Carbon-based catalyst for fuel cells with excellent durability, method for producing same, and polymer electrolyte fuel cell including same
A ceramic-coated carbon-based fuel cell catalyst with needle-shaped protrusions addresses the issue of corrosion and oxidation, enhancing durability and stability by improving corrosion resistance and catalyst stabilization.
Patent Information
- Application Number
- JP2024534054
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2022-11-02
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-02
AI Technical Summary
Conventional fuel cell catalysts using platinum on carbon-based supports suffer from rapid deterioration due to oxidation and corrosion, leading to reduced performance.
A carbon-based catalyst with a ceramic coating layer featuring needle-shaped protrusions made of TiO2, Al2O3, ZrO2, or CeO2 is applied to protect the carbon-based support, enhancing durability and corrosion resistance.
The ceramic-coated catalyst improves corrosion resistance, increases specific surface area, and stabilizes the catalyst through strong metal support interaction, reducing D-band vacancies and suppressing radical adsorption, thereby maintaining electrode performance.
Smart Images

Figure 2024544693000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon-based catalyst for fuel cells having excellent durability, a manufacturing method thereof, and a polymer electrolyte fuel cell including the same. More specifically, the present invention relates to a carbon-based catalyst for fuel cells having excellent durability, in which a ceramic coating layer having needle-like protrusions is formed by coating a highly corrosion-resistant ceramic material to protect a carbon-based support that is rapidly corroded in the operating environment of the fuel cell, and a manufacturing method thereof, and a polymer electrolyte fuel cell including the same.
[0002] The information on the national research and development project of the present invention is as follows: [Project unique number]1711120511 [Proposal number] 2020M3H4A3105824 [Department name] Ministry of Science, ICT and Technology [Name of issue management (specialized) organization] Korea Research Foundation [Research Project Name] Materials Innovation Leading Project [Research title] Development of core technology for the basic materials of ultra-high durability carbon-based supports [Contribution rate] 1 / 1 [Name of project execution organization] Korea Ceramic Technology Institute [Research period] August 24, 2020 to December 31, 2024 [Background technology]
[0003] A fuel cell is a device that generates electricity by converting chemical energy into electrical energy through the oxidation of hydrogen fuel. Fuel cells can use hydrogen produced using renewable energy, and produce water as a reaction product. They are garnering attention as an environmentally friendly energy source because they do not produce air pollutants or greenhouse gases.
[0004] Depending on the type of electrolyte and fuel used, these fuel cells include Proton Exchange Membrane Fuel Cells (PEMFC), Direct Methanol Fuel Cells (DMFC), Phosphoric Acid Fuel Cells (PAFC), Molten Carbonate Fuel Cells (MCFC), and Solid Oxide Fuel Cells (SOFC).
[0005] Among these, polymer electrolyte fuel cells have a relatively low operating temperature, high energy density, and excellent fast start-up and response characteristics, and technical research is being actively conducted for their use as an energy source for automobiles, various electronic devices, transportation, and power generation.
[0006] In a fuel cell, hydrogen is supplied to the anode and oxygen is supplied to the cathode, and the catalyst in the anode oxidizes the hydrogen to form protons. At this time, the protons pass through the proton conductive membrane and undergo a reduction reaction with oxygen by the catalyst in the cathode to produce electricity.
[0007] The fuel cell includes an anode, a cathode, and an electrolyte membrane disposed between the anode and the cathode, where each of the anode and cathode includes a catalyst including an active support and a carbon-based support supporting the active support.
[0008] Hydrogen injected into the anode of the fuel cell is separated into hydrogen ions and electrons, and air is injected into the cathode of the fuel cell, where oxygen ions and electrons are separated. Electricity is generated by the movement of the separated electrons, and water (H2O) is produced when hydrogen and oxygen come into contact with each other, generating heat.
[0009] Meanwhile, FIG. 1 is a schematic diagram for explaining a conventional fuel cell catalyst, and a more specific explanation will be given with reference to this.
[0010] As shown in Figure 1, conventional fuel cells use catalysts to increase reaction efficiency. Conventional fuel cell catalysts use platinum (Pt), which has excellent oxygen reduction reaction properties, and use a carbon-based support as a support for platinum (Pt).
[0011] However, conventional fuel cell catalysts undergo an oxidation reaction of the carbon-based support (C+2H2O→CO2+4H++4e - ), which causes desorption and aggregation of platinum (Pt), resulting in a phenomenon in which the performance of the catalyst is reduced.
[0012] Furthermore, in the operating environment of the fuel cell, the carbon-based support rapidly oxidizes and corrodes, causing a rapid decrease in the performance of the electrode.
[0013] A related prior document is Korean Patent Publication No. 10-0708732 (published on April 17, 2007), which describes an anode for a fuel cell, a manufacturing method thereof, and a fuel cell including the same. Summary of the Invention [Problem to be solved by the invention]
[0014] The object of the present invention is to provide a carbon-based catalyst for fuel cells having excellent durability, in which a ceramic coating layer having needle-like protrusions is formed by coating a highly corrosion-resistant ceramic material to protect the carbon-based support, which is subject to rapid corrosion in the operating environment of the fuel cell, and a method for manufacturing the same, and a polymer electrolyte fuel cell including the same. [Means for solving the problem]
[0015] In order to achieve the above object, a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention includes a carbon-based support, a ceramic coating layer covering a surface of the carbon-based support, and an active support supported on the ceramic coating layer covering the carbon-based support, and the ceramic coating layer is formed so that a part of it protrudes in a needle-like shape from the surface of the carbon-based support.
