Zn-Al-Mg alloy plated steel containing V and B and its manufacturing method
By optimizing Al and Mg contents and adding V and B, the Zn-Al-Mg alloy plated steel material addresses formability and corrosion resistance issues, ensuring durability and performance in demanding applications.
Patent Information
- Application Number
- JP2024532883
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-08-03
- Publication Date
- 2024-12-03
AI Technical Summary
Current Zn-Al-Mg alloy plated steel sheets with medium to high aluminum compositions struggle to meet formability and welding performance requirements in applications like home appliances and automobiles, despite having improved corrosion resistance.
A Zn-Al-Mg alloy plated steel material with controlled Al and Mg contents, along with the addition of vanadium (V) and boron (B), optimized through specific manufacturing processes to enhance formability and corrosion resistance.
The alloy achieves high corrosion resistance and formability, withstanding over 400 hours of neutral salt spray testing and 0T bending without visible cracks, and maintaining excellent paint adhesion, suitable for home appliances and automobiles.
Smart Images

Figure 2024544667000001 
Figure 2024544667000002 
Figure 2024544667000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a Zn-Al-Mg alloy-plated steel material containing V and B and a manufacturing method thereof, which belongs to the technical field of steel metallurgy production. [Background technology]
[0002] Zn-Al-Mg alloy coating layers attracted widespread attention overseas in the 1980s and became an important research topic in the specialized field of hot-dip galvanized and zinc alloy coating layers. Research results by domestic and foreign peers have shown that when the Zn and Al contents in the coating layer are the same, hot-dip Zn-Al-Mg alloy coating steel sheets with added Mg have better corrosion resistance and better material processing and application performance (formability, weldability and paintability), and can replace the traditional corresponding hot-dip galvanized steel sheets or zinc alloy coating steel sheets, and a wide range of market demand is expected.
[0003] Hot-dip Zn-Al-Mg alloy-plated steel sheets were industrialized and applied by steel companies such as Nippon Steel Corporation, Nisshin Steel Co., Ltd., and ThyssenKrupp Co., Ltd. in the 2000s, and are currently mainly used in the construction industry, and are gradually entering the home appliance and automobile manufacturing industries. In China, research into Zn-Al-Mg alloy plating is relatively slow, and currently only manufacturers such as Baosteel, Shougang, Jiuquan iron and steel, and Pangang are selling hot-dip Zn-Al-Mg alloy-plated steel sheets.
[0004] Conventional hot-dip Zn-Al-Mg alloy-coated steel sheets can be divided into three types: "low aluminum" (WAl<5%), "medium aluminum" (5%≦WAl<13%), and "high aluminum" (47%≦WAl≦57%). Different types of Zn-Al-Mg alloy-coated steel sheets have different Al and Mg contents in the coating layer, so there are differences in the structure and quality performance of the coating layer, and their application fields are also different.
[0005] Patent Document 1 discloses a highly corrosion-resistant single-bath Zn-Al-Mg rare earth protective plating layer and its manufacturing method, which uses a single-bath hot-dip plating method to form a Zn-Al-Mg alloy plating layer on a metal surface. The plating layer and the metal substrate each maintain their original properties, while having a metallurgical bonding surface of 99.9% or more. The plating layer has a dense structure, stable composition, zero leakage plating, and excellent corrosion resistance, and can resist salt spray corrosion for up to 2060 hours. The corrosion resistance of the alloy plating layer is better than that of ordinary hot-dip pure zinc plating layers, improving the service life. This single-bath plating method is recyclable and industrializable, and overcomes the shortcomings of the difficulty of plating between metal and Zn-Al-Mg alloy plating solution, the difficulty of forming a good bonding surface between the two, and the tendency of leakage plating, so it can be widely applied to produce a co-penetrating layer on metal surface with Zn-Al-Mg alloy plating solution containing 5%-12% Al and 1%-6% Mg, and the co-penetrating layer forms ternary eutectic of Zn / Al / MgZn2 and various binary eutectic, which is the main reason for its high corrosion resistance. The above single-bath Zn-Al-Mg rare earth protective plating layer with high corrosion resistance adopts a composition system of medium aluminum.
