Energy Storage Device

The use of high aspect ratio carbon elements with polyamide binders in lithium-ion battery electrodes addresses the environmental and mechanical limitations of conventional binders, enhancing energy density and charging speed.

JP2024544917APending Publication Date: 2024-12-05FASTCAP SYSTEMS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024527515
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-12
Filing Date
2022-11-14
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional lithium-ion battery binders are not environmentally friendly and require toxic solvents for processing, and they fail to maintain mechanical integrity during battery expansion and contraction.

Method used

The use of a network of high aspect ratio carbon elements with polyamide-based binders in the anode and cathode, which includes silicon and NMC/NCA active materials, respectively, to form electrodes that are environmentally friendly and maintain mechanical stability during charging and discharging.

Benefits of technology

The solution enhances the mechanical and electrical properties of the electrodes, allowing for higher energy density and faster charging capabilities while reducing environmental impact and manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544917000001_ABST
    Figure 2024544917000001_ABST
Patent Text Reader

Abstract

An anode is disclosed herein, the anode comprising: a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network; an active layer comprising: a plurality of electrode active material particles disposed in the voids within the network and comprising silicon; and a polymeric additive that is at least one of (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides. Also disclosed herein, the cathode comprises: a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network; an active layer comprising: a plurality of electrode active material particles disposed in the voids within the network and a polymeric additive that is at least one of (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Application No. 63 / 278,782, filed November 12, 2021, the entire disclosure of which is incorporated herein by reference.

[0002] The present invention relates to energy storage devices, particularly ultracapacitors and lithium ion batteries, and electrodes used therein. [Background technology]

[0003] Lithium batteries are used in many products, including medical devices, electric vehicles, aircraft, and consumer products such as laptop computers, cell phones, cameras, etc. Due to their high energy density, high operating voltage, and low self-discharge, lithium-ion batteries have dominated the secondary battery market and continue to find new applications in products and developing industries.

[0004] Generally, a lithium ion battery ("LIB" or "LiB") includes an anode, a cathode, and an electrolyte material, such as an organic solvent containing a lithium salt. More specifically, the anode and cathode (collectively referred to as "electrodes") are formed by mixing either the anode or cathode active material with a binder and a solvent to form a paste or slurry, which is then coated onto a current collector, such as aluminum or copper, and dried to form a film on the current collector. The anode and cathode are then layered or coiled and contained within a pressurized casing that contains the electrolyte material, which collectively form a lithium ion battery.

[0005] The binder serves to adhere the active material to the current collector with a suitable coating. It is important that the binder facilitates maintaining sufficient contact between the active material and the current collector. Additionally, it is important to select a binder that is mechanically compatible with the electrode active material(s) so that it can withstand the degree of expansion and contraction of the electrode active material(s) during charging and discharging of the battery. The binder must also be sufficient to withstand the manipulation of the electrode as it is fitted into the battery casing.

[0006] Therefore, binders such as cellulosic or cross-linked polymeric binders have been used to provide good mechanical properties, however, in conventional electrodes the binders selected are generally environmentally unfriendly or require toxic solvents for processing. Summary of the Invention [Means for solving the problem]

[0007] Disclosed herein is an anode comprising: a network of high aspect ratio carbon elements that define voids within the network; an active layer comprising a plurality of electrode active material particles disposed in the voids within the network and comprising silicon; and a polymeric additive that is at least one of: (i) selected from the family of polyamides; or (ii) modified polyamides or derivatives of polyamides.

[0008] Also disclosed herein is a cathode, the cathode comprising: an active layer comprising a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network; a plurality of electrode active material particles disposed in the voids within the network; and a polymeric additive that is at least one of: (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.

[0009] The following is a brief description of the drawings, in which like elements are numbered likewise, which are presented for the purpose of illustrating, and not for the purpose of limiting, the exemplary embodiments disclosed herein. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 illustrates an example of an electrode disclosed herein. [Figure 2A] 1 is a flow chart illustrating an example of a method that can be used to manufacture the electrodes disclosed herein. [Figure 2B] 1 is a flow chart illustrating an exemplary method of manufacturing an anode for an energy storage device. [Diagram 3] FIG. 13 is a diagram showing the electrode arrangement in a pouch cell device. [Figure 4] FIG. 1 is a schematic cross-sectional view illustrating an embodiment of an energy storage device (ESD). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The components, processes, and devices disclosed herein can be more fully understood by referring to the accompanying drawings. These figures are merely schematic diagrams for convenience and ease of demonstration of the present disclosure, and are therefore not intended to illustrate the relative sizes and dimensions of the devices or their components, and / or to define or limit the scope of the exemplary embodiments. Although specific terms are used in the following description for clarity, these terms are intended to refer only to the specific structures of the embodiments selected for illustration in the drawings, and are not intended to define or limit the scope of the present disclosure. It should be understood that in the drawings and the following description, like number designations refer to components of similar function.

[0012] Disclosed herein is an electrolytic cell that includes a housing that contains electrodes (anode and cathode). The housing contains an electrolyte in contact with the anode and cathode. Both electrodes (anode and cathode) include current collectors on which an active layer is disposed. The active layer may be disposed on an optional adhesive layer in contact with the electrodes.

[0013] 1 is a diagram of an example of an electrode (anode or cathode) disclosed herein. In the illustrated example, the electrode 100 includes a current collector 102 and an active layer 106. The electrode 100 may optionally include an adhesion layer 104. By way of example, the adhesion layer 104 includes a material that promotes adhesion between the current collector 102 and the active layer 106. The active layer 106 includes an electrode active material 110 in a binder and a conductive element 108. The conductive element may include a high aspect ratio element.

[0014] The current collector 102 is a conductive element. The current collector can include a metal (e.g., a substantially pure metal or a metal alloy). As another example, the current collector 102 can be in the form of a metal strip or foil. For example, the current collector 102 can be an aluminum foil or strip, an aluminum alloy foil or strip, a copper foil or strip, or a copper alloy foil or strip. The current collector 102 can have a thickness of 15 μm (microns) or less, 10 μm or less, 8 μm or less, or 5 μm or less. In some embodiments, the current collector can have a thickness of at least 3 μm. For example, the current collector 102 can have a thickness of 3 to 15 μm, preferably 6 to 10 μm. As another example, the current collector 102 is an aluminum or aluminum alloy foil having a thickness of 5 to 7 μm.

[0015] The active layer 106 includes a conductive material, a binder material, and an electrode active material. The active layer can be made by mixing the conductive material, the binder material, and the electrode active material with a solvent to form a mixture. The mixture can be applied directly to the current collector or onto an adhesive layer that can adhere to the current collector. If an adhesive layer is used, it can be conductive. The mixture can be dried to remove the solvent, leaving a solid active layer. The anode and cathode active layers 106 will now be described in detail separately.

[0016] The binder material of both the anode and cathode active layers is a polyamide, preferably a water-soluble or alcohol-soluble polyamide. The active material of the anode comprises silicon, while the active material of the cathode is NMC, NCA, NCMA, or a combination thereof.

[0017] anode As mentioned above, the anode includes a conductive element, a binder, and an electrode active material, which are mixed together to form a mixture. The mixture is disposed on a current collector and dried to form an active layer. Each of the components of the anode active material layer is described in more detail below.

[0018] The conductive elements (also referred to as conductive materials) can include carbon. For example, the conductive elements can be high aspect ratio carbon elements. The term "high aspect ratio carbon elements" refers to carbonaceous elements in which the size of one or more dimensions ("major dimension(s)") of the element is significantly greater than the size of the lateral dimensions ("minor dimensions"). High aspect ratio carbon elements can comprise a substantially cylindrical network of carbon atoms. The conductive material can include carbon nanotubes or multiple bundles of carbon nanotubes.

[0019] In one embodiment, the conductive material used in the anode may include graphite flakes, as described below.

[0020] The conductive material can form a conductive percolation network (also referred to herein as a network of high aspect ratio carbon elements) that can transmit electric current between any two distant points located on the surface of the (solvent-free) solid active layer. In other words, physical contact or electronic hopping between the conductive elements in the electrode active layer can transmit electric current from one surface or end of the active layer to the opposite surface or end. The percolation network can include voids between the high aspect ratio carbon elements that can contain or house the electrode active material. The high aspect ratio conductive material can be substantially oriented in the electrode active layer 106 in a direction substantially parallel to the current collector to facilitate the conduction of electric current from one end of the electrode to the other while maintaining some weak orientation throughout the thickness of the active layer.

