Organic solvent purification

Modified zeolites with hydrogen or ammonium functional groups effectively remove metal impurities and contaminants from organic solvents to ppb and ppt levels, addressing the limitations of existing purification methods and achieving high-purity solvents for electronics applications.

JP2024544204APending Publication Date: 2024-11-28DOW GLOBAL TECHNOLOGIES LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024533020
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-14
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing purification methods, such as distillation, are inadequate for achieving the stringent purity requirements of organic solvents used in electronics processing, as they cannot effectively remove metal impurities to the low ppb and ppt levels needed.

Method used

A modified zeolite with hydrogen or ammonium functional groups and tailored pore sizes is used to adsorb metal impurities and contaminants from organic solvents, achieving high removal efficiency through a fixed-bed process.

Benefits of technology

The modified zeolite achieves metal contaminant levels below 1 ppb and water removal above 80%, suitable for high-purity solvent applications like electronics processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544204000001
    Figure 2024544204000001
  • Figure 2024544204000002
    Figure 2024544204000002
  • Figure 2024544204000003
    Figure 2024544204000003
Patent Text Reader

Abstract

1. A modified zeolitic material for use in removing metal impurities from an organic solvent composition, the modified zeolitic material comprising: (i) a hydrogen-based zeolite having hydrogen functional groups; (ii) an ammonium-based zeolite having ammonium functional groups; or (iii) a combination of a hydrogen-based zeolite having hydrogen functional groups and an ammonium-based zeolite having ammonium functional groups, the modified zeolitic material having a pore size of 3 Å to 20 Å, and selectively removing metal impurities present in the solvent to an impurity content of less than 1 ppb; a process for preparing the modified zeolitic material; and a process for removing contaminants from an organic solvent using the modified zeolitic material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to modified zeolites, processes for purifying organic solvents by removing contaminants from the organic solvents, processes for purifying organic solvents by removing metal contaminants using modified zeolites, and purified organic solvents. [Background technology]

[0002] Organic solvents are widely used in polymer cleaning, dissolving, and stripping applications. In certain applications, such as electronics processing, pharmaceuticals, and everyday products, the use of pure solvents, i.e., solvents free of metals and other contaminants, is required by users of such industries. For example, solvents used in the manufacture of electronic materials (e.g., electronics processing chemicals) must contain very low (e.g., less than 10 ppb) concentrations of impurities.

[0003] In the past, distillation methods or processes using multiple purification steps have been implemented to purify chemicals (solvents) and provide electronic grade standard products. The reason is that most single-step purification processes other than distillation can only selectively remove one targeted impurity. Such single purification techniques cannot meet the stringent quality requirements of the electronics industry for the purification of solvents used in electronics processing.

[0004] What is needed in the industry is a simpler, less expensive method for purifying organic solvents that is different from distillation. In particular, it is desirable to purify organic solvents such as glycol ethers and glycol ether acetates used in applications such as electronics processing where the amount of metals and other contaminants present in the organic solvent is strictly controlled to a very low maximum level. Therefore, an effective and efficient method for removing metal impurities from organic solvents is highly desirable.

[0005] Some known processes for removing various metal contaminants from solutions or aqueous media use materials such as silicate compositions as described in WO 2021091816 (A1); zeolite-type materials as described in WO 2021032754 (A1), JP 03770538 (B2), JP 2006052118 (A), JP 2004250259 (A), CN 111807635 (A), and CN 108033456 (B); porous materials incorporating oxygen-containing compounds of iron, copper, aluminum, titanium, and / or zirconium as described in U.S. Pat. No. 7,429,551 (B2); or molecular sieves in a packed bed as described in Chine Patent No. 109476582 (A0). However, it is desirable to have an effective and efficient method for removing metals present in organic solvents. Summary of the Invention

[0006] In one embodiment, the present invention relates to a modified zeolite for removing heavy metals and anions from an organic solvent composition containing more than 1 ppb of metal impurities to less than 1 ppb of heavy metals and anions, the modified zeolite comprising (i) a hydrogen-based zeolite having hydrogen functional groups, (ii) an ammonium-based zeolite having ammonium functional groups, or (iii) a mixture of such hydrogen-based and ammonium-based zeolites, containing an average pore size sufficient to adsorb metal impurities and other contaminants. For example, the average pore size of the modified zeolite can be 3 Å to 20 Å in a typical embodiment to selectively adsorb metal impurities and water present in the organic solvent to provide a purified organic solvent.

[0007] In another embodiment, the present invention relates to a purification process for removing contaminants from organic solvents using the above modified zeolite. For example, in a preferred aspect, the process of the present invention comprises removing metal contaminants and non-metal ion contaminants from an organic solvent or a mixture of organic solvents using the above modified zeolite. For example, in another preferred embodiment, the present invention relates to a purification process comprising using the above modified zeolite in a fixed bed with high metal removal efficiency (up to ppt metal level) and water removal in an organic solvent. For example, in yet another preferred embodiment, the present invention relates to the purification of organic solvents such as glycol ethers and glycol ether acetates. In yet another preferred embodiment, the present invention relates to a process for removing metal contaminants and cationic contaminants from an organic solvent or a mixture of two or more organic solvents, comprising the steps of: (a) preparing a fixed bed of the above modified zeolite absorbent material; and (b) contacting an organic solvent or a mixture of organic solvents with the fixed bed of the modified zeolite absorbent material of step (a).

