Positive electrode material composition, its method of manufacture, positive electrode sheet containing the same, secondary battery, and power consumption device

A core-shell structured positive electrode material with crystalline coatings and an organopolysiloxane compound addresses manganese ion elution in lithium manganese phosphate, enhancing the cycle, safety, and rate performance of secondary batteries.

JP2024545195AActive Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED

Patent Information

Application Number
JP2024534749
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-12-05
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

Lithium manganese phosphate cathode active materials in secondary batteries suffer from manganese ion elution, leading to decreased capacity and safety issues due to interfacial side reactions and electrolyte erosion.

Method used

A core-shell structured positive electrode material composition is developed, comprising a lithium manganese phosphate kernel coated with multiple layers of crystalline pyrophosphate and phosphate, combined with an organopolysiloxane compound to reduce manganese ion elution and enhance stability.

Benefits of technology

The solution significantly improves the cycle performance, safety, and rate performance of secondary batteries by reducing manganese ion elution and electrolyte erosion, maintaining high energy density and structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545195000001_ABST
    Figure 2024545195000001_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode material composition, a method for producing the same, and a positive electrode sheet, a secondary battery, and a power consuming device each including the same. The positive electrode material composition includes a positive electrode active material having a core-shell structure and an organopolysiloxane compound, the positive electrode active material including a kernel and a shell that covers the kernel, and the chemical formula of the kernel is Li 1+x Mn 1-y A y P 1-z R z O4, and the shell includes a first coating layer that coats the kernel, a second coating layer that coats the first coating layer, and a third coating layer that coats the second coating layer. The positive electrode material composition can provide a secondary battery with high energy density and simultaneously achieve improved cycle performance, safety performance, and / or rate performance. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material composition, a manufacturing method thereof, and a positive electrode sheet, a secondary battery, and a power consuming device containing the same. [Background technology]

[0002] In recent years, secondary batteries have been widely used in many fields, such as energy storage power systems for hydroelectric, thermal, wind and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. With the application and popularity of secondary batteries, their safety performance has been attracting more and more attention. Lithium manganese phosphate is one of the most popular positive electrode active materials at present, due to its advantages of high capacity, good safety and abundant raw material supply sources. However, it is prone to manganese ion elution during charging, which causes rapid capacity decay. Summary of the Invention

[0003] The present application aims to provide a positive electrode material composition, a method for producing the same, and a positive electrode sheet, a secondary battery, and a power consuming device each including the same. A secondary battery using the positive electrode material composition has a high energy density and can simultaneously achieve improved cycle performance, safety performance, and / or rate performance.

[0004] A first aspect of the present application is a positive electrode material composition including a positive electrode active material having a core-shell structure and an organopolysiloxane compound, the positive electrode active material including a kernel and a shell that covers the kernel, the chemical formula of the kernel being Li 1+x Mn 1-y A y P 1-z R zO4, x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, z is any number within the range of 0.001 to 0.100, and A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally Fe, Ti, V, Ni, Co, and Mg; R is one or more elements selected from B, Si, N and S; optionally, R is one element selected from B, Si, N and S; the values ​​of x, y and z satisfy the condition that the entire kernel maintains electrical neutrality; the shell includes a first coating layer covering the kernel, a second coating layer covering the first coating layer and a third coating layer covering the second coating layer; the first coating layer is a crystalline pyrophosphate Li a MP2O7 and / or M b (P2O7) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP2O7 and M b (P2O7) c M is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al, and the values ​​of a, b and c are each independently one or more elements selected from the group consisting of crystalline pyrophosphate Li a MP2O7 or M b (P2O7) c satisfies the condition of maintaining electrical neutrality, the second coating layer contains a crystalline phosphate XPO4, where X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon.

[0005] The inventors have conducted a great deal of research and found that by modifying lithium manganese phosphate and coating the lithium manganese phosphate with multiple layers, it is possible to significantly reduce the elution of manganese ions and reduce the lattice change rate, and obtain a novel positive electrode active material having a core-shell structure that can be used in secondary batteries to improve the cycle performance, rate performance, and safety performance of the battery and improve the capacity of the battery. The use of the positive electrode active material of the present application in combination with an organopolysiloxane compound can mitigate the erosion of the surface of the positive electrode active material by the electrolyte and reduce the elution of manganese ions, which is advantageous for improving the electrochemical performance of the positive electrode active material. Therefore, the positive electrode sheet and secondary battery, etc., which employ the positive electrode material composition of the present application, can have a high energy density and simultaneously achieve improved cycle performance, safety performance, and / or rate performance.

[0006] In any embodiment of the present application, the organopolysiloxane compound comprises at least one structural unit represented by formula 1. [ka] R1 and R2 each independently represent at least one selected from the group consisting of -COOH, -OH, -SH, -CN, -SCN, an amino group, a phosphate ester group, a carboxylate ester group, an amide group, an aldehyde group, a sulfonyl group, a polyether segment, a C1-C20 aliphatic hydrocarbon group, a C1-C20 halogenated aliphatic hydrocarbon group, a C1-C20 heteroaliphatic hydrocarbon group, a C1-C20 halogenated heteroaliphatic hydrocarbon group, a C6-C20 aromatic hydrocarbon group, a C6-C20 halogenated aromatic hydrocarbon group, a C2-C20 heteroaromatic hydrocarbon group, and a C2-C20 halogenated heteroaromatic hydrocarbon group, or H. Alternatively, R1 and R2 each independently represent at least one selected from the group consisting of -COOH, -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, a C2-C8 halogenated alkenyl group, and a phenyl group, or H. More preferably, R1 and R2 each independently represent at least one selected from the group consisting of -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, and a C2-C8 halogenated alkenyl group, or H. This can further reduce the elution of manganese ions, thereby significantly improving the cycle performance and storage performance of the secondary battery.

[0007] In any embodiment of the present application, the organopolysiloxane compound includes one or more selected from a polysiloxane having a linear structure and a polysiloxane having a cyclic structure. Optionally, the organopolysiloxane compound is selected from a polysiloxane having a linear structure.

[0008] This further alleviates the erosion of the surface of the positive electrode active material by the acidic substance in the electrolyte, reduces the elution of manganese ions, and significantly improves the cycle performance and storage performance of the secondary battery. Since the electrons in the ring of the cyclic polysiloxane have a certain degree of delocalization, the affinity of the Si-O skeleton for the electron-rich F-containing ions is low compared to the linear polysiloxane, and the removal rate of the F-containing ions in the electrolyte is somewhat low, the effect of reducing the elution of manganese ions is somewhat weak, and the effect of improving the cycle performance of the secondary battery is somewhat low.

[0009] In any embodiment of the present application, the linear polysiloxane further comprises a blocking group. Optionally, the blocking group comprises at least one selected from the group consisting of polyether, C1-C8 alkyl group, C1-C8 halogenated alkyl group, C1-C8 heteroalkyl group, C1-C8 halogenated heteroalkyl group, C2-C8 alkenyl group, C2-C8 halogenated alkenyl group, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy group, C2-C8 epoxy group, hydroxyl group, C1-C8 hydroxyalkyl group, amino group, C1-C8 aminoalkyl group, carboxyl group, and C1-C8 carboxyalkyl group.

[0010] In any embodiment of the present application, the linear polysiloxane is selected from the group consisting of polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl-functionalized polysiloxane, polymethylchloropropylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, mercaptopropylpolysiloxane, and aminoethylaminopropylpolydimethylsiloxane. , methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, aminopropyl-terminated polydimethylsiloxane, epoxy-terminated polysiloxane, hydroxy-terminated polydimethylsiloxane, polyether-terminated polydimethylsiloxane, side chain aminopropyl polysiloxane, side chain hydroxylmethyl polysiloxane, side chain hydroxylpropyl polysiloxane, side chain polyether-grafted polydimethylsiloxane, side chain phosphate ester-grafted polydimethylsiloxane. Optionally, the linear structure polysiloxane includes one or more of polydimethylsiloxane, polymethylchloropropyl siloxane, polymethyltrifluoropropyl siloxane, mercaptopropyl polysiloxane, aminoethylaminopropyl polydimethylsiloxane, hydroxy-terminated polydimethylsiloxane, polyether-terminated polydimethylsiloxane, side chain phosphate ester-grafted polydimethylsiloxane.

[0011] In any embodiment of the present application, the polysiloxane of the cyclic structure includes one or more of cyclic polydimethylsiloxane, cyclic polymethylvinylsiloxane, cyclic polymethylhydrogensiloxane, cyclic polymethyltrifluoropropylsiloxane. Optionally, the polysiloxane of the cyclic structure includes one or more of 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, hexadecamethyloctasiloxane, and tetradecamethylcycloheptasiloxane.

[0012] In any embodiment of the present application, the number average molecular weight of the organopolysiloxane compound is not more than 300000, and optionally is 400 to 80000. This allows the secondary battery to have both good dynamic performance and high-temperature storage performance.

[0013] In any embodiment of the present application, the mass percentage of the polar functional group in the organopolysiloxane compound is α, and 0≦α<50%, optionally 5%≦α≦30%, thereby further improving the cycle performance and storage performance of the secondary battery.

[0014] In any embodiment of the present application, the content of the organopolysiloxane compound is 0.01% by weight to 2% by weight, and optionally 0.1% by weight to 2% by weight, based on the total weight of the positive electrode material composition, thereby making it possible to further improve the cycle performance and storage performance of the secondary battery.

[0015] In any embodiment of the present application, the coating amount of the first coating layer is greater than 0 and less than 6 wt %, optionally greater than 0 and less than 5.5 wt %, and more optionally greater than 0 and less than 2 wt %, based on the weight of the kernel.

[0016] In any embodiment of the present application, the coating amount of the second coating layer is greater than 0 and less than 6 wt %, optionally greater than 0 and less than 5.5 wt %, and more optionally 2 wt % to 4 wt %, based on the weight of the kernel.

[0017] In any embodiment of the present application, the coating amount of the third coating layer is greater than 0 and less than 6 wt %, optionally greater than 0 and less than 5.5 wt %, and more optionally greater than 0 and less than 2 wt %, based on the weight of the kernel.

[0018] In the positive electrode active material having a core-shell structure according to the present application, the coating amount of the three coating layers is preferably within the above range, which allows the kernel to be sufficiently coated and further improves the cycle performance, safety performance, and / or rate performance of the secondary battery without sacrificing the gram capacity (capacity per gram) of the positive electrode active material.

[0019] In any embodiment of the present application, the thickness of the first coating layer is 1 nm to 10 nm, which can avoid a negative effect on the dynamic performance of the positive electrode active material that may occur when the first coating layer is too thick, and can also avoid a problem that the migration of transition metal ions cannot be effectively inhibited when the first coating layer is too thin.

[0020] In any embodiment of the present application, the second coating layer has a thickness of 2 nm to 15 nm, in which case the surface structure of the second coating layer is stable and the side reaction with the electrolyte is small, effectively reducing the side reaction at the interface, thereby improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery.

[0021] In any embodiment of the present application, the third coating layer has a thickness of 2 nm to 25 nm, which can improve the conductivity of the positive electrode active material and the compressed density of the positive electrode sheet produced using the positive electrode active material.

[0022] In any embodiment of the present application, the lattice spacing of the crystalline pyrophosphate in the first coating layer is in the range of 0.293 nm to 0.470 nm, and the included angle of the (111) crystal orientation is in the range of 18.00° to 32.00°.

[0023] In any embodiment of the present application, the lattice spacing of the crystalline phosphate in the second coating layer is in the range of 0.244 nm to 0.425 nm, and the included angle of the (111) crystal orientation is in the range of 20.00° to 37.00°.

[0024] The crystalline pyrophosphate and crystalline phosphate within the above lattice spacing and included angle ranges can more effectively suppress the lattice change rate of lithium manganese phosphate and the elution of manganese ions during the lithium insertion / extraction process, thereby improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery.

[0025] In any embodiment of the present application, in the kernel, the ratio of y to 1-y is 1:10 to 1:1, and optionally 1:4 to 1:1, thereby further improving the cycle performance and rate performance of the secondary battery.

[0026] In any embodiment of the present application, in the kernel, the ratio of z to 1-z is 1:9 to 1:999, and optionally 1:499 to 1:249, thereby further improving the cycle performance and rate performance of the secondary battery.

[0027] In any embodiment of the present application, the carbon of the third coating layer is a mixture of SP2 carbon and SP3 carbon, and optionally, the molar ratio of the SP2 carbon to the SP3 carbon is any value within the range of 0.1 to 10, and optionally, any value within the range of 2.0 to 3.0. The present application improves the overall performance of the secondary battery by limiting the molar ratio of the SP2 carbon to the SP3 carbon within the above range.

[0028] In any embodiment of the present application, the content of manganese element is within the range of 10% by weight to 35% by weight, preferably within the range of 15% by weight to 30% by weight, more preferably within the range of 17% by weight to 20% by weight, based on the weight of the positive electrode active material. In this case, if the content of manganese element is too large, the structural stability of the positive electrode active material is deteriorated, and the density is reduced, etc., problems can be effectively avoided, and the performance of the cycle, storage, compression density, etc. of the secondary battery can be improved, and if the content of manganese element is too small, the problem of low voltage platform, etc. can be avoided, and the energy density of the secondary battery can be improved.

[0029] In any embodiment of the present application, the content of phosphorus element is in the range of 12 wt% to 25 wt% based on the weight of the positive electrode active material, and optionally in the range of 15 wt% to 20 wt%. In this case, the following situation can be effectively avoided. If the content of phosphorus element is too large, the covalent bond of PO is too strong, which may affect the conductivity of small polarons and affect the conductivity of the positive electrode active material; if the content of phosphorus element is too small, the stability of the lattice structure of the kernel, the pyrophosphate in the first coating layer, and / or the phosphate in the second coating layer may decrease, which may affect the stability of the entire positive electrode active material.

[0030] In any embodiment of the present application, the weight ratio of manganese element to phosphorus element is in the range of 0.90-1.25, and optionally 0.95-1.20, relative to the weight of the positive electrode active material. In this case, the following situation can be effectively avoided: if the weight ratio is too large, the elution of manganese ions increases, which may affect the stability of the positive electrode active material and the cycle performance and storage performance of the secondary battery; if the weight ratio is too small, the discharge voltage platform of the positive electrode active material may decrease, which may reduce the energy density of the secondary battery.

[0031] In any embodiment of the present application, the positive electrode active material has a lattice change rate before and after complete insertion and extraction of lithium of 4% or less, optionally 3.8% or less, and more preferably 2.0% to 3.8%, in which case the positive electrode active material can improve the capacity and rate performance of a secondary battery.

[0032] In any embodiment of the present application, the Li / Mn antistructural defect concentration of the positive electrode active material is 4% or less, preferably 2.2% or less, and more preferably 1.5% to 2.2%. By having the Li / Mn antistructural defect concentration within the above range, Mn 2+ Li + This makes it possible to avoid impeding the transport of the positive electrode active material, while improving the capacity and rate performance of the positive electrode active material.

[0033] In any embodiment of the present application, the positive electrode active material has a compressed density at 3 T of 2.2 g / cm 3 or more, and optionally 2.2 g / cm 3 Above 2.8g / cm 3 This is advantageous for improving the volumetric energy density of the secondary battery.

[0034] In any embodiment of the present application, the oxygen valence number on the surface of the positive electrode active material is −1.90 or less, and optionally −1.90 to −1.98. By setting the oxygen valence number on the surface of the positive electrode active material within the above range, it is possible to reduce side reactions at the interface between the positive electrode active material and the electrolyte, and improve the cycle performance, storage performance, etc. of the secondary battery.

[0035] In any embodiment of the present application, the positive electrode material composition further includes a conductive agent and a binder, and optionally, the content of the binder is 1.79 wt% to 10 wt% based on the total weight of the positive electrode material composition, and optionally, the content of the conductive agent is 0.2 wt% to 10 wt% based on the total weight of the positive electrode material composition.

