Silicon subhalide-containing composite particles

Subhalogenated silicon-containing composite particles address the limitations of silicon-based anodes by enhancing stability and reducing energy consumption, achieving high capacity and stability in lithium-ion batteries through halogen-containing precursors and porous structures.

JP2024545001AActive Publication Date: 2024-12-05WACKER CHEMIE AG

Patent Information

Application Number
JP2024529182
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-16
Publication Date
2024-12-05
Estimated Expiration
2041-11-16

AI Technical Summary

Technical Problem

Current silicon-based anode materials for lithium-ion batteries suffer from low electrochemical capacity, irreversible capacity decay due to mechanical stress from volume changes and excessive SEI formation, and require high-energy, time-consuming deposition processes.

Method used

Development of subhalogenated silicon-containing composite particles with silicon deposited within and on the pores of porous particles, utilizing halogen-containing silicon precursors to enhance stability and reduce decomposition temperatures, while maintaining comparable performance to halogen-free materials.

Benefits of technology

The composite particles exhibit improved cycle stability, reduced SEI formation, and lower energy consumption in production, resulting in high volumetric capacity and excellent performance properties for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545001000001
    Figure 2024545001000001
  • Figure 2024545001000002
    Figure 2024545001000002
  • Figure 2024545001000003
    Figure 2024545001000003
Patent Text Reader

Abstract

The present invention relates to silicon subhalide-containing composite particles having 3. a Si content >30 wt. %, 4. silicon disposed in and on the pores of a porous matrix, 5. a halogen concentration of 0.0003-16 wt. %, 6. a pH value of 3-9 and 7. a volume weighted particle size distribution with a diameter percentile d50 in the range of 0.5-20 μm, a method for producing the silicon subhalide-containing composite particles, an anode material for a lithium ion battery, the anode material comprising the composite particles, an anode comprising a current collector coated with the anode material and at least one anode comprising the composite particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to porous particles, silicon subhalide-containing composite particles based on silicon and halogens, a method for making the composite particles and their use as active materials in anodes for lithium ion batteries. [Background technology]

[0002] As a storage medium for electric current, lithium-ion batteries are currently the most practical electrochemical energy storage devices with the highest energy density. They are mainly used in the field of portable electronics, but also in tools and motorized means of transport such as bicycles, scooters or cars. Graphitic carbon is currently widely used as the active material of the negative electrode ("anode") of the corresponding batteries. However, such graphitic carbon has the disadvantage of having a relatively low electrochemical capacity. This corresponds theoretically to a maximum of 372 mAh per gram of graphite, thus only about one tenth of the theoretically achievable electrochemical capacity with lithium metal. An alternative active material for the anode uses the addition of silicon, as described for example in EP 3 335 262 B1. Silicon forms a binary electrochemically active alloy with lithium, allowing very high electrochemically achievable lithium contents of up to 4200 mAh per gram of silicon.

[0003] The incorporation and removal of lithium ions in silicon has the drawback of causing very large volume changes, which can reach up to 300% in the case of complete incorporation. Such volume changes subject the silicon-containing active material to severe mechanical stresses that can ultimately result in its decomposition. This method, also known as electrolytic grinding, leads to a permanent and irreversible loss of capacity in the electrode due to the loss of electrical contact in the active material and in the electrode structure.

[0004] Furthermore, the surface of the silicon-containing active material reacts with the constituents of the electrolyte by the continuous formation of a passivating protective layer (solid electrolyte interface; SEI). The formed components are no longer electrochemically active. The lithium bound therein is no longer available to the system, and therefore the battery capacity is continuously and significantly reduced. Due to the extreme change in the volume of silicon during the charging and discharging process of the battery, the SEI periodically ruptures. This exposes the still unoccupied surface of the silicon-containing active material, which is then exposed to further SEI formation. Since the amount of mobile lithium throughout the cell corresponding to the available capacity is limited by the cathode material, the cathode material is increasingly consumed and the capacity of the cell decreases to an extent that is unacceptable from the point of view of the application after only a few cycles.

[0005] The decrease in capacity over the course of several charge and discharge cycles is also called capacity fade or continuous loss, and is usually irreversible.

[0006] Some silicon-carbon composite particles have been described as silicon-containing active materials for the anodes of lithium-ion batteries. Silicon-carbon composite particles are obtained, for example, from the deposition of silicon in porous carbon particles by its pyrolysis of a gaseous or liquid silicon precursor. For example, US 10,147,950 B2 describes the deposition of silicon in porous carbon particles from monosilane SiH4 in a tube furnace or equivalent furnace type at high temperatures of 300-900 °C, preferably with stirring of the particles, by the CVD ("chemical vapor deposition") or PE-CVD ("plasma-enhanced chemical vapor deposition") method. Even composites that can be obtained in this way have insufficient cycle stability for use in demanding applications. In addition, the deposition of silicon requires high temperatures and / or long reaction times, which therefore require a great deal of energy and time. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] European Patent No. 3335262 [Patent Document 2] U.S. Patent No. 10,147,950 Summary of the Invention [Problem to be solved by the invention]

[0008] However, known materials do not claim halogens as constituents. US20140272592A, for example, describes Si / C composites with chlorine contents of up to 1000 ppm (measured by X-ray fluorescence, TXRF), and hypothesizes that higher levels of contamination are detrimental to electrochemical performance. [Means for solving the problem]

[0009] The present invention relates to 1.Si content>30wt%, 2. Silicon disposed within and on the pores of the porous matrix; 3. A halogen concentration of 0.0003 to 16% by weight; 4. pH 3~9 and 5. Diameter percentile d from 0.5 to 20 μm 50 A volume-weighted particle size distribution having The present invention provides silicon subhalide-containing composite particles having the following formula:

[0010] Surprisingly, it has been found that the performance of the halogen-containing materials is comparable to that of non-halogen-containing materials having similar physical properties, and in addition, the halogen-containing materials can be produced from substantially less expensive halogen-containing precursors.

[0011] These halogen-containing precursors are at the same time industrial precursors of halogen-free SiH4, which are produced from H3SiCl, SiH2Cl2 or HSiCl3 and require subsequent energy-intensive distillative purification. Therefore, the use of halosilanes can significantly reduce the CO2 footprint of the entire material concept.

[0012] Moreover, it has been surprisingly found that the decomposition temperatures of halogen-containing silanes in the presence of reactive surfaces (e.g., activated carbon) are substantially lower than previously assumed (J. Phys. Chem. 1990, 94, 327-331, >600° C.).

[0013] The preparation of the silicon subhalide-containing composite particles according to the present invention can be carried out by any desired method.The preparation by deposition of silicon from gas or liquid silicon precursor by infiltration into porous particles, similar to the method described in US10,147,950B2, is a particularly suitable route to the silicon subhalide-containing composite particles according to the present invention.

[0014] The deposition of silicon by pyrolysis from a gas or liquid silicon precursor within the pores and on the surfaces of the porous particles is in this case referred to as silicon infiltration.

[0015] The same or different silicon precursors may be reacted with the same or different porous particles.

[0016] The present invention also relates to a method for producing subhalide silicon-containing composite particles according to the invention by silicon infiltration from silicon precursors selected from halogen-containing silicon precursors which are gaseous and / or liquid at 20° C. and 1013 mbar, wherein at least one halogen-containing silicon precursor is 1. Diameter percentile d from 0.5 to 20 μm 50 A volume weighted particle size distribution having 2.0.4~2.2cm 3 the total pore volume of the micropores and mesopores (Grbic pore volume) measured by N2 adsorption in the range of / g, and PD50 pore diameter measured by N2 adsorption below 3.30 nm wherein the porous particles are in the presence of the porous particles having the formula: DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The silicon is deposited within the pores and on the surfaces of the porous particles.

[0018] Any material may be employed as the porous particles for the composite particles, including porous carbon particles or oxides such as silicon dioxide, aluminum oxide, silicon-aluminum mixed oxide, magnesium oxide, lead oxide, and zirconium oxide, carbides such as silicon carbide and boron carbide, nitrides such as silicon nitride and boron nitride, and oxides having the following formula: Al a B b C c Mg d N e O f S g Other ceramic materials are preferred that can be described by the formula: 3 e*3+f*2.