[0006] Patent Document 2 discloses a hot-dip plated steel sheet having high corrosion resistance and a manufacturing method thereof. The hot-dip plated steel sheet includes a substrate and an Al-Zn-Si-Mg plating layer formed on the substrate, and the chemical components of the plating layer are, in mass%, Al: 45% to 65%, Si: 0.1% to 3%, Mg: 0.2% to 5%, Zr: 0.001% to 0.15%, Cr: 0.001% to 0.5%, and the balance: Zn and unavoidable impurities. The manufacturing method includes (1) pre-treating the steel sheet, (2) immersing the steel sheet in a plating solution tank at 560 to 595°C to perform hot-dip plating, and (3) removing the steel sheet from the plating solution and cooling it stepwise. The hot-dip plated steel sheet has excellent corrosion resistance and significantly suppresses the generation of white rust and the development of red rust, as well as the dispersion of coating layer destruction from notches. The hot-dip galvanized steel sheet having excellent corrosion resistance described above employs a high aluminum composition.
[0007] Therefore, high corrosion resistance Zn-Al-Mg steel sheets are mainly composed of medium and high aluminum composition systems. As the Al and Mg content increases, the corrosion resistance of the coating layer improves, but the forming and welding performance decreases. In the application fields of home appliances and automobiles, Zn-Al-Mg alloy coated steel sheets must have good formability to meet the stamping forming performance requirements of users, but the current Zn-Al-Mg alloy coated steel sheets with medium and high aluminum composition systems are still unable to meet the requirements of users. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] China Patent Application Publication No. 105063532 [Patent Document 2] China Patent Publication No. 109402547 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in view of the above, and provides a Zn-Al-Mg alloy-plated steel material containing V and B, which has high formability and high corrosion resistance, and a method for producing the same. [Means for solving the problem]
[0010] In order to solve the above technical problems, the present invention employs the following technical means. A Zn-Al-Mg alloy plated steel material containing V and B according to one embodiment of the present invention has a plating layer having chemical compositions, in mass%, of Al: 0.4-2.8%, Mg: 0.5-3.0%, V: 0.005-0.50%, B: 0.001-0.20%, and the balance: Zn and unavoidable impurities, in which the Al / Mg ratio is 0.8-1.5 and the total amount of V and B is 0.01-0.50%.
[0011] Furthermore, the chemical composition of the coating layer satisfies at least one of the following conditions (1) to (3): (1) the coating layer contains 1.0 to 2.5% Al, 1.0 to 2.0% Mg, 0.02 to 0.30% V, and 0.03 to 0.20% B, (2) the Al / Mg ratio is 0.75 to 1.25, and (3) the total amount of V and B is 0.05 to 0.20%.
[0012] Furthermore, the total amount of the unavoidable impurities is 0.010% or less, of which Pb≦0.003%, Sb≦0.002%, Sn≦0.002%, As≦0.001%, Te≦0.001%, and Cd≦0.002%.
[0013] Furthermore, the weight of the plating layer on both sides is 20 to 600 g / m 2 and preferably, the weight of the plating layer on both sides is 40 to 400 g / m 2 It is.
[0014] Furthermore, the steel base material of the steel material is at least one selected from IF steel, BH steel, SPCC, SEDDQ, QP steel, DP steel, and TRIP steel, and preferably the IF steel is a high-strength IF steel containing P.
[0015] The method for producing the Zn-Al-Mg alloy plated steel material includes a degreasing and cleaning step for the steel substrate, a continuous annealing step, a hot dip plating step, and an air knife purging step.
[0016] Furthermore, the H2 content in the furnace during the continuous annealing process is controlled to 4.0% or more by volume, and preferably, the H2 content in the furnace during the continuous annealing process is controlled to 4.0 to 6.0% by volume.
[0017] Furthermore, the temperature of the steel substrate when it enters the molten zinc pot is kept at 400 to 520°C, the temperature of the plating solution during the hot-dip plating process is 390 to 500°C, and the temperature difference between the temperature of the steel substrate when it enters the molten zinc pot and the temperature of the plating solution is kept to ±20°C.
