Formation method of metal oxide thin film for electrode interphase control
By forming a metal oxide layer on the cathode using ALD/CVD, the SEI stability and cathode integrity are enhanced, addressing issues of capacity loss and degradation in lithium-ion batteries.
Patent Information
- Application Number
- JP2024530411
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-12-01
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-12-01
AI Technical Summary
The formation of a non-uniform and unstable solid electrolyte interface (SEI) during the first cycle of a lithium-ion battery leads to capacity loss, physical cracking, lithium dendrite formation, and potential short circuits, while high nickel cathode materials suffer from transition metal dissolution and electrolyte decomposition, causing rapid battery degradation.
A method involving atomic layer deposition (ALD) or chemical vapor deposition (CVD) is used to form a metal oxide layer on the cathode or cathode active material, composed of volatile chemical precursors like M(=NRa)(ORb)2(NRc)2, to stabilize the electrode interface and reduce parasitic reactions.
The metal oxide layer enhances electrochemical performance by minimizing electrolyte decomposition and transition metal dissolution, improving cycle stability and reducing capacity loss, thereby extending battery life and safety.
Smart Images

Figure 2024545016000001_ABST
Abstract
Description
[Background technology]
[0001] During the first cycle of a lithium-ion battery, the formation of a solid electrolyte interface (SEI) on the anode and / or cathode is observed from the decomposition of the electrolyte at the electrolyte / electrode interface. The initial capacity decline of a lithium-ion battery occurs as a result of the consumption of lithium during the formation of this SEI. Furthermore, the formed SEI layer is non-uniform and unstable, and is not efficient for passivating the electrode surface against the degradation of the electrode active material due to the continuous decomposition of the electrolyte. The SEI layer may undergo physical cracking during the cycling of the battery, and lithium dendrites may form, leading to short circuits and subsequent thermal runaway. Furthermore, the SEI layer also creates a barrier potential that makes the intercalation of lithium ions in the electrode more difficult.
[0002] In current designs, lithium-ion batteries use (lithium) metal oxide, phosphate or fluoride coatings (e.g., Al) on the surfaces of the electrodes and / or electrode active materials by wet coating, dry coating or sputtering of continuous films of metal oxides and / or phosphates to stabilize the interphase between the electrode and the electrolyte. x O y , Li x M y PO z , M=Nb, Zr, AlTi, etc. or AlM x F yM=W, Y, etc. Lithium-containing thin films are known for their use as surface coating layers of electrode materials in lithium-ion battery applications. Examples of lithium-containing thin films include LiPON, lithium phosphate, lithium borate, lithium borophosphate, lithium niobate, lithium titanate, lithium zirconium oxide, etc. Surface coating of electrodes by ALD / CVD techniques is a preferred means of forming the above-mentioned solid electrolyte interfacial thin films, thus avoiding the formation of these unstable layers. However, deposition of lithium-containing films is difficult to carry out due to the lack of suitable lithium precursors for mass production. Most are not volatile, are not stable enough, and they may contain undesirable impurities. Another important application of mesophase thin films is in the formation of solid electrolyte materials used in solid-state batteries. Solid-state batteries are solvent-free systems with longer service life, faster charging times, and higher energy density than conventional lithium-ion batteries. They are considered to be the next technological step in battery development. ALD / CVD techniques can also provide uniform and conformal electrode / electrolyte interfacial thin films on complex structures such as 3D batteries.
[0003] Silicon anodes are also in the scope of mesophase thin film applications. Silicon is considered to be the next generation of anodes in the development of lithium-ion batteries, and graphite anodes (Li + / Li) at the same potential level (0.05V vs. + / Li at 0.2 V) with a graphite anode (372 mAhg -1 ) with higher specific capacity (3600mAhg -1 The main drawback of silicon anodes is their volume expansion of up to 300% during charge / discharge, leading to destabilization of the SEI and physical cracking of the electrode.
[0004] The application of mesophase thin films can be extended to lithium metal anode technology. Lithium metal anodes are considered to be post-lithium ion batteries (LIBs) because they can provide at least three times the theoretical capacity compared to LIBs. Lithium metal is also attracting attention due to its high capacity (10 times the capacity of graphite), reduced battery volume, and process simplicity. However, uncontrolled lithium metal surfaces can lead to the growth of Li dendrites, which can cause short circuits and ultimately fires.
