Negative electrode active material, negative electrode containing the same, and secondary battery
The formulation of artificial graphite particles with specific solid content and surface treatment addresses dispersibility and phase stability issues, enhancing the efficiency and quality of lithium secondary battery production.
Patent Information
- Application Number
- JP2024528560
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-21
- Filing Date
- 2022-12-21
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing negative electrode active materials, particularly artificial graphite, exhibit poor dispersibility and phase stability when used in high solid content slurries, leading to filter clogging and reduced manufacturing efficiency in lithium secondary batteries.
A negative electrode active material comprising artificial graphite particles with a solid content of 69.5% by weight, measured using a torque rheometer, is formulated to enhance dispersibility and phase stability by adjusting particle shape and surface properties through spheronization and heat treatment, ensuring excellent fluidity and wettability.
The improved dispersibility and phase stability of the negative electrode slurry result in enhanced productivity and quality of the secondary battery, preventing filter clogging and maintaining high manufacturing efficiency.
Smart Images

Figure 2024544988000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0184259 filed on December 21, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a negative electrode active material, and a negative electrode and a secondary battery each including the same. [Background technology]
[0003] As interest in environmental issues grows, much research is being conducted on electric vehicles (EVs) and hybrid electric vehicles (HEVs) that can replace vehicles that use fossil fuels such as gasoline and diesel vehicles, which are one of the main causes of air pollution. Lithium secondary batteries, which have high energy density, high discharge voltage and output stability, are mainly researched and used as the power source for such electric vehicles (EVs) and hybrid electric vehicles (HEVs).
[0004] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode or the negative electrode is manufactured by mixing a positive electrode active material or a negative electrode active material with a binder or the like, dispersing the mixture in a solvent to prepare a slurry, applying the slurry to a surface of an electrode current collector, and drying the slurry to form an electrode active material layer.
[0005] Meanwhile, as the negative electrode active material, a carbon-based active material is used that is capable of reversible lithium ion intercalation and deintercalation and maintains structural and electrical properties. As the carbon-based active material, various types of carbon-based materials such as artificial graphite, natural graphite, and hard carbon are used, among which graphite-based active materials that can guarantee the life characteristics of lithium secondary batteries due to their excellent reversibility are most widely used. The graphite-based active material has a lower discharge voltage of -0.2V compared to lithium, and thus a battery using the graphite-based active material can exhibit a high discharge voltage of 3.6V, providing many advantages in terms of the energy density of lithium batteries.
[0006] Among them, artificial graphite has the advantage that it has a relatively low degree of orientation during rolling of the electrode compared to natural graphite and has good lithium ion inflow / outflow characteristics, resulting in excellent quick charging performance of the battery, low expansion due to charging / discharging, and excellent life characteristics.
[0007] However, since artificial graphite exhibits hydrophobicity, when water is used as a solvent for the negative electrode slurry, it is difficult to disperse, and the phase stability of the slurry is reduced. In particular, attempts have been made to increase the solid content of the negative electrode slurry for reasons such as increasing the negative electrode loading amount, improving the efficiency of the drying process, and improving binder migration, and the increase in solid content has made the above-mentioned problems of the decrease in dispersibility of artificial graphite and the phase stability of the slurry more pronounced. In addition, such a dispersibility problem causes a filter clogging problem during the transfer of the negative electrode slurry during the negative electrode manufacturing process, which reduces the overall efficiency and quality of the secondary battery manufacturing process.
[0008] Japanese Patent No. 4403327 discloses graphite powder for use in the negative electrode of a lithium ion secondary battery, but fails to provide an alternative to the above-mentioned problems. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 4403327 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide an anode active material that has excellent dispersibility and can improve the phase stability of an anode slurry even when the solid content of the anode slurry is increased.
[0011] Another object of the present invention is to provide a negative electrode slurry containing the above-mentioned negative electrode active material.
[0012] Still another object of the present invention is to provide a negative electrode comprising the above-mentioned negative electrode active material.
[0013] A further object of the present invention is to provide a secondary battery including the above-mentioned negative electrode. [Means for solving the problem]
[0014] The present invention provides a negative electrode active material comprising artificial graphite particles, wherein when a sample comprising the negative electrode active material and water is measured with a torque rheometer, the solids content at the time when the sample has a maximum torque value is 69.5% by weight or more, and the solids content at the time when the sample has a maximum torque value is measured by a method comprising the following steps (a) to (c): (a) placing the negative electrode active material in a sample container of a torque rheometer; (b) operating the torque rheometer while injecting water into a sample container of the torque rheometer at a predetermined rate to measure a torque value according to a solid content value of the sample; and (c) deriving a value for the solids content at the time when the sample has a maximum torque value in step (b).
[0015] The present invention also provides a negative electrode slurry containing the above-mentioned negative electrode active material, a negative electrode binder, a negative electrode conductive material, and a solvent.
[0016] The present invention also provides a negative electrode including a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including the above-mentioned negative electrode active material.