[0036] In any embodiment of the present application, the powder resistivity of the positive electrode material composition at 12 MPa is 4Ω / cm to 55Ω / cm, and optionally 4Ω / cm to 40Ω / cm, so that the secondary battery has better dynamic performance.

[0037] In any embodiment of the present application, the specific surface area of ​​the positive electrode material composition is 8 m 2 / g~20m 2 / g, and selectively 8m 2 / g~15m 2 / g, which allows the secondary battery to have better electrochemical performance.

[0038] A second aspect of the present application provides a method for producing a positive electrode material composition, comprising the steps of providing a kernel material, coating, and mixing.

[0039] Providing a kernel material, the kernel having a chemical formula of Li 1+x Mn 1-y A y P 1-z R z O4, where x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, and z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg, R is one or more elements selected from B, Si, N, and S, and optionally one element selected from B, Si, N, and S, and the values ​​of x, y, and z satisfy the condition that the entire kernel maintains electrical neutrality.

[0040] The coating steps are Li a MP2O7 and / or M b (P2O7) cand XPO4 suspension, and adding the kernel material to the suspension, mixing and sintering to obtain a positive electrode active material, wherein the positive electrode active material has a core-shell structure, which includes the kernel and a shell covering the kernel, the shell includes a first coating layer covering the kernel, a second coating layer covering the first coating layer and a third coating layer covering the second coating layer, and the first coating layer is a crystalline pyrophosphate Li a MP2O7 and / or M b (P2O7) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP2O7 and M b (P2O7) c M is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al, and the values ​​of a, b and c are each independently one or more elements selected from the group consisting of crystalline pyrophosphate Li a MP2O7 or M b (P2O7) c satisfies the condition of maintaining electrical neutrality, the second coating layer contains crystalline phosphate XPO4, where X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon.

[0041] In the mixing step, the obtained positive electrode active material is uniformly mixed with an organopolysiloxane compound, an optional binder, and an optional conductive agent to obtain a positive electrode material composition.

[0042] In any embodiment of the present application, the step of providing the kernel material comprises the following steps (1) and (2).

[0043] In step (1), a manganese source, a dopant of element A, and an acid are mixed and stirred in a container to obtain manganese salt particles doped with element A.

[0044] In step (2), the manganese salt particles doped with element A are mixed with a lithium source, a phosphorus source and a dopant of element R in a solvent to obtain a slurry, which is then sintered under the protection of an inert gas atmosphere to obtain a kernel doped with element A and element R, where the kernel doped with element A and element R is Li 1+x Mn 1-y A y P 1-z R z O4, where x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, and z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg, and R is one or more elements selected from B, Si, N, and S, and optionally one element selected from B, Si, N, and S.

[0045] In any embodiment of the present application, the step (1) is performed at a temperature of 20°C to 120°C, optionally 40°C to 120°C.

[0046] In any embodiment of the present application, the stirring in step (1) is carried out at 400 rpm to 700 rpm for 1 hour to 9 hours, selectively for 3 hours to 7 hours.

[0047] When the heating temperature and stirring time during the production process of the kernel particles are within the above ranges, the produced kernel and the positive electrode active material produced therefrom have few lattice defects, which is advantageous in suppressing the dissolution of manganese ions, reducing interfacial side reactions between the positive electrode active material and the electrolyte, and improving the cycle performance and safety performance of the secondary battery.

[0048] In any embodiment of the present application, the step (2) is performed by mixing at a temperature of 20° C. to 120° C., optionally 40° C. to 120° C., for 1 hour to 10 hours.

[0049] In any embodiment of the present application, the dopant of the element A is one or more selected from the group consisting of a simple substance, a carbonate, a sulfate, a chloride, a nitrate, an organic acid salt, an oxide, and a hydroxide of one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge.

[0050] In any embodiment of the present application, the dopant of the element R is one or more selected from inorganic acids, organic acids, sulfates, chlorides, nitrates, organic acid salts, oxides, and hydroxides of one or more elements selected from B, Si, N, and S.

[0051] In any embodiment of the present application, the coating step includes a first coating step, a second coating step and a third coating step.

[0052] In the first coating step, a source of element M, a phosphorus source and an acid, and an optional lithium source are dissolved in a solvent to obtain a first coating layer suspension, and the kernel obtained in the step of providing a kernel material and the first coating layer suspension obtained in the first coating step are thoroughly mixed, dried, and then sintered to obtain a material coated with a first coating layer.

[0053] In the second coating step, a source of element X, a phosphorus source, and an acid are dissolved in a solvent to obtain a second coating layer suspension, and the material coated with the first coating layer obtained in the first coating step and the second coating layer suspension obtained in the second coating step are thoroughly mixed, dried, and then sintered to obtain a material coated with two coating layers.

[0054] In the third coating step, the carbon source is dissolved in a solvent and sufficiently dissolved to obtain a third coating layer solution, and then the material coated with two coating layers obtained in the second coating step is added to the third coating layer solution, mixed uniformly, dried, and then sintered to obtain a material coated with three coating layers, i.e., a positive electrode active material.

[0055] In any embodiment of the present application, in the first coating step, the pH of a solution of a source in which element M is dissolved, a phosphorus source, an acid, and a selectable lithium source is controlled to 3.5 to 6.5, and then the solution is stirred for 1 to 5 hours to react, and then the solution is heated to 50°C to 120°C and maintained at that temperature for 2 to 10 hours.

[0056] In any embodiment of the present application, in the first coating step, the sintering is carried out at 650° C. to 800° C. for 2 hours to 6 hours.

[0057] By setting the conditions of the first coating step within the above ranges, it is possible to not only maintain but also improve the capacity, cycle performance, high-temperature storage performance, and rate performance of a secondary battery manufactured using the positive electrode active material.

[0058] In any embodiment of the present application, in the second covering step, a source of element X, a phosphorus source, and an acid are dissolved in a solvent, and then the solution is reacted with each other by stirring for 1 hour to 10 hours, and then the solution is heated to 60°C to 150°C and maintained at the temperature for 2 hours to 10 hours.

[0059] In any embodiment of the present application, in the second coating step, sintering is carried out at 500° C. to 700° C. for 6 hours to 10 hours.

[0060] In the step of providing the kernel material, the first coating step and the second coating step, before sintering, i.e., in the production of the kernel material in which a chemical reaction occurs (step (1) and step (2)) and the production of the first coating layer suspension and the second coating layer suspension, the reaction temperature and reaction time selected as above can avoid the following situations: if the reaction temperature is too low, the reaction cannot occur or the reaction rate is slow; if the temperature is too high, the product will decompose or form impurities; if the reaction time is too long, the product will have a large particle size, which may increase the time and difficulty of subsequent processes; and if the reaction time is too short, the reaction will be incomplete and the product will be small.

[0061] In any embodiment of the present application, the sintering in the third coating step is carried out at 700° C. to 800° C. for 6 hours to 10 hours.

[0062] By setting the conditions of the third covering step within the above ranges, the capacity development and compressed density of the positive electrode active material can be improved.

[0063] The method for producing a positive electrode active material according to the present application has a wide supply source of raw materials, low cost, and a simple process, which is advantageous for industrialization.

[0064] A third aspect of the present application provides a positive electrode sheet including a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, the positive electrode film layer including the positive electrode material composition according to the first aspect of the present application or a positive electrode material composition produced by the method according to the second aspect of the present application, and a content of the positive electrode material composition in the positive electrode film layer is 50 wt % or more with respect to a total weight of the positive electrode film layer.

[0065] In any embodiment of the present application, the content of the positive electrode material composition in the positive electrode membrane layer is 90% by weight to 100% by weight with respect to the total weight of the positive electrode membrane layer.

[0066] In any embodiment of the present application, the solid-liquid contact angle between the positive electrode film layer and the nonaqueous organic solvent is 3° to 90°, optionally 3° to 60°, and further 10° to 30°. When the contact angle is within an appropriate range, the secondary battery can achieve both high energy density and improved cycle performance, safety performance, and / or rate performance.

[0067] In any embodiment of the present application, the porosity of the positive electrode membrane layer is 15% to 50%, and optionally 15% to 30%. When the porosity is within an appropriate range, the secondary battery can achieve both high energy density and improved cycle performance, safety performance, and / or rate performance.

[0068] In any embodiment of the present application, the resistance of the positive electrode film layer is greater than 0 and less than or equal to 6Ω, so that the secondary battery can have better dynamic performance.

[0069] In any embodiment of the present application, the adhesive strength between the positive electrode film layer and the positive electrode current collector is 0.5 MPa or more, which is advantageous for exhibiting the performance of the secondary battery.

[0070] In any embodiment of the present application, the areal density of the positive electrode film layer is 0.006 g / cm 2 ~0.065g / cm 2 This is advantageous for improving the volumetric energy density of the secondary battery.

[0071] In any embodiment of the present application, the positive electrode membrane layer has an electrolyte absorption rate of 0.0125 μg / s to 100 μg / s, and optionally 0.5 μg / s to 40 μg / s, which is advantageous for improving the electrochemical performance of the secondary battery.

[0072] The positive electrode sheet of the present application can be used in a secondary battery to improve the energy density, cycle performance, safety performance, and / or rate performance of the secondary battery.

[0073] A fourth aspect of the present application provides a secondary battery including the positive electrode active material of the first aspect of the present application, or the positive electrode active material produced by the method of the second aspect of the present application, or the positive electrode sheet of the third aspect of the present application.

[0074] A fifth aspect of the present application provides a power consuming device including the secondary battery of the fourth aspect of the present application.

[0075] The positive electrode sheet, secondary battery, and power consuming device of the present application contain the positive electrode material composition of the present application, and therefore have at least the same advantages as the positive electrode material composition. [Brief description of the drawings]

[0076] In order to more clearly describe the technical solutions of the embodiments of the present application, the drawings that need to be used in the embodiments of the present application are briefly described below. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on the drawings without creative efforts. [Figure 1] FIG. 1 is a schematic diagram of one embodiment of a secondary battery of the present disclosure. [Diagram 2] FIG. 2 is an exploded schematic view of the embodiment of the secondary battery of FIG. 1. [Diagram 3] FIG. 1 is a schematic diagram of one embodiment of a battery module of the present application. [Figure 4] FIG. 1 is a schematic diagram of one embodiment of a battery pack of the present application. [Diagram 5] 5 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 4. [Figure 6] 1 is a schematic diagram of one embodiment of a power consuming device including a secondary battery of the present application as a power source. [Explanation of symbols]

[0077] 1 Battery pack 2 Upper case 3 Lower case 4 Battery Module 5 Secondary battery 51 cases 52 Electrode Assembly 53 Cover plate DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0078] Hereinafter, the embodiments of the positive electrode material composition specifically disclosed in this application, the manufacturing method thereof, and the positive electrode sheet, secondary battery, and power consumption device containing the same will be described in detail with reference to the drawings as appropriate. However, unnecessary detailed explanations may be omitted. For example, detailed explanations of already well-known matters and duplicated explanations of substantially the same configurations may be omitted. This is to avoid the following explanation becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Note that the attached drawings and the following explanation are provided to enable those skilled in the art to fully understand this application, and are not intended to limit the subject matter described in the claims.

[0079] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such a defined range may be an end value or a range that does not include end values, and may be combined in any way, i.e., any lower limit may be combined with any upper limit. For example, if the ranges 60-120 and 80-110 are recited for a particular parameter, the ranges 60-110 and 80-120 are also contemplated. Also, if the minimum range values ​​1 and 2 and the maximum range values ​​3, 4 and 5 are recited, the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 may all be contemplated. In this application, unless otherwise stated, the numerical range "a-b" is represented by the abbreviation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, with "0-5" being an abbreviation for combinations of these numerical values. Furthermore, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0080] Unless otherwise specified, all the embodiments and optional embodiments of the present application may be combined with each other to form a new technical solution, and such technical solution should be considered to be included in the disclosure content of the present application.

[0081] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form a new technical solution, and such technical solution should be considered as included in the disclosure content of the present application.

[0082] Unless otherwise stated, all steps in this application may be performed in sequence, randomly, and preferably in sequence. For example, the method includes steps (a) and (b) indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, when it is stated that the method may further include step (c), it indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.

[0083] Unless otherwise specified, the terms "comprise", "have", and "comprise" used herein mean open-ended and may also be closed-ended. For example, the terms "comprise", "have", and "comprise" may mean "comprise", "have", or "comprise" other components not listed, or "comprise", "have", or "comprise" only the listed components.

[0084] In this application, the term "or" is inclusive unless otherwise specified. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or, both A and B are true (or exist).

[0085] As used herein, the terms "plurality" and "plurality" mean two or more.

[0086] In this specification, the term "about" refers to a range of a certain numerical value, and refers to a range of ±10% of the said numerical value.

[0087] In this specification, the term "coating layer" refers to a material layer that coats the lithium manganese phosphate kernel, and the material layer can completely or partially coat the lithium manganese phosphate kernel, and the term "coating layer" is used for convenience of explanation and is not intended to limit the present application. Furthermore, each coating layer may completely coat or partially coat. Similarly, the term "thickness of coating layer" refers to the thickness of the material layer coated on the lithium manganese phosphate kernel in the radial direction of the lithium manganese phosphate kernel.

[0088] In this specification, the median diameter Dv50 refers to the particle size corresponding to the cumulative volume distribution percentage of the material reaches 50%. In this application, the median diameter Dv50 of the material can be measured by laser diffraction granulometry. For example, refer to standard GB / T 19077-2016 and use a laser granulometer (e.g. Malvern Master Size 3000) to measure.

[0089] Substituents of compounds are disclosed herein in groups or ranges, and such descriptions specifically contemplate that each of the members of these groups and ranges also include each individual subcombination. For example, the term "C1-C8 alkyl group" is expressly expected to disclose C1, C2, C3, C4, C5, C6, C7, C8, C1-C8, C1-C7, C1-C6, C1-C5, C1-C4, C1-C3, C1-C2, C2-C8, C2-C7, C2-C6, C2-C5, C2-C4, C2-C3, C3-C8, C3-C7, C3-C6, C3-C5, C3-C4, C4-C8, C4-C7, C4-C6, C4-C5, C5-C8, C5-C7, C5-C6, C6-C8, C6-C7, and C7-C8 alkyl groups singly.

[0090] As used herein, the term "aliphatic hydrocarbon group" includes alkyl groups, alkenyl groups, and alkynyl groups, and the term "heteroaliphatic hydrocarbon group" means an aliphatic hydrocarbon group containing a heteroatom (e.g., N, O, S, etc.). The term "heteroalkyl group" refers to an alkyl group containing a heteroatom (e.g., N, O, S, etc.), and may be, for example, an alkoxy group, an alkylthio group, etc.

[0091] In practical work, the inventors of the present application have found that the current conventional lithium manganese phosphate LiMnPO4 positive electrode active material has serious manganese ion elution during deep charge and discharge processes. In the prior art, lithium manganese phosphate is coated with lithium iron phosphate to reduce the interfacial side reaction, but such a coating cannot prevent the eluted manganese ions from continuing to move to the electrolyte. The eluted manganese ions are reduced to metallic manganese after moving to the negative electrode. The metallic manganese thus generated corresponds to a "catalyst" and can catalyze the decomposition of the SEI film (solid electrolyte interphase) on the surface of the negative electrode to generate by-products. Since some of the by-products are gases, they cause the expansion of the secondary battery and affect the safety performance of the secondary battery, and the other part of the by-products is deposited on the surface of the negative electrode, blocking the channel through which lithium ions enter and exit the negative electrode, causing an increase in the resistance of the secondary battery and affecting the dynamic performance of the secondary battery. In addition, in order to compensate for the loss of the SEI film, the electrolyte and active lithium inside the battery continue to be consumed, which has an irreversible effect on the capacity retention rate of the secondary battery.