[0016] The carbon-based support includes at least one selected from the group consisting of carbon nanotubes, graphene, and activated carbon.
[0017] The ceramic coating layer is made of one or more materials selected from the group consisting of TiO2, Al2O3, ZrO2, and CeO2.
[0018] The ceramic coating layer has a thickness of 10 nm to 10 μm.
[0019] The ceramic coating layer has a surface portion covering the surface of the carbon-based support, and a plurality of protrusions arranged spaced apart from one another from the surface portion, protruding outward from the surface portion, some of which are formed in a needle shape.
[0020] The active support includes at least one selected from platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au).
[0021] In order to achieve the above object, a polymer electrolyte fuel cell including a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention includes a cathode, an anode disposed at a distance from the cathode, an electrolyte membrane disposed between the cathode and the anode, gas diffusion layers disposed on the outsides of the cathode and the anode, respectively, and a separator disposed on the outsides of the gas diffusion layers, wherein at least one of the cathode and the anode includes a carbon-based support, a ceramic coating layer covering a surface of the carbon-based support, and a carbon-based catalyst having an active support supported on the ceramic coating layer covering the carbon-based support, and the ceramic coating layer is formed such that a portion of the ceramic coating layer protrudes in a needle-like shape from the surface of the carbon-based support.
[0022] The ceramic coating layer is made of one or more materials selected from the group consisting of TiO2, Al2O3, ZrO2, and CeO2.
[0023] The ceramic coating layer has a thickness of 10 nm to 10 μm.
[0024] The ceramic coating layer has a surface portion covering the surface of the carbon-based support, and a plurality of protrusions arranged spaced apart from one another from the surface portion, protruding outward from the surface portion, some of which are formed in a needle shape.
[0025] In order to achieve the above object, a method for producing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention includes the steps of: (a) treating a carbon-based support with an acid; (b) forming a ceramic coating layer on the surface of the acid-treated carbon-based support; and (c) supporting an active support on the ceramic coating layer covering the surface of the carbon-based support, wherein in the step (b), the ceramic coating layer is formed such that a part of it protrudes in a needle-like shape from the surface of the carbon-based support.
[0026] The step (a) includes the steps of: (a-1) mixing the carbon-based support with an acidic solution and stirring at a speed of 500 to 1,500 rpm to perform an acid treatment; and (a-2) filtering and washing the acid-treated carbon-based support.
[0027] In the above step (a-1), the acid treatment is carried out at a temperature of 100 to 140° C. for 1 to 10 hours.
[0028] The step (b) includes the steps of: (b-1) adding the acid-treated carbon-based support to a solvent and then mixing by ultrasonic treatment; (b-2) mixing a ceramic precursor and a curing agent into the ultrasonic-treated suspension and stirring to perform hydrothermal synthesis; and (b-3) filtering, washing, and drying the result of the hydrothermal synthesis to form a ceramic coating layer that covers the surface of the carbon-based support.
[0029] In the above step (b-2), the hydrothermal synthesis is carried out at 160 to 240° C. for 10 to 30 hours.
[0030] In the step (b-3), the ceramic coating layer is made of one or more materials selected from the group consisting of TiO2, Al2O3, ZrO2, and CeO2.
[0031] The step (c) includes the steps of: (c-1) immersing the ceramic coating layer covering the surface of the carbon-based support in an active support precursor solution, and then adding a strong base solution to perform hydrothermal synthesis; and (c-2) filtering, washing, and drying the result of the hydrothermal synthesis to support an active support on the ceramic coating layer covering the surface of the carbon-based support.
[0032] In the above step (c-1), the hydrothermal synthesis is carried out at 100 to 200° C. for 1 to 6 hours.
[0033] In the step (c-2), the active support includes at least one selected from platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au). Effect of the Invention
[0034] The carbon-based catalyst for fuel cells and the polymer electrolyte fuel cell including the same according to the present invention have a ceramic coating layer formed to cover the surface of a carbon-based support, and an active support is supported on the ceramic coating layer covering the surface of the carbon-based support, thereby improving corrosion resistance and preventing the carbon-based support from being oxidized and corroded in the operating environment of the fuel cell, thereby improving the performance of the electrode.
[0035] Furthermore, the carbon-based catalyst for fuel cells and the polymer electrolyte fuel cell including the same according to the present invention have the effect of reducing the D-band vacancy of the active support (Pt) through electron transfer from the carbon-based support and the ceramic coating layer, and improving the stabilization of the catalyst through strong metal support interaction (SMSI).
