Pad-in-bottle chemical mechanical planarization polishing using cost-effective non-porous solid polishing pads
Non-porous solid polishing pads with micron-sized polyurethane beads and a specialized CMP slurry composition address the high costs and waste issues of conventional CMP processes, enhancing process stability and efficiency while reducing environmental impact.
Patent Information
- Application Number
- JP2024527389
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-10
- Filing Date
- 2022-11-08
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional chemical-mechanical planarization (CMP) processes using polyurethane polishing pads are costly due to frequent replacement and irregularity issues, leading to variable removal rates and environmental waste, with expensive pads and conditioners contributing to high operational costs and environmental health concerns.
The use of non-porous solid polishing pads with micron-sized polyurethane beads and a specialized CMP slurry composition, including abrasive particles, dispersants, and oxidizing agents, to enhance process stability and reduce waste by minimizing pad and conditioner consumption.
This approach reduces waste generation, stabilizes process conditions, and lowers operational costs by extending pad life, while maintaining high removal rates and reducing irregularities, thus improving the efficiency and sustainability of CMP processes.
Smart Images

Figure 2024544897000001 
Figure 2024544897000002 
Figure 2024544897000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority under 35 USC § 119(e) to earlier-filed U.S. Provisional Application No. 63 / 277,914, filed November 10, 2021, which is incorporated herein by reference in its entirety. [Background technology]
[0002] The present invention relates generally to novel pad-in-a-bottle (PIB) technology and PIB-based advanced chemical-mechanical planarization (CMP) slurries, systems and processes. Specifically, the present invention relates to PIB technology for use with PIB-based Cu and Through Silicon Vias (TSV) CMP slurries, systems and processes.
[0003] Reducing the cost of ownership of expensive polyurethane polishing pads is very important for the semiconductor industry in the CMP process. In the present invention, a cost-effective non-porous solid polishing pad is used to replace the expensive porous polishing pad using PIB type Cu and TSV CMP slurry.
[0004] In CMP, the irregularities on the polyurethane (PU) pad are irreversibly deformed by the wafer contact and also worn away by the composition particles. Therefore, to ensure the process stability, the pad surface needs to be continuously renewed with diamond disks. Because the diamond disks need to cut the pad surface to remove the old irregularities and create new ones, they also gradually thin the pad, forcing its replacement.
[0005] In Cu and TSV CMP, a porous on polyurethane (PU) pad is required to facilitate wafer contact. Moreover, the surface of the pad is constantly worn away by the composition particles. Therefore, to ensure process stability, the pad surface needs to be continuously renewed with a diamond disk, because the diamond disk needs to cut the pad surface to remove the old irregularities and create new ones, which gradually thins the pad and forces its replacement.
[0006] Therefore, conventional CMP has several weaknesses, such as (a) a large amount of waste generated (due to frequent replacement of pads and conditioners), (b) difficult-to-control pad topography causing highly variable contact area distribution, which results in removal rate (RR) variations and adversely affects wafer-level topography among others, and (c) a large amount of expensive polishing pads is consumed.
[0007] This invention discloses a new and novel pad-in-bottle (PIB) technology for advanced node copper and TSV CMP compositions, systems and processes, and related PIB-based Cu CMP slurries, developed using cost-effective, non-porous, solid polishing pads to meet the challenging requirements. Summary of the Invention
[0008] This need is met by using the disclosed compositions, methods, non-porous solid polishing pads and planarization systems for CMP of copper and TSV substrates.
[0009] In one embodiment, a CMP polishing composition is provided. The CMP polishing composition comprises: Abrasive particles; micron-sized polyurethane (PU) beads having a size in the range of 2-100 μm, 10-80 μm, 20-70 μm, or 30-50 μm; a silicone-containing dispersant; A liquid carrier such as water; and optionally, a chelating agent, a dual chelating agent, or a tri-chelating agent; A corrosion inhibitor; an organic quaternary ammonium salt; A biocide; A pH adjuster, and an oxidizing agent added at the time of use; The pH of the composition is 3.0 to 12.0, 5.5 to 8.0, or 6.0 to 7.5.
[0010] In another aspect, a CMP polishing method is provided, comprising: Providing a semiconductor substrate having a surface containing copper or through silicon via (TSV) copper; To provide a cost-effective non-porous solid polishing pad; Providing a chemical mechanical polishing (CMP) formulation as described above; contacting a surface of a semiconductor substrate with a non-porous solid polishing pad and a chemical-mechanical polishing formulation; polishing the surface of the semiconductor; At least a portion of the surface containing the Cu film is in contact with both the polishing pad and the chemical-mechanical polishing formulation.
[0011] In yet another aspect, a CMP polishing system is provided, comprising: a semiconductor substrate having a surface containing copper or through silicon via (TSV) copper; To provide a non-porous, cost-effective solid polishing pad; Providing a PIB type chemical mechanical polishing (CMP) formulation according to the preceding claims, At least a portion of the surface containing the Cu film is in contact with both the solid polishing pad and the chemical-mechanical polishing formulation.
[0012] The abrasive particles are nano-sized particles and include, but are not limited to, colloidal silica, colloidal silica particles doped with other metal oxides within the colloidal silica lattice, colloidal aluminum oxide selected from the group consisting of alpha, beta, and gamma aluminum oxide, colloidal photoactive titanium dioxide, cerium oxide (ceria), colloidal cerium oxide, zirconium oxide (zirconia), nano-sized diamond particles, nano-sized silicon nitride particles, mono-, bi-, or multi-modal colloidal abrasive particles, organic polymer-based soft abrasives, surface coated or modified abrasives, and mixtures thereof, or other composite particles, and mixtures thereof.
[0013] The preferred abrasive particle is colloidal silica.