[0017] The present invention also provides a secondary battery including the above-mentioned negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. Effect of the Invention
[0018] The present invention relates to an anode active material containing artificial graphite particles, wherein the solid content value at the maximum torque value of the sample, measured by a specific method, is 69.5% by weight or more when the sample is composed of the anode active material and water and is measured by a torque rheometer. When the solid content value at the maximum torque value is within the above range, the anode active material can be evaluated as having excellent powder fluidity, and when the anode active material is included in an anode slurry, the dispersibility and phase stability can be improved. Therefore, the productivity and quality of the anode slurry containing the anode active material of the present invention, and the anode and secondary battery manufactured therefrom are improved. [Brief description of the drawings]
[0019] [Figure 1] 1 shows a graph of the solids content and torque value of a sample consisting of the negative electrode active material according to Example 1 and water. [Diagram 2] 1 shows a graph of the solids content and torque value of a sample consisting of the negative electrode active material and water according to Example 2. [Diagram 3] 1 shows a graph of the solid content and torque value of a sample made of the negative electrode active material and water according to Comparative Example 1. [Figure 4] 1 shows a graph of the solid content and torque value of a sample made of a negative electrode active material and water according to Comparative Example 2. [Diagram 5] 1 is a graph showing the change in shear viscosity according to the shear rate for Example A, Example B, Example C, Comparative Example A, Comparative Example B, and Comparative Example C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their general or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.
[0021] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless it has a clearly different meaning in the context.
[0022] It should be understood that in this specification, terms such as "comprises," "comprises," or "having" specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more different features, numbers, steps, components, or combinations thereof.
[0023] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and can provide results with high reproducibility and high resolution.
[0024] As used herein, the term "primary particle" refers to a single particle, and the term "secondary particle" refers to an aggregate formed by agglomerating a plurality of the primary particles through an intentional granulation or bonding process.
[0025] The present invention will be specifically described below.
[0026] negative electrode active material The present invention relates to a negative electrode active material, specifically, to a negative electrode active material for a lithium secondary battery.
[0027] Specifically, the negative electrode active material is a negative electrode active material containing artificial graphite particles, and when a sample consisting of the negative electrode active material and water is measured with a torque rheometer, the solid content value of the sample at the time when it has a maximum torque value is 69.5 wt % or more, and the solid content value of the sample at the time when it has a maximum torque value is measured by a method including the following steps (a) to (c).
[0028] (a) placing the negative electrode active material in a sample container of a torque rheometer; (b) operating the torque rheometer while injecting water into a sample container of the torque rheometer at a predetermined rate to measure a torque value according to a solid content value of the sample; and (c) deriving a value of the solids content at the time when the sample has a maximum torque value in step (b).
[0029] Conventionally, artificial graphite exhibits hydrophobicity, and therefore when it is added to water as a negative electrode slurry solvent, it has a problem of poor dispersibility and reduced slurry phase stability. In addition, such a dispersibility problem causes a filter clogging problem during the transfer of the negative electrode slurry during the negative electrode manufacturing process, which reduces the efficiency and quality of the entire secondary battery manufacturing process.
[0030] In order to solve such problems, the present invention relates to an anode active material containing artificial graphite particles, wherein the solid content value at the maximum torque value of the sample measured by a specific method during torque rheometer measurement of a sample consisting of the anode active material and water is 69.5% by weight or more. When the solid content value at the maximum torque value during torque rheometer measurement satisfies the above range, the anode active material can be evaluated as having excellent powder fluidity, and when the anode active material is included in an anode slurry, dispersibility and phase stability can be improved. Therefore, the productivity and quality of the anode slurry containing the anode active material of the present invention, and the anode and secondary battery manufactured therefrom are improved.
[0031] The negative electrode active material includes artificial graphite particles. Artificial graphite is manufactured by heat treating amorphous carbon at a high temperature (e.g., 2,500°C to 3,200°C), and is different from natural graphite in that it is an artificially synthesized graphite.
[0032] The artificial graphite particles may be in the form of primary particles, or in the form of secondary particles formed by granulating two or more primary particles. More specifically, the artificial graphite particles may be in the form of secondary particles formed by granulating two or more primary particles, which is preferable in terms of slurry dispersibility and phase stability.
[0033] When the artificial graphite particles are in the form of secondary particles, voids may be formed within the artificial graphite particles, and the voids may be empty spaces formed between primary particles, may be amorphous, and there may be two or more voids.
[0034] In the present invention, the method for producing the artificial graphite particles is not particularly limited as long as it satisfies the "solid content value at which the maximum torque value is obtained" described below.