[0036] In addition, the carbon-based catalyst for a fuel cell having excellent durability according to the present invention and the polymer electrolyte fuel cell including the same have a ceramic coating layer formed in a needle shape with a portion protruding outward from the surface of the carbon-based support, which not only improves the specific surface area but also reduces the amount of OH. - This makes it possible to suppress the adsorption of radicals such as H2O2 and improve durability. [Brief description of the drawings]
[0037] [Figure 1] FIG. 1 is a schematic diagram for explaining a conventional fuel cell catalyst. [Diagram 2] FIG. 2 is a schematic diagram showing a polymer electrolyte fuel cell including a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view showing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram for explaining the operation principle of a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram for explaining the operation principle of a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Figure 6] 1A to 1C are schematic process diagrams illustrating a method for producing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Figure 7] 1A to 1C are schematic process diagrams illustrating a method for producing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Figure 8] 1A to 1C are schematic process diagrams illustrating a method for producing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention. [Figure 9] 1 is a graph showing the results of XRD measurement for catalysts according to Examples 1 and 2 and Comparative Example 1. [Figure 10] 1 is a photograph showing catalysts according to Examples 1 and 2. [Figure 11] 1 is a graph showing the evaluation results of physical properties of half cells produced using catalysts according to Examples 1 and 2 and Comparative Example 1. [Figure 12] 1 is a graph showing the evaluation results of physical properties of half cells produced using catalysts according to Examples 1 and 2 and Comparative Example 1. [Figure 13] 1 is a graph showing the evaluation results of physical properties of half cells produced using catalysts according to Examples 1 and 2 and Comparative Example 1. [Figure 14] 1 is a graph showing the results of evaluating the physical properties of fuel cells manufactured using catalysts according to Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 15] 1 is a graph showing the results of evaluating the physical properties of fuel cells manufactured using catalysts according to Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The advantages and features of the present invention, and the method of achieving them, will become clear from the following detailed description of the embodiments in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be embodied in various different forms. However, the embodiments are provided to complete the disclosure of the present invention and to fully inform those skilled in the art of the present invention of the scope of the invention, and the present invention is only defined by the scope of the claims. The same reference numerals in the entire specification refer to the same components.
[0039] Hereinafter, a carbon-based catalyst for a fuel cell having excellent durability, a method for manufacturing the same, and a polymer electrolyte fuel cell including the same according to a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0040] FIG. 2 is a schematic diagram showing a polymer electrolyte fuel cell including a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention, and FIG. 3 is a cross-sectional view showing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention.
[0041] 2 and 3, a polymer electrolyte fuel cell 100 including a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention includes a cathode 110, an anode 120 disposed apart from the cathode 110, and an electrolyte membrane 130 disposed between the cathode 110 and the anode 120. Here, the cathode 110, the anode 120, and the electrolyte membrane 130 constitute a membrane-electrode assembly (MEA) 150.
[0042] In addition, the polymer electrolyte fuel cell 100 including a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention may further include gas diffusion layers 162, 164 arranged on the outside of the cathode 110 and the anode 120, respectively, and separation plates 172, 171 arranged on the outside of the gas diffusion layers 162, 164, respectively.
[0043] Here, the gas diffusion layers 162, 164 may include a first gas diffusion layer 162 disposed on the outside of the cathode 110 and a second gas diffusion layer 164 disposed on the outside of the anode 120. Furthermore, the separation plates 172, 174 may include a first separation plate 172 disposed on the outside of the first gas diffusion layer 162 and a second separation plate 174 disposed on the outside of the second gas diffusion layer 164.
[0044] In this case, at least one of the cathode 110 and the anode 120 includes a carbon-based catalyst 50 having a carbon-based support 10, a ceramic coating layer 20 covering the surface of the carbon-based support 10, and an active support 30 supported on the ceramic coating layer 20 covering the carbon-based support 10.
[0045] Thus, the carbon-based catalyst 50 for a fuel cell having excellent durability according to an embodiment of the present invention includes the carbon-based support 10 , the ceramic coating layer 20 , and the active carrier 30 .
[0046] The carbon-based support 10 serves as a support for supporting the active carrier 30. These carbon-based supports 10 include one or more selected from carbon nanotubes, graphene, and activated carbon, among which carbon nanotubes are more preferably used.
[0047] The ceramic coating layer 20 is formed so as to cover the surface of the carbon-based support 10. At this time, the ceramic coating layer 20 is for protecting the carbon-based support 10 which is rapidly corroded in the operating environment of the fuel cell, and is preferably formed of a ceramic material having high corrosion resistance. For this reason, the ceramic coating layer 20 is preferably formed of one or more materials selected from TiO2, Al2O3, ZrO2, and CeO2, and is more preferably formed of TiO2.
[0048] The ceramic coating layer 20 is formed so that a part of it protrudes in a needle-like shape from the surface of the carbon-based support 10. More specifically, the ceramic coating layer 20 has a surface portion 22 that covers the surface of the carbon-based support 10, and a plurality of protrusions 24 that are arranged spaced apart from one another from the surface portion 22, protrude outward from the surface portion 22, and are partially formed in a needle shape.
[0049] In this manner, the protrusions 24 of the ceramic coating layer 20 are arranged so as to protrude outward from the surface of the carbon-based support 110 at a distance from each other, thereby providing a structural advantage in that the specific surface area can be greatly expanded.
[0050] Therefore, in the carbon-based catalyst 100 for fuel cells having excellent durability according to an embodiment of the present invention, the protrusions 24 of the ceramic coating layer 20 are formed so as to protrude outward from the surface of the carbon-based support 10, so that not only can a high specific surface area be secured, but also durability can be improved by suppressing the adsorption of radicals such as OH and H2O2.