[0014] Silicone-containing dispersants include, but are not limited to, silicone polyethers that contain both a water-insoluble silicone backbone and several water-soluble polyether pendant groups, such as ethylene oxide (EO) and propylene oxide (PO) repeating units (EO-PO) functional groups, that provide surface wetting properties.
[0015] Corrosion inhibitors include, but are not limited to, the family of heteroaromatic compounds containing one or more nitrogen atoms in the aromatic ring, such as 1,2,4-triazole, amitrole (3-amino-1,2,4-triazole), benzotriazole and its derivatives, tetrazole and its derivatives, imidazole and its derivatives, benzimidazole and its derivatives, pyrazole and its derivatives, and tetrazole and its derivatives.
[0016] Chelating agents (or chelators) include, but are not limited to, amino acids, amino acid derivatives, and organic amines.
[0017] Amino acids and amino acid derivatives include, but are not limited to, glycine, D-alanine, L-alanine, DL-alanine, beta-alanine, valine, leucine, isoleucine, phenylamines, proline, serine, threonine, tyrosine, glutamine, asparagine, glutamic acid, aspartic acid, tryptophan, histidine, arginine, lysine, methionine, cysteine, iminodiacetic acid, and combinations thereof.
[0018] Organic amines include, but are not limited to, 2,2-dimethyl-1,3-propanediamine and 2,2-dimethyl-1,4-butanediamine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and the like.
[0019] An organic diamine compound having two primary amine moieties can be described as a binary chelating agent.
[0020] Biocides include, but are not limited to, Kathon™, Kathon™ CG / ICP II from Dow Chemical Co. They have active ingredients of 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-4-isothiazolin-3-one.
[0021] Oxidizing agents include, but are not limited to, periodic acid, hydrogen peroxide, potassium iodate, potassium permanganate, ammonium persulfate, ammonium molybdate, ferric nitrate, nitric acid, potassium nitrate, and mixtures thereof.
[0022] Organic quaternary ammonium salts as Cu removal rate accelerators and defect reducers include, but are not limited to, choline salts with various counterions such as choline bicarbonate, choline hydroxide, choline dihydrogen citrate salts, choline ethanolamine, choline bitartrate, etc.
[0023] pH adjusters include, but are not limited to, the following: nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and mixtures thereof. pH adjusters also include basic pH adjusters, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic amines, and other chemical reagents that can be used to adjust the pH to a more alkaline direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] This application discloses a PIB type Cu CMP slurry in which a cost-effective non-porous solid pad can be used in the Cu CMP process, in which the role of pad asperities is fulfilled by high-quality micron-sized polyurethane (PU) beads with sizes ranging from 2-100 μm, 10-80 μm, 20-70 μm, or 30-50 μm, which are comparable to the sizes of pores and asperities in commercial polishing pads.
[0025] The beads are suspended in a Cu CMP polishing composition having abrasive particles such as calcined ceria, colloidal silica, or composite particles with the aid of a dispersing agent that disperses the polyurethane beads in the aqueous composition.
[0026] The beads contact the wafer surface by means described below and facilitate polishing in much the same way as conventional asperities.
[0027] By selecting both the size of the beads and their concentration in the composition, much better control of the height, curvature, and areal density of the "peaks" that contact the wafer is achieved, significantly reducing the process variations associated with traditional asperity contacts.
[0028] The use of beads still requires a second surface, or counter surface, for the abrasion to occur, which in our case continues to be a conventional polyurethane-based pad, but one that requires minimal conditioning since it is no longer the primary surface on which abrasion occurs. Alternatively, an inexpensive, partially conditioned pad can be used as the counter surface.
[0029] A polisher may use two to three pads and conditioners simultaneously. The end of life of a pad and conditioning disk is typically reached after only two days of continuous use. Thus, since each platen in a CMP tool uses hundreds of pads and conditioners per year, and a wafer fabrication facility can have dozens of tools (including two or three platens for each tool), the total cost of just the pads and pad conditioners becomes substantial. Thus, the use of highly cost-effective non-porous solid pads instead of porous and expensive polishing pads provides significant cost reduction in the semiconductor device fabrication process.
[0030] Since it can take several hours to remove a used pad and install and qualify a new one, engineering and product losses due to tool downtime and the consumables used to qualify the new pad are also significant. The used PU pads and discarded diamond disc conditioner represent waste products from the CMP process that pose several Environmental Health and Safety (EHS) issues.
[0031] For polishing pads, only about two-thirds of the pad thickness is used before the pad needs to be stripped and discarded. For conditioners, only a few hundred of the tens of thousands of diamonds control the product life, after which the conditioner needs to be discarded. Furthermore, pads and conditioners do not have regeneration or reuse options available. Our work provides a novel solution to the current standard CMP process by addressing the above EHS issues and eliminating the use of many pads and diamond disk conditioners.
[0032] The polyurethane beads used in the disclosed polishing composition have a size ranging from 2 to 100 μm, 10 to 80 μm, 20 to 70 μm, or 30 to 50 μm.
[0033] Some specific aspects of the invention are outlined below.
[0034] In one embodiment, a CMP polishing composition is provided. Aspect 1: An abrasive; Micron-sized polyurethane (PU) beads, a silicone-containing dispersant; A liquid carrier such as water; and optionally a chelating agent, a dual chelating agent, or a tri-chelating agent; A corrosion inhibitor; an organic quaternary ammonium salt; A biocide; A pH adjuster, and an oxidizer added at the time of use, The CMP polishing composition, wherein the pH of the composition is 3.0 to 12.0, 4.0 to 10.0, 5.5 to 8.0, or 6.0 to 7.5.
[0035] Aspect 2: Providing a semiconductor substrate having a surface containing copper or TSV copper; Providing a non-porous, solid, cost-effective polishing pad; Providing a chemical mechanical polishing (CMP) formulation as described above; contacting a surface of a semiconductor substrate with a non-porous solid polishing pad and a chemical-mechanical polishing formulation; and polishing a surface of a semiconductor, comprising: The method, wherein at least a portion of the surface containing the Cu film is in contact with both the polishing pad and the chemical mechanical polishing formulation.
