Anode materials, batteries
The continuous graphitization process for artificial graphite addresses production inefficiencies and uneven heating in conventional methods, achieving improved lithium ion diffusion and capacity through controlled pore structure and surface area, resulting in high-performance negative electrode materials.
Patent Information
- Application Number
- JP2024508517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-11-16
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-11-16
AI Technical Summary
Conventional graphite-based negative electrode materials for lithium-ion batteries face limitations in continuous production, long production cycles, uneven heating leading to uncontrolled variations in pore structure, and inadequate synergistic effects between multiple elements, failing to meet market demands for low-cost, high-performance materials.
A continuous graphitization process is employed to produce artificial graphite with controlled pore volume, specific surface area, and tap density within specific ranges, ensuring uniform release and absorption of lithium ions, and incorporating amorphous carbon to enhance diffusion channels and electrochemical reactions.
The process results in improved lithium ion diffusion, reduced diffusion resistance, enhanced electrochemical reaction interfaces, and increased capacity and rate characteristics of the negative electrode material, with lower energy consumption and production costs.
Smart Images

Figure 2024543293000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of anode materials, specifically to anode materials, batteries. [Background technology]
[0002] At present, graphite has become the mainstream negative electrode material for commercial lithium-ion batteries due to its advantages such as high electrical conductivity, large lithium ion diffusion coefficient, small volume change before and after lithium absorption in its layered structure, high lithium absorption capacity, and low lithium absorption potential.
[0003] Conventional graphitization equipment for graphite anodes is mainly divided into two types: crucible furnace and box furnace. Both of them are batch-type operations, and the graphitization process requires power outages, making it impossible to realize continuous production. In addition, the heating and cooling processes of the equipment are particularly limited, and the heating and cooling speed is slow, resulting in a long production cycle. Generally, the graphitization cycle is within 15 to 45 days. In the graphitization production process, volatile components and impurity elements in the raw materials are released under high temperature conditions, forming pores inside and / or on the surface of the graphite. Generally, all artificial graphites have a certain number of pore structures, and the presence of pores is due to the Li + increases the diffusion channels inside the graphite material, and Li + It can reduce the diffusion resistance of the graphite, thereby effectively improving the rate performance of the material. In fact, simply improving the pore structure alone cannot achieve optimal rate performance, and there is still a lot of room for improvement. Researchers have only studied the effect of a single element on the performance of graphite materials, and have not deeply studied the synergistic effects between multiple elements to maximize the improvement of graphite rate performance.
[0004] Therefore, at the current stage when graphite materials are already mature, improving a single parameter alone cannot meet the market demand for low-cost, high-performance graphite materials. It is necessary to study the synergistic action mechanism of various factors and develop graphite anode materials that meet the market demand. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of this, the present application provides a negative electrode material and a battery that can improve the rate characteristics and capacity of the negative electrode material while improving the processing performance of the material. [Means for solving the problem]
[0006] According to a first aspect, the present application provides an anode material, the anode material comprising artificial graphite, the artificial graphite having an internal and / or surface pore structure, the anode material having a pore volume of Vcm 3 / kg, specific surface area is Sm 2 / g and tap density is Tg / mL, V×S / T is 8.5≦V×S / T≦27, The pore volume was measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated within the pore diameter range of 17 Å to 3000 Å using the BJH Desorption cumulative volume of pores model.
[0007] In some embodiments, the negative electrode material has a pore volume of Vcm 3 / kg, 5.0≦V≦8.0.
[0008] In some embodiments, the negative electrode material has a specific surface area of Sm 2 / g, 1.78≦S≦3.00.
[0009] In some embodiments, the negative electrode material has a tap density, Tg / mL, of 0.734≦T≦1.160.
[0010] In some embodiments, the pores include at least one of micropores and mesopores.
[0011] In some embodiments, the pores have an average pore diameter of 50 Å to 200 Å.
[0012] In some embodiments, the negative electrode material has a d spacing of the (002) plane of the graphite crystal measured by X-ray diffraction. 002 When the 002 ≦3.364 Å.
[0013] In some embodiments, the particle size D of the negative electrode material 50 is 10 μm to 30 μm.
[0014] In some embodiments, the negative electrode material includes primary particles of synthetic graphite and / or secondary particles of synthetic graphite.
[0015] In some embodiments, the negative electrode material further comprises amorphous carbon.
[0016] In some embodiments, the negative electrode material further includes amorphous carbon, and a mass percentage of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.
[0017] According to a second aspect, the present application provides a battery comprising the anode material according to the first aspect. Effect of the Invention
[0018] The technical solution of the present application has at least the following beneficial effects: The negative electrode material provided by the present application includes artificial graphite having internal and / or surface pores, and the pore volume of the negative electrode material is Vcm 3 / kg, specific surface area is Sm 2 / g and tap density Tg / mL, 8.5≦V×S / T≦27. In general, a certain range of pore volume of artificial graphite can increase the diffusion channel of lithium ions, reduce the diffusion resistance of lithium ions, and effectively improve the rate characteristics of the material, and a certain range of specific surface area can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce the concentration polarization, and is favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has found through a large amount of intensive research that when lithium ions move, the migration speed is not only related to the migration space (i.e., the size of the pore volume) and the size of the reaction interface, but also related to the friction conditions of the artificial graphite surface, so even if the pore volume and specific surface area are sufficient, it does not necessarily guarantee that lithium ions are completely released and absorbed, and the friction conditions can directly affect the size of the tap density. By limiting V×S / T to this range, it is possible to ensure that lithium ions are released and absorbed more smoothly inside the artificial graphite material particles at appropriate spatial and reaction interfaces, thereby greatly improving the rate and capacity of the material.