[0021] The network of high aspect ratio carbon elements includes a first set of carbon nanotubes comprising a plurality of first carbon nanotubes or a plurality of bundles of the first carbon nanotubes, and a second set of carbon nanotubes comprising a plurality of second carbon nanotubes or a plurality of bundles of the second carbon nanotubes, the second set of carbon nanotubes having one or more properties different from the first set of carbon nanotubes. In one embodiment, the first set of carbon nanotubes comprises multi-walled nanotubes and the second set of carbon nanotubes comprises single-walled nanotubes, and the weight ratio of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:1.

[0022] In one embodiment, the first average aspect ratio of the first set of carbon nanotubes is greater than the second average aspect ratio of the second set of carbon nanotubes. In another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes, and the distribution of lengths of the plurality of multi-walled carbon nanotubes is biased toward a nominal length of the multi-walled carbon nanotubes. In another embodiment, the nominal length of the multi-walled carbon nanotubes is at least 15 micrometers.

[0023] In yet another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes, at least 50% of the plurality of multi-walled carbon nanotubes having a length greater than 8 micrometers. In yet another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes, at least 50% of the plurality of multi-walled carbon nanotubes having a length greater than 12 micrometers. In one embodiment, when both the first set of carbon nanotubes and the second set of carbon nanotubes are swollen by an electrolyte, the first set of carbon nanotubes swell more than the second set of carbon nanotubes.

[0024] The conductive material can be present in the mixture in an amount of 0.1 to 2.0, or 0.15 to 1.2, or 0.3 to 1 weight percent (wt%), based on the total weight of the mixture (the mixture including the conductive material, the electrode active material, the binder material, and the solvent). The conductive material can be present in the active layer in an amount of 0.2 to 3.5, or 0.3 to 3, or 0.5 to 2 wt%, based on the total weight of solids in the active layer (the total weight of solids includes the conductive material, the binder material, and the electrode active material, excluding the solvent).

[0025] The high aspect ratio carbon elements can be single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWNTs), multi-walled carbon nanotubes (MWNTs), or a mixture of both.

[0026] The single-walled carbon nanotubes can have an outer diameter of 0.5 to 5.0 nanometers, preferably 1.0 to 3.5 nanometers. The single-walled carbon nanotubes can have an aspect ratio (length to diameter ratio) of greater than about 2.0, preferably greater than 5.0, preferably greater than 10.0, greater than 50, more preferably greater than 100. In an exemplary embodiment, the single-walled carbon nanotubes can have an average aspect ratio of 5 to 200.

[0027] The single-walled carbon nanotubes can have a length of greater than 6 nanometers, preferably greater than 10 nanometers, preferably greater than 15 nanometers, preferably greater than 30 nanometers, preferably greater than 50 nanometers, more preferably greater than 100 nanometers, preferably greater than 1 micrometer, preferably greater than 5 micrometers, preferably greater than 10 micrometers, more preferably greater than 15 micrometers, up to at least 200 micrometers. In an exemplary embodiment, the single-walled carbon nanotubes can have an average length of 10 nanometers to 20 micrometers, preferably 20 nanometers to 15 micrometers.

[0028] The single-walled carbon nanotubes may be present in the mixture of the conductive material, binder material, electrode active material and solvent in an amount of 0.1 to 0.3 wt %, preferably 0.15 to 0.25 wt %, based on the total weight of the mixture.

[0029] The single-walled carbon nanotubes are present in the electrode active layer (the conductive material excluding the solvent, the binder material, and the electrode active material) in an amount of 0.2 to 0.6 wt %, preferably 0.3 to 0.5 wt %, based on the total weight of the electrode active layer.

[0030] The number of carbon walls in a multi-walled carbon nanotube can be 2 or more, 5 or more, 10 or more, or 50 or more. A multi-walled carbon nanotube can contain, on average, 3 to 15 walls, 4 to 12 walls, 5 to 10 walls, or 6 to 8 walls.

[0031] The active layer 106 can include multi-walled carbon nanotubes and single-walled carbon nanotubes. The multi-walled carbon nanotubes swell more than single-walled carbon nanotubes when wetted with an electrolyte in an energy storage device in which the electrode 100 is disposed. For example, the multi-walled carbon nanotubes can swell at least 15%, or at least 25%, or at least 50% more than single-walled carbon nanotubes when wetted with an electrolyte in an energy storage device in which the electrode 100 is disposed. For example, the length of the multi-walled carbon nanotubes can expand at least 15%, or at least 25%, or at least 50% more than the length of single-walled carbon nanotubes when wetted with electrolyte. As another example, the multi-walled carbon nanotubes swell up to 50% when wetted (e.g., the length of the multi-walled carbon nanotubes is 50% larger after wetted with electrolyte and / or the diameter of the multi-walled carbon nanotubes is 50% larger after wetted, etc.).

[0032] The multi-walled carbon nanotubes can have an outer diameter of 2.0 to 50 nanometers, 5.0 to 40 nanometers, or 6 to 10 nanometers. The multi-walled carbon nanotubes can have a length of more than 10 nanometers, more than 15 nanometers, more than 30 nanometers, more than 50 nanometers, more than 100 nanometers, more than 500 nanometers, more than 1 micrometer, more than 5 micrometers, more than 10 micrometers, or more than 15 micrometers. At the same time, the multi-walled carbon nanotubes can have an average length of up to 25 micrometers or up to 20 micrometers. In an exemplary embodiment, the multi-walled carbon nanotubes have an average length of 10 nanometers to 20 micrometers, or 20 nanometers to 15 micrometers. The multi-walled carbon nanotubes can have an aspect ratio (length to diameter ratio) of more than 5.0, more than 10.0, more than 50, more than 100, or more than 500. In an embodiment, the multi-walled carbon nanotubes can be branched nanotubes.

[0033] The electrodes include multi-walled carbon nanotubes that may be relatively long compared to multi-walled carbon nanotubes included in related art electrodes. It has been found that the use of relatively long multi-walled carbon nanotubes in electrodes provides beneficial mechanical and / or electrical properties. For example, multi-walled carbon nanotubes provide relatively good power output at low density. As another example, shorter multi-walled carbon nanotubes generally do not swell (e.g., expand) as much as longer multi-walled carbon nanotubes. Thus, some of the beneficial properties associated with carbon nanotube swelling are lost (or reduced) when shorter multi-walled carbon nanotubes are used. As an extreme example, carbon black does not exhibit swelling because it is simply a particle of carbon that does not have the entanglement exhibited by a set of multi-walled carbon nanotubes. That a certain amount of multi-walled carbon nanotubes have a length above a threshold length and therefore sufficient swelling properties is indicated by observations during the calendering process, i.e., the relatively high pressure or effort to calender the slurry in conjunction with application to the foil indicates that the collective swelling (e.g., average swelling) of the multi-walled carbon nanotubes in the active layer meets a certain performance threshold. However, multi-walled carbon nanotubes are generally difficult to process.

[0034] The processing of multi-walled carbon nanotubes in connection with the fabrication / formation of the active layer and / or electrode is gentler than the processing of related art electrodes. Thus, the process according to various embodiments preserves longer multi-walled carbon nanotubes (e.g., fewer multi-walled carbon nanotubes are crushed, fragmented, broken, etc.). In some embodiments, the active layer of the electrode includes a set of multi-walled carbon nanotubes having an average length longer than the average length of the multi-walled carbon nanotubes in the related art electrodes. According to various embodiments, the length distribution of the set of multi-walled carbon nanotubes is biased toward the nominal length of the multi-walled carbon nanotubes. In one example, the nominal length of the multi-walled carbon nanotubes is about 16 microns. For example, the multi-walled carbon nanotubes are processed and / or applied in a manner that reduces or minimizes the crushing or breaking of the multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more biased toward the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., 13.4 microns to about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., 13.4 microns to about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 8 microns.In some embodiments, at least 50% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 13 microns.

[0035] According to various embodiments, the length distribution of the set of multi-walled carbon nanotubes is biased toward the nominal length of the multi-walled carbon nanotubes. For example, the multi-walled carbon nanotubes are processed and / or applied in a manner that reduces or minimizes the crushing or breaking of the multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements is generally the nominal length of the multi-walled carbon nanotubes, or the lengths of such multi-walled carbon nanotubes tend to be more biased toward the nominal length.

