Reflective mask blank and method for producing the same
Electron beam annealing addresses the issue of elemental diffusion in EUV lithography masks by focusing on surface treatment, resulting in improved reflectance and flatness of the multilayer reflective films, which enhances the integration density and performance of EUV lithography masks.
Patent Information
- Application Number
- JP2024529200
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-17
- Filing Date
- 2022-11-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-16
AI Technical Summary
Existing EUV lithography technologies face challenges in improving the reflectance of reflective masks due to elemental diffusion at the interfaces of multilayer reflective films, leading to reduced reflectivity and limited integration density.
Applying electron beam annealing to the multilayer reflective film of reflective mask blanks, specifically targeting the surface layers to prevent elemental diffusion and enhance the flatness and reflectance without heating the underlying layers.
The method improves the reflectance and flatness of the multilayer reflective film, enhancing the integration density and reducing surface roughness, thereby improving the performance of EUV lithography masks.
Smart Images

Figure 2024543848000001_ABST
Abstract
Description
[Technical field]
[0001]
[0002] The present invention relates to a reflective mask blank and a method for manufacturing the same, and more particularly to a reflective mask blank used in an EUV lithography process and a method for manufacturing the same. [Background technology]
[0003] Recently, in order to improve the integration density of semiconductors, lithography technology using extreme ultraviolet (hereinafter referred to as "EUV") has been attracting attention as an alternative to conventional lithography technology using ultraviolet light (wavelength 193~365nm) or ArF excimer laser light (wavelength 193nm).
[0004] For example, the EUV lithography technology currently under development uses light with an extreme ultraviolet wavelength of 13.5 nm, enabling a high level of miniaturization of integrated circuits that could not be achieved with conventional lithography technologies that use wavelengths of 100 nm or longer.
[0005] EUV light has the advantage of being able to increase integration density, but it has the disadvantage of being easily absorbed by all materials due to its very short wavelength. This means that refractive optical systems such as transmissive masks, which were mainly used in conventional lithography technology, cannot be used. Therefore, reflective optical systems such as reflective masks must be used in EUV lithography.
[0006] A reflective mask is formed by forming a multi-layer reflective film on a substrate so that it can reflect EUV light, and then forming an absorbing film on the multi-layer reflective film to absorb EUV light. When this absorbing film is etched with a semiconductor pattern, the EUV light reflected by the reflective film below the etched surface forms a pattern, and the pattern is exposed on the wafer. In other words, a reflective mask is obtained by removing a part of the absorbing film to form a specified pattern using a reflective mask blank (blank mask) formed by sequentially stacking a multi-layer reflective film and an absorbing film on a substrate as an original plate.
[0007] In order to improve the integration density in such an EUV lithography process, a technology is required to improve the physical properties of the reflective mask blank itself, such as increasing the reflectivity of the multilayer reflective film in the layered structure of the reflective mask and increasing the contrast with the absorbing film.
[0008] Japanese Patent Publication No. 2004-104118 (title of invention: Reflective mask blank and manufacturing method of reflective mask, published on 2004.04.02) discloses a heat treatment technique for manufacturing a reflective mask blank, in which a multilayer reflective film is laminated and then heated at a temperature lower than the pre-bake temperature of the registry film to offset the film stress formed in the multilayer reflective film, thereby improving the flatness of the multilayer reflective film and increasing the reflectivity. However, heat treatment at a certain temperature or higher causes mutual diffusion of the elements constituting the multilayer reflective film, making the boundaries between the reflective films unclear, and instead reduces the reflectivity of the mask.
[0009] Japanese Patent Publication No. 2006-013280 (title of invention: Reflective mask blank and manufacturing method of semiconductor device using a reflective mask, published on January 12, 2006) discloses a technology for preventing diffusion by performing hydrogen termination on the surface of the top layer of a multilayer reflective film in order to prevent a decrease in reflectivity during heating in a baking process of a photoresist film, which is a subsequent process for a reflective mask blank. However, although such hydrogen termination can prevent diffusion of Si, which is a constituent element of the top layer, by mixing hydrogen into the top layer of the multilayer reflective film, it has a problem of generating a new factor for reducing reflectivity by doping hydrogen, which corresponds to impurity.
[0010] Japanese Patent Publication No. 2018-029498 (title of invention: Reflective mask blank and method for manufacturing a semiconductor device using a reflective mask, published on June 7, 2018) discloses a technology in which a protective film made of ruthenium (Ru) is laminated between the multilayer reflective film and absorbing film of a reflective mask blank, and an annealing treatment (80°C, 1 hour) is performed on this protective film in air, oxygen gas, or ozone gas atmosphere to form a diffusion prevention layer made of ruthenium and oxygen, thereby preventing interdiffusion between the absorbing film and the protective film in a subsequent heat treatment process, thereby preventing a decrease in the reflectivity of EUV light.
[0011] However, such an annealing treatment is also not a method for improving the flatness of the multilayer reflective film itself, and therefore there is a limit to how much the annealing treatment can improve the overall reflectivity of the reflective mask.
[0012] As described above, in manufacturing a reflective mask for use in EUV lithography, various heat treatment methods have been applied to improve the reflectivity. However, these methods do not affect the multilayer reflective film itself, and they also induce interdiffusion of elements constituting the multilayer reflective film, ultimately resulting in a problem that they do not contribute significantly to improving the reflectivity of the reflective mask.
[0013] Prior art documents (Patent Document 1) Japanese Patent Publication No. 2004-104118 (Patent Document 2) Japanese Patent Publication No. 2006-013280 (Patent Document 3) Japanese Patent Publication No. 2018-029498 Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention has been developed to solve such conventional problems, and has an object to provide a technology for manufacturing a reflective mask blank for use in EUV lithography, which can improve the flatness of a multilayer reflective film without inducing diffusion of elements on the interface of the multilayer reflective film by applying an electron beam annealing technology to the multilayer reflective film itself, thereby improving the reflectivity of the mask blank.
[0015] In particular, the electron beam annealing process heats not by replication or conduction but by the collision of electrons having kinetic energy, thereby enabling heat treatment limited to the surface layer where the electron beam collides, and has the advantage of preventing heat transfer to the underlying layer below the surface. As a result, the purpose is to enable heat treatment of the surface layer while preventing element diffusion in the underlying multilayer reflective film. [Means for solving the problem]
[0016] To achieve the above-mentioned object, one aspect of the present invention relates to a method for producing a reflective mask blank having a multilayer reflective film in which high refractive index layers and low refractive index layers are alternately and periodically stacked on a substrate to reflect extreme ultraviolet light (EUV light), and the multilayer reflective film can be subjected to an electron beam annealing treatment.
[0017] In this case, it is preferable that the multilayer reflective film has high refractive index layers / low refractive index layers, which are periodically laminated with Si / Mo, Si / Ru, Si / Nb, Be / Mo, Be / Nb, La / Nb, Si compound / Mo compound, Si / Mo / Ru, Si / Mo / Ru / Mo, or Si / Ru / Mo / Ru.
[0018] In addition, it is preferable that the electron beam annealing treatment is performed every time the high refractive index layer is laminated and / or every time the low refractive index layer is laminated.
[0019] It is preferable that the electron beam annealing treatment is performed when the high refractive index layer is laminated and each time a low refractive index layer is laminated.
[0020] Moreover, it is preferable that the electron beam annealing treatment is performed every 1 to 5 periods, where one period is composed of alternately laminating the high refractive index layers and the low refractive index layers.
[0021] In addition, it is preferable that the high refractive index layer is doped with one functional element selected from nitrogen (N), carbon (C), boron (B), oxygen (O), hydrogen (H), fluorine (F) and zirconium (Zr), and the electron beam annealing treatment is performed on the high refractive index layer doped with the functional element.
