Production method of steel plate with excellent workability before hot forming, steel plate, manufacturing process of hot stamped parts and hot stamped parts
A steel sheet with a controlled chemical composition and microstructure, combined with a specific manufacturing process, addresses the hardness issue in multi-stage hot stamping, ensuring easy processing before hot stamping and high strength after, enhancing production flexibility and reducing tool wear.
Patent Information
- Application Number
- JP2024526615
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-05
- Filing Date
- 2022-11-02
- Publication Date
- 2024-11-26
AI Technical Summary
The challenge of producing steel sheets suitable for multi-stage hot stamping processes is that they become too hard during production, making them difficult to wind into coils and cut into blanks without damaging cutting tools, especially when coated or annealed, which affects their workability before hot stamping.
A steel sheet with a specific chemical composition and microstructure that allows for low hardness before hot stamping, enabling easy processing, combined with a manufacturing process that includes controlled annealing and cooling to maintain softness, ensuring a microstructure with at least 60% ferrite and limited bainite, martensite, and carbides.
The steel sheets remain soft enough for easy handling and processing before hot stamping, while achieving high hardness and strength after hot stamping, reducing tool wear and maintaining flexibility in production lines without requiring specific cooling rate controls.
Smart Images

Figure 2024543823000001 
Figure 2024543823000002 
Figure 2024543823000003
Abstract
Description
[Technical field]
[0001] The present invention relates to steel sheets and high strength press hardened steel parts having excellent formability before hot forming. [Background technology]
[0002] Multi-stage processing of steel sheets to create complex parts using hot forming is becoming more and more popular. By increasing the number of operations that can be performed on the steel sheet, the multi-stage process allows hot stampers to produce parts with more complex shapes compared to traditional single-stage hot stamping. It also allows the number of post-processing steps on the parts to be reduced. This in turn makes it possible to better address the challenges facing the automotive industry of improving the safety and environmental performance of vehicles while maintaining high industrial production rates and low manufacturing costs.
[0003] Compared to standard single-stage hot stamping, the amount of processing time is longer in multi-stage hot stamping. As a consequence, the very rapid cooling rates obtained in single-stage hot stamping cannot be achieved in multi-stage processes. It is therefore necessary to use specific steel compositions, which make it possible to harden the steel and reach the desired very high mechanical properties even at the relatively low cooling rates of multi-stage processing. For example, it is interesting to use steel compositions that can be transformed into an austenite or ferrite + austenite structure and hardened into a martensite microstructure even at cooling rates of less than 20 ° C / s, preferably less than 16 ° C / s.
[0004] However, such steel compositions present the technical disadvantage that they can easily be hardened during the production of the steel coils themselves, for example on the metal coating line in the case of coated steels or on the continuous annealing line in the case of bare steels. Indeed, the steel compositions of steels suitable for multi-stage processing make it possible to harden them even at the relatively low cooling rates carried out after the annealing furnaces on these lines. Summary of the Invention [Problem to be solved by the invention]
[0005] This is a problem for processing the steel before hot stamping: in fact, the steel is too hard to be easily wound in the form of a coil on the line where the annealing is carried out, and then cut into steel blanks before hot stamping, without excessive maintenance of cutting tools, or preformed before hot stamping, as is the case in the indirect hot stamping process.
[0006] The object of the present invention is to address this problem by providing a steel sheet that is soft enough for good workability before hot stamping, yet has a chemistry and microstructure suitable for use in a multi-stage hot stamping process.
[0007] A further object of the present invention is to provide a process for manufacturing said steel sheet.
[0008] A steel plate refers to a flat steel plate having an upper and lower surface, also called the upper and lower surfaces or the upper and lower surfaces. The distance between said surfaces is designated as the thickness of the steel plate. The thickness can be measured, for example, using a micrometer, the spindle and anvil of which are placed on the upper and lower surfaces. Similarly, the thickness can also be measured on a molded part.
[0009] A blank refers to a flat steel sheet from which it is cut into any shape suitable for its use.
[0010] In the following description, claims and examples, the term steel sheet generally refers to the material before further processing operations such as cutting into blanks and before hot stamping, whereas the term blank refers to the material cut from the steel sheet to be used in the hot stamping process.