[0051] The ceramic coating layer 20 preferably has a thickness of 10 nm to 10 μm, and more preferably has a thickness of 100 nm to 1 μm. If the thickness of the ceramic coating layer 20 is less than 10 nm, the thickness is too thin and the effect of improving corrosion resistance may not be fully exhibited. Conversely, if the thickness of the ceramic coating layer 20 exceeds 10 μm, it is not preferable because the electrical conductivity may be reduced due to the excessive thickness design.
[0052] The active support 30 is supported on a ceramic coating layer 20 that covers a carbon-based support 10. Here, a precious metal having excellent oxygen reduction reaction properties is used for the active support 30. More specifically, the active support 30 may be made of one or more selected from platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au), and among these, it is more preferable to use platinum (Pt).
[0053] Meanwhile, FIGS. 4 and 5 are schematic diagrams for explaining the operation principle of a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention.
[0054] As shown in Figures 4 and 5, the carbon-based catalyst 50 for a fuel cell having excellent durability according to an embodiment of the present invention is formed by coating the surface of a carbon-based support with a highly corrosion-resistant ceramic material to protect the carbon-based support, which is rapidly corroded in the operating environment of a fuel cell, to form a ceramic coating layer 20 having needle-like protrusions in some parts.
[0055] Furthermore, the carbon-based catalyst 50 for fuel cells having excellent durability according to an embodiment of the present invention has the effect of reducing the D-band vacancy of the active support 30 (Pt) through electron transfer from the carbon-based support and the ceramic coating layer 20, and improving the stabilization of the catalyst through strong metal-support interaction (SMSI).
[0056] Furthermore, in the carbon-based catalyst 50 for fuel cells having excellent durability according to an embodiment of the present invention, the ceramic coating layer 20 is formed in a needle shape with a portion protruding outward from the surface of the carbon-based support, which not only increases the specific surface area but also suppresses the adsorption of radicals such as OH and H2O2, thereby improving durability.
[0057] The carbon-based catalyst for fuel cells having excellent durability according to the above-mentioned embodiments of the present invention and the polymer electrolyte fuel cell including the same have a ceramic coating layer formed to cover the surface of the carbon-based support, and an active carrier is supported on the ceramic coating layer covering the surface of the carbon-based support, thereby improving corrosion resistance and preventing the carbon-based support from being oxidized and corroded in the operating environment of the fuel cell, thereby improving the performance of the electrode.
[0058] Furthermore, the carbon-based catalyst for fuel cells having excellent durability according to the embodiments of the present invention and the polymer electrolyte fuel cell including the same have the effect of reducing the D-band vacancy of the active support (Pt) due to the electron transfer from the carbon-based support and the ceramic coating layer, and improving the stabilization of the catalyst due to the strong metal support interaction (SMSI).
[0059] In addition, the carbon-based catalyst for a fuel cell having excellent durability and the polymer electrolyte fuel cell including the same according to the embodiment of the present invention have a ceramic coating layer formed in a needle shape with a part protruding outward from the surface of the carbon-based support, which not only improves the specific surface area but also reduces the amount of OH. - This makes it possible to suppress the adsorption of radicals such as H2O2 and improve durability.
[0060] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a method for manufacturing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention will be described with reference to the accompanying drawings.
[0061] 6 to 8 are schematic process diagrams showing a method for producing a carbon-based catalyst for a fuel cell having excellent durability according to an embodiment of the present invention.
[0062] As shown in Fig. 6, the carbon-based support 10 is subjected to an acid treatment. This acid treatment includes a process of mixing the carbon-based support 10 with an acid solution and stirring the mixture at a speed of 500 to 1,500 rpm, and a process of filtering the acid-treated carbon-based support 10 and then washing it.
[0063] In this case, it is preferable that the acid treatment be performed using an acidic aqueous solution containing one or more acids selected from sulfuric acid, nitric acid, and hydrochloric acid having a pH of 2 or less. This is because, although using an acidic aqueous solution having a pH exceeding 2 is advantageous in terms of modifying the surface of the carbon-based support 10, it may cause environmental pollution.
[0064] These acid treatments are preferably carried out at a temperature of 100 to 140° C. for 1 to 10 hours. If the acid treatment temperature is less than 100° C. or the acid treatment time is less than 1 hour, the acid treatment is not sufficiently carried out, and it is difficult to fully exhibit the effect of improving the specific surface area. Conversely, if the acid treatment temperature exceeds 140° C. or the acid treatment time exceeds 10 hours, the effect does not increase any more and may act as a factor that only increases the production cost, which is not economical.
[0065] Next, as shown in FIG. 7, a ceramic coating layer 20 is formed on the surface of the acid-treated carbon-based support 10.
[0066] The steps of forming the ceramic coating layer include a process of adding the acid-treated carbon-based support 10 to a solvent and then mixing by ultrasonic treatment, a process of mixing a ceramic precursor and a curing agent into the ultrasonic-treated suspension and stirring to perform hydrothermal synthesis, and a process of filtering, washing, and drying the result of the hydrothermal synthesis to form a ceramic coating layer 20 that covers the surface of the carbon-based support 10.
[0067] Here, the ultrasonic treatment is preferably carried out for 30 to 180 minutes under the conditions of a frequency of 25 to 35 KHz and an output voltage of 5 to 10 W. If the ultrasonic output voltage is less than 5 W or the ultrasonic treatment time is less than 30 minutes, the effect of improving dispersibility may not be fully exhibited. Conversely, if the ultrasonic output voltage exceeds 10 W or the ultrasonic treatment time exceeds 180 minutes, it is not preferable because excessive ultrasonic application may cause a problem of damage to the acid-treated carbon-based support.