[0092] The inventors have found through intensive research that by modifying lithium manganese phosphate and coating the lithium manganese phosphate with multiple layers, it is possible to obtain a novel core-shell structured positive electrode active material that can be used in secondary batteries to improve the cycle performance, rate performance, and safety performance of the battery and improve the capacity performance of the battery. At the same time, the inventors of the present application have found that the use of a combination of a positive electrode active material and an organopolysiloxane compound can mitigate the erosion of the surface of the positive electrode active material by the electrolyte, which is advantageous for fully demonstrating the electrochemical performance of the positive electrode active material. Positive electrode material composition

[0093] Specifically, a first aspect of the present application proposes a positive electrode material composition including a positive electrode active material having a core-shell structure and an organopolysiloxane compound.

[0094] The positive electrode active material includes a kernel and a shell that covers the kernel. The chemical formula of the kernel is Li 1+x Mn 1-y A y P 1-z R z O4, where x is any number within the range of -0.100 to 0.100, y is any number within the range of 0.001 to 0.500, z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally is one or more elements selected from Fe, Ti, V, Ni, Co, and Mg, R is one or more elements selected from B, Si, N, and S, and optionally is one element selected from B, Si, N, and S, and the values ​​of x, y, and z satisfy the condition for maintaining the entire kernel electrically neutral. The shell includes a first coating layer that coats the kernel, a second coating layer that coats the first coating layer, and a third coating layer that coats the second coating layer, and the first coating layer is made of crystalline Li pyrophosphate. a MP2O7 and / or M b (P2O7) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP2O7 and M b (P2O7) c M is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al, and the values ​​of a, b and c are each independently one or more elements selected from the group consisting of crystalline pyrophosphate Li a MP2O7 or M b (P2O7) c satisfies the condition of maintaining electrical neutrality, the second coating layer contains crystalline phosphate XPO4, where X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon.

[0095] Unless otherwise specified, in the above kernel chemical formula, when A is two or more elements, the above-mentioned limit on the numerical range of y is not only a limit on each of the stoichiometric numbers of A as an element, but also a limit on the sum of the stoichiometric numbers of A as an element. For example, when A is two or more elements A1, A2...An, each of the stoichiometric numbers y1, y2...yn of A1, A2...An must be within the numerical range limited for y in this application, and the sum of y1, y2...yn must also be within the numerical range. Similarly, when R is two or more elements, the limit on the numerical range of the stoichiometric numbers of R in this application has the above meaning.

[0096] In one alternative embodiment, when A is one, two, three or four elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, A y Q n1 D n2 E n3 K n4 and n1+n2+n3+n4=y, and n1, n2, n3, n4 are all positive numbers and not zero at the same time. Q, D, E, and K are each independently one selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally at least one of Q, D, E, and K is Fe. Alternatively, one of n1, n2, n3, and n4 is zero and the remaining is not zero, more preferably, two of n1, n2, n3, and n4 are zero and the remaining is not zero, and even more preferably, three of n1, n2, n3, and n4 are zero and the remaining is not zero. The kernel Li 1+x Mn 1-y A y P 1-z R z In O4, it is advantageous to dope the manganese site with one, two, three or four of the above A elements, and selectively dope the phosphorus site with one, two or three of the above A elements, and it is advantageous to dope the phosphorus site with one or two R elements, thus making the doping elements uniformly distributed.

[0097] The kernel Li 1+x Mn 1-y A y P 1-z R z In O4, the magnitude of x is influenced by the magnitude of the valence of A and R and the magnitude of y and z, and ensures that the whole system exhibits electrical neutrality. If the value of x is too small, the lithium content of the whole kernel system will decrease, affecting the capacity of the positive electrode active material. The value of y limits the total amount of all doping elements, and if y is too small, that is, if the doping amount is too small, the doping elements will not function, and if y is more than 0.5, the Mn content in the system will be low, affecting the voltage platform of the material. The R element is doped at the P position, PO tetrahedrons are stabilized, and if the z value is too large, it will affect the stability of the material, so the z value is limited to 0.001 to 0.100.

[0098] The positive electrode active material of the present application can improve the capacity, cycle performance and safety performance of the secondary battery. Although the mechanism is not clear, the possible reason is that the positive electrode active material of the lithium manganese phosphate of the present application has a core-shell structure, and the manganese site and phosphorus site of the lithium manganese phosphate kernel are doped with element A and element R, respectively, to effectively reduce the dissolution of manganese ions, further reduce the manganese ions transferred to the negative electrode, reduce the electrolyte consumed by the decomposition of the SEI film, and improve the cycle performance and safety performance of the secondary battery, as well as promote the adjustment of Mn-O bonds, reduce the lithium ion migration barrier, promote the lithium ion migration, and improve the rate performance of the secondary battery. By coating the kernel with a first coating layer containing crystalline pyrophosphate, the migration resistance of manganese ions can be further increased, the dissolution can be reduced, the content of lithium impurities on the surface can be reduced, and the contact between the kernel and the electrolyte can be reduced, thereby reducing the side reaction at the interface, reducing gas generation, and improving the high temperature storage performance, cycle performance and safety performance of the secondary battery. By further coating with a crystalline phosphate coating layer having excellent lithium ion conducting ability, the side reaction at the interface between the positive electrode active material and the electrolyte can be effectively reduced, and the high temperature cycle and storage performance of the secondary battery can be further improved. By further coating with a carbon layer as a third coating layer, the safety performance and dynamic performance of the secondary battery can be improved.

[0099] In addition, in the kernel, the element A doped into the manganese site of the lithium manganese phosphate reduces the lattice change rate of the lithium manganese phosphate during the lithium insertion and desorption process of the material, improves the structural stability of the lithium manganese phosphate positive electrode active material, greatly reduces the dissolution of manganese ions, and also helps to reduce the oxygen activity of the particle surface. The element R doped into the phosphorus site also helps to change the difficulty of the length change of the Mn-O bond, thereby improving the electronic conduction, lowering the lithium ion migration barrier, promoting the lithium ion migration, and improving the rate performance of the secondary battery.

[0100] In addition, when the entire kernel system maintains electrical neutrality, defects and impurity phases in the positive electrode active material can be kept as small as possible. If an excess transition metal (e.g., manganese) is present in the positive electrode active material, the structure of the material system itself is stable, so that the excess transition metal may precipitate as a single element or form an impurity phase inside the crystal lattice. By maintaining electrical neutrality, such heterogeneous phases can be reduced as much as possible. In addition, while ensuring electrical neutrality of the system, lithium deficiency can be caused in the positive electrode active material in some cases, and the dynamic performance of the positive electrode active material can be improved.

[0101] The positive electrode material composition of the present application includes a positive electrode active material and an organopolysiloxane compound. The inventors of the present application have found that the use of the above positive electrode active material in combination with the organopolysiloxane compound can alleviate the erosion of the surface of the positive electrode active material by the electrolyte and reduce the elution of manganese ions, which is advantageous for improving the electrochemical performance of the positive electrode active material. Possible causes include the Si-O skeleton of the organopolysiloxane compound being able to remove F-containing ions in the electrolyte, thereby reducing the acidity of the electrolyte and alleviating the erosion of the surface of the positive electrode active material by the acidic substances in the electrolyte; the organopolysiloxane compound also has a certain water repellency, and after producing a positive electrode sheet together with the positive electrode active material, the contact angle between the obtained positive electrode sheet and the electrolyte increases, which can alleviate the erosion of the surface of the positive electrode active material by the electrolyte.

[0102] Therefore, a power consuming device such as a positive electrode sheet and a secondary battery that employs the positive electrode material composition of the present application can have a high energy density and simultaneously achieve improved cycle performance, safety performance, and / or rate performance.

[0103] The average particle size of the kernel produced in the present application is in the range of 50 nm to 500 nm, and Dv50 is 200 nm to 300 nm. The size of the primary particles of the kernel is always 50 nm to 500 nm, and Dv50 is 200 nm to 300 nm. If the average particle size of the kernel is too large (more than 500 nm), it affects the capacity of the secondary battery using this material, and if the average particle size of the kernel is too small, the specific surface area is large and the material is prone to aggregation, making it difficult to achieve a uniform coating.

[0104] Process control (e.g., thoroughly mixing and polishing various source materials) can ensure that each element is uniformly distributed in the crystal lattice and does not aggregate. The main characteristic peak positions in the X-ray diffraction (XRD) pattern of lithium manganese phosphate doped with A and R elements are consistent with those of undoped LiMnPO4, indicating that no impurity phase is introduced during the doping process. Therefore, the improvement in kernel performance is mainly due to element doping, not due to impurity phase. After the inventor of the present application produced the positive electrode active material of the present application, the inventor cut out the middle region (kernel region) of the positive electrode active material particle produced by focused ion beam (FIB) and measured it by transmission electron microscope (TEM) and X-ray spectroscopy (EDS), and found that each element is uniformly distributed and no aggregation occurs.

[0105] In the present application, crystalline (crystalline state) means that the degree of crystallinity is 50% or more, i.e., 50% to 100%. A crystallinity of less than 50% is called glass state (or amorphous). The crystallinity of the crystalline pyrophosphate and crystalline phosphate described in the present application is 50% to 100%. Pyrophosphates and phosphates having a certain degree of crystallinity are not only advantageous in that the pyrophosphate coating layer can fully exhibit the functions of inhibiting the elution of manganese ions, the excellent lithium ion conducting ability of the phosphate coating layer, and reducing interfacial side reactions, but also can achieve better lattice matching between the pyrophosphate coating layer and the phosphate coating layer, thereby realizing closer bonding of the coating layer.

[0106] In the present application, the crystallinity of the crystalline pyrophosphate of the first coating layer material and the crystalline phosphate of the second coating layer material of the positive electrode active material may be measured by conventional technical means in the art, such as density method, infrared spectroscopy, differential scanning calorimetry, and nuclear magnetic resonance spectroscopy, and may also be measured by, for example, X-ray diffraction method.

[0107] A specific method for measuring the crystallinity of the crystalline pyrophosphate of the first coating layer and the crystalline phosphate of the second coating layer of a positive active material by X-ray diffraction includes the steps of taking a certain amount of positive active material powder, measuring the total scattering intensity, which is the sum of the scattering intensity of the entire spatial material, by X-ray, and finding that the total scattering intensity is related only to the intensity of the primary radiation, the chemical structure of the positive active material powder, and the total number of electrons participating in the diffraction, i.e., mass, and not related to the order state of the sample, and then separating the crystalline scattering and non-crystalline scattering from the diffraction pattern, and the crystallinity is the ratio of the scattering of the crystalline part to the total scattering intensity.

[0108] In the present application, the crystallinity of the pyrophosphate and phosphate in the coating layer can be adjusted by adjusting the process conditions of the sintering process, such as the sintering temperature and sintering time.

[0109] In this application, since metal ions are difficult to move to pyrophosphate, the pyrophosphate can be used as the first coating layer to effectively isolate the doped metal ions from the electrolyte. Since the crystalline pyrophosphate has a stable structure, the crystalline pyrophosphate coating can effectively inhibit the elution of transition metals and improve cycle performance.

[0110] The bond between the first coating layer and the core is similar to a heterojunction, and the strength of the bond is limited by the degree of lattice matching. When the lattice mismatch is 5% or less, the lattice matching is good and the two are easily bonded tightly. The tight bond can ensure that the coating layer does not fall off during the subsequent cycle process, which is advantageous for ensuring the long-term stability of the positive electrode active material. The degree of bond between the first coating layer and the core is mainly evaluated by calculating the degree of mismatch of each lattice constant of the core and the coating. In the present application, after the kernel is doped with the A and R elements, the matching degree between the kernel and the first coating layer is improved compared to when no doping elements are present, and the kernel and the pyrophosphate coating layer can be bonded more tightly.

[0111] The crystalline phosphate is selected as the second coating layer because, first, it has a high degree of lattice matching with the crystalline pyrophosphate of the first coating layer (the degree of mismatch is only 3%), and second, the stability of the phosphate itself is better than that of pyrophosphate, so that coating with pyrophosphate is advantageous for improving the stability of the positive electrode active material. Since the crystalline phosphate has a stable structure and excellent lithium ion conductivity, coating with the crystalline phosphate effectively reduces side reactions at the interface between the positive electrode active material and the electrolyte, thereby improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery. The manner of lattice matching between the second coating layer and the first coating layer is similar to that of the bonding between the first coating layer and the core described above, and when the lattice mismatch is 5% or less, the lattice matching is good and the two are easily bonded closely.

[0112] The main reason for choosing carbon as the third coating layer is that the carbon layer has good electronic conductivity. When applied to a secondary battery, an electrochemical reaction occurs, which requires the participation of electrons. Therefore, the positive electrode active material can be coated with carbon, which has excellent conductive performance, to increase the electron transport between particles and between different positions on the particle. The carbon coating can effectively improve the conductive performance and desolvation ability of the positive electrode active material.

[0113] In some embodiments, the average particle size of the primary particles of the positive electrode active material is 50 nm to 500 nm, and the volume median diameter Dv50 is within the range of 200 nm to 300 nm. Since the particles aggregate, the size of the secondary particles after the aggregation actually measured may be 500 nm to 40000 nm. The size of the positive electrode active material particles affects the processing of the material and the compressed density performance of the electrode sheet. By selecting the average particle size of the primary particles to be within the above range, it is possible to effectively avoid that if the average particle size of the primary particles of the positive electrode active material is too small, the particles may aggregate, making dispersion difficult, and a large amount of binder is required, which may deteriorate the brittleness of the electrode sheet, and if the average particle size of the primary particles of the positive electrode active material is too large, the gaps between the particles may become large, which may reduce the compressed density.

[0114] The above technical solution can effectively suppress the lattice change rate of lithium manganese phosphate and the elution of manganese ions during the lithium insertion / extraction process, thereby improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery.

[0115] In some embodiments, the lattice spacing of the crystalline pyrophosphate in the first coating layer ranges from 0.293 nm to 0.470 nm and the included angle of the (111) crystal orientation ranges from 18.00° to 32.00°, and the lattice spacing of the crystalline phosphate in the second coating layer ranges from 0.244 nm to 0.425 nm and the included angle of the (111) crystal orientation ranges from 20.00° to 37.00°.

[0116] The first and second coating layers in the positive electrode active material according to the present application are both made of crystalline materials. The crystalline pyrophosphate and crystalline phosphate in the coating layers can be characterized by conventional technical means in the art. For example, they can be characterized by a transmission electron microscope (TEM). In the TEM, the kernel and the coating layer can be distinguished by measuring the lattice spacing.

[0117] The specific method for measuring the lattice spacing and included angle between the crystalline pyrophosphate and the crystalline phosphate in the coating layer can include the steps of: putting a certain amount of coated positive active material sample powder into a test tube, injecting a solvent, such as alcohol, into the test tube, and then thoroughly stirring and dispersing, and then taking an appropriate amount of the above solution with a clean disposable plastic pipette and dropping it onto a 300 mesh copper mesh, at this time, some powder remains on the copper mesh, and the copper mesh is transferred together with the sample to a TEM sample chamber for testing, and obtaining the original image of the TEM test. The original image obtained by the above TEM test is run through a diffraction device software, and a diffraction pattern is obtained by performing Fourier transformation, and the distance from the diffraction spot to the center position in the diffraction pattern is measured, so that the lattice spacing can be obtained, and the included angle can be calculated according to the Bragg equation.

[0118] Crystalline pyrophosphate is distinguished from crystalline phosphate by the range of lattice spacing, which can be directly determined by the numerical value of the lattice spacing.

[0119] The crystalline pyrophosphate and crystalline phosphate within the above lattice spacing and included angle ranges can more effectively suppress the lattice change rate of lithium manganese phosphate and the elution of manganese ions during the lithium insertion / extraction process, thereby improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery.

[0120] In the kernel, x may be any number within the range of -0.100 to 0.100, for example, x may be 0.001, 0, -0.001, -0.002, -0.003, -0.004, -0.005. Optionally, x may be any number within the range of -0.005 to 0.002.

[0121] In the kernel, y may be any number within the range of 0.001 to 0.500, for example, y may be 0.001, 0.100, 0.200, 0.300, 0.350, 0.400, 0.450, or 0.500.