[0011] Hot stamping is a steel forming technique that involves heating a steel blank, or a preform made from a steel blank, to a temperature at which the microstructure of the steel is at least partially transformed into austenite, forming the blank or preform at high temperature by stamping, and simultaneously quenching the formed part to obtain a microstructure with very high strength, possibly with an additional distribution or tempering step in the heat treatment.
[0012] A multi-step hot stamping process is a specific type of hot stamping process consisting of at least two process steps, including at least one stamping step, carried out at high temperatures above 300°C. For example, a multi-step process can involve a first stamping operation and a subsequent hot trimming operation, so that there is no need to further trim the finished part at the end of the hot stamping process. For example, a multi-step process can involve several successive stamping steps to produce parts with more complex shapes than can be realized using a single stamping operation. For example, the parts are automatically transferred from one operation to another in a multi-step process, for example using a transfer press. For example, the parts remain in the same tool, which is a multi-purpose tool that can perform different operations, such as a first stamping and a subsequent in-tool trimming operation.
[0013] Hot stamping makes it possible to obtain very high strength parts with complex shapes and presents many technical advantages. Multi-stage hot stamping makes it possible to obtain even more complex shapes than single-stage hot stamping.
[0014] Hardness is a measure of resistance to localized plastic deformation induced by mechanical indentation. It correlates well with the mechanical properties of materials and is a useful local measurement method that does not require cutting out samples for tensile testing. In the present invention, hardness measurements are performed using a Vickers indenter according to the ISO 6507-1 standard. Vickers hardness is expressed using the unit Hv.
[0015] In the present specification, examples and claims, the terms annealing, annealing furnace and annealing process all refer to a metallurgical process in which cold rolled steel sheet is recrystallized by heating it. For steels with phases other than ferrite, annealing is carried out at a temperature at least above Ac1 (the temperature at which the microstructure starts to transform to austenite).
[0016] The term cooling rate refers to the rate at which the steel plate is cooled during the annealing process while it is being manufactured. The soaking temperature refers to the maximum temperature the steel plate reaches in the annealing furnace. The cooling rate, expressed in °C / s, is the average rate at which the steel plate is cooled between the soaking temperature and 300 °C. The cooling rate can be expressed using the following formula: Cooling rate = (annealing temperature - 300°C) / (time the steel sheet takes to reach 300°C after leaving the annealing furnace).
[0017] The terms austenitizing and quenching refer to the hot stamping process of a steel blank.
[0018] Quenching speed or quenching speed The term quenching rate refers to the average rate, expressed in °C / s, at which the steel blank is cooled to 300 °C during the hot stamping process. The austenitizing temperature refers to the maximum temperature reached by the steel blank in the austenitizing furnace before hot stamping. The quenching rate can be expressed using the following formula: Quenching rate = (austenitizing temperature - 300°C) / (time taken by the steel blank to reach 300°C after leaving the austenitizing furnace).
[0019] The composition of the steel according to the invention will now be described, the contents being expressed in percentages by weight. The chemical composition is given in terms of lower and upper limits of a compositional range, said limits themselves being included within the possible compositional range according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] According to the present invention, the carbon content is in the range of 0.13% to 0.4% to ensure a satisfactory strength. If the carbon content exceeds 0.4%, the weldability and bendability of the steel sheet may be deteriorated. If the carbon content is less than 0.13%, the tensile strength after hot stamping does not reach the target value.
[0021] The manganese content ranges from 0.4% to 4.2%. If the addition amount exceeds 4.2%, the risk of central segregation increases, which leads to loss of workability, and the risk of crack formation during hot stamping and subsequent use of the part increases. If it is less than 0.4%, the hardenability of the steel sheet decreases and the required strength is not achieved after hot stamping.
[0022] The silicon content ranges from 0.1% to 2.5%. Silicon is an element involved in hardening in solid solution. Silicon is added to limit the formation of carbides. If it exceeds 2.5%, silicon oxide forms on the surface, which impairs the coatability of the steel. Also, the weldability of the steel plate may decrease.
[0023] The chromium content does not exceed 2%. Chromium is the element responsible for hardening in solid solution. The chromium content is preferably limited to less than 2% in order to limit workability problems and costs.
[0024] The molybdenum content does not exceed 0.65%. Molybdenum improves the hardenability of the steel. Molybdenum is below 0.65% to limit costs.