[0036] Aspect 3: A semiconductor substrate having a surface containing a Cu film; To provide a non-porous and inexpensive solid polishing pad; Providing a chemical mechanical polishing (CMP) formulation according to any of the preceding claims, A CMP polishing system, wherein at least a portion of the surface containing the Cu film is in contact with both a polishing pad and a chemical mechanical polishing formulation.
[0037] The abrasive particles are nano-sized particles and include, but are not limited to, colloidal silica, colloidal silica particles doped with other metal oxides within the colloidal silica lattice, colloidal aluminum oxide selected from the group consisting of alpha, beta, and gamma aluminum oxide, colloidal photoactive titanium dioxide, cerium oxide (ceria), colloidal cerium oxide, zirconium oxide (zirconia), nano-sized diamond particles, nano-sized silicon nitride particles, mono-, bi-, or multi-modal colloidal abrasive particles, organic polymer-based soft abrasives, surface coated or modified abrasives, and mixtures thereof, or other composite particles, and mixtures thereof.
[0038] The preferred abrasive particles are colloidal silica.Colloidal silica can be produced from silicate, and high-purity colloidal silica can be produced from TEOS or TMOS.Colloidal silica or high-purity colloidal silica can have a narrow or wide particle size distribution, monomodal or multimodal, various sizes, and various shapes, such as spherical, cocoon, aggregate, and other shapes.
[0039] The nano-sized particles can also have a variety of shapes, such as spherical, cocoon-shaped, aggregate-shaped, and the like.
[0040] The particle size of the abrasive used in the Cu CMP slurry is in the range of 5 nm to 500 nm, 10 nm to 250 nm, or 25 nm to 100 nm.
[0041] The Cu CMP polishing composition comprises 0.0025% to 25% by weight of an abrasive, 0.0025% to 2.5% by weight, or 0.005% to 1.5% by weight of an abrasive.
[0042] The CMP polishing composition includes a silicone-containing dispersant for dispersing polyurethane beads in an aqueous solution, the silicone-containing dispersant also functioning as a surface wetting agent dispersant.
[0043] Silicone-containing dispersants include, but are not limited to, silicone polyethers that contain both a water-insoluble silicone backbone and some water-soluble polyether pendant groups, such as repeating units of EO-PO functionality that provide surface wetting properties.
[0044] Examples of silicone-containing dispersants include silsurf® E608, silsurf® J208-6, silsurf® A208, silsurf® CR1115, silsurf® A204, silsurf® A004-UP, silsurf® A008-UP, silsurf® B608, silsurf® C208, silsurf® C410, silsurf® D208, silsurf® D208, silsurf® D208-30, silsurf® Di-1010, s silsurf® Di-1510, silsurf® Di-15-I, silsurf® Di-2012, silsurf® Di-5018-F, silsurf® G8-I, silsurf® J1015-O, silsurf® J1015-O-AC, silsurf® J208, silsurf® J208-6, siltech® OP-8, siltech® OP-11, siltech® OP-12, siltech® OP-15, siltech® OP-20; products from Siltech Corporation; 225 Wicksteed Avenue, Toronto Ontario, Canada M4H 1G5.
[0045] The concentration range of the silicone-containing dispersant is 0.001% by mass to 2.0% by mass, 0.002% by mass to 1.0% by mass, or 0.005% by mass to 0.5% by mass.
[0046] The CMP slurry contains polyurethane beads of various sizes.
[0047] The concentration range of the polyurethane beads is 0.01% by mass to 2.0% by mass, 0.025% by mass to 1.0% by mass, or 0.05% by mass to 0.5% by mass.
[0048] Organic quaternary ammonium salts as Cu removal rate accelerators and defect reducers include, but are not limited to, choline salts, such as choline bicarbonate, or any other salt formed between choline and other anionic counterions.
[0049] The CMP slurry contains 0.005% by mass to 0.5% by mass, 0.001% by mass to 0.25% by mass, or 0.002% by mass to 0.1% by mass of a quaternary ammonium salt.
[0050] Chelating agents (or chelators) include, but are not limited to, amino acids, amino acid derivatives, and organic amines.
[0051] Amino acids and amino acid derivatives include, but are not limited to, glycine, D-alanine, L-alanine, DL-alanine, beta-alanine, valine, leucine, isoleucine, phenylamines, proline, serine, threonine, tyrosine, glutamine, asparagine, glutamic acid, aspartic acid, tryptophan, histidine, arginine, lysine, methionine, cysteine, iminodiacetic acid, and combinations thereof.
[0052] Organic amines include, but are not limited to, 2,2-dimethyl-1,3-propanediamine and 2,2-dimethyl-1,4-butanediamine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and the like.
[0053] An organic diamine compound having two primary amine moieties can be described as a binary chelating agent.
[0054] The CMP slurry contains 0.1% to 18%, 0.5% to 15%, or 1.0% to 10.0% by mass of at least one chelator, dual chelator, or tri-chelator.
[0055] The corrosion inhibitor may be any known reported corrosion inhibitor.
[0056] Corrosion inhibitors include, but are not limited to, the family of heteroaromatic compounds containing one or more nitrogen atoms in the aromatic ring, such as, for example, 1,2,4-triazole, amitrole (3-amino-1,2,4-triazole), benzotriazole and its derivatives, tetrazole and its derivatives, imidazole and its derivatives, benzimidazole and its derivatives, pyrazole and its derivatives, and tetrazole and its derivatives.
[0057] The CMP slurry contains 0.001% by mass to 1.0% by mass, 0.005% by mass to 0.5% by mass, or 0.01% by mass to 0.25% by mass of a corrosion inhibitor.