[0019] The ceramic material may be, for example, a binary, ternary, quaternary, pentanary, hexanary or heptanary compound having the following formula: Non-stoichiometric Boron Nitride BN z In the formula, z=0.2 to 1, Non-stoichiometric carbon nitride CN z Wherein z=0.1 to 4 / 3; Boron carbonitride B x CN z where x=0.1 to 20 and z=0.1 to 20, and where x*3+4 3 z*3, Boron Nitride Oxide BN z O r wherein z=0.1 to 1 and r=0.1 to 1, and wherein 3 3 r*2+z*3), Boron Carbonitride Oxide B x CN z O r where x=0.1 to 2, z=0.1 to 1, and r=0.1 to 1, and where x*3+4 3 r*2+z*3, Silicon Carboxide Si x CO zwhere x=0.1 to 2 and z=0.1 to 2, and where x*4+4 3 z*2, Silicon carbonitride Si x CN z where x=0.1 to 3 and z=0.1 to 4, and where x*4+4 3 z*3, Silicon borocarbonitride Si w B x CN z In the formula, w=0.1 to 3, x=0.1 to 2, and z=0.1 to 4, and in the formula, w*4+x*3+4 3 z*3, Silicon borocarboxide Si w B x CO z In the formula, w=0.10 to 3, x=0.1 to 2, and z=0.1 to 4, and in the formula, w*4+x*3+4 3 z*2), Silicon borocarbonitride oxide Si v B w CN x O z In the formula, v=0.1 to 3, w=0.1 to 2, x=0.1 to 4, and z=0.1 to 3, and in the formula, v*4+w*3+4 3 x*3+z*2 and Aluminum borosilicocarbonitride oxide Al u B v S x CN w O z In the formula, u=0.1 to 2, v=0.1 to 2, w=0.1 to 4, x=0.1 to 2, and z=0.1 to 3, and in the formula, u*3+v*3+x*4+4 3 w*3+z*2 Ceramic materials having the following structure are preferred.

[0020] Preferred porous particles are based on carbon, silicon dioxide, boron nitride, silicon carbide, silicon nitride or mixed materials based on these compounds, in particular based on silicon dioxide or boron nitride.

[0021] Particularly preferred porous particles are porous boron nitride particles, porous silicon oxide particles and / or microporous carbon particles.

[0022] It is preferred to dry the porous particles prior to reaction with the gas or liquid silicon precursor.

[0023] Drying of the porous particles can be carried out at high temperatures of 50-400°C in an inert gas atmosphere in any desired reactor suitable for drying. Inert gases that can be employed are, for example, nitrogen or argon. Alternatively, drying can be carried out at high temperatures of 50-400°C and reduced pressures of 0.001-900 mbar. The drying time is preferably 0.1 seconds to 48 hours. Drying of the porous particles can be carried out in the same reactor as the reaction with the gas or liquid silicon precursor or in a separate reactor suitable for drying.

[0024] The porous particles preferably have a density of 0.1 to 4 g / cm as measured by helium pycnometry. 3 , particularly preferably 0.3 to 3 g / cm 3 It is.

[0025] The porous particles preferably have a diameter percentile d of ≧0.5 μm, particularly preferably ≧1.5 μm, most preferably ≧2 μm. 50 The diameter percentile d 50 is preferably ≦20 μm, particularly preferably ≦12 μm, most preferably ≦8 μm.

[0026] The volume weighted particle size distribution of the porous particles is preferably determined by the diameter percentile d 10 ≧0.2μm~d 90 ≦20.0 μm, particularly preferably d 10 ≧0.4μm~d 90 ≦15.0 μm, most preferably d 10 ≧0.6μm~d 90 ≦12.0 μm.

[0027] The porous particles preferably have a diameter percentile d of ≦10 μm, particularly preferably ≦5 μm, especially preferably ≦3 μm, most preferably ≦2 μm. 10 The diameter percentile d 10 is preferably ≧0.2 μm, particularly preferably ≧0.4, most preferably ≧0.6 μm.

[0028] The porous particles preferably have a diameter percentile d of ≧4 μm, particularly preferably ≧8 μm. 90 The diameter percentile d 90 is preferably ≦20 μm, particularly preferably ≦15, most preferably ≦12 μm.

[0029] The volume-weighted particle size distribution of the porous particles preferably has a width d 90 ~d 10 The volume-weighted particle size distribution of the porous particles preferably has a width d of ≧0.6 μm, particularly preferably ≧0.7 μm, most preferably ≧1.0 μm. 90 ~d 10 has.

[0030] The volume weighted particle size distribution can be measured according to ISO 13320 using static laser scattering using the Mie model on a Horiba LA 950 measuring device with ethanol as the dispersion medium for the porous particles.

[0031] The porous particles can be, for example, isolated or agglomerated. The porous particles are preferably non-agglomerated, preferably non-agglomerated. Agglomerates generally mean that in the course of the production of the porous particles, primary particles are first formed and then fuse and / or the primary particles are linked to each other, for example by covalent bonds, thus forming agglomerates. The primary particles are generally isolated particles. The agglomerates or isolated particles can form agglomerates. Agglomerates are loose collections of agglomerates or primary particles linked to each other, for example by van der Waals interactions or hydrogen bonds. Agglomerated agglomerates can be easily divided back into agglomerates again by common kneading and dispersion processes. Agglomerates can only be partially broken down into primary particles by such processes, if at all. The presence of the porous particles in the form of agglomerates, agglomerates or isolated particles can be visualized, for example, using a conventional scanning electron microscope (SEM). In contrast, static light scattering methods for measuring particle size distribution or particle diameter cannot distinguish between strong and weak agglomerates.

[0032] The porous particles may have any desired morphology, i.e., for example, lobed, flake, spherical or needle-like, preferably lobed or spherical porous particles.

[0033] The morphology can be characterized, for example, by the sphericity ψ or sphericity S. According to Wadell's definition, the sphericity ψ is the ratio of the surface area of ​​a sphere of equal volume to the actual surface area of ​​the object. For a sphere, ψ has the value 1. According to this definition, the porous particles preferably have a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, most preferably 0.65 to 1.0.

[0034] The sphericity S is the ratio of the circumference of a circle with the same area A as the projection of a particle onto a surface to the measured circumference U of this projection: S = 2πA / U. For an ideal circular particle, S can have a value of 1. For a porous particle, the sphericity S is the percentile S of the sphericity distribution. 10 ~S90 Based on the above, it is preferably in the range of 0.5 to 1.0, particularly preferably 0.65 to 1.0. The measurement of the sphericity S is carried out, for example, using photomicrographs of the individual particles by optical microscopy or, in the case of particles <10 μm, preferably using a scanning electron microscope, by graphic evaluation using image analysis software, such as ImageJ.

[0035] The porous particles are preferably ≥ 0.2 cm 3 / g, particularly preferably ≧0.6 cm 3 / g, most preferably ≥ 1.0 cm 3 / g, which is useful for obtaining high-capacity lithium-ion batteries. The gas-accessible pore volume is determined by gas adsorption measurements with nitrogen according to DIN 66134.

[0036] The porous particles are preferably open-pore. Open-pore generally means that the pores are connected to the surface of the particle, for example through channels, and can preferably exchange mass with the environment, especially gaseous compounds. This can be demonstrated by gas adsorption measurements (analysis by Brunauer, Emmett and Teller, "BET"), i.e. specific surface area.

[0037] The porous particles are preferably ≧50 m 2 / g, particularly preferably ≥ 500m 2 / g, most preferably ≥ 1000m 2 / g. The BET surface area is determined in accordance with DIN 66131 (with nitrogen).

[0038] The pores of the porous particles can have any diameter, i.e. generally in the range of macropores (>50 nm), mesopores (2-50 nm) and micropores (<2 nm). The porous particles can be used as any mixture of different pore types. It is preferable to use porous particles with up to 30% macropores, based on the total pore volume, particularly preferably porous particles with no macropores, and especially preferably porous particles with at least 50% pores with an average pore diameter of less than 5 nm. It is particularly preferable for the porous particles to have only pores with a pore diameter of less than 2 nm (measurement method: pore size distribution according to BJH (gas adsorption) in the mesopore range according to DIN 66134 and Horvath-Kawazoe (gas adsorption) in the micropore range according to DIN 66135, evaluation of the pore size distribution in the macropore range is carried out by mercury porosimetry in accordance with DIN ISO 15901-1).