[0122] In the kernel, z is an arbitrary value within the range of 0.001 to 0.100, and for example, z may be 0.001, 0.002, 0.003, 0.004, 0.005, or 0.100.

[0123] In some embodiments, the ratio of y to 1-y in the kernel is 1:10 to 1:1, and optionally 1:4 to 1:1, where y represents the sum of the stoichiometric numbers of the doping elements A at the Mn site. By satisfying the above conditions, the energy density and cycle performance of a secondary battery using the positive electrode active material can be further improved.

[0124] In some embodiments, the ratio of z to 1-z in the kernel is 1:9 to 1:999, and optionally 1:499 to 1:249, where z represents the sum of the stoichiometric numbers of the doping elements R in the P site. By satisfying the above condition, the energy density and cycle performance of the secondary battery using the positive electrode active material can be further improved.

[0125] In some embodiments, the carbon of the third coating layer is a mixture of SP2 and SP3 forms of carbon, and optionally the molar ratio of the SP2 and SP3 forms of carbon is any number in the range of 0.1 to 10, and optionally any number in the range of 2.0 to 3.0.

[0126] In some embodiments, the molar ratio of carbon in the SP2 form to carbon in the SP3 form can be about 0.1, about 0.2, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, or about 10, or can be within any range of any of the above values.

[0127] By selecting the form of carbon in the carbon coating layer, the overall electrochemical performance of the secondary battery is improved. Specifically, by using a mixture of SP2 carbon and SP3 carbon and limiting the ratio of SP2 carbon to SP3 carbon within a certain range, it is possible to effectively avoid a situation in which the conductivity is poor if all the carbon in the coating layer is in the amorphous SP3 form, and the conductivity is good if all the carbon is in the graphitized SP2 form, but there are few lithium ion channels and it does not contribute to lithium ion insertion and desorption. In addition, by limiting the molar ratio of SP2 carbon to SP3 carbon within the above range, it is possible to secure the lithium ion channel while realizing good conductivity, which is advantageous for improving the dynamic performance and cycle performance of the secondary battery.

[0128] The mixture ratio of the SP2 form and the SP3 form of the third coating carbon can be controlled by sintering conditions such as sintering temperature and sintering time. For example, when the third coating layer is produced using sucrose as a carbon source, the sucrose is decomposed at high temperature and then deposited on the second coating layer, and a carbon coating layer having both SP3 and SP2 forms is produced at high temperature. The ratio of the SP2 form carbon and the SP3 form carbon can be controlled by selecting the high-temperature decomposition conditions and the sintering conditions.

[0129] The structure and characteristics of the carbon of the third coating layer can be measured by Raman spectroscopy. The specific test method is to perform peak division on the energy spectrum of the Raman test to obtain the I d / I g (I d is the peak intensity of the SP3 form of carbon, and I g is the peak intensity of SP2 form carbon) and confirm the molar ratio of the two.

[0130] In some embodiments, the coating amount of the first coating layer is greater than 0 and less than 6 wt %, optionally greater than 0 and less than 5.5 wt %, and more optionally greater than 0 and less than 2 wt %, based on the weight of the kernel.

[0131] In some embodiments, the amount of the second coating layer is greater than 0 and less than 6% by weight, optionally greater than 0 and less than 5.5% by weight, and more optionally 2% to 4% by weight, based on the weight of the kernel.

[0132] In some embodiments, the coating amount of the third coating layer is greater than 0 and less than 6 wt %, optionally greater than 0 and less than 5.5 wt %, and more optionally greater than 0 and less than 2 wt %, based on the weight of the kernel.

[0133] In the present application, the coverage of each layer is not zero.

[0134] In the positive electrode active material having a core-shell structure according to the present application, the coating amount of the three coating layers is preferably within the above range, which allows the kernel to be sufficiently coated and further improves the cycle performance, safety performance, and / or rate performance of the secondary battery without sacrificing the gram capacity of the positive electrode active material.

[0135] For the first coating layer, the coating amount is within the above range. If the coating amount is too small, it means that the coating layer is too thin, which may not be able to effectively inhibit the migration of transition metals. If the coating amount is too large, it means that the coating layer is too thick, which may cause Li + This can effectively avoid affecting the movement of the positive electrode active material, and thus affecting the rate performance of the positive electrode active material.

[0136] For the second coating layer, by having the coating amount within the above range, it is possible to effectively avoid the possibility that a coating amount that is too large will affect the plateau voltage of the entire positive electrode active material, and the possibility that a coating amount that is too small will not provide a sufficient coating effect.

[0137] For the third coating layer, the carbon coating mainly plays the role of enhancing the electron transport between particles, but because it contains a lot of amorphous carbon in the structure, the density of carbon is low. Therefore, if the coating amount is too large, it will affect the compression density of the pole sheet.

[0138] In some embodiments, the first coating layer has a thickness of 1 nm to 10 nm.

[0139] In some embodiments, the second coating layer has a thickness of 2 nm to 15 nm.

[0140] In some embodiments, the third coating layer has a thickness of 2 nm to 25 nm.

[0141] In some embodiments, the thickness of the first coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, or about 10 nm, or any range of any of the above values.

[0142] In some embodiments, the thickness of the second coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, or any range of any of the above values.

[0143] In some embodiments, the thickness of the third coating layer may be about 2 nm, about 3 nm, about 4 nm, about 5 nm, about 6 nm, about 7 nm, about 8 nm, about 9 nm, about 10 nm, about 11 nm, about 12 nm, about 13 nm, about 14 nm, about 15 nm, about 16 nm, about 17 nm, about 18 nm, about 19 nm, about 20 nm, about 21 nm, about 22 nm, about 23 nm, about 24 nm, or about 25 nm, or may be within any range of any of the above numerical values.

[0144] When the thickness of the first coating layer is in the range of 1 nm to 10 nm, it is possible to avoid the problem that if the first coating layer is too thick, it will have a negative effect on the dynamic performance of the positive electrode active material, and if the first coating layer is too thin, it will be possible to avoid the problem that the migration of transition metal ions cannot be effectively inhibited.

[0145] When the thickness of the second coating layer is within the range of 2 nm to 15 nm, the surface structure of the second coating layer is stable and the side reaction with the electrolyte is small, thereby effectively reducing the interfacial side reaction and improving the high-temperature cycle performance and high-temperature storage performance of the secondary battery.

[0146] When the thickness of the third coating layer is in the range of 2 nm to 25 nm, the conductivity of the positive electrode active material can be improved, and the compressed density of the positive electrode sheet produced using the positive electrode active material can be improved.

[0147] The thickness of the coating layer is mainly tested by FIB. A specific method includes the steps of randomly selecting a single particle from the powder of the positive electrode active material to be tested, cutting out a slice of about 100 nm thickness from the middle position or near the middle position of the selected particle, performing TEM measurement on the slice, measuring the thickness of the coating layer, measuring 3 to 5 positions, and taking the average value.

[0148] In some embodiments, the content of elemental manganese is in the range of 10 wt % to 35 wt %, optionally in the range of 15 wt % to 30 wt %, and more optionally in the range of 17 wt % to 20 wt %, based on the weight of the positive electrode active material.

[0149] In some embodiments, the content of elemental phosphorus is in the range of 12% to 25% by weight, and optionally in the range of 15% to 20% by weight, based on the weight of the positive electrode active material.

[0150] In some embodiments, the weight ratio of elemental manganese to elemental phosphorus ranges from 0.90 to 1.25, and optionally from 0.95 to 1.20.

[0151] In the present application, when manganese is contained only in the kernel of the positive electrode active material, the manganese content may correspond to the content of the kernel.

[0152] In the present application, the manganese element content is limited within the above range, which can effectively avoid problems such as poor structural stability and reduced density of the positive electrode active material caused by an excessively large manganese element content, thereby improving the cycle, storage, compression density, and other performances of the secondary battery; and can avoid problems such as low voltage platform caused by an excessively small manganese element content, thereby improving the energy density of the secondary battery.

[0153] In the present application, by limiting the content of the phosphorus element within the above range, it is possible to effectively avoid the following problems: if the content of the phosphorus element is too large, the covalent bond of PO is too strong, which may affect the conductivity of small polarons and affect the conductivity of the positive electrode active material; and if the content of the phosphorus element is too small, the stability of the lattice structure of the kernel, the pyrophosphate in the first coating layer, and / or the phosphate in the second coating layer may decrease, which may affect the stability of the entire positive electrode active material.

[0154] The weight ratio of the manganese and phosphorus contents has the following effects on the performance of the secondary battery: if the weight ratio is too large, it means that the manganese element is too much, which increases the elution of manganese ions, affecting the stability and capacity of the positive electrode active material, and further affecting the cycle performance and storage performance of the secondary battery; if the weight ratio is too small, it means that the phosphorus element is too much, which is easy to form impure phases, reducing the discharge voltage platform of the positive electrode active material, and reducing the energy density of the secondary battery.

[0155] The manganese and phosphorus elements can be measured using standard technical means in this technical field. Specifically, the material is dissolved in dilute hydrochloric acid (concentration 10 to 30%), the content of each element in the solution is measured by ICP, and then the manganese element content is measured and converted to obtain the weight ratio, thereby measuring the manganese and phosphorus element contents.

[0156] In some embodiments, the positive electrode active material having a core-shell structure has a lattice change rate before and after complete lithium insertion / extraction of 4% or less, optionally 3.8% or less, and more preferably 2.0% to 3.8%.

[0157] The lithium insertion and extraction process of lithium manganese phosphate (LiMnPO4) is a two-phase reaction. The interfacial stress between the two phases is determined by the magnitude of the lattice change rate before and after lithium insertion and extraction. The smaller the lattice change rate, the smaller the interfacial stress. + Therefore, reducing the lattice change rate of the kernel is + This is advantageous in increasing the transport capacity of lithium and improving the rate performance of secondary batteries. The core-shell structured positive electrode active material according to the present application can reduce the lattice change rate before and after lithium insertion / extraction to 4% or less, thereby improving the rate performance of secondary batteries. The lattice change rate can be measured by a method known in the art, for example, an X-ray diffraction (XRD) pattern.

[0158] In some embodiments, the Li / Mn antistructure defect concentration of the positive electrode active material having a core-shell structure is 4% or less, optionally 2.2% or less, and more preferably 1.5% to 2.2%. The Li / Mn antistructure defect described in the present application refers to a LiMnPO4 crystal lattice in which Li + and Mn 2+ The Li / Mn antistructure defect concentration corresponds to the exchange of the Mn 2+ Li exchanged for + Li + In the present application, the Li / Mn antistructural defect concentration can be measured, for example, in accordance with JIS K0131-1996.

[0159] The positive electrode active material having a core-shell structure according to the present application can achieve the above-mentioned low Li / Mn antistructural defect concentration. Although the mechanism has not been fully elucidated, the inventors of the present application speculate that in the LiMnPO4 crystal lattice, Li + and Mn 2+ The positions of Li are exchanged. +Since the transport channel of Mn is one-dimensional, 2+ Li + It is difficult to move in the channel, + As a result, the positive electrode active material having a core-shell structure according to the present application has a low Li / Mn antistructure defect concentration within the above range, and therefore, Mn 2+ Li + This makes it possible to avoid impeding the transport of the positive electrode active material and improve the capacity and rate performance of the positive electrode active material.

[0160] In some embodiments, the core-shell structured cathode active material has a compressed density of 2.2 g / cm at 3 T. 3 or more, and optionally 2.2 g / cm 3 Above 2.8g / cm 3 The higher the compressed density, the greater the weight per volume of the positive electrode active material, so increasing the compressed density contributes to increasing the volumetric energy density of the secondary battery. The compressed density can be measured according to GB / T24533-2009.

[0161] In some embodiments, the oxygen valence number of the surface of the positive electrode active material having the core-shell structure is -1.90 or less, and optionally -1.90 to -1.98. The stable valence number of oxygen is -2, and the closer the valence number is to -2, the stronger its electron acquisition ability, i.e., the stronger its oxidizing property, and the valence number of the surface is usually -1.7 or less. In the present application, by limiting the surface oxygen valence number of the positive electrode active material within the above range as described above, it is possible to reduce the interfacial side reaction between the positive electrode active material and the electrolyte, and improve the cycle performance and storage performance of the secondary battery. The oxygen valence number of the surface can be measured by a method known in the art, for example, electron energy loss spectroscopy (EELS).

[0162] In some embodiments, the organopolysiloxane compound comprises at least one structural unit represented by Formula 1. [ka] R1 and R2 each independently represent at least one selected from the group consisting of -COOH, -OH, -SH, -CN, -SCN, an amino group, a phosphate ester group, a carboxylate ester group, an amide group, an aldehyde group, a sulfonyl group, a polyether segment, a C1-C20 aliphatic hydrocarbon group, a C1-C20 halogenated aliphatic hydrocarbon group, a C1-C20 heteroaliphatic hydrocarbon group, a C1-C20 halogenated heteroaliphatic hydrocarbon group, a C6-C20 aromatic hydrocarbon group, a C6-C20 halogenated aromatic hydrocarbon group, a C2-C20 heteroaromatic hydrocarbon group, and a C2-C20 halogenated heteroaromatic hydrocarbon group, or H. Alternatively, R1 and R2 each independently represent at least one selected from the group consisting of -COOH, -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, a C2-C8 halogenated alkenyl group, and a phenyl group, or H. More preferably, R1 and R2 each independently represent at least one selected from the group consisting of -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, and a C2-C8 halogenated alkenyl group, or H.

[0163] These functional groups can complex manganese ions and / or react with acidic substances in the electrolyte, thereby reducing the elution of manganese ions and further improving the cycle performance and storage performance of the secondary battery.

[0164] When these functional groups further have electron-withdrawing properties, the Si in the Si-O skeleton of the organopolysiloxane compound can be made more electron-deficient, which can further increase the affinity with F ions in the electrolyte, further mitigate the erosion of the surface of the positive electrode active material by acidic substances in the electrolyte, reduce the elution of manganese ions, and significantly improve the cycle performance and storage performance of the secondary battery.

[0165] In some embodiments, the organopolysiloxane compound includes one or more selected from a polysiloxane having a linear structure and a polysiloxane having a cyclic structure. Optionally, the organopolysiloxane compound is selected from a polysiloxane having a linear structure.

[0166] This further alleviates the erosion of the surface of the positive electrode active material by the acidic substance in the electrolyte, reduces the elution of manganese ions, and significantly improves the cycle performance and storage performance of the secondary battery. Since the electrons in the ring of the cyclic polysiloxane have a certain degree of delocalization, the affinity of the Si-O skeleton for the electron-rich F-containing ions is low compared to the linear polysiloxane, and the removal rate of the F-containing ions in the electrolyte is somewhat low, the effect of reducing the elution of manganese ions is somewhat weak, and the effect of improving the cycle performance of the secondary battery is somewhat low.

[0167] In some embodiments, the linear polysiloxane may further include a blocking group. Optionally, the blocking group includes at least one selected from the group consisting of polyether, C1-C8 alkyl group, C1-C8 halogenated alkyl group, C1-C8 heteroalkyl group, C1-C8 halogenated heteroalkyl group, C2-C8 alkenyl group, C2-C8 halogenated alkenyl group, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy group, C2-C8 epoxy group, hydroxyl group, C1-C8 hydroxyalkyl group, amino group, C1-C8 aminoalkyl group, carboxyl group, and C1-C8 carboxyalkyl group.