[0019] The negative electrode material provided by the present application is produced and processed by a continuous graphitization process, in which all materials are continuously charged and discharged, and the time and temperature of all materials passing through the high temperature zone are the same, and the graphitization process controls the temperature rise and fall rate, so that volatile components, impurity elements and other substances in the material can be uniformly and quickly released, thereby realizing accurate control of the graphite internal and / or surface pore volume, and realizing control of the pore volume and material specific surface area. The above process methods are used synergistically to overcome the problems of uneven heating of materials due to the temperature gradient at different positions in the graphitization furnace, and the large variation and inability to control indexes such as the specific surface area, pore volume, tap density and other indexes of the produced and processed products, so that the pore volume, specific surface area and tap density of the processed material reach the ideal control design requirements.
[0020] The negative electrode material provided by the present application has low energy consumption per unit mass, obvious advantages in cost and production cycle, and is environmentally friendly. [Brief description of the drawings]
[0021] [Figure 1] 1 is a scanning electron microscope photograph of the negative electrode material provided in Example 10 of the present application. [Diagram 2] FIG. 2 is a magnified view of a scanning electron microscope photograph of the negative electrode material provided in Example 10 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] In order to better explain the present application and facilitate understanding of the technical solution of the present application, the present application will be described in more detail below, however, the following examples are merely simplified examples of the present application, and do not indicate or limit the scope of protection of the present application, and the scope of protection of the present application shall be governed by the claims.
[0023] In the field of anode materials, the development of continuous graphitization equipment has continued for decades, and as early as 1987, a patent (US06619591) disclosed an apparatus capable of performing continuous graphitization treatment on carbon-containing materials. In recent years, applicants have also continued to develop continuous graphitization equipment, for example, a patent with registration publication number CN211425033U filed in 2019 discloses a vertical continuous kiln for producing anode materials for lithium batteries, which can continuously discharge from an outlet and continuously charge from a material pipe. Compared with conventional processes, the continuous graphitization process shortens the graphitization time from several days to several hours, which significantly reduces energy consumption, but compared with conventional artificial graphite, the continuous graphitization process can result in changes in the microstructure of artificial graphite, especially changes in the internal pore structure and crystal form of artificial graphite. Conventionally, the industry has found that such modifications are difficult to meet the required performance of artificial graphite and difficult to improve, so even though continuous graphitization equipment has existed for 30 to 40 years, there is no precedent for successful mass production of continuously graphitized artificial graphite anode products.
[0024] In recent years, with the increasing energy scarcity, in order to further reduce the cost of artificial graphite, the applicant continues to develop the application of continuous graphitization equipment, develops an artificial graphite anode material that is equivalent to or even better than the current normal graphitized anode material in terms of performance, and aims to reduce the energy consumption of the artificial graphite anode material and further reduce the cost. The applicant has developed a variety of means to improve the rapid rise and fall of temperature that brings unfavorable changes to artificial graphite products through the development of a large-scale preparation process, and obtains a series of different types of artificial graphite anode materials through product selection. Although these artificial graphite anode materials have different microstructures from normal artificial graphite products, their electrical performances can all be basically equivalent to normal artificial graphite products, and in some respects, the electrical performance and processing performance are better or more stable, and thus meet the conditions to replace normal artificial graphite products.
[0025] The preparation process and related products will be described in more detail below, taking the preparation process developed by the applicant as an example.
[0026] A method for producing a negative electrode material, Step S10 of shaping the raw coke to obtain coke powder; A mixture containing coke powder, a binder, and a solvent is pressed at a pressure of 5 MPa to 100 MPa to obtain a precursor, where the coke powder, the binder, and the solvent are in a mass ratio of 100:(3-20):(5-50) in step S20; Step S30: subjecting the precursor in S20 to a temperature of 1000°C to 1500°C for 2h to 6h to carbonization treatment, and cooling to obtain a carbonized product; The precursor is placed in a continuous graphitization furnace and graphitized to obtain a negative electrode material. A specific method of the graphitization is to heat the precursor to 2800°C to 3200°C at a heating rate of 12°C / min to 25°C / min, and then to keep the temperature at 2800°C to 3200°C for 2 to 5 hours, and then to cool the precursor to 30°C at a heating rate of 22°C / min to 26°C / min, including a step S40 of controlling the ratio of the heating rate in the graphitization process to the heating rate in the carbonization process to 4 to 8.
[0027] The method for preparing the negative electrode material provided by the present application is to press a mixture of coke powder, binder and solvent, carbonize the pressed product under a certain temperature condition, and then directly place the carbonized product in a continuous graphitization furnace, and after a rapid heating, the heating rate is very fast so that the precursor can reach the graphitization temperature in a relatively short period of time, and impurity atoms can volatilize and escape, forming pores inside and / or on the surface of the graphite particles. In addition, the process of loading and unloading the material in the continuous graphitization furnace can be completed within only a few hours, and a continuous operation mode is adopted, and the material is continuously loaded and unloaded, during this period, there is no power outage process, the difference in temperature gradient at different positions in the continuous graphitization furnace is small, the uniformity of graphitization of the negative electrode material can be improved, and the thermal energy utilization rate of the continuous graphitization furnace is high, which can also reduce production costs.