[0005] For next-generation cathode active materials, much research has been focused on identifying and developing metal oxide cathode materials. Among the wide range of layered oxides, high-Ni cathode materials such as NMC (nickel-lithium manganese cobalt oxide) and NCA (nickel-lithium cobalt aluminum oxide) are the most promising current candidates for practical application. However, high-Ni cathode materials tend to become amorphous when high voltages are applied. One of the main drawbacks of these metal oxide materials is the continuous dissolution of transition metals, especially nickel, due to parasitic reactions of the cathode material with the electrolyte. This leads to structural degradation of the cathode active material along with gas (O2) evolution at the electrode / electrolyte interface during charging of the battery. Furthermore, the dissolved nickel ions migrate to the anode side, and their deposition on the anode surface causes rapid decomposition of the SEI in the anode, ultimately leading to the failure of the battery.
[0006] Spinel cathode materials have been extensively investigated for their high rate capability and low or zero cobalt content. One of the main issues with spinel cathode materials such as LMO (lithium manganese oxide), LNMO (lithium nickel manganese oxide) is the dissolution of divalent manganese ions (2Mn 3+ →Mn 4+ +Mn 2+ ), which occurs primarily at the electrode / electrolyte interface followed by redeposition on the anode and destruction of its SEI as by the same mechanism for high Ni cathode materials.
[0007] Deposition of thin films on the cathode and / or cathode materials can be used to address interface issues between the electrolyte and the cathode electrode, such as dissolution of transition metals, excessive electrolyte decomposition, etc. For example, US Patent No. 8,535,832 B2 discloses wet coating of metal oxides (Al2O3, Bi2O3, B2O3, ZrO2, MgO, Cr2O3, MgAl2O4, Ga2O3, SiO2, SnO2, CaO, SrO, BaO, TiO2, Fe2O3, MoO3, MoO2, CeO2, La2O3, ZnO, LiAlO2 or combinations thereof) onto cathode active materials containing Ni, Mn and Co. US Patent No. 9,543,581 B2 discloses dry coating of amorphous Al2O3 onto precursor particles of cathode active materials containing Ni, Mn and Co elements. U.S. Pat. No. 9,614,224 B2 describes the deposition of Li on a cathode active material containing Mn using a sputtering method. x PO y Mn z Coatings are described. US Patent No. 9,837,665 B2 describes lithium phosphate oxynitride (LiPON) thin film coatings using a sputtering method on cathode active materials including Li, Mn, Ni, and oxygen-containing compounds with at least one dopant of Ti, Fe, Ni, V, Cr, Cu, and Co. US Patent No. 9,196,901 B2 describes Al2O3 thin film coatings using an atomic layer deposition (ALD) method on cathode stacks and cathode active materials including Co, Mn, V, Fe, Si, or Sn and being oxides, phosphates, silicates, or mixtures of two or more thereof. US Patent No. 10,224,540 B2 describes Al2O3 thin film coatings using an ALD method on porous silicon anodes. US Patent No. 10,177,365 B2 describes AlW thin film coatings using ALD on cathode active materials including LiCoO2. x F y Or AlW x F y C z Thin film coatings are described. US Pat. No. 9,531,004 B2 describes lithium titanate Li (4+x) Ti5O 12Hybrid thin film coatings including a first layer of Al2O3, TiO2, SnO2, V2O5, HfO2, ZrO2, ZnO and a second layer of fluoride-, carbide-, and nitride-based coatings using ALD methods on anode materials consisting of (0≦x≦3) (LTO), graphite, silicon, silicon-containing alloys, tin-containing alloys, and combinations thereof are described. Summary of the Invention [Means for solving the problem]
[0008] The present invention provides the following solution, by depositing, by ALD or CVD, metal oxide layers on the cathode or cathode active material, forming an artificial intermediate phase on the electrode to protect it from rapid degradation of electrochemical properties. These metal oxide layers reduce the excessive decomposition of the electrolyte at the electrode / electrolyte interface during the SEI formation, reducing the capacity loss in the first cycle. The presence of such metal oxide layers also reduces the dissolution of the transition metal cations of the cathode active material, caused by parasitic reactions between the electrolyte and the cathode active material, and then their redeposition on the anode. The electrochemical activity of the battery is thereby improved. As described above, other types of membranes have been proposed, in particular high purity metal oxides such as Al2O3. However, this type of material acts as an ionic insulator and therefore does not allow the best electrochemical performance of the obtained cathode and battery.
[0009] The present invention can be further understood in connection with the following non-limiting exemplary embodiments, which are set forth as enumerated sentences:
[0010] 1. Coating A method for coating a cathode or cathode active material with a metal oxide film, comprising the steps of: The cathode or cathode active material is a compound having the formula M(=NR a )(OR b )2(NR c 2) to a vapor of a chemical precursor comprising the chemical precursor of and a source of oxygen as an oxidizing co-reactant, wherein: M is selected from Nb, Ta, or V; Ra is selected from iPr, tBu, and t-Am; each Rb is independently selected from Et, iPr, tBu, sBu, and SPen; a step a1. in which each Rc is independently selected from Et or Me; A method comprising the step b1. depositing a metal oxide film on a cathode or cathode active material.