[0008] In general, the metal contaminants present in the organic solvent may be, for example, Na, K, Ca, Al, Fe, Ni, Zn, Cu, Cr, and Sn, and the initial concentration of each of the metal contaminants in the organic solvent may be 0.1 ppb or more. Thus, it is an object of some embodiments of the present invention to provide a process that can be used to remove high levels of one or more metal contaminants, which is more efficient than known processes. For example, it is an object of some embodiments of the present invention to provide a process for obtaining purified organic solvents having metal contaminant levels of less than 50 ppt.

[0009] Various embodiments of the invention are described in more detail in the detailed description that follows. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Specific embodiments of the present application are described herein below.

[0011] Unless otherwise stated, or implied from the context, or customary in the art, all percentages, parts, ratios, and other amounts are defined by or based on weight, and the part and percentage values ​​are based on weight.For example, all percentages described herein are weight percentages (wt%) unless otherwise indicated.In addition, all test methods disclosed herein are current as of the filing date of this disclosure.

[0012] All temperatures used herein are in degrees Celsius (°C).

[0013] As used herein, "room temperature (RT)" and "ambient temperature" mean a temperature between 20° C. and 26° C., unless otherwise specified.

[0014] As used herein, the term "composition" refers to a mixture of materials that make up the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0015] As used herein, the term "zeolite" refers to a microporous aluminosilicate mineral commonly used as a commercial absorbent.

[0016] As used herein, the term "modified zeolite" means a conventional zeolite that has been treated to remove the alkali or alkali metals present in the conventional zeolite.

[0017] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed herein. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless specifically stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any succeeding description any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or" refers to the listed members individually and in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0018] Numerical ranges disclosed herein include all values ​​between the lower limit and the upper limit (inclusive). In the case of ranges containing explicit values ​​(e.g., ranges 1, or 2, or 3-5, or 6, or 7), any subranges between any two explicit values ​​are included (e.g., the range 1-7 above includes the subranges 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0019] As used throughout this specification, the following abbreviations have the following meanings unless the context clearly dictates otherwise: "=" means "equal to" or "equal to", "<" means "less than", ">" means "greater than", "≦" means "less than or equal to", "≧" means "greater than or equal to", "@" means "at", ppm = parts per million, ppb = parts per billion, ppt = parts per trillion, BV / hr = bed volume per hour, "MT" = metric ton, g = grams, mg = milligrams, Kg = kilogram, L = liter, g / L = grams per liter, μL = microliter, "g / cm 3" or "g / cc" = grams per cubic centimeter, g / 10min = grams per 10 minutes, mg / mL = milligrams per milliliter, "kg / m 3 = kilograms per cubic meter, ppm = parts per million by weight, pbw = parts by weight, rpm = revolutions per minute, m = meters, mm = millimeters, cm = centimeters, μm = microns or micrometers, nm = nanometers, Å = angstroms, min = minutes, s = seconds, ms = milliseconds, hr = hours, Pa = pascals, MPa = megapascals, Pa-s = pascal seconds, mPa-s = millipascal seconds, g / mol = grams per mole, g / eq = grams per equivalent, M n = number average molecular weight, M w = weight average molecular weight, pts = parts by weight, 1 / s or seconds -1 = reciprocal of seconds [s -1 ], °C = degrees Celsius, °C / min = degrees Celsius per minute, psi = pounds per square inch, kPa = kilopascals, % = percent, vol% = volume percent, mol% = mole percent, and wt% = weight percent.

[0020] In general, the absorbent material of the present invention is a modified zeolite comprising the following matrix: MO·xAl2O3·ySiO2·zH2O In the matrix, M is at least one of hydrogen (H), ammonium (NH4), NRH3, NR2H2, NR3H, and NR4, and R is methyl and metal oxides, including, for example, Li2O, Na2O, and K2O, and mixtures thereof. In another embodiment, the M2O component of the molecular structure M2O·xAl2O3·ySiO2·zH2 can be M'O, where M' includes divalent metals, such as MgO, CaO, SrO, BaO, and mixtures thereof. In the matrix, x, y, and z are molar ratios, and x is 0.2 to 5 in one embodiment, 0.5 to 3 in another embodiment, and 0.8 to 1.5 in yet another embodiment. In the matrix, y is 1 to 25 in one embodiment, 1.5 to 10 in another embodiment, and 2 to 5 in yet another embodiment. In the matrix, z is 1 to 20 in one embodiment, 2 to 10 in another embodiment, and 3 to 6 in yet another embodiment.

[0021] In other embodiments, the modified zeolite has an average pore size of 3 Å to 20 Å (0.3 nm to 2.0 nm) in one typical embodiment, 3 Å to 15 Å in another embodiment, 3 Å to 11 Å in yet another embodiment, 3 Å to 10 Å in yet another embodiment, and 4 Å to 10 Å in yet another embodiment.

[0022] In another embodiment, the modified zeolite is 500 m 2 / g, in another embodiment 500m 2 / g~5,000m 2 / g, and in yet another embodiment 1,000m 2 / g~2,000m 2 / g.