[0028] In some embodiments, the green coke comprises at least one of petroleum coke, needle coke, pitch coke, and isotropic coke.
[0029] In some embodiments, the shaping comprises at least one of milling, spheronizing, or sieving, and the shaping process is advantageous for improving particle morphology and increasing tap density.
[0030] The median diameter of the coke powder obtained by shaping is 10 μm to 20 μm, and more specifically, it may be 10 μm, 11.5 μm, 12 μm, 13 μm, 15 μm, 17 μm, 18 μm, 18.5 μm, 19 μm, or 20 μm, but is not limited to the numerical values listed, and other numerical values not listed within the numerical range are also applied. Controlling the median diameter of the coke powder within the above range by multiple tests is advantageous in achieving both processing performance, capacity, and rate characteristics.
[0031] In some embodiments, the mass content of carbon in the coke powder is 80% or more, and may be specifically 80%, 81%, 82%, 85%, 90%, 95%, or 96%, but is not limited to the recited values, and other unrecited values within the numerical range also apply.
[0032] In some embodiments, the solvent comprises at least one of water, ethanol, acetone, benzene, toluene, quinoline, tetrahydrofuran, and carbon tetrachloride.
[0033] In some embodiments, the binder comprises at least one of heavy oil, mineral oil, coal tar, ethylene tar, pitch, petroleum resin, phenolic resin, epoxy resin, coumarone resin, potato starch, wheat starch, corn starch, sweet potato starch, arrowroot, and tapioca flour. The pitch may comprise at least one of petroleum-based liquid pitch and coal-based liquid pitch. Specifically, the petroleum-based liquid pitch may be petroleum pitch, modified pitch, mesophase pitch, etc.
[0034] In some embodiments, the mass ratio of the coke powder, binder, and solvent is 100:(3-20):(5-50), and may be specifically 100:3:5, 100:10:15, 100:15:20, 100:20:20, 100:20:15, 100:10:10, or 100:15:25, but is not limited to the recited numerical values, and other unrecited numerical values within the numerical range also apply.
[0035] As can be seen, in the examples, when the binder ratio is low (the mass ratio of binder to coke powder is 3 to 10:100), the obtained artificial graphite is mainly composed of primary particles, and in the examples, when the binder ratio is high (the mass ratio of binder to coke powder is 10 to 20:100), the obtained artificial graphite is mainly composed of secondary particles.
[0036] In some embodiments, the mixing method of the mixture includes at least one of mechanical stirring and ultrasonic dispersion. When mechanical stirring is adopted for mixing, a propeller type stirrer, a turbine type stirrer, a flat blade type stirrer, etc. can be adopted as long as each fraction in the mixture is mixed sufficiently uniformly.
[0037] In some embodiments, the stirring speed is 10 r / min to 1000 r / min, specifically, 10 r / min, 50 r / min, 70 r / min, 100 r / min, 120 r / min, 150 r / min, 200 r / min, 300 r / min, 350 r / min, 400 r / min, 500 r / min, or 1000 r / min, etc., but is not limited thereto. By controlling the stirring speed within the above range, it is advantageous to mix each fraction to form a uniform mixture.
[0038] The stirring may be performed at room temperature or in a preheated state, and preferably, the stirring temperature may be controlled to 25°C to 200°C. As will be understood, appropriate preheating is advantageous for mixing each fraction to form a uniform mixture.
[0039] In some embodiments, the pressing method includes at least one of extrusion, die pressing, roll pressing, and isostatic pressing.
[0040] In some embodiments, the pressing pressure is 5 MPa to 100 MPa, specifically 5 MPa, 15 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, or 100 MPa, etc., and the pressing process can improve the fluidity of the material in the graphitization process, thereby accelerating the cooling rate in the graphitization temperature drop process, which is favorable for controlling the micro-morphology, specific surface area, and tap density, and can improve the furnace loading and production capacity.
[0041] In some embodiments, the carbonization temperature may be specifically 1000° C., 1050° C., 1100° C., 1200° C., 1300° C., 1400° C., or 1500° C., but is not limited to the listed values, and other unlisted values within the ranges also apply. As will be understood, when the carbonization temperature is within the above ranges, it is favorable for the discharge of substances such as volatile components in the raw material and the formation of a pore structure that meets the demand.
[0042] In some embodiments, the incubation time for the carbonization treatment is 2 h to 6 h, and specifically may be 2 h, 2.5 h, 3 h, 4 h, 5 h, or 6 h, but is not limited to the recited values, and other unrecited values within the range also apply.
[0043] In some embodiments, the carbonized product is obtained by naturally cooling after the carbonization treatment.
[0044] In some embodiments, the graphitization treatment temperature may be, for example, 2800° C., 2900° C., 3000° C., 3050° C., 3100° C., 3150° C., 3180° C., or 3200° C., but is not limited to the listed values, and other unlisted values within the range apply as well.
[0045] In some embodiments, the graphitization treatment is performed for a period of 2h to 5h, specifically, 2h, 2.5h, 3h, 3.5h, 3.8h, 4h, 4.5h, 5h, etc., but is not limited to the recited values, and other unrecited values within the range of values also apply. Preferably, the graphitization treatment is performed for a period of 2h to 3h.
