of 0.5-20% retained austenite and 80-99.5% martensite, enhancing strength and elongation.

Benefits of technology

The solution achieves a steel sheet with a tensile strength of 1.5 GPa and an elongation of 10% or more, suitable for cold stamping with improved formability and workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543182000001_ABST
    Figure 2024543182000001_ABST
Patent Text Reader

Abstract

The present invention relates to an ultra-high strength cold-rolled steel sheet having excellent elongation and a manufacturing method thereof, and more particularly to a cold-rolled steel sheet having a tensile strength of 1.5 GPa and at the same time having excellent elongation and suitable for cold stamping, and a manufacturing method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ultra-high strength cold-rolled steel sheet having excellent elongation and a manufacturing method thereof, and more particularly to a cold-rolled steel sheet having a tensile strength of 1.5 GPa and at the same time having excellent elongation and suitable for cold stamping, and a manufacturing method thereof. [Background technology]

[0002] In the domestic and overseas automobile industry, as carbon dioxide regulations are gradually tightening, the objectives of improving fuel efficiency, vehicle body stability for passenger protection, and weight reduction are emerging. To achieve these objectives, the use and development of ultra-high strength cold stamping steel sheets having tensile strength of 1.3 GPa or more is increasing compared to the high strength steels used in existing automobile parts. However, cold rolled sheets have poor formability because of the inverse proportional relationship in which the elongation rate decreases as the strength increases, and the application of cold stamping materials is generally very limited.

[0003] In order to solve the above problems, advanced high strength steels such as dual phase steels (DP steels) and transformation induced plasticity steels (TRIP steels) are used as composite steels that introduce low temperature transformation phases into a soft matrix to ensure excellent strength and elongation. As the times progress, there is a demand for cold rolled steel sheets with relatively excellent elongation and formability to be applied to corresponding vehicle parts while requiring improved strength rather than reduced thickness in the case of weight reduction to improve fuel efficiency. However, high strength steels with a strength of 1 GPa or more have the disadvantage of poor elongation and hole expansion ratio (HER) due to the occurrence of localized interphase hardness differences.

[0004] To overcome these shortcomings, ultra-high strength steel (UHSS) consisting only of bainite, which is a low-temperature transformation phase, and especially martensite, has been manufactured. This steel is mainly used for parts that can be formed by roll forming, even though it has low bendability.

[0005] Meanwhile, as the use of high-strength steel parts is gradually increasing, there is an increasing need for ultra-high strength steel with high ductility and its manufacturing method to satisfy the characteristics of various parts. However, the current situation is that a technology and manufacturing method for the high level that can meet the high-grade demand of having a tensile strength of 1.5 GPa or more and high ductility has not been developed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Korean Publication No. 2017-7022118 [Patent Document 2] Japan Application Publication No. 2016-28760 Summary of the Invention [Problem to be solved by the invention]

[0007] According to one aspect of the present invention, there is provided an ultra-high strength cold rolled steel sheet having an excellent elongation rate and a manufacturing method thereof.

[0008] Alternatively, according to one aspect of the present invention, there is provided a cold-rolled steel sheet having an ultra-high strength of 1.5 GPa or more, a total elongation of 10% or more, and suitable for use in cold stamping, and a manufacturing method thereof.

[0009] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding additional objects of the present invention from the entire contents of the specification of the present invention. [Means for solving the problem]

[0010] One aspect of the present invention is In weight percent, C: 0.15-0.3%, Si: 0.1-1.5%, Mn: 2.5-5.0%, P: 0.1% or less (0% excluded), S: 0.03% or less (0% excluded), Al: 0.01-0.1%, N: 0.01% or less (0% excluded), B: 0.005% or less (0% excluded), the balance being Fe and other unavoidable impurities. The microstructure contains, in terms of area percentage, retained austenite: 0.5 to 20% and martensite: 80 to 99.5%. A cold-rolled steel sheet is provided that satisfies the following relational expression 1-1. [Equation 1-1]