[0039] The PD50 pore diameter of the porous particles is preferably in the range of 0.5 to 30 nm, preferably in the range of 0.5 to 20 nm, particularly preferably in the range of 0.5 to 10 nm. The term "PD50 pore diameter" as used herein refers to the average pore diameter on a volume basis based on the total volume of micropores and mesopores (i.e. 50% of the total volume of micropores and mesopores is found at a pore diameter below that). Thus, according to the present invention, preferably at least 50% of the total volume of micropores and mesopores is in the form of pores with a diameter of less than 30 nm.

[0040] For clarity, it should be noted that in determining the PD50 value, not all macropore volume (pore diameters greater than 50 nm) is taken into account.

[0041] The porous particles preferably have a pH of > 3, preferably > 5, particularly preferably > 6. The pH of the porous particles can be measured according to ASTM Standard No. D1512, Method A.

[0042] The silicon subhalide composite particles according to the invention are composed of one or more porous particles in which silicon subhalide is deposited in the pores and on the surface of the porous particles. The deposited subhalide is composed of silicon and a halogen, preferably chlorine, and has a molar composition SiCl in the range of x=0.00001-0.15, preferably x=0.00001-0.01, particularly preferably x=0.0001-0.05. x In another embodiment, the deposited subhalide has a molar composition SiBr x and / or SiF x and / or SiI x has.

[0043] The silicon subchloride composite particles according to the present invention preferably have a chlorine content of 0.0003 to 16% by weight, preferably 0.0003 to 12% by weight, particularly preferably 0.0003 to 6% by weight.

[0044] The silicon subbromide composite particles according to the present invention preferably have a bromine content of 0.0009 to 30% by weight, preferably 0.0009 to 22% by weight, particularly preferably 0.0009 to 15% by weight.

[0045] The silicon subfluoride composite particles according to the present invention preferably have a fluorine content of 0.0002 to 9% by weight, preferably 0.0002 to 7% by weight, particularly preferably 0.0002 to 3.5% by weight.

[0046] The silicon subiodide composite particles according to the present invention preferably have an iodine content of 0.0015 to 41% by weight, preferably 0.0015 to 31% by weight, particularly preferably 0.0015 to 18% by weight.

[0047] (Method of measurement: preferably X-ray fluorescence analysis on a Bruker AXS S8 Tiger 1 instrument, especially with a rhodium anode).

[0048] The deposited subhalides may further contain the following elements as constituents: H, O, N, C, S, Fe, Ni, Cu, Mo, W, Mn, Al, K, Na, Ca, Ba, Sr, Cr, Mg, Zn, P.

[0049] The silicon subhalide-containing composite particles according to the invention preferably have a diameter percentile d of ≧1.5 μm, particularly preferably ≧2 μm. 50 The diameter percentile d 50 is preferably ≦13 μm, particularly preferably ≦8 μm.

[0050] The volume weighted particle size distribution of the silicon subhalide-containing composite particles according to the present invention is preferably determined by the diameter percentile d 10 ≧0.2μm~d 90 ≦20.0 μm, particularly preferably d 10 ≧0.4μm~d 90 ≦15.0 μm, most preferably d 10 ≧0.6μm~d 90 ≦12.0 μm.

[0051] The silicon subhalide-containing composite particles according to the invention preferably have a diameter percentile d of ≦10 μm, particularly preferably ≦5 μm, especially preferably ≦3 μm, most preferably ≦1 μm. 10 The diameter percentile d 10 is preferably ≧0.2 μm, particularly preferably ≧0.4 μm, most preferably ≧0.6 μm.

[0052] The silicon subhalide-containing composite particles according to the invention preferably have a diameter percentile d of ≧5 μm, particularly preferably ≧10 μm. 90 The diameter percentile d 90 is preferably ≦20.0 μm, particularly preferably ≦15.0 μm, and most preferably ≦12.0 μm.

[0053] The volume-weighted particle size distribution of the silicon subhalide-containing composite particles according to the invention preferably has a width d 90 ~d 10 The volume-weighted particle size distribution of the silicon subhalide-containing composite particles according to the invention preferably has a width d 90 ~d 10 has.

[0054] The silicon-containing composite particles of the present invention are preferably in the form of particles.Particles can be isolated or agglomerates.The silicon-containing composite particles of the present invention are preferably non-agglomerates, preferably non-agglomerates.The terms isolated, agglomerates and non-agglomerates have already been further defined above with respect to porous particles.The presence of the silicon-containing composite particles of the present invention in the form of agglomerates or agglomerates can be visualized, for example, using a conventional scanning electron microscope (SEM).

[0055] The silicon subhalide-containing composite particles according to the present invention may have any desired morphology, i.e., may be, for example, lobed, flake-like, spherical or acicular, preferably lobed or spherical particles.

[0056] According to Wadell's definition, the sphericity ψ is the ratio of the surface area of ​​a sphere of equal volume to the actual surface area of ​​the object. For a sphere, ψ has a value of 1. According to this definition, the silicon subhalide-containing composite particles according to the invention preferably have a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, most preferably 0.65 to 1.0.

[0057] The sphericity S is the ratio of the circumference of a circle having the same area A as the projection of the particle onto the surface to the measured circumference U of this projection: S=2πA / U. For an ideal circular particle, S may have a value of 1. For silicon subhalide-containing composite particles according to the invention, the sphericity S is the percentile S of the sphericity distribution. 10 ~S 90 Based on the above, it is preferably in the range of 0.5 to 1.0, particularly preferably 0.65 to 1.0. The measurement of the sphericity S is carried out, for example, using photomicrographs of the individual particles by optical microscopy or, in the case of particles <10 μm, preferably using a scanning electron microscope, by graphic evaluation using image analysis software, such as ImageJ.

[0058] The cycle stability of lithium ion batteries can be further enhanced by the morphology, material composition, particularly the specific surface area or internal porosity of the silicon subhalide-containing composite particles according to the present invention.

[0059] The silicon subhalide-containing composite particles according to the present invention preferably contain 10 to 90% by weight, more preferably 20 to 80% by weight, particularly preferably 30 to 60% by weight, and especially preferably 40 to 50% by weight of silicon obtained by silicon infiltration, based on the total weight of the silicon subhalide-containing composite particles according to the present invention (preferably measured by elemental analysis such as ICP-OES).

[0060] The volume of silicon subhalide introduced into the porous particles is determined by multiplying the total mass of the silicon subhalide-containing composite particles according to the present invention by the density of silicon (2.336 g / cm 3 ) divided by the mass fraction of silicon subhalide obtained by infiltration from the silicon precursor.

[0061] The pore volume P of the silicon subhalide-containing particles according to the present invention is derived from the sum of the gas-accessible pore volume and the gas-inaccessible pore volume. The Grbic gas-accessible pore volume of the silicon subhalide-containing composite particles according to the present invention can be measured by gas adsorption measurement with nitrogen according to DIN 66134.

[0062] The gas inaccessible pore volume of the silicon subhalide-containing composite particles according to the present invention can be measured by the formula: gas inaccessible pore volume=1 / skeletal density-1 / pure material density.

[0063] Here, the skeletal density is the density of the composite particles according to the invention measured by helium pycnometry according to DIN 66137-2, and the pure material density of the composite particles according to the invention is the theoretical density calculable from the sum of the theoretical pure material densities of the components present in the composite particles according to the invention multiplied by their respective weight percentage proportions in the total material, which gives for the silicon subhalide-containing composite particles: Pure material density = theoretical pure material density of silicon (2.336 g / cm 3 )*proportion of silicon in weight%+density of porous particles (measured by helium pycnometry)*proportion of porous particles in weight%.

[0064] The pore volume P of the silicon subhalide-containing composite particles according to the present invention is preferably in the range of 0 to 400 vol. %, more preferably in the range of 100 to 350 vol. %, particularly preferably in the range of 200 to 350 vol. %, based on the volume of silicon present in the composite particles according to the present invention obtained from silicon infiltration.