[0036] In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., 13.4 micrometers to about 15 micrometers). In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 12 micrometers. In some embodiments, at least 75% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 13 micrometers. In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., 13.4 micrometers to about 15 micrometers). In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 12 micrometers. In some embodiments, at least 50% of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements have a length of at least 13 micrometers.

[0037] The multi-walled carbon nanotubes can be present in the mixture (the mixture includes the conductive material, the electrode active material, the binder material, and the solvent or combination of solvents) in an amount of 0.3 to 1.0 wt %, preferably 0.4 to 0.9 wt %, based on the total weight of the mixture. The multi-walled carbon nanotubes are present in the solid anode active layer (the solid active layer includes the conductive material, the binder material, and the electrode active material, excluding the solvent) in an amount of 0.8 to 2.6 wt %, preferably 1.0 to 1.8 wt %, based on the total weight of the solid anode active material.

[0038] In instances where both multi-walled and single-walled carbon nanotubes are used, the weight ratio of multi-walled carbon nanotubes to single-walled carbon nanotubes in the mixture or solid active material layer can be at least 2:1.

[0039] In one example, the three-dimensional network of high aspect ratio carbon elements 108 includes carbon nanotubes, which are multi-walled carbon nanotubes and / or fragments of such carbon nanotubes only.

[0040] In another example, the multi-walled carbon nanotubes are present in the mixture or solid anode active material layer in an amount at least twice the amount of the single-walled carbon nanotubes, based on the weight of the conductive material.

[0041] The three-dimensional network of high aspect ratio carbon elements 108 can comprise at least 99% carbon by weight.

[0042] In addition to the high aspect ratio carbon elements (carbon nanotubes), the conductive material may optionally include graphite flakes, carbon black, or a combination thereof.

[0043] The graphite flakes are preferably high aspect ratio graphite flakes having at least one dimension greater than any other dimension. The graphite flakes may be naturally occurring or commercially synthesized flakes. The graphite flakes may be particulate and elliptical in shape. The aspect ratio of these graphite flakes may range from 2:1 to 20:1, preferably 5:1 to 12:1. In one embodiment, the graphite flakes may be intercalated with metal ions. In another embodiment, the graphite flakes may be exfoliated flakes.

[0044] The graphite flakes may be present in the solid anode active layer (the solid active layer includes the conductive material, the binder material, and the electrode active material, excluding the solvent) in an amount of 5 to 65% by weight, preferably 8 to 50% by weight, based on the total weight of the solid anode active material.

[0045] In addition to carbon nanotubes, carbon black can also be used. Carbon black typically has a density of 50 square meters per gram (m 2 / gm), preferably 200m 2 / gm, more preferably 500m 2 A high surface area carbon black is a carbon black having a surface area of ​​more than 100000 / gm. An example of a high surface area carbon black is KELTJEN black. Carbon black is optional and may be present in the solid anode active layer (the solid active layer includes the conductive material, binder material, and electrode active material, excluding the solvent) in an amount of 0.5 to 2.0 wt %, preferably 0.8 to 1.6 wt %, based on the total weight of the solid anode active material.

[0046] The three-dimensional network of high aspect ratio carbon elements 108 can include a network of electrically interconnected carbon elements that exhibit connectivity above a percolation threshold, which defines one or more highly conductive pathways having lengths greater than 100 μm. The percolation threshold is the threshold at which conductive elements contact each other to form a conductive network measured across any two points on any surface of the network.

[0047] Anode Binder In one embodiment, the anode active layer includes a polymer binder that includes nylon (i.e., a polyamide), a family of polyamides, or a derivative of a polyamide. In an exemplary embodiment, the polyamide is a water-soluble polyamide, an alcohol-soluble polyamide, or a combination thereof (i.e., soluble in a combination of water and alcohol). The anode active layer does not include a polymeric material that is insoluble in water or alcohol. In other words, the anode active layer does not include a polyamide or any other polymeric binder that is not water-soluble.

[0048] Polyamides (used in the anode and cathode polymer binders) may include aliphatic polyamides, aromatic polyamides, or combinations thereof. In one embodiment, polyamides include the general family of resins known as nylons, characterized by the presence of amide groups (-C(O)NH-). Any amide-containing polymers may be used individually or in combination. Nylon-6 and nylon-6,6 are suitable polyamide resins available from a variety of commercial sources. However, other polyamides may also be useful, such as nylon-4, nylon-4,6 (PA 46), nylon-12, nylon-6,10, nylon-6,9, nylon-6,12, nylon-9T, copolymers of nylon-6,6 and nylon-6, nylon 610 (PA610), nylon 11 (PA11), nylon 12 (PA 12), nylon 6-3-T (PA 6-3-T), polyarylamide (PA MXD 6), polyphthalamide (PPA) and / or polyether-block amides, as well as amorphous nylons. Mixtures of various polyamides, and various polyamide copolymers, may also be useful.

[0049] Polyamides can be obtained by many well-known methods, such as those described in U.S. Patents 2,071,250, 2,071,251, 2,130,523, 2,130,948, 2,241,322, 2,312,966, and 2,512,606. For example, nylon-6 is a polymerization product of caprolactam. Nylon-6,6 is a condensation product of adipic acid and 1,6-diaminohexane. Similarly, nylon 4,6 is a condensation product of adipic acid and 1,4-diaminobutane. In addition to adipic acid, other diacids useful in the manufacture of nylon include azelaic acid, sebacic acid, dodecanedioic acid, and terephthalic and isophthalic acids. Other useful diamines include m-xylylenediamine, di-(4-aminophenyl)methane, di-(4-aminocyclohexyl)methane, 2,2-di-(4-aminophenyl)propane, 2,2-di-(4-aminocyclohexyl)propane, among others. Copolymers of caprolactam with diacids and diamines are also useful.

[0050] Polyamides are generally derived from the polymerization of organic lactams having from 4 to 12 carbon atoms. In one embodiment, the lactam has the formula (I): [ka] where n is 3 to 11. In one embodiment, the lactam is epsilon-caprolactam, where n is equal to 5.

[0051] Polyamides can also be synthesized from amino acids having 4 to 12 carbon atoms. In one embodiment, the amino acid has the formula (II): [ka] where n is 3 to 11. In one embodiment, the amino acid is epsilon-aminocaproic acid, where n is equal to 5. The polyamide can also be polymerized from an aliphatic dicarboxylic acid having 4 to 12 carbon atoms and an aliphatic diamine having 2 to 12 carbon atoms. In one embodiment, the aliphatic diamine is represented by formula (III): H2N-(CH2) n -NH2(III) where n is from about 2 to about 12. In one embodiment, the aliphatic diamine is hexamethylenediamine (H2N(CH2)6NH2). In one embodiment, the molar ratio of dicarboxylic acid to diamine is from 0.66 to 1.5. Within this range, it is generally advantageous for the molar ratio to be 0.81 or greater. In another embodiment, the molar ratio is 0.96 or greater. In yet another embodiment, the molar ratio is 1.22 or less. In yet another embodiment, the molar ratio is 1.04 or less. Examples of polyamides useful in the present invention include nylon 6, nylon 6,6, nylon 4,6, nylon 6,12, nylon 10, or a combination comprising at least one of the foregoing polyamides.

[0052] The molecular weight of the polyamide is more than 200 g / mol, preferably more than 500,000 g / mol, preferably more than 1,000,000 g / mol, more preferably from 500,000 g / mol to 1,500,000 g / mol.

[0053] In one embodiment, the anode active layer comprises at least 0.5 wt %, preferably 0.5-1.5 wt %, of the polymer additive, the weight percentage being based on the total weight of the active layer.

[0054] Anode Active Material In one embodiment, the anode comprises a network of high aspect ratio carbon elements defining voids within the network, an active layer comprising a plurality of electrode active material particles disposed in the voids within the network and comprising silicon, and a polymeric additive that is at least one of: (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.

[0055] In one embodiment, the silicon contained in the electrode active material particles is in the form of SiO. The silicon contained in the electrode active material particles is microsilicon. In one embodiment, the silicon contained in the electrode active material particles is greater than 50% by weight of the active layer. The silicon in the electrode active material particles is at least 80% by weight of the active layer.

[0056] Anode Summary In one embodiment, the anode comprises a network of high aspect ratio carbon elements that define voids within the network, an active layer comprising a plurality of electrode active material particles disposed in the voids within the network and comprising silicon, and a polymeric additive that is at least one of: (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.