[0058] A biocide having an active ingredient to provide a more stable shelf life for the Cu chemical mechanical polishing composition can be used.
[0059] Biocides include, but are not limited to, Kathon™, Kathon™ CG / ICP II from Dow Chemical Co., which have active ingredients of 5-chloro-2-methyl-4-isothiazolin-3-one and / or 2-methyl-4-isothiazolin-3-one.
[0060] The CMP slurry contains 0.0001% to 0.05%, 0.0001% to 0.025%, or 0.0001% to 0.01% by weight of a biocide.
[0061] Acidic or basic compounds or pH adjusters can be used to make it possible to adjust the pH of the CMP polishing composition to an optimized pH value.
[0062] pH adjusters include, but are not limited to, the following: nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and mixtures thereof, as well as other chemical reagents that can be used to adjust the pH to a more acidic direction. pH adjusters also include basic pH adjusters, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic amines, and other chemical reagents that can be used to adjust the pH to a more alkaline direction.
[0063] The CMP slurry contains 0% to 1% by mass, 0.01% to 0.5% by mass, or 0.1% to 0.25% by mass of a pH adjuster.
[0064] The pH of the Cu polishing composition is from about 3.0 to about 12.0, with a preferred pH range of 5.5 to 8.0, and a most preferred pH range of 6.0 to 7.5.
[0065] A variety of peroxy inorganic or organic oxidizing agents or other types of oxidizing agents can be used to oxidize the metallic copper film to a mixture of copper oxides to allow for rapid reaction with the chelating agents and corrosion inhibitors.
[0066] Oxidizing agents include, but are not limited to, periodic acid, hydrogen peroxide, potassium iodate, potassium permanganate, ammonium persulfate, ammonium molybdate, ferric nitrate, nitric acid, potassium nitrate, and mixtures thereof. A preferred oxidizing agent is hydrogen peroxide.
[0067] The CMP composition contains 0.1% to 10% by mass, 0.25% to 7% by mass, or 0.5% to 5.0% by mass of an oxidizing agent. Experimental Section Parameters: Å: Angstrom - unit of length BP: Back pressure, in psi CMP: chemical mechanical planarization = chemical mechanical polishing CS: Carrier Speed DF: Downforce: pressure applied during CMP, unit: psi min:minutes ml: milliliter mV: millivolt psi: pounds per square inch PS: Platen rotation speed of the polishing tool, unit: rpm (revolutions per minute) SF: flow rate of polishing composition, ml / min Removal rate (RR): Cu RR 1.5psi Measured copper removal rate at 1.5 psi down pressure on a CMP tool Cu RR 2.5psi Measured copper removal rate at 2.5 psi down pressure on a CMP tool Cu RR 3.5psi Measured copper removal rate at 3.5 psi down pressure on a CMP tool
[0068] General Experimental Procedures Unless otherwise indicated, all percentages in compositions are percentages by weight.
[0069] In the examples given below, CMP experiments were performed using the procedures and experimental conditions given below. The CMP tool used in the examples was a 300 mm APD-800® polisher manufactured by Fujikoshi Machinery Corporation (Nagano Japan). The pad was broken in by polishing 25 dummy oxide (deposited by plasma-enhanced CVD from a TEOS precursor, PETEOS) wafers. To qualify the tool settings and pad break-in, two PETEOS monitors were polished at baseline conditions with Syton® OX-K colloidal silica supplied by the Planarization Platform of Versum Materials, Inc. The polishing experiments were performed using blanket Cu wafers and Cu MIT854 200 mm patterned wafers. These blanket wafers were purchased from Silicon Valley Microelectronics, 1150 Campbell Ave, CA, 95126.
[0070] Polishing pads supplied by Kuraray Corporation of Japan, i.e., non-porous solid CH34 pad or CH52 pad, were used on the platen for the blanket wafer polishing study. Polishing pads supplied by Thomas West Inc., 470 Mercury Drive, Sunnyvale, CA 94085, USA, non-porous solid pad TWI 312HTG, were used on the platen for the blanket wafer polishing study. EXAMPLES
[0071] The reference (Ref.) non-PIB Cu CMP polishing composition was composed of 5.20 wt. % glycine, 2.40 wt. % alanine, 0.016 wt. % amitrole, 0.0231 wt. % choline bicarbonate, 0.0016 wt. % Neolone M10 biocide, 0.2705 wt. % high purity colloidal silica particles, and 0.050 wt. % Silsurf E608 as a dispersant.
[0072] Silsurf E608, which contains EO-PO wetting functionality, was used as the silicone-containing dispersant.
[0073] The test sample PIB-type Cu CMP polishing composition was composed of 5.20 wt.% glycine, 2.40 wt.% alanine, 0.016 wt.% amitrole, 0.0231 wt.% choline bicarbonate, 0.0016 wt.% Neolone M10 biocide, 0.2705 wt.% high purity colloidal silica particles, and 0.050 wt.% Silsurf E608 as a dispersant, and 0.10 wt.% 35 micron sized polyurethane beads.
[0074] 2.5 wt % H2O2 was added to the CMP composition at the time of use.
[0075] Both the reference and test polishing compositions had a pH of about 7.20.
[0076] In the following examples, two non-porous, inexpensive solid pads, CH34 and CH52, were used. Examples 1-3 were carried out on a first CH34 pad. The same measurements were carried out in Examples 4-6 using a second CH52 pad.
[0077] Example 1 Cu removal using CH34 non-porous solid pad These non-PIB and PIB Cu CMP polishing compositions and the first CH34 pad were used to test the Cu removal rate, and the results are listed in Table 1. [Table 1]
[0078] As shown in the Cu removal rate results in Table 1, the Cu removal rate was increased for the PIB-Cu polishing composition relative to the non-PIB-Cu polishing composition under three different applied down forces times three different sliding velocities, which demonstrated one important advantage of using the PIB-type Cu polishing composition on a less expensive non-porous solid polishing pad relative to the non-PIB Cu polishing composition.