[0065] The pores present in the composite particles according to the present invention may be gas-accessible or gas-inaccessible. The volume ratio of gas-accessible pores to gas-inaccessible pores of the silicon subhalide-containing composite particles according to the present invention can generally be in the range of 0 (no gas-accessible pores) to 1 (all pores are gas-accessible). The volume ratio of gas-accessible pores to gas-inaccessible pores of the composite particles according to the present invention is in the range of 0 to 0.8, particularly preferably in the range of 0 to 0.3, particularly preferably in the range of 0 to 0.1.

[0066] The pores of the silicon subhalide-containing composite particles according to the invention can have any desired diameter, for example in the range of macropores (>50 nm), mesopores (2-50 nm) and micropores (<2 nm). The composite particles according to the invention can also contain any desired mixture of different pore types. The composite particles according to the invention preferably contain up to 30% macropores based on the total pore volume, composite particles according to the invention having no micropores are particularly preferred, and composite particles according to the invention comprising at least 50% pores with an average pore diameter of less than 5 nm are very particularly preferred. It is particularly preferred when the silicon subhalide-containing composite particles according to the invention only comprise pores with a diameter of up to 2 nm.

[0067] The silicon subhalide-containing composite particles according to the invention preferably have silicon structures in at least one dimension, preferably with a structure size of up to 1000 nm, more preferably less than 100 nm, particularly preferably less than 5 nm (measurement method: scanning electron microscope (SEM) and / or high-resolution transmission electron microscope (HR-TEM)).

[0068] It is preferred if the silicon subhalide-containing composite particles according to the invention contain silicon or silicon subhalide in the form of a layer in the pores and / or on the outer surface, with a layer thickness of up to 1000 nm, more preferably less than 100 nm, particularly preferably less than 5 nm (measurement method: scanning electron microscope (SEM) and / or high-resolution transmission electron microscope (HR-TEM)). The composite particles according to the invention can also contain silicon or silicon subhalide in the form of a layer formed from silicon particles. The silicon particles preferably have a diameter of up to 1000 nm, more preferably less than 100 nm, particularly preferably less than 10 nm (measurement method: scanning electron microscope (SEM) and / or high-resolution transmission electron microscope (HR-TEM)). The data on the silicon particles preferably relate here to the diameter of the circumference of the particle in the microscopic image.

[0069] The silicon subhalide-containing composite particles according to the present invention have a maximum particle size of 170 m 2 / g, preferably 100m 2 / g, and even more preferably less than 60m 2 / g, particularly preferably less than 20m 2 / g. The BET surface area is measured according to DIN 66131 (with nitrogen). Therefore, the use of the silicon subhalide-containing composite particles according to the present invention as an active material in an anode for a lithium-ion battery can reduce SEI formation and increase initial coulombic efficiency.

[0070] Furthermore, the silicon deposited from the silicon precursor in the silicon-containing material may contain a dopant selected from the group including, for example, Fe, Al, Cu, S, Cl, Zr, Ti, Pt, Ni, Cr, Sn, Ag, Co, Zn, B, P, Sb, Pb, Ge, Bi, rare earths or combinations thereof. Li and / or Sn are preferred. The content of dopant in the silicon subhalide-containing composite particles is preferably at most 1 wt.%, particularly preferably at most 100 ppm, based on the total weight of the composite particles that can be measured by ICP-OES.

[0071] The silicon subhalide-containing composite particles according to the present invention generally have a surprisingly high stability under compressive load and / or shear load.The compressive load stability and shear stability of the composite particles according to the present invention are demonstrated, for example, by the fact that the composite particles according to the present invention show little, if any, change in their porous structure under compressive stress (e.g., during electrode compression) or shear stress (e.g., during electrode preparation) in SEM.

[0072] The preparation of silicon-containing composite particles containing subhalide according to the present invention can be carried out in any desired reactor that is generally used for silicon infiltration.Preferred reactor is selected from fluidized bed reactor, rotary kiln that can be oriented in any desired configuration from horizontal to vertical and fixed bed reactor that can be operated as open or closed system, for example as pressure reactor.Particularly preferred is a reactor that allows homogeneous mixing of the porous particles formed during the infiltration of silicon precursor and silicon-containing material.This is advantageous for the most homogeneous deposition of silicon possible in the pores and on the surface of the porous particles.The most preferred reactor is a fluidized bed reactor, a rotary kiln or a pressure reactor, in particular a fluidized bed reactor or a pressure reactor.

[0073] Silicon is generally deposited from halogen-containing silicon precursors by pyrolysis. Silicon infiltration can employ one silicon precursor or two or more silicon precursors mixed or alternating, and at least one chlorine-containing precursor must be employed. Preferred halogen-containing silicon precursors are trichlorosilane HSiCl3, trifluorosilane HSiF3, tribromosilane HSiBr3, triiodosilane HSiI3, dichlorosilane H2SiCl2, difluorosilane H2SiF2, dibromosilane H2SiBr2, diiodosilane H2SiI2, monochlorosilane H3SiCl, monofluorosilane H3SiF, monobromosilane H3SiBr, monoiodosilane H3SiI, tetrachlorosilane SiCl4, tetrafluorosilane SiF4, tetrabromosilane SiBr4, tetraiodosilane SiI4, hexachlorodisilane Si2 Cl6, hexafluorodisilane Si2F6, hexabromodisilane Si2Br6, hexaiododisilane Si2I6 and higher linear, branched or cyclic homologues, for example 1,1,2,2-tetrachlorodisilane Cl2HSi-SiHCl2, halogenated and partially halogenated oligo- and polysilanes, such as trichloromethylsilane MeSiCl3, dichlorodimethylsilane Me2SiCl2, chlorotrimethylsilane Me3SiCl, tetramethylsilane Me4Si, dichloromethylsilane MeHSiCl2, chloromethylsilane MeH2SiCl, methylchlorosilanes.

[0074] The halogen-free silicon precursors in the mixture are monosilane SiH4, disilane Si2H6 and their higher linear, branched or cyclic homologues, neopentasilane Si5H 12 , Cyclopentasilane, Cyclohexasilane Si6H 12Silicon-hydrogen compounds such as methylsilanes MeH3Si, chlorodimethylsilane Me2HSiCl, dimethylsilane Me2H2Si, trimethylsilane Me3SiH or mixtures of the silicon compounds mentioned. In particular, the silicon precursor is selected from trichlorosilane HSiCl3, dichlorosilane H2SiCl2, monochlorosilane H3SiCl, tetrachlorosilane SiCl4, hexachlorodisilane Si2Cl6 and / or mixtures thereof with H-containing silanes such as monosilane SiH4 or disilane Si2H6. More than 5 ppm of chlorosilanes SiH n Cl 4-n Dichlorosilane H2SiCl2, monochlorosilane H3SiCl and monosilane SiH4 having a ratio of (n=0 to 3) are particularly preferred.

[0075] Silicon-free reactive components may also be present in mixtures or alternation with the silicon precursor.Further reactive components that may be present in the silicon-free reactive components include hydrogen or hydrocarbons selected from the group including aliphatic hydrocarbons having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, such as methane, ethane, propane, butane, pentane, isobutane, hexane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, ethene, acetylene, propene or butene, isoprene, butadiene, divinylbenzene, vinylacetylene, cyclohexadiene, cyclooctadiene, cyclic unsaturated hydrocarbons such as cyclopropene, cyclobutene, cyclopentene, cyclohexene, cyclohexadiene, cyclopentadiene, dicyclopentadiene or norbornadiene, aromatic hydrocarbons such as benzene, toluene, p-, m-, o-xylene, styrene (vinylbenzene), ethylene, ... methylbenzene, diphenylmethane or naphthalene, further aromatic hydrocarbons such as phenol, o-, m-, p-cresol, cymene, nitrobenzene, chlorobenzene, pyridine, anthracene or phenanthrene, myrcene, geraniol, thioterpineol, norbornane, borneol, isoborneol, bornane, camphor, limonene, terpinene, pinene, pinane, carene, phenol, aniline, anisole, furan, furfural, furfuryl alcohol, hydroxymethylfurfural, bishydroxymethylfuran and mixed fractions containing a number of such compounds, for example from natural gas condensates, petroleum distillates or coke oven condensates, mixed fractions from the output streams of fluid catalytic crackers (FCC), steam crackers or Fischer-Tropsch synthesis plants or more generally from hydrocarbon-containing material streams from wood, natural gas, petroleum and coal processing.