[0011] 2. The method according to claim 1, in which step a1 of exposing the cathode or cathode active material to vapor of a chemical precursor and step a2 of exposing the cathode or cathode active material to a co-reactant are carried out sequentially.
[0012] 3. The method of claim 2, further comprising the step a1.i of purging the vapor of the chemical precursor prior to step a2 of exposing the cathode or cathode active material to the co-reactant.
[0013] 4. The method of claim 3, wherein step b1. of depositing a metal oxide film on the cathode or cathode active material comprises an atomic layer deposition process.
[0014] 5. The method of claim 3, wherein step b1. of depositing a metal oxide film on the cathode or cathode active material comprises a chemical vapor deposition process.
[0015] 6. The method of any one of sentences 1 to 5, wherein the co-reactant is O2, O3, H2O, H2O2, NO, NO2, N2O or NOx; an oxygen source such as an oxygen-containing silicon precursor, an oxygen-containing tin precursor, trimethyl phosphate, a phosphate such as diethyl phosphoramidate, or a sulfate.
[0016] 7. The precursor has the formula M(=NR a )(OR b ) 2(NMeEt).
[0017] 8. R bThe method according to any one of sentences 1 to 7, wherein at least one of is independently selected from sBu, SPen.
[0018] 9. The precursor has the formula M(=NR a )(OR b )2(NMeEt), R b The method according to any one of sentences 1 to 7, wherein at least one of is independently selected from sBu, SPen.
[0019] 10. Both R b The method of claim 8 or 9, wherein is independently selected from sBu, SPen.
[0020] 11. The metal oxide film produced by step b1. is Nb x O y D z wherein O is oxygen, D is any other atom, and x=0.3 to 0.4, y=0.4 to 0.65, and z=0.01 to 0.1.
[0021] 12. The method according to any one of sentences 1 to 11, wherein the temperature of the vapor of the chemical precursor and / or the cathode or cathode active material is 100°C to 300°C, more preferably 125°C to 275°C, even more preferably 125°C to 175°C.
[0022] 13. The method according to any one of sentences 1 to 12, wherein the metal oxide film has an average thickness of 0.02 nm to 10 nm, preferably 0.1 nm to 5 nm, and most preferably 0.2 to 2 nm.
[0023] 14. The method according to any one of sentences 1 to 13, wherein the cathode active material, or the cathode active material in the cathode, is selected from the group consisting of: a) layered oxides, such as high Ni cathode materials, such as NMC (cobalt manganese nickel lithium oxide) and NCA (cobalt nickel lithium aluminum oxide); b) spinel cathode materials, such as LMO (lithium manganese oxide), LNMO (lithium manganese nickel lithium oxide); c) olivine structured cathode materials, in particular olivine phosphate types, such as LCP (lithium cobalt phosphate), LNP (lithium nickel phosphate), LFP (lithium iron phosphate); and combinations thereof.
[0024] 15. The method according to any one of sentences 1 to 14, wherein one or more of steps a1. and b1. are carried out 1 to 10 times, preferably 1 to 3 times, more preferably only once.
[0025] 16. The method according to any one of sentences 1 to 15, wherein a) the temperature of the chemical precursor vapor and / or the cathode or cathode active material is between 100°C and 300°C, more preferably between 125°C and 275°C, b) the metal oxide film has an average thickness of between 0.02 nm and 10 nm, preferably between 0.1 nm and 5 nm, most preferably between 0.2 and 2 nm, and c) the metal oxide film is at least 50% continuous on the surface of the cathode or cathode active material, preferably 95% or more continuous, more preferably 98% or more continuous.