[0168] In some embodiments, the molecular formula of the cyclic polysiloxane is represented by Formula 2, where n represents the degree of polymerization of the structural unit represented by Formula 1. Optionally, n≦12, n≦11, n≦10, n≦9, or n≦8. [ka]

[0169] Examples of the linear polysiloxane include polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl-functionalized polysiloxane, polymethylchloropropylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, mercaptopropylpolysiloxane, aminoethylaminopropylpolydimethylsiloxane, methoxy-terminated polydimethylsiloxane, and the like. The linear polysiloxane may include, but is not limited to, one or more of the following: ethyl siloxane, hydroxypropyl terminated polydimethylsiloxane, aminopropyl terminated polydimethylsiloxane, epoxy terminated polysiloxane, hydroxyl terminated polydimethylsiloxane, polyether terminated polydimethylsiloxane, side chain aminopropyl polysiloxane, side chain hydroxylmethyl polysiloxane, side chain hydroxylpropyl polysiloxane, side chain polyether grafted polydimethylsiloxane, side chain phosphate ester grafted polydimethylsiloxane. Optionally, the linear polysiloxane may include one or more of the following: polydimethylsiloxane, polymethylchloropropyl siloxane, polymethyltrifluoropropyl siloxane, mercaptopropyl polysiloxane, aminoethylaminopropyl polydimethylsiloxane, hydroxyl terminated polydimethylsiloxane, polyether grafted polydimethylsiloxane, side chain phosphate ester grafted polydimethylsiloxane.

[0170] For example, the polysiloxane of the cyclic structure includes, but is not limited to, one or more of cyclic polydimethylsiloxane, cyclic polymethylvinylsiloxane, cyclic polymethylhydrogensiloxane, and cyclic polymethyltrifluoropropylsiloxane. Optionally, the polysiloxane of the cyclic structure includes one or more of 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, hexadecamethyloctasiloxane, and tetradecamethylcycloheptasiloxane.

[0171] In some embodiments, the number average molecular weight of the organopolysiloxane compound is 300000 or less, and may be, for example, 400-300000, 400-200000, 400-100000, 400-80000, 400-50000, 400-20000, 400-10000, 1000-100000, 1000-50000, 1000-20000, or 1000-10000. The number average molecular weight of the organopolysiloxane compound can be measured by a method known in the art, for example, gel permeation chromatography (GPC). The measuring instrument can be a PL-GPC220 high temperature gel permeation chromatography. In the present application, the "organopolysiloxane compound" may be an oligomer or a high polymer.

[0172] When the number average molecular weight of the organopolysiloxane compound is within a suitable range, the secondary battery can achieve both good dynamic performance and high temperature storage performance. The following situation can be effectively avoided. If the number average molecular weight of the organopolysiloxane compound is too small, its hydrophobicity may be poor, so that the contact angle between the positive electrode film layer and the electrolyte cannot be effectively increased, and the erosion of the electrolyte on the surface of the positive electrode active material cannot be effectively alleviated, so that the improvement effect of the cycle performance and storage performance of the secondary battery may not be significant. In addition, if the number average molecular weight of the organopolysiloxane compound is too large, its hydrophobicity may be strong, and at the same time, it is also disadvantageous to the dispersion of the slurry, which affects the improvement effect of the performance of the secondary battery.

[0173] In some embodiments, the weight percentage of polar functional groups in the organopolysiloxane compound is α, where 0≦α<50%, alternatively 5%≦α≦30%.

[0174] In this application, the "mass percentage of polar functional groups in the organopolysiloxane compound" refers to the mass ratio of polar functional groups in R1, R2 and blocking groups in the organopolysiloxane compound. In this application, the polar functional groups include one or more of -COOH, -OH, -SH, -CN, -SCN, amino groups (including -NH2, -NH-), phosphate ester groups, carboxylate groups (-COO-), amide groups (-CONH-), aldehyde groups (-CHO), sulfonyl groups (-S(=O)2-), polyether segments, halogen atoms, alkoxy groups, and epoxy groups. When the polar functional groups are directly bonded to silicon atoms, α represents the mass fraction of these polar functional groups in the organopolysiloxane compound. In the case where the polar functional group is not directly linked to the silicon atom, α represents the sum of the mass fractions of the polar functional group and the divalent to tetravalent methyl groups (such as -CH2, -CH-, -C-, etc.) directly linked to it in the organopolysiloxane compound, where the "divalent to tetravalent methyl group" represents the carbon atom directly linked to the polar functional group and located between the polar functional group and the silicon atom, and other non-polar functional groups linked to the carbon atom. Taking polymethyltrifluoropropylsiloxane as an example, α means the mass percentage of -CF3 therein, not including the ethylene group therein. Taking polymethylchloropropylsiloxane as an example, α means the mass percentage of -CH2Cl therein, not including the ethylene group therein. Taking hydroxypropyl-terminated polydimethylsiloxane as an example, α means the mass percentage of -CH2OH. The mass percentage of the polar functional groups in the organopolysiloxane compound can be measured by methods known in the art, for example, titration methods (e.g., acid-alkali titration, oxidation-reduction titration, precipitation titration), infrared spectroscopy, and nuclear magnetic resonance spectroscopy.

[0175] When the content of polar functional groups in the organopolysiloxane compound is within an appropriate range, the effect of reducing the acidity of the electrolyte and removing F ions in the electrolyte is better, which can better mitigate the erosion of the surface of the positive electrode active material by the acidic substances in the electrolyte, and can better improve the cycle performance and storage performance of the secondary battery. In addition, the following situation can be effectively avoided. When the content of polar functional groups in the organopolysiloxane compound is too high, the effect of reducing the acidity of the electrolyte and removing F ions in the electrolyte is not further improved, but the contact angle between the positive electrode film layer and the electrolyte is small, so that the effect of improving the cycle performance of the secondary battery is not significant.

[0176] In some embodiments, the content of the organopolysiloxane compound is 0.01% to 2% by weight, and optionally 0.1% to 2% by weight, based on the total weight of the positive electrode material composition.

[0177] When the content of the organopolysiloxane compound is within an appropriate range, the effect of reducing the acidity of the electrolyte and removing F ions in the electrolyte is better, which can better alleviate the erosion of the surface of the positive electrode active material by the acidic material in the electrolyte, and better improve the cycle performance and storage performance of the secondary battery. In addition, the following situation can be effectively avoided. If the content of the organopolysiloxane compound is too high, it may affect the wettability of the positive electrode film layer to the electrolyte, which may affect the dynamic performance of the secondary battery; and if the content is too high, the energy density of the secondary battery may be reduced because the organopolysiloxane compound does not provide capacity. If the content of the organopolysiloxane compound is too low, the effect of reducing the acidity of the electrolyte and removing F ions in the electrolyte is not obvious, and the erosion of the surface of the positive electrode active material by the acidic material in the electrolyte cannot be effectively alleviated, so the effect of improving the cycle performance and high temperature storage performance of the secondary battery is not obvious.

[0178] In some embodiments, the positive electrode material composition may further include a binder. The binder may be a material having a binding effect known in the art. Optionally, the binder includes at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0179] Alternatively, the content of the binder is 1.79 wt % to 10 wt %, and optionally 2 wt % to 5 wt %, based on the total weight of the positive electrode material composition.

[0180] In some embodiments, the cathode material composition may further include a conductive agent. The conductive agent may be a substance known in the art that has an electron transport effect. Optionally, the cathode conductive agent includes at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Optionally, the content of the conductive agent is 0.2 wt% to 10 wt%, and optionally 0.5 wt% to 5 wt%, based on the total weight of the cathode material composition.

[0181] In some embodiments, the powder resistivity of the positive electrode material composition at 12 MPa is 4Ω / cm to 55Ω / cm, and optionally 4Ω / cm to 40Ω / cm or less. By adjusting the powder resistivity of the positive electrode material composition to a suitable range, the dynamic performance of the secondary battery can be improved. The powder resistivity of the positive electrode material composition can be measured by a method known in the art. For example, it can be tested using a powder resistivity meter with reference to GB / T 30835-2014. An exemplary test method includes weighing a specified amount of powder of a measurement sample and placing it in a special mold, and setting a test pressure to obtain powder resistivities under different pressures. In the present application, the test pressure can be set to 12Mpa. The measurement instrument can be a Suzhou Jingge ST2722-SZ four-probe powder resistivity meter.

[0182] In some embodiments, the specific surface area of ​​the positive electrode material composition is 8 m 2 / g~20m 2 / g, and selectively 8m 2 / g~15m 2 / g. By adjusting the specific surface area of ​​the positive electrode material composition to an appropriate range, it is possible to reduce the interfacial side reaction between the positive electrode sheet using the composition and the electrolyte, and reduce the volume expansion of the secondary battery. This makes it possible to improve the electrochemical performance of the secondary battery. The specific surface area of ​​the positive electrode material composition can be measured by a method known in the art. For example, it can be tested by the nitrogen gas adsorption specific surface area analysis test method with reference to GB / T19587-2017, and calculated by the BET (BrunauerEmmett Teller) method. The nitrogen gas adsorption specific surface area analysis test can be performed using a Tri-Star 3020 type specific surface area pore size analysis tester from Micromeritics, USA. Manufacturing method

[0183] A second aspect of the present application provides a method for producing a positive electrode material composition capable of producing the positive electrode material composition of the first aspect of the present application.

[0184] Specifically, the manufacturing method includes the steps of providing a kernel material, coating and mixing.

[0185] Providing a kernel material, the kernel having a chemical formula of Li 1+x Mn 1-y A y P 1-z R z O4, where x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, and z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg, R is one or more elements selected from B, Si, N, and S, and optionally one element selected from B, Si, N, and S, and the values ​​of x, y, and z satisfy the condition that the entire kernel maintains electrical neutrality.

[0186] The coating steps are Li a MP2O7 and / or M b (P2O7) c and XPO4 suspension, and adding the kernel material to the suspension, mixing and sintering to obtain a positive electrode active material, wherein the positive electrode active material has a core-shell structure, which includes the kernel and a shell covering the kernel, the shell includes a first coating layer covering the kernel, a second coating layer covering the first coating layer and a third coating layer covering the second coating layer, and the first coating layer is a crystalline pyrophosphate Li a MP2O7 and / or M b (P2O7) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP2O7 and M b (P2O7) cM is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb and Al, and the values ​​of a, b and c are each independently one or more elements selected from the group consisting of crystalline pyrophosphate Li a MP2O7 or M b (P2O7) c satisfies the condition of maintaining electrical neutrality, the second coating layer contains crystalline phosphate XPO4, where X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon.

[0187] In the mixing step, the obtained positive electrode active material is uniformly mixed with an organopolysiloxane compound, an optional binder, and an optional conductive agent to obtain a positive electrode material composition.

[0188] In some embodiments, the step of providing the kernel material comprises the following steps (1) and (2).

[0189] In step (1), a manganese source, a dopant of element A, and an acid are mixed and stirred in a container to obtain manganese salt particles doped with element A.

[0190] In step (2), the manganese salt particles doped with element A are mixed with a lithium source, a phosphorus source and a dopant of element R in a solvent to obtain a slurry, which is then sintered under the protection of an inert gas atmosphere to obtain a kernel doped with element A and element R, where the kernel doped with element A and element R is Li 1+x Mn 1-y A y P 1-z R zO4, where x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, and z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg, and R is one or more elements selected from B, Si, N, and S, and optionally one element selected from B, Si, N, and S.

[0191] The manufacturing method of the present application is not particularly limited with respect to the source of the material, and the source of a certain element may include one or more of the element's simple substance, sulfate, halide, nitrate, organic acid salt, oxide, or hydroxide, on the premise that the source can achieve the purpose of the manufacturing method of the present application.

[0192] In some embodiments, the dopant of element A is one or more selected from the group consisting of a simple substance, a carbonate, a sulfate, a chloride, a nitrate, an organic acid salt, an oxide, and a hydroxide of one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge.

[0193] In some embodiments, the dopant of element R is one or more selected from inorganic acids, acid substitutes, organic acids, sulfates, chlorides, nitrates, organic acid salts, oxides, and hydroxides of one or more elements selected from B, Si, N, and S.

[0194] In the present application, the manganese source may be any manganese-containing material known in the art that can be used to prepare lithium manganese phosphate. By way of example, the manganese source may be one or more selected from elemental manganese, manganese dioxide, manganese phosphate, manganese oxalate, and manganese carbonate.

[0195] In the present application, the acid may be one or more selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, organic acids such as silicic acid, silicous acid, and organic acids such as oxalic acid. In some embodiments, the acid is a dilute organic acid having a concentration of 60% by weight or less.

[0196] In the present application, the lithium source may be any lithium-containing material known in the art that can be used to prepare lithium manganese phosphate. For example, the lithium source may be one or more selected from lithium carbonate, lithium hydroxide, lithium phosphate, and lithium dihydrogen phosphate.

[0197] In the present application, the phosphorus source may be any phosphorus-containing material known in the art that can be used to prepare lithium manganese phosphate. For example, the phosphorus source is one or more selected from diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, and phosphoric acid.

[0198] In some embodiments, the manganese source, the element A dopant, and the acid are reacted in a solvent to obtain a manganese salt suspension doped with element A, and the suspension is then filtered, dried, and sand-milled to obtain manganese salt particles doped with element A having a particle size of 50 to 200 nm.

[0199] In some embodiments, the slurry in step (2) is dried to obtain a powder material, and then the powder material is sintered to obtain a kernel doped with element A and element R.

[0200] In some embodiments, the mixing in step (1) is carried out at a temperature of 20°C to 120°C, optionally 40°C to 120°C.

[0201] In some embodiments, in step (1), the stirring is carried out at 400 rpm to 700 rpm for 1 hour to 9 hours, optionally for 3 hours to 7 hours.

[0202] Alternatively, the reaction temperature in step (1) can be about 30° C., about 50° C., about 60° C., about 70° C., about 80° C., about 90° C., about 100° C., about 110° C., or about 120° C. The stirring in step (1) can be performed for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, or about 9 hours. Alternatively, the reaction temperature and stirring time in step (1) can be within any range of any of the above numerical values.

[0203] In some embodiments, the step (2) is performed at a temperature of 20°C to 120°C, and optionally 40°C to 120°C, for 1 hour to 12 hours. Optionally, the reaction temperature in the step (2) can be about 30°C, about 50°C, about 60°C, about 70°C, about 80°C, about 90°C, about 100°C, about 110°C, or about 120°C. The mixing in the step (2) can be performed for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, or about 12 hours. Optionally, the reaction temperature and mixing time in the step (2) can be within any range of any of the above numerical values.

[0204] When the temperature and time during the production process of the kernel particles are within the above ranges, the produced kernel and the positive electrode active material produced therefrom have few lattice defects, which is advantageous in suppressing the dissolution of manganese ions, reducing interfacial side reactions between the positive electrode active material and the electrolyte, and improving the cycle performance and safety performance of the secondary battery.

[0205] In some embodiments, in the process of producing lithium manganese phosphate particles doped with A and R elements, the pH of the solution is selectively controlled to 3.5 to 6, selectively controlled to 4 to 6, and more selectively controlled to 4 to 5. In this application, the pH of the resulting mixture can be adjusted by a method commonly used in this technical field, for example, by adding an acid or a base.

[0206] In some embodiments, optionally, in step (2), the molar ratio of the manganese salt particles doped with element A to the lithium source and the phosphorus source is 1:(0.5-2.1):(0.5-2.1), and more preferably, the molar ratio of the manganese salt particles doped with element A to the lithium source and the phosphorus source is about 1:1:1.

[0207] In some embodiments, the sintering conditions in the process of producing lithium manganese phosphate doped with A and R elements are sintering at 600°C to 950°C for 4 to 10 hours under an inert gas or a mixed atmosphere of inert gas and hydrogen gas. Optionally, the sintering can be performed at about 650°C, about 700°C, about 750°C, about 800°C, about 850°C, or about 900°C for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, the sintering temperature and sintering time can be within any range of the above-mentioned arbitrary values. In the process of preparing lithium manganese phosphate doped with A and R elements, if the sintering temperature is too low and the sintering time is too short, the crystallinity of the kernel of the positive active material will be low, which will affect the overall performance; if the sintering temperature is too high, impurities will easily occur in the kernel of the positive active material, which will affect the overall performance; if the sintering time is too long, the particles of the kernel of the positive active material will be elongated, which will affect the capacity performance, compression density, rate performance, etc.

