Materials and methods for tandem photovoltaic devices
The intermediate layer in tandem photovoltaic devices, composed of insulating protective layers and a high-melting-point core layer, addresses the challenge of bridging the gap between theoretical and actual performance by ensuring insulation resistance and minimizing defects, enhancing manufacturability and reliability.
Patent Information
- Application Number
- JP2024527346
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-10
- Filing Date
- 2022-11-10
- Publication Date
- 2024-11-21
AI Technical Summary
The challenge in producing efficient and manufacturable tandem photovoltaic devices lies in providing an interlayer with desired electrical, optical, physical, and thermal properties that bridge the gap between theoretical and actual performance, minimizing voids and defects, and preventing short circuits between submodules.
A tandem photovoltaic device with an intermediate layer comprising a first and second insulating protective layer and a core layer, where the protective layers have melting points below 170°C and the core layer has a melting point above 200°C, ensuring insulation resistance, optical interface optimization, and preventing short circuits.
The intermediate layer maintains insulation resistance, minimizes voids and defects, and enhances optical performance, leading to improved manufacturability and reliability of tandem photovoltaic devices by preventing short circuits and maintaining electrical isolation between submodules.
Smart Images

Figure 2024543374000001_ABST
Abstract
Description
[Technical field]
[0001]
[0001] This technology relates to interlayers for photovoltaic devices, and more particularly to the use of certain layers to improve tandem photovoltaic devices. [Background technology]
[0002]
[0002] Photovoltaic devices generate power by converting light into electricity using semiconductor materials that exhibit the photovoltaic effect. Certain semiconductor materials are more efficient at absorbing certain ranges of the electromagnetic spectrum. To improve the overall efficiency of a photovoltaic device, the device can incorporate stacked sub-modules, also called subcells, that utilize semiconductor materials with different absorption characteristics to form a tandem photovoltaic device.
[0003]
[0003] In an exemplary tandem photovoltaic device, solar radiation or light enters through the top submodule and a portion of the radiation passes from the top submodule to the bottom submodule. The top submodule can absorb more of the higher energy photons having shorter wavelengths, while the bottom submodule can absorb more of the lower energy photons having longer wavelengths. An intermediate layer may be positioned between the top and bottom submodules.
[0004]
[0004] Laboratory experiments measuring the absorption efficiency in the relevant spectral ranges of separate submodules have shown that there are promising submodules that may be used together to absorb a larger fraction of the incident radiation. However, as the complexity of tandem architectures increases, it may also be difficult to bridge the gap between actual and theoretical performance. A major challenge to producing tandem photovoltaic devices with good efficiency and manufacturability is to provide an intermediate layer with the desired electrical, optical, physical and thermal properties. Summary of the Invention [Problem to be solved by the invention]
[0005]
[0005] Thus, a need exists for alternative interlayer structures for use in tandem photovoltaic devices, as well as methods and materials useful in the fabrication of tandem photovoltaic device architectures. [Means for solving the problem]
[0006] In accordance with this disclosure, the present technology provides articles of manufacture, systems, and methods for making and using tandem photovoltaic devices.
[0007] A tandem photovoltaic device is provided that may include a first submodule, a second submodule, and an intermediate layer disposed between the first submodule and the second submodule. The intermediate layer is capable of passing a portion of light. The intermediate layer may include a first insulating protective layer (conformal layer), a second insulating protective layer, and a core layer. The first insulating protective layer may conform in direct contact with a portion of a surface of the first submodule. The first insulating protective layer may include a first polymer having a melting point less than about 170°C. The second insulating protective layer may conform in direct contact with a portion of a surface of the second submodule. The second insulating protective layer may include a second polymer having a melting point less than about 170°C. The core layer may be disposed between the first insulating protective layer and the second insulating protective layer and may directly contact the first insulating protective layer and the second insulating protective layer. The core layer may include a third polymer having a melting point greater than about 200°C. Thus, solar radiation or light can enter from the first submodule and a portion of the radiation can pass through the first submodule and the intermediate layer to the second submodule. The intermediate layer can maintain a desired insulation resistance between the first submodule and the second submodule. The intermediate layer can minimize voids or defects between the surface of the first submodule and the surface of the second submodule and optimize the optical interface therebetween.
[0007]
[0008] Methods of making and using tandem photovoltaic devices utilizing the intermediate layers of the present technology are provided. A portion of a surface of the first submodule may be in direct contact with the first insulating protective layer. The first insulating protective layer may then conform to a portion of a surface of the first submodule. Similarly, a portion of a surface of the second submodule may be in direct contact with the second insulating protective layer. The second insulating protective layer may then conform to a portion of a surface of the second submodule. Various methods of contacting and conforming the intermediate layer to the first and second submodules are provided.
[0008]
[0009] Further areas of applicability will become apparent from the description provided herein. The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.
[0009]
[0010] The drawings described herein are only for purposes of illustrating selected embodiments rather than all possible implementations and are not intended to limit the scope of the present disclosure. [Brief description of the drawings]
[0010] [Figure 1]
[0011] FIG. 2A-2C are schematic diagrams illustrating cross-sectional views of a tandem photovoltaic device according to one or more embodiments shown and described herein. [Diagram 2]
[0012] 2A-2C are schematic diagrams illustrating example sub-modules of the photovoltaic device of FIG. 1 according to one or more embodiments shown and described herein. [Diagram 3]
[0013] FIG. 3 is a schematic diagram illustrating a cross-sectional view of the photovoltaic sub-module of FIG. 2 along 3-3 according to one or more embodiments shown and described herein. [Figure 4]
[0014] 1A and 1B illustrate schematic diagrams of a substrate according to one or more embodiments shown and described herein. [Diagram 5]
[0015] FIG. 2 illustrates a schematic cross-sectional view of the tandem photovoltaic device of FIG. 1 according to one or more embodiments shown and described herein. [Figure 6]
[0016] FIG. 2A illustrates a schematic cross-sectional view of an interlayer stack according to one or more embodiments shown and described herein. [Figure 7]
[0017] FIG. 2 illustrates an example of a method for making a tandem photovoltaic device according to one or more embodiments shown and described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011]
[0018] The following description of the technology is merely exemplary in nature of the subject matter, manufacture and use of one or more inventions, and is not intended to limit the scope, application, or use of any particular invention claimed in this application, or in any other application that may be filed claiming priority to this application, or in any patent issued therefrom. With respect to the disclosed methods, the order of steps presented is exemplary in nature, and thus the order of steps may vary in various embodiments, including cases where certain steps may be performed simultaneously, unless expressly stated otherwise. As used herein, "a" and "an" indicate the presence of "at least one" of an item; where possible, a plurality of such items may be present. Unless otherwise expressly stated, all numerical quantities herein are understood to be modified by the word "about" in describing the broadest scope of the technology, and all geometric and spatial descriptors are understood to be modified by the word "substantially". When applied to a numerical value, "about" indicates that the calculation or measurement allows for some imprecision in the value (with some approximation to the precision of the value; roughly or reasonably close to the value; approximately). If for any reason the imprecision implied by "about" and / or "substantially" is not otherwise understood in the art to have its ordinary meaning, then "about" and / or "substantially" as used herein will at least account for the variation that can result from ordinary methods of measuring or using such parameters.
[0012]
[0019] Unless otherwise specified, values of material properties correspond to conditions of room temperature, 20° C. and 1 atmosphere pressure.
[0020] Unless otherwise specified, values in the ranges provided are inclusive of the endpoints and include all explicit values and sub-divided ranges within the entire range.
[0013]
[0021] When an element or layer is referred to as "resting," "engaged," "connected," or "coupled" with another element or layer, it may be directly resting, engaged, connected, or coupled with the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as "directly resting," "directly engaged," "directly connected," or "directly coupled" with another element or layer, there may not be intervening elements or layers. Other words used to describe relationships between elements should be interpreted similarly (e.g., "between" vs. "directly between," "adjacent" vs. "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.
[0014]
[0022] Terms such as first, second, third, etc. may be used herein to describe various elements, components, regions, layers, and / or sections, but these elements, components, regions, layers, and / or sections should not be limited by these terms. These terms may be used only to distinguish one element, component, region, layer, or section from another region, layer, or section. Terms such as "first," "second," and other numerical terms, when used herein, do not imply any permutation or order unless clearly indicated by the context. Thus, a first element, component, region, layer, or section discussed below may be referred to as a second element, component, region, layer, or section without departing from the teachings of the exemplary embodiments.
[0015]
[0023] Spatially relative terms such as "inside," "outside," "lower," "below," "bottom," "upper," "top," and the like may be used herein for ease of description to describe the relationship of one element or feature shown in a figure to another element or feature. Spatially relative terms may be intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figure. For example, if a device in a figure is turned over, an element described as "below" or "below" the other element or feature would be oriented "above" the other element or feature. The device may be oriented differently (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein may be interpreted accordingly.
[0016]
[0024] The term "light" may refer to various wavelengths in the electromagnetic spectrum, including, but not limited to, wavelengths in the ultraviolet (UV), infrared (IR), and visible portions of the electromagnetic spectrum. As used herein, "solar light" refers to light emitted by the sun. As used herein, near infrared (NIR) refers to wavelengths in the range of approximately 700 nm to 1300 nm.
[0017]
[0025] The term "layer" may refer to a thickness of material applied onto a surface. A layer may cover all or a portion of a surface. A layer may include sublayers and may have a compositional gradient within the layer. A layer may include one or more functional layers of material.
[0018]
[0026] While the present technology relates to a tandem photovoltaic device including a first submodule and a second submodule, it should be appreciated that such a tandem photovoltaic device may include additional submodules, as well as additional arrangements of submodules. In the structure of the tandem photovoltaic device provided herein, an intermediate layer is disposed between the first submodule and the second submodule, and the intermediate layer passes a portion of the light. In this manner, a portion of the light passing through the first submodule may further pass through the intermediate layer to the second submodule. The intermediate layer may be transparent to light of near infrared wavelengths. Near infrared light incident on the front surface of the tandem device may pass through the first submodule and the intermediate layer to be absorbed in the second submodule. The intermediate layer may operate to maintain a desired insulation resistance between the first submodule and the second submodule. The intermediate layer may further minimize voids or defects between the surface of the first submodule and the surface of the second submodule, optimizing the optical interface therebetween.