[0046] In some embodiments, the heating rate of the graphitization treatment is 12° C. / min to 25° C. / min, and may be, for example, 12° C. / min, 13° C. / min, 15° C. / min, 18° C. / min, 20° C. / min, or 25° C. / min, but is not limited to the listed values, and other unlisted values within the range of values also apply. Rapid heating is advantageous for controlling the pore volume and specific surface area of the material on the one hand, and can simultaneously reduce heat dissipation and production costs.
[0047] In some embodiments, the graphitization treatment temperature drop rate is 22° C. / min to 26° C. / min, and may be, specifically, 22° C. / min, 23° C. / min, 24° C. / min, 24.5° C. / min, 25° C. / min, 25.5° C. / min, or 26° C. / min, but is not limited to the listed values, and other unlisted values within the range apply as well. Rapid temperature drop can significantly shorten the graphitization processing cycle and reduce production costs.
[0048] In some embodiments, the ratio of the heating rate in the graphitization process to the heating rate in the carbonization process is controlled to be between 4 and 8, and may be specifically 4, 4.5, 5, 6, 7, or 8. By maintaining both heating rates within the above range, it is possible to affect the pore structure, surface micromorphology, and friction state of the material, which is advantageous for controlling the specific surface area and tap density of the material, and also to realize the formation of a certain amount of pore volume inside the artificial graphite without using a pore-forming agent.
[0049] In some embodiments, the graphitization process includes at least one of crushing, sieving, and degaussing. Preferably, the carbonization process includes crushing, degaussing, and sieving in that order.
[0050] In some embodiments, the grinding means is one of a mechanical grinder, an airflow grinder, and a cryogenic grinder.
[0051] In some embodiments, the sieving method is any one selected from a fixed sieve, a drum screen, a resonating sieve, a roller sieve, a vibrating sieve, and a chain grizzly, and the mesh number of the sieving is 100 to 500 mesh. Specifically, the mesh number of the sieving may be 100 mesh, 200 mesh, 250 mesh, 325 mesh, 400 mesh, 500 mesh, etc., and controlling the particle size of the negative electrode material within the above range contributes to improving the processing characteristics of the negative electrode material.
[0052] In some embodiments, the demagnetizing device is any one selected from a permanent magnet drum type magnetic separator, an electromagnetic iron remover, and a pulsating high gradient magnetic separator, and the demagnetizing is for controlling the content of magnetic materials in the negative electrode material finally, for avoiding the discharging effect of magnetic materials on the battery, and for ensuring the safety of the battery during use.
[0053] The negative electrode material according to one embodiment includes artificial graphite and has pores in and / or on the surface of the artificial graphite. The negative electrode material has a pore volume of Vcm 3 / kg, specific surface area is Sm 2 When the pore volume is measured using an ASAP 2460 device manufactured by Micromeritics, USA, and the tap density is Tg / mL, the V×S / T is 8.5≦V×S / T≦27. The pore volume is measured using an ASAP 2460 device manufactured by Micromeritics, USA, and calculated using the BJH Desorption cumulative volume of pores model within the pore diameter range of 17 Å to 3000 Å.
[0054] The negative electrode material provided by the present application is produced and processed by a continuous graphitization process, and the time and temperature of all materials passing through the high temperature zone are synchronized, and the temperature rise and fall rate is controlled, so that the volatile components, impurity elements and other substances in the material can be uniformly and quickly released, so that the pore volume, specific surface area and tap density of the material can reach the ideal adjustment and control design requirements.
[0055] Generally, the pore volume of artificial graphite within a certain range is Li +Increase the diffusion channel of Li + The specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and is favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has found through a large amount of intensive research that when lithium ions move, the movement speed is not only related to the movement space (i.e., the size of the pore volume) and the size of the reaction interface, but also related to the friction condition of the artificial graphite surface, so that even if the pore volume and specific surface area are sufficient, it cannot necessarily guarantee that the lithium ions can be completely and smoothly released and absorbed, and the friction condition can directly affect the size of the tap density. By limiting V×S / T to this range, it can ensure that the lithium ions can be released and absorbed more smoothly inside the artificial graphite material particles at the appropriate space and reaction interface, and the rate and capacity of the material can be greatly improved.
[0056] In some embodiments, the negative electrode material has a pore volume of Vcm 3 / kg, V is 5.0≦V≦8.0, and specifically, V may be 5.0, 5.1, 5.2, 5.5, 5.8, 6.0, 6.3, 6.5, 6.8, 6.9, 7.0, 7.1, 7.5, 7.6, 7.8, or 8.0, etc., but is not limited thereto.
[0057] In some embodiments, the pores include at least one of micropores and mesopores. Micropores are pores with a pore diameter of less than 2 nm, and mesopores are pores with a pore diameter of 2 nm to 50 nm. The formation of abundant pores in and / or on the surface of graphite is favorable for creating more lithium ion diffusion channels, thereby improving the electrochemical performance of the negative electrode material.
[0058] In some embodiments, the average pore diameter of the pores is 50 Å to 200 Å. Specifically, the average pore diameter of the pores may be specifically 50 Å, 60 Å, 70 Å, 100 Å, 150 Å, or 200 Å, etc.