[0025] The niobium content is limited to 0.1%. Niobium improves the ductility of the steel. Above 0.1%, the risk of formation of coarse NbC or Nb(C,N) precipitates increases with loss of workability. Preferably, the niobium content is in the range of 0.02% to 0.06%.
[0026] According to the present invention, aluminum is limited to 3.0%. Aluminum is a very effective element to deoxidize steel in the liquid phase during smelting. Aluminum can protect boron when the titanium content is not sufficient. The aluminum content is less than 3.0% to avoid oxidation problems and ferrite formation during press hardening.
[0027] According to the invention, titanium is limited to 0.1%. Titanium can protect boron. Boron can be trapped in BN precipitates. The titanium content is limited to 0.1% to avoid excessive TiN formation.
[0028] According to the invention, the boron content is limited to 0.005%. Boron improves the hardenability of the steel. The boron content is less than or equal to 0.005% in order to avoid the problem of slab fracture during continuous casting.
[0029] Phosphorus is controlled to less than 0.025% as it causes brittleness and weldability problems.
[0030] Since the presence of sulfur in the molten steel can result in the formation of MnS precipitates which are detrimental to bendability, sulfur is controlled to less than 0.01%.
[0031] Nitrogen is controlled to less than 0.01%. The presence of nitrogen can lead to the formation of precipitates such as TiN or TiNbCN, which adversely affects the workability of the steel.
[0032] Nickel is optionally added up to a level of 2.0%. Nickel can be used to protect the steel from delayed cracking. The nickel content is limited to limit cost.
[0033] Calcium may also be added as an optional element up to 0.1%. The addition of Ca at the liquid stage allows for the production of fine oxides which promote castability in continuous casting.
[0034] Tungsten may also be added as an optional element up to 0.3%. In these amounts, tungsten enhances hardenability and hardenability due to the formation of carbides.
[0035] Vanadium may be added up to 0.1%. It improves the ductility of the steel. Above 0.1%, the risk of forming coarse precipitates increases with loss of workability.
[0036] Copper is limited to 0.2%. Cu acts to strengthen the steel by solid solution strengthening. Above 0.2%, there is a risk of high temperature embrittlement during the hot rolling process.
[0037] The balance of the steel composition are inevitable impurities resulting from the iron and smelting process and depending on the process route. In the case of the production route using a blast furnace, the level of inevitable impurities is very low. In the case of the production route using an electric arc furnace loaded with scrap, the steel plate may further contain residual elements coming from such scrap, such as up to 0.03% antimony, arsenic and lead, and up to 0.05% tin. These are considered inevitable impurities.
[0038] In a particular embodiment, the chemical composition of the steel sheet is (in weight percent): C: 0.15-0.25% Mn: 0.5-1.8% Silicon: 0.1 to 1.25% Cr: 0.1-1.0% Al: 0.01 to 0.1% Ti: 0.01 to 0.1% B: 0.001 to 0.004% P≦0.020% S≦0.010% N≦0.010% and optionally including, in weight percent, one or more of the following elements: Mo≦0.40% Nb≦0.08% Ca≦0.1% The balance of the composition is iron and inevitable impurities resulting from smelting.
[0039] In a particular embodiment, the chemical composition of the steel sheet is (in weight percent): C: 0.26-0.40% Mn: 0.5-1.8% Silicon: 0.1 to 1.25% Cr: 0.1-1.0% Al: 0.01 to 0.1% Ti: 0.01 to 0.1% B: 0.001 to 0.004% P≦0.020% S≦0.010% N≦0.010% and optionally including, in weight percent, one or more of the following elements: Ni≦0.5% Mo≦0.40% Nb≦0.08% Ca≦0.1% The balance of the composition is iron and inevitable impurities resulting from smelting. In a particular embodiment, the chemical composition of the steel sheet is (in weight percent): C: 0.3-0.4% Mn: 0.5-1.0% Silicon: 0.4 to 0.8% Cr: 0.1-0.4% Mo: 0.1-0.5% Nb: 0.01 to 0.1% Al: 0.01 to 0.1% Ti: 0.008~0.03% B: 0.0005~0.003% P≦0.020% S≦0.004% N≦0.005% Ca≦0.001% and optionally, Ni<0.5% The balance of the composition is iron and inevitable impurities resulting from smelting, In a particular embodiment, the chemical composition of the steel sheet is (in weight percent): C: 0.24-0.38% Mn: 0.40~3% Silicon: 0.10 to 0.70% Cr: 0~2% Al: 0.015 to 0.070% Nb≦0.060% Ti: 0.015~0.10% N: 0.003~0.010% S: 0.0001 to 0.005% P: 0.0001 to 0.025% Ni: 0.25~2% and Ti / N>3,42,
[0040]
number
[0041] In a particular embodiment, the steel sheet composition comprises the following elements expressed in weight percent: C: 0.15-0.4% Mn: 1-3.5% Silicon: 1.0 to 1.65% Cr≦2% Al≦0.5% Ti≦0.1% B≦0.005% The balance of the composition is iron and inevitable impurities resulting from smelting.