[0035] Specifically, when the artificial graphite particles are in the form of secondary particles, the artificial graphite particles may be prepared by mixing a carbon precursor and a binder material (e.g., pitch), performing a spheronization and granulation process to prepare an intermediate in the form of secondary particles, and heat-treating the intermediate at a temperature of 2,500°C or more, specifically 3,000°C or more to graphitize it. Here, the carbon precursor may be coal-based heavy oil, petroleum-based heavy oil, tar, pitch, coke, etc., and specifically may be at least one selected from the group consisting of coke and pitch. Here, a spheronization process may be further performed on the carbon precursor, in which case the surface of the primary artificial graphite particles may be made smoother, thereby improving the wettability of the secondary-particle artificial graphite particles, improving the fluidity of the negative electrode active material powder, and improving the solid content value at the maximum torque value of a sample consisting of the negative electrode active material and water described below to a preferred level. The spheronization process performed on the carbon precursor may be performed, for example, using a jet mill, specifically a counter jet mill, in which the rotation speed of the jet mill may be 8 Hz or more, specifically 10 Hz or more, more specifically 15 Hz or more, and 50 Hz or less, specifically 40 Hz or less, and further specifically 30 Hz or less. The spheronization process performed on the carbon precursor may be performed for 3 minutes to 60 minutes, specifically 5 minutes to 15 minutes.
[0036] In addition, when the artificial graphite particles are in the form of secondary particles, the artificial graphite particles may be prepared by mixing the artificial graphite particles in the form of primary particles with a binder material (e.g., pitch), spheroidizing, agglomerating, and heat-treating the primary particles to agglomerate them into secondary particles. Here, the primary particles of the artificial graphite particles may be prepared by graphitizing a carbon precursor through heat treatment at a temperature of 2,500°C or higher, specifically 3,000°C or higher. The carbon precursor may be coal-based heavy oil, petroleum-based heavy oil, tar, pitch, coke, etc., and specifically may be at least one selected from the group consisting of coke and pitch. Here, the primary particle-shaped artificial graphite particles or the carbon precursor used in the preparation of the primary particle-shaped artificial graphite particles may be subjected to a spheronization process, in which case the surface of the primary artificial graphite particles may be made smoother, thereby improving the wettability of the secondary particle-shaped artificial graphite particles, improving the fluidity of the negative electrode active material powder, and improving the solid content value at the maximum torque value of a sample consisting of the negative electrode active material and water, which will be described later, to a preferred level. The primary particle-shaped artificial graphite particles or the carbon precursor used in the preparation of the primary particle-shaped artificial graphite particles may be subjected to a spheronization process using, for example, a jet mill, specifically a counter jet mill, in which the rotation speed of the jet mill may be 8 Hz or more, specifically 10 Hz or more, more specifically 15 Hz or more, and 50 Hz or less, specifically 40 Hz or less, more specifically 30 Hz or less. In addition, the spheronization process performed on the primary particle-type artificial graphite particles or the carbon precursor used in the preparation of the primary particle-type artificial graphite particles may be performed for 3 minutes to 60 minutes, specifically 5 minutes to 15 minutes.
[0037] In the present invention, the solid content of a sample consisting of the negative electrode active material and water is 69.5% by weight or more when the sample has a maximum torque value in torque rheometer measurement.
[0038] The solid content value at the time when the sample has the maximum torque value can be measured by a method including the following steps (a) to (c).
[0039] (a) placing the negative electrode active material in a sample container of a torque rheometer; (b) operating the torque rheometer while injecting water into a sample container of the torque rheometer at a predetermined rate to measure a torque value according to a solid content value of the sample; and (c) deriving a value of the solids content at the time when the sample has a maximum torque value in step (b).
[0040] The torque rheometer is a device for measuring rheological properties caused by flow generated by rotating a fluid, etc., and can measure, for example, viscosity-related torque generated by resistance of a fluid formed by shearing action, and various rheological properties resulting therefrom, etc. An example of the torque rheometer is a Measuring Mixers device manufactured by Brabender.
[0041] Specifically, in the present invention, the negative active material is placed in a sample container of the torque rheometer, and while water is being poured into the sample container at a predetermined speed, the sample in the sample container is stirred using two blades, and the torque value depending on the solid content of the sample consisting of the negative active material and water can be measured. A graph showing the torque value depending on the solid content of the sample can be obtained by the analysis device of the torque rheometer.
[0042] The phase stability and dispersibility of the negative electrode slurry containing the negative electrode active material can be predicted by measuring the solid content of the sample when the sample has a maximum torque value using a torque rheometer. When the solid content of the sample consisting of the negative electrode active material and water is 69.5 wt % or more when the sample has a maximum torque value, the negative electrode active material can be evaluated as having excellent wettability with respect to water and excellent fluidity of the negative electrode active material powder. The negative electrode active material having the above-mentioned characteristics has the advantage of being excellent in dispersibility when added to a negative electrode slurry, improving the phase stability of the slurry, and improving the productivity and quality of the negative electrode manufacturing process. For example, when the solid content of the sample consisting of the negative electrode active material and water is less than 69.5 wt %, the fluidity of the powder is poor, reducing the dispersibility and phase stability of the negative electrode slurry, which may cause filter clogging during the negative electrode slurry transfer process, thereby reducing the productivity and quality of the negative electrode.