number

[0011] Another aspect of the present invention is reheating a steel slab having a composition, by weight percent, of C: 0.15-0.3%, Si: 0.1-1.5%, Mn: 2.5-5.0%, P: 0.1% or less (0% excluded), S: 0.03% or less (0% excluded), Al: 0.01-0.1%, N: 0.01% or less (0% excluded), B: 0.005% or less (0% excluded), the balance being Fe and other unavoidable impurities, to 1100-1300°C; hot rolling the reheated slab at 800 to 1000 ° C to obtain a hot rolled steel sheet; coiling the hot-rolled steel sheet at 400 to 700 ° C; cold rolling the coiled hot-rolled steel sheet at a rolling reduction of 20 to 75% to obtain a cold-rolled steel sheet; A first annealing step of heating the cold-rolled steel sheet to a temperature in the range of 600 to 700 ° C. and maintaining the temperature for 2 to 24 hours; a first cooling stage in which the cold-rolled steel sheet after the first annealing is cooled at an average cooling rate of 30°C / s or more; A secondary annealing step in which the above-mentioned primarily cooled cold-rolled steel sheet is heated to a temperature above the austenite single phase region at an average heating rate of 30°C / s or more; and a secondary cooling step of cooling the cold-rolled steel sheet after the secondary annealing at an average cooling rate of 30° C. / s or more. Effect of the Invention

[0012] According to one aspect of the present invention, there is provided an ultra-high strength cold rolled steel sheet having an excellent elongation rate and a method for producing the same.

[0013] Alternatively, according to one aspect of the present invention, it is possible to provide a cold-rolled steel sheet having an ultra-high strength of 1.5 GPa or more, a total elongation of 10% or more, and suitable for use in cold stamping, and a manufacturing method thereof.

[0014] According to one aspect of the present invention, instead of controlling a microstructure having a uniform chemical composition by utilizing the C and Mn contents of the entire steel sheet, a non-uniform gradient in chemical composition occurs despite the same main structure due to a gradient in the Mn content between the martensite main structure and the retained austenite obtained in the annealing region, and during processing, the microstructure with a relatively low Mn content yields, and as hard martensite deformation progresses, local stress and deformation occur within the boundary, and the elongation rate has the effect of increasing the strength of the microstructure with a low Mn content, thereby providing a 1.5 GPa class ultra-high strength steel sheet.

[0015] In addition, due to the Mn distribution, C and Mn in the martensite are additionally distributed to the remaining austenite, which ultimately ensures a more stable austenite than before. This minimizes martensite transformation in the uniform elongation region during sintering deformation, thereby providing a manufacturing method for cold-rolled steel sheet with high strength / yield ratio and excellent workability.

[0016] The various and beneficial advantages and effects of the present invention are not limited to the above-mentioned contents, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing a manufacturing process of a cold-rolled steel sheet according to one aspect of the present invention. [Diagram 2] FIG. 2(a) shows a crystallographic orientation map (Inverse Pole Figure, IPF), FIG. 2(b) shows a phase distribution map for the inventive steel, and FIG. 2(c) shows a phase distribution map enlarging a specific region where retained austenite is distributed in the final microstructure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0019] On the other hand, the terms used in this specification are intended to describe specific embodiments and are not intended to limit the present invention. For example, the singular form used in this specification includes the plural form unless the relevant definition clearly indicates otherwise. Furthermore, the meaning of "comprise" used in this specification embodies a configuration and does not exclude the presence or addition of other configurations.

[0020] Hereinafter, an ultra-high strength cold rolled steel sheet having an excellent elongation rate according to one aspect of the present invention will be described in detail.

[0021] According to one aspect of the present invention, the cold-rolled steel sheet contains, by weight%, C: 0.15-0.3%, Si: 0.1-1.5%, Mn: 2.5-5.0%, P: 0.1% or less (0% excluded), S: 0.03% or less (0% excluded), Al: 0.01-0.1%, N: 0.01% or less (0% excluded), B: 0.005% or less (0% excluded), the balance being Fe and other unavoidable impurities.

[0022] Hereinafter, the reasons for adding elements and the reasons for limiting the content of the cold rolled steel sheet according to the present invention will be described in detail. In this specification, the content of each element is expressed in weight percent unless otherwise specified.

[0023] Carbon (C): 0.15~0.3% Carbon (C) is an essential element for ensuring the strength and hardenability of martensitic steel, and is preferably added at 0.15% or more to obtain a tensile strength of 1.5 GPa or more. However, if the C content exceeds 0.3%, not only does the strength increase excessively and the elongation rate decrease compared to the target, but there is also a high potential for inducing brittle fracture, resulting in inferior spot weldability, so the upper limit is preferably controlled to 0.3% or less. On the other hand, the higher the carbon content, the greater the degree of carbide generation during martensite formation, so more preferably, the upper limit of the C content can be controlled to 0.27%.