[0023] In some embodiments, the modified zeolite of the present invention having the molecular structure of MO·xAl2O3·ySiO2·zH2O has a cation exchange capacity of 0.1 eq / mol to 1.5 eq / mol in one embodiment, 0.5 eq / mol to 1.4 eq / mol in another embodiment, and 1.0 eq / mol to 1.3 eq / mol in yet another embodiment.

[0024] The modified zeolites of the present invention are also stable in liquids having pH values ​​of 0-12 in one embodiment, 3-10 in another embodiment, and 5-8 in yet another embodiment. In relation to the modified zeolites of the present invention, "stable" in liquid means that the elements (e.g., metals) of the zeolite do not leach / release into the liquid (e.g., solvent) and the zeolite maintains its integrity in liquids having a pH of 0-12. In relation to the modified zeolites of the present invention, "unstable" in liquid means that the elements (e.g., metals) of the zeolite leach into the liquid (at a pH of 0-12) and thus, for example, the leached metals add to the metal contaminant content of the liquid. Unstable zeolites are undesirable because they will increase the metal contaminant content of the solvent, which is the opposite effect to that desired by the use of the modified zeolites of the present invention.

[0025] The shape of the modified zeolite is not critical and may be, for example, in the form of beads, rods, cubes, powders, other irregular shapes, and mixtures thereof.

[0026] In general, the modified zeolite may include A, X, Y, USY, and STI types. In a preferred embodiment, the modified zeolite includes A and Y types.

[0027] In another embodiment, the modified zeolite composition may include, for example, a composition comprising a combination of the following matrices: (a) MO·xAl2O3·ySiO2·zH2O, where M=hydrogen; (b) MO·xAl2O3·ySiO2·zH2O, where M'=ammonium; and (c) optionally MO"2OxAl2O3·ySiO2·zH2O, where M"=metal oxide.

[0028] In a preferred embodiment, the modified zeolite composition is a combination of components (a) and (b) in a weight ratio a:b of 1:99 to 99:1.

[0029] When optional component (c) is used, the weight ratio (mixture of components (a) and (b)):c is, in one embodiment, 1:1 to 99:1. In a preferred embodiment, when optional component (c) is used in the preparation of the modified zeolite composition, components (a) to (c) are mixed according to the following process steps: step (I): providing component (c); step (II): mixing components (a) and (b); step (III): mixing component (c) with the mixture of components (a) or (b).

[0030] In a broad embodiment, the process for preparing the modified zeolite useful in the present invention comprises, for example, the following steps: Step (I): Placing unmodified (conventional) zeolite material in a fixed bed column; Step (II): Treating the unmodified (conventional) zeolitic material of step (I) in the fixed bed column of step (I) by flushing the unmodified zeolitic material with a weak acid (for hydrogen-based zeolites), a weak base / ammonia salt (for ammonium-based zeolites), or a mixture thereof (for a mixture of hydrogen-based and ammonium-based zeolites); and Step (III): Activating the zeolitic material from step (II) by calcining the zeolitic material from step (II) at a dehydration temperature of 200° C. to 400° C. to provide a dehydrated zeolitic material.

[0031] The weak acid used in step (II) can include, for example, acetic acid, propanoic acid, phosphoric acid; tartaric acid; and mixtures thereof. The weak base used in step (II) can include, for example, ammonia, ammonia salts, and mixtures thereof. The ammonia salts used in step (II) to treat the unmodified zeolite material to prepare the modified zeolite can include, for example, (NH4)2SO4, CH3COONH4, CH3COON(CH3)4, [N(CH3)]4Cl, and mixtures thereof.

[0032] The flow rate of the flushing step (II) may be, for example, in one typical embodiment, from 0.1 BV / hr to 20 BV / hr (BV=bed volume), in another embodiment, from 0.5 BV / hr to 10 BV / hr, and in yet another embodiment, from 1 BV / hr to 5 BV / hr.

[0033] The temperature of the flushing step (II) can be, for example, from room temperature to 100°C in one typical embodiment, from 40°C to 80°C in another embodiment, and from 50°C to 70°C in yet another embodiment.

[0034] The temperature of the activation step (III) may be, for example, 200°C to 400°C in one typical embodiment, 220°C to 350°C in another embodiment, and 250°C to 300°C in yet another embodiment.

[0035] In carrying out the above process, an optional inert gas padding may be used if desired. For example, the inert gas may be nitrogen, argon, and mixtures thereof.

[0036] The above-mentioned embodiment of the process of the present invention for preparing the modified zeolite composition and the above-mentioned steps thereof can be carried out by conventional equipment known to those skilled in the art. For example, the flushing step (II) for forming hydrogen-based zeolite and / or ammonium-based zeolite material can be carried out by a known fixed bed component, and the heating step (III) can be carried out by a heater commonly known in the art.