[0022] In addition, it is preferable that the low refractive index layer is doped with one functional element selected from nitrogen, carbon, boron, oxygen, hydrogen, fluorine, niobium, and zirconium, and the electron beam annealing treatment is performed on the low refractive index layer doped with the functional element.
[0023] The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The protective film is made of ruthenium (Ru) or a ruthenium alloy, and the protective film can be subjected to an electron beam annealing treatment.
[0024] The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The absorber film is made of tantalum (Ta) or a tantalum alloy, and the absorber film can be subjected to an electron beam annealing treatment.
[0025] In addition, a stress correction film for offsetting film stress caused by deposition of the multilayer reflective film is formed between the substrate and the multilayer reflective film, and this stress correction film can be subjected to electron beam annealing treatment.
[0026] Also, A defect propagation prevention film for preventing defects of the substrate from being propagated to the multilayer reflective film is formed between the substrate and the multilayer reflective film, and the defect propagation prevention film can be subjected to an electron beam annealing treatment.
[0027] Also, The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, A thermal diffusion barrier film may be formed between the multilayer reflective film and the protective film, and the thermal diffusion barrier film may be subjected to an electron beam annealing treatment.
[0028] On the other hand, the thermal diffusion preventing film is composed of 1) at least one metal selected from molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La), 2) a compound containing at least one selected from molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La) and at least one selected from oxygen (O), boron (B), nitrogen (N), carbon (C), fluorine (F), and silicon (Si), and 3) a compound containing at least one selected from carbon (C), oxygen (O), boron (B), nitrogen (N), fluorine (F), and silicon (Si), It is preferable that the material be one selected from the group consisting of:
[0029] The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The protective film is made of ruthenium (Ru) or a ruthenium alloy, the absorber film is made of tantalum (Ta) or a tantalum alloy, and a diffusion-inhibiting film containing ruthenium and oxygen is formed on the surface of the protective film on the side in contact with the absorber film as part of the protective film to prevent interdiffusion with the absorber film, and the diffusion-inhibiting film can be subjected to electron beam annealing treatment.
[0030] According to another aspect of the present invention, there is provided a reflective mask blank produced by the above-mentioned production method. Effect of the Invention
[0031] According to the present invention configured as described above, in the process of manufacturing a reflective mask blank including a multilayer reflective film that reflects extreme ultraviolet light, an electron beam annealing process is performed, which limits the thickness of the stacked multilayer reflective film to several to several tens of atomic layers without increasing the temperature of the substrate, and transmits the kinetic energy of electrons to more precisely planarize the atomic arrangement, thereby improving the reflectivity of the mask blank, as compared to existing heat treatment methods.
[0032] Furthermore, according to the present invention, by adding an electron beam annealing treatment not only to the multilayer reflective film of the reflective mask blank but also to various laminated films such as a protective film, an absorber film, a stress compensation film, a thermal diffusion prevention film, and a diffusion suppression film, the flatness of each layer is increased and / or a surface crystallization treatment is performed, thereby ultimately improving the reflectivity of the mask blank.
[0033] In this way, in place of the classical heat treatment method for manufacturing a reflective mask, a surface treatment method of irradiating an electron beam onto a multi-layer thin film material having high and low refractive indexes or a material constituting a reflective mask blank for improving its performance uses electrons to strike surface atoms and penetrate between stacked atoms, inducing vibration of the surface atoms' constituent material, thereby raising the surface temperature. This is fundamentally different in operation principle and functional role from an ion beam treatment method in which an ion beam having a weight similar to that of the atoms of the surface constituent material is irradiated to sputter and peel off the surface atoms and / or induce surface migration of the surface atoms. Therefore, the present invention has a technical feature of improving the reflectance of a reflective mask blank using such an electron beam annealing treatment technology. [Brief description of the drawings]
[0034] [Figure 1] 1 is a diagram showing a network environment of a body fluid management server according to an embodiment of the present invention. [Diagram 2] 1 is a block diagram showing the configuration of a body fluid management server according to a first embodiment of the present invention. [Diagram 3] FIG. 2 is a data flow diagram for a body fluid management method according to a first embodiment of the present invention. [Figure 4] FIG. 11 is a data flow diagram for a body fluid management method according to a second embodiment of the present invention. [Diagram 5] FIG. 11 is a block diagram showing the configuration of a body fluid management server according to a second embodiment of the present invention. [Figure 6] 1 is a diagram illustrating information sharing using a block chain network according to an embodiment of the present invention. [Figure 7] FIG. 11 is a block diagram showing the configuration of a body fluid management server according to a third embodiment of the present invention. [Figure 8] FIG. 11 is a data flow diagram for a body fluid management method according to a third embodiment of the present invention. [Figure 9] 1 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. [Figure 10]1 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. [Figure 11] 1 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. [Figure 12] 1 is a transmission electron microscope (TEM) photograph of a multi-layer reflective film stack state of a reflective mask blank (EUV Reticle: Mo / Si 80 Multi-layer) manufactured according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Hereinafter, the embodiments disclosed herein will be described in detail with reference to the accompanying drawings, and the same or similar components will be given the same reference numerals regardless of the drawing numerals, and duplicated descriptions thereof will be omitted. In addition, in describing the embodiments disclosed herein, if a detailed description of related known technology is determined to make the gist of the embodiments disclosed herein unclear, the detailed description will be omitted.
[0036] Terms including ordinal numbers such as first, second, etc. may be used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another.
[0037] A singular expression includes a plural expression unless the context clearly dictates otherwise.
[0038] In this application, the steps described may be performed in any order relative to the order listed, unless a specific causal relationship dictates that the steps be performed in the order listed.
[0039] In this application, the terms "comprise" or "have" and the like are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof set forth in the specification, but should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0040] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a reflective mask blank and a manufacturing method thereof according to an embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0041] FIG. 1 shows an ion beam sputtering apparatus for producing an EUV reflective mask blank related to the present invention.
[0042] The ion beam sputtering apparatus can be used to form a multilayer reflective film, which is a main component of a reflective mask blank. The ion beam sputtering apparatus 10 includes an ion source 12 for irradiating an ion beam into a vacuum chamber 11, a sputtering target support means 14, and a substrate support means 2. The sputtering target support means 14 is rotatably installed, and at least two sputtering targets 15, 16 for forming a multilayer reflective film are attached to both sides of the support means. The substrate support means 2 is installed with a substrate 1 facing the sputtering target surface, and is installed so that the substrate 1 can rotate at a constant speed with the center of the main surface of the substrate 1 as the rotation axis.
[0043] When forming a multilayer reflective film, inert gas ions 13 are generated from the sputtering ion source 12 and irradiated onto the sputtering targets 15 and 16. Atoms constituting the sputtering targets 15 and 16 are released from the target surfaces due to the collision of the inert gas ions, and the released target atoms 17 fly toward the substrate 1, which is charged with the opposite charge, and are deposited. When the first sputtering target 15 is deposited to a certain thickness, the sputtering target support means 14 is rotated and the same deposition operation is performed on the second sputtering target 16. By repeating this process, a multilayer reflective film composed of two elements is formed. For example, a multilayer reflective film in which a low refractive index layer, a molybdenum (Mo) layer, and a high refractive index layer, a silicon (Si) layer, are alternately stacked for about 40 periods can be formed and used as an EUV reflective film.
[0044] EUV reflective masks usually use 13.5 nm EUV light, and to increase the reflectance of this wavelength band, each layer of the multilayer reflective film must be deposited thinly, at just a few nm. The reflectance of the multilayer reflective film is one of the main factors in improving the integration level in the EUV lithography process. Therefore, the thin film deposition process must be very precise, and the surface flatness of each deposited layer must be excellent. However, EUV mask blanks deposited using ion beam sputtering equipment have limitations in improving the surface flatness of each layer, and the reflectance of currently commercialized reflective mask blanks does not exceed 70%.