[0076] These non-silicon-containing reactive components may also be introduced into the gas space of the reactor alternately with the silicon precursor.

[0077] In a particular embodiment of this process, a mixture of monosilanes or silanes, such as a mixture of monosilane SiH4, trichlorosilane HSiCl3, dichlorosilane H2SiCl2, monochlorosilane H3SiCl and tetrachlorosilane SiCl4, where each component may be present in 0-99.9% by weight, is produced by a suitable process only immediately before use in the reactor. These processes generally proceed from trichlorosilane HSiCl3, which is reconstituted by a suitable catalyst (e.g. AmberLyst™ A21DRY) into the other components of the described mixture. The composition of the resulting mixture is mainly determined by work-up of the mixture formed at one or more different temperatures after one or more reconstitution steps.

[0078] Particularly preferred reactive components are monosilanes SiH4, oligomeric or polymeric silanes, especially those of the general formula Si n H n+2 where n can include an integer ranging from 2 to 10, and the general formula -[SiH2] n -cyclic silanes of the formula: -, where n may comprise an integer ranging from 3 to 10, selected from the group comprising trichlorosilane HSiCl3, dichlorosilane H2SiCl2 and monochlorosilane H3SiCl, which may be employed alone or in mixtures, the use of SiH4, HSiCl3 and H2SiCl2 alone or in mixtures being quite particularly preferred.

[0079] Furthermore, the reactive component may further contain further reactive constituents, such as dopants based on compounds containing boron, nitrogen, phosphorus, arsenic, germanium, iron or nickel, preferably selected from the group comprising ammonia NH3, diborane B2H6, phosphane PH3, germane GeH4, arsane AsH3, iron pentacarbonyl Fe(CO)4 and nickel tetracarbonyl Ni(CO)4.

[0080] The composition of the gas phase may be measured, for example, by a gas chromatograph and / or a thermal conductivity detector and / or an infrared spectrometer and / or a Raman spectrometer and / or a mass spectrometer, thus allowing targeted control of the deposition process. In a preferred embodiment, the hydrogen content is measured using a thermal conductivity detector and / or any chlorosilanes present are measured using a gas chromatograph or a gas infrared spectrometer.

[0081] The silicon subhalide-containing composite particles can also be post-treated and / or passivated. The composite particles are preferably purged with oxygen, in particular with a mixture of inert gas and oxygen, in the same or another reactor. This makes it possible, for example, to modify and / or passivate the surface of silicon and silicon subhalide. It is possible, for example, to cause the reaction of any reactive groups present on the surface of silicon and silicon subhalide. For this purpose, it is preferred to employ a mixture of nitrogen, oxygen and optionally alcohol and / or water, preferably containing up to 20% by volume, particularly preferably up to 10% by volume, particularly preferably up to 5% by volume of oxygen and preferably up to 100% by volume, particularly preferably up to 10% by volume, particularly preferably up to 1% by volume of water. This step is preferably carried out at a temperature of up to 200° C., particularly preferably up to 100° C., particularly preferably up to 50° C. Passivation of the particle surface may also be carried out using a gas mixture containing an inert gas and an alcohol. Here, it is preferred to employ nitrogen and isopropanol. However, it is also possible to employ methanol, ethanol, butanol, pentanol or longer chain and branched alcohols and diols.

[0082] Inactivation of the composite particles may also be carried out by dispersion in a liquid solvent or solvent mixture, which may include, for example, isopropanol or an aqueous solution.

[0083] Passivation of the composite particles can also be selectively carried out by coating using C-, Al- and B-containing precursors at temperatures between 200 and 800° C. and optionally subsequent treatment in an oxygen-containing atmosphere.

[0084] Alternatively, post-treatment of the composite particles can be carried out with water or an aqueous solution. It is preferred to wash the particles several times with water until the pH of the wash water is > 3. The sample can be treated, for example, with ultrasound.

[0085] The process for producing a composite article according to the invention is preferably carried out in an inert gas atmosphere, for example in a nitrogen or argon atmosphere.

[0086] In this method, the silicon infiltration is preferably carried out at temperatures between 280 and 900°C, particularly preferably between 320 and 600°C, in particular between 350 and 450°C.

[0087] Silicon infiltration can be carried out at reduced pressure, normal pressure or elevated pressure, it being preferred if infiltration is carried out at normal pressure or elevated pressure up to 50 bar.

[0088] In all other respects the process may be carried out in a conventional manner as is common for the infiltration of silicon from silicon precursors, using, where necessary, the usual adjustments familiar to those skilled in the art.

[0089] The present invention further provides an anode material for a lithium ion battery containing the silicon subhalide-containing composite particles according to the present invention.

[0090] The anode material is preferably based on a mixture comprising silicon subhalide-containing composite particles according to the present invention, one or more binders, optionally graphite as further active material, optionally one or more further conductive components, and optionally one or more additives.

[0091] The anode material contains silicon subhalide-containing composite particles according to the present invention, preferably one or more binders, optionally graphite as a further active material, optionally one or more further conductive components, and optionally one or more additives.

[0092] The use of other conductive components in the anode material can reduce the contact resistance within the electrode and between the electrode and the current collector, thereby improving the current carrying capacity of the lithium ion battery. Preferred additional conductive components are conductive carbon black, carbon nanotubes or metal particles, such as copper.

[0093] The primary particles of the conductive carbon black preferably have a diameter percentile d 10 = 5nm and d 90 = 200 nm. The primary particles of conductive carbon black can also branch like chains to form structures up to μm in size. The carbon nanotubes preferably have a diameter of 0.4 to 200 nm, more preferably 2 to 100 nm, and most preferably 5 to 30 nm. The metal particles have a diameter percentile d 10 = 5nm and d 90 = 800 nm.

[0094] The anode material preferably comprises 0 to 95% by weight, particularly preferably 0 to 40% by weight, most preferably 0 to 25% by weight of one or more further conductive components, based on the total weight of the anode material.

[0095] The silicon subhalide-containing composite particles according to the invention may be present in the anode for a lithium-ion battery preferably in an amount of 5 to 100% by weight, particularly preferably 30 to 100% by weight, most preferably 60 to 100% by weight, based on the total active material present in the anode material.

[0096] Preferred binders are polyacrylic acid or an alkali metal salt thereof, in particular the lithium or sodium salt, polyvinyl alcohol, cellulose or a cellulose derivative, polyvinylidene fluoride, polytetrafluoroethylene, polyolefin, polyimide, in particular polyamideimide or a thermoplastic elastomer, in particular an ethylene-propylene-diene terpolymer. Particular preference is given to polyacrylic acid, polymethacrylic acid or a cellulose derivative, in particular carboxymethylcellulose. Particular preference is also given to the alkali metal salts of the above-mentioned binders, in particular the lithium or sodium salt. Most preferred are the alkali metal salts of polyacrylic acid or polymethacrylic acid, in particular the lithium or sodium salt. All or preferably part of the acid groups of the binder may be present in the form of a salt. The binder preferably has a molar mass of 100000 to 1000000 g / mol. Mixtures of two or more binders can also be used.

[0097] The graphite used can generally be natural or synthetic graphite. The graphite particles preferably have a diameter percentile d 10 >0.2μm~d 90 Has a volume weighted particle size distribution of <200 μm.

[0098] Examples of additives are pore formers, dispersants, levelling agents or dopants such as elemental lithium.

[0099] A preferred formulation for the anode material preferably contains 5 to 95% by weight, in particular 60 to 90% by weight, of silicon subhalide-containing composite particles according to the invention, 0 to 90% by weight, in particular 0 to 40% by weight of further conductive components, 0 to 90% by weight, in particular 5 to 40% by weight of graphite, 0 to 25% by weight, in particular 5 to 20% by weight of a binder and optionally 0 to 80% by weight, in particular 0.1 to 5% by weight of further additives, the amounts in % by weight being based on the total weight of the anode material, the proportions of all components of the anode material adding up to 100% by weight.

[0100] The present invention further relates to an anode comprising a current collector coated with the anode material according to the present invention, the anode being preferably used in a lithium-ion battery.