[0068] Furthermore, the hydrothermal synthesis is preferably carried out at 160 to 240° C. for 10 to 30 hours. If the hydrothermal synthesis temperature is less than 160° C. or the hydrothermal synthesis time is less than 10 hours, the hydrothermal synthesis may not be performed sufficiently, and the ceramic coating layer 20 may not be completely coated on the surface of the carbon-based support 10. On the other hand, if the hydrothermal synthesis temperature exceeds 240° C. or the hydrothermal synthesis time exceeds 30 hours, there is a risk that the effect will not be further increased and only the production cost and time will increase, which is not preferable from the economical point of view.
[0069] Here, washing is preferably carried out at least twice using distilled water, and drying can be carried out at 60 to 80° C. for 10 to 20 hours, but is not limited thereto.
[0070] At this time, the ceramic coating layer 20 is preferably formed of one or more materials selected from TiO2, Al2O3, ZrO2, and CeO2, and more preferably formed of TiO2. In this manner, the surface of the carbon-based support 10 is coated with a ceramic material having excellent corrosion resistance, and then dried to form the ceramic coating layer 20, thereby improving the corrosion resistance of the catalyst.
[0071] These ceramic coating layers 20 are formed so that parts thereof protrude in a needle-like shape from the surface of the carbon-based support 10. More specifically, the ceramic coating layer 20 has a surface portion that covers the surface of the carbon-based support 10, and a plurality of protruding portions that are arranged spaced apart from one another from the surface portion, protrude outward from the surface portion, and are partly formed in a needle shape.
[0072] In this manner, the protrusions of the ceramic coating layer 20 are arranged so that multiple protrusions are spaced apart from each other and protrude outward from the surface of the carbon-based support 10, thereby providing a structural advantage in that the specific surface area can be greatly expanded.
[0073] Therefore, the carbon-based catalyst for fuel cells having excellent durability manufactured by the method according to the embodiment of the present invention is formed such that the protrusions of the ceramic coating layer 20 protrude outward from the surface of the carbon-based support 10, and therefore not only can it ensure a high specific surface area, but it can also suppress the adsorption of radicals such as OH and H2O2, thereby improving durability.
[0074] The ceramic coating layer 20 preferably has a thickness of 10 nm to 10 μm, and more preferably has a thickness of 100 nm to 1 μm. If the thickness of the ceramic coating layer 20 is less than 10 nm, the thickness is too thin and the effect of improving corrosion resistance may not be fully exhibited. Conversely, if the thickness of the ceramic coating layer 20 exceeds 10 μm, it is not preferable because the electrical conductivity may be reduced due to the excessive thickness design.
[0075] Next, as shown in FIG. 8, an active support 30 is supported on the ceramic coating layer 20 covering the surface of the carbon-based support 10 .
[0076] In this case, the supporting step includes a process of immersing the ceramic coating layer 20 covering the surface of the carbon-based support 10 in an active support precursor solution, adding a strong base solution to perform hydrothermal synthesis, and a process of filtering, washing, and drying the result of the hydrothermal synthesis to support the active support 30 on the ceramic coating layer 20 covering the surface of the carbon-based support 10.
[0077] The strong base solution may be a 0.5 to 1.5 M aqueous solution of sodium hydroxide.
[0078] Here, the hydrothermal synthesis is preferably carried out at 100 to 200° C. for 1 to 6 hours. If the hydrothermal synthesis temperature is less than 100° C. or the hydrothermal synthesis time is less than 1 hour, the active support 30 may not be uniformly supported on the ceramic coating layer 20 covering the surface of the carbon-based support 10. Conversely, if the hydrothermal synthesis temperature exceeds 200° C. or the hydrothermal synthesis time exceeds 6 hours, the effect does not increase any more and may act as a factor that increases only the production cost, which is not economical.
[0079] Here, a precious metal having excellent oxygen reduction reaction properties is used for the active support 30. More specifically, the active support 30 may be made of one or more selected from platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au), and among these, it is more preferable to use platinum (Pt).
[0080] As described above, the method for producing a carbon-based catalyst for a fuel cell having excellent durability according to the embodiment of the present invention is completed.
[0081] Working Example The present invention will be described in more detail below with reference to preferred embodiments thereof, which are presented as preferred examples of the present invention and are not to be construed as limiting the present invention in any sense.
[0082] Contents not described here will not be explained since those skilled in the art can easily deduce them from a technical standpoint.
[0083] 1. Manufacturing of carbon-based catalysts for fuel cells Example 1 1 g of multi-walled carbon nanotubes (MWCNTs) was mixed with 130 ml of an aqueous sulfuric acid solution and 70 ml of an aqueous nitric acid solution, and the mixture was stirred at 1,000 rpm at 120° C. for 4 hours for acid treatment, and then filtered and washed.
[0084] Next, 0.1 g of acid-treated multi-walled carbon nanotubes (MWCNTs) was added to 50 mL of IPA, and then ultrasonically treated and mixed for 1 hour under conditions of a frequency of 20 KHz and an output voltage of 8 W.