[0019]
[0027] Tandem photovoltaic devices can generate electrical power by converting light into direct current electricity using semiconductor materials that exhibit the photovoltaic effect. The photovoltaic effect generates electrical power upon exposure to light because photons are absorbed in the semiconductor material, exciting electrons to a higher energy state. These excited electrons can move within the material, generating an electrical current. Semiconductor materials suitable for use in photovoltaic devices can include, for example, II-VI materials including cadmium telluride alloys, III-V materials including GaAs and InGaN, I-III-VI materials including CIGS and CIS materials, as well as silicon and perovskites.
[0020]
[0028] Tandem photovoltaic devices can achieve higher total conversion efficiencies than single photovoltaic devices by capturing a larger portion of the solar spectrum. Tandem devices may be formed using more than one p-n junction and materials with different bandgap properties that respond to different ranges of the electromagnetic spectrum, including infrared, visible, and ultraviolet light. In devices where the primary light source is from above, the light incident top cell or top submodule may have a large bandgap to capture high energy short wavelengths such as visible and uv, while the bottom cell or bottom submodule may use absorber materials with smaller bandgaps to capture longer wavelengths and reflected photons, including near infrared. Tandem devices may have two or more stacked subcells or submodules, with each submodule containing an active region formed from semiconductor materials with different absorption properties, including different types of semiconductor materials.
[0021]
[0029] The sub-modules of the tandem photovoltaic devices described herein may be stacked and separated by intermediate layers. Incident electromagnetic radiation, i.e., light, enters the device from the front or top surface and enters the top sub-module. Light that is not absorbed by the top sub-module reaches the intermediate layer. The intermediate layer may be configured to reflect some light energy, or photons, back to the top sub-module and also transmit photons of light to the back cell or bottom sub-module. In most tandem devices, it is beneficial for the intermediate layer structure to be substantially transparent to the spectral radiation wavelengths that are configured to be absorbed by the bottom sub-module. In photovoltaic devices with multiple stacked sub-modules, additional intermediate layers may be provided between each sub-module. The tandem photovoltaic device may include a bifacial device configured to receive incident radiation through both the front and back surfaces. The bifacial tandem device may be configured to receive solar radiation directly at the top or front surface and radiation reflected from an external surface, including visible and infrared light, at the back or back surface.
[0022]
[0030] The interlayer structure may be exposed to stresses including high temperatures, ultraviolet light, mechanical stress, and temperature fluctuations. Undesirably, in certain photovoltaic devices, these stresses may cross the interlayer and cause shorts between the submodules, potentially damaging the photovoltaic device. To prevent shorts, it is desirable for the interlayer structure to have a suitable insulation breakthrough strength to electrically isolate the first and second submodules. To design efficient and reliable tandem photovoltaic devices, it is also desirable to prevent gaps or air bubbles between the interlayer structure and the interface of the first and second submodules. In some tandem architectures, it may be desirable for the interlayer to have a suitable refractive index to transmit photons to the second submodule and / or reflect some photons back to the first submodule.
[0023]
[0031] In tandem photovoltaic modules, the risk of shorting from the active surface of one submodule to the active surface of the other submodule is significant. Electrical isolation between the active surfaces of the submodules maintains a minimum breakdown distance. At the same time, an encapsulant may be formed between the first and second submodules and around other system components to provide good contact for light transmission and protect the submodules from degradation. An interlayer structure that can both isolate and encapsulate the surfaces of adjacent submodules is desirable. To achieve the desired properties, methods and structures are provided for an interlayer formed from a multilayer film having outer layers that provide the desired adhesion and encapsulation, and a central core layer that maintains the desired dielectric and structural properties.
[0024]
[0032] In certain embodiments, an interlayer is provided that includes multiple layers. The interlayer includes one or more core layers, each of which has a high dielectric strength and may be non-flowable at the expected operating conditions of the tandem photovoltaic device, and the material of each core layer may have a high melting point. The interlayer structure includes an outer layer or first insulating protection layer that is flowable and has a low melting point. The interlayer structure may also include another outer layer or second insulating protection layer, with the first and second insulating protection layers positioned on either side of the core layer. The insulating protection layer may include a layer of a flowable polymer with a melting point below 170° C. to conform to the system components during stacking and operation at higher temperatures. The core layer includes a non-flowable polymer material with a melting point above 200° C. to maintain a dielectric and physical barrier that resists deformation and narrowing of the dielectric breakdown distance. The interlayer structure, including the multilayer film, provides insulation resistance over a wide operating temperature range. Thus, the interlayer may be configured as a transparent multilayer film for mechanically stacked multijunction solar cells that provides transparency, thermal stability, adhesive strength, moisture resistance, prevents short circuits, and maintains a minimum breakdown distance between submodules separated by the interlayer. The interlayer may also prevent moisture penetration and may be used to electrically connect to different system components or cooperate with other parts of the tandem photovoltaic device.
[0025]
[0033] A tandem photovoltaic device constructed according to the present technology may include a first submodule, a second submodule, and an intermediate layer disposed between the first submodule and the second submodule. The intermediate layer is capable of passing a portion of light. The intermediate layer may include a first insulating protective layer, a second insulating protective layer, and a core layer. The first insulating protective layer may conform in direct contact with a portion of a surface of the first submodule, the first insulating protective layer comprising a first polymer having a melting point less than about 170°C. The second insulating protective layer conforms in direct contact with a portion of a surface of the second submodule, the second insulating protective layer comprising a second polymer having a melting point less than about 170°C. The core layer is disposed between the first insulating protective layer and the second insulating protective layer, and in direct contact with the first insulating protective layer and the second insulating protective layer, the core layer comprising a third polymer having a melting point greater than about 200°C. In certain embodiments, the third polymer may have a melting point greater than about 250°C.
[0026]
[0034] The intermediate layer provided herein may include various aspects. For example, the intermediate layer may have a refractive index of about 1.2 to about 2.0. In some embodiments, the intermediate layer has a refractive index greater than 1.4, greater than 1.5, greater than 1.6, or greater than 1.7. In some embodiments, the intermediate layer has a refractive index in the range of 1.5 to 1.8, 1.6 to 1.8, 1.7 to 1.9, or 1.6 to 1.7 for wavelengths in the range of 800 nm to 1200 nm. Particular embodiments include where the intermediate layer has a refractive index of about 1.6. Still further embodiments include where the intermediate layer has a refractive index greater than about 1.6. In this manner, the intermediate layer can provide an optical interface that effectively transmits light through one submodule to another submodule. The intermediate layer can also exhibit a dielectric strength greater than 10 kV / mm. Thus, the opportunity for electrical shorting between the submodules is minimized. An embodiment of the intermediate layer may have a thickness of about 100 μm to about 1500 μm, which may include the combined thickness of the first and second insulating protective layers and the core layer. The intermediate layer may be capable of transmitting a portion of near infrared light. The intermediate layer may be configured to transmit at least 85% of light having a wavelength of 700 nm to 1300 nm. The intermediate layer may be configured to transmit at least 90% of light having a wavelength of about 800 nm to about 1200 nm. In some embodiments, the intermediate layer may be capable of transmitting a portion of visible light. The intermediate layer may further be configured to transmit at least 90% of light having a wavelength of about 400 nm to about 800 nm that passes through it. Particular embodiments of the intermediate layer may have an optical transmittance of at least 85% for wavelengths of 750 nm to 1200 nm. Yet further embodiments of the intermediate layer may have an optical transmittance of at least 90% at 800 nm.
[0027]
[0035] The polymers used to form the first and second insulating protective layers of the intermediate layer and the core layer may include various aspects. The first polymer and the second polymer of each of the first and second insulating protective layers may independently include one or more of polyethylene; ethylene-vinyl acetate; polyolefin elastomer (POE); pressure sensitive adhesive; hot melt adhesive; polyvinyl butyral; thermoplastic polyurethane; silicone; silicone / polyurethane hybrid; ionomer; UV curable resin; fluororesins of ethylene tetrafluoroethylene (e.g., Tefzel), polyvinyl fluoride (e.g., Tedlar), tetrafluoroethylene, hexafluoropropylene, and vinylidene fluoride (e.g., THV220); and polyethylene naphthalate. Particular embodiments include cases where the first polymer and the second polymer include the same material. The third polymer of the core layer may include one or more of oriented polyethylene terephthalate, polytetrafluoroethylene, polycyclooctene, biaxially oriented polyethylene terephthalate (boPET), and polyimide.
[0028]
[0036] The various layers of the intermediate layer may have various thicknesses. The first and second insulating protective layers may have different thicknesses. The insulating protective layers may act as adhesives as well as sealants. When the polymers of the insulating protective layers are substantially at their respective melting points, the insulating protective layers may flow and spread across a portion of the surface of each submodule.
[0029]
[0037] The core layer may include various embodiments. The core layer may have a thickness of about 25 μm to about 500 μm. Embodiments of the core layer may also have a dielectric strength of greater than about 50 kV / mm. One or more polymers of the core layer may be selected to have a melting point higher than the expected operating temperature of the tandem photovoltaic device. In this manner, the integrity of the core layer may be maintained during operation of the tandem photovoltaic device, including where the core layer maintains a desired thickness and provides a desired dielectric strength between the submodules during operation of the tandem photovoltaic device.
[0030]
[0038] Particular embodiments of the intermediate layer may include where the first and second insulating protective layers have a thickness of 300 μm, the core layer has a thickness of 100 μm, and the third polymer of the core layer comprises biaxially oriented polyethylene terephthalate.