[0043] In step (a), the volume of the negative electrode active material placed in the sample container can be 55 mL.
[0044] In step (b), the rate at which the water is injected may be 1 mL / min. The stirring speed of the sample container or the rotation speed of the two blades in the sample container may be 50 rpm. The temperature of the sample container when the torque rheometer is driven may be 25° C.
[0045] The solid content value at which the sample comprising the negative active material and water according to the present invention has a maximum torque value can be obtained by adjusting the shape, surface roughness, etc., in the manufacturing process of the negative active material, for example, by adjusting the spheroidization speed, spheroidization time, etc., in the manufacturing process of artificial graphite. For example, the solid content value at which the sample has a maximum torque value according to the present invention can be achieved by increasing the spheroidization speed in order to make the shape of the negative active material smooth and gentle, and more specifically, by performing a spheroidization process on primary artificial graphite particles or a carbon precursor that will become primary artificial graphite particles in the manufacturing process of artificial graphite in the form of secondary particles, and appropriately adjusting the spheroidization speed and time, but is not limited thereto.
[0046] The compressed density of the negative electrode active material measured by a powder flow test is 850 kg / m 3 ~1,200kg / m 3 , specifically 900kg / m 3 ~950kg / m 3 When the compressed density of the negative active material measured by a powder flow test satisfies the above range, the negative active material can be evaluated as being close to a sphere, and thus the flowability and dispersibility of the negative active material can be further improved.
[0047] The compressed density of the negative active material may be measured using a powder flow analyzer, for example, by repeating a process of placing the negative active material in a powder flow analyzer and applying normal stress and shear stress to the negative active material with a lid five times, and measuring the density of the compressed negative active material. The compressed density of the negative active material may be measured using a powder flow analyzer (instrument name: PFT) manufactured by Brookfield Engineering Laboratories, Inc., Middleborough, Massachusetts, USA. The compressed density may be measured in accordance with ASTM D6128.
[0048] The sphericity of the negative electrode active material may be 0.75 to 1, specifically 0.78 to 0.95. When it is within the above range, the fluidity and dispersibility of the negative electrode active material can be further improved. However, the effect of improving the fluidity and dispersibility of the negative electrode active material cannot be achieved by only increasing the sphericity of the negative electrode active material, and it is necessary to satisfy the "solid content value at the time when the maximum torque value is obtained" of the sample consisting of the negative electrode active material and water described above.
[0049] The sphericity can be measured using a particle shape analyzer (eg, a Morphologi M4 instrument manufactured by Malvern Panalytical).
[0050] The average particle size (D 50 In the above range, the specific surface area is adjusted to a small level, the amount of dispersant that must be added during preparation of the negative electrode slurry can be minimized, and the average particle diameter (D 50 ) becomes excessively large, the problems of aggregation and decreased phase stability can be prevented, and this is preferable in terms of improving processability and thereby improving battery performance.
[0051] The BET specific surface area of the negative electrode active material is 0.1 m 2 / g~2.0m 2 / g, specifically 0.6m 2 / g~1.2m 2 / g, more specifically 0.6m 2 / g~0.9m 2 / g, and within this range, the specific surface area can be adjusted to a suitable small level, minimizing the amount of dispersant that must be added during preparation of the negative electrode slurry, which is preferable in terms of improving processability and therefore battery performance. The BET specific surface area can be measured using a BEL Sorption instrument (manufactured by BEL Japan).
[0052] The negative active material may further include an amorphous carbon coating layer located on a surface of the artificial graphite particle, which may improve the structural stability of the artificial graphite particle and help prevent a side reaction between the negative active material and an electrolyte.
[0053] The amorphous carbon coating layer may be formed in an amount of 0.1 wt % to 10 wt %, preferably 1 wt % to 5 wt %, based on the total weight of the negative active material. The presence of the amorphous carbon coating layer can improve the structural stability of the negative active material, but excessive formation of the amorphous carbon coating layer can cause a decrease in initial efficiency due to an increase in specific surface area during rolling of the negative electrode, and can degrade high-temperature storage performance, so it is preferable to form the carbon coating layer in the above-mentioned range.
[0054] The amorphous carbon coating layer may be formed by providing a carbon coating layer precursor to artificial graphite particles and then heat treating the same.
[0055] The carbon coating layer precursor may include at least one selected from the group consisting of polymer resin and pitch. Specifically, the polymer resin may include at least one selected from the group consisting of sucrose, phenol resin, naphthalene resin, polyvinyl alcohol resin, furfuryl alcohol resin, polyacrylonitrile resin, polyamide resin, furan resin, cellulose resin, styrene resin, polyimide resin, epoxy resin, vinyl chloride resin, and polyvinyl chloride. The pitch may include at least one selected from the group consisting of coal-based pitch, petroleum-based pitch, and mesophase pitch. The heat treatment process for forming the amorphous carbon coating layer may be performed at 1,000°C to 1,500°C in order to uniformly form the amorphous carbon coating layer.