[0208] In some embodiments, the protective atmosphere is optionally a mixture of 70-90% by volume of nitrogen gas and 10-30% by volume of hydrogen gas.

[0209] In some embodiments, the coating step includes a first coating step, a second coating step, and a third coating step.

[0210] In the first coating step, a source of element M, a phosphorus source and an acid, and an optional lithium source are dissolved in a solvent to obtain a first coating layer suspension, and the kernel obtained in the step of providing a kernel material and the first coating layer suspension obtained in the first coating step are thoroughly mixed, dried, and then sintered to obtain a material coated with a first coating layer.

[0211] In the second coating step, a source of element X, a phosphorus source, and an acid are dissolved in a solvent to obtain a second coating layer suspension, and the material coated with the first coating layer obtained in the first coating step and the second coating layer suspension obtained in the second coating step are thoroughly mixed, dried, and then sintered to obtain a material coated with two coating layers.

[0212] In the third coating step, the carbon source is dissolved in a solvent and sufficiently dissolved to obtain a third coating layer solution, and then the material coated with two coating layers obtained in the second coating step is added to the third coating layer solution, mixed uniformly, dried, and then sintered to obtain a material coated with three coating layers, i.e., a positive electrode active material.

[0213] In some embodiments, the source of element M is one or more selected from the group consisting of simple substances, carbonates, sulfates, chlorides, nitrates, organic acid salts, oxides, and hydroxides of one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al.

[0214] In some embodiments, the source of element X is one or more selected from the group consisting of a simple substance, a carbonate, a sulfate, a chloride, a nitrate, an organic acid salt, an oxide, and a hydroxide of one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al.

[0215] The amount of each of the sources of the elements A, R, M, and X added depends on the target doping amount, and the ratio of the amount of the lithium source, the manganese source, and the phosphorus source used satisfies the stoichiometric ratio.

[0216] By way of example, the carbon source is one or more selected from starch, sucrose, glucose, polyvinyl alcohol, polyethylene glycol, and citric acid.

[0217] In some embodiments, in the first coating step, the pH of the solution in which the source of element M, the phosphorus source, the acid, and the optional lithium source are dissolved is controlled to 3.5 to 6.5, and then the solution is stirred for 1 to 5 hours to react, and then the solution is heated to 50°C to 120°C and maintained at that temperature for 2 to 10 hours. In some embodiments, in the first coating step, sintering is performed at 650°C to 800°C for 2 to 6 hours.

[0218] Optionally, in the first coating step, the reaction is allowed to proceed sufficiently. Optionally, in the first coating step, the reaction is allowed to proceed for about 1.5 hours, about 2 hours, about 3 hours, about 4 hours, about 4.5 hours, or about 5 hours. Optionally, in the first coating step, the reaction time of the reaction can be within any range of any of the above values.

[0219] Optionally, in the first coating step, the pH of the solution is controlled to 4 to 6. Optionally, in the first coating step, the solution is heated to about 55°C, about 60°C, about 70°C, about 80°C, about 90°C, about 100°C, about 110°C, or about 120°C, and held at that temperature for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, in the first coating step, the temperature of the heating and the holding time may be within any range of any of the above numerical values.

[0220] Optionally, in the first coating step, the sintering may be performed at about 650° C., about 700° C., about 750° C., or about 800° C. for about 2 hours, about 3 hours, about 4 hours, about 5 hours, or about 6 hours. Optionally, the sintering temperature and sintering time may be within any range of any of the above values.

[0221] In the first coating step, the sintering temperature and time are controlled within the above ranges. If the sintering temperature is too low and the sintering time is too short, the crystallinity of the first coating layer is low and the amount of amorphous material is large, which reduces the effect of inhibiting the elution of metal, and affects the cycle performance and storage performance of the secondary battery. If the sintering temperature is too high, impurity phases appear in the first coating layer, which also affects the effect of inhibiting the elution of metal, and affects the cycle performance and storage performance of the secondary battery. If the sintering time is too long, the thickness of the first coating layer increases, which increases the Li + This can effectively avoid a situation in which the movement of the positive electrode active material is affected, thereby affecting the capacity exhibited and the rate performance, etc. of the positive electrode active material.

[0222] In some embodiments, in the second coating step, a source of element X, a phosphorus source, and an acid are dissolved in a solvent, and then the solution is reacted by stirring for 1 hour to 10 hours, and then the solution is heated to 60°C to 150°C and maintained at that temperature for 2 hours to 10 hours. In some embodiments, in the second coating step, sintering is performed at 500°C to 700°C for 6 hours to 10 hours.

[0223] Optionally, in the second coating step, the reaction is allowed to proceed sufficiently. Optionally, in the second coating step, the reaction is carried out for about 1.5 hours, about 2 hours, about 3 hours, about 4 hours, about 4.5 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, in the second coating step, the reaction time of the reaction can be within any range of any of the above values.

[0224] Optionally, in the second coating step, the solution is heated to about 65° C., about 70° C., about 80° C., about 90° C., about 100° C., about 110° C., about 120° C., about 130° C., about 140° C., or about 150° C. and held at that temperature for about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, in the second coating step, the elevated temperature and holding time can be within any range of any of the values ​​recited above.

[0225] In the step of providing a kernel material, the first coating step and the second coating step, before sintering, i.e., in the preparation of the kernel material in which chemical reactions occur (step (1) and step (2)), and in the preparation of the first coating layer suspension and the second coating layer suspension, by selecting an appropriate reaction temperature and reaction time as described above, it is possible to effectively avoid the following situations: if the reaction temperature is too low, the reaction cannot occur or the reaction rate is slow; if the temperature is too high, the product will decompose or form impure phases; if the reaction time is too long, the product will have a large particle size, which may increase the time and difficulty of subsequent processes; and if the reaction time is too short, the reaction will be incomplete and little product will be obtained.

[0226] Optionally, in the second coating step, the sintering can be performed at about 550° C., about 600° C., or about 700° C. for about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, the sintering temperature and sintering time can be within any range of any of the above values.

[0227] In the second coating step, the sintering temperature and time are controlled within the above ranges, so that if the sintering temperature is too low and the sintering time is too short in the second coating step, the second coating layer will have low crystallinity and be more amorphous, which will reduce the ability to reduce the surface reaction activity of the positive active material, affecting the cycle performance and storage performance of the secondary battery; if the sintering temperature is too high, impure phases will appear in the second coating layer, which will also affect the effect of reducing the surface reaction activity of the positive active material, affecting the cycle performance and storage performance of the secondary battery; if the sintering time is too long, the thickness of the second coating layer will increase, which will affect the voltage platform of the positive active material, reducing the energy density of the secondary battery, etc., can be effectively avoided.

[0228] In some embodiments, the sintering in the third coating step is performed at 700° C. to 800° C. for 6 hours to 10 hours. Optionally, in the third coating step, the sintering can be performed at about 700° C., about 750° C., or about 800° C. for about 6 hours, about 7 hours, about 8 hours, about 9 hours, or about 10 hours. Optionally, the sintering temperature and sintering time can be within any range of any of the above numerical values.

[0229] In the third coating step, the sintering temperature and time are controlled within the above ranges. If the sintering temperature in the third coating step is too low, the degree of graphitization of the third coating layer is reduced, affecting its electrical conductivity and affecting the capacity of the positive electrode active material; if the sintering temperature is too high, the degree of graphitization of the third coating layer is too high, resulting in the Li + If the sintering time is too short, the coating layer will be too thin, which will affect the electrical conductivity and affect the capacity of the positive active material; if the sintering time is too long, the coating layer will be too thick, which will affect the compression density of the positive active material.

[0230] In the first coating step, the second coating step, and the third coating step, the drying can be carried out at a drying temperature of 100° C. to 200° C., optionally 110° C. to 190° C., more optionally 120° C. to 180° C., further optionally 120° C. to 170° C., and most optionally 120° C. to 160° C. The drying time can be 3 hours to 9 hours, optionally 4 hours to 8 hours, more optionally 5 hours to 7 hours, and most optionally about 6 hours.

[0231] The positive electrode active material produced by the method for producing a positive electrode active material according to the present application has a reduced amount of elution of Mn and doping elements at Mn sites after cycling of the produced secondary battery, and has improved high-temperature storage performance, cycle performance and rate performance, and is also advantageous in industrialization due to its wide supply source of raw materials, low cost and simple process. Positive electrode sheet

[0232] A third aspect of the present application provides a positive electrode sheet comprising a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, the positive electrode film layer comprising the positive electrode material composition of the first aspect of the present application or a positive electrode material composition produced by the method of the second aspect of the present application, and the content of the positive electrode material composition in the positive electrode film layer is 50 wt% or more based on the total weight of the positive electrode film layer. The positive electrode current collector has two surfaces facing each other in the thickness direction, and the positive electrode film layer is provided on the two facing surfaces of the positive electrode current collector.

[0233] In some embodiments, optionally, the content of the positive electrode material composition in the positive electrode membrane layer is 90% by weight to 100% by weight based on the total weight of the positive electrode membrane layer.

[0234] The positive electrode membrane layer does not exclude other components than the positive electrode material composition of the first aspect of the present application or the positive electrode material composition produced by the method of the second aspect of the present application. For example, the positive electrode membrane layer may further include other positive electrode active materials other than the positive electrode active material coated with the above three layers of the present application. Optionally, the other positive electrode active materials may include at least one of lithium transition metal oxides and their modified compounds. For example, the other positive electrode active materials may include at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds.

[0235] In some embodiments, the positive electrode current collector can be a metal foil or a composite current collector. An example of the metal foil can be aluminum foil. The composite current collector can include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material can be at least one selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer can be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), and the like.

[0236] In some embodiments, the solid-liquid contact angle between the positive electrode film layer and the non-aqueous organic solvent is 3° to 90°, optionally 3° to 60°, or even 10° to 30°. When the contact angle is within a suitable range, the secondary battery can achieve both high energy density and improved cycle performance, safety performance, and / or rate performance. In addition, the following situations can be effectively avoided. If the contact angle is too small, the erosion of the surface of the positive electrode active material by the acidic substance in the electrolyte cannot be effectively alleviated, and the effect of improving the cycle performance may not be clear. If the contact angle is too large, the wettability of the positive electrode film layer to the electrolyte may be poor, which may affect the rate performance and cycle performance of the secondary battery. The solid-liquid contact angle between the positive electrode film layer and the non-aqueous organic solvent is a meaning known in the art, and can be tested using a method known in the art. For example, it can be measured with reference to GBT 30693-2014. One exemplary test method includes dropping a droplet of a non-aqueous organic solvent onto the surface of the positive electrode sheet at room temperature and measuring the contact angle for 60 seconds using a contact angle measuring device. The test equipment may be an LSA 200-type optical contact angle measuring device manufactured by LAUDA Scientific, Germany. As the non-aqueous organic solvent, any non-aqueous organic solvent known in the art that is used in non-aqueous electrolytes of secondary batteries may be used. Optionally, the non-aqueous organic solvent may be ethylene carbonate (EC).

[0237] In some embodiments, the porosity of the positive electrode film layer is 15% to 50%, and optionally 15% to 30%. When the porosity is within an appropriate range, the secondary battery can achieve both high energy density and improved cycle performance, safety performance, and / or rate performance. In addition, the following situations can be effectively avoided. If the porosity is too small, the wettability of the positive electrode film layer to the electrolyte may be poor, which may affect the rate performance and cycle performance of the secondary battery, and if the porosity is too large, it may affect the energy density of the entire secondary battery. The porosity of the positive electrode film layer has a meaning known in the art and can be measured by a method known in the art. For example, it can be measured by referring to GB / T 24586-2009 after peeling off the positive electrode film layer with an adhesive tape. The porosity P=[(V2-V1) / V2]×100%. V1(cm 3 ) represents the true volume and can be measured by combining Archimedes' principle and Bohr's law using a substitution method with an inert gas (e.g., helium gas) having a small molecular diameter. V2 (cm 3 ) represents the apparent volume, V2 = S × H × A, S (cm 2 ) represents the area, H (cm) represents the thickness, and A represents the number of samples.

[0238] In some embodiments, the resistance of the positive electrode film layer is greater than 0 and less than or equal to 6Ω. This allows the positive electrode sheet to have good conductive ability, so that the secondary battery can have better dynamic performance. The resistance of the positive electrode film layer can be tested using a method known in the art, for example, using a pole piece resistor. As an exemplary measurement method, a positive electrode sheet coated on one side and cold pressed (if the positive electrode sheet is coated on both sides, the positive electrode film layer can be wiped off on one side first) is placed parallel between two conductive terminals of a pole sheet resistor, and a certain pressure is applied to fix it, that is, the resistance of the positive electrode film layer is obtained. Optionally, the diameter of the conductive terminal can be 14mm, the applied pressure can be 15-27Mpa, and the time range of the adopted point can be 10-20s. The test equipment can adopt IEST BER1000 type pole piece resistor, which is from Yuan Neng Science and Technology Co., Ltd.

[0239] In some embodiments, the adhesive strength between the positive electrode film layer and the positive electrode current collector is 0.5 MPa or more. In this range, the occurrence of powder falling phenomenon of the positive electrode sheet can be prevented, which is advantageous for exerting secondary battery performance. The adhesive strength between the positive electrode film layer and the positive electrode current collector has a meaning well known in the art, and can be tested using a method well known in the art. As an exemplary test method, the positive electrode sheet is cut into a test sample having a length of 100 mm and a width of 10 mm, a stainless steel plate having a width of 25 mm is taken, and a double-sided tape (e.g., a width of 11 mm) is attached to the test sample, and the test sample is attached to the double-sided tape of the stainless steel plate, and the surface is reciprocated three times with a 2000 g press roll (e.g., roll press speed 300 mm / min), the test sample is bent 180°, and the positive electrode film layer and the positive electrode current collector of the test sample are manually peeled off by 25 mm, the test sample is fixed to a test machine (e.g., INSTRON336), the peeling surface is aligned with the force line of the test machine, and the test machine is continuously peeled off at 30 mm / min, and the peel force curve obtained by gentle peeling is the average value of the pieces as the peel force F0, and the adhesive force between the positive electrode film layer and the positive electrode current collector = F0 / width of the test sample.

[0240] In some embodiments, the surface density of the positive electrode membrane layer is 0.006 g / cm 2 ~0.065g / cm 2 This is advantageous for improving the volumetric energy density of the secondary battery. The areal density of the positive electrode film layer has a meaning well known in the art, and can be tested using a method well known in the art. As an exemplary test method, a positive electrode sheet coated on one side and cold pressed (if the positive electrode sheet is coated on both sides, the positive electrode film layer on one side can be wiped off first) is punched into a wafer with a small area of ​​S1, and its weight is recorded as M1, and then the positive electrode film layer of the weighed positive electrode sheet is wiped off, and the weight of the positive electrode current collector is weighed and recorded as M0, and the areal density of the positive electrode film layer=(M1-M0) / S1.

[0241] In some embodiments, the positive electrode membrane layer has an absorbing rate of the electrolyte of 0.0125 μg / s to 100 μg / s, and optionally 0.5 μg / s to 40 μg / s, which ensures that the electrolyte has good wettability in the electrode assembly, and allows it to quickly enter the inside of the electrode assembly, and promptly form an SEI film on the surface of the positive electrode sheet, thereby improving the electrochemical performance of the secondary battery.

[0242] The positive electrode membrane layer is usually formed by applying a positive electrode slurry to a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is usually formed by dispersing a positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).

[0243] In addition, the parameters of each positive electrode film layer provided in this application (e.g., contact angle, porosity, resistance, adhesive strength, surface density, electrolyte absorption rate, etc.) all refer to the parameters of the positive electrode film layer on one side of the positive electrode current collector. When positive electrode film layers are provided on both sides of the positive electrode current collector, if the parameters of either one of the positive electrode film layers satisfy the parameters of this application, it is considered to be within the protection scope of this application.

[0244] The testing of each parameter of the positive electrode film layer may be performed by sampling during the manufacturing process of the positive electrode sheet or the battery, or by sampling from the manufactured battery.