[0042] In a particular embodiment, the steel sheet composition comprises the following elements expressed in weight percent: C: 0.15% to 0.25% Mn: 1.5% to 2.5% Silicon: 0.1% to 0.4% Cr≦0.5% Al: 0.03% to 1% Ti: 0.02% to 0.1% B: 0.0015% to 0.0050% P≦0.012% The balance of the composition is iron and inevitable impurities resulting from smelting.
[0043] In a particular embodiment, the steel sheet composition comprises the following elements expressed in weight percent: C: 0.1 to 0.3% Mn: 3-4.2% Silicon: 0.7 to 2% Al: 0.1-1% Mo: 0.1-0.5% Nb: 0.01 to 0.05% Ti: 0.01 to 0.05% B: 0.001 to 0.005% The balance of the composition is iron and inevitable impurities resulting from smelting.
[0044] In order to be suitable for use in a multi-stage hot stamping process, the chemical composition of the steel sheet according to the invention further satisfies the following formula (the elements are expressed in % by weight): Q<20 In the formula, Q=114-68*C-18*Mn+20*Si-56*Cr-61*Ni-37*Al+39*Mo+79*Nb-17691*B This formula was established using dilatometric experiments on samples with different steel compositions. The samples were heated in a furnace to a temperature of 900°C and held at that temperature for 2 minutes. The samples were then quenched using different quenching rates. Metallographic investigations were carried out on the quenched samples to determine their microstructures. The critical quenching rate for a given sample was defined as the quenching rate at which the quenched sample has a fully martensitic microstructure. A linear regression was then established between the chemical composition of the sample and the critical quenching rate determined by the above protocol. The factor Q was determined by this linear regression and corresponds to a very good approximation of the limiting quenching rate for low carbon steels.
[0045] The inventors have found that if Q<20, the steel can withstand the relatively low cooling rates of the multi-stage hot stamping process.
[0046] Preferably, the steel has an even lower coefficient Q, Q≦16.
[0047] The steel sheet according to the invention has the following microstructure (expressed as surface fraction): -At least 60% ferrite - Less than 40% of the sum of bainite + martensite + carbides Less than 5% non-recrystallized ferrite Ferrite is a soft phase. The presence of at least 60% ferrite in the steel sheet ensures that the sheet is soft enough for processing.
[0048] By limiting the amount of bainite, martensite and carbides in the microstructure, the inventors have found that the steel sheet has a sufficiently low hardness to machine well in the cold state prior to hot stamping.
[0049] By limiting the amount of non-recrystallized ferrite, the inventors have found that the steel sheet has a sufficiently low hardness to machine well in the cold state prior to hot stamping.
[0050] For example, the steel sheet according to the invention has a hardness of less than 270 Hv, which roughly corresponds to a tensile strength of more than 800 MPa. Above this strength level, mechanical processing such as cutting becomes increasingly difficult, requiring difficult and expensive maintenance operations of the cutting tools.
[0051] In a particular embodiment, the steel sheet according to the invention has high hardenability after hot stamping and quenching.
[0052] Hardenability is characterized by the increased hardness of the steel blank obtained from the steel sheet after hot stamping. It can be measured by subjecting the steel sheet to a hot stamping operation and measuring the hardness before and after.