[0045] As mentioned above, ion beam sputtering equipment uses strong electrical energy to bombard a target with an ion beam, which then detaches atoms from the target surface, and these detached atoms fly away with energy and are deposited on the surface of a substrate. This is a very rough process on a nano-scale, so even a target atomic layer formed to a thickness of a few nanometers will inevitably have low surface flatness immediately after deposition. Various methods are being researched to overcome the process limitations of ion beam sputtering equipment and improve the reflectivity of multilayer reflective films.
[0046] As a result of many years of research aimed at this goal, the present inventors have developed a method for improving the surface flatness of a multilayer reflective film by using an electron beam annealing process.
[0047] Electron beams are generated according to two principles. The first method is to generate electron beams by heating a metal filament inside an electron gun made of a cathode ray tube (CRT), generating thermal electrons, accelerating these thermal electrons at high speeds, and colliding them with a screen surface coated with phosphor to generate an electron beam. This method is capable of producing high-energy electron beams, but has the characteristic of a very narrow beam size. The second method is to extract electron particles in a plasma state, accelerate them, and then focus and emit them. This method can generate electron beams with a wide beam width by controlling the width and energy of the irradiated electron beam, and is used in a variety of industrial applications.
[0048] The present invention may use either one of these two types of electron beams, but in order to improve the uniformity of the electron beam annealing effect over the entire surface area of a substrate, it is preferable to use the plasma type electron beam.
[0049] FIG. 2 shows a simplified diagram of the electron beam generation principle of this plasma method.
[0050] In the plasma electron beam device 20, when an inert gas such as Ar is injected into the plasma chamber 21 and an RF power source is applied to the antenna 22 installed outside the plasma chamber 21, plasma is formed inside the plasma chamber 21, and electron particles from the plasma are emitted to the outside of the outlet through the beam width control unit 25 by the potential applied to the primary grid 23 and the secondary grid 24. At this time, the electron beams tend to diffuse radially due to the repulsive forces acting between each other in the space they fly through, so they are accumulated on the inner surface of the beam width control unit 25. As the electrons continue to accumulate on the inner surface of the beam width control unit 25 and the charge increases, the repulsive forces of the accumulated electrons are balanced above a certain critical value, and the electron beam advances in a direction parallel to the beam width control unit 25. As a result, an electron beam having a relatively wide beam width is irradiated onto the substrate 1 while moving in a relatively stable linear motion.
[0051] The present invention aims to improve the reflectivity of a multilayer reflective film by installing the above-mentioned ion beam sputtering device and electron beam annealing device together and performing an annealing process using the electron beam annealing device on the surface of the multilayer reflective film formed through the ion beam sputtering process.
[0052] FIG. 3 illustrates one embodiment of an ion beam sputtering system 10 and an electron beam annealing system 20 installed together in accordance with the present invention.
[0053] In the ion beam sputtering device 10, high energy inert gas ions (Ar) emitted from an ion source 12 are irradiated toward a sputtering target support means 14, whereby atoms of the sputtering target are emitted and deposited on a substrate 1, and this target is changed and repeated to form a multilayer reflective film 100 of a reflective mask blank. For example, a silicon (Si) target surface for forming a high refractive index layer is mounted on the sputtering target support means 14 so that the ion beam emitted from the ion source 12 faces the surface, and a high refractive index layer is formed on the multilayer reflective film 100. After the high refractive index layer is formed to a predetermined thickness of several nanometers, an electron beam emitted from an electron beam annealing device 20 is irradiated onto the surface of the high refractive index layer formed through the sputtering process. The electron beam rearranges silicon atoms on the surface of the nano-thick layer without increasing the temperature of the high refractive index layer, thereby increasing the surface flatness. The effect of the electron beam irradiation will be described in detail later with reference to FIG. 4.
[0054] The electron beam annealing process can cover the entire area of the multilayer reflective film in one irradiation process depending on the irradiation width of the electron beam, and if necessary, the electron beam can be irradiated in a linear form while the substrate 1 is moved back and forth linearly or rotated to perform the electron beam annealing sequentially from one side of the multilayer reflective film surface. At this time, it is preferable that the irradiation time of the electron beam is short, within a few seconds, so as not to increase the temperature of the multilayer reflective film, and the increase in thermal energy is limited to the surface atomic layer.
[0055] When the ion beam sputtering deposition process and the electron beam annealing process for the high refractive index layer are completed, the sputtering target support means 14 is rotated so that the surface of the molybdenum (Mo) target for forming the low refractive index layer provided on the opposite side faces the ion beam irradiated from the ion source 12, and a low refractive index layer is formed on the multilayer reflective film 100. After the low refractive index layer is formed to a predetermined thickness of several nanometers, an electron beam emitted from the electron beam annealing device 20 is irradiated onto the surface of the low refractive index layer formed through the sputtering process to perform an annealing operation.
[0056] A multilayer reflective film having excellent surface flatness is manufactured by the above-mentioned electron beam annealing treatment. In this embodiment, the electron beam annealing treatment is performed each time a high refractive index layer and a low refractive index layer are formed. However, according to another embodiment, the electron beam annealing treatment may be performed once every certain period (one period is the formation of one set of a high refractive index layer / a low refractive index layer), that is, after the multilayer reflective film is formed 3 to 5 times. In addition, since various types of layers such as a protective film, an absorbing film, a stress compensation film, a thermal diffusion prevention film, and a diffusion suppression film are additionally formed in the EUV reflective mask blank in addition to the multilayer reflective film, the electron beam annealing treatment is performed on each layer to contribute to improving the physical properties of the reflective mask blank. The method of performing the electron beam annealing on each layer will be described in detail below with reference to FIG. 8 to FIG. 11.
[0057] FIG. 4 is a schematic diagram illustrating the effect of an electron beam annealing process according to an embodiment of the present invention.
[0058] As shown in FIG. 4(a), a substrate 1 for multilayer reflective film deposition is provided. This substrate is 0±1.0×10 -7It is desirable for the material to have a low thermal expansion coefficient within the range of 100 / °C. Any of amorphous glass, ceramic, and metal can be used as a material having a low thermal expansion coefficient within this range. For example, SiO2-TiO2-based glass and quartz glass (Quartz) can be used as amorphous glass, alumina (Al2O3), beryllia (BeO), aluminum nitride (AIN) can be used as ceramic materials, and Invar alloy (Fe-Ni-based alloy) can be used as metal materials. Also, single crystal silicon substrates, sapphire substrates, diamond substrates, and the like can be used.
[0059] As shown in FIG. 4(b), a layer constituting the multilayer reflective film 100 is formed on the prepared substrate 1 by an ion beam sputtering device. This layer can be a high refractive index layer made of silicon (Si), a low refractive index layer made of molybdenum (Mo), or a set of high refractive index layer / low refractive index layer of one or more periods. As described above, when the multilayer reflective film 100 after the film formation is viewed on a nano-scale, not only is it amorphous because the target atoms are deposited through a forced collision process, but the film surface is also formed roughly at the atomic layer level, and there may be defects due to the formation of vacancies in which atoms are vacant inside the film. Such low surface flatness and defects are the main causes of the reduction in reflectance of the multilayer reflective film 100.
[0060] As shown in Fig. 4(c), when an electron beam is irradiated onto the formed multilayer reflective film 100, the atoms constituting the multilayer reflective film 100 receive the energy of the electron beam and undergo strong vibration due to heat, which rearranges the atoms and greatly improves the surface flatness. During this atomic rearrangement process, the surface of the formed layer may be crystallized by the electron beam, further improving the flatness. The atomic rearrangement process through electron beam irradiation is performed in a high vacuum atmosphere with a process pressure of E-4 or less, and when plasma is generated in the ion source using Ar gas, electrons accelerated at an acceleration voltage of several tens to several KeV are irradiated onto the surface of the multilayer reflective film, thereby performing surface flattening or atomic crystallization processing.