[0026] For a further understanding of the nature and objects of the present invention, reference should be made to the following detailed description taken in conjunction with the accompanying drawings, in which like elements are given the same or similar reference numerals, and in which: [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 shows photoelectron spectroscopy results for the deposition of NbO thin films on NMC622 powder using Nb(=NtBu)(NEt2)(O-tBu)2 (“Nau2”) / H2O using a powder ALD (PALD) reactor. [Diagram 2]FIG. 2 shows the normalized C-rate performance (normalized to their original discharge capacity at 2 C) of NbO thin films deposited on NMC622 powder using Nb(=NtBu)(NEt)(O-tBu) / HO in a powder ALD (PALD) reactor. [Diagram 3] FIG. 3 shows the long-term cyclic performance of NbO thin films deposited on NMC622 powder using Nb(=NtBu)(NEt2)(O-tBu)2 / H2O in a powder ALD (PALD) reactor. [Figure 4] FIG. 4 shows an electron micrograph of NMC 811 powder coated with a layer of NbO after three ALD cycles using the AL conditions described in the Examples below. The layer is identified by an arrow and also shown in the lined section. The layer is visually confirmed as continuous and conformal with a thickness of about 1.5 nm to 2 nm. The conformal coverage and Nb content of the layer were further confirmed by energy dispersive X-ray spectroscopy (not shown). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present disclosure provides a solution to form an interphase on an electrode to protect it from rapid degradation of its electrochemical properties. The interphase is formed on the cathode active material before or after its incorporation into the final cathode. The metal oxide layer is formed by the formation of a volatile chemical precursor species M(=NR a )(OR b )2(NR c 2) is formed by chemical vapor deposition (CVD) or atomic layer deposition (ALD). M is selected from Nb, Ta, or V; R a is selected from iPr, tBu, and t-Am Each R b are independently selected from Et, iPr, tBu, sBu, and SPen; Each R c is independently selected from Et or Me.
[0029] These volatile chemical precursors are delivered simultaneously, sequentially, and / or by pulses of the precursor vapor phase. This process exploits this type of unexpected efficiency to achieve improved cathode performance after fewer than nine ALD deposition cycles, preferably three or fewer cycles. This relatively low number of required ALD cycles significantly reduces the consumption of metals such as Nb or Ta and the time required to process the cathode or cathode active material.
[0030] As used herein, "metal oxide" and "metal oxide film" refer to a transition metal oxide film having one or more additional elements in an atomic ratio of MxOyDz, where M=the aggregate moiety of the transition metal, O is oxygen, and D is the aggregate moiety of other elements such as aluminum, zinc, tin, carbon, lithium, and phosphorus. Typically, x is in the range of 10-60%, y is in the range of 10-60%, and z is undetectable to 10%, preferably 0-5%.
[0031] Preferably, M is a transition metal that forms one or more stable ions with incompletely filled d-orbitals. In particular, M is Nb, but may optionally further include one or more of Ti, Zr, Hf, V, Ta, Cr, Mo, or W.
[0032] The metal oxide film is formed by a CVD or ALD process that deposits a metal oxide layer on the cathode active material before, during, or after its introduction into the final cathode intermediate manufacturing process. The metal oxide film can be a continuous film that completely coats the cathode active material before inclusion in the cathode, for example by powder ALD of the powdered cathode active material. The film can be discontinuous, either by controlled deposition conditions that limit film growth or as a result of the cathode active material being introduced into the cathode such that only a portion of its surface is subjected to the CVD or ALD deposition process. Typically, the metal oxide film has an average thickness of 0.125 to 10 nm, for example 0.125 nm to 1.25 nm, preferably 0.3 nm to 4 nm.
[0033] A metal oxide deposit may be deposited on the electrode consisting of: - layered structured oxides, preferably "NMC" (lithium nickel manganese cobalt oxide, e.g. NMC811 (Ni:Mn:Co=8:1:1), even more preferably NMC955 (Ni:Mn:Co=9:0.5:0.5)), NCA (lithium nickel cobalt aluminium oxide) or LNO (lithium nickel oxide); • spinels, preferably LNMO (lithium nickel manganese oxide) or LMO (lithium manganese oxide); ● Olivine (lithium metal phosphate, metals can be iron, cobalt, manganese); ● A form of carbon anode, such as graphite, doped or undoped; ● Silicon anode, ● Silicon-carbon anodes, ● Tin anode, Silicon-tin anodes, or ● Lithium metal.
[0034] Deposition can be performed on electrode active material powder, on electrode active material porous material, on different shapes of electrode active material, or in a preformed electrode where the electrode active material can already be mixed with conductive carbon and / or binder and already supported by a current collector foil.
[0035] "Cathode" in a lithium-ion battery refers to the positive electrode in an electrochemical cell (battery) where reduction of the cathode material occurs by insertion of electrons and lithium ions during charging. During discharging, the cathode material is oxidized by releasing electrons and lithium ions. Lithium ions move from the cathode to the anode in the electrochemical cell through the electrolyte, or vice versa, while electrons move through an external circuit. The cathode is generally composed of a cathode active material (i.e., lithiated metal layered oxide) and a conductive carbon black agent (acetylene black Super C65, Super P) and a binder (PVDF, CMC).
[0036] A "cathode active material" is a major element in the composition of a cathode (positive electrode) for a battery cell. Cathode active materials are, for example, cobalt, nickel, and manganese in a crystalline structure, such as a layered structure, forming a multi-metal oxide material into which lithium is intercalated. Examples of cathode active materials are layered lithium cobalt manganese nickel oxide (LiNixMnyCozO2), spinel lithium manganese oxide (LMn2O4), and olivine lithium iron phosphate (LiFePO4).