[0031]
[0039] A particular embodiment of the tandem photovoltaic device includes a first submodule, a second submodule, and an intermediate layer disposed between the first submodule and the second submodule. The intermediate layer is configured to transmit a portion of light and has a refractive index of about 1.2 to about 2.0, a dielectric strength greater than about 10 kV / mm, and a thickness of about 100 μm to about 1500 μm. The intermediate layer includes a first insulating protective layer, a second insulating protective layer, and a core layer. The first insulating protective layer conforms directly to a portion of a surface of the first submodule, the first insulating protective layer includes a first polymer having a melting point less than about 170° C., the first polymer includes a member selected from the group consisting of polyethylene; ethylene-vinyl acetate; polyolefin elastomer; and combinations thereof. The second insulating protective layer is in direct contact with and conforms to a portion of the surface of the second submodule, the second insulating protective layer comprising a second polymer having a melting point less than about 170° C., the second polymer comprising a member selected from the group consisting of polyethylene; ethylene-vinyl acetate; polyolefin elastomer; and combinations thereof. The core layer is disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, the core layer comprising a third polymer having a dielectric strength greater than about 50 kV / mm and a melting point greater than about 200° C. The third polymer comprises a member selected from the group consisting of oriented polyethylene terephthalate; polytetrafluoroethylene; polycyclooctene; biaxially oriented polyethylene terephthalate; polyimide; and combinations thereof.
[0032]
[0040] The present technology further provides various methods of making a tandem photovoltaic device. Such methods include providing an intermediate layer as described herein. A portion of the surface of the first submodule may be in direct contact with the first insulating protective layer of the intermediate layer. The first insulating protective layer may be conformed to a portion of the surface of the first submodule. A portion of the surface of the second submodule may be in direct contact with the second insulating protective layer of the intermediate layer. The second insulating protective layer may be conformed to a portion of the surface of the second submodule. In this way, in certain embodiments, the core layer may electrically connect the two submodules while preventing the ingress of moisture into the tandem photovoltaic device.
[0033]
[0041] The provision of the intermediate layer can take a variety of forms. Particular embodiments include where the core layer is laminated between the first and second insulating protective layers to provide the intermediate layer. Similarly, the core layer can be extruded between the first and second insulating protective layers to provide the intermediate layer. Other means of forming the intermediate layer include hot melt, deposition of one or more layers, and co-extrusion of one or more layers.
[0034]
[0042] The method of making a tandem photovoltaic device may include various embodiments. The step of fitting the first insulating protective layer to a portion of the surface of the first submodule may include heating the first insulating protective layer to at least the melting point of the first polymer. The step of fitting the second insulating protective layer to a portion of the surface of the second submodule may also include heating the second insulating protective layer to at least the melting point of the second polymer. It is also possible that a portion of the surface of the first submodule and one of the first insulating protective layer may be heated to at least the melting point of the first polymer before directly contacting the first insulating protective layer with a portion of the surface of the first submodule, and that a portion of the surface of the second submodule and one of the second insulating protective layer may be heated to at least the melting point of the second polymer before directly contacting the second insulating protective layer with a portion of the surface of the second submodule.
[0035]
[0043] Certain methods may include applying a first insulating protective layer to a portion of a surface of the first submodule, which may include directly contacting the first insulating protective layer with a portion of the surface of the first submodule and directly contacting the second insulating protective layer with a portion of the surface of the second submodule, followed by simultaneously heating the first submodule, the intermediate layer, and the second submodule to at least the melting point of the first polymer and at least the melting point of the second polymer. It is also possible to include applying a first insulating protective layer to a portion of a surface of the first submodule, which includes pressing the intermediate layer and the first submodule together, or applying a second insulating protective layer to a portion of a surface of the second submodule, which includes pressing the intermediate layer and the second submodule together. Embodiments of the method may further include conforming a first insulating protective layer to a portion of a surface of the first submodule, and conforming the first insulating protective layer to a portion of a surface of the first submodule may further include pressing an intermediate layer between the first submodule and the second submodule.
[0036]
[0044] In certain embodiments, the precursor of the interlayer may be formed as a continuous sheet having multiple layers, including a core layer disposed between a first insulating protective layer and a second insulating protective layer. The precursor may be placed between a first submodule and a second submodule to form an unbonded tandem photovoltaic device. The unbonded tandem photovoltaic device is subjected to a lamination heat treatment sufficient to cause the first insulating protective layer and the second insulating protective layer to flow and bond with their respective adjacent submodules to form a bonded tandem photovoltaic device. At least a portion of each insulating protective layer melts during lamination to achieve the desired wettability and adhesion of the interlayer to the respective submodule, while the core layer does not melt during lamination to maintain a physical and electrical barrier between the submodules. After lamination, the interlayer physically and electrically isolates the active surfaces of the submodules of the tandem photovoltaic device. The bonded tandem photovoltaic device may be subjected to finishing processing steps, such as adding additional encapsulation layers, bussing, etc., to produce a completed tandem photovoltaic device.
[0037]
[0045] Aspects of the technology may be applied in various combinations, interdependencies, and multiple dependencies, as illustrated in the examples, implementations, and embodiments that follow.
[0045] In an embodiment, a tandem photovoltaic device includes a first submodule; a second submodule; and an intermediate layer disposed between the first submodule and the second submodule, the intermediate layer allowing a portion of light to pass therethrough, the intermediate layer including: a first insulating protective layer conforming in direct contact with a portion of a surface of the first submodule, the first insulating protective layer comprising a first polymer having a melting point less than about 100°C; a second insulating protective layer conforming in direct contact with a portion of a surface of the second submodule, the second insulating protective layer comprising a second polymer having a melting point less than about 100°C; a core layer disposed between the first insulating protective layer and the second insulating protective layer, the core layer comprising a third polymer having a melting point greater than about 200°C.
[0038]
[0046] In some cases, the intermediate layer has a refractive index from about 1.2 to about 2.0.
[0047] In some cases, the intermediate layer has a dielectric strength greater than about 10 kV / mm.
[0048] In some cases, the intermediate layer has a thickness of about 400 μm to about 1500 μm.
[0039]
[0049] In some cases, the intermediate layer is configured to transmit at least 90% of incident light having a wavelength between 800 nm and 1200 nm.
[0050] In some cases, the first polymer and the second polymer independently comprise a member selected from the group consisting of polyethylene, ethylene-vinyl acetate, a polyolefin elastomer, and combinations thereof. In some cases, the first polymer consists essentially of a polyolefin elastomer.
[0040]
[0051] In some cases, the first polymer and the second polymer comprise the same material. In some cases, the first polymer and the second polymer consist essentially of, or consist of, the same material.
[0041]
[0052] In some cases, the third polymer comprises a member selected from the group consisting of polyethylene terephthalate, oriented polyethylene terephthalate, polytetrafluoroethylene, polycyclooctene, biaxially oriented polyethylene terephthalate, polyimide, and combinations thereof. In some cases, the core layer consists essentially of polyethylene terephthalate.
[0042]
[0053] In some cases, the core layer has a thickness of from 25 μm to 200 μm.
[0054] In some cases, the core layer has a dielectric strength of greater than 50 kV / mm.
[0055] In some cases, the first insulating protective layer and the second insulating protective layer have different thicknesses.
[0043]
[0056] In some cases, the first insulating protective layer has a thickness of about 300 μm, the second insulating protective layer has a thickness of 300 μm, the core layer has a thickness of 100 μm, and the third polymer of the core layer comprises biaxially oriented polyethylene terephthalate.
[0044]
[0057] According to embodiments provided herein, a tandem photovoltaic device may include a first submodule; a second submodule; and an intermediate layer disposed between the first submodule and the second submodule, the intermediate layer transmitting a portion of light and having a refractive index of about 1.2 to about 2.0, a dielectric strength of greater than about 10 kV / mm, and a thickness of about 400 μm to about 1500 μm, the intermediate layer comprising: a first insulating protective layer in direct contact and conforming to a portion of a surface of the first submodule, the first insulating protective layer comprising a first polymer having a melting point less than about 170° C., the first polymer comprising a member selected from the group consisting of: polyethylene; ethylene-vinyl acetate; polyolefin elastomer; and combinations thereof; a second insulating protective layer comprising a second polymer having a melting point less than about 170°C, the second polymer comprising a member selected from the group consisting of: polyethylene; ethylene-vinyl acetate; polyolefin elastomer; and combinations thereof; a core layer disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, the core layer having a dielectric strength greater than about 50 kV / mm, the core layer comprising a third polymer having a melting point greater than about 200°C, the third polymer comprising a member selected from the group consisting of: oriented polyethylene terephthalate; polytetrafluoroethylene; polycyclooctene; biaxially oriented polyethylene terephthalate; polyimide; and combinations thereof.
[0045]
[0058] According to an embodiment of the present disclosure, a method of making a tandem photovoltaic device may include: providing an intermediate layer, the intermediate layer transmitting a portion of light, the intermediate layer including: a first insulating protective layer including a first polymer having a melting point less than about 170° C.; a second insulating protective layer including a second polymer having a melting point less than about 170° C.; a core layer disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, the core layer including a third polymer having a melting point greater than about 200° C.; directly contacting a portion of a surface of the first submodule with the first insulating protective layer; conforming the first insulating protective layer to a portion of a surface of the first submodule; directly contacting a portion of a surface of the second submodule with the second insulating protective layer; and conforming the second insulating protective layer to a portion of a surface of the second submodule.
[0046]
[0059] In some cases, the method further includes laminating the core layer between the first insulating protective layer and the second insulating protective layer to provide an intermediate layer.
[0060] In some cases, the method further includes co-extruding the core layer between the first insulating protective layer and the second insulating protective layer to provide an intermediate layer.
[0047]
[0061] In some cases, conforming the first insulating protective layer to a portion of a surface of the first submodule includes heating the first insulating protective layer to at least a melting temperature of the first polymer. In some cases, conforming the second insulating protective layer to a portion of a surface of the second submodule includes heating the second insulating protective layer to at least a melting temperature of the second polymer.