[0037] Some advantageous properties and / or benefits exhibited by the modified zeolite material used in the solvent purification process of the present invention can include, for example: (1) The alkali or alkali metals present in the zeolite are effectively replaced using ammonia-based chemicals; (2) the use of the modified zeolite material of the present invention results in lower concentrations of metal leaching, e.g., the amount of leaching is maintained at levels of less than 1 ppb to 1 ppm in one typical embodiment; (3) prior to using the zeolite material to purify the solvent, the alkali in the zeolite material can be reduced, e.g., the concentration of alkali can be from 0.01 wt % to less than 0.1 wt % in one typical embodiment; (4) after modification of the zeolite material, the zeolite material provides a solvent with increased purity to low ppt levels, e.g., in one typical embodiment, less than 1,000 ppt.

[0038] Once the modified zeolitic material useful in the present invention has been prepared as described above, the zeolitic material is placed in a column and subjected to dehydration according to the following steps: Step (1): The modified zeolite material prepared by the above zeolite preparation process steps is placed in a column; Step (2): In a typical embodiment, an inert gas such as nitrogen or argon is filled into the column at a gas pressure of 0.1 MPa to 0.3 MPa. Step (3): The column, with the zeolite material and the solvent therein, is heated in one typical embodiment to a temperature between room temperature and 100° C., in one typical embodiment for a period between 10 minutes and 1,000 minutes to form a dehydrated zeolite material.

[0039] After the modified zeolitic material useful in the present invention has been dehydrated as described above, the solvent to be purified is passed through the dehydrated zeolitic material in a column and subjected to metal exchange. The metal exchange process may be carried out following the additional steps described above in steps (1)-(3): Step (4): In one typical embodiment, the solvent to be purified is passed through the bed of hydrated zeolite material in the column at a flow rate of 0.1 BV / hr to 20 BV / hr; and Step (5): The column, in which the zeolite material and the solvent are present, is heated to a temperature of 200° C. to 400° C. in one typical embodiment, for a period of 60 minutes to 300 minutes in one typical embodiment.

[0040] After passing a solvent through the modified zeolite material to activate the metal exchange process as described above, the modified zeolite material can be used again to process another solvent to be purified by regenerating the zeolite material in a column before passing the solvent through the zeolite material. Typically, the regeneration process is carried out using the same zeolite modification process (steps (I)-(III)) described above.

[0041] In general, the process of the present invention is applicable to the purification of organic solvents, particularly the purification of a single organic solvent and / or a mixture of two or more organic solvents.For example, the organic solvent to be purified can include dipropylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, ethylene glycol propyl ether, ethylene glycol butyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol propyl ether, diethylene glycol butyl ether, ethanol, isopropanol, propylene glycol methyl ether, propylene glycol methyl ether acetate, diethylene glycol ethyl ether acetate, butanol, methyl isobutyl ketone, isopropyl acetate, ethyl lactate, butyl lactate, ethyl acetate, butyl acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol diacetate, ethyl 3-ethoxypropionate, gamma-butyrolactone, and mixtures thereof. In some preferred embodiments, the solvents to be purified include, for example, propylene glycol methyl ether acetate, propylene glycol methyl ether, and mixtures thereof.

[0042] In one embodiment, organic solvents useful in the present invention include, but are not limited to, for example, propylene glycol methyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, ethylene glycol propyl ether, ethylene glycol butyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol propyl ether, diethylene glycol butyl ether, ethanol, isopropanol, and the like, and mixtures thereof.

[0043] In other embodiments, organic solvents useful in the present invention include, but are not limited to, for example, "hydrolyzable organic solvents". As used herein, "hydrolyzable organic solvents" refers to solvents that contain compounds that can be decomposed into acidic and basic components by water, with or without a catalyst. Hydrolyzable organic solvents include, but are not limited to, for example, esters, amides, carbonates, and mixtures thereof. Examples of esters useful in the present invention include propylene glycol methyl ether acetate (PGMEA), ethyl lactate, butyl lactate, ethyl acetate, butyl acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol diacetate, ethyl 3-ethoxypropionate, gamma-butyrolactone, and mixtures thereof.

[0044] In a preferred embodiment, the solvents to be purified (ie, treated with the modified zeolite material) include, for example, glycol ethers, glycol ether acetates, alcohols, ketones, esters, and mixtures thereof.

[0045] By way of illustration and not limitation, some examples of solvents that may be purified include propylene glycol methyl ether, propylene glycol methyl ether acetate, diethylene glycol ethyl ether, butanol, methyl isobutyl ketone, isopropyl acetate, and the like, and mixtures thereof.

[0046] In some embodiments, various metal impurities may be present in the solvent before the solvent is purified with the modified zeolitic material of the present invention, including, for example, Li, Na, K, Mg, Ca, Sr, Ba, Al, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ag, Cd, Pb, Sb, and the like, and combinations thereof. In other embodiments, specific contaminants that are desired to be removed from the solvent may include, for example, Na, K, Ca, Al, Fe, Ni, Zn, Cu, Sn, Cr, and mixtures thereof. In a preferred embodiment, the metal impurities removed from the solvent include, for example, Ni, Cu, Sn, Cr, Ba, Cd, Pb, and mixtures thereof.

[0047] In a typical embodiment, the target metal impurity level of the organic solvent is below the ppb level after the solvent is treated with the modified zeolite treatment described above. For example, in some embodiments, the target metal impurity level of the organic solvent is less than 1,000 ppt (parts per trillion) after the solvent is treated with the modified zeolite treatment described above. Thus, the organic solvent obtained using the purification process of the present invention may be useful in applications requiring a solvent with a fairly high level of purity, such as, for example, the manufacture of pharmaceuticals and electronic materials, and in particular, for example, for use in semiconductor fabrication processes.