[0079] Example 2: Friction coefficient when using CH34 non-porous solid pad The coefficient of friction (COF) using these non-PIB and PIB Cu CMP polishing compositions and the results are compared in Table 2. [Table 2]
[0080] As shown in the COF comparison results in Table 2, the COF was decreased for the PIB-Cu polishing composition relative to the non-PIB-Cu polishing composition under three different applied down forces times three different sliding velocities, which demonstrated another important advantage of using the PIB-type Cu polishing composition on a less expensive non-porous solid polishing pad relative to the non-PIB Cu polishing composition.
[0081] Example 3 Cu dishing when using a CH34 non-porous solid polishing pad A 200 mm Cu patterned wafer was polished under a down force of 2.5 psi and a sliding speed of 1.6 m / s using a non-PIB Cu polishing composition as a reference sample and a PIB type Cu polishing composition as a test sample.
[0082] A comparison of Cu line dishing for six different sizes of Cu line features is compared in Table 3. [Table 3]
[0083] As shown in the Cu line dishing comparison results in Table 3, Cu line dishing was reduced with the PIB-Cu polishing composition relative to the non-PIB Cu polishing composition across all six different Cu line features, which demonstrated a third important advantage of using a PIB-type Cu polishing composition on a less expensive non-porous solid polishing pad relative to a non-PIB Cu polishing composition to achieve lower Cu line dishing performance with a PIB-type Cu CMP slurry.
[0084] In general, using a non-porous, inexpensive, and non-porous solid CH34 polishing pad, the PIB-type Cu CMP polishing compositions provided higher Cu film removal rates, slightly lower average COFs, and reduced Cu line dishing across all tested Cu line features than those from the non-PIB Cu polishing compositions.
[0085] Example 4 Cu removal using CH52 non-porous solid pad These two non-PIB and PIB Cu CMP polishing compositions were used to test the Cu removal rate on a second non-porous, inexpensive solid CH52 pad. The results are listed in Table 4. [Table 4]
[0086] As with the Cu removal rate results shown in Table 4 using the second CH52 pad, Table 4 provided consistent results using the second CH52 pad as did those Cu removal rate results obtained using the first CH34 pad.
[0087] Example 5: Friction coefficient when using CH52 non-porous solid pad The coefficient of friction (COF) of these two non-PIB and PIB Cu CMP polishing compositions when used with a CH52 polishing pad was compared, and the results are compared in Table 5. [Table 5]
[0088] Like the COF comparison results shown in Table 2 using the first CH52 pad, Table 5 provided consistent results using the second CH52 polishing pad, as did these Cu coefficient of friction results obtained using the first CH34 pad.
[0089] Example 6 Cu dishing when using CH52 non-porous solid pad A 200 mm Cu patterned wafer was polished using a second non-porous solid CH52 polishing pad under conditions of 2.5 psi down force and 1.6 m / s sliding speed using a non-PIB Cu polishing composition as a reference sample and a PIB type Cu polishing composition as a test sample.
[0090] A comparison of Cu line dishing for six different sizes of Cu line features is compared in Table 6. [Table 6] As shown in the Cu line dishing comparison results shown in Table 6 using the second CH52 pad, Table 6 provides consistent results using the second CH52 solid polishing pad as those Cu line dishing results obtained using the first CH34 pad.
[0091] Example 7 Cu Removal Using TWI 312HTG Non-Porous Solid Pad These two non-PIB and PIB Cu CMP polishing compositions were used to test Cu removal rates on a third non-porous, inexpensive solid Thomas West CMP polishing pad (TWI 312HTG). The results are listed in Table 7. [Table 7]
[0092] As shown in the Cu removal rate results shown in Table 7 using the third Thomas West polishing pad, the Cu removal rate increased significantly under different sliding speed conditions at a down force of 1.5 psi.
[0093] Example 8: Coefficient of friction using TWI 312HTG non-porous solid pad The coefficient of friction (COF) of these two non-PIB and PIB Cu CMP polishing compositions was compared using a TWI 312HTG polishing pad, and the results are compared in Table 8. [Table 8]
[0094] As shown in the COF comparison results in Table 8 using the third TWI 312HTG non-porous solid polishing pad, the PIB-type Cu CMP slurry with polyurethane beads provided a reduced COF than the COF obtained from using the non-PIB Cu slurry without polyurethane beads under nine different combinations of applied down morphology and sliding speed, which clearly demonstrated the important advantages of using PIB technology and PIB-type Cu CMP slurry in Cu and TSV CMP polishing processes.
[0095] Example 9 Cu dishing when using TWI 312HTG non-porous solid pad A 200 mm Cu patterned wafer was polished using a third TWI 312HTG non-porous solid pad under conditions of 2.5 psi down force and 1.6 m / s sliding speed using the non-PIB Cu polishing composition as the reference sample and the PIB type Cu polishing composition as the test sample.
[0096] A comparison of Cu line dishing for six different sizes of Cu line features is compared in Table 9. [Table 9]
[0097] As shown in the Cu line dishing comparison results shown in Table 9 using the third TWI 312HTG non-porous solid pad, the PIB-based Cu CMP slurry with polyurethane beads provided significantly reduced Cu line dishing across all six tested Cu line features than the Cu line dishing obtained from using the non-PIB Cu slurry without polyurethane beads, which clearly demonstrated the important advantages of using PIB technology and PIB-based Cu CMP slurries in Cu and TSV CMP polishing processes to achieve improved Cu removal rates while at the same time achieving much lower Cu line dishing.