[0057] In one embodiment, the silicon contained in the electrode active material particles is in the form of SiO. The silicon contained in the electrode active material particles is microsilicon. In one embodiment, the silicon contained in the electrode active material particles is greater than 50% by weight of the active layer. The silicon in the electrode active material particles is at least 80% by weight of the active layer.

[0058] The network of high aspect ratio carbon elements includes a mesh of carbon nanotubes that maintains electrical connectivity between at least a subset of the carbon nanotubes contained within the mesh during expansion of silicon.

[0059] The network of high aspect ratio carbon elements comprises a mesh of carbon nanotubes that maintains electrical connectivity between at least a subset of the carbon nanotubes present in the mesh during charging and discharging of a battery in which the electrode is included. The network of high aspect ratio carbon elements has been described in detail above, most of which will not be repeated here for the sake of brevity. However, some features of the network of high aspect ratio carbon nanotubes in the anode active layer that differ from the corresponding network present in the cathode will now be described in detail.

[0060] In one embodiment, the network of high aspect ratio carbon elements contains graphite particles within the voids. The graphite is generally present in the anode active layer in an amount of up to 10% by weight, preferably up to 5% by weight.

[0061] The multi-walled carbon nanotubes (first set of carbon nanotubes) are present in the anode active layer in an amount of at least 3 wt%, preferably at least 4.5 wt%, based on the weight of the anode active layer. In one embodiment, the multi-walled carbon nanotubes are present in the anode active layer in an amount of 3-5 wt%, based on the weight of the anode active layer.

[0062] The single-walled carbon nanotubes (the second set of carbon nanotubes) are present in the anode active layer in an amount of at least 1.5% by weight, and preferably at least 2% by weight, based on the weight of the anode active layer.

[0063] In one embodiment, the ratio by weight of the first set of carbon nanotubes (multi-walled carbon nanotubes (including double-walled carbon nanotubes)) to the second set of carbon nanotubes (single-walled carbon nanotubes) is at least 5:1, preferably at least 9:1.

[0064] In one embodiment, the active layer increases in thickness after swelling with the electrolyte, hi one embodiment, the active layer (either the anode or cathode) increases in average thickness by an amount (based on the initial dimensions before wetting with the electrolyte) of less than 15%, preferably less than 10%, preferably less than 5% upon wetting with the electrolyte.

[0065] The first set of carbon nanotubes has a first average aspect ratio greater than a second average aspect ratio of the second set of carbon nanotubes. The first set of carbon nanotubes has an average aspect ratio of at least 100 to 1000, preferably 200-1000.

[0066] In one embodiment, the network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes comprising a plurality of multi-walled carbon nanotubes, the plurality of multi-walled carbon nanotubes having an average length greater than 5 microns, preferably greater than 10 micrometers.

[0067] In one embodiment, an energy storage device includes an anode and a cathode, the anode or cathode including an active layer including a first set of carbon nanotubes including multi-walled carbon nanotubes, a second set of carbon nanotubes including single-walled carbon nanotubes, and a network of high aspect ratio carbon elements further including graphite, wherein the multi-walled nanotubes exhibit less swelling than the single-walled carbon nanotubes when wetted with an electrolyte.

[0068] The polymer additive in the anode active layer is a polyamide, preferably a water-soluble polyamide, an alcohol-soluble polyamide, or a polyamide that is soluble in water and alcohol, which are described in detail below and will not be repeated here.

[0069] The anode active layer has an average thickness of 20 microns to 100 micrometers, preferably 30 to 50 micrometers. The anode active layer comprises anode active particles (e.g., silicon-containing, such as silicate) in an amount of 96 to 99% by weight, preferably 96 to 98.5% by weight of the anode active layer.

[0070] The anode active layer also includes a surface treatment on the surface of the high aspect ratio carbon element that promotes adhesion between the high aspect ratio carbon element and the active material particles. The surface treatment can include a surfactant. The surfactant can be present in the active layer in an amount of at least 0.5 wt % based on the weight of the active layer. The surfactant forms a surfactant layer that is bonded to the high aspect ratio carbon element and includes a plurality of surfactant elements, each having a hydrophobic end and a hydrophilic end, where the hydrophobic end is disposed proximal to one surface of the carbon element and the hydrophilic end is disposed distal to said one surface of the carbon element. The surface treatment can include a polymer additive (i.e., it can be a polyamide).

[0071] The multi-walled carbon nanotubes may be substantially aligned in a direction perpendicular to the surface of the active layer or perpendicular to a metal foil used as an electrode, which may comprise copper or aluminum.

[0072] In one embodiment, an energy storage device (i.e., ultracapacitor or battery) comprises a cathode, an electrolyte, and an anode, the anode comprising a network of high aspect ratio carbon elements defining voids within the network, an active layer comprising a plurality of electrode active material particles disposed in the voids within the network and comprising silicon, and a polymeric additive that is at least one of (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides, where the active layer comprises sufficient silicon such that at least a portion of the silicon is not utilized during charge and discharge cycles.

[0073] Anode preparation The anode can be manufactured by first preparing a mixture (sometimes called a slurry) of the conductive element, active material, and binder in a solvent or solvent mixture. The method used to manufacture the anode can also be used to manufacture the cathode. For the sake of brevity, this method will not be repeated again during the manufacture of the cathode. An advantage of the binders described herein is that a useful slurry can be formed using water, alcohol, or a combination thereof as the solvent. The slurry can then be coated directly onto the current collector or applied to the current collector using an intermediate adhesive layer.

[0074] The slurry can be prepared in a single step. Figures 2A and 2B show a process for making either an anode or a cathode. They show how to make the active layer of the anode and cathode and apply the active layer to a current collector. Alternatively, the slurry can be prepared according to a multi-step process as shown in the flow chart of Figure 2A, which illustrates an example of a process 200 provided for the electrode 100 of Figure 1. In 202, a conductive material, such as a high aspect ratio carbon element, and a surface treatment material (e.g., a surfactant, a binder material described herein, or both) are mixed with a solvent (e.g., water, alcohol, or a combination thereof) to form a first slurry. In 204, any additional binder can be added to the first slurry to form a second slurry. In 206, the slurry is applied to a metal foil (current collector). The solvent present in the slurry is removed by vacuum or heat to form an active layer on the current collector.

[0075] 2B illustrates another method 300 for fabricating an anode (or cathode) for an energy storage device. At 302, a conductive material, such as high aspect ratio elemental carbon, and a surface treatment material (e.g., a surfactant, a binder material described herein, or both) are mixed with a solvent (e.g., water, alcohol, or a combination thereof) to form an initial slurry. The materials can be mixed in a blade mixer 303.

[0076] At 304, the initial slurry is treated to ensure good dispersion of the solid materials in the slurry. Li-SiO-C active material (or NMC material) may be added to the slurry. Graphite powder and optional dispersants may be added at step 306. Blade mixing may be performed at mixing steps 305 and 307. Polymer solution may be added at step 308 and additional deionized water may be added at step 310. Blade mixing and dispersive mixing may be used at steps 307 and 309. The prepared slurry may then be added to a current collector at step 312.

[0077] The process can include introducing mechanical energy into the mixture of solvent and solid material (e.g., using a sonicator, sometimes referred to as a "sonifier," or other suitable mixing device (e.g., a high shear mixer)). For example, the mechanical energy introduced into the mixture can be at least 0.4 kilowatt-hours per kilogram (kWh / kg), 0.5 kWh / kg, 0.6 kWh / kg, 0.7 kWh / kg, 0.8 kWh / kg, 0.9 kWh / kg, 1.0 kWh / kg, or more. For example, the mechanical energy introduced into the mixture per kilogram of mixture can be in the range of 0.4 kWh / kg to 1.0 kWh / kg, or any subrange therein, such as 0.4 kWh / kg to 0.6 kWh / kg.

[0078] As an example, an ultrasonic bath mixer may be used in steps 302, 304, or 306. As another example, a probe sonicator may be used. Probe sonication can be significantly more powerful and effective compared to ultrasonic baths for nanoparticle applications. The high shear forces generated by ultrasonic cavitation have the ability to break down particle agglomerates, resulting in smaller, more uniform particle sizes. Among other things, sonication results in a stable, homogenous suspension of solids in a slurry. Generally, this results in dispersion, deagglomeration, and other breakdown of solids. An example of a probe sonicator includes the Q Series Probe Sonicator available from QSonica LLC of Newtown, Connecticut. Another example includes the Branson Digital SFX-450 Sonicator available from Thomas Scientific of Swedesboro, New Jersey.