[0024] Silicon (Si): 0.1-1.5% Silicon (Si) is added as a deoxidizer in the steelmaking process and, together with solid solution strengthening elements, suppresses the formation of carbides. In addition, the addition of Si plays a role in uniformly dispersing the structure during annealing heat treatment, and increases the stability of austenite during cooling, making it possible to secure retained austenite at room temperature. Therefore, in order to secure the above-mentioned effects, it is preferable to add Si at 0.15% or more. However, if the Si content exceeds 1.5%, excessive Si-based oxides are generated on the steel sheet surface during hot rolling, which may induce surface defects during cold rolling. In addition, the resistivity of the final cold-rolled steel sheet increases, resulting in poor spot weldability, so the Si content is controlled to 1.5% or less. Meanwhile, in order to improve the above-mentioned effects, the upper limit of the Si content may be more preferably 1.25%.

[0025] Manganese (Mn): 2.5-5.0% Manganese (Mn) is an austenite stabilizing element, and is added to ensure the hardening ability of martensite, and is easy to suppress the formation of ferrite during annealing heat treatment after cold rolling. If the Mn content is less than 2.5%, it is possible to ensure the hardening ability of martensite, but it is difficult to generate a gradient of Mn concentration in the cold rolled steel sheet, and it is difficult to ensure the non-uniform fine structure due to the Mn concentration difference pursued in the present invention. In addition, if the Mn content exceeds 5.0%, excessive strength and Mn bands in the base steel may occur in the thickness direction from the steelmaking and continuous casting stages, which deteriorates the impact resistance, so it is preferable to control the upper limit of the Mn content to 5.0% or less. However, in order to achieve the object of the present invention, it is more preferable to control the lower limit of the Mn content to 3.0% and the upper limit of the Mn content to 4.12%.

[0026] Phosphorus (P): 0.1% or less (0% excluded) Phosphorus (P) is an impurity element in steel, and when it exceeds 0.1%, P segregation not only deteriorates weldability, but also has a high potential to cause embrittlement of the steel, so the upper limit of the P content is controlled to 0.1%. Meanwhile, the lower limit of the P content can be set to 0% or less (i.e., more than 0%) in consideration of cases where P is unavoidably contained. However, in order to achieve the object of the present invention, the lower limit of the P content can be more preferably controlled to 0.005. Alternatively, the upper limit of the P content can be controlled to 0.03%, and most preferably to 0.02%.

[0027] Sulfur (S): 0.03% or less (0% excluded) Sulfur (S) is an impurity element that is inevitably added to steel, similar to P, and has the property of impairing the ductility and weldability of the final cold-rolled steel sheet. In addition, if the S content exceeds 0.03%, the precipitates generated in the hot rolling process due to the precipitation of MnS are not completely decomposed during the annealing heat treatment, which deteriorates the ductility of the steel sheet. In addition, there is a risk of causing problems in weldability, so the upper limit of the S content is controlled to 0.03% or less. Meanwhile, the lower limit of the S content may be excluded from 0% (i.e., more than 0%) in consideration of cases where it is unavoidably contained. However, in order to achieve the object of the present invention, more preferably, the lower limit of the S content may be controlled to 0.002% and the upper limit of the S content may be controlled to 0.005%.

[0028] Aluminum (Al): 0.01-0.1% Aluminum (Al), like Si, is added to remove oxygen from molten steel during steelmaking and is an element that is advantageous in removing impurity elements from steel. Although it is relatively weaker than Si, it is useful for suppressing carbide formation and contributes to stabilizing austenite C, making it possible to manufacture steel sheets with excellent elongation. Therefore, in order to ensure the above-mentioned effects, the Al content is controlled to 0.01% or more. However, if Al is added excessively, excessive precipitation of AlN may cause cracks in the slab, which may cause defects in the processed product, so the upper limit of the Al content is limited to 0.1%. Meanwhile, in order to ensure the effects of the present invention, more preferably, the lower limit of the Al content may be 0.02% and the upper limit of the Al content may be 0.06%.

[0029] Nitrogen (N): 0.01% or less (0% excluded) Nitrogen (N) is an impurity element in steel, and if its content exceeds 0.01%, the risk of cracks occurring during continuous casting due to the formation of AlN increases significantly, so the upper limit of the N content is limited to 0.01%. Meanwhile, the lower limit of the N content may exclude 0% (i.e., more than 0%) in consideration of cases where N is inevitably contained. However, in order to achieve the object of the present invention, it is more preferable that the lower limit of the N content be controlled to 0.007% and the upper limit of the N content be controlled to 0.03%.