[0061] In this case, the energy of the electron beam irradiated to heat only the surface without increasing the temperature of the multilayer reflective film may be irradiated continuously for a short period of time, or a process having a rest period after irradiation for a certain period of time may be repeated, and the acceleration energy level may be varied according to a certain period of time and / or a certain level of energy may be irradiated repeatedly in a cyclic form.
[0062] The effect of electron beam annealing will be explained in detail using the surface planarization process of silicon, a high refractive index layer, as an example. When silicon (Si) is deposited by sputtering, the temperature is not high enough and the thermal energy does not reach the activation energy required for planarization, so the surface roughness is high and / or the layer grows into an amorphous layer. If new energy that can replace the thermal energy is supplied at this time, it increases the surface mobility of silicon particles on the substrate surface, so that the silicon particles can properly search for and stack vacant sites on the surface, reducing the surface roughness and inducing them to fill vacant sites inside the thin film. Meanwhile, an electron beam, which is generally a collection of countless accelerated electrons, is an individual particle with an extremely light weight. When it collides with the deposited thin film atoms, which are several thousand times heavier than itself, it transfers its momentum through almost inelastic collisions, generating heat in the thin film atoms, and creating atomic vibrations due to the heat, allowing the atoms to fill vacant sites.
[0063] In this way, the electron beam annealing process uses the kinetic energy of electrons having the above momentum as a means to substitute for the thermal energy shortage in the sputtering process. That is, electrons generated and accelerated in the electron beam source are provided onto the substrate and collide with silicon particles deposited on the substrate, thereby improving the mobility of the silicon particles.
[0064] In order to increase the reflectance of a multilayer reflective film, the interface between the high and low refractive index layers must be formed smoothly and clearly. When high energy is applied during the manufacturing process, the atoms constituting each layer are mutually diffused between the interfaces, making the boundary of the interface unclear, which is the main cause of the decrease in reflectance of the multilayer reflective film. However, the electron beam annealing process of the present invention controls the energy of the electron beam and the total time of irradiation with the electron beam (electron beam dose) to limit the penetration depth of the electron beam to the nanoscale, so that unnecessary energy is not transferred to other layers of the multilayer reflective film, and only the target film layer is selectively treated to achieve surface flattening. Since the reflective multilayer reflective film is composed of about 40 periods of high and low refractive index layers of several nanometers each, there are many interfaces at nanoscale intervals, and the electron beam irradiation according to the present invention can be the most effective method for heat-treating only the target interface without affecting other interfaces.
[0065] Currently, the heat treatment methods used in the semiconductor thin film manufacturing process include the furnace method, which heats the entire substrate in a heating furnace, the RTA (Rapid Thermal Annealing) method, which uses IR heat transfer, the excimer laser method, which uses laser, and the microwave method, which heats the substrate using microwaves. The furnace method is the cheapest, but has problems with particle generation and surface contamination during the process, the RTA method has a fast heat treatment speed but is difficult to uniformly heat treat the entire substrate, the excimer laser method requires the use of expensive laser scanning equipment, and the microwave method has problems with localized heating due to electric field concentration. Compared to these existing heat treatment methods, the electron beam annealing process of the present invention can be said to be the most effective heat treatment process, as it can heat treat only the desired interface on a nanoscale and does not cause problems such as particle generation or localized heating.
[0066] FIG. 5(a) shows the results of measuring the roughness of a surface on which a Si layer was deposited by ion beam sputtering, and FIG. 5(b) shows the results of measuring the surface roughness of the test piece of (a) after irradiating the Si surface of the test piece according to the present invention with an electron beam (electron beam energy: 3 keV, irradiation for 10 seconds). This was measured using an alpha step with a resolution capable of measuring roughness on an atomic scale, and the surface roughness R of (a) when only deposition was performed by ion beam sputtering was 1.2 mm. a The surface roughness R of the Si deposition layer (b) was 0.57 to 0.59 nm. b is 0.45~0.46nm. This means that when an electron beam with 3keV energy collides with a silicon surface, the electron beam, which has a different mass from the silicon atoms, collides inelastically with the silicon surface atoms with a kinetic energy of 3keV, and the energy transferred heats the silicon atoms, and the atoms in the silicon deposition layer close to the surface vibrate strongly due to the heat, and the silicon atoms located on the surface improve their surface mobility due to this vibration.
[0067] As a result, the vacancies inside the Si deposition layer on the surface side are filled, as shown in Figure 4, and the aligned surface atomic layer creates a smoother surface with lower roughness. In this way, if the surface roughness is reduced by irradiating the upper surface of the Si deposition layer with an electron beam, and then a low refractive index Mo layer is deposited by ion beam sputtering, a Si / Mo interface with smooth roughness is formed. In addition, if an electron beam is irradiated onto the Mo surface in the same way, a Si / Mo interface with smooth roughness is also created.
[0068] 6 and 7 show the layout structure of a reflective mask blank manufacturing means (ion beam sputtering means) and an electron beam annealing means according to one embodiment of the present invention.
[0069] As shown in FIG. 6(a), the reflective mask blank manufacturing means 10 and the electron beam annealing means 20 can be arranged in one chamber 5. The apparatus described with reference to FIG. 3 corresponds to this embodiment. This is the most compact arrangement, and since it is possible to perform not only the ion beam sputtering process for manufacturing a multilayer reflective film, which is a manufacturing process of a reflective mask blank, but also the electron beam annealing process for the surface of the laminated reflective film without a substrate transfer process in one chamber, it is possible to manufacture a reflective mask blank most quickly. However, in this arrangement, since the process conditions for ion beam sputtering and the electron beam annealing process conditions must be quickly changed back and forth in one chamber, not only is process control difficult, but particles generated in the ion beam sputtering process may cause surface contamination in the electron beam annealing process.
[0070] As shown in FIG. 6(b), the reflective mask blank manufacturing means 10 and the electron beam annealing means 20 may be installed independently in two different chambers 5 and 6, and the chambers 5 and 6 may be connected to each other through a transfer port 7 equipped with a gate valve. According to this arrangement, after the ion beam sputtering process for manufacturing a multilayer reflective film of the reflective mask blank is completed in the first chamber 5, the substrate on which the reflective film is laminated is transferred to the second chamber 6 through the transfer port 7 by a separate transfer means, and the electron beam annealing process is performed on the laminated reflective film. According to this arrangement, since the ion beam sputtering process and the electron beam annealing process are performed in separate independent chambers 5 and 6, it is not necessary to change the process conditions in each chamber at any time, and it is possible to prevent deterioration of the physical properties of the reflective mask blank due to the mutual interference between the two process environments or results. However, this arrangement has problems in that a separate transfer device must be additionally installed, which increases the manufacturing cost, and the manufacturing time is increased since the substrate must be transferred between the two chambers 5 and 6 several times during the manufacturing process of the reflective mask blank.
[0071] FIG. 7 shows a configuration in which, in a structure in which a reflective mask blank manufacturing means 10 and an electron beam annealing means 20 are arranged in one chamber 5 as in FIG. 6(a), a sputtering means 30 is installed separately in a chamber 6.
[0072] The process pressure of the reflective mask blank manufacturing means 10 and the electron beam annealing means 20 is 10 -4 Torr, whereas the process pressure of the sputtering means 30 is 10 -3 Torr is even higher. Therefore, if the sputtering means 30 is installed in the same chamber as the reflective mask blank manufacturing means 10 or the electron beam annealing means 20, the process efficiency will decrease due to the difference in process conditions. Therefore, it is preferable that the other two chambers 5 and 6 are arranged to be interconnected through a transfer port 7 equipped with a gate valve, and that the reflective mask blank manufacturing means 10 and the electron beam annealing means 20, which have similar process conditions, are installed in the first chamber 5, and the sputtering means 30 is installed in the second chamber 6.