[0053] The fast quench rate hardenability ΔHvhi of a steel sheet is defined as ΔHvhi=Hvfast-Hvini, where Hvfast is the hardness of the steel sheet after heating it to a temperature of 900°C for 7 minutes and quenching it at a rate of 100°C / s, and Hvini is the hardness of the steel sheet before heat treatment.
[0054] For example, the high quench rate hardenability ΔHvhi of the steel plate is at least 200 Hv.
[0055] The low quench rate hardenability ΔHvlo of a steel plate is defined as ΔHvlo=Hvslow-Hvini, where Hvslow is the hardness of the steel plate after heating it to a temperature of 900°C for 7 minutes and quenching it at a rate of 20°C / s, and Hvini is the hardness of the steel plate before heat treatment.
[0056] Thanks to the fact that the steel sheet according to the invention can be quenched at a low quenching rate and still has a very high hardness after hot stamping, the low quenching rate hardenability ΔHvlo of the steel sheet according to the invention remains high, for example ΔHvlo is at least 150Hv, more preferably at least 180Hv, even more preferably at least 200Hv.
[0057] Another way to express the fact that the steel sheets according to the invention can be quenched at low quenching rates and still have a very high hardness after hot stamping is to consider the difference ΔHvhi-ΔHvlo, which is the same as the difference Hvfast-Hvslow. The difference Hvfast-Hvslow of the steel sheets according to the invention is low because the material still reaches a very high hardness after hot stamping at low quenching rates. For example, the difference Hvfast-Hvslow is less than 100Hv, preferably less than 50Hv, even more preferably less than 40Hv.
[0058] The steel sheet according to the invention is manufactured according to the following process path: - Casting a steel slab having the above-mentioned composition and subjecting it to a temperature T reheat After being reheated to 300° C., the steel sheet is hot-rolled at a finish hot-rolling temperature in the range of 800° C. to 950° C. to obtain a hot-rolled steel sheet.
[0059] -The hot rolled steel is then cooled and coiled at a temperature T below 670 °C and optionally pickled to remove oxidation.
[0060] The coiled steel sheet is then cold rolled to obtain a cold rolled steel sheet. The cold rolling reduction is in the range of 20% to 80%, preferably 35% to 80%. Below 20%, recrystallization during the subsequent heat treatment is not favorable, which may impair the ductility of the steel sheet. Above 80%, there is a risk of edge cracking during cold rolling.
[0061] The cold rolled steel sheet is then subjected to an annealing step, and optionally subsequently subjected to a metal coating step, for example, the steel sheet is coated with an aluminum-based metal coating, for example, the steel sheet is coated with a zinc-based metal coating.
[0062] For example, a steel sheet may be coated with an aluminium-based metallic coating containing, by weight, 7% to 15% silicon, 2% to 4% iron and optionally 15 ppm to 30 ppm calcium, the balance being aluminium and unavoidable impurities resulting from smelting.
[0063] For example, a steel sheet is coated with an aluminium-based metallic coating comprising 2.0-24.0 wt. % zinc, 1.1-12.0 wt. % silicon, optionally 0-8.0 wt. % magnesium and optionally an additional element selected from Pb, Ni, Zr or Hf, the weight content of each additional element being lower than 0.3 wt. %, the balance being aluminium and unavoidable impurities.
[0064] The annealing process is conducted such that the K factor, as further defined below, remains less than 0.50.
[0065] The K-factor is defined according to the steel composition of the steel plate by the following formula (all elements expressed in weight percent): For steel compositions where Mn-Si>1.5%:
[0066]
number
[0067]
number
[0068] Ae1=734+77*C-29*Mn+14*Si+7*Cr-38*Ni-22*Al-25*Mo+123*Nb-8621*B Ae3=935-257*C-25*Mn+32*Si-17*Cr-83*Ni+17*Al+129*Mo+156*Nb-19473*B The inventors have found, through numerous experiments and numerical correlations, that the steel sheets produced using the above-mentioned processing route have a sufficiently low hardness in the cold state before the hot stamping operation in order to be easily processed. In particular, when annealing the cold-rolled steel sheets to reach a sufficiently low hardness, it is important to respect the above K<0.50. The final product after annealing and optionally coating the steel sheets has a hardness of less than 270Hv.