[0098] In summary, the present invention by using non-porous, inexpensive solid CH34 or CH52 polishing pads, PIB-based Cu CMP polishing compositions provided higher Cu film removal rates, slightly lower average COF, and reduced Cu line dishing across all tested Cu line features than those from non-PIB Cu polishing compositions.
[0099] The results listed above have shown one of the advantages of using micron-sized PU beads in PIB-type Cu CMP compositions: Cu removal rate can be increased using non-porous, less expensive solid polishing pads.
[0100] Clearly, when using non-porous, inexpensive solid polishing pads, the PIB-type Cu CMP polishing composition containing PU beads outperforms the Cu polishing composition without PU beads.
[0101] The embodiments of the invention listed above, including the examples, are illustrative of the numerous embodiments that may be made from the present invention. It is contemplated that numerous other configurations of the process may be used and that the materials used in the process may be selected from numerous materials other than those specifically disclosed.
Claims
1. An abrasive; micron-sized polyurethane (PU) beads in the range of 2-100 μm, 10-80 μm, 20-70 μm, or 30-50 μm; a silicone-containing dispersant; At least one chelating agent; A corrosion inhibitor; and optionally an organic quaternary ammonium salt; A biocide; A pH adjuster; and An oxidizing agent added at the time of use; A chemical mechanical polishing (CMP) composition comprising: the pH of the composition is from 3.0 to 12.0, from 5.5 to 8, or from 6.0 to 7.5; A chemical mechanical polishing (CMP) composition, wherein the chelating agent is selected from the group consisting of amino acids, amino acid derivatives, organic amines, and combinations thereof.
2. 2. The CMP composition of claim 1, wherein the abrasive is selected from the group consisting of colloidal silica, colloidal silica particles doped with other metal oxides within the colloidal silica lattice, colloidal aluminum oxide selected from the group consisting of alpha, beta, and gamma aluminum oxide, colloidal photoactive titanium dioxide, cerium oxide, colloidal cerium oxide, zirconium oxide, nano-sized diamond particles, nano-sized silicon nitride particles, mono-modal, bi-modal, or multi-modal colloidal abrasive particles, organic polymer-based soft abrasives, surface coated or modified abrasives, and combinations thereof, and the abrasive is in the range of 0.0025% to 25%, 0.0025% to 2.5%, or 0.005% to 1.5% by weight.
3. 2. The CMP composition of claim 1, wherein the micron-sized polyurethane (PU) beads are in the range of 0.01% to 2.0% by weight, 0.025% to 1.0% by weight, or 0.05% to 0.5% by weight.
4. 2. The CMP composition of claim 1, wherein the silicone-containing dispersant comprises a silicone polyether that contains both a water-insoluble silicone backbone and several water-soluble polyether pendant groups that include repeating units of ethylene oxide (EO) and propylene oxide (PO) (EO-PO) functional groups, and the silicone-containing dispersant ranges from 0.01% to 2.0% by weight, 0.001% to 2.0% by weight, 0.002 to 1.0% by weight, or 0.005% to 0.5% by weight.
5. 2. The CMP composition of claim 1, wherein the at least one chelating agent is selected from the group consisting of glycine, D-alanine, L-alanine, DL-alanine, beta-alanine, valine, leucine, isoleucine, phenylamine, proline, serine, threonine, tyrosine, glutamine, asparagine, glutamic acid, aspartic acid, tryptophan, histidine, arginine, lysine, methionine, cysteine, iminodiacetic acid, 2,2-dimethyl-1,3-propanediamine and 2,2-dimethyl-1,4-butanediamine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations thereof, and the at least one chelating agent is in the range of 0.1% to 18%, 0.5% to 15%, or 1.0% to 10.0% by weight.
6. 2. The CMP composition of claim 1, wherein the corrosion inhibitor is selected from the family of heteroaromatic compounds containing one or more nitrogen atoms in an aromatic ring, such as the group consisting of 1,2,4-triazole, 3-amino-1,2,4-triazole, benzotriazole and its derivatives, tetrazole and its derivatives, imidazole and its derivatives, benzimidazole and its derivatives, pyrazole and its derivatives, and tetrazole and its derivatives, and the corrosion inhibitor is in the range of 0.001% to 1.0%, 0.005% to 0.5%, or 0.01% to 0.25% by weight.
7. 2. The CMP composition of claim 1, wherein the biocide has an active ingredient selected from the group consisting of 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, and combinations thereof, and the biocide is in the range of 0.0001% to 0.05%, 0.0001% to 0.025%, or 0.0001% to 0.01% by weight.
8. 2. The CMP composition of claim 1, wherein the oxidizing agent is selected from the group consisting of periodic acid, hydrogen peroxide, potassium iodate, potassium permanganate, ammonium persulfate, ammonium molybdate, ferric nitrate, nitric acid, potassium nitrate, and mixtures thereof, and the oxidizing agent is in the range of 0.1% to 10%, 0.25% to 7%, or 0.5% to 5.0% by weight.
9. 2. The CMP composition of claim 1, wherein the organic quaternary ammonium salt is selected from the group consisting of choline salts having various counterions selected from the group consisting of choline bicarbonate, choline hydroxide, choline dihydrogen citrate, choline ethanolamine, choline bitartrate, and combinations thereof, and the organic quaternary ammonium salt is in the range of 0.005% to 0.5%, 0.001% to 0.25%, or 0.002% to 0.1% by weight.
10. 2. The CMP composition of claim 1, wherein the pH adjuster is selected from the group consisting of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and other chemical reagents that can be used to adjust the pH in the acidic direction.
11. 2. The CMP composition of claim 1, wherein the pH adjuster is selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic amines, and other chemical reagents that can be used to adjust the pH in an alkaline direction.