[0037] "Continuity" in reference to a coating on a surface refers to the percentage of that surface that has a given thickness of coating material. Continuity is typically measured by imaging the coated material, such as by grid mapping the surface, and measuring the percentage of the surface that is and is not covered by the film (e.g., in nm 2 The coverage is evaluated optically by quantifying the coverage (in units of 100 nm). Electron microscopy can be used to image the surface. Coverage can be expressed as a percentage of the substrate surface area. Pinholes, voids, or other discontinuities in the film mean that the continuity is less than 100%.
[0038] Metal oxide films are formed by reacting volatile chemical precursor species M (=NR a )(OR b )2(NR c 2) and, optionally, one or more other chemical precursors that contribute to the final film formation. Any additional suitable precursors can be selected for use based on their known applicability for the formation of metal oxides for other uses.
[0039] A wide variety of optional precursors can be used to form metal oxides, preferably at Nau2, under optimized deposition conditions.
[0040] Preferred IVA metal precursors are: M(OR)4, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OMe)4, M(OiPr)4, M(OtBu)4, M(OsBu)4 ● M(NR 1 R 2 )4, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)4, M(NMeEt)4, M(NEt2)4 ● ML(NR 1 R 2 )3, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, or cyclooctadienyl, and each R 1 and R 2 are independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3, MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3, M(iPrCp)(NMe2)3, M(sBuCp)(NMe2)3, M(tBuCp)(NMe2)3, N(secPenCp)(NMe2)3, M(nPrCp)(NMe2)3 ● ML(OR)3, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, MCp*(OEt)3, M(iPrCp)(NMe2)3, M(sBuCp)(NMe2)3, M(tBuCp)(NMe2)3, N(secPenCp)(NMe,)3, M(nPrCp)(NMe2)3
[0041] Preferred VA metal precursors are as follows: M(OR)5, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OEt)5, M(OiPr)5, M(OtBu)5, M(OsBu)5 ● M(NR 1 R 2 )5, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)5, M(NMeEt)5, M(NEt2)5 ● ML(NR 1 R 2 ) x , x=3 or 4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the form NR, each R 1 and R 2 are independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3M(=NtBu)(NMe2)3, M(=NtAm)(NMe2)3, M(=NtBu)(NEt2)3, M(=NtBu)(NEtMe)3, M(=NiPr)(NEtMe)3. ● M(=NR 1 )L(NR 2 R 3 ) x , x=1 or 2, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, or cyclooctadienyl, and each R 1 and R 2 and R 3 are independently a C1 to C6 carbon chain, most preferably MCp(=NtBu)(NMe2)2, M(MeCp)(N=tBu)(NMe2)2, M(EtCp)(N=tBu)(NMe2)2, MCp*(=NtBu)(NMe2)2, MCp(=NtBu)(NEtMe)2, M(MeCp)(N=tBu)(NEtMe)2, M(EtCp)(N=tBu)(NEtMe)2. ● ML(OR) xx=3 or 4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the NR form, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, MCp*(OEt)3M(=NtBu)(OiPr)3, M(=NtAm)(OiPr)3, ● ML(OR) x (NR 1 R 2 ) y , x and y are independently equal to 1 or 2, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or imide of the NR form, and each R is independently a C1-C6 carbon chain (linear or branched), most preferably MCp(OiPr)2(NMe2), M(MeCp)(OiPr)2(NMe2), M(EtCp)(OEt)2(NMe2), M(=NtBu)(OiPr)2(NMe2), M(=NtBu)(OiPr)(NMe2), M(=NtBu)(OiPr)2(NMe2), M(=NtBu)(OiPr)2(NMe2), (NMe2), M(=NtBu)(OiPr)2(NEtMe), M(=NtBu)(OiPr)2(NEt2), M(=NtBu)(OEt)2(N Me2), M(=NtBu)(OEt)2(NEtMe), M(=NtBu)(OEt)2(NEt2), M(=NiPr)(OiPr)2(NMe2 ), M(=NiPr)(OiPr)2(NMe2)2, M(=NiPr)(OiPr)2(NEtMe), M(=NiPr)(OiPr)2(NEt2 ), M(=NiPr)(OEt)2(NMe2), M(=NiPr)(OEt)2(NEtMe), orM(=NiPr)(OEt)2(NEt2).