[0059] In some embodiments, the negative electrode material has a specific surface area of Sm 2 / g, 1.78≦S≦3.00, specifically, 1.78, 1.85, 1.95, 2.00, 2.25, 2.43, 2.57, 2.61, 2.72, 2.75, 2.80, 3.00, etc., but not limited thereto. As can be understood, if the specific surface area is too large, it is easy to cause the formation of a solid electrolyte membrane, and the irreversible lithium salt is excessively consumed, which reduces the initial efficiency of the battery.
[0060] In some embodiments, the tap density of the negative electrode material, expressed as Tg / ml, is 0.734≦T≦1.160, and specifically may be, but is not limited to, 0.734, 0.751, 0.768, 0.784, 0.797, 0.818, 0.822, 0.837, 0.863, 0.989, 0.963, 0.958, 0.983, 0.981, 0.997, 1.012, 1.023, 1.033, 1.041, 1.086, or 1.160.
[0061] In some embodiments, the negative electrode material has a (002) plane spacing of d 002 When the 002 ≦3.364 Å. Interplanar spacing d 002 Since is within the above range, it can be seen that the graphite crystallinity of the artificial graphite particles is high, that is, the degree of graphitization is high.
[0062] In some embodiments, the negative electrode material has a particle size D 50 is 10 μm to 30 μm. Specifically, it may be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 20 μm, 25 μm, or 30 μm, and is not limited thereto. Specifically, it can be obtained by measuring the 50% particle size in the cumulative particle size distribution on a volume basis of the negative electrode material by a laser diffraction method. Preferably, the particle size D of the negative electrode material 50 is 10μm~20μm.
[0063] In some embodiments, the negative electrode material includes synthetic graphite primary particles and / or synthetic graphite secondary particles.
[0064] In some embodiments, the negative electrode material further comprises amorphous carbon. As will be understood, after the adhesive is graphitized, a portion is difficult to convert to graphitized carbon, and a portion that cannot be converted to graphitized carbon exists on the surface of the artificial graphite particles in the form of amorphous carbon.
[0065] In some embodiments, the mass ratio of amorphous carbon in the negative electrode material is 0.1 wt% to 5 wt%, and the presence of a small amount of amorphous carbon provides more irregular and more open diffusion paths for lithium ions, which is favorable for improving the rate capability of the material.
[0066] In some embodiments, the negative electrode material has a specific capacity of 320 mAh / g to 370 mAh / g, and specifically may be 320 mAh / g, 340 mAh / g, 342 mAh / g, 345 mAh / g, 353 mAh / g, 355 mAh / g, 357 mAh / g, 360 mAh / g, 365 mAh / g, or 370 mAh / g, etc., but is not limited thereto.
[0067] In some embodiments, the initial coulombic efficiency of the negative electrode material is 93% or greater, and may be, for example, but not limited to, 93.0%, 93.1%, 94.3%, 94.4%, 94.5%, 94.6%, 94.7%, 94.8%, 94.9%, or 95.1%.
[0068] A battery comprising the above-described negative electrode material.
[0069] As will be apparent to those skilled in the art, the battery manufacturing method described above is merely an example, and other methods commonly used in the art may be adopted without departing from the scope of the present invention, and other types of batteries, such as sodium ion batteries, potassium ion batteries, etc., may be manufactured and measured. EXAMPLES
[0070] The embodiments of the present application will be further described below through a number of examples. However, the embodiments of the present application are not limited to the following specific examples. Appropriate modifications can be made within the scope of protection.
[0071] Example 1 The method for producing the negative electrode material according to this embodiment is as follows: (1) crushing Shandong Jingyang coke and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 12 μm; (2) uniformly mixing coke powder, coal tar and quinoline in a mass ratio of 100:5:20 to obtain a mixture; (3) pressing the mixture at a pressure of 20 MPa to obtain a precursor; (4) carbonizing the precursor at a temperature of 1100°C for 4 hours, the heating rate during the carbonization process is 3.3°C / min, and cooling to obtain a carbonized product; (5) The carbonized product is graphitized in a continuous graphitization furnace at 3100°C to obtain a graphitized product. The temperature rise curve is as follows: the temperature is raised to 3100°C at a temperature rise rate of 17.2°C / min, the temperature is kept at 3100°C for 3 hours, and after the temperature is kept, the temperature is lowered to 30°C at a temperature drop rate of 25.6°C / min. The ratio of the temperature rise rate in the graphitization process to the temperature rise rate in the carbonization process is controlled to 5.2. (6) Processing the graphitized product through a dispersion, demagnetization and sieving process to obtain an artificial graphite negative electrode material.
[0072] The negative electrode material includes primary particles of artificial graphite and secondary particles of artificial graphite, the majority of which is primary particles of artificial graphite.
[0073] Example 2 The method for producing the negative electrode material according to this embodiment is as follows: (1) crushing raw coke from Jingyang Needle Coke Co., Ltd. in Shandong Province and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 12 μm; (2) uniformly mixing coke powder, phenolic resin and water in a mass ratio of 100:5:20 to obtain a mixture; (3) pressing the mixture at a pressure of 20 MPa to obtain a precursor; (4) carbonizing the precursor at a temperature of 1100°C for 4 hours, the heating rate during the carbonization process is 3.3°C / min, and cooling to obtain a carbonized product; (5) The carbonized product is graphitized in a continuous graphitization furnace at 3100°C to obtain a graphitized product. The temperature rise curve is as follows: heat up to 3100°C at a heating rate of 16.0°C / min for 3.2 hours, hold at 3100°C for 3 hours, and then cool down to 30°C at a heating rate of 22°C / min for 2.3 hours. The ratio of the heating rate in the graphitization process to the heating rate in the carbonization process is controlled to 4.8. (6) Processing the graphitized product through a dispersion, demagnetization and sieving process to obtain an artificial graphite negative electrode material.