[0030] Boron (B): 0.005% or less (0% excluded) Boron (B) is an element that is advantageous in suppressing the ferrite phase transformation during annealing heat treatment, and can improve the hardening ability of martensite through strengthening of grain boundaries and solid solution strengthening. However, if the B content exceeds 0.005%, the Fe 23Since (B,C)6 is formed in the austenite grain system and may cause brittle fracture in the hot rolling state, the upper limit of the B content is limited to 0.005% or less. Meanwhile, the lower limit of the B content may be set to 0% or less (i.e., more than 0%) in consideration of cases where B is inevitably contained. However, in order to achieve the object of the present invention, it is more preferable that the lower limit of the B content be controlled to 0.001% and the upper limit of the B content be controlled to 0.003%.

[0031] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, there is a possibility that unintended impurities are inevitably mixed in due to variables in the raw materials and surrounding environment, and it is not possible to exclude them. Since these impurities are known to anyone skilled in the normal steel manufacturing process, the contents of all of them will not be mentioned in this specification.

[0032] Meanwhile, according to one aspect of the present invention, the cold rolled steel sheet may further include at least one selected from Cr: 0.1% or less and Mo: 0.1% or less. Hereinafter, the reasons for adding each element and the reasons for limiting the content will be described.

[0033] Chromium (Cr): 0.1% or less (including 0%) Chromium (Cr) is an element that increases the hardening ability of martensite like Mn and inhibits ferrite transformation, thereby enabling the formation of martensite with an appropriate strength. Therefore, when the Mn content is designed within a certain range, the hardening effect of the Cr content is low, so that martensite strength can be ensured without adding Cr, and a small amount of Cr can be added. On the other hand, if the Cr content exceeds 0.1%, there is a risk of cracking due to local deformation and stress occurring at the boundary between the carbide and the structure in the steel during part molding due to the formation of coarse Cr-based carbides, so the upper limit of the Cr content can be controlled to 0.1%. However, since the case where Cr is not added can also be included, the lower limit of the Cr content can be 0%. On the other hand, when Cr is added, in order to achieve the object of the present invention, more preferably, the lower limit of the Cr content can be controlled to 0.005% and the upper limit of the Cr content can be controlled to 0.05%.

[0034] Molybdenum (Mo): 0.1% or less (including 0%) Molybdenum (Mo) is an element that, like Cr, enhances martensite hardening ability and is effective in suppressing ferrite formation in the cooling section during annealing heat treatment. However, since Mo is expensive compared to other elements, excessive addition of Mo causes a problem of increasing the cost of ferroalloy due to excessive alloy input. Therefore, in the present invention, the upper limit of the Mo content is limited to 0.1% or less. However, since Mo is expensive, if the object of the present invention can be achieved without adding Mo, it can be included in the scope of the present invention, so the lower limit of the Mo content can be 0% and the upper limit of the Mo content can be 0.05%.

[0035] According to one aspect of the present invention, the microstructure of the cold-rolled steel sheet contains, in terms of area fraction, 0.5 to 20% retained austenite and 80 to 99.5% martensite.

[0036] If the microstructure of the cold-rolled steel sheet contains less than 0.5% retained austenite or more than 99.5% martensite, the Mn content distribution is not properly performed, and the cold-rolled steel sheet is manufactured with a martensite matrix, which may cause a problem of insufficient elongation. If the microstructure of the cold-rolled steel sheet contains more than 20% retained austenite or less than 80% martensite, the carbon stability in the retained austenite may be reduced, and the formability may be deteriorated due to martensite transformation caused by deformation-induced transformation during processing. Meanwhile, according to one aspect of the present invention, in order to further improve the above-mentioned effects, the lower limit of the area fraction of the retained austenite may be 1.2%, or the upper limit of the area fraction of the retained austenite may be 10%. Meanwhile, according to another aspect of the present invention, in order to further improve the above-mentioned effects, the lower limit of the area fraction of the martensite may be 90%, or the upper limit of the area fraction of the martensite may be 98.5%.

[0037] According to one aspect of the present invention, the cold-rolled steel sheet can satisfy the following relational expression 1-1. [Equation 1-1]

number

[0038] According to the present invention, the above AF Mn_s / AF Mn_h If the value of AF is less than 5, it is difficult to realize the additional strength effect resulting from the difference in Mn content, and it is difficult to secure the retained austenite, which may limit the production of cold-rolled steel sheets having a total elongation of 10% or more. Mn_s / AF Mn_hIf the value of AF exceeds 25, the C and Mn contents are correspondingly high, and a problem may occur in that the workability is deteriorated due to the formation of Mn bands and carbides in the cold rolled steel sheet. Mn_s / AF Mn_h The lower limit of the value of AF may be 9, or Mn_s / AF Mn_h The upper limit of the value of can be 19.