[0048]
[0062] In some embodiments, a portion of a surface of the first submodule and one of the first insulating protective layer are heated to at least the melting point of the first polymer before directly contacting the portion of the surface of the first submodule with the first insulating protective layer, and a portion of a surface of the second submodule and one of the second insulating protective layer are heated to at least the melting point of the second polymer before directly contacting the portion of the surface of the second submodule with the second insulating protective layer.
[0049]
[0063] In some embodiments, the method may include applying a first insulating protective layer to a portion of a surface of the first submodule, applying a second insulating protective layer to a portion of a surface of the second submodule, and subsequently directly contacting the first insulating protective layer with a portion of a surface of the first submodule and the second insulating protective layer with a portion of a surface of the second submodule, and then simultaneously heating the first submodule, the intermediate layer, and the second submodule to at least a melting point of the first polymer and at least a melting point of the second polymer.
[0050]
[0064] In some embodiments, the method may include, wherein the step of conforming a first insulating protective layer to a portion of a surface of the first sub-module includes pressing an intermediate layer and the first sub-module together; or, the step of conforming a second insulating protective layer to a portion of a surface of the second sub-module includes pressing an intermediate layer and the second sub-module together.
[0051]
[0065] In some embodiments, the method may include the steps of conforming a first insulating protective layer to a portion of a surface of the first sub-module and conforming a second insulating protective layer to a portion of a surface of the second sub-module including pressing an intermediate layer between the first sub-module and the second sub-module. EXAMPLES
[0052]
[0066] Exemplary embodiments of the present technology are provided with reference to the figures enclosed herein.
[0067] 1 and 5, an embodiment of a tandem photovoltaic device 300 is shown. The tandem photovoltaic device 300 may be configured to receive light and convert the light into electrical energy as photons are absorbed from the light and converted into electrical current via the photovoltaic effect. For purposes of discussion and clarity, the tandem photovoltaic device 300 may define a front side 302 configured to face a primary light source, such as the sun. Additionally, the tandem photovoltaic device 300 may also define a back side 304 that is offset from the front side 302, such as by a functional layer of a plurality of materials.
[0053]
[0068] The tandem photovoltaic device 300 may have a first submodule 100, a second submodule 500, and an intermediate layer 400 therebetween. The first submodule 100 may also be referred to as a top cell or upper submodule. The second submodule 500 may also be referred to as a bottom cell or lower submodule. The intermediate layer 400 may also be referred to as an intermediate layer stack, a dielectric stack, or a transparent interconnect layer. Each of the first submodule 100, the second submodule 500, and the intermediate layer 400 may include multiple layers. Each of the first and second submodules 100, 500 of the tandem photovoltaic device 300 may include one or more absorber layers for converting light into charge carriers and conductive layers for collecting the charge carriers.
[0054]
[0069] The first sub-module 100 may have a first surface 102 that substantially faces the front side 302 of the tandem photovoltaic device 300, and a second surface 104 that substantially faces the back side 304 of the photovoltaic device 300. The intermediate layer 400 may have a first surface 402 that substantially faces the front side 302 of the photovoltaic device 300, and a second surface 404 that substantially faces the back side 304 of the photovoltaic device 300. The second sub-module 500 may have a first surface 502 that substantially faces the front side 302 of the photovoltaic device 300, and a second surface 504 that substantially faces the back side 304 of the photovoltaic device 300.
[0055]
[0070] As depicted in FIG. 1 , incident light (hv) 10 may enter the front side 302 of the tandem photovoltaic device 300 through the first submodule 100, a first portion of the light energy 11 may be absorbed by the first submodule 100, and a remaining portion of the light energy 12 may pass from the first submodule 100 to the intermediate layer 400. In the intermediate layer 400, the reflected light 13 may be directed back toward the absorbing region of the first submodule 100, and the transmitted light 14 may pass to the second submodule 500. Optionally, in a bifacial tandem device, backside light energy 16 may enter the backside 304 of the tandem photovoltaic device 300 toward the second submodule 500. In many implementations, the backside light energy 16 may include externally reflected visible and near infrared light. The first sub-module can absorb a first portion of light energy 11, which may include an absorbed combination of incident light 10 and reflected light 13. The second sub-module may absorb a second portion of light energy 15, which includes transmitted light 14, and optionally backside light energy 16.
[0056]
[0071] 2 and 3, an exemplary embodiment of a first submodule 100 of a tandem photovoltaic device 300 is shown. The first submodule 100 may include multiple layers disposed between a front side 102 and a back side 104. In some embodiments, the layers of the first submodule 100 may be divided into an array of photovoltaic cells 200. For example, the first submodule 100 may be scribed according to a plurality of series scribes 202 and a plurality of parallel scribes 204. The series scribes 202 may extend along the length Y of the first submodule 100 and partition the photovoltaic cells 200 along the length Y of the first submodule 100. Adjacent cells 200 of the photovoltaic cells may be connected in series along the width X of the first submodule 100. In other words, a monolithic interconnection of adjacent cells 200 may be formed, for example, adjacent to the series scribes 202. The parallel scribes 204 may extend along the width X of the first submodule 100 and section the photovoltaic cells 200 along the width X of the first submodule 100. In operation, current 205 may flow along the width X primarily through the photovoltaic cells 200 connected in series by the series scribes 202. In operation, the parallel scribes 204 may limit the ability of the current 205 to flow along the length Y. The parallel scribes 204 are optional and may be configured to separate the series connected photovoltaic cells 200 into groups 206 arranged along the length Y.
[0057]
[0072] 2, the parallel scribes 204 may electrically isolate groups 206 of series-connected photovoltaic cells 200. In some embodiments, the groups 206 of photovoltaic cells 200 may be connected in parallel, for example, via an electrical bus connection. Optionally, the number of parallel scribes 204 may be configured to limit the maximum current generated by each group 206 of photovoltaic cells 200. In some embodiments, the maximum current generated by each group 206 may be about 200 milliamps (mA) or less, such as, for example, about 100 mA or less in one embodiment, about 75 mA or less in another embodiment, or about 50 mA or less in further embodiments.
[0058]
[0073] With particular reference to FIG. 3, the layers of the first sub-module 100 may include a thin film stack provided on a substrate 110. The substrate 110 may be configured to facilitate transmission of light into the first sub-module 100. The substrate 110 may be disposed on a front side 102 of the first sub-module 100. With reference collectively to FIGS. 2 and 3, the substrate 110 may have a first surface 112 that substantially faces the front side 102 of the first sub-module 100, and a second surface 114 that substantially faces the back side 104 of the first sub-module 100. One or more layers of material may be disposed between the first surface 112 and the second surface 114 of the substrate 110.
[0059]
[0074] 4, the substrate 110 may include a transparent layer 120 having a first surface 122 substantially facing the front side 102 of the first submodule 100 and a second surface 124 substantially facing the back side 104 of the first submodule 100. In some embodiments, the second surface 124 of the transparent layer 120 may form the second surface 114 of the substrate 110. The transparent layer 120 may be formed from a substantially transparent material, such as, for example, glass. Suitable glasses may include soda-lime glass or any glass with reduced iron content. The transparent layer 120 may have any suitable transmittance range, in some embodiments, including from about 250 nm to about 1,300 nm. The transparent layer 120 may also have any suitable transmittance percentage, including, for example, greater than about 50% in one embodiment, greater than about 60% in another embodiment, greater than about 70% in yet another embodiment, greater than about 80% in a further embodiment, or greater than about 85% in yet a further embodiment. In one embodiment, the transparent layer 120 may be formed from glass having a transmittance of about 90% or greater. Optionally, the substrate 110 may include a coating 126 applied to the first surface 122 of the transparent layer 120. The coating 126 may be configured to interact with light or improve the durability of the substrate 110, such as, but not limited to, an anti-reflective coating, an anti-soiling coating, or a combination thereof.
[0060]
[0075] 3 , the first sub-module 100 may include a barrier layer 130 configured to mitigate diffusion of contaminants from the substrate 110 that may result in degradation or delamination of other layers of the photovoltaic stack. The barrier layer 130 may have a first surface 132 that substantially faces the front side 102 of the first sub-module 100 and a second surface 134 that substantially faces the back side 104 of the first sub-module 100. In some embodiments, the barrier layer 130 may be provided adjacent to the substrate 110. For example, the first surface 132 of the barrier layer 130 may be provided on the second surface 114 of the substrate 110.
[0061]
[0076] In general, the barrier layer 130 may be substantially transparent, thermally stable, have a low number of pinholes, have a high sodium blocking capability, and have good adhesion properties. Alternatively or additionally, the barrier layer 130 may be configured to apply color suppression to light. The barrier layer 130 may include one or more layers of suitable materials including, but not limited to, tin oxide, silicon dioxide, aluminum doped silicon oxide, silicon oxide, silicon nitride, or aluminum oxide. The barrier layer 130 may have any suitable thickness bounded by the first surface 132 and the second surface 134, including, for example, greater than about 10 nanometers in one embodiment, greater than about 15 nm in another embodiment, or less than about 20 nm in a further embodiment.
[0062]
[0077] Continuing to refer to FIG. 3, the first sub-module 100 may include a transparent conductive oxide (TCO) layer 140 configured to provide an electrical contact for transporting charge carriers generated by the first sub-module 100. The TCO layer 140 may have a first surface 142 that faces substantially the front side 102 of the first sub-module 100 and a second surface 144 that faces substantially the back side 104 of the first sub-module 100. In some embodiments, the TCO layer 140 may be provided adjacent to the barrier layer 130. For example, the first surface 142 of the TCO layer 140 may be provided on the second surface 134 of the barrier layer 130. In general, the TCO layer 140 may be formed from one or more layers of a substantially transparent, wide bandgap n-type semiconductor material. In particular, the wide bandgap may have a large energy value compared to the energy of the photons of light, thereby mitigating undesired absorption of light. The TCO layer 140 may include one or more layers of suitable materials, including, but not limited to, tin dioxide, doped tin dioxide (e.g., F-SnO2), indium tin oxide, or cadmium tin oxide (Cd2SnO4). In embodiments in which the TCO layer 140 includes cadmium stannate, the cadmium stannate may be provided in a crystalline form. For example, the cadmium stannate may be deposited as a film and then subjected to an annealing process that converts the thin film into a crystallized film.