[0079] The locality of each probe within the probe assembly can sometimes result in non-uniform mixing and suspension. For example, this can be the case with large samples. This can be overcome by using a device with a continuous flow cell and proper mixing. For example, such a device can be used to mix a slurry to achieve a reasonably uniform dispersion.

[0080] The initial slurry, once processed, can have a viscosity in the range of 5,000 cps to 25,000 cps, or any subrange therein, such as 6,000 cps to 19,000 cps.

[0081] In an optional step (e.g., used if no binder was added in step 302), a binder or additional binder may be applied so that the surface treatment may be fully or partially formed on the conductive material (e.g., high aspect ratio carbon elements) in the initial slurry. In some embodiments, at this stage, the surface treatment may self-assemble.

[0082] The resulting surface treatment can include functional groups or other features that can promote adhesion between the high aspect ratio carbon elements and the active material particles, as described in further steps below. For example, functional groups on a binder can provide the aforementioned surface treatment.

[0083] At 304 and 306, active material particles can be mixed with the initial slurry to form a final slurry containing active material particles with high aspect ratio carbon elements having a surface treatment formed thereon.

[0084] The active material may be added directly to the initial slurry, or it may be first dispersed in a solvent (e.g., in water, alcohol, or a combination thereof, using the techniques described above for the initial solvent) to form an active material slurry, which may then be mixed with the initial slurry to form the final slurry.

[0085] Suitable solvents are water, alcohol, or combinations thereof. Examples of alcohols are ethanol, methanol, propanol, butyl alcohol, ethylene glycol, propylene glycol, or combinations thereof. In addition to water and alcohol, other solvents may be added to facilitate solubilization and / or dispersion of the polymer. Other solvents include polar solvents, non-polar solvents, etc. The addition of other solvents should preferably not change the solubility of the polymer in water or alcohol. To dissolve the polymer, liquid aprotic polar solvents such as propylene carbonate, ethylene carbonate, butyrolactone, acetonitrile, benzonitrile, nitromethane, nitrobenzene, sulfolane, dimethylformamide, N-methylpyrrolidone, or combinations thereof can be added to water or alcohol. Polar protic solvents such as acetonitrile, nitromethane, acetone, dimethylsulfoxide, dimethylformamide, or combinations thereof can be used. Other non-polar solvents such as benzene, toluene, methylene chloride, carbon tetrachloride, hexane, diethyl ether, tetrahydrofuran, or combinations thereof can also be used. Co-solvents, including at least one aprotic polar solvent and at least one non-polar solvent, can also be utilized to modify the solubilizing ability of the solvent.

[0086] When water and alcohol are used as the solvent for the anode active layer (used in the anode), the ratio of water to alcohol is 80:20 to 95:5, preferably 88:12 to 92:8. In an exemplary embodiment, the ratio of water to alcohol is 90:10.

[0087] The solvent may be added to the mixture of binder, conductive material, and active material in an amount of 10-1000% by weight, preferably 50-500% by weight, and more preferably 100-200% by weight of the total weight of the solids used to form the active layer. The solids include the materials (e.g., binder, conductive material, and active material) that do not evaporate and that ultimately become the active material layer disposed on the current conductor.

[0088] At 312, the final slurry is processed to ensure good dispersion of the solid materials in the final slurry. Any suitable mixing process known in the art can be used. For example, this can use techniques described above with reference to 303, 305, 307, 309, and 311, etc. Alternatively, a planetary mixer can be used, such as a multi-shaft (e.g., three or more) planetary mixer. The planetary mixer can feature multiple blades, such as two or more mixing blades, and one or more (e.g., two, three or more) dispersion blades, such as a disk dispersion blade.

[0089] During 312, the matrix that entangles the active materials may fully or partially self-assemble because interactions between the surface treatment (eg, binder) and the active materials facilitate the self-assembly process.

[0090] In some embodiments, the final slurry, once processed, has a viscosity in the range of 1,000 cps to 10,000 cps, or any subrange therein, such as 2,500 cps to 6000 cps.

[0091] At 312, the active layer 106 is formed from the final slurry. In some embodiments, the final slurry can be poured wet directly onto the current collector conductive layer 102 (or optional adhesive layer 104) and dried. By way of example, pouring can be done by applying at least one of heat and vacuum until substantially all of the solvent and any other liquids are removed, thereby forming the active layer 106. It may be desirable to protect various portions of the underlying layers. For example, if the electrode 100 is intended for single-sided operation, it may be desirable to protect the underside of the conductive layer 102. Protection may include, for example, protection from the solvent by masking certain areas or providing a drain to drain the solvent.

[0092] In another example, the final slurry can be transferred onto the adhesive layer 104 or the conductive layer 102 using any suitable technique (e.g., roll-to-roll layer application) after being at least partially dried elsewhere to form the active layer 106. As another example, the wet mixed slurry can be placed onto an intermediate material having a suitable surface and dried to form a layer (e.g., the active layer 106). While any material having a suitable surface can be used as the intermediate material, an exemplary intermediate material includes polytetrafluoroethylene (PTFE) because its properties facilitate its subsequent removal from the surface. The layer can be formed in a press to provide a layer exhibiting a desired thickness, area, and density.

[0093] In yet another example, the final slurry can be formed into a sheet and coated onto the adhesive layer 104 or the conductive layer 102 as needed. For example, the final slurry can be applied through a slot die to control the thickness of the applied layer. As another example, the slurry can be applied and then leveled to the desired thickness using, for example, a doctor blade. Various other techniques can be used to apply the slurry. For example, coating techniques can include, but are not limited to, comma coating, comma reverse coating, doctor blade coating, slot die coating, direct gravure coating, air doctor coating (air knife), chamber doctor coating, offset gravure coating, one roll kiss coating, reverse kiss coating with a small diameter gravure roll, bar coating, 3 reverse roll coating (top feed), 3 reverse roll coating (fountain die), reverse roll coating, and the like.

[0094] The viscosity of the final slurry may vary depending on the application technique. For example, for comma coating, the viscosity may range from about 1,000 cps to about 200,000 cps. Lip die coating provides coatings with slurries exhibiting viscosities of about 500 cps to about 300,000 cps. Reverse kiss coating provides coatings with slurries exhibiting viscosities of about 5 cps to 1,000 cps. In some applications, each layer may be formed in multiple passes.

[0095] If desired, the active layer 106 formed from the final slurry can be compressed (e.g., using a calendaring apparatus) before or after it is applied to the electrode 100. The slurry can be partially or completely dried (e.g., by application of heat, vacuum, or a combination thereof) before or during the compression process. For example, in some embodiments, the active layer can be compressed (e.g., in a direction perpendicular to the current collector layer 102) to a final thickness that is 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of its pre-compression thickness.

[0096] If a partially dried layer is formed during the coating or pressing process, the layer can then be completely dried (e.g., by application of heat, vacuum, or a combination thereof). In some embodiments, substantially all of the solvent is removed from the active layer 106.

[0097] The solvent used to form the slurry can be recovered and recycled into the slurry manufacturing process.

[0098] The active layers 106 may be compressed, for example, to break down some of the constituent high aspect ratio carbon elements or other carbonaceous materials and increase the surface area of ​​each layer. This compression process may increase one or more of the adhesion between the layers, the rate of ion transport within the layers, and the surface area of ​​the layers. In various embodiments, compression may be applied before or after each layer is applied to or formed on the electrode 100.

[0099] When using calendaring to compress the active layer 106, the calendaring equipment can be set with gap spacing of 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of the pre-compressed thickness of the layer (e.g., set at about 33% of the pre-compressed thickness of the layer). The calendar rolls can be configured to provide suitable pressure, for example, greater than 1 ton per cm of roll length, greater than 1.5 ton per cm of roll length, greater than 2.0 ton per cm of roll length, greater than 2.5 ton per cm of roll length, or more. The active layer after compression can have a density in the range of 1 g / cc to 10 g / cc, or any subrange thereof, such as 2.0 g / cc to 4.0 g / cc. Note that the cathode active layer has a density of 2 to 4 g / cc. The anode active layer generally has a density of 1.0 to 1.8 g / cc. The calendaring process can be carried out at a temperature in the range of 20° C. to 140° C., or any subrange thereof. In some embodiments, the active layer 106 can be preheated prior to calendering, for example at a temperature in the range of 20° C. to 100° C., or any subrange thereof.