[0048] In other embodiments, the metal contaminants and other contaminants in the organic solvents treated through the modified zeolite process of the present invention may be, for example, 0 ppt to less than 1,000 ppt in one general embodiment, 1 to 800 ppt in another embodiment, 1 to 500 ppt in yet another embodiment, 1 ppt to 400 ppt in a further embodiment, 1 ppt to 300 ppt in a still further embodiment, 1 ppt to 200 ppt in a still further embodiment, 1 ppt to 100 ppt in another embodiment, and 1 ppt to 50 ppt in a still further embodiment. In other embodiments, some of the specific individual metal contaminants may be at concentration levels below 50 ppt. In some applications, the total concentration of contaminants in the solvent may not exceed a certain concentration. For example, if the total contaminant level in the solvent is above 50 ppt and cannot be reduced to below 50 ppt, the solvent may not be useful for a particular application, such as electronics processing.

[0049] Water may be present in the solvent, and the modified zeolite material can remove water from the solvent being purified. In one embodiment, the target water removal rate from the solvent is 80% or more, in another embodiment, 80%-100%, in yet another embodiment, 85%-98%, and in yet another embodiment, 90%-95%.

[0050] Sometimes, the zeolitic material originally provided for use in the modification process of the present invention may contain certain metal compounds originating from the manufacturing process of the zeolitic material. Such metal compounds in the original (unmodified) zeolitic material may leach out of the zeolitic material and cause contamination in the solvent to be purified. Therefore, it is desirable to minimize the amount of metal compounds, leachable species, and / or other undesirable compounds such as water present in the zeolitic material to reduce the possibility of such contaminants contaminating the solvent to be purified. In order to prevent metal contamination of the solvent when the contaminants originate from the zeolitic material, the content of metal compounds in the zeolitic material used in one or more application embodiments of the present invention is usually 20% by weight or less.

[0051] The original (unmodified) zeolite material before modification may contain undesirable amounts of water. In one typical embodiment, the water content in the zeolite material is reduced to 50% by weight or less, and in another embodiment, to 5% to 30% by weight, before use. To reduce the water content in the zeolite material, the zeolite material may be regenerated before contacting it with an organic solvent. The regeneration equipment and conditions for drying the zeolite material, such as temperature, time, and pressure, can be selected using techniques known to those skilled in the art. For example, the zeolite material may be heated at a temperature of 250° C. to 300° C. under reduced pressure for 0.5 to 16 hours.

[0052] In some embodiments, the final metal content of the solvent used in various applications requiring low metal content is less than 1 ppb, which the zeolitic material of the present invention can achieve. In some embodiments, the final water content of the solvent may depend on the application in which the solvent is used. For various applications requiring low water content, the zeolitic material of the present invention can provide a solvent having a water content of 300 ppm or less in one typical embodiment, 280 ppm or less in another embodiment, 200 ppm or less in yet another embodiment, 100 ppm or less in yet another embodiment, 50 ppm or less in yet another embodiment, and 10 ppm or less in yet another embodiment. In other embodiments, the zeolitic material of the present invention can provide a water content of the solvent of 0.01 ppm to 300 ppm in one typical embodiment, and 1 ppm to 280 ppm in another embodiment. In a preferred embodiment, the water content of the solvent may be 1 ppm to 10 ppm in one typical embodiment.

[0053] In a broad embodiment, a process for removing metal contaminants from an organic solvent comprises the steps of (a) providing a fixed bed of the modified zeolite described above, and (b) contacting an organic solvent or mixture of organic solvents with the modified zeolite material in the fixed bed of step (a).

[0054] When the organic solvent is contacted with the fixed bed of modified zeolite, any known conventional method for contacting a liquid with the modified zeolite can be used. For example, the fixed bed of modified zeolite can be packed in a column, and the solvent can be poured through the fixed bed of modified zeolite from the top of the column. In the contact step (b) of the process, the flow rate of the solvent passing through the fixed modified zeolite bed can be, for example, 0.1 BV / h to 20 BV / h (BV=bed volume) in one typical embodiment, 0.5 BV / h to 10 BV / h in another embodiment, and 1 BV / h to 5 BV / h in yet another embodiment. If the flow rate of the solvent passing through the fixed modified zeolite bed is more than 20 BV / h, the metal removal rate decreases, and if the flow rate of the solvent passing through the fixed modified zeolite bed is less than 0.1 BV / h, the purification efficiency of the solvent decreases. As used herein, "BV" means bed volume, which refers to the amount of liquid that contacts the same amount of fixed bed of modified zeolite. For example, when using 120mL of fixed bed of modified zeolite, 1BV means that 120mL of organic solvent contacts the fixed bed of modified zeolite. "BV / hr" is calculated by dividing the flow rate (mL / hr) by the bed volume (mL).