[0069] Furthermore, the inventors have found that when applying the present invention, the hardness of the steel sheet is surprisingly almost independent of the cooling rate after the annealing step: even if the steel sheet has a chemical composition that ensures that it has a low critical quenching rate after being fully austenitized before hot stamping it (thanks to Q<20 or even preferentially Q≦16), the material surprisingly does not reach very high hardness levels even when cooled relatively fast on the line where it is annealed after cold rolling.
[0070] This behavior of the steel sheets on the annealing line is very beneficial from an industrial point of view, since it means that the steel sheets have a sufficiently low hardness regardless of the thermal path that follows after annealing. This brings robustness to the product properties and allows for a higher flexibility after annealing. In particular, it means that no specific adaptations have to be made to the layout of existing production lines after annealing to accommodate multi-stage steels. It also makes it possible to apply any type of metallic coating, the application of which affects the thermal path, without having to worry about the hardness of the final product, especially when performing hot-dip coatings.
[0071] Next, the manufacturing process of the pressed parts and the subsequent properties of the pressed parts will be described in detail.
[0072] A steel blank is cut from the steel sheet according to the invention and heated in an austenitizing furnace to a temperature above Ac1. Preferably, the steel blank is heated to a temperature comprised between 880°C and 950°C for 10 seconds to 15 minutes to obtain a heated steel blank. The heated blank is then transferred to a forming press before being hot formed. For example, the hot forming process is a multi-stage process. For example, the hot forming process has a quenching rate of less than 20°C / s, greater than or equal to 3°C / s, preferably greater than or equal to 5°C / s.
[0073] The microstructure of the hot stamped component includes a surface fraction of greater than 95% martensite and less than 5% bainite + ferrite, for example, the hot stamped component has a hardness greater than 400 Hv, and even more preferably greater than 440 Hv.
[0074] The present invention is illustrated by the following examples which are not intended to be limiting in any way.
[0075] In all tables, sample values and references that are outside the invention are underlined.
[0076] [Table 1]
[0077] Table 1 lists the six different chemical compositions tested, along with the associated Q-factors Ae1 and Ae3, all calculated using the formula above.
[0078] A, B, C, D and E are all within the scope of the present invention, while F is outside the scope since the Q factor calculation for F gives a result of 27. It is noted that steel composition F corresponds to a typical composition of 22MnB5 steel for hot stamping.
[0079] As will be explained in more detail below, this difference in Q-factors between Steels A-E and Steel F means that samples made using Steels A-E can be hot stamped and simultaneously quenched at a low quench rate and still obtain greater than 95% martensitic microstructure, but if the quench rate is too low, Steel F will not have a 95% martensitic microstructure.
[0080] [Table 2]
[0081] Table 2 lists the production parameters for the hot and cold rolling processes, all of which are also within the scope of the present invention. The same set of parameters was used for each chemistry.
[0082] [Table 3]
[0083] [Table 4]
[0084] Table 3 lists the process parameters used during the annealing step. These parameters were varied to produce examples within and outside the production process of the present invention.
[0085] Table 4 lists the results of hardness testing and microstructural analysis for each sample.
[0086] In Tables 3 and 4, references to examples within the invention begin with an I (for the invention) and counterexamples begin with an R (for the reference).
[0087] Referring to Table 3, all of the examples within the present invention have K-factors strictly less than 0.50, whereas the reference examples all have annealing process parameters which, when formulated through the K-factor equation, result in a K-factor of 0.50 or greater.
[0088] With reference to Table 4, thanks to the specific set of process parameters of the examples of the present invention resulting in a K factor of less than 0.50, all examples within the present invention present a steel hardness (Hvini) before hot stamping that is less than 270Hv, which allows the steel sheets to be easily processed before hot forming, for example to mechanically cut the steel sheets without damaging the cutting tools, or to wind and unwind them in forms such as coils.
[0089] Referring to Table 4, all samples according to the present invention have a microstructure before hot stamping that includes a surface fraction of 60% to 100% recrystallized ferrite, less than 40% total martensite, bainite and carbides, and less than 5% non-recrystallized ferrite. This particular microstructure, which includes a large amount of ferrite that is soft and limits the amount of hard phases (martensite, bainite, carbides and non-recrystallized ferrite), makes it possible to limit the hardness of the steel sheet to less than 270 Hv.