[0245] When the test sample is sampled from the manufactured battery, for example, the battery is discharged (for safety reasons, the battery is generally fully discharged); the battery is disassembled, the positive electrode sheet is removed, and the positive electrode sheet is immersed in dimethyl carbonate (DMC) for a certain time (e.g., 2 hours to 10 hours), and then the positive electrode sheet is removed and dried at a certain temperature and time (e.g., 60°C, 4 hours). After drying, the positive electrode sheet is removed, and the parameters related to the positive electrode film layer of the present application can be sampled and tested from the dried positive electrode sheet. secondary battery

[0246] A fourth aspect of the present application provides a secondary battery including the positive electrode sheet of the third aspect of the present application.

[0247] A secondary battery, also called a rechargeable battery or storage battery, is a battery that can continue to be used by activating the active material by charging after discharging the battery. Typically, a secondary battery includes an electrode assembly and an electrolyte, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent short-circuiting between the positive and negative electrodes, while allowing active ions to pass through. The electrolyte serves to transport active ions between the positive electrode sheet and the negative electrode sheet. [Positive electrode sheet]

[0248] The positive electrode sheet used in the secondary battery of the present application is the positive electrode sheet described in any of the Examples of the third aspect of the present application. [Negative electrode sheet]

[0249] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces facing each other in a thickness direction, and the negative electrode film layer is provided on the two facing surfaces of the negative electrode current collector.

[0250] The negative electrode active material may be a negative electrode active material for secondary batteries known in the art. For example, the negative electrode active material may include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate, but is not limited thereto. The silicon-based material may include at least one of elemental silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy material. The tin-based material may include at least one of elemental tin, tin oxide, and tin alloy material. The present application is not limited to these materials, and other materials known in the art that are used as negative electrode active materials for secondary batteries may be used. These negative electrode active materials may be used alone or in combination of two or more.

[0251] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. In the present application, the type of the negative electrode conductive agent is not particularly limited. For example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0252] In some embodiments, the negative electrode membrane layer may optionally further include a negative electrode binder. In the present application, the type of the negative electrode binder is not particularly limited. For example, the negative electrode binder may include at least one of styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0253] In some embodiments, the negative electrode membrane layer may optionally further include other auxiliary agents. For example, the other auxiliary agents may include a thickener such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, etc.

[0254] In some embodiments, the negative electrode current collector can be a metal foil or a composite current collector. An example of the metal foil can be copper foil. The composite current collector can include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material can be at least one selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer can be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), and the like.

[0255] The negative electrode film layer is typically formed by applying a negative electrode slurry to a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing a negative electrode active material, an optional conductive agent, an optional binder, and other optional auxiliary agents in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0256] The negative electrode sheet does not exclude additional functional layers other than the negative electrode film layer. For example, in some embodiments, the negative electrode sheet according to the present application further includes a conductive primer layer (e.g., made of a conductive agent and a binder) sandwiched between the negative electrode collector and the negative electrode film layer and provided on the surface of the negative electrode collector. In some other embodiments, the negative electrode sheet described in the present application further includes a protective layer covering the surface of the negative electrode film layer. [Electrolyte]

[0257] In the present application, the type of the electrolyte is not particularly limited and can be selected according to requirements. For example, the electrolyte may be at least one selected from a solid electrolyte and a liquid electrolyte (electrolytic solution).

[0258] In some embodiments, the electrolyte uses an electrolyte solution, the electrolyte solution including an electrolyte salt and a solvent.

[0259] The type of the electrolyte salt is not particularly limited and can be selected according to actual requirements.In some embodiments, as an example, the electrolyte salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium disoxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodisoxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0260] The type of the solvent is not particularly limited and can be selected according to actual requirements. In some embodiments, by way of example, the solvent may include at least one of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0261] In some embodiments, the electrolyte may further include an additive. For example, the additive may include an anode film-forming additive, a cathode film-forming additive, or an additive that can improve a part of the performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high-temperature performance of the battery, or an additive that improves the low-temperature power performance of the battery. [Separator]

[0262] In secondary batteries using an electrolyte or solid electrolyte, a separator is also included. The separator is provided between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent short circuiting of the positive and negative electrodes, while allowing active ions to pass through. In the present application, the type of the separator is not particularly limited, and any known porous structure separator having good chemical stability and mechanical stability can be selected.

[0263] In some embodiments, the separator may be made of at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a monolayer film or a multilayer composite film. When the separator is a multilayer composite film, the materials of the layers may be the same or different.

[0264] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly by a rolling process or a lamination process.

[0265] In some embodiments, the secondary battery may include an exterior case that is used to seal the electrode assembly and electrolyte described above.

[0266] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, or a steel case. The exterior of the secondary battery may be a soft bag, such as a bag soft bag. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0267] In the present application, the shape of the secondary battery is not particularly limited, and may be cylindrical, rectangular, or any other shape. Fig. 1 shows a secondary battery 5 having a rectangular structure as an example.

[0268] In some embodiments, as shown in FIG. 2, the exterior may include a case 51 and a cover plate 53. The case 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are surrounded to form a chamber. The case 51 has an opening communicating with the chamber, and the cover plate 53 covers the opening to seal the chamber. The positive electrode sheet, the negative electrode sheet and the separator can form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the chamber. The electrolyte is permeated into the electrode assembly 52. ​​The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to requirements.

[0269] The method for manufacturing the secondary battery of the present application is known. In some embodiments, a secondary battery can be formed by assembling a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte. For example, a positive electrode sheet, a separator, and a negative electrode sheet can be formed into an electrode assembly by a winding process or a lamination process, and the electrode assembly can be placed in an outer casing, dried, and then an electrolyte can be injected, and a secondary battery can be obtained through processes such as vacuum sealing, standing, chemical formation, and shaping.

[0270] In some embodiments of the present application, the secondary battery of the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.

[0271] Fig. 3 is a schematic diagram of an example battery module 4. As shown in Fig. 3, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by a fastener.

[0272] Optionally, the battery module 4 further includes a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.

[0273] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0274] 4 and 5 are schematic diagrams of an example battery pack 1. As shown in Fig. 4 and 5, the battery pack 1 may include a battery housing and a plurality of battery modules 4 provided in the battery housing. The battery housing includes an upper housing 2 and a lower housing 3, and the upper housing 2 covers the lower housing 3 to form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery housing in any manner. power consumption equipment

[0275] A fifth aspect of the present application provides a power consuming device including at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack may be used as a power source for the power consuming device, or may be used as an energy storage means for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, and a satellite, an energy storage system, etc.

[0276] The power consumption device can select a secondary battery, a battery module or a battery pack according to the demand.

[0277] 6 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the power consuming device, a battery pack or a battery module can be adopted.

[0278] Another example of the power consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. This power consuming device is usually required to be thin and may employ a secondary battery as a power source. Working Example

[0279] The following examples are provided to more specifically describe the contents of the present application, but these examples are merely illustrative, and it will be apparent to those skilled in the art that various modifications and changes may be made within the scope of the disclosure of the present application. All parts, percentages, and ratios described in the following examples are based on mass unless otherwise specified. In addition, all reagents used in the examples are commercially available or may be synthesized according to conventional methods, and can be used as is without further treatment. In addition, all devices used in the examples are commercially available.

[0280] The raw materials for the examples of this application are as follows:

[0281] [Table 1] I. Battery Construction Example 1 Step 1: Manufacture of cathode active material Step S1: Preparation of Fe, Co, V and S co-doped manganese oxalate

[0282] 689.6g of manganese carbonate, 455.27g of ferrous carbonate, 4.65g of cobalt sulfate, and 4.87g of vanadium dichloride were mixed thoroughly in a mixer for 6 hours. The mixture was then transferred to a reaction vessel, and 5L of deionized water and 1260.6g of oxalic acid dihydrate were added, heated to 80°C, and thoroughly stirred at a rotation speed of 500 rpm for 6 hours, and mixed uniformly until the end of the reaction, to obtain a manganese oxalate suspension co-doped with Fe, Co, and V. The suspension was then filtered, dried at 120°C, and further subjected to a sand mill to obtain manganese oxalate particles with a particle size of 100 nm. Step S2: Kernel Li 0.997 Mn 0.60Fe 0.393 V 0.004 Co 0.003 P 0.997 S 0.003 O4 Production

[0283] 1793.1g of manganese oxalate produced in (1), 368.3g of lithium carbonate, 1146.6g of ammonium dihydrogen phosphate, and 4.9g of dilute sulfuric acid were added to 20L of deionized water, thoroughly stirred, and reacted uniformly at 80°C for 10 hours to obtain a slurry. The slurry was transferred to a spray dryer, spray-dried and granulated, and dried at a temperature of 250°C to obtain a powder. The powder was sintered in a roller hearth kiln at 700°C for 4 hours in a protective atmosphere (90% nitrogen gas and 10% hydrogen gas) to obtain the above kernel material. Step S3: Preparation of first coating layer suspension

[0284] A Li2FeP2O7 solution was prepared by dissolving 7.4 g of lithium carbonate, 11.6 g of ferrous carbonate, 23.0 g of ammonium dihydrogen phosphate, and 12.6 g of oxalic acid dihydrate in 500 mL of deionized water, adjusting the pH to 5, and reacting the solution at room temperature with stirring for 2 hours to obtain a solution. The solution was then heated to 80°C and maintained at this temperature for 4 hours to obtain a first coating layer suspension. Step S4: Coating the first coating layer

[0285] 1571.9 g of the doped lithium manganese phosphate kernel material obtained in step S2 was added to the first coating layer suspension obtained in step S3 (containing 15.7 g of coating material), and thoroughly stirred and mixed for 6 hours to achieve uniform mixing. The mixture was then transferred to a 120°C oven for drying for 6 hours, and then sintered at 650°C for 6 hours to obtain a pyrophosphate-coated material. Step S5: Preparation of second coating layer suspension

[0286] 3.7 g of lithium carbonate, 11.6 g of ferrous carbonate, 11.5 g of ammonium dihydrogen phosphate, and 12.6 g of oxalic acid dihydrate were dissolved in 1500 mL of deionized water, and the mixture was reacted with stirring for 6 hours to obtain a solution. The solution was then heated to 120°C and maintained at this temperature for 6 hours to obtain a second coating layer suspension. Step S6: Coating the second coating layer

[0287] 1586.8 g of the pyrophosphate-coated material obtained in step S4 was added to the second coating layer suspension obtained in step S5 (with a coating material content of 47.1 g), and mixed thoroughly for 6 hours to achieve uniform mixing, then transferred to an oven at 120°C for drying for 6 hours, and then sintered at 700°C for 8 hours to obtain a two-layer coated material. Step S7: Preparation of the third coating layer aqueous solution

[0288] 37.3 g of sucrose was dissolved in 500 g of deionized water, and then stirred to thoroughly dissolve the solution, to obtain an aqueous sucrose solution. Step S8: Coating the third coating layer

[0289] 1633.9 g of the two-layer coated material obtained in step S6 was added to the sucrose solution obtained in step S7, and the mixture was stirred for 6 hours to be homogeneously mixed. The mixture was then transferred to an oven at 150°C for drying for 6 hours, and then sintered at 700°C for 10 hours to obtain a three-layer coated material, i.e., a positive electrode active material. Step 2: Manufacturing the positive electrode sheet

[0290] The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (with polar functional groups -CH2NH2 and -CH2NH-, mass percentage α of about 12%, and number average molecular weight of 3700) were mixed in a weight ratio of 93.4:1.5:4.5:0.6 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Next, the positive electrode material composition was added to N-methylpyrrolidone (NMP), and the mixture was stirred and mixed uniformly to obtain a positive electrode slurry. Next, the positive electrode slurry was applied to a coating surface density of 0.018 g / cm 2The mixture was uniformly applied to an aluminum foil, which was then dried, cold pressed, and slit to obtain a positive electrode sheet. Step 3: Manufacturing the negative electrode sheet

[0291] The negative electrode active material artificial graphite, hard carbon, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were dissolved in deionized water as a solvent in a weight ratio of 90:5:2:2:1, and mixed uniformly with stirring to prepare a negative electrode slurry. The negative electrode slurry was applied with a surface density of 0.0075 g / cm. 2 The mixture was uniformly applied to a negative electrode current collector copper foil, which was then dried, cold pressed, and slit to obtain a negative electrode sheet. Step 4: Making the electrolyte

[0292] In a glove box (H2O<0.1ppm, O2<0.1ppm) with an argon gas atmosphere, the organic solvents ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3 / 7, and 12.5 wt% (based on the weight of the ethylene carbonate / ethyl methyl carbonate solvent) LiPF6 was added and dissolved in the organic solvent, and stirred uniformly to obtain an electrolyte solution. Step 5: Making the separator

[0293] A commercially available microporous film of PP-PE copolymer with a thickness of 20 μm and an average pore size of 80 nm was used (manufactured by Zhuo Electronics Science and Technology Co., Ltd., model number 20). Step 6: Building the entire battery

[0294] The positive electrode sheet, separator, and negative electrode sheet obtained above are stacked in order, the separator is placed between the positive and negative electrodes to serve as an insulator, and the stack is wound to obtain an electrode assembly. The electrode assembly is placed in an outer casing, and the electrolyte is injected and sealed to obtain a full cell (hereinafter also referred to as "full cell"). [Coin cell manufacturing]

[0295] The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropyl polydimethylsiloxane (polar functional groups are -CH2NH2 and -CH2NH-, mass percentage α is about 12%, and number average molecular weight is 3700) were mixed in a weight ratio of 89.4:5:5:0.6 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition, which was then added to N-methylpyrrolidone (NMP) and stirred in a drying chamber to prepare a slurry. The slurry was applied to aluminum foil, dried, and cold pressed to prepare a positive electrode sheet. The coating surface density was 0.015 g / cm 2 and the compressed density is 2.0 g / cm 3 It was.

[0296] A lithium sheet was used as the negative electrode, and a solution of 1 mol / L LiPF6 in ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1 was used as the electrolyte. A coin cell (hereinafter also referred to as "coin cell") was assembled in an electric buckle box together with the positive electrode sheet prepared above. Examples 2 to 29

[0297] Positive electrode active materials of Examples 2 to 29 were produced in a manner similar to that of Example 1, but differences in the production of the positive electrode active materials are shown in Tables 2 to 7. The other steps were the same as those of Example 1. Examples 30 to 42

[0298] Positive electrode active materials of Examples 30 to 42 were produced in a manner similar to that of Example 1. See Tables 8 and 9 for differences in the production of the positive electrode active materials. The other steps were the same as those of Example 1. Examples 43 to 47

[0299] In the preparation of the full cell and the coin cell, except that the weight percentage of aminoethylaminopropylpolydimethylsiloxane in the positive electrode material composition was adjusted, the other processes were the same as those in Example 1. See Table 10 for the differences. Example 43

[0300] Preparation of full cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 93.99:1.5:4.5:0.01 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition.

[0301] Manufacturing of coin cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (polar functional groups are -CH2NH2 and -CH2NH-, mass percentage α is about 12%, and number average molecular weight is 3700) were mixed in a weight ratio of 89.99:5:5:0.01 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Example 44

[0302] Preparation of full cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and alkylaminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 93.9:1.5:4.5:0.1 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition.

[0303] Manufacturing of coin cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (polar functional groups are -CH2NH2 and -CH2NH-, mass percentage α is about 12%, and number average molecular weight is 3700) were mixed in a weight ratio of 89.9:5:5:0.1 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Example 45

[0304] Preparation of full cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 93:1.5:4.5:1 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition.

[0305] Manufacturing of coin cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 89:5:5:1 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Example 46

[0306] Preparation of full cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 92:1.5:4.5:2 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition.

[0307] Manufacturing of coin cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (polar functional groups are -CH2NH2 and -CH2NH-, mass percentage α is about 12%, and number average molecular weight is 3700) were mixed in a weight ratio of 88:5:5:2 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Example 47

[0308] Preparation of full cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (having polar functional groups -CH2NH2 and -CH2NH-, a mass percentage α of about 12%, and a number average molecular weight of 3700) were mixed in a weight ratio of 89:1.5:4.5:5 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition.