[0063]
[0078] The first sub-module 100 may include a buffer layer 150 configured to provide an insulating layer between the TCO layer 140 and any adjacent semiconductor layers. The buffer layer 150 may have a first surface 152 that faces substantially the front side 102 of the first sub-module 100 and a second surface 154 that faces substantially the back side 104 of the first sub-module 100. In some embodiments, the buffer layer 150 may be provided adjacent to the TCO layer 140. For example, the first surface 152 of the buffer layer 150 may be provided on the second surface 144 of the TCO layer 140. The buffer layer 150 may be formed of any suitable material, including, but not limited to, intrinsic tin dioxide, zinc magnesium oxide (e.g., Zn 1-x Mgx The buffer layer 150 may comprise a material having a higher resistivity than the TCO layer 140, including silicon dioxide (SiO), silicon oxide (SiO), aluminum oxide (Al2O3), aluminum nitride (AlN), zinc tin oxide, zinc oxide, silicon tin oxide, or any combination thereof. In some embodiments, the material of the buffer layer 150 may be configured to substantially match the band gap of an adjacent semiconductor layer (e.g., absorber). The buffer layer 150 may have a suitable thickness between the first surface 152 and the second surface 154, including, for example, greater than about 10 nm in one embodiment, between about 10 nm and about 80 nm in another embodiment, or between about 15 nm and about 60 nm in further embodiments.
[0064]
[0079] 3, the first submodule 100 may include an absorber layer 160 configured to cooperate with another layer to form a pn junction within the first submodule 100. Thus, absorbed photons of light can release electron-hole pairs and generate carrier flow, thereby resulting in electrical energy. The absorber layer 160 may have a first surface 162 that substantially faces the front side 102 of the first submodule 100, and a second surface 164 that substantially faces the back side 104 of the first submodule 100. A thickness of the absorber layer 160 may be defined between the first surface 162 and the second surface 164. The thickness of the absorber layer 160 may be, for example, from about 0.5 μm to about 10 μm, such as from about 1 μm to about 7 μm in one embodiment, or from about 1.5 μm to about 4 μm in another embodiment.
[0065]
[0080] The absorber layer 160 may be formed from a p-type semiconductor material that has an excess of positive charge carriers, i.e., holes or acceptors. In one example, the absorber layer 160 may include a Group I-III-VI absorber material, such as, for example, copper indium gallium sulfide / selenide (CIGS), copper gallium sulfide / selenide (CGS), or CuInSe2 (CIS), and may be provided as a thin film. The absorber layer 160 may include a suitable p-type semiconductor material, such as a Group II-VI semiconductor, for example, cadmium and tellurium (CdTe) or cadmium selenide (CdSe). Further examples of Group II-VI absorber materials include, but are not limited to, semiconductor materials that include cadmium, zinc, tellurium, selenium, or any combination thereof. In some embodiments, the absorber layer 160 may include a ternary system of cadmium, selenium, and tellurium (e.g., CdSe x Te 1-x ), or a compound including cadmium, selenium, tellurium, and one or more additional elements (e.g., CdZnSeTe). The absorber layer 160 may further include one or more dopants. The first sub-module 100 provided herein may include multiple absorber materials.
[0066]
[0081] In embodiments in which the absorber layer 160 includes tellurium and cadmium, the average atomic percentage of tellurium in the absorber layer 160 may be greater than about 25 atomic percent and less than about 50 atomic percent, such as, for example, greater than about 30 atomic percent and less than about 50 atomic percent in one embodiment, greater than about 40 atomic percent and less than about 50 atomic percent in a further embodiment, or greater than about 47 atomic percent and less than about 50 atomic percent in yet another embodiment. Alternatively or additionally, the average atomic percentage of tellurium in the absorber layer 160 may be greater than about 45 atomic percent, such as, for example, greater than about 49 atomic percent in one embodiment. It should be noted that the average atomic percentages described herein represent the entirety of the absorber layer 160, and that the atomic percentage of material at a particular location within the absorber layer 160 may be graded through the thickness as compared to the overall composition of the absorber layer 160. For example, the absorber layer 160 may have a graded composition.
[0067]
[0082] In embodiments in which absorber layer 160 includes selenium and tellurium, the average atomic percent of selenium in absorber layer 160 may be greater than 0 atomic percent and less than or equal to about 25 atomic percent, such as, for example, greater than about 1 atomic percent and less than about 20 atomic percent in one embodiment, greater than about 1 atomic percent and less than about 15 atomic percent in another embodiment, or greater than about 1 atomic percent and less than about 8 atomic percent in a further embodiment. Note that the concentration of tellurium, selenium, or both may be graded through the thickness of absorber layer 160. For example, if absorber layer 160 includes a compound including a mole fraction of selenium of x and a mole fraction of tellurium of 1-x (Se x Te 1-x ), x may vary within the absorber layer 160 with distance from the first surface 162 of the absorber layer 160.
[0068]
[0083] 3, the absorber layer 160 may be doped with a dopant configured to manipulate the charge carrier concentration. In some embodiments, the absorber layer 160 may be doped with a Group VA (Group 15) dopant, such as, for example, arsenic, phosphorus, antimony, or a combination thereof. Alternatively or additionally, the absorber layer 160 may be doped with a Group IB (Group 11) dopant, such as, for example, copper, silver, gold, or a combination thereof. The total density of dopants in the absorber layer 160 may be controlled. Additionally, the amount of dopant may vary with distance from the first surface 162 of the absorber layer 160.
[0069]
[0084] FIG. 3 shows an exemplary layer structure, and the composition has been described with an example including II-VI materials. In other embodiments, the first sub-module 100 of the tandem photovoltaic device 300 can use other photovoltaic materials with alternative layer structures to produce a photovoltaic sub-module. In one example, the first sub-module 100 may include a I-III-VI absorber material, such as, for example, copper indium gallium sulfide / selenide (CIGS) or CuInSe2 (CIS), and may be provided as a thin film. In another example, the first sub-module 100 may include a perovskite absorber. In a further example, the first sub-module 100 may include a silicon absorber, which may include amorphous, polycrystalline, crystalline, or thin film silicon.
[0070]
[0085] According to embodiments provided herein, a p-n junction may be formed by providing an absorber layer 160 in sufficient proximity to a portion of the first submodule 100 that has an excess of negative charge carriers; e.g., electrons or donors. In some embodiments, the absorber layer 160 may be provided adjacent to an n-type semiconductor material. Alternatively, one or more intervening layers may be provided between the absorber layer 160 and the n-type semiconductor material. In some embodiments, the absorber layer 160 may be provided adjacent to the buffer layer 150. For example, the first surface 162 of the absorber layer 160 may be provided on the second surface 154 of the buffer layer 150.
[0071]
[0086] The first submodule 100 may include a back contact layer 170 configured to mitigate undesired alterations of the dopant and to provide electrical contact to the absorber layer 160. The back contact layer 170 may have a first surface 172 that substantially faces the front side 102 of the first submodule 100 and a second surface 174 that substantially faces the back side 104 of the first submodule 100. A thickness of the back contact layer 170 may be defined between the first surface 172 and the second surface 174. The thickness of the back contact layer 170 may be from about 5 nm to about 200 nm, such as from about 10 nm to about 50 nm in one embodiment.
[0072]
[0087] In some embodiments, the back contact layer 170 may be provided adjacent to the absorber layer 160. For example, the first surface 172 of the back contact layer 170 may be provided on the second surface 164 of the absorber layer 160. In some embodiments, the back contact layer 170 may include a combination of materials from groups I, II, VI, such as, for example, one or more layers including zinc and tellurium in various compositions. Further suitable materials include, but are not limited to, bilayers of cadmium zinc telluride and zinc telluride, or zinc telluride doped with a group V (group 15) dopant, such as nitrogen. The thin film junction 176 may be defined as the thin film stack that primarily contributes to the photovoltaic effect. For example, in some embodiments, the thin film junction 176 may include the transparent conductive oxide layer 140, the buffer layer 150, the absorber layer 160, the back contact layer 170, or a combination thereof.
[0073]
[0088] Referring to FIG. 3, the first submodule 100 may include a conductive layer 180, which may be transparent and configured to provide electrical contact with the back contact layer 170, the absorber layer 160, or both. In some embodiments, the conductive layer 180 may be formed toward the backside of the first submodule 100 relative to the absorber layer 160. When provided in a single junction device or as part of a lower or rear submodule (e.g., the second submodule 500), the conductive layer 180 may be disposed on the backside of the submodule (e.g., the second submodule 500) and may use a turbid opaque metal layer as a component. However, opaque layers may not be suitable for use as the conductive layer 180 of the first submodule 100, which is disposed between the junctions of a multijunction or tandem photovoltaic device. The conductive layer 180 may have a first surface 182 that substantially faces the front side 102 of the first submodule 100, and a second surface 184 that substantially faces the back side 104 of the first submodule 100. In some embodiments, the conductive layer 180 may be provided adjacent to the back contact layer 170 or the absorber layer 160. For example, the first surface 182 of the conductive layer 180 may be provided on the second surface 174 of the back contact layer 170 or the second surface 162 of the absorber layer 160. A thickness of the conductive layer 180 may be defined between the first surface 182 and the second surface 184. The thickness of the conductive layer 180 may be less than about 500 nm, such as, for example, from about 40 nm to about 400 nm, or from about 60 nm to about 350 nm in one embodiment.