[0085] Next, 0.3 mL of titanium tetraisopropoxide (TTIP) and 0.26 mL of diethylenetriamine (DETA) were added to the ultrasonically treated suspension, which was then stirred at a speed of 1,500 rpm for 30 minutes and subjected to hydrothermal synthesis at a temperature of 200° C. for 12 hours.
[0086] Next, the hydrothermally synthesized product was filtered, washed, and then dried at 70°C for 12 hours to produce a TiO2 coating layer covering the surface of the multi-walled carbon nanotubes (MWCNTs).
[0087] Next, the TiO2 coating layer covering the surface of multi-walled carbon nanotubes (MWCNTs) was immersed in H2PtCl6·6H2O, and then an aqueous NaOH solution was added and hydrothermal synthesis was performed at a temperature of 160℃ for 2 hours.
[0088] Next, the hydrothermally synthesized product was filtered and washed, and then dried at 70℃ for 12 hours to support Pt on the TiO2 coating layer covering the surface of multi-walled carbon nanotubes (MWCNTs), producing a carbon-based catalyst (TiO2-CNT@30Pt) for fuel cells.
[0089] Example 2 A carbon-based catalyst (TiO2-CNT@30Pt) for fuel cells was prepared in the same manner as in Example 1, except that the TiO2 coating layer covering the surface of the multi-walled carbon nanotubes (MWCNTs) was prepared by hydrothermal synthesis at a temperature of 200°C for 24 hours.
[0090] Comparative Example 1 1 g of multi-walled carbon nanotubes (MWCNTs) was mixed with 130 ml of an aqueous sulfuric acid solution and 70 ml of an aqueous nitric acid solution, and the mixture was stirred at 1,000 rpm at 120° C. for 4 hours for acid treatment, and then filtered and washed.
[0091] Next, 0.1 g of acid-treated multi-walled carbon nanotubes (MWCNTs) was added to 50 mL of IPA, and then ultrasonically treated and mixed for 1 hour under conditions of a frequency of 20 KHz and an output voltage of 8 W.
[0092] Next, multi-walled carbon nanotubes (MWCNTs) were immersed in H2PtCl6·6H2O, and then NaOH aqueous solution was added and hydrothermal synthesis was performed at a temperature of 160 °C for 2 h.
[0093] Next, the result of the hydrothermal synthesis was filtered, washed, and then dried at 70°C for 12 hours to support Pt on multi-walled carbon nanotubes (MWCNTs) to prepare a carbon-based catalyst (CNT@30Pt) for fuel cells.
[0094] Comparative Example 2 A commercial catalyst (40 wt% Pt / C) was obtained from Premetek.
[0095] 2. Observation of microstructure Fig. 9 is a graph showing the XRD measurement results for the catalysts according to Examples 1 and 2 and Comparative Example 1, and Fig. 10 is a photograph showing the catalysts according to Examples 1 and 2. Here, Fig. 10(a) and (b) are SEM and TEM photographs showing the catalyst according to Example 1, and Fig. 10(c) and (d) are SEM and TEM photographs showing the catalyst according to Example 2.
[0096] 9, it can be seen that the catalysts according to Examples 1 and 2 have TiO2 coated on the CNT surface and Pt loading, so that Pt, C and TiO2(anatase) peaks were detected. On the other hand, the catalyst according to Comparative Example 1 does not have TiO2 coated on the CNT surface, so no TiO2(anatase) peak was detected.
[0097] As shown in FIG. 10, it can be seen that in the catalysts according to Examples 1 and 2, a TiO2 coating layer is formed on the surface of the CNT, and a part of the CNT is formed so as to protrude outward in a needle-like shape.
[0098] 3. Evaluation of physical properties Table 1 shows the results of evaluating the physical properties of the half-cells manufactured using the catalysts according to Examples 1 and 2 and Comparative Example 1. Also, Figs. 11 to 13 are graphs showing the results of evaluating the physical properties of the half-cells manufactured using the catalysts according to Examples 1 and 2 and Comparative Example 1.
[0099] [Table 1]
[0100] As shown in Table 1 and FIGS. 11 to 13, the physical property test results for the half cells according to Examples 1 and 2 and the half cell according to Comparative Example 1 are shown.
[0101] The electrolyte used was a 0.1M perchloric acid solution, which was fully saturated with nitrogen before the measurement. The electrochemical active surface area (ECSA), which means more exposed active sites per unit weight, was measured, and the results showed similar values for Comparative Example 1 and Example 1, but Example 2, which had a thick ceramic coating layer, showed a lower value due to insufficient electrical conductivity caused by the insulation of the ceramic coating layer and the clumping phenomenon within the catalyst.
[0102] The onset potential and half potential, which indicate the reaction rate of the catalyst, are the highest in Example 1. This is because the reaction rate between oxygen gas and platinum is improved due to an increase in the active sites in the catalyst, some of which protrude like needles. This can also be proven by the Tafel slope, which is another indicator of the reaction rate in relation to the overvoltage of the electrochemical reaction rate. The gentler the slope, the more active the reaction in the catalyst. Compared to Comparative Example 1, the slope of Example 1 is low, which shows that the internal reaction of the catalyst is active. The mass activity, which indicates the activity relative to the mass of platinum, is the highest in Example 1, while the specific activity, which indicates the specific activity per unit area, is about 0.1 V lower than that of Comparative Example 1. This is thought to be due to the lack of electrical conductivity and particle agglomeration due to the insulation of the ceramic coating layer, as shown by the ECSA value. As can be seen from the limit current density at which the concentration of reactants in the catalyst layer converges to 0, Comparative Example 1 shows a higher value than Example 1. This is because the more excellent the electrical conductivity of the sample, the higher the value shown, which means that a ceramic coating layer is located inside the catalyst of Example 1, resulting in an insulating phenomenon.