[0074] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0075] Example 3 The method for producing the negative electrode material according to this embodiment is as follows: (1) crushing raw coke from Daqing petroleum coke and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 15 μm; (2) uniformly mixing coke powder, coal tar and quinoline in a mass ratio of 100:5:15 to obtain a mixture; (3) pressing the mixture at a pressure of 20 MPa to obtain a precursor; (4) carbonizing the precursor at a temperature of 1200°C for 3 hours, the heating rate of the carbonization is 3.2°C / min, and cooling to obtain a carbonized product; (5) The carbonized product is graphitized in a continuous graphitization furnace at 3000°C to obtain a graphitized product. The temperature rise curve is as follows: heat up to 3000°C at a heating rate of 13.5°C / min for 3.7 hours, keep at 3000°C for 3 hours, and then cool down to 30°C at a heating rate of 24.7°C / min for 2 hours. The ratio of the heating rate for the graphitization treatment to the heating rate for the carbonization treatment is controlled to 4.2. (6) Processing the graphitized product through a dispersion, demagnetization and sieving process to obtain an artificial graphite negative electrode material.
[0076] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0077] Example 4 The method for producing the negative electrode material of this embodiment is as follows: (1) crushing raw coke from Daqing petroleum coke and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 15 μm; (2) uniformly mixing coke powder, phenolic resin and water in a mass ratio of 100:5:15 to obtain a mixture; (3) pressing the mixture at a pressure of 20 MPa to obtain a precursor; (4) carbonizing the precursor at a temperature of 1150°C for 4 hours, the heating rate of the carbonization is 3.1°C / min, and cooling to obtain a carbonized product; (5) The carbonized product is graphitized in a continuous graphitization furnace at 3000°C to obtain a graphitized product. The temperature rise curve is as follows: heat up to 3000°C at a heating rate of 14.3°C / min for 3.5 hours, hold at 3000°C for 3 hours, and then cool down to 30°C at a heating rate of 22.5°C / min for 2.2 hours. The ratio of the heating rate in the graphitization process to the heating rate in the carbonization process is controlled to 4.6. (6) Processing the graphitized product through a dispersion, demagnetization and sieving process to obtain an artificial graphite negative electrode material.
[0078] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0079] Example 5 The difference from Example 1 is that the carbonization temperature in step (4) is 1500°C.
[0080] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0081] Example 6 The difference from Example 1 is that the carbonization temperature in step (4) is 1000°C.
[0082] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0083] Example 7 The difference from Example 1 is that the carbonization time in step (4) is 3 hours.
[0084] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0085] Example 8 The difference from Example 1 is that the carbonization time in step (4) is 6 hours.
[0086] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0087] Example 9 The difference from Example 1 is that in step (2), coke powder, coal tar and quinoline are uniformly mixed in a mass ratio of 100:3:20 to obtain a mixture.
[0088] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0089] Example 10 The difference from Example 9 is that the raw material used in step (1) is Daqing petroleum coke, and in step (2), coke powder, coal tar and quinoline are uniformly mixed in a mass ratio of 100:20:20 to obtain mixture A.
[0090] The negative electrode material obtained in this example includes primary artificial graphite particles and secondary artificial graphite particles, and as can be seen from the scanning electron microscope images of Figures 1 and 2, most of it is secondary artificial graphite particles, has a flat surface overall, and has a good morphology.
[0091] Example 11 The difference from Example 9 is that the raw material used in step (1) is raw coke from Jinzhou Petrochemical Petroleum Co., Ltd., and in step (2), coke powder, coal tar and quinoline are uniformly mixed in a mass ratio of 100:5:5 to obtain a mixture.
[0092] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0093] Example 12 The difference from Example 10 is that in step (2), coke powder, coal tar and quinoline are uniformly mixed in a mass ratio of 100:5:50 to obtain a mixture.
[0094] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0095] Example 13 The difference from Example 10 is that in step (2), coke powder, phenol resin, and ethanol are uniformly mixed in a mass ratio of 100:5:20 to obtain a mixture.
[0096] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0097] Example 14 The difference from Example 10 is that in step (2), coke powder, epoxy resin and water are uniformly mixed in a mass ratio of 100:5:20 to obtain a mixture.
[0098] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0099] Example 15 The difference from Example 10 is that the pressing pressure in step (3) is 5 MPa.
[0100] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0101] Example 16 The difference from Example 10 is that the pressing pressure in step (3) is 100 MPa.
[0102] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0103] Example 17 The difference from Example 10 is that the graphitization temperature in step (5) is 3000°C.
[0104] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0105] Example 18 The difference from Example 10 is that the graphitization temperature in step (5) is 3200°C.
[0106] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0107] Example 19 The difference from Example 10 is that the temperature rise curve in the graphitization process in step (5) is increased to 3000° C. at a temperature rise rate of 12° C. / min.
[0108] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0109] Example 20 The difference from Example 10 is that the heat retention time for the graphitization treatment in step (5) is 5 hours.