[0055] In general, the temperature of step (b) of the process, i.e., the step of contacting the organic solvent with the fixed bed of the modified zeolite, can be, for example, in one embodiment, 0° C. to 100° C., in another embodiment, 10° C. to 60° C., and in yet another embodiment, 20° C. to 40° C. If the temperature is above 100° C., the modified zeolite may be damaged, and if the temperature is below 0° C., part of the solvent being treated may freeze.

[0056] Generally, the purified organic solvent obtained by processing through the zeolite material of the present invention has an improvement of at least 80%, i.e., the amount of contaminant is reduced by at least 80% from the original amount of contaminant present in the original solvent containing the metal contaminant. For example, the reduction in contaminant in the solvent can be 80% or more to 100% in one typical embodiment, 90% to 100% in another embodiment, and 95% to 99% in yet another embodiment. Alternatively, for example, as described above, in some embodiments, metal contaminants and other contaminants in the organic solvent processed through the modified zeolite process of the present invention can be removed and reduced to levels measured below ppb levels, and in preferred embodiments, the contaminants can be removed and reduced to levels measured below ppt levels. For example, as described above, the metal contaminant content of the solvent can be reduced to levels of 0 ppt to less than 1,000 ppt in one typical embodiment, and in other embodiments as already described above.

[0057] Further, the purified organic solvent obtained by processing through the zeolitic material of the present invention has an improvement of at least 80%, i.e., the water content is reduced by at least 80% from the original water content present in the water-containing organic solvent. Alternatively, for example, as discussed above, in some embodiments, the water content in the solvent using the modified zeolitic material of the present invention can be reduced by 80% or more in one general embodiment, by 80% or more to 100% in another embodiment, by 90% to 100% in yet another embodiment, and by 95% to 99% in yet another embodiment.

[0058] In some embodiments, the purified solvents of the present invention are used in, for example, display pixel processing applications, display thin film transistor processing applications, and semiconductor circuit processing applications. EXAMPLES

[0059] The following inventive examples (Inv. Ex.) and comparative examples (Comp. Ex.) (collectively "Examples") are presented herein to further illustrate the features of the present invention, but are not intended to be construed as limiting the scope of the claims, either explicitly or implicitly. Inventive examples are identified by Arabic numerals, and comparative examples are represented by alphabetical letters. The following experiments analyzed the performance of embodiments of the compositions described herein. Unless otherwise indicated, all parts and percentages are by weight based on total weight.

[0060] Abbreviation Various terms and names used in the Inventive Examples (Inv. Ex.) and Comparative Examples (Comp. Ex.) are explained as follows. "BV" means bed volume. "HDPE" means high density polyethylene. "PTFE" means polytetrafluoroethylene. "PFA" means polyfluoroalkoxy.

[0061] raw materials Table I lists the raw materials (ingredients) including the solvents and different zeolite materials used in the examples. The solvents purified and used in the examples were glycol ether acetates, more specifically propylene glycol methyl ether acetate (e.g., DOWANOL™ PMA).

[0062] [Table 1]

[0063] [Table 2]

[0064] General procedure for zeolite modification In one part of the procedure, hydrogen-based zeolite was first prepared by placing 50 mL of unmodified zeolite with pore size of 4 Å-10 Å into a column of 5 cm diameter and 30 cm length as a fixed bed. The unmodified zeolite was modified by flushing acetic acid through the fixed bed column at a flow rate of 2 BV / hr for 1 day. The flushing step was controlled at a temperature of 120°C with application of nitrogen gas. After the above flushing step for 180 minutes, the obtained 4 Å-10 Å zeolite was converted into hydrogen-based zeolite (e.g., Zeolite A and Zeolite D).

[0065] In another part of the procedure, ammonia-based zeolites were prepared by first placing 50 mL of unmodified zeolites with pore sizes of 4-10 Å into a column of 5 cm diameter and 30 cm length as a fixed bed. The unmodified zeolites were modified by flushing with 1 mol% (NH4)2SO4 aqueous solution at a flow rate of 2 BV / hr for 1 day. The flushing step was controlled at a temperature of 120 °C while applying nitrogen gas. After the above flushing step for 180 min, the obtained 4-10 Å zeolites were converted into ammonia-based zeolites (e.g., Zeolite B and Zeolite E).

[0066] In yet another part of the general procedure, a modified zeolite material useful in the present invention was prepared by mixing (i) a hydrogen-based zeolite (Zeolite A) prepared as above and (ii) an ammonia-based zeolite (Zeolite B) prepared as above, the two zeolite materials being mixed together in a 1:1 volume ratio of Zeolite A:Zeolite B.

[0067] The modified zeolitic material containing a mixture of hydrogen-based and ammonia-based zeolites was activated by calcining the mixed zeolites at a temperature of 250° C. for 8 hours in a nitrogen atmosphere (0.1 MPa) to effect dehydration.

[0068] Dehydration and metal exchange 100 mL of a mixture of zeolite A and zeolite B (1:1 by volume) was placed at the bottom of the column. Then, 50 mL of zeolite C was placed on top of the mixture of zeolite A and zeolite B. The comparative example (Comp. Ex. A) used a column with only zeolite C.

[0069] The solvent, propylene glycol methyl ether acetate, was passed through the zeolite bed at a flow rate of 2 BV / h. Nitrogen (N2) padding was applied inside the column at 0.1 MPa N2 pressure. The solvent passing through the zeolite bed serves the functions of dehydration and metal exchange. The solvent passing through the zeolite bed step was carried out at a controlled temperature of 80°C.