[0100] The process 300 of FIG. 2B may include any of the following features (individually or in any suitable combination).

[0101] The initial slurry has a solids content of 0.1% to 20.0% by weight (or any subrange therein) and / or the final slurry has a solids content of 10.0% to 80% by weight (or any subrange therein).

[0102] As mentioned above, a scaffold or matrix of conductive material and binder can hold the active material particles together to form a cohesive layer that also adheres strongly to the metal current collector. Such active material structures can be formed during the preparation of the slurry as well as during the subsequent roll-to-roll ("R2R") coating and drying process. One of the main advantages of the present technology is its scalability and "drop-in" nature, since various embodiments are compatible with conventional electrode manufacturing processes.

[0103] The matrix can be formed during slurry preparation using techniques described herein. For example, the high aspect ratio carbon material is appropriately dispersed and chemically functionalized as desired using those described above with reference to processes 200 and 300 in Figures 2A and 2B. The chemical functionalization is designed to form organized self-assembled structures with the surfaces of the active material particles, e.g., NMC particles (described in detail below) for use in the cathode or silicon particles ("Si") or silicon oxide ("SiOx") particles in the case of the anode. The slurry thus formed can be based on water and / or alcohol solvents for the cathode and water for the anode, such solvents being highly evaporative and easy to handle during the manufacturing process. Electrostatic interactions promote the self-assembled structures within the slurry, and after the drying process, the bond between the carbon matrix containing the active material particles so formed and the surface of the current collector is promoted by the surface treatment (e.g., functional groups on the matrix) and the strong entanglement of the active material in the carbon matrix.

[0104] The mechanical properties of the electrodes can be altered depending on the application and mass loading requirements by tuning the surface functionalization versus the entanglement effect.

[0105] After coating and drying, the electrode can undergo a calendaring step to control the density and porosity of the active material. Densities of 3.5 g / cc or higher and porosities of 20% or higher can be achieved for NMC cathode electrodes. Depending on the mass loading and requirements of the lithium-ion battery cell, the porosity can be optimized. For silicon oxide or silicon-based anodes, the porosity can be specifically controlled to accommodate the expansion of the active material during the lithiation process.

[0106] The teachings herein can result in up to 20% reduction in $ / kWh. By using water, alcohol, or a mixture of water and alcohol as the solvent, these solvents evaporate easily, allowing for higher electrode manufacturing throughput, and more importantly, energy consumption due to long dryers can be significantly reduced. Traditional recovery systems required when using NMP or similar compounds as the solvent are also greatly simplified when using water, alcohol, or a combination thereof.

[0107] The teachings herein provide an active layer with a 3D matrix that can dramatically increase the electrode conductivity by 10 to 100 times compared to electrodes using traditional binders such as PVDF, thereby enabling fast charging at the battery level. This technology allows for thick electrode coatings of the cathode up to 150 um per side (or more) of the current collector. The solvents used in the slurry in combination with the strong 3D carbon matrix are designed to provide a thick wet coating without cracking during the drying step. The thick cathode with high capacity anode allows for a significant increase in energy density to 400 Wh / kg or more.

[0108] Cathode The cathode includes one or more polymer binders (cathode polymer binders), one or more active materials, and a conductive material. The one or more polymer binders, the one or more active materials, and the conductive material are mixed with a solvent to form a cathode mixture. The cathode mixture is then disposed on a current collector (usually metal) and dried to form a solid cathode active layer.

[0109] The cathode polymer binder (used in the cathode) comprises a first cathode polymer binder comprising a polyamide, which has been described in detail above and will not be described in detail again for the sake of brevity.

[0110] The cathode polymer binder is present in an amount of 0.1 to 0.4 wt %, preferably 0.15 to 0.375 wt %, based on the weight of the cathode mixture (including the cathode polymer binders (first and second cathode polymer binders), the cathode active material, the cathode conductive material and the solvent). The cathode polymer binder is present in the cathode active layer in an amount of 0.2 to 0.5 wt %, preferably 0.25 to 0.45 wt %, based on the total weight of the cathode active layer.

[0111] Cathode Active Material Cathode active materials can include lithium cobalt oxide (LCO, sometimes called "lithium cobaltate" or "lithium cobaltite"). Examples of LCO formulations include LiCoO2, lithium nickel manganese cobalt oxide (NMC, having a formula of LiNiMnCo), lithium manganese oxide (LMO, having a formula of LiMn2O4, Li2MnO3, or combinations thereof), lithium titanate oxide (LTO, one formula is Li4Ti5O 12 Lithium iron phosphate oxide (LFP, one variant is LiFePO4), Lithium nickel cobalt aluminum oxide (and its variants as NCA), and other similar materials. Other variants of the foregoing may also be included.

[0112] In one embodiment, the cathode active material can include NMC, NCA, NCMA, or a combination thereof.

[0113] When NMC is used as the cathode active material, nickel-rich NMC can be used. For example, a variant of NMC is LiNi x Mn y Co (1-x-y) where x is about 0.7, 0.75, 0.80, 0.85 or more, y is 0.1, 0.15, 0.2, or 0.25 or more, and x+y is less than 1. For example, NMC811 can be used, where x is about 0.8 and y is about 0.1. Alternatively, the cathode active material can be lithium nickel manganese cobalt (LiNi x Mn y Co z O2). Variations of this formula that can be used for the active material layer include NMC 111 (discussed in more detail below), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC622(LiNi 0.6 Mn 0.2 Co 0.2 O2), or a combination thereof.

[0114] In one embodiment, NMC91 can be used as the cathode active material. NMC91 contains 91 mole % or more of nickel. One example of NMC91 is LiNi 0.91 Co 0.06 Mn 0.03 O2. Li[Ni 1-x-y Co x Al y ]O2NCA) can also be used as the cathode active material. An example of an NCA is NCA89.

[0115] In yet another embodiment, the cathode active material may be an NCMA material. One example of an NCMA is Li[Ni 0.89 Co 0.05 Mn 0.05 Al 0.01 ]O2.

[0116] In one embodiment, the cathode active material can also include a nickel-rich combination of nickel, manganese, and cobalt. Lithium nickel manganese cobalt oxide (LiNiMnCoO2) (abbreviated as NMC) provides strong overall performance, excellent specific energy, and the lowest self-heating rate of all mainstream cathode powders. NMC powder can include nickel in an amount of 20-40% by weight, manganese in an amount of 20-40% by weight, and cobalt in an amount of 20-40% by weight, based on the total weight of the NMC blend. Although the term "NMC powder" can refer to various blends, it is desirable to use a blend that includes 33% by weight nickel, 33% by weight manganese, and 33% by weight cobalt. This blend, sometimes referred to as 1-1-1 (NMC 111), is useful for applications that use frequent cycling (automotive, energy storage) because the lower cobalt content of the nickel-rich combination of nickel, manganese, and cobalt (NMC) reduces material costs. NMC powders can contain nickel in an amount of 20-40% by weight, manganese in an amount of 20-40% by weight, and cobalt in an amount of 20-40% by weight, based on the total weight of the NMC blend. Although the term "NMC powder" can refer to a variety of blends, it is desirable to use a blend containing 33% by weight nickel, 33% by weight manganese, and 33% by weight cobalt. This blend, sometimes referred to as 1-1-1, is useful for applications that use frequent cycling (automotive, energy storage) because the lowered cobalt content reduces material costs. Lithium nickel manganese cobalt oxide (LiNiMnCoO2) delivers strong overall performance, excellent specific energy, and the lowest self-heating rate of all mainstream cathode powders. Lithium-rich NCM materials, such as 424 and 523 manufactured by BASF, can also be used as cathode active materials.

[0117] Generally, increasing the loading of active material in the cathode (measured relative to the total weight of the cathode) increases the areal capacity and specific energy level of the cathode.

[0118] As mentioned above, the cathode active material can be contained or accommodated within the network of the high aspect ratio conductive material present in the cathode active layer. The cathode active material can be present in the mixture used to form the cathode in an amount of 90 to 99 wt%, preferably 96 to 98.5 wt%, based on the total weight of the cathode mixture (the mixture including the cathode binder material, the cathode active material, the cathode conductive material, and the solvent used to make the cathode active layer). The cathode active material is present in the cathode active layer (excluding the solvent) in an amount of 95 to 98.5 wt%, based on the total weight of the cathode active layer.