[0101] The components of the anode material may be processed into an anode ink or paste, for example, preferably using a rotor-stator machine, a high energy mill, a planetary kneader, an agitator bead mill, a vibrating plate or an ultrasonic device, in a solvent preferably selected from the group including water, hexane, toluene, tetrahydrofuran, N-methylpyrrolidone, N-ethylpyrrolidone, acetone, ethyl acetate, dimethylsulfoxide, dimethylacetamide and ethanol and mixtures of these solvents.

[0102] The anode ink or paste preferably has a pH of 2 to 10 (measured, for example, at 20° C. using a WTW pH 340i pH meter with a SenTix RJD probe).

[0103] For example, the anode ink or paste may be knife coated onto a copper foil or another current collector. Other coating methods such as spin coating, roller, dip or slot coating, brushing or spraying may also be used in accordance with the present invention.

[0104] Before the copper foil is coated with the anode material according to the invention, it may be treated with a commercially available primer, for example based on polymer resins or silanes, which may provide improved adhesion to the copper, but which generally have virtually no electrochemical activity themselves.

[0105] The anode material is preferably dried to a constant weight. The drying temperature depends on the components and the solvent used. The drying temperature is preferably 20°C to 300°C, particularly preferably 50°C to 150°C.

[0106] The layer thickness, ie the dry layer thickness of the anode coating, is preferably between 2 μm and 500 μm, particularly preferably between 10 μm and 300 μm.

[0107] Finally, the electrode coating may be calendered to achieve a defined porosity. The electrodes thus produced preferably have a porosity of 15-85%, which may be measured by mercury porosimetry according to DIN ISO 15901-1. Preferably, 25-85% of the pore volume thus measurable is provided by pores with a pore diameter of 0.01-2 μm.

[0108] The present invention further provides a lithium ion battery comprising at least one anode containing the silicon subhalide-containing composite particles according to the present invention. The lithium ion battery may further comprise a cathode, two conductive connections to the electrodes, a separator, an electrolyte in which the separator and the two electrodes are impregnated, and a housing to contain the components.

[0109] In the context of the present invention, the term lithium-ion battery also includes a cell. A cell generally comprises a cathode, an anode, a separator and an electrolyte. In addition to one or more cells, a lithium-ion battery preferably also includes a battery management system. A battery management system is generally used to control the battery, for example for deep discharge protection or overcharge protection, in particular using electronic circuits for detecting the charge state.

[0110] Preferred cathode materials used may be lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide (doped or undoped), lithium manganese oxide (spinel), lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium vanadium phosphate or lithium vanadium oxide.

[0111] The separator is preferably an ion-permeable, electrically insulating film, preferably made of polyolefin, such as polyethylene (PE) or polypropylene (PP) or polyester or a corresponding laminate. Alternatively, the separator may be made of or coated with a glass or ceramic material, as is common in battery manufacturing. As is known, the separator separates the first electrode from the second electrode, thus preventing an electronically conductive connection (short circuit) between the electrodes.

[0112] The electrolyte is preferably a solution containing one or more lithium salts (=conductive salts) in an aprotic solvent. The conductive salts are preferably selected from the group comprising lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, lithium tetrafluoroborate, lithium imide, lithium methide, LiCF3SO3, LiN(CF3SO2) and lithium borate. The concentration of the conductive salt, based on the solvent, is preferably between 0.5 mol / l and the solid solubility limit of the relevant salt. Particularly preferred is 0.8 to 1.2 mol / l.

[0113] Examples of solvents that can be used are cyclic carbonates, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxyethane, diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, gamma-butyrolactone, dioxolane, acetonitrile, organic carbonates or nitriles, either individually or as mixtures thereof.

[0114] The electrolyte preferably contains a film former such as vinylene carbonate or fluoroethylene carbonate. As a result, a significant improvement in the cycle stability of the anode containing the silicon-containing material according to the invention can be achieved. This is mainly due to the formation of a solid electrolyte interface on the surface of the active particles. The proportion of the film former in the electrolyte is preferably 0.1-20.0% by weight, particularly preferably 0.2-15.0% by weight, most preferably 0.5-10% by weight.

[0115] In order to match the actual capacity of the electrodes of a lithium-ion cell as best as possible, it is advantageous to achieve a balance in terms of the amounts of positive and negative electrode materials. In this context, it is particularly important that during the first or initial charge / discharge cycle (so-called formation) of a secondary lithium-ion cell, a coating layer is formed on the surface of the electrochemically active material in the anode. This top layer is called the "solid electrolyte interface" (SEI) and generally consists mainly of electrolyte decomposition products and a certain amount of lithium, which is therefore no longer available for further charge / discharge reactions. The thickness and composition of the SEI depend on the anode material used and the type and quality of the electrolyte solution used.

[0116] In the case of graphite, the SEI is particularly thin. With graphite, there is a typical loss of 5% to 35% of the mobile lithium in the cell during the first charging step. Thus, the reversible capacity of the battery is also reduced.

[0117] In the case of an anode having silicon subhalide-containing composite particles according to the invention, in the first charging step there is preferably a loss of mobile lithium of at most 30%, particularly preferably at most 20% and most preferably at most 10%, which is significantly below the values ​​of the prior art described, for example, in US 10,147,950 B1, for silicon-containing composite anode materials.

[0118] The lithium-ion battery according to the invention can be manufactured in all the usual configurations, for example in a wound, folded or stacked form.

[0119] As mentioned above, all substances and materials used to manufacture the lithium-ion battery according to the invention are known, except for the composite particles according to the invention. The manufacture of the parts of the battery according to the invention and their assembly to obtain the battery according to the invention is carried out by methods known in the art of battery manufacturing.

[0120] The silicon subhalide-containing composite particles according to the invention are characterized by very good electrochemical behavior, resulting in lithium-ion batteries with high volumetric capacity and excellent performance characteristics. The composite particles according to the invention are permeable to lithium ions and electrons, thus allowing charge transport. The amount of SEI in lithium-ion batteries can be significantly reduced using the silicon subhalide-containing composite particles according to the invention. In addition, due to the design of the composite particles according to the invention, the SEI no longer peels off from the surface of the composite particles according to the invention, or at least peels off from it to a much lesser extent. All this results in high cycle stability of the corresponding lithium-ion batteries. Attenuation and scavenging can be minimized. Furthermore, the lithium-ion batteries according to the invention show low initial and continuous losses of available lithium in the cell, and therefore high coulombic efficiency.

[0121] In the following examples, all amounts and percentages are by weight, all pressures are 0.10 MPa (absolute) and all temperatures are 20° C., unless otherwise specified in each case. EXAMPLES

[0122] The pH is measured according to ASTM Standard No. D1512, Method A.

[0123] Scanning electron microscopy (SEM / EDX): Microscopic analysis was carried out using a Zeiss Ultra 55 scanning electron microscope and an energy dispersive Oxford X-Max 80N X-ray spectrometer. Prior to analysis, samples were subjected to deposition of carbon using a Safematic Compact Coating Unit 010 / HV to prevent charging phenomena. Cross sections of silicon-containing materials were prepared using a Leica TIC 3X ion cutter at 6 kV.

[0124] Inorganic / elemental analysis: The C content was measured using a Leco CS 230 analyzer, while a Leco TCH-600 analyzer was used to measure the oxygen and nitrogen content. Qualitative and quantitative determination of other elements, especially alkali or alkaline earth metals, was carried out by ICP (inductively coupled plasma) optical emission spectrometry (Optima 7300 DV, Perkin Elmer). For this purpose, samples were subjected to acid digestion (HF / HNO3) in a microwave (Microwave 3000, Anton Paar). The ICP-OES measurements were guided by ISO 11885 "Water quality - Determination of selected elements by inductively coupled plasma optical emission spectrometry (ICP-OES) (ISO 11885:2007), the German version EN ISO 11885:2009", which is used for the analysis of acidic aqueous solutions (e.g. acidified drinking water, wastewater and other water samples, aqua regia extracts of soils and sediments).

[0125] X-ray fluorescence analysis: The chlorine content was measured by X-ray fluorescence analysis on a Bruker AXS SB Tiger 1 with a rhodium anode.

[0126] For this purpose, 5.00 g of sample was mixed with 1.00 g of Boreox and 2 drops of ethanol and compressed into tablets in a Herzog HP 40 tablet press at a pressure of 150 kN for 15 seconds.