[0070] Samples of the solvent passing through the zeolite bed were collected in 100 mL plastic (HDPE) bottles at various times during the dehydration and metal exchange process described above. The first 100 mL sample of solvent was collected at 0 hours, followed by solvent samples for specific examples at 2 hours, 4 hours, 6 hours, and / or 8 hours.

[0071] [Table 3]

[0072] Test Methods and Measurements The columns and pipelines used in the examples were made from fluoroplastics (eg, PTFE or PFA) or electropolished stainless steel.

[0073] metal concentration The metal content of the solvent samples treated through the above dehydration and metal exchange processes was measured and analyzed by conventional equipment such as an ICP-MS (Inductively Coupled Plasma-Mass Spectrometry) instrument available from Rion according to the metal test method using ICP-MS, and the analytical results are shown in Tables IV to VI.

[0074] Water Test The water content of the solvent processed through the above dehydration and metal exchange process was measured by Karl Fischer titration using the water test method described in ASTM E203.

[0075] Test results The percent metal contaminant removal can be determined by comparing the data at 2, 4, or 6 hours (after zeolite treatment) compared to the data at 0 hours (before zeolite treatment), as reported in Tables IV-VI. Generally, over a period of time, the metal content in the solvent sample will increase or decrease, and eventually, the metal content will reach an equilibrium level.

[0076] [Table 4]

[0077] [Table 5]

[0078] [Table 6]

[0079] Discussion of results Comparative Example A: A commercially available sodium-based zeolite with a pore size of 4 Å was used in Comparative Example A. The sodium-based zeolite removed water from the solvent sample but was unable to remove most of the metals from the solvent sample, except for purified Pb at 6 hours (40% removal). Instead, the sodium-based zeolite captured metals from the processing of the preceding material and released them into the subsequent material, gradually increasing the metal content, especially in the case of Na, where the metal content increased significantly.

[0080] Inventive Example 1: Half the volume of hydrogen-based zeolite with pore size of 4 Å and the other half the volume of ammonium-based zeolite with pore size of 4 Å were used in Inventive Example 1. This combination removed Cr, Sn, and Ba in PMA after treatment. The Sn removal rate in 4 hours showed an efficiency of more than 70%. The results show that the modified zeolite of the present invention advantageously and effectively removes transition metals from the solvent.

[0081] Inventive Example 2: Half the volume of the zeolite composite material of Inventive Example 1 and half the volume of the sodium-based zeolite of Comparative Example A were used in Inventive Example 2. The top layer of zeolite material in the column was the zeolite of Comparative Example A, and the bottom layer of zeolite material in the column was the zeolite of Inventive Example 1. The zeolite material of Inventive Example 2 removed most of the metals except Cr and Na. The Cu removal rate in 6 hours showed an efficiency of 70%. The results show that the modified zeolite of the present invention advantageously and effectively removes transition metals from solvents.

[0082] Inventive Example 3: Half the volume of the zeolite material of Inventive Example 4 (see Inventive Example 4 below) and half the volume of the sodium-based zeolite of Comparative Example A were used in Inventive Example 3. The top layer of zeolite material in the column was the zeolite of Comparative Example A, and the bottom layer of zeolite material in the column was the zeolite of Inventive Example 4. This zeolite material in Inventive Example 3 removed most metals from the solvent sample except Cr and Na. The Sn removal rate at 6 hours and the Pb removal rate at 6 hours showed an efficiency of over 90%. The results also show that the modified zeolite of the present invention (as a multi-layer design) removes small amounts of water from the solvent. The advantage of the zeolite material of Inventive Example 3 is its effectiveness in removing some transition metals from the solvent.

[0083] Inventive Example 4: Half the volume of hydrogen-based zeolite material with 10 Å pore size and the other half of ammonia-based zeolite material with 10 Å pore size were used in Inventive Example 4. This combination of zeolite materials in Inventive Example 4 removed all metals, and most metal removal rates reached 80% or higher efficiency. In addition, water reduction was better than that of CE1. The advantage of the zeolite material in Inventive Example 4 is its effectiveness in removing all transition metals and water.

[0084] The data of Comparative Example A shows an increase in metals during the solvent purification process. It was theorized that the increase in metals was caused by metals captured from the previously processed solvent material being subsequently released into the subsequent solvent material processed subsequent to the previously processed solvent material. The zeolite material of Comparative Example A shows weak metal exchange strength. In contrast, most of the zeolite materials of Examples 1-4 of the present invention showed strong metal exchange strength, indicating that they could reduce the metal content of the solvent. The metal removal rate of over 70% shown by the zeolite material of the present invention is considered to be an efficient performance. In terms of pore size, the use of a zeolite material with a pore size of 10 Å is more efficient in terms of metal removal and water removal than the use of a zeolite material with a pore size of 4 Å.