[0039] The above AF Mn_s and A.F. Mn_h There is no particular limitation on the method of measurement. However, as a representative example, mechanical polishing is performed from the surface of the steel sheet to a position 1 / 4t away from the total thickness t of the steel sheet, and then an EPMA surface analysis is performed to quantitatively measure the Mn content at an area magnification of 30 μm×30 μm. Then, the area having a martensite structure with a locally high Mn content and the area having a martensite structure with a locally low Mn content are analyzed, respectively, so that the measurement can be performed.

[0040] Meanwhile, although not particularly limited, according to one aspect of the present invention, the cold-rolled steel sheet may satisfy the following Relational Expression 1-2. At this time, by satisfying the following Relational Expression 1-2, additional strength is realized in a region where the Mn content is relatively low, and a cold-rolled steel sheet of 1.5 GPa class can be manufactured, so that the hardness difference in the structure can be reduced and a superior elongation rate can be secured compared to existing martensitic steel. Meanwhile, according to one aspect of the present invention, the Δσ TS The lower limit of the value of Δσ can be 829 MPa, or the above Δσ TS The upper limit of the value may be 1844 MPa. [Equation 1-2]

number

[0041] On the other hand, the above σ TS_Mn_h and σ TS_Mn_s For each region, σ is defined by the following equation 1-3. TS Therefore, the above σ TS_Mn_h can be determined by the content of each component determined through EPMA analysis in a region having a martensite structure with a locally high Mn content. TS_Mn_s can be determined by the content of each component determined through EPMA analysis in a region having a martensite structure with a locally low Mn content.

[0042] [Equation 1-3]

number

[0043] In order to achieve the intended effect of the present invention, it is necessary to control the annealing heat treatment process to distribute the Mn concentration in martensite, obtain hard / soft phases according to the Mn concentration, and induce additional strengthening in the hard phase through deformation distribution. By ensuring austenite stability in the hard Mn phase through such a Mn concentration gradient, it is possible to provide an ultra-high strength steel with excellent elongation by securing retained austenite at room temperature.

[0044] The cold-rolled steel sheet according to the present invention has a tensile strength of 1500 MPa or more (or 1500 MPa to 1700 MPa, or 1554 MPa to 1660 MPa) and a total elongation rate of 10% or more (or 10% to 12%, or 10.2% to 11.2%), and can be used as an ultra-high strength cold-rolled steel sheet with excellent elongation rate suitable for cold stamping. Meanwhile, although not particularly limited, in order to achieve the object of the present invention, the yield strength of the cold-rolled steel sheet may be 940 MPa or more (or 940 MPa to 1200 MPa, or 1000 MPa or more, or 1000 MPa to 1200 MPa). In addition, according to one aspect of the present invention, the uniform elongation rate of the cold-rolled steel sheet may be 5.0% or more, or 5.0% to 7.0%.

[0045] Hereinafter, a method for producing a cold-rolled steel sheet according to one aspect of the present invention will be described in detail. However, the method for producing a cold-rolled steel sheet according to the present invention does not necessarily mean that the cold-rolled steel sheet must be produced by the following production method.

[0046] Slab reheat stage A method for producing a cold-rolled steel sheet according to one aspect of the present invention includes a step of reheating a steel slab having the above-mentioned composition to 1,100 to 1,300° C. At this time, the composition of the steel slab is the same as that of the above-mentioned cold-rolled steel sheet, and the reasons for adding each component and the reasons for limiting the content in the slab can be the same as those described above for the cold-rolled steel sheet.

[0047] Meanwhile, in the present invention, it is preferable to reheat the steel slab and perform a homogenization process prior to hot rolling, and the reheating temperature is preferably 1,100 to 1,300°C. If the reheating temperature is less than 1,100°C, there is a risk of a problem that the load increases suddenly during the subsequent hot rolling. Also, if the reheating temperature exceeds 1,300°C, there is a risk of the amount of surface scale increasing, leading to material loss.

[0048] Hot rolling stage The reheated slab is preferably hot-rolled at 800 to 1,000°C to produce a hot-rolled steel sheet. If the hot-rolling temperature is less than 800°C, the rolling load may increase due to the introduction of unrecrystallized ferrite, which is not preferred. On the other hand, if the hot-rolling temperature exceeds 1,000°C, the possibility of surface defects due to scale and increased wear of the rolling rolls is high, which is not preferred.

[0049] Winding stage The hot-rolled steel sheet manufactured by the above-mentioned hot rolling is preferably coiled at 400 to 700°C. If the coiling temperature exceeds 700°C, an excessive oxide film is formed on the surface of the steel sheet, which induces defects, and therefore it is preferable to limit this. On the other hand, if the coiling temperature is low, below 400°C, the strength of the hot-rolled steel sheet becomes excessively high, which not only increases the rolling load in the cold rolling process, but also increases the number of control variables during the cold rolling process in order to control this, which may result in poor productivity.