[0018] Furthermore, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 280°C or less until it reaches the top turning roll, and preferably, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 240 to 260°C until it reaches the top turning roll. Effect of the Invention
[0019] The beneficial effects of the present invention are as follows: The Zn-Al-Mg alloy-plated steel of the present invention adopts a low aluminum composition system and controls the composition of the plating layer, thereby obtaining a Zn-Al-Mg alloy-plated steel sheet with high corrosion resistance and high formability. According to tests, the Zn-Al-Mg alloy-plated steel of the present invention has a time until red rust appears under neutral salt spray test conditions of 400 hours, even 4500 hours or more, no obvious cracks are visible to the naked eye after 0T bending, and the time until red rust appears on the bent part under neutral salt spray test conditions of 300 hours, even 4000 hours or more, and has excellent adhesion of the paint layer after painting. The Zn-Al-Mg alloy-plated steel is particularly applicable to the fields of home appliances and automobiles, and is expected to be well applied and popularized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention provides a Zn-Al-Mg alloy plated steel material containing V and B. The steel material has a plating layer having chemical compositions, in mass%, of Al: 0.4% to 2.8%, Mg: 0.5% to 3.0%, V: 0.005% to 0.50%, B: 0.001% to 0.20%, and the balance: Zn and unavoidable impurities, in which the Al / Mg ratio is 0.8 to 1.5, and the total amount of V and B is 0.01 to 0.50%.
[0021] Currently, in this field, medium and high aluminum composition systems are mainly adopted to ensure the corrosion resistance of Zn-Al-Mg alloy plated steel. However, as the Al and Mg content increases, the forming performance and welding performance of the steel material are significantly reduced, making it difficult to meet the requirements for stamping forming performance in the fields of home appliances and automobiles. In view of the above problems, the present invention optimizes the Mg and Al content (content) in the plating layer and adds other alloying elements to achieve various effects as follows. V causes heterogeneous nucleation during the formation of the plating layer to refine the grain size of the plating layer, thereby improving the ductility of the plating layer and improving the corrosion resistance of the plating layer. B fills the gaps in the crystalline plating layer to reduce defects inside the plating layer, and increases the strength and hardness of the plating layer through solid solution strengthening, strengthening the wear resistance, and meeting the user's requirements for high corrosion resistance and high formability.
[0022] In the manufacturing process of the coating layer, the process needs to be limited to ensure that the coating layer has good surface quality and performance. The thickness of the coating layer needs to be limited within a certain range, taking into account the strength of the air knife jet and the fluidity of the coating solution. If the weight of the coating layer is too large and the pressure of the air knife jet is small, the surface quality and thickness of the coating layer cannot be controlled. On the other hand, if the flow rate of the air knife jet is finite and the fluidity of the coating solution is constant, the thickness of the coating layer will be too thin. The coating solution has different wettability to the surface of different steel sheets, and only steel sheets with good wettability can form a coating layer with good adhesion. The annealing atmosphere is to improve the good reducibility of the steel substrate surface, and generally the higher the H2 content, the more appropriate it is, but the higher the H2 content, the higher the risk of explosion. The temperature of the coating solution needs to be such that the coating solution is in a molten state and has appropriate fluidity. The temperature range of the coating solution is improved by adding V, but if the temperature is too high, it is easy to increase zinc oxide slag. In order to ensure complete solidification of the coating layer, the temperature of the steel sheet needs to be reduced to below its freezing point before it reaches the first turning roll. Furthermore, zinc, aluminum and magnesium are easily oxidized, so rapid cooling can improve the surface quality.
[0023] The technical means of the present invention will be described below with reference to examples. Those skilled in the art will understand that the following examples are for illustrating the present invention and do not limit the scope of the present invention. If no specific techniques or conditions are shown in the examples, they will be in accordance with the techniques or conditions described in the literature in the field or the product specifications. If no manufacturer is shown, the reagents or equipment used are commercially available and common.
[0024] (Example 1) Production of Zn-Al-Mg alloy plated steel material of the present invention The plating layer weighs 60g / m 2 (Both sides) and the main components are, in mass%, Al: 2.8%, Mg: 2.0%, V: 0.10%, B: 0.02%, Pb: 0.002%, Sb: 0.001%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is TRIP steel.