[0085] The results show that the zeolite materials of Inventive Example 2 and Inventive Example 3 were less efficient than Comparative Example A in terms of water removal, but the zeolite materials of Inventive Example 2 and Inventive Example 3 show the effectiveness of the zeolite materials of the present invention in terms of metal removal, even when mixed with sodium-based zeolite having a pore size of 4 Å. The combination of hydrogen-based zeolite and ammonia-based zeolite used in Inventive Example 1 and Inventive Example 4 was significantly better than Comparative Example A in terms of metal removal rate.

Claims

1. A modified zeolite comprising a zeolite material for purifying a solvent, the zeolite material being selected from the group consisting of: (i) a hydrogen-based zeolite having hydrogen functional groups, (ii) an ammonium-based zeolite having ammonium functional groups, and (iii) a combination of a hydrogen-based zeolite having hydrogen functional groups and an ammonium-based zeolite having ammonium functional groups, the zeolite having a pore size of 3 Å to 20 Å for selectively adsorbing metal impurities and water present in the solvent.

2. 2. The modified zeolite of claim 1, wherein the zeolite comprises an aluminosilicate framework containing aluminum, silicon, oxygen, and countercations, and a honeycomb structure.

3. The zeolite is M 2 O.xAl 2 O 3 ySiO 2 ・zH 2 O (wherein M is H, NH 4 , N.R.H. 3 , N.R. 2 H 2 , N.R. 3 H, N.R. 4 or at least one of a metal oxide, R is methyl, x is 0.2-5, x is 1-25, and y is 1-20.

4. The zeolite is 500m 2 / g to 5,000m 2 2. The modified zeolite of claim 1, having a surface area of ​​0.1 eq / mol to 1.5 eq / mol, a cation exchange capacity of 0.1 eq / mol to 1.5 eq / mol, and a stability of a liquid pH value of 0 to 12.

5. 2. The modified zeolite of claim 1, wherein the zeolite material is prepared by an alkali metal reduction process, and the zeolite material is an alkaline-based zeolite, an alkali-based zeolite, a hydrogen-based zeolite, or a mixture thereof.

6. A process for preparing the modified zeolite of claim 1, comprising: (a) placing unmodified zeolitic material in a column to form a fixed bed of unmodified zeolitic material; (b) modifying the fixed bed of unmodified zeolitic material from step (a) to form a modified zeolitic material by (i) flushing at least one weak acid through the fixed bed column of step (a) to form a hydrogen-based zeolite, or (ii) flushing at least one weak base or at least one ammonia salt through the fixed bed column of step (a) to form an ammonium-based zeolite; (c) activating the modified zeolitic material from step (b) by calcining the zeolitic material at a temperature between 200° C. and 400° C. to dehydrate the zeolitic material; The process includes:

7. 1. A process for removing metal contaminants from a contaminated organic solvent or a mixture of contaminated organic solvents, comprising: (a) placing unmodified zeolitic material in a column to form a fixed bed of unmodified zeolitic material; (b) modifying the fixed bed of unmodified zeolitic material from step (a) by flushing a weak acid to form a hydrogen-based zeolite or a weak base or an ammonia salt to form an ammonium-based zeolite through the fixed bed column of step (a) to form a modified zeolite; (c) activating the modified zeolitic material from step (b) by calcining the zeolitic material at a temperature between 200° C. and 400° C. to substantially dehydrate the zeolitic material and form a modified zeolite; (d) providing a fixed bed of the modified zeolitic material from step (c); (e) contacting the metal-contaminated organic solvent or mixture of metal-contaminated organic solvents to be purified with the modified zeolitic material in the fixed bed from step (d) to form a purified solvent having a metal content of less than 1 parts per billion; The process includes:

8. 8. The process of claim 7, wherein the weak acid in the flashing step (b) is acetic acid, propanoic acid, or a mixture thereof, or the weak base in the flashing step (b) is ammonia, the flow rate of the flashing step (b) is from 0.1 BV / hr to 20 BV / hr, the flashing step (b) is carried out at a temperature from room temperature to 100° C., the flashing step (b) is carried out in an inert gas atmosphere at an inert gas pressure of from 0.1 MPa to 0.3 MPa, and the inert gas is nitrogen, argon, or a mixture thereof.

9. 8. The process of claim 7, wherein the solvent to be purified is selected from the group consisting of alcohols, ethers, ketones, acetates, hydrocarbons, halogenated compounds, esters, and mixtures thereof.

10. 8. The process of claim 7, wherein the solvent to be purified is a glycol ether or a glycol ether acetate.

11. 2. The process of claim 1 , wherein the solvent to be purified is propylene glycol methyl ether acetate.

12. 8. The process of claim 7, wherein the purified solvent has a metal impurity content of greater than 1 parts per billion and the purified solvent is contacted in step (e) with a modified zeolite to form a purified solvent containing a metal impurity content of less than 1 parts per billion, and the water content of the solvent is reduced to less than 0.1 weight percent.

13. A purified solvent prepared by the process of claim 7.

14. 14. The refinement solvent of claim 13, wherein the concentration of individual metal impurities present in the refinement solvent is less than parts per trillion.

Citation Information

Patent Citations

  • Production method of edible acetic acid

    CN101445443A

  • Method for separating and extracting natural theanine

    CN101805269A

  • Method for extracting fucoidan and removing heavy metals from kelps

    CN103387622A

  • Removal of impurity in liquid crystal

    JP1992013795A