[0073] As described above, the reflective mask blank not only includes a multilayer reflective film in which high refractive index layers and low refractive index layers are alternately laminated, but also basically includes an absorber film that absorbs extreme ultraviolet rays and is laminated on a protective film that is laminated on the top layer of the multilayer reflective film to protect the multilayer reflective film in a subsequent etching process, etc., and, if necessary, various functional films are additionally laminated to improve the physical properties of the reflective mask blank, such as a stress compensation film and a thermal diffusion prevention film.
[0074] These protective films, absorber films, and various functional films can be manufactured by the ion beam sputtering apparatus used to form a multilayer reflective film in the reflective mask blank manufacturing means 10. In this case, as explained above with reference to Figures 6(a) and (b), the reflective mask blank can be manufactured without a separate sputtering means 30.
[0075] Recently, in order to improve the manufacturing productivity of reflective mask blanks, an arrangement structure as shown in Fig. 7 has been used in which the protective film, absorber film, and various functional films are manufactured by a sputtering means 30 provided separately from the ion beam sputtering device for manufacturing the multilayer reflective film. The sputtering means 30 can be one of various sputtering means currently available commercially, such as DC sputtering, RF sputtering, reactive sputtering, and magnetron sputtering.
[0076] The various arrangements of the reflective mask blank manufacturing means 10, the electron beam annealing means 30, and the sputtering means 30 described with reference to Figures 6 and 7 provide various options in the manufacturing process, so that the most efficient arrangement can be selected in accordance with the required physical properties of the reflective mask blank at the manufacturing site.
[0077] In the following, reflective mask blanks having various laminated structures produced by the reflective mask blank manufacturing method according to the present invention explained so far will be described.
[0078] First, FIG. 8 shows the basic layered structure of the reflective mask blank 100, in which a multilayer reflective film 120 in which high refractive index layers / low refractive index layers are alternately layered in 40 cycles on a substrate 110, a protective film 130 that is layered on the multilayer reflective film 120 and protects the multilayer reflective film 120 in a subsequent dry etching process, and an absorber film 140 that is layered on the protective film 130 and patterned into a specific semiconductor pattern shape in a subsequent dry etching process, and then absorbs EUV light in an EUV irradiation process.
[0079] Among these, the multilayer reflective film 120 is the most important component that determines the reflectance of the reflective mask blank, and the flatness of the interfaces between the 40 periods of high refractive index layers and low refractive index layers that make up the multilayer reflective film 120 determines the overall reflectance of the mask blank.
[0080] This multilayer reflective film 120 can reflect light of a specific wavelength through a structure in which materials with different refractive indices are alternately laminated. For example, a Si / Mo periodic multilayer reflective film can be produced in which Si and Mo are alternately laminated for about 40 periods, which has a high reflectivity for EUV light of 13 to 14 nm. In the case of a Si / Mo multilayer reflective film, the layer with a relatively low refractive index can be Mo, and the layer with a relatively high refractive index can be Si. The material forming the multilayer reflective film is appropriately selected depending on the wavelength of the exposure light to be used.
[0081] Other examples of multilayer reflective films used in the EUV light region include Si / Ru, Si / Nb, Be / Mo, La / Nb periodic multilayer reflective films, Si compound / Mo compound periodic multilayer reflective films, Si / Mo / Ru periodic multilayer reflective films, Si / Mo / Ru / Mo periodic reflective films, etc. Multilayer reflective film-attached substrates having these multilayer reflective films formed thereon are used as, for example, EUV reflective mask blanks or multilayer reflective film mirrors in EUV lithography systems.
[0082] According to an embodiment of the present invention, an electron beam annealing process is performed during the lamination process of the multilayer reflective film 120 to improve the flatness of the interface of the multilayer reflective film. More specifically, the electron beam annealing process may be performed every time a high refractive index layer is laminated, and / or every time a low refractive index layer is laminated, and / or every time a high refractive index layer is laminated and every time a low refractive index layer is laminated. In addition, the electron beam annealing process may be configured to be performed every 1 to 5 periods, where alternating lamination of the high refractive index layer / low refractive index layer is one period.
[0083] When the interface between the high refractive index layer and / or the low refractive index layer is subjected to an electron beam annealing treatment, the target atoms that were unevenly and amorphously stacked at the interface are rearranged, thereby increasing the flatness of the interface, as described above with reference to FIG. 4, and for more details, please refer to the same.
[0084] For example, after the lamination process of the multilayer reflective film is completed, if it is determined that the flatness of the upper outer surface of the Si layer, which is a high refractive index layer, is low as a result of measuring the reflectance together with a cross-sectional inspection using a transmission electron microscope (TEM), an electron beam annealing process can be performed every time a Si layer, which is a high refractive index layer, is laminated in a future manufacturing process. Conversely, if it is determined that the flatness of the upper outer surface of the Mo layer, which is a low refractive index layer, is low, an electron beam annealing process can be performed every time a Mo layer, which is a low refractive index layer, is laminated in a future manufacturing process. If necessary, an electron beam annealing process can be performed every time a Si layer, which is a high refractive index layer, and a Mo layer, which is a low refractive index layer, are laminated. Such a difference in the flatness of the surfaces of the high refractive index layer and / or the low refractive index layer may occur due to the purity of the target to be deposited, the difference in manufacturing process conditions, etc.
[0085] Although the electron beam annealing process can improve the interface flatness of the multilayer reflective film and contribute to improving the reflectivity, frequent electron beam annealing can increase manufacturing costs. In particular, in the configuration shown in FIG. 6(b) in which the electron beam annealing means 20 is installed in a separate second chamber 6 and the multilayer reflective film substrate must be transferred every time the electron beam annealing process is performed, not only does the cost increase but additional process problems may occur. It is preferable to experimentally determine at what point in the multilayer reflective film process the electron beam annealing process should be performed, making a trade-off between the advantages and disadvantages of the electron beam annealing process.
[0086] According to another embodiment of the present invention, the high refractive index layer is doped with one functional element selected from nitrogen, carbon, boron, oxygen, hydrogen, fluorine, and zirconium, and the electron beam annealing treatment can be performed on the high refractive index layer doped with the functional element.
[0087] The functional element is doped into the surface of the high refractive index layer to relieve the film stress of the film material forming the high refractive index layer and suppress the interdiffusion of the film material, thereby increasing the flatness of the surface and improving the reflectance. In addition, the functional element reduces the roughness of the surface of the high refractive index layer due to its fine crystal size, ultimately increasing the flatness of the surface and improving the reflectance of the film material.
[0088] The doping process of the functional element is performed by supplying a specific gas containing the functional element to the chamber in which the process is performed during the ion beam sputtering process of the elements constituting the high refractive index layer, and / or supplying it together with argon gas to the gas supply unit of the ion beam source, and the functional element is adsorbed and / or chemically bonded to the atoms of the high refractive index layer by the action of this supply gas. Meanwhile, in the case of a metal material such as zirconium among the functional elements, the sputtering target itself can be made by mixing the elements, and the sputtered mixture can be deposited by ion beam sputtering. The gas used in this embodiment is a gas of an element or compound having two or more single electrons in the atomic state, that is, a gas other than rare gas, halogen, and hydrogen, and can be used as a single element or a compound. Specifically, in addition to single elements such as oxygen and nitrogen, gases of hydrocarbons such as CH4 and C2H6, alcohols, ethers, ammonia, and silanes can be used.