[0090] On the other hand, all the reference samples with annealing process parameters such that the K-factor is 0.50 or more exhibit a steel sheet hardness Hvini of more than 270 Hv. Their microstructures contain less than 60% recrystallized ferrite. Furthermore, the amount of non-recrystallized ferrite is either more than 5% (sample R2) or the sum of the surface fractions of martensite, bainite and carbides is more than 40% (all other reference samples).
[0091] Due to their very high hardness before hot stamping, said reference samples are difficult to process before hot stamping, which creates production problems in the facilities of the manufacturers of the steel sheets themselves (difficulty in leading the material on the production line, winding in coils, cutting at the exit of the line, etc.) as well as in the facilities of the hot stampers and intermediates (difficulty in cutting blanks, punch holes, etc.).
[0092] Furthermore, it is noted that the above properties and results are obtained for a wide range of cooling rates after the annealing furnace. Indeed, the cooling rates in Table 3 range from 3°C / s to 100°C / s. This means that the annealing process according to the invention is robust, regardless of the subsequent cooling rate on the line where the annealing is performed. There is no need to specifically control the cooling rate, for example by using an overaged section of the cooling section after the annealing. This is of great interest to steel sheet manufacturers who do not need to introduce specific cooling rate control measures after the annealing furnace.
[0093] [Table 5]
[0094] Table 5 shows the results of tests on steels A to F at high and low quenching rates.
[0095] The samples in Table 5 were subjected to two different hot stamping process thermal paths for each chemistry using the same set of parameters in the austenitizing furnace and two different sets of quenching parameters. The samples produced using the high quenching rate were quenched at 100°C / s after leaving the austenitizing furnace. The samples produced using the low quenching rate were quenched at rates ranging from 5°C / s to 20°C / s after leaving the austenitizing furnace according to the sample. All samples were heated in the same manner to 900°C and held at that temperature for a dwell time of 387 seconds.
[0096] The microstructure of the samples thus produced and their hardness are reported in Table 5.
[0097] In all cases, when high quench rates are used, the subsequent hot stamped parts have a microstructure containing greater than 95% martensite and a hardness greater than 440 Hv, which translates to a tensile strength greater than about 1400 MPa.
[0098] On the other hand, when using a slow cooling rate, a hot stamped part produced using steel F with a Q factor of 27 has a microstructure containing only 30% martensite and a large proportion of the softer phases ferrite (30%) and bainite (40%). As a result, the hardness of the hot stamped parts thus produced is much lower, with a significant gap of 127 Hv between the hardness of the high quench rate parts and the low quench rate parts.
[0099] However, steel compositions A-E all have a Q factor below 20, and even more preferably below 16, resulting in hot stamped parts with more than 95% martensite even at low quenching rates of 20°C / s or less. This is thanks to their low Q factors that allow them to be much less sensitive to quenching rate. As a result, the hardness of hot stamped parts at low quenching rates produced with steels A-E remains above 440Hv, and the hardness gap between high and low quenching rate parts remains very low at below 40Hv.
[0100] This means that steel compositions A to E are suitable for use in hot stamping processes having low cooling rates, e.g. below 20 °C / s, e.g. these steel compositions are suitable for use in multi-stage hot stamping processes.
[0101] In conclusion, samples produced with steels A to E and using annealing process parameters such that the K factor is kept below 0.50 are both suitable for use in hot stamping processes with low quenching rates, e.g. below 20°C / s or even below 16°C / s, but are soft enough before hot stamping to be easily processed, e.g. by cutting or preforming.