[0050] Cold rolling stage The oxide layer formed on the surface of the hot-rolled steel sheet coiled after the hot rolling is removed in a pickling process, and then cold rolling is performed at a rolling reduction of 20 to 75% to produce a cold-rolled steel sheet. If the rolling reduction is less than 20% during the cold rolling, not only is it difficult to ensure the target thickness, but the remaining hot-rolled crystal grains affect the formation of austenite during annealing heat treatment and the final physical properties. Therefore, it is preferable to perform the cold rolling at a rolling reduction in the range of 20 to 75%.

[0051] The present invention is directed to producing a highly elongated cold rolled steel sheet having mechanical properties with an elongation rate of 10% or more while ensuring a tensile strength of 1.5 GPa class, and for this purpose, a two-stage annealing process including a primary annealing-primary cooling-secondary annealing-secondary cooling process is carried out as shown in Fig. 1. The following will explain the process in detail.

[0052] First annealing stage The cold-rolled steel sheet obtained by the above-mentioned cold rolling is heated to a temperature range of 600 to 700°C (or 620 to 700°C) and maintained for 2 to 24 hours. In the present invention, in order to reduce the influence of reverse transformation due to the average heating rate during heating in the first annealing stage, the two-phase region temperature (T IA The annealing temperature is controlled to be in the range of 600°C to 700°C, and the maintenance time is controlled to be 2 hours or more so that Mn decomposition occurs.

[0053] Although not particularly limited, if the heating rate during the primary annealing is less than 30°C / s, a problem may occur in that the effect of C and Mn non-uniformity is small during the primary two-phase annealing. On the other hand, if the heating rate during the primary annealing exceeds 50°C / s, the accuracy of the target temperature of the primary annealing decreases, and a problem may occur in the quality of the final steel grade due to the temperature deviation in the annealing region.

[0054] The heat treatment conditions in the first annealing step described above are controlled to be satisfied, and at the same time, cooling is carried out at an average cooling rate of 30°C / s or more in the first cooling step described below, and this heat treatment generates a difference in Mn concentration between ferrite and austenite generated in the two-phase region, and obtains ferrite with a low Mn concentration and martensite with a high Mn content upon cooling. In the first annealing, the maintenance time is preferably within a range of up to 24 hours to more preferably maximize the Mn concentration.

[0055] Meanwhile, although not particularly limited, in order to further improve the intended effect of the present invention, the primary annealing step may be performed by heating the steel sheet so that the maximum temperature is in the range of 600 to 700°C based on the surface temperature of the steel sheet, and the time for maintaining the temperature range of 600 to 700°C from the time the maximum temperature is reached may be 2 to 24 hours.

[0056] In addition, if the duration of the primary annealing is less than 2 hours, the effect of C and Mn distribution in the two-phase temperature range is small, and the C and Mn concentrations in the ferrite martensite during cooling may be uniform. On the other hand, if the duration of the primary annealing is more than 24 hours, the grains may become coarse, causing deterioration of the material properties, and the heterogeneity of the C and Mn concentrations in the ferrite and austenite during annealing may be weakened.

[0057] First cooling stage The cold-rolled steel sheet after the primary annealing is subjected to primary cooling at an average cooling rate of 30° C. / s or more. More specifically, the primary cooling step may be performed at an average cooling rate of 30 to 50° C. / s to 25° C. or less.

[0058] If the average cooling rate in the first cooling step is less than 30°C / s, redistribution of C and Mn occurs during cooling after the first annealing, which may cause problems in ensuring chemical non-homogeneity. Also, if the temperature range in the first cooling step exceeds 25°C, extreme Mn and C distribution during the first annealing causes differences in the formation and end temperatures of martensite between grains, and even in the low temperature region, problems with the introduction of second phases may occur due to the fraction of untransformed austenite.

[0059] Second annealing stage In order to ultimately obtain an annealed cold-rolled steel sheet having an area fraction of martensite of 80% or more (and retained austenite of 20% or less), the above-mentioned primarily cooled cold-rolled steel sheet is subjected to secondary annealing in which the sheet is heated to a temperature above the austenite single phase region at an average heating rate of 30°C / s or more (more preferably, in the range of 30 to 50°C / s).

[0060] At this time, in the second annealing step, the average heating rate is controlled to 30° C. / s or more in order to maintain the Mn distribution obtained in the first annealing step. If the average heating rate in the second annealing step is less than 30° C. / s, a problem may occur in which the Mn concentration difference becomes uniform due to Mn redistribution.