[0119] Fabrication of the cathode active layer The cathode active layer is disposed on a current collector. The cathode active layer is fabricated in a similar manner to the anode active layer. The cathode binder, cathode active material, and cathode conductive material are mixed with a solvent to form a slurry. The slurry is disposed on a cathode current collector. The solvent is evaporated and the cathode current collector is further finished on a roll mill to form a cathode that can then be used in an energy storage device, as described in more detail below.

[0120] Cathode Summary In one embodiment, the cathode comprises an active layer comprising a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network, a plurality of electrode active material particles disposed in the voids within the network, and a polymeric additive that is at least one of: (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.

[0121] The cathode comprises a network of high aspect ratio carbon elements including a first set of carbon nanotubes comprising a plurality of first carbon nanotubes or a plurality of bundles of the first carbon nanotubes, and a second set of carbon nanotubes comprising a plurality of second carbon nanotubes or a plurality of bundles of the second carbon nanotubes, the second set of carbon nanotubes having one or more properties different from the first set of carbon nanotubes.

[0122] The first set of carbon nanotubes comprises multi-walled carbon nanotubes. The second set of carbon nanotubes comprises single-walled carbon nanotubes. In one embodiment, the first set of carbon nanotubes comprises multi-walled carbon nanotubes and the second set of carbon nanotubes comprises single-walled carbon nanotubes, and the weight ratio of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:1.

[0123] In one embodiment, the network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes, some of which are branched, interdigitated, entangled, and / or share a common wall, and the active layer comprises 0.2-2 wt. % multi-walled carbon nanotubes, or 0.25-1.5 wt. % multi-walled carbon nanotubes.

[0124] In one embodiment, the energy storage device includes an electrolyte, an anode, and a cathode, and when wetted with the electrolyte, the multi-walled carbon nanotubes (the first set of carbon nanotubes) in the cathode active layer swell more than the single-walled carbon nanotubes (the second set of carbon nanotubes).

[0125] In one embodiment, the multi-walled carbon nanotubes of the cathode active layer comprise an average diameter of 6 nm to 10 nm or 6 nm to 15 nm, an average wall thickness of 6 nm to 7 nm, and an average length of about 16 micrometers. In one embodiment, the cathode active layer can comprise single-walled carbon nanotubes having an average diameter of 1 nm to 5 nm and an average length of about 5 micrometers or more up to about 200 micrometers. In one embodiment, the cathode active layer can comprise single-walled carbon nanotubes having an average diameter of 2 nm to 4 nm and an average length of about 6 micrometers or more up to about 8 micrometers. The single-walled carbon nanotubes comprise, on average, one or two walls.

[0126] In one embodiment, the carbon nanotubes used in the cathode active layer have an average thickness increase (diameter increase) of less than 10% when wetted with electrolyte. In one embodiment, a first average aspect ratio of the first set of carbon nanotubes is greater than a second average aspect ratio of the second set of carbon nanotubes. In another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes, the distribution of lengths of the plurality of multi-walled carbon nanotubes being biased towards a nominal length of the multi-walled carbon nanotubes, where the nominal length of the multi-walled carbon nanotubes is at least 15 micrometers.

[0127] In one embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes, at least 50% of the plurality of multi-walled carbon nanotubes having a length greater than 8 micrometers, preferably greater than 12 micrometers.

[0128] In one embodiment, the first set of carbon nanotubes has an average aspect ratio of at least 100, preferably between 200 and 1000. In one embodiment, the network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes comprising a plurality of multi-walled carbon nanotubes, the plurality of multi-walled carbon nanotubes having at least five walls, preferably at least six walls, more preferably at least seven walls.

[0129] In another embodiment, the high aspect ratio carbon elements used in the cathode active layer comprise at least one material selected from the group consisting of carbon nanostructures, carbon nanostructure fragments, and crushed multi-walled carbon nanotubes.

[0130] In one embodiment, the cathode active layer includes a polymer binder that includes nylon (i.e., a polyamide). In an exemplary embodiment, the polyamide is a water-soluble polyamide, an alcohol-soluble polyamide, or a combination thereof (i.e., soluble in a combination of water and alcohol). The cathode active layer does not include a polymeric material that is insoluble in water or alcohol. In other words, the cathode active layer does not include a polyamide or any other polymeric binder that is not water-soluble.

[0131] The molecular weight of the polyamide is more than 200 g / mol, preferably more than 500,000 g / mol, preferably more than 1,000,000 g / mol, more preferably from 500,000 g / mol to 1,500,000 g / mol.

[0132] In one embodiment, the cathode active layer comprises at least 0.5 weight percent, preferably 0.5 to 1.5 weight percent, of the polymer additive, the weight percentage being based on the total weight of the active layer.

[0133] In one embodiment, the cathode active layer has an average thickness of 20 to 100 micrometers, preferably 30 to 80 micrometers.

[0134] In one embodiment, the active material particles present in the active layer include at least one of lithium iron phosphate, lithium metal oxide, lithium sulfur, lithium cobalt oxide, lithium nickel manganese cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, and combinations thereof.

[0135] In one embodiment, the cathode active material is LiCoO2, LiNiO2, LiMn2O4, LiCoPO4, LiFePO4, LiNiMhCoO2, and LiNi 1-x-y-z Co x M1 y M2 z O z (wherein M1 and M2 are each independently selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, and x, y, and z represent the atomic fractions of the corresponding constituent elements of the oxide, and satisfy the relationships 0≦x<0.5, 0≦y<0.5, and 0≦z<0.5.) The active layer contains at least 96% by weight, preferably 96.0% to 98.5% by weight, of the active material particles.

[0136] In one embodiment, the cathode active layer comprises about 25% by weight of the dispersant.

[0137] In one embodiment, the cathode active layer includes a surface treatment on the surface of the high aspect ratio carbon elements that promotes adhesion between the high aspect ratio carbon elements and the active material particles. In one embodiment, the surface treatment includes a material that is soluble in a solvent having a boiling point less than 202° C., preferably less than 185° C. In one embodiment, the surface treatment includes a surfactant layer, where the surfactant layer is bonded to the high aspect ratio carbon elements and includes a plurality of surfactant elements each having a hydrophobic end and a hydrophilic end, the hydrophobic end disposed proximal to the surface that includes one of the carbon elements and the hydrophilic end disposed distal to said surface that includes one of the carbon elements.

[0138] In one embodiment, the surface treatment includes a polymer additive (polyamide). In another embodiment, the polymer additive is a polymer binder. The polymer additive is at least partially disposed within at least one void defined by the network of high aspect ratio carbon elements. The polymer additive is at least 1.135 g / cm 3 More than 1.20 g / cm 3The polymer additive has a specific heat of greater than 2.0 J / g°C at 23°C, preferably greater than 2.2 J / g°C at 23°C, more preferably greater than 2.4 J / g°C at 23°C. The polymer additive has a tensile strength of less than 70 MPa, preferably less than 50 MPa, preferably less than 25 MPa, preferably less than 10 MPa, preferably less than 7.5 MPa, when measured when the polymer additive is dry. The polymer additive has a tensile strength of 5-6 MPa, when measured when the polymer additive is dry.

[0139] The polymeric additive has an elongation at yield of greater than 5%, preferably greater than 10%, preferably greater than 20%, more preferably greater than 30%, when measured when the polymeric additive is dry. Tensile strength and elongation at yield are measured according to ASTM D 638.

[0140] The polymer additive has a glass transition temperature of less than 0° C., preferably less than −10° C., preferably less than −25° C., preferably less than −30° C., preferably less than −45° C., as measured using differential scanning calorimetry (DSC) at a temperature ramp rate of 10° C. / min. The polymer additive has a 5% weight loss temperature of 375° C. to 400° C.

[0141] When a mixture of the polymer additive and ethyl cellosolve is cooled, the polymer additive exhibits gelation. The polymer additive is completely soluble in each of water, ethylene glycol, benzyl alcohol, acetic acid, N-methylpyrrolidone, and isobutanol.

[0142] In one embodiment, an aqueous solution of the polymer additive and at least one of water and an alcohol exhibits a viscosity of at least 60 Pa·s at a concentration of about 50% by weight of the polymer additive. In one embodiment, the mixture of the polymer additive and the water-soluble polymer forms a clear mixture.