[0042] Preferred VIA metal precursors are as follows: M(OR)6, each R is independently a C1 to C6 carbon chain (linear or branched), most preferably M(OEt)5, M(OiPr)5, M(OtBu)5, M(OsBu)5 ● M(NR 1 R 2 )6, each R 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably M(NMe2)6, M(NMeEt)6, M(NEt2)6 ● M(NR 1 R 2 ) x L y , x and y are independently equal to 1 to 4; L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, or an imide of the NR form; 1 and R 2 are independently C1 to C6 carbon chains (linear or branched), most preferably MCp(NMe2)3, M(MeCp)(NMe2)3, M(EtCp)(NEt2)3, MCp*(NMe2)3, M(=NtBu)2(NMe2)2, M(=NtAm)2(NMe2)2, M(=NtBu)(NEt2)2 ● M(OR) x (NR 1 R 2 ) y L z ML, x, y and z are independently equal to 0 to 4, L represents an imide of the form unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl or NR, and each R is independently a C1 to C6 carbon chain (linear or branched), most preferably MCp(OiPr)3, M(MeCp)(OiPr)3, M(EtCp)(OEt)3, M(=NtBu)2(OiPr)2, M(=NtAm)2(OiPr)2, M(=NtBu)2(OtBu)2, M(=NiPr)2(OtBu)2, M(=NtBu)2(OiPr)2, M(=NiPr)2(OiPr)2. ● M(=O)xLy, x, y and z are independently equal to 0-4, L represents unsubstituted or substituted allyl, cyclopentadienyl, pentadienyl, hexadienyl, cyclohexadienyl, cycloheptadienyl, cyclooctadienyl, amide or imide in NR form, each R is independently a C1-C6 carbon chain (linear or branched), most preferably M(=O)2(OtBu)2, M(=O)2(OiPr)2, M(=O)2(OsecBu)2, M(=O)2(OsecPen)2, M(=O)2(NMe2)2, M(=O)2(NEt2)2, M(=O)2(NiPr2)2, M(=O)2(NnPr2)2, M(=O)2(NEtMe)2, M(=O)2(NPen2)2.
[0043] Metal oxide films can be formed using one member of the volatile chemical precursor species, either as a single precursor or in combination with one or more other precursors, and in each case, optionally using an oxidizing co-reactant (if necessary or desirable). Those skilled in the art can select suitable additional precursors and co-reactants from those known in the art to produce metal oxide films having the desired composition when used under optimized deposition conditions to "tune" the composition of the metal oxide. Typical of the various precursor options include the following: - Oxygen can come from an O source such as O2, O3, H2O, H2O2, NO, NO2, N2O or Nox. - The oxygen can come from a dopant source such as an oxygen-containing silicon precursor, an oxygen-containing tin precursor, a phosphate such as trimethyl phosphate, diethyl phosphoramidate, or a sulfate. - Nitrogen can come from N sources such as N2, NH3, N2H4, N2H4 containing mixtures, alkylhydrazines, NO, NO2, N2O or NOx. - Nitrogen can come from dopant sources such as nitrogen-containing silicon precursors, nitrogen-containing tin precursors, or phosphates such as diethyl phosphoramidate. ● Carbon can come from C sources such as hydrocarbons, carbon-containing silicon precursors, carbon-containing tin precursors, carbon-containing boron precursors, carbon-containing aluminum precursors, carbon-containing phosphorus precursors, trimethyl phosphate, phosphates such as diethyl phosphoramidate, or sulfates. - Silicon can come from a Si source such as a silane or silicon-containing organometallic precursor. - Tin can come from a Sn source such as a stannane or a tin-containing organometallic precursor. - Aluminium can come from an Al source such as an alane, such as an alkylalane, or an aluminium-containing organometallic precursor. Phosphorus can be derived from a phosphine, such as an organophosphine, or a phosphate, such as trimethyl phosphate or diethyl phosphoramidate. • Sulfur can come from S sources such as sulfur, S8, H2S, H2S2, SO2, organic sulfites, sulfates, or sulfur-containing organometallic precursors. - First row transition metals may be derived from known organometallic or other precursors suitable for use in vapor deposition. EXAMPLES
[0044] Examples 1-5: Deposition and electrochemical performance of NbO thin films deposited using Nau2 / H2O on NMC622 powder at 250 °C Experimental conditions for deposition / film formation: The number of cycles for NMC622 electrodes or NMC powders is typically limited to 20 ALD cycles, which corresponds to approximately 1.5-4 angstroms, an insufficient thickness to achieve the film composition. Therefore, such characterization was performed on films deposited after 300 ALD cycles with O3 on blank silicon wafers. The corresponding growth rates and film compositions by X-ray photoelectron spectroscopy (XPS) are as follows: ● GPC approximately 2.96Å. Nb: approx. 38.7%, O: approx. 54.8%, C: approx. 3%, N: approx. 2%, Si approx. 1.4% • The refractive index of these films is 2.38.