[0089] If such a gas is to be supplied to the surface of the multilayer reflective film, the simplest method is, for example, to supply the raw material of the high refractive index layer constituting the multilayer reflective film, form the high refractive index layer on the substrate, and then introduce an activated gas into the chamber to adsorb the substance contained in the gas onto the surface of the high refractive index layer. Of course, various surface treatment methods can be used in addition to the above. For example, as already mentioned above, in the case of a metal material such as zirconium among the functional elements, it is possible to perform a doping treatment on the surface of the high refractive index layer using an ion beam sputtering device.
[0090] In this way, when the electron beam annealing process according to the present invention is performed after the functional element is adsorbed or co-sputtered on the high refractive index layer of the multilayer reflective film, the flatness of the film surface can be further increased, contributing to improved reflectivity. This is believed to be because the kinetic energy of the elements of the film material that becomes the high refractive index layer and the functional element is increased by the inelastic collision of electrons during the electron beam annealing process, and they move relative to each other, reducing the surface roughness that occurs during a separate doping process such as the deposition or implantation of the functional element, making the surface more dense.
[0091] In the same manner, the low refractive index layer may be doped with one functional element selected from nitrogen, carbon, boron, oxygen, hydrogen, fluorine, and zirconium, and the electron beam annealing treatment may be performed on the low refractive index layer doped with the functional element. In this manner, the adsorption or co-sputtering deposition treatment of the functional element on the low refractive index layer may be performed in the same manner as the treatment on the surface of the high refractive index layer described above. As a result, the functional element doped on the surface of the low refractive index layer relieves the surface stress of the deposition material, suppresses mutual diffusion, and reduces the surface roughness of the low refractive index layer, thereby increasing the ultimate surface flatness and improving the reflectance of the deposition material, which is the same as the action and effect of the functional element on the high refractive index layer described above.
[0092] In this way, when the electron beam annealing process according to the present invention is performed after the functional element is adsorbed or co-sputtered onto the surface of the low refractive index layer of the multilayer reflective film, the flatness of the film surface can be further increased, contributing to improved reflectivity. This is believed to be because, as in the case of the high refractive index layer described above, the kinetic energy of the elements of the film material constituting the low refractive index layer and the functional element increases due to inelastic collision of electrons during the electron beam annealing process, and they move relative to each other, reducing the surface roughness generated during the doping process and making the surface more dense.
[0093] Meanwhile, the protective film 130 is laminated on the multilayer reflective film 120 to protect the multilayer reflective film 120 from dry etching and cleaning in the manufacturing process of the reflective mask. The protective film 120 also functions to protect the multilayer reflective film 120 when repairing defects in the mask pattern. The protective film 130 may be formed in one layer or in multiple layers of two or more layers as required.
[0094] The protective film 130 is generally formed of a material containing ruthenium (Ru) as a main component. Examples of materials containing ruthenium as a main component include ruthenium metal alone, ruthenium titanium (Ti), niobium (Nb), molybdenum (Mo), zirconium (Zr), yttrium (Y), boron (B), lanthanum (La), cobalt (Co), and rhenium (Re), and ruthenium alloys containing at least one metal selected from these materials, and nitrogen. Among these, if a ruthenium alloy material containing titanium is used, the phenomenon of silicon diffusing from the surface of the multilayer reflective film 120 to the protective film 130 can be reduced when the element forming the high refractive index layer of the multilayer reflective film 130 is silicon (Si).
[0095] According to an embodiment of the present invention, an electron beam annealing process may be performed after the protective film 130 is deposited. Since defects in the protective film 130 directly affect the reduction in reflectance of the multilayer reflective film 120 to EUV light, it is necessary to eliminate surface defects in the protective film 130 and improve the surface flatness and surface roughness through the electron beam annealing process. Such improvement in the surface flatness of the protective film 130 may also bring about effects such as improved exposure efficiency of EUV light and improved throughput.
[0096] Meanwhile, the absorber film 140 is laminated on the protective film 130 and functions to absorb EUV light, and / or absorb part of EUV light and reflect the other part to shift the phase of the reflected light. For this reason, the absorber film 140 is sometimes called a phase shift film. The phase shift function is that if the phase difference between the light reflected through the absorber film 140 in the region where the absorber film 140 is formed and the light reflected through the multilayer reflective film 120 in the region where the absorber film 140 is not formed is adjusted to about 170 to 190 degrees, interference occurs between the reflected lights with a phase difference of about 180 degrees, improving the image contrast of the projected optical image. Such improvement in image contrast can increase various latitudes related to exposure, such as latitude in exposure amount and latitude in focus.
[0097] The absorber film 140 is formed of a material that has an absorbing function for EUV light and can be processed by etching or the like (preferably dry etching with chlorine (Cl) or fluorine (F)-based gas). As a material having such a function, a tantalum (Ta) alloy alone or a tantalum alloy containing tantalum as a main component is used. As the tantalum alloy, a compound containing tantalum and boron, a compound containing tantalum and nitrogen, a compound containing tantalum, oxygen, and nitrogen, a compound containing tantalum, boron, and at least one of oxygen and nitrogen, a compound containing tantalum and silicon, a compound containing tantalum, silicon, and nitrogen, a compound containing tantalum, germanium, and a compound containing tantalum, germanium, and nitrogen, and the like can be used. As a material constituting the absorber film 140, in addition to tantalum or a tantalum compound, materials such as chromium, CrN, CrCON, CrCO, CrCOH, and CrCONH, chromium compounds, WN, TiN, and Ti can be used.
[0098] According to an embodiment of the present invention, an electron beam annealing process may be performed after stacking the absorber film 140. Since surface defects of the absorber film 140 cause problems such as a decrease in reflectance of the multilayer reflective film 120 against EUV light and a decrease in image contrast, it is necessary to eliminate the surface defects of the absorber film 140, improve the surface roughness and surface flatness, and / or induce surface crystallization through the electron beam annealing process.
[0099] 9 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. This reflective mask blank 100 is basically the same as that shown in FIG. The device is composed of a substrate 110, a multilayer reflective film 120, a protective film 130, and an absorber film 140, and a stress compensation film (buffer layer) 150 is additionally deposited between the substrate 110 and the multilayer reflective film 120. The basic film formation has been described in detail with reference to FIG. 8, so please refer to this.
[0100] Since this embodiment is an example in which a stress correction film 150 is additionally fixed to the laminated structure of the basic reflective mask blank, the stress correction film 150 will be mainly described.
[0101] The stress compensation film 150 is selected from those having a stress in the opposite direction to the stress of the multilayer reflective film 120. In general, the multilayer reflective film 120 is densely formed and has compressive stress, so the stress compensation film 150 is selected from those having tensile stress. In this way, the stress compensation film 150 offsets the film stress of the multilayer reflective film 120, thereby preventing the multilayer reflective film 120 from warping due to excessive compressive stress and causing wafer transfer errors in subsequent processes.
[0102] For this reason, the stress correction film 150 is selected so that the magnitude (size, absolute value) of the stress of the stress correction film 150 is increased by the heat treatment. More specifically, the stress is shifted more toward the tensile stress side. In addition, it is desirable to use a film with high flatness for the stress correction film 150. The surface roughness indicating the surface flatness of the stress correction film 150 is preferably 0.2 nm or less, and more preferably 0.15 nm or less.
[0103] The material of the stress correction film 150 may be a material mainly composed of tantalum (Ta). Examples of materials mainly composed of tantalum include tantalum alloys. Furthermore, amorphous materials mainly composed of tantalum are preferable. Examples of such materials include alloys containing tantalum and boron, such as tantalum boride (TaB) and tantalum boride alloy nitride (TaBN). In addition, the stress correction film 150 may be a material mainly composed of silicon (Si) or a material mainly composed of chromium (Cr).