[0025] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel substrate is rinsed and cleaned after the degreasing treatment. During the continuous annealing process, the H2 content in the furnace is controlled to 6.0% by volume. The temperature of the steel sheet when it enters the molten zinc pot is 500°C, and the temperature of the coating solution is maintained at 480°C during the hot dip coating process. After coating, the steel sheet is rapidly cooled so that the temperature of the strip is 260°C when it reaches the top turning roll.
[0026] (Test Method) Corrosion resistance: Neutral salt spray test is used to accelerate corrosion. The test conditions and methods are carried out in accordance with GB / T10125-2012 "Salt spray test of artificial atmosphere corrosion test". The test equipment is a salt spray corrosion test box, the corrosive medium is a deionized NaCl solution with a concentration of 50g / L and a pH value of 6.5, the test temperature is set at 35±2℃, the size of the test piece is 75mm×150mm×0.8mm, and the edges are sealed with 5mm of transparent tape to prevent edge corrosion from affecting the results. The test piece is placed at an angle of 15°~25° to the vertical. The time until red rust appears on the surface of the test piece is observed.
[0027] Formability: The test piece is bent at 0T (180° bend, the radius of the bend is 0), and the appearance of cracks is observed with the naked eye. In addition, the time until red rust appears on the bent part is observed under the neutral salt spray test conditions, and the neutral salt spray test conditions and methods are carried out in accordance with GB / T10125-2012 "Salt spray test for artificial atmosphere corrosion test".
[0028] Hardness: Using an INNOVATESTE Europe BV general-purpose hardness tester, measure the surface hardness (HV0.01) of the plating layer at three points and take the average value.
[0029] Paintability: After oil-coated plated steel sheets are degreased, cleaned, ceramic-coated or phosphate-treated, spray-painted and dried. The adhesion between the paint layer and the steel sheet is then inspected by a cross-cut test. If the paint layer does not fall off, this indicates good adhesion.
[0030] Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel shows red rust after 600 hours or more under neutral salt spray test conditions, no obvious cracks are visible to the naked eye after 0T bending, and shows red rust after 500 hours or more under neutral salt spray test conditions. The hardness of the plated layer is 110, and the adhesion of the coating layer after painting is excellent, which meets the requirements of users.
[0031] (Example 2) Production of Zn-Al-Mg alloy plated steel material of the present invention The plating layer weighs 200g / m 2 (Both sides) and the main components are, in mass%, Al: 1.5%, Mg: 2.0%, V: 0.05%, B: 0.10%, Pb: 0.001%, Sb: 0.002%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is SEDDQ steel.
[0032] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel substrate is rinsed and cleaned after the degreasing treatment. During the continuous annealing process, the H2 content in the furnace is controlled to 5.0% by volume. The temperature of the steel sheet when it enters the molten zinc pot is 450°C, and the temperature of the coating solution is maintained at 450°C during the hot dip coating process. After coating, the steel sheet is rapidly cooled so that the temperature of the strip is 240°C when it reaches the top turning roll.
[0033] The test method was the same as in Example 1. Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel has a time until red rust appears in more than 2000 hours under neutral salt spray test conditions, a hardness of the plated layer is 120, no obvious cracks are visible to the naked eye after 0T bending, and a time until red rust appears in the bent part in neutral salt spray test conditions is more than 1800 hours, and the adhesion of the coating layer after painting is excellent, which meets the requirements of users.
[0034] (Example 3) Preparation of Zn-Al-Mg alloy plated steel material of the present invention The plating layer weighs 500g / m 2 (Both sides) and the main components are, in mass%, Al: 1.0%, Mg: 1.0%, V: 0.20%, B: 0.15%, Ca: 0.05%, Pb: 0.002%, Sb: 0.001%, Cr: 0.001%, Cd: 0.002%, Sn: 0.002%, and the balance is Zn. The steel substrate is QP steel.
[0035] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel substrate is rinsed and cleaned after the degreasing treatment. During the continuous annealing process, the H2 content in the furnace is controlled to 4.0% by volume. The temperature of the steel strip when it enters the molten zinc pot is 440°C, and during the hot dip coating process, the temperature of the coating solution is maintained at 430°C. After coating, the steel strip is rapidly cooled so that the temperature of the strip when it reaches the top turning roll is 260°C.