[0103] Meanwhile, Table 2 summarizes the assembly and test conditions for the fuel cells manufactured using the catalysts according to Examples 1-2 and Comparative Examples 1-2, and Table 3 shows the physical property evaluation results for the fuel cells manufactured using the catalysts according to Examples 1-2 and Comparative Examples 1-2. Also, Figures 14 and 15 are graphs showing the physical property evaluation results for the fuel cells manufactured using the catalysts according to Examples 1-2 and Comparative Examples 1-2.
[0104] [Table 2]
[0105] [Table 3]
[0106] As shown in Tables 2 and 3, and FIGS. 14 and 15, the physical property test results for the fuel cells according to Examples 1 and 2 and the fuel cells according to Comparative Examples 1 and 2 are shown.
[0107] For performance experiments and durability tests in the actual operating environment of the fuel cell, a membrane electrode assembly (MEA) for a polymer electrolyte fuel cell was fabricated. The components and test conditions used are as shown in Table 2.
[0108] The electrolyte used in this experiment was Nafion212 (Dupont), and the fuel electrode was a commercial gas diffusion electrode (GDE) coated with 0.5 mg of platinum per area. The air electrode was a gas diffusion layer (GDL) coated with 0.2 mg of platinum catalyst per area by hand spraying, and a membrane electrode assembly (MEA) was completed by applying heat and pressure to nearly 130°C. The electrode area was 0.5 cm for both the hot electrode and the air electrode. 2 was identical to
[0109] The flow rates of the fuel electrode and air electrode of the membrane electrode assembly were set at 105 mL / min of hydrogen gas and 330 mL / min of oxygen gas, respectively, and after sufficient humidification at 70° C., an IV curve was obtained.
[0110] In order to evaluate the long-term durability of fuel cell catalysts, the accelerated stability test (AST) protocol for polymer electrolyte fuel cell membrane electrode assemblies (MEA) published by the US Department of Energy (DOE) was used to rapidly repeat tests at a speed of 500mV / s at a potential range of 1.0~1.5V, where carbon oxidation occurs rapidly, to examine the degree of catalyst degradation by measuring the changes in the electrochemically active area (ECSA) of the catalyst and the maximum power density (MPD) on the IV curve after 5,000 cycles.
[0111] As shown in FIG. 14 and Table 3, the initial performance of Comparative Examples 1 and 2 is better than that of Examples 1 and 2. When comparing the open circuit voltage (OCV), which means the resistance of the circuit when no voltage is applied, it can be seen that Examples 1 and 2 have a higher OCV, which is because the ceramic coating layer, which acts as an insulator, acts as an antibacterial agent. As a result, the maximum power density (MPD) is also different, with Example 2, which has the thickest ceramic coating layer, being the lowest, and Comparative Example 2, which has the smallest catalyst particle size and the best platinum particle dispersion, being the highest. However, the electrochemically active surface area degradation rate (ECSA) after 5,000 cycles is better in Examples 1 and 2, which shows that the ceramic coating layer on the surface of the carbon-based support maintains the cell performance of the membrane electrode assembly (MEA) even after a rigorous durability test.
[0112] This shows that the ceramic coating layer inside the catalyst not only successfully prevents the carbon-based support from oxidizing and corroding, but also exerts a strong metal-support interaction (SMSI) effect, reducing the D-band vacancy of the active support (Pt) due to electron transfer from the carbon-based support and the ceramic coating layer.
[0113] In addition, as shown in FIG. 15, the deterioration rate of not only the electrochemically active surface area (ECSA) of the cathode but also the maximum power density (MPD), which means the overall cell performance, is 6 to 8 times lower than those of Comparative Examples 1 and 2. This is because OH - This means less adsorption of radicals such as H2O2, improving not only degradation at the cathode but the overall durability of the cell.
[0114] Although the present invention has been described above with a focus on the embodiments, various modifications and variations can be made by those skilled in the art who have ordinary skill in the art to which the present invention pertains. These modifications and variations are considered to belong to the present invention as long as they do not deviate from the scope of the technical idea provided by the present invention. Therefore, the scope of the present invention should be determined by the scope of the claims set forth below. [Explanation of symbols]
[0115] 100 Polymer electrolyte fuel cell 110 Cathode 120 Anode 130 Electrolyte Membrane 150 Membrane electrode assembly 162 First gas diffusion layer 164 Second gas diffusion layer 172 1st separation plate 174 Second separation plate
Claims
1. A carbon-based support; a ceramic coating layer covering the surface of the carbon-based support; an active carrier supported on a ceramic coating layer covering the carbon-based support; Including, The ceramic coating layer is formed so that a part of the ceramic coating layer protrudes in a needle-like shape from the surface of the carbon-based support. A highly durable carbon-based catalyst for fuel cells.
2. The carbon-based support is The present invention is characterized in that the material contains at least one selected from carbon nanotubes, graphene, and activated carbon.