[0074]
[0089] The first submodule 100 may have a back layer 199 on the backside 104 of the first submodule 100. The back surface of the back layer 199 defines the front submodule backside 104. In some embodiments, the back layer 199 is a region of the conductive layer 180. In some embodiments, the back layer 199 includes an electron reflector layer. In some embodiments, the back layer 199 includes a tunnel junction having a p+ subregion and an n+ subregion. In some embodiments, the back layer 199 includes a tunnel junction having a p++ subregion and an n++ subregion.
[0075]
[0090] Materials such as semiconductors and transparent conducting oxides may be doped with impurities to alter their electrical and optical properties. Dopants may be incorporated into functional layers to modify the n-type or p-type charge carrier concentration. Charge densities of around 1×10 16 cm -3 If the electron donor carrier is greater than about 1×10, it may be considered to be of the "+" type. The boundary is not strict, but it is 11 cm -3 ~Approx. 1×10 16 cm -3 in the range, the material may be considered n-type, with a donor carrier density of approximately 1×10 16 cm -3 Similarly, if the electron acceptor carriers (i.e., "holes") are greater than about 1×10 11 cm -3 ~Approx. 1×10 16 cm -3 in the range, the material is generally considered p-type, with an acceptor carrier density of approximately 1 × 10 16 cm -3 If the carrier concentration is greater than 100 times higher, it is considered p+ type. Regardless of the absolute carrier density, the boundary is not exact and may overlap, since a layer can be p+ for a layer that is p-type (or n+ for a layer that is n-type) if the carrier concentration is at least two orders of magnitude (i.e., 100 times) higher. Furthermore, the boundary is not exact and may overlap, since a layer can be p+ for a layer that is p-type (or n+ for a layer that is n-type) if the carrier concentration is at least two orders of magnitude (i.e., 100 times) higher. 18 cm -3 The greater charge density may be considered to be of the "++" type. Thus, a layer of either n-type or p-type may be "++" relative to a layer of the same type which is itself "+" relative to a third layer if the ++ layer has more than 100 times the carrier density of the same type as the + layer.
[0076]
[0091] 1 and 5, the tandem photovoltaic device 300 includes a second sub-module 500. The second sub-module 500 may be disposed below or below the first sub-module 100, with the front side 302 of the tandem photovoltaic device 300 as the top surface facing the primary light. The photovoltaic device sub-module 500 may include multiple layers disposed between a first surface 502 of the front side of the second sub-module 500 and a second surface of the back side of the second sub-module 500. One or more of the multiple layers may include a photovoltaic absorber material. In some embodiments, the layers of the photovoltaic device sub-module 500 may be divided into multiple photovoltaic cells.
[0077]
[0092] The second sub-module 500 of the tandem photovoltaic device 300 may include one or more absorber materials in a layered structure. In one example, the second sub-module 500 may include a silicon absorber, which may include amorphous, polycrystalline, crystalline, or thin-film silicon. In another example, the second sub-module 500 may include a perovskite absorber material. In a further example, the second sub-module 500 may include a I-III-VI absorber material, such as CIGS, and may be provided as a thin film. In another example, the second sub-module 500 may include a II-VI absorber material, such as CdTe, CdZnTe, HgCdTe, or CdSeTe.
[0078]
[0093] The second sub-module 500 may share various aspects with the first sub-module 100. The second sub-module 500 may have a front layer 501 on a front side 502 of the second sub-module 500. The front surface of the front layer 501 may define the front surface 502 of the second sub-module 500. In some embodiments, the front layer 501 is a buffer layer. In some embodiments, the front layer 501 is a conductive layer. In some embodiments, the front layer 501 includes a conductive metal grid. In some embodiments, the front layer 501 includes a transparent conductive oxide. In certain embodiments, the remainder or the entirety of the second sub-module 500 may be configured the same or substantially the same as the first sub-module 100. An embodiment of the second sub-module 500 may include portions that are the same or substantially the same in function and structure as portions of the first sub-module 100. In some embodiments, the tandem photovoltaic device 300 includes a second intermediate layer and a backing sheet on a second surface 504 of the second sub-module. In some embodiments, the second intermediate layer comprises a material that comprises the same matrix polymer as the second insulating protective layer 430. In some embodiments, the second intermediate layer is fused to the second insulating protective layer 430 at the periphery of the device. In some embodiments, the backing sheet comprises a material that comprises the same material as the core layer 420. In other embodiments, the backing sheet comprises glass. In some embodiments, the second sub-module is substantially encapsulated by the polymer that comprises the second insulating protective layer 430, and electrical connectors such as bus connections pass therethrough. The encapsulation of the sub-modules by the intermediate layer and the second intermediate layer may contribute to improved robustness of the tandem module.
[0079]
[0094] With continued reference to Figures 1 and 5, the tandem photovoltaic device 300 includes an intermediate layer 400. As shown, the intermediate layer structure is positioned between the first sub-module 100 and the second sub-module 500. An example of the intermediate layer 400 structure is depicted in cross-section in Figure 6. According to embodiments provided herein, the intermediate layer 400 may include a first insulating protective layer 410 and a core layer 420, where the first insulating protective layer 410 is disposed between the core layer 420 and the back layer 199 of the first sub-module 100. In some embodiments, the core layer 420 may be provided between the first insulating protective layer 410 and the second insulating protective layer 430. In some embodiments, the core layer 420 may be provided adjacent to the first insulating protective layer 410 and adjacent to the second insulating protective layer 430. For example, the first surface 422 of the core layer 420 may be provided on the second surface 414 of the first insulating protective layer 410, and the first surface 432 of the second insulating protective layer 430 may be provided on the second surface 424 of the core layer 420. Thus, in some embodiments, the first surface 402 of the intermediate layer 400 may be formed by the first surface 412 of the first insulating protective layer 410, and the second surface 402 of the intermediate layer 400 may be formed by the second surface 434 of the second insulating protective layer 430.
[0080]
[0095] According to embodiments provided herein, the thickness of the intermediate layer 400 may be defined between the first surface 402 and the second surface 404. The thickness of the intermediate layer 400 may be continuous and substantially uniform in certain embodiments, with a thickness deviation across the intermediate layer 400 of less than 25%. In one example, the thickness of the intermediate layer 400 may be about six hundred fifty microns (650 μm). In some embodiments, the thickness is in the range of 100 μm to 2500 μm, such as, for example, about 250 μm to 1500 μm, or about 400 μm to 1000 μm.
[0081]
[0096] In some embodiments, the thickness of the intermediate layer 400 may be continuous and irregular. In one example, the core layer is substantially uniform, while one or both of the first and second insulating protective layers 410, 430 are substantially irregular in thickness. As an example, the intermediate layer includes a substantially uniform core layer combined with a substantially irregular insulating protective layer. This combination benefits from the electrical isolation and mechanical strength of the core material combined with the flowability and adhesion of the insulating protective layer to fill and mitigate surface irregularities of adjacent module surfaces. The insulating protective layer adheres continuously to directly adjacent surfaces of the submodules and core layer. In some embodiments, the uniform layer deviates from the average thickness by no more than 25%, or in the range of 0% to 25%. In some embodiments, the irregular or non-uniform layer includes a thickness deviation of more than 30%, more than 40%, or more than 50% of its average thickness. In some embodiments, the irregular or non-uniform layer comprises a thickness deviation in the range of 30% to 100%, in the range of 30% to 90%, in the range of 40% to 90%, in the range of 40% to 80%, or in the range of 45% to 75% of the average thickness of the irregular layer.
[0082]
[0097] Particular embodiments of the intermediate layer 400 may include cases where the entire intermediate layer 400 or one or more layers of the intermediate layer 400 have a refractive index of about 1.2 to about 2.0 (e.g., about 1.6) for light having a wavelength of 800 nm. In some embodiments, at least one of the first insulating protective layer 410, the second insulating protective layer 430, and the core layer 420 may have a refractive index of about 1.2 to about 2.0, and particular embodiments include one or more layers having a refractive index greater than 1.6 for light having a wavelength of 800 nm. In some embodiments, at least one of the first insulating protective layer 410, the second insulating protective layer 430, and the core layer 420 may have a refractive index in the range of 1.6 to 2.5 for light having a wavelength of 800 nm.
[0083]
[0098] Interlayer 400 may have an average transmittance of greater than 20% for light having wavelengths between 800 nm and 1200 nm. Optionally, interlayer 400 may have an average transmittance of greater than about 25% for light having wavelengths between 800 nm and 1200 nm, such as, for example, greater than about 50% in one embodiment, or greater than about 60% in another embodiment, or greater than about 75% in a further embodiment.
[0084]
[0099] Without being bound by theory, the interlayer 400 provided herein provides synergistic advantages to tandem photovoltaic devices. Providing the interlayer 400 with the core layer 420 between the insulating protective layers 410, 430 provides advantages in both manufacturability and operation. The core layer 420 can prevent short circuits and provide physical and electrical isolation. The insulating protective layers 410, 430 can provide good contact to the core layer 420 and the respective sub-modules 100, 500, thereby providing reliable optical properties between the sub-modules 100, 500 with minimal irregularities such as voids and bubbles. Additionally, the interlayer 400 encapsulates the sub-modules 100, 500, preventing moisture ingress thereto and mitigating corrosion, degradation and performance degradation that may be associated with humid environments.
[0085]
[0100] The core layer 420 of the intermediate layer 400 can provide a dielectric and physical barrier that resists deformation and narrowing of the dielectric breakdown distance. The core layer 420 can have a melting point greater than 200° C. In certain embodiments, the core layer 420 can have a melting point greater than 250° C., while other embodiments include when the core layer 420 has a melting point in the range of about 225° C. to about 550° C. In some embodiments, the core layer 420 can have a dielectric breakthrough strength greater than 10 kV / mm, greater than 20 kV / mm, greater than 50 kV / mm, in the range of 10 kV / mm to 250 kV / mm, or in the range of 10 kV / mm to 200 kV / mm.