[0110] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, the majority of which is primary artificial graphite particles.
[0111] Comparative Example 1 The difference from Example 1 is that in step (5), the carbonized product is placed in a graphite crucible, and then the graphite crucible is transferred to an Acheson furnace for graphitization to obtain a negative electrode material. The temperature rise curve for the graphitization process is to raise the temperature to 3100°C at a heating rate of 0.7°C / min, maintain the temperature for 3 hours, and cool to 30°C at a heating rate of 0.1°C / min. The ratio of the heating rate for the graphitization process to the heating rate for the carbonization process is controlled to 0.2 to obtain a negative electrode material.
[0112] Comparative Example 2 Raw coke raw material from Jingyang needle coke in Shandong Province is crushed and shaped by a shaping device, and the resulting coke powder with a median diameter of 12 μm is carbonized at a temperature of 1100°C for 4 hours, and the carbonized coke powder is placed in a graphite crucible, which is then transferred to an Acheson furnace for graphitization to obtain the negative electrode material. The temperature rise curve for the graphitization process is to raise the temperature to 3100°C at a heating rate of 0.7°C / min, keep the temperature for 8 hours, and cool to 30°C at a heating rate of 0.1°C / min, and the ratio of the heating rate for the graphitization process to the heating rate for the carbonization process is controlled to 0.2 to obtain the negative electrode material.
[0113] Comparative Example 3 The raw coke raw material from Jingyang needle coke in Shandong Province is carbonized at a temperature of 1100°C for 4 hours, and then fed into a conventional continuous graphitization furnace for graphitization. The heating curve for the graphitization process is to heat up to 2900°C at a heating rate of 9.6°C / min, keep the temperature for 3 hours, and cool to 30°C at a heating rate of 10°C / min. The ratio of the heating rate in the graphitization process of the negative electrode material obtained after shaping and crushing to the heating rate in the carbonization process is controlled to 2, to obtain the negative electrode material.
[0114] Measurement method (1) The method for measuring the particle size of the negative electrode material is to measure the particle size distribution range of the negative electrode material using a Malvern laser particle sizer. (2) The specific surface area of the negative electrode material was measured using a dynamic specific surface area high-speed measuring device JW-DX manufactured by Beijing Jingwei Gaobo Science and Technology Co., Ltd. The unit is m 2 / g. (3) The method for measuring the surface morphology of the negative electrode material is to observe the surface morphology of the negative electrode material particles using a Hitachi S4800 scanning electron microscope. (4) The tap density of the negative electrode material was measured using a Quanta tap density analyzer Dual Autotap from Anton Paar (Shanghai) Trading Co. Ltd. The tap density T was measured after 1000 vibrations, and its unit is g / mL. (5) The method for measuring the interlayer distance of the graphite crystal planes in the negative electrode material is to measure the interlayer distance d 002 and has units of Å. (6) The method for measuring the battery performance was as follows: the negative electrode materials prepared in Examples 1 to 20 and Comparative Examples 1 to 3, carboxymethyl cellulose, conductive carbon black and styrene butadiene rubber were mixed uniformly in deionized water in a mass ratio of 95:1.5:1.5:2 by magnetic stirring for 8 hours. The mixed slurry was applied onto copper foil and vacuum dried at 60°C to obtain a working electrode. Metallic lithium was used as the counter electrode and reference electrode, the separator was Celgard2325, and the electrolyte was 1 mol L-1LiPF6-EC (ethylene carbonate) / DMC (dimethyl carbonate) / EMC (ethyl methyl carbonate) (volume ratio 1:1:1), and the assembly of a CR2016 coin battery was completed in a glove box filled with high-purity argon gas.
[0115] The initial discharge capacity / initial discharge efficiency measurements were performed using a LAND battery measuring device, and the charge / discharge conditions were as follows: leave it for 2 hours, discharge at 0.1C to 0.005V, discharge at 0.09C, 0.08C...0.02C to 0.001V, leave it for 15 minutes, charge at 0.1C to 1.5V, and leave it for 15 minutes.
[0116] The rate characteristics of the button cell are measured in an environment of 25±2°C to obtain the charge / discharge specific capacity and coulombic efficiency at 0.2C, 1C, and 2C. The charge and discharge conditions for rate measurement of the button cell were: (1) discharge at 0.1C to 0.01V, constant voltage for 5h, and charge at 0.1C to 1.5V; (2) discharge at 0.2C to 0.01V, constant voltage to 0.01C, and charge at 0.2C to 1.5V; (3) discharge at 0.2C to 0.01V, constant voltage to 0.01C, and charge at 2C to 1.5V; (4) discharge at 0.2C to 0.01V, constant voltage to 0.01C, and charge at 0.2C to 1.5V; (5) discharge at 1C to 0.01V, constant voltage to 0.01C, and charge at 0.2C to 1.5V; (6) discharge at 2C to 0.01V.
[0117] All battery measurements are as follows: The negative electrode material manufactured in each Example was used as the negative electrode active material, and the mass percentage of the negative electrode active material, conductive agent, binder, and dispersant was 95.2:1.5:2:1.3, so that they were dissolved and mixed in water to control the solid content to 50wt%, and the mixture was applied to a copper foil collector with a thickness of 8μm and dried in a vacuum to manufacture a negative electrode piece. Lithium iron phosphate, polyvinylidene fluoride, and conductive carbon black were uniformly mixed with a solvent NMP (N-methylpyrrolidone) in a mass ratio of 95:2:3, and then the mixture was applied to an aluminum foil with a thickness of 16μm and dried in a vacuum to manufacture a positive electrode piece. The coated positive and negative electrode pieces were subjected to the processes of manufacturing pieces, winding, drying, injection, sealing, chemical synthesis, and capacity grading to manufacture a 554065 type soft pack lithium ion battery.