[0056] Anode slurry The present invention also provides an anode slurry, which may be used to manufacture an anode for a lithium secondary battery.
[0057] The negative electrode slurry may include the above-mentioned negative electrode active material, a negative electrode binder, a negative electrode conductive material, and a solvent.
[0058] The negative electrode slurry according to the present invention includes the above-mentioned negative electrode active material, and has excellent dispersibility and improved phase stability. In particular, the negative electrode slurry according to the present invention exhibits excellent dispersibility and phase stability even when the solid content of the negative electrode slurry is increased, thereby improving the productivity and quality of high-capacity negative electrodes and secondary batteries.
[0059] The negative electrode active material may be contained in the negative electrode slurry in an amount of 80% by weight to 99% by weight, preferably 88% by weight to 98% by weight, based on the weight of the solid content of the negative electrode slurry.
[0060] The rest of the negative electrode active material is as described above.
[0061] The negative electrode binder is a component that helps bind between the negative electrode active material and / or the current collector, and may be included in the negative electrode slurry in an amount of 1 wt % to 30 wt %, preferably 1 wt % to 10 wt %, based on the weight of the solid content of the negative electrode slurry.
[0062] The negative electrode binder can include at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, and fluororubber, preferably at least one selected from polyvinylidene fluoride and styrene-butadiene rubber.
[0063] The negative electrode conductive material is a component for further improving the conductivity of the negative electrode active material, and may be contained in the negative electrode slurry in an amount of 1 wt % to 30 wt %, preferably 1 wt % to 10 wt %, based on the weight of the solid content of the negative electrode slurry.
[0064] The negative electrode conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the negative electrode conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based materials (such as those manufactured by Chevron Chemical Company, Denka Singapore Private Limited, or Gulf Oil Company), Ketjenblack, EC-based materials (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).
[0065] The solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and more specifically, may be water. The negative electrode slurry according to the present invention can significantly prevent problems of decreased dispersibility and decreased phase stability caused by using a negative electrode active material including artificial graphite particles.
[0066] The negative electrode slurry may further include a thickener to improve dispersibility.
[0067] As the thickener, any thickener that has been used in the prior art lithium secondary batteries may be used, and an example thereof is carboxymethyl cellulose (CMC).
[0068] The negative electrode slurry may have a solid content of 46 wt % or more, specifically, 47 wt % to 56 wt %, based on the total weight of the negative electrode slurry.
[0069] According to the present invention, the use of the above-mentioned negative electrode active material improves the dispersibility and phase stability of the negative electrode slurry, so that even when the negative electrode slurry is prepared with a solid content within the above range, excellent levels of dispersibility and phase stability can be ensured.
[0070] When the negative electrode slurry has a solid content of 46 wt % or more, specifically 47 wt % to 56 wt %, the viscosity at 23° C. may be 4,500 cP to 10,000 cP, specifically 4,800 cP to 7,800 cP.
[0071] Meanwhile, when the solid content of the negative electrode slurry is 46 wt % or more, specifically, 47 wt % to 56 wt %, the gradient of the shear thickening slope obtained when measuring the shear viscosity according to the shear rate may have a negative (-) value.
[0072] When the gradient of the thickening slope of the negative electrode slurry is negative (-), the slurry can pass through a filter smoothly, specifically, can pass through a 125 mesh filter, and does not clog the filter when passed through. The less the thickening phenomenon of the negative electrode slurry is, the smoother the slurry passes through the filter. When a strong shear is applied to the filter, the negative electrode active material slurry that shows a large thickening is likely to clog the filter, and this tendency can be quantitatively evaluated by the thickening slope value.
[0073] The thickening slope gradient can be determined by measuring the shear viscosity of the negative active material slurry according to the shear rate using a rheometer, converting the viscosity value of a section showing a thickening phenomenon to a log value, and drawing a straight line graph by linear fitting from the start point to the end point of the thickening phenomenon.
[0074] negative electrode The present invention also provides a negative electrode, specifically a negative electrode for a lithium secondary battery, which may include the above-mentioned negative electrode active material.
[0075] Specifically, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, and the negative electrode active material layer includes the above-mentioned negative electrode active material.
[0076] The negative electrode current collector can be any negative electrode current collector commonly used in the art, and is not particularly limited as long as it does not cause chemical changes in the lithium secondary battery and has high conductivity. For example, the negative electrode current collector can include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and aluminum-cadmium alloy, and preferably copper.
[0077] The negative electrode current collector may have fine irregularities on its surface to strengthen the binding force of the negative electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0078] The negative electrode current collector may generally have a thickness of 3 μm to 500 μm.
[0079] The negative electrode active material layer may be disposed on at least one surface of the negative electrode current collector. Specifically, the negative electrode active material layer may be disposed on one or both surfaces of the negative electrode current collector.