12. 2. The CMP composition of claim 1, wherein the CMP composition comprises at least one of a chelating agent selected from the group consisting of glycine, D-alanine, L-alanine, DL-alanine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations; a corrosion inhibitor selected from the group consisting of 3-amino-1,2,4-triazole, 1,2,4-triazole, imidazole and imidazole derivatives, and combinations; choline bicarbonate or choline hydroxide; a biocide; colloidal silica particles; a silicone-containing dispersant; and 30-50 μm polyurethane (PU) beads.
13. 2. The CMP composition of claim 1, wherein the CMP composition comprises glycine and alanine, 3-amino-1,2,4-triazole, ethylenediamine, choline bicarbonate, a biocide, and colloidal silica particles, a silicone-containing dispersant, and 30 μm to 50 μm polyurethane (PU) beads.
14. 1. A method for chemical mechanical polishing a semiconductor substrate, comprising: providing the semiconductor substrate having a surface containing copper or through silicon via (TSV) copper; Providing a non-porous solid polishing pad; Providing a chemical mechanical polishing (CMP) composition according to claim 1; contacting a surface of the semiconductor substrate with the polishing pad and the chemical mechanical polishing composition; and polishing the surface of the semiconductor. The method, wherein at least a portion of the surface containing copper or TSV copper is in contact with both the non-porous, solid polishing pad and the chemical-mechanical polishing composition.
15. 15. The method of claim 14, wherein the abrasive in the CMP composition is selected from the group consisting of colloidal silica, colloidal silica particles doped with other metal oxides within the colloidal silica lattice, colloidal aluminum oxide selected from the group consisting of alpha, beta, and gamma aluminum oxide, colloidal photoactive titanium dioxide, cerium oxide, colloidal cerium oxide, zirconium oxide, nano-sized diamond particles, nano-sized silicon nitride particles, mono-, bi-, or multi-modal colloidal abrasive particles, organic polymer-based soft abrasives, surface-coated or modified abrasives, and mixtures thereof, and the abrasive ranges from 0.0025% to 25%, 0.0025% to 2.5%, or 0.005% to 1.5% by weight.
16. 15. The method of claim 14, wherein the micron-sized polyurethane (PU) beads in the CMP composition range from 0.01% to 2.0% by weight, 0.025% to 1.0% by weight, or 0.05% to 0.5% by weight.
17. 15. The method of claim 14, wherein the silicone-containing dispersant in the CMP composition comprises a silicone polyether containing both a water-insoluble silicone backbone and several water-soluble polyether pendant groups comprising repeating units of ethylene oxide (EO) and propylene oxide (PO) (EO-PO) functional groups, and the silicone-containing dispersant ranges from 0.01% to 2.0% by weight, 0.001% to 2.0% by weight, 0.002 to 1.0% by weight, or 0.005% to 0.5% by weight.
18. 15. The method of claim 14, wherein the at least one chelating agent in the CMP composition is selected from the group consisting of glycine, D-alanine, L-alanine, DL-alanine, beta-alanine, valine, leucine, isoleucine, phenylamine, proline, serine, threonine, tyrosine, glutamine, asparagine, glutamic acid, aspartic acid, tryptophan, histidine, arginine, lysine, methionine, cysteine, iminodiacetic acid, 2,2-dimethyl-1,3-propanediamine and 2,2-dimethyl-1,4-butanediamine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations thereof, and the at least one chelating agent is in the range of 0.1% to 18%, 0.5% to 15%, or 1.0% to 10.0% by weight.
19. 15. The method of claim 14, wherein the corrosion inhibitor in the CMP composition is selected from the family of heteroaromatic compounds containing one or more nitrogen atoms in an aromatic ring, e.g., the group consisting of 1,2,4-triazole, 3-amino-1,2,4-triazole, benzotriazole and its derivatives, tetrazole and its derivatives, imidazole and its derivatives, benzimidazole and its derivatives, pyrazole and its derivatives, and tetrazole and its derivatives, and the corrosion inhibitor is in the range of 0.001% to 1.0%, 0.005% to 0.5%, or 0.01% to 0.25% by weight.
20. 15. The method of claim 14, wherein the biocide in the CMP composition has an active ingredient selected from the group consisting of 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, and combinations thereof, and the biocide ranges from 0.0001% to 0.05%, 0.0001% to 0.025%, or 0.0001% to 0.01% by weight.
21. 15. The method of claim 14, wherein the oxidizing agent in the CMP composition is selected from the group consisting of periodic acid, hydrogen peroxide, potassium iodate, potassium permanganate, ammonium persulfate, ammonium molybdate, ferric nitrate, nitric acid, potassium nitrate, and mixtures thereof, and the oxidizing agent is in the range of 0.1% to 10%, 0.25% to 7%, or 0.5% to 5.0% by weight.
22. 15. The method of claim 14, wherein the organic quaternary ammonium salt in the CMP composition is selected from the group consisting of choline salts having various counterions selected from the group consisting of choline bicarbonate, choline hydroxide, choline dihydrogen citrate salt, choline ethanolamine, choline bitartrate, and combinations thereof, and the organic quaternary ammonium salt is in the range of 0.005% to 0.5%, 0.001% to 0.25%, or 0.002% to 0.1% by weight.
23. 15. The method of claim 14, wherein the pH adjuster in the CMP composition is selected from the group consisting of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and other chemical reagents that can be used to adjust the pH in the acidic direction.
24. 15. The method of claim 14, wherein the pH adjuster in the CMP composition is selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic amines, and other chemical reagents that can be used to adjust the pH in an alkaline direction.
25. 15. The method of claim 14, wherein the CMP composition comprises at least one of a chelating agent selected from the group consisting of glycine, glycine, D-alanine, L-alanine, DL-alanine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations; the corrosion inhibitor selected from the group consisting of 3-amino-1,2,4-triazole, 1,2,4-triazole, imidazole and imidazole derivatives, and combinations; choline bicarbonate or choline hydroxide; a biocide; colloidal silica particles; a silicone-containing dispersant; and 30-50 μm polyurethane (PU) beads.