[0061] In the second annealing step, the temperature above the austenite single phase region may be 820°C or higher (more preferably, 850°C or higher and 900°C or lower), and the reason for controlling the temperature within the above range is to generate 80% or more martensite, which is the final microstructure, from the Mn-distributed austenite.

[0062] Meanwhile, in order to further improve the intended effect of the present invention, it is preferable to control the average heating rates in the first annealing step and the second annealing step so as to satisfy the following Relational Formula 2. [Equation 2] 1.0≦TH1 / TH2≦1.5 (In the above Relational Formula 2-1, TH1 indicates the maximum temperature of the steel sheet surface in the first annealing stage, and TH2 indicates the maximum temperature of the steel sheet surface in the second annealing stage.)

[0063] Secondary cooling stage Next, the cold-rolled steel sheet after the secondary annealing is subjected to secondary cooling at an average cooling rate of 30°C / s or more (more preferably, in the range of 30 to 50°C / s). At this time, if the average cooling rate in the secondary cooling step is less than 30°C / s, a problem may occur in ensuring the elongation rate due to redistribution of C and Mn during cooling.

[0064] According to the present invention, in order to obtain a cold-rolled steel sheet having mechanical properties of 1.5-grade strength and a total elongation of 10% or more, precise control of the critical heating rate and heat treatment temperature in the two-stage annealing process and the critical cooling rate and cooling temperature in the cooling process is required. If the critical heating rate and heat treatment temperature are not controlled, it may be difficult to obtain the tensile strength and elongation within the ranges targeted by the present invention. EXAMPLES

[0065] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for the purpose of illustrating the present invention and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.

[0066] (Example) Steel having the composition shown in Table 1 below was vacuum melted into an ingot, which was then maintained at 1200°C for 1 hour, finish-rolled at 900°C, loaded into a furnace preheated to 600°C and maintained there for 1 hour, and then cooled in the furnace to simulate hot rolling and coiling. After pickling, the ingot was cold-rolled at a reduction ratio of 50% to produce a cold-rolled steel sheet.

[0067] The cold-rolled steel sheets thus manufactured were heated in various two-phase temperature ranges at an average heating rate of 30°C / s and then subjected to primary annealing with different maintenance times under the conditions shown in Table 2. Then, primary cooling was performed to 25°C at an average cooling rate of 30°C / s, and secondary annealing was performed by heating to 870°C in the austenite single phase region at an average heating rate of 30°C / s, and secondary cooling was performed at an average cooling rate of 30°C / s to simulate continuous annealing heat treatment.

[0068] For each heat-treated specimen, the residual austenite fraction in the specimen, including the micro-austenite, was measured using the magnetic induction method (Metis), and the fraction outside the specimen was calculated from the martensite. In order to analyze the Mn concentration difference within the same martensite, EPMA surface analysis was performed at 1,000 times magnification or more, and the results are shown in Table 2 below, and the results of measuring the mechanical properties are shown in Table 3 below. At this time, to measure the mechanical properties, the specimens were processed perpendicular to the rolling direction according to the JIS standard, and a tensile tester and elongation meter were attached to measure the yield strength, tensile strength, and elongation. In addition, AF Mn_s / AF Mn_h and Δσ TS was measured in the same manner as described herein.

[0069] [Table 1]

[0070] [Table 2] (In Table 2 above, F: ferrite, M: martensite, P: pearlite, and γ: retained austenite.)

[0071] [Table 3]

[0072] In the case of Examples 2, 3, 5, 7 and 8, which satisfy the alloy composition and manufacturing conditions of the present invention, the relational formula 1-1 is satisfied, and thus not only are the tensile strength of 1500 MPa or more, the yield strength of 1000 MPa or more, the total elongation rate of 10% or more, and the uniform elongation rate of 5.0% or more satisfied, but the relational formula 1-2 is also satisfied, ensuring uniformity.

[0073] In particular, the final microstructure after the second annealing and second cooling for Example 8 was measured at a high degree of accuracy using electron backscatter diffraction (EBSD) and is shown in Figure 2. Figure 2(a) shows a crystallographic orientation map (inverse pole figure, IPF), Figure 2(b) shows a phase distribution map for the inventive steel, and Figure 2(c) shows a phase distribution map enlarging a specific region where retained austenite is distributed in the final microstructure.

[0074] On the other hand, it was confirmed that Examples 9 to 15, which do not satisfy the alloy composition of the present invention, fail to satisfy at least one of the tensile strength of 1500 MPa or more, the yield strength of 1000 MPa or more, the total elongation rate of 10% or more, and the uniform elongation rate of 5.0% or more.