[0080] The negative electrode active material layer contains the above-mentioned negative electrode active material.
[0081] The negative electrode active material layer may contain 80% by weight to 99% by weight, preferably 88% by weight to 98% by weight, of the negative electrode active material.
[0082] The rest of the negative electrode active material is as described above.
[0083] The negative electrode active material layer may further include a negative electrode binder, a negative electrode conductive material, and / or a thickener in addition to the above-mentioned negative electrode active material.
[0084] The negative electrode binder, which is a component that helps bind between the active material and / or the current collector, may be typically included in the negative electrode active material layer in an amount of 1 wt % to 30 wt %, preferably 1 wt % to 10 wt %.
[0085] The rest of the negative electrode binder is as described above.
[0086] As the thickener, any thickener that has been used in the past for lithium secondary batteries can be used, and an example thereof is carboxymethyl cellulose (CMC).
[0087] The negative electrode conductive material can be contained in the negative electrode active material layer in an amount of 1 to 30% by weight, preferably 1 to 10% by weight, as a component for further improving the conductivity of the negative electrode active material.
[0088] The rest of the negative electrode conductive material is as described above.
[0089] The thickness of the negative electrode active material layer may be, but is not limited to, 10 μm to 150 μm, specifically 50 μm to 100 μm.
[0090] The negative electrode active material layer may be manufactured by applying the above-mentioned negative electrode slurry to the negative electrode current collector, rolling, and drying the slurry.
[0091] secondary battery The present invention also provides a secondary battery, more specifically a lithium secondary battery, including the above-mentioned negative electrode.
[0092] The secondary battery may include the above-mentioned negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte.
[0093] The positive electrode can face the negative electrode.
[0094] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.
[0095] The positive electrode current collector can be any positive electrode current collector commonly used in the art, and is not particularly limited as long as it does not cause chemical changes in the secondary battery and has high conductivity.For example, the positive electrode current collector can include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and aluminum-cadmium alloy, and preferably aluminum.
[0096] The positive electrode current collector may have fine irregularities on its surface to strengthen the binding force of the positive electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0097] The positive electrode current collector can generally have a thickness of 3 μm to 500 μm.
[0098] The positive electrode active material layer may include a positive electrode active material.
[0099] The positive electrode active material can include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium as a compound capable of reversible intercalation and deintercalation of lithium. More specifically, the lithium composite metal oxide can be a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), a lithium-nickel-manganese-cobalt-based oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or a lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are, as atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc.), and one or more of these compounds can be included. Among them, in terms of enhancing the capacity characteristics and stability of the battery, the lithium composite metal oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Mn 0.15 Co 0.05 )O2, etc.), and considering the significance of the improvement effect by controlling the types and content ratios of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide can be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and one or more mixtures of these can be used.
[0100] The positive electrode active material can be contained in the positive electrode active material layer in an amount of 80% to 99% by weight.
[0101] The positive electrode active material layer may further contain, in addition to the positive electrode active material, at least one selected from the group consisting of a binder and a conductive material.
[0102] The binder is a component that facilitates binding between the active material and the conductive material and between the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the positive electrode mixture. Examples of such binders include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber.
[0103] The binder may be included in the positive electrode active material layer in an amount of 1% by weight to 30% by weight.
[0104] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black (Chevron Chemical Company, Denka Singapore Private Limited, Gulf Oil Company, etc.), Ketjenblack, EC (Armak Company), Vulcan XC-72 (Cabot Company), and Super P (Timcal).
[0105] The conductive material may be added in an amount of 1% by weight to 30% by weight in the positive electrode active material layer.
[0106] The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.
[0107] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0108] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0109] The organic solvent can be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant capable of enhancing the charge / discharge performance of a battery and a low-viscosity linear carbonate-based compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, and the electrolyte solution can exhibit excellent performance.
[0110] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0111] As described above, the lithium secondary battery according to the present invention stably exhibits excellent discharge capacity, rapid charging characteristics and capacity retention rate, and is therefore useful in portable devices such as mobile phones, notebook computers, digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), and can be particularly preferably used as a constituent battery of medium- to large-sized battery modules. Thus, the present invention also provides a medium- to large-sized battery module including the above-mentioned secondary battery as a unit cell.
[0112] Such a medium- to large-sized battery module can be preferably used as a power source that requires high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.
[0113] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.
[0114] Examples and Comparative Examples (1) Preparation of negative electrode active material Negative electrode active materials of Example 1, Example 2, Comparative Example 1, and Comparative Example 2 as shown in Table 1 below were prepared.
[0115] Example 1: Preparation of negative electrode active material The coke raw material was pulverized, air-classified, and spheronized to produce a carbon precursor in the form of primary particles, and then the carbon precursor was mixed with pitch and spheronized to produce an intermediate in the form of secondary particles, which was then heat-treated at 3,000°C to be graphitized, thereby producing artificial graphite particles in the form of secondary particles in which two or more primary artificial graphite particles are aggregated. Here, the spheronization during the production of the carbon precursor was performed for 10 minutes using a counter jet mill (rotation speed: 10 Hz).