[0104] In the case of the tantalum boride alloy, it can be formed on a substrate at room temperature in an argon gas atmosphere using magnetron sputtering. In this case, the stress changes from the compressive stress side to the tensile stress side by increasing the gas pressure, so that the stress control can be precisely adjusted by changing the sputtering gas pressure under a constant input power. In order to obtain a good amorphous state, the alloy film containing tantalum and boron preferably has a boron content of 10 to 30 at%.
[0105] According to an embodiment of the present invention, the stress compensation film 150 having a film stress in the opposite direction to the film stress of the multilayer reflective film is formed between the substrate 110 and the multilayer reflective film 120, and the electron beam annealing process can be performed on the stress compensation film 150. The electron beam annealing process not only improves the flatness of the surface of the stress compensation film 150, but also has a local heat treatment effect, so that the film stress of the stress compensation film 150 can be precisely controlled through the above-mentioned gas pressure control as well as the electron beam annealing control. Any stress can be removed by heating through the electron beam annealing, so that the irradiation of the electron beam can be appropriately adjusted to relieve excessive stress. The warping phenomenon of the multilayer reflective film 120 deposited on the thus adjusted stress compensation film 150 is prevented in advance, improving the precision of the mask.
[0106] Meanwhile, a defect propagation preventing film 151 may be formed between the substrate 110 and the multilayer reflective film 120. The defect propagation preventing film 151 is preferably made of the same material as the substrate, and silicon oxide may be used as an example. The defect propagation preventing film 151 is configured to be deposited in several to several tens of atomic layers.
[0107] According to an embodiment of the present invention, an electron beam annealing process can be performed on the defect propagation preventing film 151. The electron beam annealing process can be performed simultaneously with and / or after the deposition of the defect propagation preventing film 151. The electron beam annealing fills and / or flattens vacancies or defects such as peeled off layers of several atoms on the surface of the substrate, so that the structure of the substrate defects is not continuously propagated to the multilayer reflective film.
[0108] In particular, in the case of a substrate containing quartz, defects present on the surface continue to exist until the deposition of the multilayer reflective film, causing fatal defects in the reflective mask blank. The presence of defects such as vacancies on the surface of the substrate or defects several to several tens of atomic layers away is the most important factor that determines the defects of the reflective mask blank. Therefore, if the defect propagation preventing film 151 is deposited to a low thickness of several tens of atomic layers or less in order to prevent the propagation of substrate defects and then irradiated with electron beams according to the present invention, the atoms of the defect propagation preventing film 151 that have sufficient mobility due to the energy transfer of the electron beam will perform surface migration to fill the defects and perform the planarization process by themselves. The electron beam annealing process for the defect propagation preventing film 151 for removing such defects is a very important factor that can affect the quality and mass productivity.
[0109] Meanwhile, Fig. 10 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. As shown in Fig. 8, this reflective mask blank 100 is basically composed of a substrate 110, a multilayer reflective film 120, a protective film 130, and an absorber film 140, and a thermal diffusion barrier film 160 is additionally deposited between the substrate 110 and the protective film 130. The basic film formation has been described in detail with reference to Fig. 8, so please refer to this.
[0110] Since this embodiment is an example in which a thermal diffusion preventing film 160 is additionally fixed to a laminated structure of a basic reflective mask blank, the thermal diffusion preventing film 160 will be mainly described.
[0111] This thermal diffusion preventing film 160 is deposited between the protective film 130 made of ruthenium or a ruthenium alloy and the multilayer reflective film 120. This makes it possible to suppress the formation of a diffusion layer between the protective film 130 and the topmost Si film of the multilayer reflective film 120 during the formation of the protective film 130 or during subsequent heat treatments (e.g., heat treatments for reducing stress in the multilayer reflective film, pre-baking treatments of the resist film, exposure, cleaning, etc.), and to prevent a decrease in reflectance due to the diffusion layer.
[0112] By providing the thermal diffusion prevention film 160, not only can a high reflectance be obtained, but also the reflectance is not decreased by the subsequent heat treatment, so that the reflecting area of the reflective mask can maintain a high reflectance. The thermal diffusion prevention film 160 is preferably made of a material having a refractive index (n) greater than 0.90 and an offset coefficient (k) less than -0.020. Such a material contributes to improving the optical characteristics (reflectance) and at the same time has the effect of suppressing the formation of the diffusion layer described above.
[0113] The material forming this thermal diffusion prevention film 160 is desirably one material selected from the group including: 1) at least one metal selected from molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La); 2) a compound containing at least one selected from molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La) and at least one selected from oxygen (O), boron (B), nitrogen (N), carbon (C), fluorine (F), and silicon (Si); and 3) a compound containing carbon (C) or carbon (C) and at least one selected from oxygen (O), boron (B), nitrogen (N), fluorine (F), and silicon (Si).
[0114] As representative materials belonging to the first and second groups, compounds such as Mo2C, MoC, MoSi2, NbN, ZrC, ZrN, ZrO2, Y2O3, La2O3, LaB6, TiC, TiN, TiO2, and any one of molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La) can be used. Representative materials belonging to the third group include compounds such as SiO2, SiON, BN, and Si3N4.
[0115] According to an embodiment of the present invention, an electron beam annealing process may be performed on the thermal diffusion preventing film 160 formed between the multilayer reflective film 120 and the protective film 130. This not only increases the surface roughness of the thermal diffusion preventing film 160 itself to increase the transmittance of EUV light, thereby minimizing the loss of EUV light that does not reach the multilayer reflective film 120, but also more effectively prevents surface diffusion of the top layer of the multilayer reflective film 120 by the thermal diffusion preventing film 160, thereby increasing the surface flatness of the multilayer reflective film 120 and ultimately improving the reflectance of the multilayer reflective film 120.
[0116] Meanwhile, Fig. 11 is a diagram showing a layered structure of a reflective mask blank manufactured according to another embodiment of the present invention. As shown in Fig. 8, this reflective mask blank 100 is basically composed of a substrate 110, a multilayer reflective film 120, a protective film 130, and an absorber film 140, and a diffusion suppression film 170 is additionally deposited between the protective film 130 and the absorber film 140. The basic film formation has been described in detail with reference to Fig. 8, so please refer to this.
[0117] Since this embodiment is an example in which a diffusion suppressing film 170 is additionally fixed to the laminated structure of the basic reflective mask blank, the following description will be centered on this diffusion suppressing film 170.
[0118] The protective film 130 is made of ruthenium or a ruthenium alloy, and the absorber film 140 is made of tantalum or a tantalum alloy. A diffusion suppression film 170 containing ruthenium and oxygen is formed on the surface of the protective film on the side in contact with the absorber film as part of the protective film to prevent interdiffusion with the absorber film.
[0119] This diffusion-preventing film 170 can suppress the occurrence of mutual diffusion due to thermal diffusion between the ruthenium-based protective film 130 of the reflective mask and the adjacent absorber film 140 when the exposure light source of the EUV exposure machine is made high-powered, thereby suppressing fluctuations in the reflectance for EUV light. In other words, the diffusion-preventing film 170 can prevent a decrease in the reflectance of EUV light by suppressing mutual diffusion due to thermal diffusion between the protective film 130 and the absorber film 140 even in an operating environment where the exposure light source of the EUV exposure machine is high-powered.
[0120] The diffusion suppression film 170 is formed of a material containing ruthenium (Ru) and oxygen (O), and may also contain nitrogen and hydrogen. Ruthenium may be a simple ruthenium metal or a ruthenium alloy. For example, when the protective film 130 is ruthenium, the material of the diffusion suppression film 170 may be RuO, RuON, or the like. When the protective film 130 is a Ru alloy (e.g., RuNb), the material of the diffusion suppression film 170 may be RuNbO, RuNbON, or the like. In terms of reflectance to EUV light, the ratio (atomic %) of ruthenium to oxygen in the diffusion suppression film 170 may be 0.8 to 2.2, preferably 1.0 to 2.0, when ruthenium is taken as 1.