[0143] The active layer does not include polymeric materials that are insoluble in water or alcohol.

[0144] In one embodiment, an energy storage device (which may be an ultracapacitor or a battery) includes an anode, an electrolyte, and a cathode, the cathode including a cathode active layer including a network of high aspect ratio carbon elements that define voids within the network, a plurality of electrode active material particles disposed in the voids within the network, and a polymeric additive that is at least one of: (i) selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides.

[0145] In another embodiment, an electrode comprises an active layer comprising a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network, where the network of high aspect ratio carbon elements comprises at least one material selected from the group consisting of multi-walled carbon nanostructures, multi-walled carbon nanotubes, fragments of multi-walled carbon nanostructures, and crushed multi-walled carbon nanotubes, a plurality of electrode active material particles disposed in the voids within the network, and a polymeric additive that is a polyamide that is soluble in water or alcohol.

[0146] In another embodiment, an electrode comprises an active layer comprising a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network, a plurality of electrode active material particles disposed in the voids within the network, and a polymeric additive that is a water or alcohol soluble polyamide, where the network of high aspect ratio carbon elements forms one or more highly conductive pathways, the network of high aspect ratio carbon elements comprises multi-walled carbon nanotubes, the network of high aspect ratio carbon elements provides mechanical support to at least a portion of the plurality of electrode active material particles, and the polymeric additive provides support to at least a portion of the plurality of electrode active material particles.

[0147] Energy Storage Device Once the electrode 100 is assembled, an energy storage device can be assembled using the electrode 100. Assembly of the energy storage device can follow the conventional steps used to assemble an electrode with a separator and place it into a housing, such as a canister or pouch, and can further include additional steps for adding electrolyte and sealing the housing.

[0148] One exemplary embodiment includes a pouch cell format Li-ion battery energy storage device combining Ni-rich NMC active material in the cathode and SiOx and graphite blend active material in the anode, where both the anode and cathode are fabricated using the 3D carbon matrix process as described herein.

[0149] A schematic of the electrode arrangement of one example of a pouch cell device is shown in Figure 3. As shown, cathode active layers 760 (e.g., active layers according to various embodiments disclosed herein) are disposed on either side of a current collector 710 (e.g., an aluminum foil current collector) to form a double-sided cathode disposed between two single-sided anodes. The single-sided anodes each have an anode layer 740 or 750 (e.g., an active layer comprising a network of carbon elements as disclosed herein) disposed on a current collector 720 or 730 (e.g., a copper current collector). The electrodes are separated by a permeable separator material 780 that is wetted with an electrolyte (not shown). This arrangement can be contained within a pouch cell of a type well known in the art.

[0150] 4 shows a cross section of an energy storage device (ESD) 810. The energy storage device (ESD) 810 includes a housing 811. The housing 811 has two terminals 800 disposed on its exterior. The terminals 800 provide an internal electrical connection to a storage cell 812 contained within the housing 811 and an external electrical connection to an external device, such as a load or charging device (not shown). The energy storage devices disclosed herein may be batteries, capacitors, ultracapacitors, etc.

[0151] Alternatively, the present disclosure may comprise, consist of, or consist essentially of any suitable components disclosed herein. The present disclosure may additionally or alternatively be formulated to be free or substantially free of any components, materials, ingredients, adjuvants, or species that are used in prior art compositions or that are otherwise not necessary to the function and / or accomplishment of the purpose of the present invention.

[0152] All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term from this application contradicts or conflicts with a term from an incorporated reference, the term from this application takes precedence over the conflicting term from the incorporated reference.

[0153] Unless otherwise specified herein, all test standards are the latest standards in effect as of the filing date of this application or, if priority is claimed, the filing date of the earliest priority application in which the test standard is listed.

[0154] Although the present invention has been described with reference to several embodiments, it will be apparent to those skilled in the art that various changes can be made and equivalents substituted for elements thereof without departing from the scope of the invention. In addition, many modifications can be made to adapt a particular situation or material to the teachings of the invention without departing from the essential scope thereof. Therefore, it is not intended that the invention be limited to the particular embodiment disclosed as the best mode contemplated for carrying out this invention, but the invention is intended to include all embodiments falling within the scope of the appended claims.

Claims

1. An anode, a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network; and a plurality of electrode active material particles comprising silicon disposed in the voids within the network; A polymer additive which is at least one of (i) those selected from the family of polyamides, or (ii) modified polyamides or derivatives of polyamides; An active layer including an anode.

2. 2. The electrode of claim 1, wherein the silicon contained in the electrode active material particles is in the form of SiO.

3. The electrode according to claim 1 , wherein the silicon contained in the electrode active material is microsilicon.

4. 2. The electrode of claim 1, wherein the silicon in the electrode active material is greater than 50% by weight of the active layer.

5. 2. The electrode of claim 1, wherein the silicon contained in the electrode active material is at least 80% by weight of the active layer.

6. the network of high aspect ratio carbon elements comprises a mesh of carbon nanotubes; the mesh of carbon nanotubes maintains electrical connectivity between at least a subset of the carbon nanotubes contained within the mesh during expansion of the silicon.

2. The electrode of claim 1.

7. the network of high aspect ratio carbon elements comprises a mesh of carbon nanotubes; the mesh of carbon nanotubes maintains electrical connectivity between at least a subset of the carbon nanotubes contained in the mesh during charging and discharging of a battery in which the electrode is included.

2. The electrode of claim 1.

8. the network of high aspect ratio carbon elements being a first set of carbon nanotubes comprising a plurality of first carbon nanotubes or a plurality of bundles of first carbon nanotubes; A second set of carbon nanotubes, the second set of carbon nanotubes comprises a plurality of second carbon nanotubes or a plurality of bundles of second carbon nanotubes; a second set of carbon nanotubes, the second set of carbon nanotubes having one or more properties different from the first set of carbon nanotubes; The electrode of claim 1 , comprising:

9. The electrode of claim 8 , wherein the first set of carbon nanotubes comprises multi-walled nanotubes.

10. The electrode of claim 8 , wherein the second set of carbon nanotubes comprises single-walled nanotubes.

11. A cathode, a network of high aspect ratio carbon elements, the high aspect ratio carbon elements defining voids within the network; and an active layer comprising: a plurality of electrode active material particles disposed in the voids within the network; and a polymer additive that is at least one of: (i) selected from the family of polyamides; or (ii) modified polyamides or derivatives of polyamides. a cathode.

12. the network of high aspect ratio carbon elements being a first set of carbon nanotubes comprising a plurality of first carbon nanotubes or a plurality of bundles of first carbon nanotubes; A second set of carbon nanotubes, the second set of carbon nanotubes comprises a plurality of second carbon nanotubes or a plurality of bundles of second carbon nanotubes; a second set of carbon nanotubes, the second set of carbon nanotubes having one or more properties different from the first set of carbon nanotubes; The electrode of claim 11 , comprising:

13. The electrode of claim 12 , wherein the first set of carbon nanotubes comprises multi-walled nanotubes.

14. The electrode of claim 12 , wherein the second set of carbon nanotubes comprises single-walled nanotubes.

15. the first set of carbon nanotubes comprises multi-walled carbon nanotubes; the second set of carbon nanotubes comprises single-walled carbon nanotubes; a weight ratio of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:1; 13. The electrode of claim 12.

16. The electrode of claim 11 , wherein the network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes.

17. 17. The electrode of claim 16, wherein the active layer comprises 0.2 to 2 wt. % multi-walled carbon nanotubes, or 0.25 to 1.5 wt. % multi-walled carbon nanotubes.

18. The electrode of claim 16 , wherein the multi-walled carbon nanotubes are branched carbon nanotubes.

19. 17. The electrode of claim 16, wherein the active layer comprises 0.25 to 1.5 wt. % multi-walled carbon nanotubes.

20. The electrode of claim 16 , wherein the multi-walled carbon nanotubes are branched, interdigitated, entangled, and / or share a common wall.

21. 1. An energy storage device, comprising:

13. An energy storage device comprising an electrolyte and the electrode of claim 12, wherein when wetted with the electrolyte, the multi-walled nanotubes in the first set of carbon nanotubes swell more than the single-walled carbon nanotubes in the second set of carbon nanotubes.

Citation Information

Patent Citations

  • Electrode composition for battery

    JP2016025077A

  • Anode active material and preparation method thereof, and device using the anode active material

    WO2020186799A1