[0127] Particle size measurement: Particle size distributions are measured according to ISO 13320 by static laser scattering using a Horiba LA 950. In the preparation of the samples, special care must be taken when dispersing the particles in the measurement solution to ensure that the size of the individual particles is measured and not the size of the weak agglomerates. For the materials considered here, these were dispersed in ethanol. For this purpose, the dispersions were treated with 250W ultrasound in a Hielscher UIS250v ultrasonic laboratory instrument with a LS24d5 sonotrode, if necessary, for 4 minutes before the measurements.

[0128] BET surface area measurement: The specific surface area of ​​the materials was measured by gas adsorption with nitrogen by the BET method (measurement according to DIN ISO 9277:2003-05 with nitrogen) using a Sorptomatic 199090 instrument (Porotec) or a BELSorp MAX II instrument (Microtrac) or a SA-9603MP instrument (Horiba).

[0129] Bone Density: The skeletal density, i.e. the density of the porous solid based on the volume of only the pore space accessible to external gas, was determined by helium pycnometry according to DIN 66137-2.

[0130] Gas accessible pore volume (Grbic pore volume): The Grbic gas-accessible pore volume was determined by gas adsorption measurements with nitrogen according to DIN 66134.

[0131] PD50 pore diameter: The PD50 pore diameter was calculated as the volume-average pore diameter based on the total volume of micropores defined by the Horvath-Kawazoe method according to DIN 66135 and mesopores defined by the BJH method according to DIN 66134.

[0132] The following Examples 1-6 and Comparative Example 1 describe the preparation and characterization of porous carbon particles used in the production of silicon-carbon according to the present invention.

[0133] Manufacturing of silicon composite particles Comparative Example 1A (not of the invention): Silicon-carbon composite particles from porous carbon particles.

[0134] For the reaction, an electrically heated autoclave was used, consisting of a cylindrical lower part (cup) and a lid with multiple connections (e.g. gas inlet, gas outlet, temperature and pressure measurement) with a volume of 5.3 L. The stirrer employed was essentially a narrow clearance helical stirrer. It had a height corresponding to about 50% of the clearance height inside the reactor. The helical stirrer had a design that allowed the temperature measurement directly in the bed. 342.5 g of porous carbon (specific surface area = 1617 m) was added to the autoclave. 2 / g, Grbic pore volume = 0.80 cm 3100 g) and sealed. The autoclave was first evacuated. It was then pressurized with SiH4 (70 g) to a pressure of 16.0 bar at 350° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (59 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (57 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (55 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (54 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (52 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (51 g) to a pressure of 16.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The pressure was then reduced to 1.5 bar and the autoclave was pressurized with SiH4 (29 g) to a pressure of 10.0 bar at a temperature of 370° C. The autoclave was then heated to a temperature of 420° C. within 20 minutes and the temperature was maintained for 60 minutes. The autoclave was then cooled to a temperature of 100° C., after which it was purged five times with nitrogen, five times with lean air with an oxygen content of 5%, five times with lean air with an oxygen content of 10%, and then five times with air.

[0135] The pressure in the autoclave was reduced to 1 bar and then purged with nitrogen three times. Under Ar atmosphere, 651 g of silicon-carbon composite particles in the form of a black fine solid were isolated.

[0136] Comparative Example 1B (not of the invention): silicon subchloride-containing composite particles from porous carbon particles.

[0137] Into the tubular reactor, 3.0 g of porous carbon particles (specific surface area = 2140 m) in a quartz glass boat was added. 2 / g, Grbic pore volume = 1.01 cm 3 The reactor was filled with 1000 mL of 10 ...

[0138] [Example 1] Silicon subchloride-containing composite particles from porous carbon particles.

[0139] Into the tubular reactor, 3.0 g of porous carbon particles (specific surface area = 2140 m) in a quartz glass boat was added. 2 / g, Grbic pore volume = 1.01 cm 3 The reactor was filled with 1000 mL of ...

[0140] [Example 2] Silicon-carbon composite particles from porous carbon particles.

[0141] Into the tubular reactor, 3.0 g of porous carbon particles (specific surface area = 2140 m) in a quartz glass boat was added. 2 / g, Grbic pore volume = 1.01 cm 3 The reactor was filled with 100 mL of 10 ...

[0142] [Example 3] Silicon-carbon composite particles from porous carbon particles.

[0143] Into the tubular reactor, 3.0 g of porous carbon particles (specific surface area = 2140 m) in a quartz glass boat was added. 2 / g, Grbic pore volume = 1.01 cm 3 The reactor was filled with 1000 mL of 10000 mL of 10% dimethyl ether (DMSO) in N2 (10 NL / h, pH=5.4). After inerting with nitrogen, the reactor was heated to 380° C. Once the reaction temperature was reached, reactive gas 1 (a mixture of 33 g / h of trichlorosilane (liquid) and 10 NL / h of Ar) was passed through the reactor for 8 hours. Afterwards, reactive gas 2 (10% SiH4 in N2, 10 NL / h) was passed through the reactor for 9 hours. The reactor was then purged with inert gas, cooled to 20° C. and the product was removed.

[0144] [Example 4] Silicon-carbon composite particles from porous carbon particles.

[0145] Into the tubular reactor, 3.0 g of porous carbon particles (specific surface area = 2140 m) in a quartz glass boat was added. 2 / g, Grbic pore volume = 1.01 cm 3 After inerting with nitrogen, the reactor was heated to 380° C. Once the reaction temperature was reached, Reactive Gas 1(A mixture of 5 NL / h dichlorosilane and 10 NL / h Ar) was passed through the reactor for 15 hours. The reactor was then heated to 400° C. Once the reaction temperature was reached, Reactive Gas 2 (10% SiH4 in N2, 10 NL / h) was passed through the reactor for 7.6 hours. The reactor was then purged with inert gas, cooled to room temperature, and the product was removed.

[0146] [Example 5] Silicon-carbon composite particles from porous carbon particles by reaction in a pressure reactor.

[0147] For the reaction, an electrically heated autoclave was used, consisting of a cylindrical lower part (cup) and a lid with multiple connections (e.g. gas inlet, gas outlet, temperature and pressure measurement) with a volume of 594 ml. The stirrer employed was essentially a narrow clearance helical stirrer. It had a height corresponding to about 50% of the clearance height inside the reactor. The helical stirrer had a design that allowed direct temperature measurement in the bed. The autoclave was filled with porous carbon (specific surface area = 2010 m2). 2 / g, Grbic pore volume = 0.95 cm 3 The autoclave was first evacuated. Afterwards, it was pressurized with DCS (1 g) and SiH4 (15 g) to a pressure of 15.1 bar. The autoclave was then heated to a temperature of 420°C within 90 minutes and the temperature was maintained for 210 minutes. Over the course of the reaction the pressure rose to 74 bar. The autoclave was cooled to room temperature (20°C) within 12 hours. After cooling, an autoclave pressure of 33.5 bar remained. The pressure in the autoclave was reduced to 1 bar and then purged three times with nitrogen. Under Ar atmosphere, 20.8 g of silicon-carbon composite particles in the form of a black fine solid were isolated. After replacing the Ar atmosphere with air, the product was suspended in water (30 ml / 1 g product), treated in an ultrasonic bath at 80°C for 1 hour and filtered off on a Büchner funnel while measuring the pH. The whole procedure was repeated until the pH of the washing water was >3.

[0148] The reaction conditions for preparation and material properties of the silicon-carbon composite particles are summarized in Table 2 below.

[0149] [Table 1]

[0150] Regardless of the silicon precursor employed, the same material properties are obtained.

[0151] Evaluation of silicon-carbon composite particles in electrochemical cells Comparative Example 7: Anode containing non-inventive silicon-carbon composite particles from Comparative Example 1A and electrochemical testing in a lithium ion battery.