[0036] The test method was the same as in Example 1. Test results: The Zn-Al-Mg alloy plated steel produced in this embodiment has good surface quality, excellent corrosion resistance, formability and paintability. The plated steel can reach red rust appearance time of more than 4500 hours under neutral salt spray test conditions, the hardness of the plated layer is 110, no obvious cracks are visible to the naked eye after 0T bending, the time until red rust appears on the bent part can reach more than 4000 hours under neutral salt spray test conditions, and the adhesion of the coating layer after painting is excellent, which meets the requirements of users.
[0037] (Comparative Example) The plating layer weighs 180g / m 2 The main components are, by mass%, Al: 1.6%, Mg: 1.8%, Pb: 0.001%, Sb: 0.001%, Cr: 0.001%, Cd: 0.001%, Sn: 0.001%, and the balance is Zn. The steel substrate is BH steel.
[0038] The manufacturing process includes a degreasing and washing process, a continuous annealing process, a hot dip coating process, an air knife purging process, and a cooling process. In the degreasing and washing process, the steel substrate is rinsed and cleaned after the degreasing treatment. During the continuous annealing process, the H2 content in the furnace is controlled to 4.0% by volume. The temperature of the steel strip when it enters the molten zinc pot is 460°C, and during the hot dip coating process, the temperature of the coating solution is maintained at 450°C. After coating, the steel strip is rapidly cooled so that the temperature of the strip when it reaches the top turning roll is 320°C.
[0039] The test method was the same as in Example 1. Test results: The surface quality of the Zn-Al-Mg alloy plated steel produced in this comparative example is inferior to that of the present invention, with horizontal line defects, and the corrosion resistance, formability, and paintability are also somewhat poor. The plated steel has a time until red rust appears under neutral salt spray test conditions of 1200 hours or more, a hardness of the plating layer of 90, slight cracks are visible to the naked eye after 0T bending, the time until red rust appears on the bent part under neutral salt spray test conditions of 1100 hours or more, and excellent adhesion of the paint layer after painting.
[0040] It is to be understood that the particular features, structures, materials, or configurations described herein may be combined in any suitable manner in any one or more embodiments, and that the various features of the different embodiments and embodiments described herein may be combined with each other, unless mutually inconsistent, as would be understood by one of ordinary skill in the art.
[0041] (Additional Note) (Appendix 1) A plating layer having chemical compositions in mass% of Al: 0.4-2.8%, Mg: 0.5-3.0%, V: 0.005-0.50%, B: 0.001-0.20%, and the balance: Zn and unavoidable impurities, in which the Al / Mg ratio is 0.8-1.5 and the total amount of V and B is 0.01-0.50%. Zn-Al-Mg alloy plated steel material containing V and B.
[0042] (Appendix 2) The chemical composition of the plating layer is The plating layer contains Al: 1.0 to 2.5%, Mg: 1.0 to 2.0%, V: 0.02 to 0.30%, and B: 0.03 to 0.20%. Al / Mg is 0.75 to 1.25, and The total content of V and B is 0.05 to 0.20%, 2. A Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
[0043] (Appendix 3) The total content of the unavoidable impurities is 0.010% or less, of which Pb≦0.003%, Sb≦0.002%, Sn≦0.002%, As≦0.001%, Te≦0.001%, Cd≦0.002%; 2. A Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
[0044] (Appendix 4) The weight of the plating layer on both sides is 20 to 600 g / m 2 and preferably, the weight of the plating layer on both sides is 40 to 400 g / m 2 That is, 2. A Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
[0045] (Appendix 5) The steel substrate of the steel material is at least one selected from IF steel, BH steel, SPCC, SEDDQ, QP steel, DP steel and TRIP steel, and preferably, the IF steel is a high-strength IF steel containing P. 2. A Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
[0046] (Appendix 6) The process includes degreasing and cleaning of steel substrates, continuous annealing, hot-dip plating, and air knife purging. 6. A method for producing a Zn-Al-Mg alloy plated steel material containing V and B according to any one of claims 1 to 5.