[0045] Deposition was carried out on NMC622 powder using a fluidized bed reactor with the following experimental conditions: ALD Conditions for ALD Reactor temperature setting: 250℃ Reactor pressure: approx. 40 Torr Number of cycles: 1 / 2 / 3 / 9cy Precursors and Gases Nautilus2 canister temperature 100℃ Nautilus2 Canister Pressure 50 Torr N2 bubbling in Nautilus 2: 20 sccm O3 FR 20sccm N2 push / purge approx. 120sccm Pulse sequence Nautilus2(2sccm) 900 seconds Purge 1040 seconds H2O 180 seconds Purge 1040 seconds Input base material 5g of NMC622 powder
[0046] The chemical precursor in these examples is Nb(=NtBu)(NEt2)(O-tBu)2 ("Nau2").
[0047] Electrochemical characterization: Test conditions: Battery Cell Condition: ● Cathode material: NMC622 ○ Approximately 5mg / cm 2 Amount of ○ No calendar processing ● Coating material: Nb2O5 ○ Precursor: Nautilus2 ○ Co-reactant: O3 or H2O ○ Dep.T=250℃ Powder Reactor P<40 Torr ○ Amount of powder coated: 5g ○ Reactor filling: x% ● Membrane: Celgate 2400 ● Neat electrolyte: 1M LiPF6 in EC:EMC (1:1 by weight) ● Anode material: Li metal Measurement conditions: ● Temperature: 26℃ 0.2C, then 3 spare cycles at 1C ● Voltage: 3.0~4.3V, CC
[0048] As seen in Figure 1, the amount of niobium deposited as niobium oxide increases from 1 ALD cycle to 2-3 ALD cycles, and increases significantly with 9 ALD cycles. The effect of these niobium oxide depositions is seen in Figures 2 and 3. Battery performance is significantly improved compared to the uncoated control. However, quite unexpectedly, the best results are obtained with 1 ALD cycle, while 2-3 cycles are nearly the same. 9 ALD cycles further improve performance compared to the control, but not as well as 1-3 cycles. Typically, ALD coatings for cathode active materials require 5-20 ALD cycles for optimal effectiveness. Surprisingly, Nau2 allows for a low ALD cycle process that requires much less time and much less precursor amount per unit of cathode active material. This significantly reduces costs in industrial applications.
[0049] The same conditions and tests were used for ALD using ozone instead of water. The results for ozone were the same as for water, indicating that low cycle number deposition was not substantially affected by the oxidant used.
[0050] Similar TGA and DTA characteristics were measured for the Ta analogue Ta(=NtBu)(NEt2)(O-tBu)2. Deposition on silicon wafers with O3 for 200 cycles also yields results similar to those seen for Nb(=NtBu)(NEt2)(O-tBu)2. At 275 °C, the growth rate was 4.69 Å / cycle with a composition of Ta: 32.8%, O: 56.5%, and C: 8.1%. Based on these results, it is expected that 1-9 cycles of ALD for cathodes or cathode material coatings will provide electrode performance benefits similar to those shown for Nau2 above.
[0051] Although the present invention has been described with specific embodiments thereof, it is apparent that many alternatives, modifications, and variations will be apparent to those skilled in the art in light of the foregoing description. It is therefore intended to embrace all such alternatives, modifications, and variations that fall within the spirit and broad scope of the appended claims. The present invention may suitably comprise, consist of, or consist essentially of the elements disclosed, and may be practiced in the absence of elements not disclosed. Furthermore, where there is language referring to a sequence such as first and second, it should be understood in a typical sense and not in a limiting sense. For example, it may be recognized by one skilled in the art that certain steps may be combined into a single step.
[0052] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0053] "Comprising" in the claims is an open transition term meaning that the claim elements identified thereafter are a non-exclusive recitation, i.e., nothing else may be further included and may be within the scope of "comprising." "Comprising" is defined herein as necessarily including the more narrow transition terms "consisting essentially of" and "consisting of." Thus, "comprising" may be replaced with "consisting essentially of" or "consisting of" and is within the clearly defined scope of "comprising."
[0054] "Providing" in the claims is defined to mean providing, supplying, making available, or preparing something. Steps may be performed by any actor, absent express language to the contrary in the claims.
[0055] Optional or optional means that the subsequently described event or circumstance may or may not occur. The description includes instances where the event or circumstance occurs and instances where it does not occur.
[0056] Ranges may be expressed herein from broadly one particular value and / or to broadly another particular value. When such a range is expressed, it should be understood that another embodiment is from the one particular value and / or to the other particular value, along with all combinations within said ranges.
[0057] All documents cited herein are each incorporated by reference in their entirety into this application as well as for the specific information for which each is cited.