26. 15. The method of claim 14, wherein the CMP composition comprises glycine and alanine, 3-amino-1,2,4-triazole, ethylenediamine, choline bicarbonate, a biocide, and colloidal silica particles, a silicone-containing dispersant, and 30 μm to 50 μm polyurethane (PU) beads.
27. 1. A chemical mechanical polishing system comprising: a semiconductor substrate having a surface containing copper or through-strip via (TSV) copper; Providing a non-porous solid polishing pad; Providing the chemical mechanical polishing (CMP) composition of claim 1; A system wherein at least a portion of the surface containing copper or TSV copper is in contact with both the polishing pad and the chemical-mechanical polishing composition.
28. 28. The system of claim 27, wherein the abrasive in the CMP composition is selected from the group consisting of colloidal silica, colloidal silica particles doped with other metal oxides within the colloidal silica lattice, colloidal aluminum oxide selected from the group consisting of alpha, beta, and gamma aluminum oxide, colloidal photoactive titanium dioxide, cerium oxide, colloidal cerium oxide, zirconium oxide, nano-sized diamond particles, nano-sized silicon nitride particles, mono-, bi-, or multi-modal colloidal abrasive particles, organic polymer-based soft abrasives, surface coated or modified abrasives, and mixtures thereof, and the abrasive ranges from 0.0025% to 25%, 0.0025% to 2.5%, or 0.005% to 1.5% by weight.
29. 28. The system of claim 27, wherein the micron-sized polyurethane (PU) beads in the CMP composition range from 0.01% to 2.0% by weight, 0.025% to 1.0% by weight, or 0.05% to 0.5% by weight.
30. 28. The system of claim 27, wherein the silicone-containing dispersant in the CMP composition comprises a silicone polyether containing both a water-insoluble silicone backbone and several water-soluble polyether pendant groups comprising repeating units of ethylene oxide (EO) and propylene oxide (PO) (EO-PO) functional groups, and the silicone-containing dispersant ranges from 0.001% to 2.0%, 0.002 to 1.0%, or 0.005% to 0.5% by weight.
31. 28. The system of claim 27, wherein the at least one chelating agent in the CMP composition is selected from the group consisting of glycine, D-alanine, L-alanine, DL-alanine, beta-alanine, valine, leucine, isoleucine, phenylamine, proline, serine, threonine, tyrosine, glutamine, asparagine, glutamic acid, aspartic acid, tryptophan, histidine, arginine, lysine, methionine, cysteine, iminodiacetic acid, 2,2-dimethyl-1,3-propanediamine and 2,2-dimethyl-1,4-butanediamine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations thereof, and the at least one chelating agent is in the range of 0.1% to 18%, 0.5% to 15%, or 1.0% to 10.0% by weight.
32. 28. The system of claim 27, wherein the corrosion inhibitor in the CMP composition is selected from the family of heteroaromatic compounds containing one or more nitrogen atoms in an aromatic ring, e.g., the group consisting of 1,2,4-triazole, 3-amino-1,2,4-triazole, benzotriazole and its derivatives, tetrazole and its derivatives, imidazole and its derivatives, benzimidazole and its derivatives, pyrazole and its derivatives, and tetrazole and its derivatives, and the corrosion inhibitor is in the range of 0.001% to 1.0%, 0.005% to 0.5%, or 0.01% to 0.25% by weight.
33. 28. The system of claim 27, wherein the biocide in the CMP composition has an active ingredient selected from the group consisting of 5-chloro-2-methyl-4-isothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, and combinations thereof, and the biocide ranges from 0.0001% to 0.05%, 0.0001% to 0.025%, or 0.0001% to 0.01% by weight.
34. 28. The system of claim 27, wherein the oxidizing agent in the CMP composition is selected from the group consisting of periodic acid, hydrogen peroxide, potassium iodate, potassium permanganate, ammonium persulfate, ammonium molybdate, ferric nitrate, nitric acid, potassium nitrate, and mixtures thereof, and the oxidizing agent is in the range of 0.1% to 10%, 0.25% to 7%, or 0.5% to 5.0% by weight.
35. 28. The system of claim 27, wherein the organic quaternary ammonium salt in the CMP composition is selected from the group consisting of choline salts having various counterions selected from the group consisting of choline bicarbonate, choline hydroxide, choline dihydrogen citrate, choline ethanolamine, choline bitartrate, and combinations thereof, and the organic quaternary ammonium salt is in the range of 0.005% to 0.5%, 0.001% to 0.25%, or 0.002% to 0.1% by weight.
36. 28. The system of claim 27, wherein the pH adjuster in the CMP composition is selected from the group consisting of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and other chemical reagents that can be used to adjust the pH in the acidic direction.
37. 28. The system of claim 27, wherein the pH adjuster in the CMP composition is selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic amines, and other chemical reagents that can be used to adjust the pH in an alkaline direction.
38. 28. The system of claim 27, wherein the CMP composition comprises at least one of a chelating agent selected from the group consisting of glycine, glycine, D-alanine, L-alanine, DL-alanine, ethylenediamine, 1,3-diaminepropane, 1,4-diaminebutane, and combinations; a corrosion inhibitor selected from the group consisting of 3-amino-1,2,4-triazole, 1,2,4-triazole, imidazole and imidazole derivatives, and combinations; choline bicarbonate or choline hydroxide; a biocide; colloidal silica particles; a silicone-containing dispersant; and 30-50 μm polyurethane (PU) beads.
39. 28. The system of claim 27, wherein the CMP composition comprises glycine and alanine, 3-amino-1,2,4-triazole, ethylenediamine, choline bicarbonate, a biocide, and colloidal silica particles, a silicone-containing dispersant, and 30 μm to 50 μm polyurethane (PU) beads.