[0152] 29.71 g of polyacrylic acid (dried to constant weight at 85° C., Sigma-Aldrich, Mw approx. 450000 g / mol) and 756.60 g of deionized water were stirred with a shaker (290 rpm) for 2.5 hours until the polyacrylic acid was completely dissolved. Lithium hydroxide monohydrate (Sigma-Aldrich) was added to the solution in portions until the pH was 7.0 (measured using a WTW pH 340i pH meter and a SenTix RJD probe). The solution was then mixed with a shaker for another 4 hours. 3.87 g of the neutralized polyacrylic acid solution and 0.96 g of graphite (Imerys, KS6L C) were first charged into a 50 ml container and blended in a planetary mixer (SpeedMixer, DAC 150 SP) at 2000 rpm. Subsequently, 3.40 g of silicon-carbon composite particles according to the invention from Example 1A were stirred at 2000 rpm for 1 minute. Then, 1.21 g of 8 percent conductive carbon black dispersion and 0.8 g of deionized water were added and incorporated using a planetary mixer at 2000 rpm. This was followed by dispersion using a dissolver at 3000 rpm for 30 minutes at a constant 20° C. Degassing of the ink was performed again under vacuum using a planetary mixer at 2500 rpm for 5 minutes.

[0153] The finished dispersion was then coated onto a 0.03 mm thick copper foil (Schlenk Metallfolien, SE-Cu58) using a film stretching frame (Erichsen, model 360) with a gap clearance of 0.1 mm. The anode coating thus produced was then dried for 60 minutes at 60° C. and 1 bar air pressure. The average basis weight of the dried anode coating was 2.2 mg / cm. 2 , coating density is 0.9g / cm 3 It was.

[0154] Electrochemical studies were carried out using a button cell (type CR2032, Hohsen Corp.) with a two-electrode configuration. The electrode coating was used as the counter or negative electrode (Dm=15 mm) with a content of 94.0% and a concentration of 15.9 mg / cm. 2 A coating based on lithium-nickel-manganese-cobalt oxide 6:2:2 (obtained from SEI) with an average basis weight of was used as the working or positive electrode (Dm=15 mm). A glass fiber filter paper (Pall, GF type A / E) soaked with 60 μl of electrolyte was used as the separator (Dm=16 mm). The electrolyte employed consisted of a 1.0 molar solution of lithium hexafluorophosphate in a 1:4 (v / v) mixture of fluoroethylene carbonate and diethyl carbonate. The construction of the cell was carried out in a glove box (<1 ppm H2O, O2) and the moisture content in the dry matter of all the components employed was less than 20 ppm.

[0155] Electrochemical tests were carried out at 22°C. The cells were charged by cc / cv method (constant current / constant voltage) at a constant current of 15 mA / g (corresponding to C / 10) in the first cycle and 75 mA / g (corresponding to C / 2) in the subsequent cycles, and at a constant voltage until the current dropped below 1.5 mA / g (corresponding to C / 100) or 3 mA / g (corresponding to C / 50) when the voltage limit of 4.2 V was reached. The cells were discharged by cc method (constant current) at a constant current of 15 mA / g (corresponding to C / 10) in the first cycle and 75 mA / g (corresponding to C / 2) in the subsequent cycles until the voltage limit of 2.5 V was reached. The specific current selected was based on the weight of the coating of the positive electrode. The electrodes were selected so that a capacity ratio of cathode:anode = 1:1.2 was established.

[0156] Comparative Example 8: Anode containing non-inventive silicon-carbon composite particles from Comparative Example 1B and electrochemical testing in a lithium ion battery.

[0157] The non-inventive silicon-containing material from Comparative Example 1B was used to prepare an anode as described in Comparative Example 7. The anode was installed in a lithium ion battery as described in Comparative Example 7 and tested according to the same procedure.

[0158] Comparative Example 9: Anode containing non-inventive silicon-carbon composite particles from Comparative Example 1C and electrochemical testing in a lithium ion battery.

[0159] The non-inventive silicon-carbon composite particles from Comparative Example 1C were used to prepare an anode as described in Comparative Example 7. The anode was installed in a lithium ion battery as described in Comparative Example 7 and tested according to the same procedure.

[0160] [Example 10] Electrochemical testing in anodes containing silicon-carbon composite particles from Example 3 and lithium ion batteries.

[0161] The silicon-containing material according to the present invention from Example 3 was used to prepare an anode as described in Comparative Example 7. The anode was installed in a lithium ion battery as described in Comparative Example 7 and tested according to the same procedure.

[0162] The results of the electrochemical evaluation are summarized in Table 3 below.

[0163] [Example 11] Electrochemical testing in anodes containing silicon-carbon composite particles from Example 1 and lithium ion batteries.

[0164] The silicon-containing material according to the present invention from Example 1 was used to prepare an anode as described in Comparative Example 7. The anode was installed in a lithium ion battery as described in Comparative Example 7 and tested according to the same procedure.

[0165] The results of the electrochemical evaluation are summarized in Table 3 below.

[0166] [Table 2]

[0167] A comparison of Comparative Example 7 with Example 10 according to the invention reveals that the presence of chlorine content in the material does not adversely affect the electrochemical performance. A comparison of Comparative Example 8 with Example 11 according to the invention reveals that an excessively low pH adversely affects the electrochemical performance of the battery, while adapting the pH stabilizes the performance.

Claims

1. 1. A silicon subhalide-containing composite particle comprising:

1. Si content >30% by weight, 2. Silicon disposed within and on the pores of a porous matrix; 3. A halogen concentration of 0.0003 to 16% by weight; 4. pH 3-9, and 5. Diameter percentile d between 0.5 and 20 μm 50 A volume-weighted particle size distribution having The silicon subhalide-containing composite particle has the following formula:

2. The halogen is chlorine, having a Cl concentration of 0.0003 to 16 wt %; The composite particle according to claim 1 .

3. The silicon is at least partially silicon subchloride SiCl x 3. The composite particle according to claim 1 or 2, which exists in the form: (wherein x=0.00001 to 0.15).

4. Composite particles according to any one of claims 1 to 3, comprising at least 30% by weight of silicon obtained by silicon infiltration.

5. 5. Composite particles according to claim 1, wherein the silicon or silicon subhalide is present in the form of a layer or layers formed from silicon particles having a thickness of up to 1 μm.

6. Maximum 170m 2 The composite particles according to any one of claims 1 to 5, having a specific BET surface area of ​​1 / g.

7. A method for producing composite particles according to any one of claims 1 to 6 by silicon infiltration from silicon precursors selected from halogen-containing and halogen-free silicon precursors which are gaseous and / or liquid at 20°C and 1013 mbar, wherein at least one halogen-containing silicon precursor is 1. Diameter percentile d between 0.5 and 20 μm 50 A volume weighted particle size distribution having 2.0.4~2.2cm 3 / g range of N 2 The total pore volume of the micropores and mesopores (Grbic pore volume) measured by adsorption, and 3. N less than 30 nm 2 PD50 pore diameter measured by adsorption in the presence of porous particles having the formula:

8. 8. The method according to claim 7, wherein the silicon infiltration is carried out in a reactor selected from a fluidized bed reactor, a rotary kiln arranged in a horizontal to vertical position, an open or closed fixed bed reactor, and a pressure reactor.

9. 9. The method according to claim 7 or 8, wherein the silicon infiltration is carried out at 280°C to 900°C.

10. The method according to claims 7 to 9, wherein the composite particles are produced by silicon infiltration from a silane selected from monosilanes and chlorine-containing silanes, and at least one chlorine-containing silane is employed.

11. The method according to claims 7 to 10, wherein a silicon-free reactive component is also present in admixture with or alternating with said silicon precursor.

12. 7. An anode material for a lithium ion battery comprising the silicon subhalide composite particles according to claims 1-6.

13. An anode comprising a current collector coated with the anode material of claim 12.

14. A lithium ion battery comprising at least one anode containing the silicon subhalide-containing composite particles according to claims 1-6.

Citation Information

Patent Citations

  • Decomposition of silicon-containing precursors onto porous scaffolds

    JP2020514231A

  • Method of depositing silicon on carbon nanomaterials

    US20120264020A1

  • Methods and apparatus for determining audience metrics across different media platforms

    US20200007954A1

  • Powder for negative electrode material of lithium-ion rechargeable battery electrode, and method of producing same

    WO2011148569A1

  • Process for preparing electroactive materials for metal-ion batteries

    WO2020128523A1

Cited By

  • KRAS G12D INHIBITORS AND USES THEREOF

    JP2024525993A