[0086]
[0101] The core layer 420 may comprise a polymer sheet. In certain embodiments, the core layer 420 may have a thickness ranging from 10 μm to 400 μm. In some embodiments, the core layer 420 may have a thickness greater than 15 μm, greater than 20 μm, greater than 30 μm, greater than 40 μm, greater than 50 μm, greater than 60 μm. In some embodiments, the core layer 420 may have a thickness less than 400 μm, less than 300 μm, less than 200 μm, less than 250 μm, less than 200 μm, less than 150 μm, less than 120 μm, less than 100 μm, less than 90 μm, less than 80 μm, or less than 70 μm. In some embodiments, the core layer 420 may have a thickness of about 40 μm to 140 μm. In some embodiments, the material forming the core layer 420 is a thermoplastic polymer resin. In some embodiments, the material forming the core layer 420 may include one or more of oriented polyethylene terephthalate (OPET), polytetrafluoroethylene (PTFE), polycyclooctene (PCO), or biaxially oriented polyethylene terephthalate (boPET).
[0087]
[0102] In general, each of the insulating protective layers 410, 430 may be formed of a material including a flowable polymer with a melting point below 170°C to be compatible with system components during lamination with the submodules 100, 500 and operation at high temperatures. In some embodiments, the insulating protective layers 410, 430 are formed of a material with a melting point below 110°C. In some embodiments, one or both of the insulating protective layers 410, 430 have a melting point within a range of about 50°C to about 170°C, within a range of 70°C to 170°C, within a range of 70°C to 110°C, within a range of 90°C to 140°C, or within a range of 80°C to 110°C. In some embodiments, one or both of the insulating protective layers 410, 430 have a melting point below 150°C, below 130°C, below 120°C, below 110°C, or below 100°C.
[0088]
[0103] Materials for the first insulating protective layer 410 may include polyethylene (PE), ethylene-vinyl acetate (EVA), and / or polyolefin elastomer (POE). Other materials suitable for use in the layer include various optically compatible adhesives.
[0089]
[0104] The thickness of each of the insulating protective layers 410, 430 may be from about 180 μm to about 740 μm. In some embodiments, the first insulating protective layer 410 has a thickness greater than 180 μm, greater than 200 μm, greater than 220 μm, greater than 250 μm, or greater than 280 μm. In some embodiments, the first insulating protective layer 410 has a thickness less than 700 μm, less than 600 μm, less than 500 μm, less than 400 μm, less than 350 μm, or less than 320 μm. In some embodiments, the second insulating protective layer 430 has a thickness greater than 180 μm, greater than 200 μm, greater than 220 μm, greater than 250 μm, or greater than 280 μm. In some embodiments, the second insulating protective layer 430 has a thickness less than 700 μm, less than 600 μm, less than 500 μm, less than 400 μm, less than 350 μm, or less than 320 μm.
[0090]
[0105] The insulating protective layers 410, 430 may be configured to conform to the irregularities of nearby surfaces, including the surface roughness of either the second surface 104 of the first submodule 100 or the first surface 502 of the second submodule 500, respectively. In some embodiments, the ratio of the average surface roughness of the nearby surfaces to the thickness of the respective adjacent insulating protective layers is between 1:1 and 1:1000. In some embodiments, the ratio of the average surface roughness of the nearby surfaces to the thickness of the insulating protective layers is greater than 1:1, greater than 1:2, greater than 1:10, greater than 1:50, or greater than 1:100. In some embodiments, the ratio of the average surface roughness of the nearby surfaces to the thickness of the insulating protective layers is less than 1:900, less than 1:750, less than 1:500, less than 1:300, or less than 1:200. The flowable composition of the insulating protective layers at processing temperatures during fabrication provides beneficial wetting and adhesion despite the surface irregularities.
[0091]
[0106] 7, an embodiment of a method of making a tandem photovoltaic device is shown at 700. A first step at 705 may include providing an intermediate layer 400 as described herein, the intermediate layer 400 allowing a portion of the light to pass through. A second step at 710 may include directly contacting a first insulating protective layer 410 with a portion of a surface (e.g., second surface 104) of the first submodule 100. A third step at 715 may include conforming the first insulating protective layer 410 with a portion of a surface (e.g., second surface 104) of the first submodule 100. A fourth step at 720 may include directly contacting a second insulating protective layer 430 with a portion of a surface (e.g., first surface 502) of the second submodule 500. A fifth step at 725 may include applying a second insulating protective layer 500 to a portion of a surface (eg, first surface 502 ) of the second sub-module 500 .
[0092]
[0107] The intermediate layer 400 may be formed in a variety of ways. In certain embodiments, the core layer 420, the first insulating protective layer 410, and the second insulating protective layer 430 may be laminated together in a pre-bonding step to form the intermediate layer 400. The core layer 420 may be laminated between the first insulating protective layer 410 and the second insulating protective layer 430 to provide the intermediate layer 400. In certain embodiments, one or more layers of the intermediate layer are coextruded as a single sheet or layer. The core layer 420 may be coextruded between the first insulating protective layer 410 and the second insulating protective layer 430 to provide the intermediate layer 400.
[0093]
[0108] 7 depicts the steps of the method 700 sequentially, it is understood that certain steps may be performed simultaneously and / or certain steps may be performed in a different order than depicted. For example, the first insulating protective layer 410 may be conformed to a portion of the surface of the first sub-module 100 by heating the first insulating protective layer 410 to at least the melting point of the first polymer. Similarly, the second insulating protective layer 430 may be conformed to a portion of the surface of the second sub-module 500 by heating the second insulating protective layer 430 to at least the melting point of the second polymer. The portion of the surface of the first sub-module 100 and one of the first insulating protective layers 410 may be heated to at least the melting point of the first polymer before directly contacting the first insulating protective layer 410 with the portion of the surface of the first sub-module 100. Similarly, one of the second sub-module 500 surface portion and the second insulating protective layer 430 may be heated to at least the melting point of the second polymer before directly contacting the second sub-module 500 surface portion with the second insulating protective layer 430. Certain embodiments include where the steps of conforming the first insulating protective layer 410 to the first sub-module 100 surface portion and conforming the second insulating protective layer 430 to the second sub-module 500 surface portion include simultaneously heating the first sub-module 100, the intermediate layer 400, and the second sub-module 500 to at least the melting point of the first polymer and at least the melting point of the second polymer after directly contacting the first insulating protective layer 410 to the first sub-module 100 surface portion and directly contacting the second insulating protective layer 430 to the second sub-module 500 surface portion. Furthermore, by pressing the intermediate layer 400 and the first submodule 100 together, it is possible to conform the first insulating protective layer 410 to a portion of the surface of the first submodule 100, and by pressing the intermediate layer 400 and the second submodule 500 together, it is possible to conform the second insulating protective layer 430 to a portion of the surface of the second submodule 500.The step of conforming the first insulating protective layer 410 to a portion of the surface of the first sub-module 100 and the second insulating protective layer to a portion of the surface of the second sub-module 500 may include pressing the intermediate layer 400 between the first sub-module 100 and the second sub-module 500.
[0094]
[0109] In some embodiments, a method of forming a tandem photovoltaic device includes directly contacting the backside or second surface 104 of the first sub-module 100 with the first surface 402, 412 of the first insulating protective layer 410; directly contacting the frontside or first surface 502 of the second sub-module 500 with the second surface 404, 434 of the second insulating protective layer 430; and providing a core layer 420 between the first insulating protective layer 410 and the second insulating protective layer 430. The method may include conforming the first insulating protective layer to a surface of the first sub-module; and conforming the second insulating protective layer to a surface of the second sub-module.
[0095]
[0110] The method may be carried out at a processing temperature below the melting temperature of the core layer. The processing temperature may be near, at, or above the melting temperature of the insulating protective layer. In some cases, the processing temperature is within 15° C. above or below the melting temperature of the first polymer. In some cases, the processing temperature is within 15° C. above or below the melting temperature of the second polymer. In some cases, the processing temperature is higher than the melting temperatures of the first and second polymers. In some embodiments of the method of bonding the intermediate layer to the first and second submodules, the processing temperature is 20-150° C. lower than the melting temperature of the third polymer that constitutes the core layer. In some cases, the processing temperature is in the range of 80-170° C. In some cases, the processing temperature is less than 150° C., less than 140° C., less than 130° C., less than 120° C., less than 110° C., less than 100° C., less than 90° C., or less than 85° C.
[0096]
[0111] By controlling the thickness and composition of the sublayers of the interlayer, the heat capacity and heat transfer of the material during fabrication can be controlled to prevent damage to the temperature sensitive components of adjacent modules at processing temperatures suitable for fusion bonding the insulating protective layer to the surface of the adjacent module. During the lamination or bonding process at processing temperatures, the core layer may be a solid continuous sheet, while at the same time one or both of the insulating protective layers are heated to a flowable viscous state. The method results in a durable interlayer with good adhesion, robust electrical breakthrough strength, and high transparency to near infrared wavelengths.
[0097]
[0112] The exemplary embodiments are provided so that the disclosure is thorough and fully conveys its scope to those skilled in the art. Numerous specific details are set forth, such as examples of specific components, devices and methods, to provide a thorough understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that specific details need not be utilized, that the exemplary embodiments may be embodied in many different forms, and that none of these should be construed to limit the scope of the present disclosure. In some exemplary embodiments, well-known processes, well-known device structures, and well-known technologies are not described in detail. Equivalent changes, modifications and variations of some embodiments, materials, compositions and methods can be made within the scope of the present technology with substantially similar results.