Claims
1. 1. A method for producing a steel sheet having the following chemical composition, in weight percent: C: 0.13-0.4% Mn: 0.4-4.2% Si: 0.1-2.5% Cr≦2% Mo≦0.65% Nb≦0.1% Al≦3.0% Ti≦0.1% B≦0.005% P≦0.025% S≦0.01% N≦0.01% Ni≦2.0% Ca≦0.1% W≦0.30% V≦0.1% Cu≦0.2% The remainder of the composition is iron and inevitable impurities resulting from smelting; Q is less than 20, and the coefficient Q is: Q=114-68*C-18*Mn+20*Si-56*Cr-61*Ni-37*Al+39*Mo+79*Nb-17691*B (all elements expressed as weight percent); It is defined as The method further comprising: Before being hot-rolled at a finish hot-rolling temperature comprised between -800 ° C and 950 ° C, the cast slab having the above composition is subjected to a temperature T comprised between 1100 ° C and 1300 ° C. reheat to obtain a hot rolled steel sheet; - cooling and coiling the hot-rolled steel sheet at a temperature T below 670 ° C., and optionally pickling the hot-rolled steel sheet; cold rolling the pickled hot-rolled steel sheet by applying a rolling reduction in the range of -20% to 80% to obtain a cold-rolled steel sheet; - annealing said cold rolled steel sheet using the following annealing line process parameters: -K<0.50, where K is If the steel composition is such that Mn-Si (wt%)>1.5 wt%: [0010] In the case where the steel composition is such that Mn-Si≦1.5 wt.%: [0025] wherein: - Tsoaking is the soaking temperature, expressed in ° C., i.e. the maximum temperature reached by the steel sheet during the annealing process; -t is the recrystallization time in seconds, which is defined as the time spent above 700°C during the annealing step; the heating rate at which the steel plate reaches the soaking temperature expressed in °C / s, i.e. Heating rate = (Tsoaking-30) / (time taken from 30°C to Tsoaking) Ae1 = 734 + 77 * C - 29 * Mn + 14 * Si + 7 * Cr - 38 * Ni - 22 * Al - 25 * Mo + 123 * Nb - 8621 * B (all elements expressed in weight percent), Ae3 (all elements expressed in weight%)=935-257*C-25*Mn+32*Si-17*Cr-83*Ni+17*Al+129*Mo+156*Nb-19473*B (all elements expressed in weight%).
2. A steel plate made from a steel having a composition comprising, in weight percent: C: 0.13-0.4% Mn: 0.4-4.2% Si: 0.1-2.5% Cr≦2% Mo≦0.65% Nb≦0.1% Al≦3.0% Ti≦0.1% B≦0.005% P≦0.025% S≦0.01% N≦0.01% Ni≦2.0% Ca≦0.1% W≦0.30% V≦0.1% Cu≦0.2% The balance of the composition is iron and inevitable impurities resulting from smelting, Q is less than 20, and the coefficient Q is Q = 114 - 68 * C - 18 * Mn + 20 * Si - 56 * Cr - 61 * Ni - 37 * Al + 39 * Mo + 79 * Nb - 17691 * B (all elements expressed in weight percent) It is defined as The steel plate has a microstructure including, in terms of surface fraction, 60% to 100% recrystallized ferrite, less than 40% of the sum of martensite, bainite, and carbides, and less than 5% of non-recrystallized ferrite; The steel plate has a hardness of less than 270 Hv.
3. The steel sheet of claim 2 further comprising an Al-based metallic coating.
4. The steel sheet of claim 2 further comprising a Zn-based metallic coating.
5. 1. A method for producing a hot stamped part, comprising the steps of: - providing a blank manufactured from a steel sheet manufactured according to claim 1; - heating said blank to an austenitizing temperature above Ac1; - transferring the blank to a hot stamping tool and simultaneously forming and quenching the steel sheet at a quenching rate of less than or equal to 20°C / s and more than or equal to 5°C / s, where quenching rate = (austenitizing temperature - 300°C) / (time taken by the steel blank to reach 300°C after leaving the austenitizing furnace).
6. The method of claim 5 , wherein the hot stamping process is a multi-step process.
7. A hot stamped part made from a blank manufactured from the steel sheet according to any one of claims 2 to 4, wherein hot stamping is carried out using a quenching rate of less than 20°C / s, and the microstructure of said hot stamped part comprises a surface fraction of at least 95% martensite, said quenching rate = (austenitizing temperature - 300°C) / (time taken by the steel blank to reach 300°C after leaving the austenitizing furnace).
Citation Information
Patent Citations
Hot rolled steel sheet for hot press, method for producing the same and method for producing hot press formed member
JP2006265583A
Method of manufacturing hot press molded steel member having high strength and excellent strength-ductility balance
JP2014156653A
Plated steel sheet for hot forming with excellent impact properties, hot formed member, and manufacturing method thereof
JP2020509203A
Process for producing hot stamp molded article, and hot stamp molded article
WO2012053636A1
Steel sheet for hot-stamped member and process for producing same
WO2012128225A1