2. The carbon-based catalyst for fuel cells having excellent durability according to claim 1.
3. The ceramic coating layer is TiO 2 , Al 2 O 3 , ZrO 2 , and CeO 2 It is characterized in that it is formed of one or more materials selected from the following:
2. The carbon-based catalyst for a fuel cell according to claim 1, which has excellent durability.
4. The ceramic coating layer is Characterized in that it has a thickness of 10 nm to 10 μm; 2. The carbon-based catalyst for a fuel cell according to claim 1, which has excellent durability.
5. The ceramic coating layer is a surface portion covering the surface of the carbon-based support; a plurality of protruding portions arranged at a distance from each other on the surface portion, protruding outward from the surface portion, and having a needle-like shape; Characterized in that it has 2. The carbon-based catalyst for fuel cells having excellent durability according to claim 1.
6. The active support is The present invention is characterized in that it contains one or more selected from the group consisting of platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au).
2. The carbon-based catalyst for fuel cells having excellent durability according to claim 1.
7. A cathode; an anode disposed spaced apart from the cathode; an electrolyte membrane disposed between the cathode and the anode; gas diffusion layers disposed on the outer sides of the cathode and anode, respectively; A separation plate disposed on each of the gas diffusion layers; Including, At least one of the cathode and the anode is The carbon-based catalyst includes a carbon-based support, a ceramic coating layer covering the surface of the carbon-based support, and an active support supported on the ceramic coating layer covering the carbon-based support, The ceramic coating layer is formed so that a part of the ceramic coating layer protrudes in a needle-like shape from the surface of the carbon-based support. A polymer electrolyte fuel cell containing a carbon-based catalyst for a highly durable fuel cell.
8. The ceramic coating layer is TiO 2 , Al 2 O 3 , ZrO 2 , and CeO 2 The present invention is characterized in that the material is made of one or more materials selected from the following: A polymer electrolyte fuel cell comprising the carbon-based catalyst for a fuel cell having excellent durability according to claim 7.
9. The ceramic coating layer is Characterized in that it has a thickness of 10 nm to 10 μm; A polymer electrolyte fuel cell comprising the carbon-based catalyst for a fuel cell having excellent durability according to claim 7.
10. The ceramic coating layer is a surface portion covering the surface of the carbon-based support; a plurality of protruding portions arranged at a distance from each other on the surface portion, protruding outward from the surface portion, and having a needle-like shape; Characterized in that it has A polymer electrolyte fuel cell comprising the carbon-based catalyst for a fuel cell having excellent durability according to claim 7.
11. (a) treating a carbon-based support with an acid; (b) forming a ceramic coating layer on the acid-treated surface of the carbon-based support; (c) supporting an active support on a ceramic coating layer covering the surface of the carbon-based support; Including, In the step (b), the ceramic coating layer is formed so that a part of the ceramic coating layer protrudes from the surface of the carbon-based support in a needle-like shape. A method for producing durable carbon-based catalysts for fuel cells.
12. The above step (a) (a-1) mixing the carbon-based support with an acidic solution and stirring at a speed of 500 to 1,500 rpm to perform an acid treatment; (a-2) filtering and washing the acid-treated carbon-based support; Characterized in that it comprises A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 11.
13. In the above step (a-1), The acid treatment is Characterized in that it is carried out at a temperature of 100 to 140 ° C. for 1 to 10 hours, A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 12.
14. The above step (b) (b-1) adding the acid-treated carbon-based support to a solvent and then mixing by ultrasonic treatment; (b-2) mixing the ultrasonically treated suspension with a ceramic precursor and a curing agent, stirring and hydrothermally synthesizing the mixture; (b-3) filtering, washing, and drying the result of the hydrothermal synthesis to form a ceramic coating layer covering the surface of the carbon-based support; Characterized in that it comprises A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 11.
15. In the above step (b-2), The hydrothermal synthesis is Carrying out the reaction at 160 to 240 ° C for 10 to 30 hours, A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 14.
16. In the above step (b-3), The ceramic coating layer is TiO 2 , Al 2 O 3 , ZrO 2 , and CeO 2 The present invention is characterized in that the material is made of one or more materials selected from the following: A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 14.
17. The above step (c) (c-1) immersing the ceramic coating layer covering the surface of the carbon-based support in an active support precursor solution, and then adding a strong base solution to perform hydrothermal synthesis; (c-2) filtering, washing, and drying the result of the hydrothermal synthesis, and supporting an active support on the ceramic coating layer covering the surface of the carbon-based support; Characterized in that it comprises A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 11.
18. In the above step (c-1), The hydrothermal synthesis is Characterized in that the reaction is carried out at 100 to 200 ° C for 1 to 6 hours, A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 17.
19. In the above step (c-2), The active support is The present invention is characterized in that it contains one or more selected from the group consisting of platinum (Pt), ruthenium (Ru), palladium (Pd), rhodium (Rh), iridium (Ir), osmium (Os), and gold (Au). A method for producing the carbon-based catalyst for a fuel cell having excellent durability according to claim 17.
Citation Information
Patent Citations
Electrode catalyst material and method of producing the same
JP2011222132A
Method for forming metal oxide coating layer on catalyst supporter surface and catalyst supporter and catalyst device containing metal oxide coating layer
JP2017124390A
Catalyst for fuel cell and method of manufacturing the same
JP2018010785A
Metal structure, catalyst-supported metal structure, catalyst-supported metal structure module and preparation methods thereof
US20100261600A1