[0118] The obtained soft-pack battery was subjected to a charge / discharge test using the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd., charging and discharging at room temperature with a current of 1C / 1C, limiting the charge / discharge voltage to 3.0V to 4.35V, and measuring the initial efficiency and 500-week capacity retention rate (press density of the negative electrode piece was 1.60g / cm). 3 ), The above performance measurement results are shown in the table below.
[0119] [Table 1]
[0120] [Table 2]
[0121] As can be seen from the measurement data of Examples 1 to 20, pores are formed inside and / or on the surface of the graphite produced in the examples of the present application, and the pores serve as additional lithium storage space, thereby improving the lithium storage capacity of the negative electrode material, and the specific capacity of the negative electrode material can reach 343mAh / g or more. By controlling V×S / T within the range of 8.5 to 27, it is possible to ensure that lithium ions are more smoothly absorbed and released inside the negative electrode material particles at the appropriate space and reaction interface, and improve the electrochemical performance of the negative electrode material.
[0122] The negative electrode material produced by the discontinuous graphitization process in Comparative Example 1 had a specific surface area that was too large, a tap density that was too small, and a V×S / T that was outside the above range. As a result, the specific capacity and rate characteristics of the material were significantly reduced compared to Examples 1 and 2 produced from the same types of raw materials.
[0123] In the negative electrode material produced by the discontinuous graphitization process in Comparative Example 2, the pores of the artificial graphite were not sufficiently abundant, the pore volume V was too small, the tap density was too large, and V×S / T was outside the above range. As a result, the number of available active sites on the surface of the artificial graphite as a negative electrode material where reactions for releasing and absorbing lithium occurred was reduced, and the rate characteristics of the material were significantly deteriorated.
[0124] In Comparative Example 3, a negative electrode material was produced using a continuous graphitization process, but no binder was added, and the graphitization temperature increase / decrease rate and the ratio of the graphitization temperature increase rate to the carbonization temperature increase rate were not controlled. As a result, V×S / T was outside the above range, and the capacity and rate characteristics were inferior to those of Examples 1 and 2 produced under the same process conditions.
[0125] Although the present application has been disclosed above by way of preferred embodiments, it does not limit the scope of the claims, and any person skilled in the art may make some possible changes or modifications without departing from the technical idea of the present application, so the scope of protection of the present application should conform to the scope defined in the claims.
Claims
1. A negative electrode material comprising artificial graphite having internal and / or surface pores, The negative electrode material has a pore volume of Vcm 3 / kg, specific surface area is Sm 2 / g and tap density is Tg / mL, 8.5≦V×S / T≦27, The pore volume is measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated using the BJH Desorption cumulative volume of pores model within a pore diameter range of 17 Å to 3000 Å. A negative electrode material.
2. The pore volume is V cm 3 2. The negative electrode material according to claim 1, wherein V is 5.0≦V≦8.0 when the negative electrode material is converted to a Cr-Al-Al-Fe-O-Pt / kg.
3. The specific surface area is Sm 2 2. The negative electrode material according to claim 1, wherein, when expressed as 1.78≦S≦3.00 / g, the negative electrode material satisfies the following formula:
4. 2. The negative electrode material according to claim 1, wherein, when the tap density is expressed as Tg / mL, 0.734≦T≦1.
160.
5. The negative electrode material according to claim 1, characterized in that it satisfies at least one of the following characteristics (1) to (2). (1) The pores include at least one of micropores and mesopores; (2) The average pore diameter of the pores is 50 Å to 200 Å.
6. When measured by X-ray diffraction, the interplanar spacing of the (002) plane of the graphite crystal is d 002 When the 002 2. The negative electrode material of claim 1, wherein the thickness is ≦3.364 Å.
7. Particle size D 50 The negative electrode material according to claim 1, characterized in that the thickness of the negative electrode material is 10 μm to 30 μm.
8. 2. The negative electrode material according to claim 1, comprising primary particles of artificial graphite and / or secondary particles of artificial graphite.
9. The negative electrode material according to any one of claims 1 to 8, which satisfies at least one of the following characteristics (1) to (2): (1) The negative electrode material further includes amorphous carbon; (2) The negative electrode material further contains amorphous carbon, and the mass ratio of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.
10. A battery comprising the negative electrode material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Modified natural graphite material and preparation method thereof, negative pole piece and lithium ion battery
CN114843508A
Negative electrode material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery equipped with it
JP2011023341A
Carbon material for nonaqueous electrolyte secondary battery, negative electrode for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for manufacturing carbon material for nonaqueous electrolyte secondary battery
JP2014060148A
Graphite particle for nonaqueous secondary battery, negative electrode for nonaqueous secondary battery using the same, and nonaqueous secondary battery
JP2014067680A
Carbon material for non-aqueous electrolyte secondary battery, negative electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and manufacturing method for carbon material for non-aqueous electrolyte secondary battery
US20150243989A1