[0121] Such a diffusion suppression film 170 can be produced by a sputtering method (ion beam sputtering, DC sputtering, RF sputtering), or can be produced by annealing the surface of the ruthenium-based protective film 130 in air, oxygen, or ozone gas atmosphere. When stacking by the sputtering method, the diffusion suppression film 170 is newly stacked on the ruthenium-based protective film 130 (the film thickness increases), but when the surface of the ruthenium-based protective film 130 is annealed, a part of the ruthenium-based protective film 130 (the side in contact with the absorber film 140) has the function of the diffusion suppression film 170 without increasing the thickness of the entire film.
[0122] According to an embodiment of the present invention, an electron beam annealing process may be performed on the diffusion-preventing film 170 formed between the protective film 130 and the absorber film 140. This increases the surface roughness of the diffusion-preventing film 170 itself and enhances the transmittance of EUV light, thereby minimizing the loss of EUV light that does not reach the multilayer reflective film 120, and also more effectively prevents surface diffusion of the protective film 130 by the diffusion-preventing film 170, ultimately improving the reflectance of the multilayer reflective film 120.
[0123] Finally, Figure 12 is a transmission electron microscope (TEM) photograph of a multilayer reflective film formed with 40 periods of Mo / Si, which was manufactured through ion beam sputtering and electron beam annealing according to the present invention. In order to more accurately check the interface, the multilayer reflective film manufactured with a total thickness of 280 nm was divided into an upper portion and a lower portion at a thickness of 190 nm and enlarged. As a result, it was confirmed that the flatness of the Mo / Si interface and the Si / Mo interface was excellent.
[0124] The interface roughness of Mo / Si interface and Si / Mo interface is an important factor that determines the reflectance of EUV light of multilayer reflective film, and the flatness and roughness of the interface vary depending on the interdiffusion between Mo-Si, the deposition process and conditions, the method of processing each interface, and the foreign atoms added to each interface. By irradiating such interfaces with electron beam for a short time to prevent the interface diffusion between them due to the temperature rise, the energy is transferred only to the top surface atoms of the deposited film without inducing the temperature rise in the whole multilayer reflective film, and if the energy is transferred only to the top part of the atomic layer, the mobility of the surface atoms is improved, and the surface roughness can be improved. Therefore, electron beam irradiation can provide temperature only to the selective surface, and can be a useful method to improve the interface roughness.
[0125] The technical features disclosed in each embodiment of the present invention are not limited to the corresponding embodiment, and as long as they are not mutually incompatible, the technical features disclosed in each embodiment may be combined and applied to different embodiments.
[0126] Therefore, although each embodiment will be described focusing on its respective technical features, as long as the technical features are not mutually exclusive, they can be combined and applied.
[0127] The present invention is not limited to the above-described embodiments and the accompanying drawings, and various modifications and variations are possible from the viewpoint of those having ordinary skill in the art to which the present invention pertains. Therefore, the scope of the present invention should be determined not only by the claims of this specification, but also by equivalents to the claims. [Explanation of symbols]
[0128] 1: Substrate 10: Reflective mask blank manufacturing method 20: Electron beam annealing means 30: Sputtering means 100: Reflective mask blank 110: Substrate 120: Multilayer reflective film 130:Protective film 140: Absorbing membrane 150: Stress compensation film 151: Defect propagation prevention film 160: Heat diffusion prevention film 170: Diffusion-suppressing membrane
Claims
1. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: The multilayer reflective film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
2. 10. The method of claim 1 , The multilayer reflective film is characterized in that the high refractive index layer / low refractive index layer are periodically laminated with Si / Mo, Si / Ru, Si / Nb, Be / Mo, Be / Nb, La / Nb, Si compound / Mo compound, Si / Mo / Ru, Si / Mo / Ru / Mo, and Si / Ru / Mo / Ru. A method for manufacturing a reflective mask blank.
3. 10. The method of claim 1 , The electron beam annealing treatment is performed every time the high refractive index layer is laminated. A method for manufacturing a reflective mask blank.
4. 10. The method of claim 1 , The electron beam annealing treatment is performed every time the low refractive index layer is laminated. A method for manufacturing a reflective mask blank.
5. 10. The method of claim 1 , The electron beam annealing treatment is performed when depositing the high refractive index layer, This is performed each time a low refractive index layer is laminated. A method for manufacturing a reflective mask blank.
6. 10. The method of claim 1 , The electron beam annealing treatment is performed every 1 to 5 periods when the high refractive index layer / low refractive index layer are alternately laminated to form one period. A method for manufacturing a reflective mask blank.
7. 10. The method of claim 1 , The high refractive index layer is doped with one functional element selected from nitrogen, carbon, boron, oxygen, hydrogen, fluorine, and zirconium, and the electron beam annealing treatment is performed on the high refractive index layer doped with the functional element. A method for manufacturing a reflective mask blank.
8. 10. The method of claim 1 , The low refractive index layer is doped with one functional element selected from nitrogen, carbon, boron, oxygen, hydrogen, fluorine, niobium, and zirconium, and the electron beam annealing treatment is performed on the low refractive index layer doped with the functional element. A method for manufacturing a reflective mask blank.
9. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The protective film is made of ruthenium (Ru) or a ruthenium alloy, and the protective film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
10. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The absorber film is made of tantalum (Ta) or a tantalum alloy, and the absorber film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
11. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: a stress correction film for offsetting a film stress caused by deposition of the multilayer reflective film is formed between the substrate and the multilayer reflective film, and the stress correction film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
12. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: a defect propagation prevention film is formed between the substrate and the multilayer reflective film to prevent defects of the substrate from being propagated to the multilayer reflective film, and the defect propagation prevention film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
13. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, a thermal diffusion preventing film is formed between the multilayer reflective film and the protective film, and the thermal diffusion preventing film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
14. 14. The method of claim 13, The thermal diffusion preventing film is 1) at least one metal selected from the group consisting of molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La); 2) a compound containing at least one selected from molybdenum (Mo), niobium (Nb), zirconium (Zr), yttrium (Y), titanium (Ti), and lanthanum (La), and at least one selected from oxygen (O), boron (B), nitrogen (N), carbon (C), fluorine (F), and silicon (Si); 3) a compound containing at least one selected from carbon (C), oxygen (O), boron (B), nitrogen (N), fluorine (F), and silicon (Si); The present invention is characterized in that the material is made of one material selected from the group including A method for manufacturing a reflective mask blank.
15. A method for producing a reflective mask blank having a multilayer reflective film that reflects extreme ultraviolet light (EUV light) and in which high refractive index layers and low refractive index layers are alternately and periodically laminated on a substrate, comprising the steps of: The multilayer reflective film further includes a protective film laminated on the multilayer reflective film to protect the multilayer reflective film, and an absorber film laminated on the protective film to absorb the extreme ultraviolet light, The protective film is made of ruthenium (Ru) or a ruthenium alloy, the absorber film is made of tantalum (Ta) or a tantalum alloy, a diffusion suppression film containing ruthenium and oxygen for preventing mutual diffusion with the absorber film is formed on the surface of the protective film on the side in contact with the absorber film as a part of the protective film, and the diffusion suppression film is subjected to an electron beam annealing treatment. A method for manufacturing a reflective mask blank.
16. A reflective mask blank manufactured by the manufacturing method according to any one of claims 1 to 16.
Citation Information
Patent Citations
Multilayer mirror, manufacturing method, exposure unit and device manufacturing method
JP2007183120A
Reflective mask blank, reflective mask and manufacturing method of semiconductor device
JP2015122468A
Reflective mask blank for EUV lithography and method for producing the same
WO2010026998A1
Cited By
Reflective mask, blank substrate, method for manufacturing a reflective mask, and method for manufacturing a blank substrate
JP7911336B1