[0116] The artificial graphite particles and pitch were mixed and then heat-treated at 1,200° C. to form an amorphous carbon coating layer on the surface of the artificial graphite particles, thereby preparing a negative active material. The amorphous carbon coating layer was included in the negative active material at 3 wt %.
[0117] The negative electrode active material has a sphericity of 0.79 and an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 0.7 m 2 / g.
[0118] Example 2: Preparation of negative electrode active material A negative active material was prepared in the same manner as in Example 1, except that the rotation speed of the counter jet mill in the spheronization process in preparing the carbon precursor was adjusted to 25 Hz.
[0119] The negative electrode active material has a sphericity of 0.81 and an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 0.8 m 2 / g.
[0120] Comparative Example 1: Production of negative electrode active material A negative active material of Comparative Example 1 was prepared in the same manner as in Example 1, except that the spheronization process was not performed during the preparation of the carbon precursor.
[0121] The negative electrode active material has a sphericity of 0.74 and an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 0.8 m 2 / g.
[0122] Comparative Example 2: Production of negative electrode active material A negative active material was prepared in the same manner as in Example 1, except that the rotation speed of the counter jet mill in the spheronization process during the preparation of the carbon precursor was adjusted to 5 Hz and the spheronization time was set to 20 minutes.
[0123] The negative electrode active material has a sphericity of 0.81 and an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 0.8 m 2 / g.
[0124] [Table 1]
[0125] 1) The solid content value when the sample has the maximum torque value A Brabender Measuring Mixers instrument was used as the torque rheometer.
[0126] The "solid content value at the time when the maximum torque value is obtained" was measured by the following method.
[0127] Step (a): 55 mL of the negative electrode active material of Example 1 was placed in a sample container of the torque rheometer. Step (b): While injecting water into the sample container at a rate of 1 mL / min, the torque rheometer was operated to rotate the two blades in the sample container at 50 rpm to stir the sample. During this process, the analysis software of the torque rheometer was driven to measure the torque value according to the solid content value, and a graph of the X-axis solid content value (unit: weight %) and the Y-axis torque value (unit: N m) was drawn as shown in Figure 1. Step (c): The graph obtained in step (b) was analyzed to determine the "solid content value at which the maximum torque value was obtained" for the sample consisting of the negative electrode active material and water.
[0128] As described above, the "solid content value at the time when the sample had the maximum torque value" was determined for Example 2, Comparative Example 1, and Comparative Example 2. Graphs of the solid content value and torque value of the samples consisting of the negative electrode active material and water of Example 2, Comparative Example 1, and Comparative Example 2 are shown in Figures 2, 3, and 4, respectively.
[0129] 2) Spheroidization degree The sphericity of the negative electrode active material was measured using a Morphologi M4 instrument manufactured by Malvern Panalyrical Co., Ltd. Specifically, a sample of the negative electrode active material was prepared, and the sphericity of the powder in the sample was measured using the instrument, and the average value of these values was taken as the sphericity of the negative electrode active material.
[0130] 3) Average particle size (D 50 ) Average particle size of the negative electrode active material (D 50 The particle size distribution curve of the particles is obtained using the laser diffraction method, and the particle size corresponding to 50% of the cumulative volume is calculated. This is called the average particle size (D 50 ) was defined as
[0131] 4) BET specific surface area The BET specific surface area of the negative electrode active material was measured using a BEL Sorption instrument (manufactured by BEL Japan).
[0132] (2) Preparation of negative electrode slurry Example A The negative electrode active material of Example 1, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0133] The solid content of the negative electrode slurry was adjusted to 48 wt % based on the total weight of the negative electrode slurry.
[0134] The viscosity of the negative electrode slurry at 25° C. was 7,500 cP.
[0135] Example B The negative electrode active material of Example 2, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0136] The solid content of the negative electrode slurry was adjusted to 53 wt % based on the total weight of the negative electrode slurry.
[0137] The viscosity of the negative electrode slurry at 25° C. was 6,000 cP.
[0138] Example C The negative electrode active material of Example 2, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0139] The solid content of the negative electrode slurry was adjusted to 48 wt % based on the total weight of the negative electrode slurry.
[0140] The negative electrode slurry had a viscosity of 5,000 cP at 25°C.
[0141] Comparative example A The negative electrode active material of Comparative Example 1, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0142] The solid content of the negative electrode slurry was adjusted to 46 wt % based on the total weight of the negative electrode slurry.
[0143] The viscosity of the negative electrode slurry at 25° C. was 8,000 cP.
[0144] Comparative example B The negative electrode active material of Comparative Example 1, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0145] The solid content of the negative electrode slurry was adjusted to 48 wt % based on the total weight of the negative electrode slurry.