Claims
1. A first sub-module; A second submodule; and an intermediate layer disposed between the first submodule and the second submodule, where the intermediate layer transmits a portion of light passing through the intermediate layer, and the intermediate layer a first insulating protective layer conforming directly to a portion of a surface of the first submodule, the first insulating protective layer comprising a first polymer having a melting point less than 170° C.; a second insulating protective layer conforming in direct contact with a portion of a surface of the second submodule, said second insulating protective layer comprising a second polymer having a melting point less than 170° C.; and a core layer disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, wherein the core layer comprises a third polymer having a melting point greater than 200° C. Including, A tandem photovoltaic device comprising:
2. The tandem photovoltaic device of claim 1 , wherein the intermediate layer has a refractive index in the range of 1.4 to 1.8 at 800 nm.
3. the first polymer has a melting point in the range of 70° C. to 120° C.; the second polymer has a melting point in the range of 70° C. to 120° C.; and The tandem photovoltaic device of claim 1 , wherein the third polymer has a melting point in the range of 200° C. to 300° C.
4. The tandem photovoltaic device of claim 1 , wherein the intermediate layer has a dielectric strength greater than about 10 kV / mm.
5. The tandem photovoltaic device of claim 1 , wherein the intermediate layer has a thickness of about 100 μm to about 1500 μm.
6. The tandem photovoltaic device of claim 1 , wherein the intermediate layer is configured to transmit at least 90% of light having a wavelength between about 700 nm and about 1300 nm therethrough.
7. 10. The tandem photovoltaic device of claim 1, wherein the first polymer and the second polymer independently comprise a member selected from the group consisting of polyethylene; ethylene-vinyl acetate; polyolefin elastomers; and combinations thereof.
8. The tandem photovoltaic device of claim 1 , wherein the first polymer and the second polymer comprise the same material.
9. 10. The tandem photovoltaic device of claim 1, wherein the third polymer comprises a member selected from the group consisting of oriented polyethylene terephthalate; polytetrafluoroethylene; polycyclooctene; biaxially oriented polyethylene terephthalate; polyimide; and combinations thereof.
10. The tandem photovoltaic device of claim 1 , wherein the core layer has a thickness in the range of 25 μm to 200 μm.
11. The tandem photovoltaic device of claim 1 , wherein the core layer has a dielectric strength greater than about 50 kV / mm.
12. The tandem photovoltaic device of claim 1 , wherein the first and second insulating protective layers have different thicknesses.
13. 2. The tandem photovoltaic device of claim 1 , wherein the first insulating protective layer has a thickness of about 300 μm, the second insulating protective layer has a thickness of 300 μm, the core layer has a thickness of 100 μm, and the third polymer of the core layer comprises biaxially oriented polyethylene terephthalate.
14. 1. An interlayer for a tandem photovoltaic device comprising: the intermediate layer has a first submodule and a second submodule, and the intermediate layer is configured to be disposed between the first submodule and the second submodule, wherein the intermediate layer transmits a portion of light passing through the intermediate layer and has a refractive index of about 1.2 to about 2.0, a dielectric strength of greater than about 10 kV / mm, and a thickness of about 100 μm to about 1500 μm, the intermediate layer comprising: a first insulating protective layer conforming in direct contact with a portion of a surface of the first submodule, wherein the first insulating protective layer comprises a first polymer having a melting point less than about 170° C., the first polymer comprising a member selected from the group consisting of polyethylene, ethylene-vinyl acetate, polyolefin elastomers, and combinations thereof; a second insulating protective layer conforming directly to a portion of a surface of the second submodule, wherein the second insulating protective layer comprises a second polymer having a melting point less than about 170° C., the second polymer comprising a member selected from the group consisting of polyethylene, ethylene-vinyl acetate, polyolefin elastomers, and combinations thereof; and a core layer disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, wherein the core layer has a dielectric strength greater than about 50 kV / mm and comprises a third polymer having a melting point greater than about 200° C., the third polymer comprising a member selected from the group consisting of oriented polyethylene terephthalate, polytetrafluoroethylene, polycyclooctene, biaxially oriented polyethylene terephthalate, polyimide, and combinations thereof; Including, Including, the middle layer.
15. 1. A method of making a tandem photovoltaic device, comprising: providing an intermediate layer, wherein said intermediate layer transmits a portion of light passing through said intermediate layer, said intermediate layer comprising: a first insulating protective layer comprising a first polymer having a melting point less than about 170° C.; a second insulating protective layer comprising a second polymer having a melting point less than about 170° C.; a core layer disposed between the first insulating protective layer and the second insulating protective layer and in direct contact with the first insulating protective layer and the second insulating protective layer, the core layer comprising a third polymer having a melting point greater than about 200° C.; Including; directly contacting a portion of a surface of a first submodule with the first insulating protective layer; applying the first insulating protective layer to a portion of a surface of the first sub-module; direct contact of a portion of a surface of the second submodule with the second insulating protective layer; and Conforming the second insulating protective layer to a portion of a surface of the second sub-module. A method comprising:
16. The method of claim 15 further comprising laminating the core layer between the first and second insulating protective layers to provide the intermediate layer.
17. 16. The method of claim 15, further comprising co-extruding the core layer between the first and second insulating protective layers to provide the intermediate layer.
18. Conforming the first insulating protective layer to a portion of a surface of the first submodule includes heating the first insulating protective layer to at least a melting point of the first polymer; and 16. The method of claim 15, wherein conforming the second insulating protective layer to a portion of a surface of the second sub-module comprises heating the second insulating protective layer to at least a melting point of the second polymer.
19. one of a portion of a surface of the first submodule and the first insulating protective layer is heated to at least a melting point of the first polymer prior to directly contacting the portion of a surface of the first submodule with the first insulating protective layer; and 16. The method of claim 15, wherein one of the portion of the surface of the second sub-module and the second insulating protective layer is heated to at least a melting point of the second polymer prior to directly contacting the portion of the surface of the second sub-module with the second insulating protective layer.
20. 16. The method of claim 15, wherein conforming the first insulating protective layer to a portion of a surface of the first submodule and conforming the second insulating protective layer to a portion of a surface of the second submodule comprises directly contacting the first insulating protective layer with a portion of a surface of the first submodule and directly contacting the second insulating protective layer with a portion of a surface of the second submodule, followed by simultaneously heating the first submodule, the intermediate layer, and the second submodule to at least a melting point of the first polymer and at least a melting point of the second polymer.
21. Conforming the first insulating protective layer to a portion of a surface of the first sub-module includes pressing the intermediate layer and the first sub-module together; or The method of claim 15 , wherein conforming the second insulating protective layer to a portion of a surface of the second sub-module comprises pressing the intermediate layer and the second sub-module together.
22. 16. The method of claim 15, wherein conforming the first insulating protective layer to a portion of a surface of the first sub-module and conforming the second insulating protective layer to a portion of a surface of the second sub-module comprises pressing the intermediate layer between the first sub-module and the second sub-module.
23. 16. The method of claim 15, wherein the contacting is carried out at a process temperature of less than 120°C.
24. A first sub-module; A second sub-module; an intermediate layer disposed between the first sub-module and the second sub-module, the intermediate layer transmitting a portion of light passing through the intermediate layer, the intermediate layer comprising: a first insulating protective layer conforming in direct contact with a portion of a surface of the first submodule, the first insulating protective layer comprising a first polymer having a melting point less than 170°C; a second insulating protective layer conforming in direct contact with a portion of a surface of the second submodule, the second insulating protective layer comprising a second polymer having a melting point less than 170° C.; a core layer disposed between the first insulating protective layer and the second insulating protective layer, the core layer comprising a third polymer having a melting point greater than 200° C.; Including, A tandem photovoltaic device comprising:
25. A tandem photovoltaic device according to any one of claims 3 to 14 or claim 24, an intermediate layer according to claim 14, or a method according to any one of claims 15 to 24, wherein the intermediate layer has a refractive index in the range of 1.4 to 1.8 at 800 nm.
26. the first polymer has a melting point in the range of 70° C. to 120° C.; the second polymer has a melting point in the range of 70° C. to 120° C.; and A tandem photovoltaic device according to any one of claims 3 to 14 or claims 24 to 25, an intermediate layer according to claim 14, or a method according to any one of claims 15 to 24, wherein the third polymer has a melting point in the range of 200°C to 300°C.
27. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 26, wherein the intermediate layer has a dielectric strength of greater than about 10 kV / mm.
28. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 27, wherein the intermediate layer has a thickness of from about 100 μm to about 1500 μm.
29. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 28, wherein the intermediate layer is configured to transmit at least 90% of incident light having a wavelength from about 800 nm to about 1200 nm.
30. The tandem photovoltaic device of any one of claims 3-14 or claims 24-25, the intermediate layer of claim 14, or the method of any one of claims 15-29, wherein the first polymer and the second polymer independently comprise a member selected from the group consisting of polyethylene, ethylene-vinyl acetate, polyolefin elastomers, and combinations thereof.
31. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 30, wherein the first polymer and the second polymer comprise the same material.
32. The tandem photovoltaic device of any one of claims 3-14 or claims 24-25, the intermediate layer of claim 14, or the method of any one of claims 15-31, wherein the third polymer comprises a member selected from the group consisting of oriented polyethylene terephthalate, polytetrafluoroethylene, polycyclooctene, biaxially oriented polyethylene terephthalate, polyimide, and combinations thereof.
33. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 32, wherein the core layer has a thickness in the range of 25 μm to 200 μm.
34. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 33, wherein the core layer has a dielectric strength greater than about 50 kV / mm.
35. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, the intermediate layer of claim 14, or the method of any one of claims 15 to 34, wherein the first and second insulating protective layers have different thicknesses.
36. The tandem photovoltaic device of any one of claims 3 to 14 or claims 24 to 25, wherein the first insulating protective layer has a thickness of about 300 μm, the second insulating protective layer has a thickness of 300 μm, the core layer has a thickness of 100 μm, and the third polymer of the core layer comprises biaxially oriented polyethylene terephthalate, the intermediate layer of claim 14, or the method of any of claims 15 to 34.
Citation Information
Patent Citations
Silicon-based thin-film tandem solar cell and manufacturing method thereof
CN104538477A
Solar cell backside sheet and solar cell module
JP2013115216A