[0047] (Appendix 7) During the continuous annealing process, the H content in the furnace is controlled to 4.0% or more by volume, and preferably, during the continuous annealing process, the H content in the furnace is controlled to 4.0 to 6.0% by volume. The manufacturing method according to claim 6,
[0048] (Appendix 8) The temperature of the steel substrate when entering the molten zinc pot is controlled to 400 to 520°C, the temperature of the plating solution during the hot-dip coating process is 390 to 500°C, and the temperature difference between the temperature of the steel substrate when entering the molten zinc pot and the temperature of the plating solution is controlled to ±20°C. The manufacturing method according to claim 6,
[0049] (Appendix 9) After plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 280°C or less until it reaches the top turning roll, and preferably, after plating, the steel strip is rapidly cooled so that the temperature of the steel strip is 240-260°C until it reaches the top turning roll. The manufacturing method according to claim 6,
[0050] (Appendix 10) The Zn-Al-Mg alloy-plated steel material containing V and B is obtained by the manufacturing method described in any one of Appendices 6 to 9. Zn-Al-Mg alloy plated steel material containing V and B.
Claims
1. A plating layer having chemical compositions, in mass%, of Al: 0.4-2.8%, Mg: 0.5-3.0%, V: 0.005-0.50%, B: 0.001-0.20%, and the balance: Zn and unavoidable impurities, in which the Al / Mg ratio is 0.8-1.5, and the total amount of V and B is 0.01-0.50%, Zn-Al-Mg alloy-plated steel material containing V and B,
2. The chemical composition of the plating layer is The plating layer contains Al: 1.0 to 2.5%, Mg: 1.0 to 2.0%, V: 0.02 to 0.30%, and B: 0.03 to 0.20%. Al / Mg is 0.75 to 1.25; and The total amount of V and B is 0.05 to 0.20%.
2. The Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
3. The total amount of the unavoidable impurities is 0.010% or less, of which Pb≦0.003%, Sb≦0.002%, Sn≦0.002%, As≦0.001%, Te≦0.001%, and Cd≦0.002%; 2. The Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
4. The weight of the plating layer on both sides is 20 to 600 g / m 2 and preferably, the weight of the plating layer is 40 to 400 g / m on both sides. 2 That is, 2. The Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
5. The steel substrate of the steel material is at least one selected from IF steel, BH steel, SPCC, SEDDQ, QP steel, DP steel and TRIP steel, and preferably, the IF steel is a high-strength IF steel containing P.
2. The Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
6. The process includes degreasing and cleaning of steel substrates, continuous annealing, hot-dip plating, and air knife purging.
6. A method for producing a Zn-Al-Mg alloy-plated steel material containing V and B according to claim 1.
7. During the continuous annealing process, H in the furnace 2 The content is controlled to 4.0% by volume or more, and preferably, H in the furnace during the continuous annealing process is 2 The content is controlled to 4.0 to 6.0% by volume. The method according to claim 6 .
8. The temperature of the steel substrate when entering the molten zinc pot is controlled to 400 to 520°C, the temperature of the plating solution during the hot-dip coating process is 390 to 500°C, and the temperature difference between the temperature of the steel substrate when entering the molten zinc pot and the temperature of the plating solution is controlled to ±20°C. The method according to claim 6 .
9. After plating, the strip is cooled rapidly so that the temperature of the strip is below 280°C until it reaches the top turning roll, and preferably after plating, the strip is cooled rapidly so that the temperature of the strip is between 240 and 260°C until it reaches the top turning roll. The method according to claim 6 .
10. The Zn-Al-Mg alloy-plated steel material containing V and B is obtained by the manufacturing method according to any one of claims 6 to 9. Zn-Al-Mg alloy-plated steel material containing V and B,
Citation Information
Patent Citations
Plating solution for continuous hot dipping of steel strips and dipping method thereof
CN104498850A
Hot-dip galvanized aluminum-magnesium alloy coated steel plate for ultra-deep drawing and preparation method thereof
CN112575276A
Hot dip zn-al-mg based alloy plated steel having excellent corrosion resistance
JP2002332555A
High strength hot dip galvanized steel sheet having excellent plating adhesion on high working and excellent ductility, and production method therefor
JP2003055751A
Method for producing flat steel product coated with anti-corrosion system
JP2009537698A