[0146] The viscosity of the negative electrode slurry at 25° C. was 9,500 cP.
[0147] Comparative example C The negative electrode active material of Comparative Example 2, styrene-butadiene rubber (SBR) as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 96:1:1:2 to obtain a negative electrode slurry.
[0148] The solid content of the negative electrode slurry was adjusted to 48 wt % based on the total weight of the negative electrode slurry.
[0149] The viscosity of the negative electrode slurry at 25° C. was 8,000 cP.
[0150] Experimental Example Experimental example 1: Filter test A filter test was performed by passing each of the negative electrode slurries prepared in Example A, Example B, Example C, Comparative Example A, Comparative Example B, and Comparative Example C through a 125 mesh filter. If the filter was clogged with the negative electrode slurry, it was marked as "X", and if no filter clogging was found, it was marked as "O". The results are shown in Table 2 below.
[0151] Experimental Example 2: Measurement of thickening slope value A Hakke Rheometer (manufactured by Thermo Scientific) was used to measure the shear viscosity as a function of shear rate for the negative electrode slurries produced in Example A, Example B, Example C, Comparative Example A, Comparative Example B, and Comparative Example C. The change in shear viscosity (unit: Pa s) as a function of shear rate (unit: 1 / s) is shown in FIG.
[0152] The viscosity value in the range showing shear thickening in the measured shear viscosity was converted to a log value, and the gradient of the slope value (linear fitting value) was determined to be positive (+) or negative (-), and this is shown in Table 2.
[0153] [Table 2]
[0154] Referring to Table 2, it can be seen that the negative electrode slurries of Examples A, B, and C including the negative electrode active material according to the present invention have superior phase stability and significantly improved dispersibility of the negative electrode active material compared to the negative electrode slurries of Comparative Examples A, B, and C.
Claims
1. A negative electrode active material containing artificial graphite particles, When a sample composed of the negative electrode active material and water is measured with a torque rheometer, the solid content of the sample at the time when the sample has a maximum torque value is 69.5% by weight or more; The solid content value at the time when the sample has the maximum torque value is determined by the following steps (a) to (c): (a) placing the negative electrode active material in a sample container of a torque rheometer; (b) operating the torque rheometer while injecting water into a sample container of the torque rheometer at a predetermined rate to measure a torque value according to a solid content value of the sample; and (c) deriving a value of the solids content at the time when the sample has a maximum torque value in step (b); The negative electrode active material is measured by a method comprising the steps of:
2. The negative electrode active material according to claim 1 , wherein the negative electrode active material has a sphericity of 0.75 to 1.
3. The compressed density of the negative active material measured by a powder flow test is 850 kg / m 3 ~1,200kg / m 3 The negative electrode active material according to claim 1 ,
4. The negative electrode active material according to claim 1 , wherein the artificial graphite particles are in the form of secondary particles formed by granulating two or more primary particles.
5. The average particle size (D 50 2. The negative electrode active material according to claim 1, wherein the thickness of the first electrode is 14 μm to 20 μm.
6. The BET specific surface area of the negative electrode active material is 0.1 m 2 / g to 2.0 m 2 The negative electrode active material according to claim 1 , wherein the molecular weight of the negative electrode active material is 1 / g.
7. The negative electrode active material of claim 1 , further comprising an amorphous carbon coating layer located on a surface of the artificial graphite particles.
8. The negative active material of claim 7 , wherein the amorphous carbon coating layer is included in the negative active material in an amount of 0.01% to 10% by weight.
9. The negative electrode active material according to claim 1 , A negative electrode binder; A negative electrode conductive material; a solvent.
10. 10. The negative electrode slurry of claim 9, wherein the negative electrode slurry has a solids content of 46 wt% or more, based on a total weight of the negative electrode slurry.
11. 10. The negative electrode slurry of claim 9, wherein when the solid content of the negative electrode slurry is 46 wt% or more, a gradient of a thickening slope obtained when measuring a shear viscosity according to a shear rate has a negative value.
12. A negative electrode current collector; a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, The negative electrode active material layer comprises the negative electrode active material according to claim 1 .
13. The negative electrode according to claim 12 ; A positive electrode facing the negative electrode; a separator interposed between the negative electrode and the positive electrode; and an electrolyte.
Citation Information
Patent Citations
Slurry for forming negative electrode film of non- aqueous secondary battery and control method of slurry
JP2003217573A
Method for manufacturing graphite paste
JP2015032369A
Manufacturing method of paste anode manufacturing precursor, manufacturing method of anode manufacturing paste, manufacturing method of anode for lithium ion secondary battery, and manufacturing method of lithium ion secondary battery
JP2020074292A
Lithium ion secondary battery and production method therefor
WO2013018179A1
Method for manufacturing paste for manufacturing negative electrode, method for manufacturing negative electrode for lithium ion secondary cell, negative electrode for lithium ion secondary cell, and lithium ion secondary cell
WO2014141552A1