[0075] In addition, in the case of Example 1, which satisfies the alloy composition of the present invention but does not satisfy the manufacturing conditions because the primary annealing temperature is too low, there is a problem that the cementite formed in the ferrite is not completely dissolved and remains after the secondary annealing, and as a result, the total elongation rate was 10% or less.

[0076] In addition, in the case of Examples 4 and 6, which satisfy the alloy composition of the present invention but cannot satisfy the manufacturing conditions because the primary annealing temperature is too high, the primary annealing temperature was 720°C, which is outside the annealing range in which Mn distribution can occur at a maximum, and the Mn concentration difference was small. As a result, it was difficult to ensure the residual austenite fraction in the final microstructure, and the elongation did not reach 10%.

Claims

1. In weight percent, C: 0.15-0.3%, Si: 0.1-1.5%, Mn: 2.5-5.0%, P: 0.1% or less (0% excluded), S: 0.03% or less (0% excluded), Al: 0.01-0.1%, N: 0.01% or less (0% excluded), B: 0.005% or less (0% excluded), the balance being Fe and other unavoidable impurities, The microstructure contains, in terms of area percentage, retained austenite: 0.5 to 20% and martensite: 80 to 99.5%; A cold-rolled steel sheet satisfying the following relational formula 1-1. [Relationship 1-1] [0010] (In the above-mentioned Relational Formula 1-1, the AF Mn_s indicates the area fraction of low Mn crystal grains in the martensite having a Mn content of more than 2% and less than 5%, and its unit is area %. Mn_h indicates the area fraction of high Mn crystal grains in which the Mn content in the martensite is 5% or more, and its unit is area %.)

2. The cold-rolled steel sheet according to claim 1, which satisfies the following relational formula 1-2. [Relationship 1-2] [0025] (In the above-mentioned Relational Formula 1-2, the above-mentioned Δσ TS is the average tensile strength (σ) of high Mn grains in the martensite having an Mn content of 5% or more. TS_Mn_h ) and the average tensile strength (σ TS_Mn_s ) and its unit is MPa.

3. The cold-rolled steel sheet according to claim 1, further comprising one or more selected from the group consisting of Cr: 0.1% or less (including 0%) and Mo: 0.1% or less (including 0%).

4. The cold-rolled steel sheet according to claim 1, having a tensile strength of 1500 MPa or more and a total elongation of 10% or more.

5. The cold rolled steel sheet according to claim 1, having a yield strength of 1000 MPa or more.

6. reheating a steel slab having a composition, by weight percent, of C: 0.15-0.3%, Si: 0.1-1.5%, Mn: 2.5-5.0%, P: 0.1% or less (0% excluded), S: 0.03% or less (0% excluded), Al: 0.01-0.1%, N: 0.01% or less (0% excluded), B: 0.005% or less (0% excluded), the balance being Fe and other unavoidable impurities, to 1100-1300°C; hot rolling the reheated slab at 800 to 1000°C to obtain a hot rolled steel sheet; coiling the hot-rolled steel sheet at 400 to 700 ° C.; cold rolling the coiled hot-rolled steel sheet at a rolling reduction of 20 to 75% to obtain a cold-rolled steel sheet; a first annealing step of heating the cold-rolled steel sheet to a temperature in the range of 600 to 700 ° C. and maintaining the temperature for 2 to 24 hours; A primary cooling step of cooling the cold-rolled steel sheet after the primary annealing at an average cooling rate of 30 ° C. / s or more; A secondary annealing step of heating the primarily cooled cold-rolled steel sheet to a temperature above the austenite single phase region at an average heating rate of 30 ° C. / s or more; and a secondary cooling step of cooling the cold-rolled steel sheet after the secondary annealing at an average cooling rate of 30° C. / s or more.

7. The method for producing a cold-rolled steel sheet according to claim 6, wherein the first annealing step has an average heating rate of 30° C. / s or more.

8. The method for producing a cold-rolled steel sheet according to claim 6, which satisfies the following relational expression 2. [Relationship 2] 1.0≦TH1 / TH2≦1.5 (In the above Relational Formula 2-1, TH1 indicates the maximum temperature of the steel sheet surface in the first annealing stage, and TH2 indicates the maximum temperature of the steel sheet surface in the second annealing stage.)

Citation Information

Patent Citations

  • Steel sheet

    WO2020262652A1

  • Steel sheet and method for producing same

    WO2021200164A1

  • Eyesight display device

    JP2016028760A

  • KR2017-7022118