Claims
1. 1. A method for coating a cathode or a cathode active material with a metal oxide film comprising: The cathode or cathode active material is a compound having the formula M (=NR a ) (OR b ) 2 (NR c 2 a1. exposing the resulting mixture to vapors of chemical precursors, including precursors of the formula (I) and a source of oxygen as an oxidizing co-reactant; (b1) depositing the metal oxide film on the cathode or cathode active material; Where: M is selected from Nb, Ta, or V; R a is selected from iPr, tBu, and t-Am; Each R b are independently selected from Et, iPr, tBu, sBu, SPen; Each R c is independently selected from Et or Me; method.
2. The precursor has the formula M(=NR a ) (OR b ) 2 2. The method of claim 1, wherein the compound is of formula (NMeEt).
3. R b 2. The method of claim 1 , wherein at least one of is independently selected from sBu, SPen.
4. The precursor has the formula M(=NR a ) (OR b ) 2 (NMeEt), R b 2. The method of claim 1 , wherein at least one of is independently selected from sBu, SPen.
5. Both R b The method of claim 3 or 4, wherein is independently selected from sBu, SPen.
6. The precursor is Nb(=NtBu)(NEt 2 ) (O-tBu) 2 , Nb (=NtBu) (NEt 2 ) 2 (O-tBu), Ta (=NtBu) (NEt 2 ) (O-tBu) 2 , Ta(=NtBu)(NEt 2 ) 2 (O-tBu), and mixtures thereof.
7. 2. The method of claim 1, wherein the steps a1. of exposing the cathode or cathode active material to a vapor of a chemical precursor and a2. of exposing the cathode or cathode active material to a co-reactant are performed sequentially.
8. 3. The method of claim 2, further comprising the step a1.i of purging the chemical precursor vapor prior to step a2 of exposing the cathode or cathode active material to a co-reactant.
9. 4. The method of claim 3, wherein step b1. of depositing the metal oxide film on the cathode or cathode active material comprises an atomic layer deposition process.
10. 4. The method of claim 3, wherein step b1. of depositing the metal oxide film on the cathode or cathode active material comprises a chemical vapor deposition process.
11. 6. The method of any one of claims 1 to 5, wherein the co-reactant is O2, O3, HO, HO, NO, NO2, NO or NOx; an oxygen source such as an oxygen-containing silicon precursor, an oxygen-containing tin precursor, trimethyl phosphate, a phosphate such as diethyl phosphoramidate, or a sulfate.
12. The metal oxide film produced by step b1. is Nb x O y D z where O is oxygen and D is any other atom, and x=0.3-0.4, y=0.4-0.65 and z=0.01-0.
1.
13. 13. The method according to any one of the preceding claims, wherein the temperature of the chemical precursor vapour and / or the cathode or cathode active material is from 100°C to 300°C, more preferably from 125°C to 275°C, even more preferably from 125°C to 175°C.
14. A method according to any one of the preceding claims, wherein the metal oxide film has an average thickness of 0.02 nm to 10 nm, preferably 0.1 nm to 5 nm, most preferably 0.2 to 2 nm.
15. 15. The method of any one of claims 1 to 14, wherein the cathode active material, or the cathode active material in the cathode, is selected from the group consisting of: a) layered oxides, such as high Ni cathode materials like NMC (lithium cobalt manganese nickel oxide) and NCA (lithium cobalt nickel aluminum oxide); b) spinel cathode materials, such as LMO (lithium manganese oxide), LNMO (lithium manganese nickel oxide); c) olivine structured cathode materials, in particular olivine phosphate types, such as LCP (lithium cobalt phosphate), LNP (lithium nickel phosphate), LFP (lithium iron phosphate); and combinations thereof.
16. The method according to any one of claims 1 to 15, wherein one or more of steps a1. and b1. are carried out 1 to 10 times, preferably 1 to 3 times.
17. 17. The method of claim 16, wherein a) the temperature of the chemical precursor vapor and / or the cathode or cathode active material is from 100°C to 300°C, more preferably from 125°C to 175°C, b) the metal oxide film has an average thickness of from 0.02 nm to 10 nm, preferably from 0.1 nm to 5 nm, most preferably from 0.2 to 2 nm; and c) the metal oxide film is at least 50% continuous on the surface of the cathode or cathode active material, preferably 95% or more continuous, more preferably 98% or more continuous.
Citation Information
Patent Citations
Composite positive electrode and application of composite positive electrode in solid-state polymer lithium ion battery
CN110085805A
Battery and positive electrode material for battery
JP2016197589A
Surface-treated positive electrode active material for lithium secondary battery, method for preparing the same, and lithium secondary battery comprising the same
US20170155132A1