[0309] Manufacturing of coin cell: The positive electrode active material, acetylene black as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and aminoethylaminopropylpolydimethylsiloxane (polar functional groups are -CH2NH2 and -CH2NH-, mass percentage α is about 12%, and number average molecular weight is 3700) were mixed in a weight ratio of 85:5:5:5 with a stirrer until the materials were uniformly mixed to obtain a positive electrode material composition. Examples 48 to 65

[0310] In the manufacture of the full cell and the coin cell, the aminoethylaminopropylpolydimethylsiloxane in the positive electrode material composition was replaced with the following organopolysiloxane compounds, respectively, and the other conditions were the same as those in the process of Example 1. See Table 10 for differences.

[0311] Example 48: Polydimethylsiloxane (polar functional group content α is about 0%, number average molecular weight is 1200).

[0312] Example 49: Polymethylchloropropylsiloxane (polar functional group is -CH2Cl, mass percentage α is approximately 30.2%, number average molecular weight is 2500).

[0313] Example 50: Polymethyltrifluoropropylsiloxane (polar functional group is -CF3, mass percentage α is approximately 44.0%, number average molecular weight is 1400).

[0314] Example 51: Mercaptopropylpolysiloxane (polar functional group is -CH2SH, mass percentage α is about 15.0%, number average molecular weight is 2000).

[0315] Example 52: Hydroxy-terminated polydimethylsiloxane (polar functional group is -OH, mass percentage α is about 3.4%, number average molecular weight is 1000).

[0316] Example 53: Methoxy-terminated polydimethylsiloxane (polar functional group is a methoxy group, mass percentage α is about 3.1%, number average molecular weight is 2800).

[0317] Example 54: Polyether-terminated polydimethylsiloxane (polar functional group is a polyether segment, mass percentage α is approximately 10.0%, and number average molecular weight is 2110).

[0318] Example 55: Side chain phosphate ester grafted polydimethylsiloxane (polar functional group is a phosphate ester group, mass percentage α is about 1.4%, number average molecular weight is 15600),

[0319] Example 56: 1,3,5,7-Octamethylcyclotetrasiloxane (content α of polar functional groups is about 0%, molecular weight 280).

[0320] Example 57: Cyclopentadimethylsiloxane (mass percentage α of polar functional groups is about 0%, molecular weight is 370).

[0321] Example 58: Polyether-terminated polydimethylsiloxane (polar functional group is a polyether segment, mass percentage α is approximately 55.0%, number average molecular weight is 25132).

[0322] Example 59: Polydimethylsiloxane (polar functional group content α is about 0%, number average molecular weight is 400).

[0323] Example 60: Polydimethylsiloxane (polar functional group content α is about 0%, number average molecular weight is 10,000).

[0324] Example 61: Polydimethylsiloxane (content α of polar functional groups is about 0%, number average molecular weight is 50,000).

[0325] Example 62: Polydimethylsiloxane (content α of polar functional groups is about 0%, number average molecular weight is 80,000).

[0326] Example 63: Polydimethylsiloxane (content α of polar functional groups is about 0%, number average molecular weight is 100,000).

[0327] Example 64: Polydimethylsiloxane (polar functional group content α is about 0%, number average molecular weight is 300,000).

[0328] Example 65: Polydimethylsiloxane (content α of polar functional groups is about 0%, number average molecular weight is 400,000). Comparative Example 1 to Comparative Example 18

[0329] Positive electrode active materials of Comparative Examples 1 to 18 were manufactured similarly to Example 1, and differences in the manufacture of the positive electrode active materials are shown in Tables 2 to 7. Comparative Examples 1 to 2, 4 to 10, and 12 are not coated with a first coating layer, so steps S3 and S4 are omitted, and Comparative Examples 1 to 11 are not coated with a second coating layer, so steps S5 and S6 are omitted.

[0330] Full cells and coin cells of Comparative Examples 1 to 18 were manufactured in a manner similar to that of Example 1, and the other conditions were the same as those of Example 1, except that aminoethylaminopropylpolydimethylsiloxane was not added to the positive electrode material composition.

[0331] Also, in all examples and comparative examples in this application, unless otherwise specified, it is the default that any first coating layer material and / or second coating layer material used is crystalline.

[0332] Raw materials for the manufacture of kernels [Table 2A] [Table 2B] [Table 2C]

[0333] Preparation of the first coating layer suspension (step S3) [Table 3]

[0334] Coating of the first coating layer (step S4) [Table 4]

[0335] Preparation of second coating layer suspension (step S5) [Table 5]

[0336] Coating of the second coating layer (step S6) [Table 6A] [Table 6B]

[0337] Coating of the third coating layer (step S8) [Table 7A] [Table 7B]

[0338] Consideration of the first coating layer material [Table 8]

[0339] Consideration of the second coating layer material [Table 9]

[0340] Considerations for organopolysiloxane compounds [Table 10] II. Performance Evaluation 1.Method of measuring lattice change rate

[0341] In a constant temperature environment of 25°C, place the positive electrode active material sample in an X-ray powder diffractometer (model number: Bruker D8 Discover), measure the sample at 1° / min, organize and analyze the measurement data, and refer to the standard PDF card to calculate the lattice constants a0, b0, c0, and v0 at this time (a0, b0, and c0 represent the length magnitude in each direction of the unit lattice, v0 represents the volume of the unit lattice, which can be obtained directly from the XRD precision correction result).

[0342] The positive electrode active material sample was manufactured into a coin battery by the manufacturing method of the coin battery in the above example, and the coin battery was charged at a low rate of 0.05C until the current decreased to 0.01C. Then, the positive electrode sheet in the coin battery was taken out and immersed in dimethyl carbonate (DMC) for 8 hours. Then, it was dried, the powder was scraped off, and particles with a particle size of less than 500 nm were selected. The sample was sampled and its unit lattice volume v1 was calculated in the same manner as the fresh sample in the above test, and (v0-v1) / v0×100% is shown in the table as the lattice change rate (lattice volume change rate) before and after the lithium was completely inserted and extracted. 2. Li / Mn antistructural defect concentration

[0343] The XRD results measured by the "method for measuring the lattice change rate" are compared with the PDF (Powder Diffraction File) card of a standard crystal to obtain the Li / Mn antistructure defect concentration. Specifically, the XRD results measured by the "method for measuring the lattice change rate" are introduced into the General-purpose Structure Analysis System (GSAS) software to automatically obtain the refined correction results including the site occupancy status of different atoms, and the Li / Mn antistructure defect concentration is obtained by reading the refined correction results. 3. Surface oxygen valence

[0344] A coin battery was manufactured from 5 g of the above-produced positive electrode active material sample according to the manufacturing method of the coin battery described in the above example. The coin battery was charged at a small rate of 0.05 C until the current decreased to 0.01 C. The positive electrode sheet in the coin battery was then removed and immersed in DMC for 8 hours. It was then dried, the powder was scraped off, and particles with a particle size smaller than 500 nm were selected. The obtained particles were measured by electron energy loss spectroscopy (EELS, equipment model number Talos F200S used) to obtain the energy loss spectrum fine structure (ELNES) reflecting the state density and energy level distribution of the elements. From the state density and energy level distribution, the number of electrons occupied was calculated by integrating the state density data of the valence band, and the oxygen valence number of the surface after charging was estimated. 4.Compressed density

[0345] 5 g of the positive electrode active material powder produced above was placed in a compression mold (CARVER mold, model number 13 mm, USA), and then the mold was placed on a compression density measuring device. A pressure of 3 T (tons) was applied, and the thickness of the powder under pressure (thickness after pressure release, the area of ​​the container used for the test was 1540.25 mm 2 ) was read on the equipment, and the compressed density was calculated using the formula ρ = m / v. 5. Powder resistivity test

[0346] The sample powder of the positive electrode material composition for making an appropriate amount of full cells is placed in the special mold of the powder resistivity tester, and the test pressure is set, so that the powder resistivity at different pressures can be obtained. In this application, the test pressure is 12Mpa. The measuring instrument is a Suzhou Jingge ST2722-SZ type four-probe powder resistivity tester. 6.Specific surface area test

[0347] 5 g of sample powder of the positive electrode material composition for producing a full cell was taken, and the specific surface area was tested using a Tri-Star 3020 specific surface area pore size analyzer manufactured by Micromeritics, Inc., USA. The specific surface area was calculated by the BET (Brunauer Emmett Teller) method. 7. Contact angle test

[0348] A droplet of ethylene carbonate (EC) was dropped onto the surface of the positive electrode film layer at room temperature, and the solid-liquid contact angle was measured within 60 seconds using an LSA 200 optical contact angle measuring instrument manufactured by LAUDA Scientific, Germany. 8. How to measure the initial gram capacity of a coin cell

[0349] The coin cells manufactured in each of the above examples and comparative examples were charged to 4.3 V at 0.1 C, then charged at a constant voltage of 4.3 V until the current was 0.05 mA or less, left to stand for 5 minutes, and then discharged to 2.0 V at 0.1 C. The discharge capacity at this time is the initial gram capacity and is denoted as D0. 9.3C charging constant current ratio

[0350] In a constant temperature environment of 25°C, the new full cells manufactured in each of the above examples and comparative examples were left to stand for 5 minutes and discharged at 1 / 3C to 2.5V. After leaving it to stand for 5 minutes, it was charged to 4.3V at 1 / 3C, and then charged at a constant voltage of 4.3V until the current was 0.05mA or less. The charge capacity when left to stand for 5 minutes was recorded as C0. It was discharged to 2.5V at 1 / 3C, left to stand for 5 minutes, and further charged to 4.3V at 3C, and the charge capacity when left to stand for 5 minutes was recorded as C1. The constant current ratio of 3C charging is C1 / C0 x 100%. The higher the constant current ratio of 3C charging, the better the rate performance of the secondary battery. 10. Testing the swelling of batteries stored at 60℃ for 30 days

[0351] The full cells manufactured in each of the above examples and comparative examples at 100% state of charge (SOC) were stored at 60°C. Before, during and after storage, the open circuit voltage (OCV) and alternating current internal resistance (IMP) of the battery were measured to monitor the SOC, and the volume of the battery was measured. Every 48 hours, the full cells were taken out and left to stand for 1 hour, after which the open circuit voltage (OCV) and internal resistance (IMP) were measured. After cooling to room temperature, the battery volume was measured using the drainage method. In the drainage method, the gravity F1 of the battery was measured independently using a balance that automatically performs unit conversion using dial data, and then the battery was completely immersed in deionized water (density 1 g / cm 3The battery was placed on a surface of water (known as F1-F2) and the gravity F2 of the battery was measured. The buoyant force F received by the battery was taken as F1-F2. The battery then floated up based on Archimedes' principle F, and the battery volume V=(F1-F2) / was calculated.

[0352] From the test results of OCV and IMP, the batteries of all the examples always maintained an SOC of 99% or more until the end of storage in this test process.

[0353] After storing for 30 days, the battery volume was measured and the battery volume after storage was compared to the battery volume before storage. 11. Full cell cycle performance test at 45℃

[0354] In a constant temperature environment of 45°C, the full cell is charged at 1C to 4.3V, then charged at a constant voltage of 4.3V until the current is ≦0.05mA, left to stand for 5 minutes, and then discharged at 1C to 2.5V, and the capacity is D0. The above process is repeated until the capacity is attenuated to 80% of D0, and the number of repetitions at this time is recorded, that is, the number of cycles corresponding to 80% capacity retention at 45°C. 12. Testing the dissolution of transition metal Mn (and Fe doped on the Mn site)

[0355] The full cells prepared in the above Examples and Comparative Examples, which had been cycled at 45° C. until the capacity was attenuated to 80%, were discharged at a rate of 0.1 C to a cut-off voltage of 2.0 V. The batteries were then disassembled, the negative electrode sheet was removed, and 30 unit area (1540.25 mm ) pieces were cut from the negative electrode sheet. 2 ) wafers were randomly taken and inductively coupled plasma emission spectrometry (ICP) was measured using an Agilent ICP-OES730. From the ICP results, the amounts of Fe and Mn were calculated when Fe was doped on the Mn site of the positive electrode active material, and the amount of Mn (and Fe doped on the Mn site) eluted after cycling was calculated. The test standard was in accordance with EPA-6010D-2014. 13. Measurement of manganese and phosphorus elements in the positive electrode active material

[0356] 5 g of the positive electrode active material obtained above was dissolved in 100 mL of reverse aqua regia (concentrated hydrochloric acid:concentrated nitric acid = 1:3), and the content of each element in the solution was measured by ICP. Thereafter, the content of manganese element or phosphorus element was measured and converted (amount of manganese element or phosphorus element / amount of positive electrode active material × 100%) to obtain their weight ratio. 14. Coating layer thickness test

[0357] The thickness of the coating layer was tested mainly by cutting a thin slice about 100 nm thick from the middle of a single particle of the positive electrode active material produced above using FIB, and then performing a TEM test on the slice to obtain an original image for the TEM test.

[0358] The original images obtained in the above TEM test were processed with digital micrograph software to identify the coating layers according to the lattice spacing and included angle information, and the thickness of the coating layers was measured.

[0359] For selected particles, thickness was measured at three locations and averaged. 15. Measurement of lattice spacing and included angle

[0360] 1g of each of the positive electrode active material powders prepared above is placed in a 50mL test tube, 10mL of alcohol with a mass fraction of 75% is poured into the test tube, and the mixture is stirred for 30 minutes to disperse. Then, an appropriate amount of the above solution is taken with a clean disposable plastic pipette and dropped onto a 300 mesh copper mesh. At this time, some of the powder remains on the copper mesh. The copper mesh is transferred together with the sample to the TEM (Talos F200s G2) sample chamber for testing, and the original image of the TEM test is obtained.

[0361] The original image obtained by the above TEM test is run through digital micrograph software, and a Fourier transform (automatically completed by the software after clicking) is performed to obtain a diffraction pattern. The distance from the diffraction spot to the center position in the diffraction pattern is measured, and the lattice spacing can be obtained, and the included angle is calculated based on the Bragg equation.

[0362] By comparing the obtained lattice spacing and corresponding included angle data with their standard values, different materials of the coating layer can be distinguished. 16. Measurement of the molar ratio of SP2 to SP3 forms in the carbon of the third coating layer

[0363] This test was performed using Raman spectroscopy. By splitting the peaks in the Raman spectrum, I d / I g I d is the peak intensity of SP3 form carbon, and Ig is the peak intensity of SP2 form carbon, and the molar ratio of the two was confirmed. 17. Measurement of the Kernel Chemical Formula and Different Compositions of the Coating Layer

[0364] A spherical aberration transmission electron microscope (ACSTEM) is used to characterize the internal microstructure and surface structure of the positive electrode active material with high spatial resolution, and combined with three-dimensional reconstruction techniques, we obtain the kernel chemical formula of the positive electrode active material and the composition of different coating layers.

[0365] Table 11 shows performance data of the positive electrode active materials, positive electrode material compositions, positive electrode sheets, coin batteries, and full batteries in Examples 1 to 29 and Comparative Examples 1 to 18 measured according to the above-mentioned performance test method.

[0366] Table 12 shows the thickness of each coating layer and the weight ratio of elemental manganese to elemental phosphorus in the positive electrode active materials produced in Examples 1 to 14 and Comparative Examples 3 to 4 and 12.

[0367] Table 13 shows the lattice spacings and included angles of the first coating layer material and the second coating layer material in the positive electrode active materials produced in Examples 1 and 30-42.

[0368] Table 14 shows performance data of the positive electrode active materials, positive electrode material compositions, positive electrode sheets, coin batteries, and full batteries in Examples 30 to 42 measured according to the above-mentioned performance test method.

[0369] Table 15 shows performance data for the positive electrode material compositions, positive electrode sheets, coin batteries, and full batteries in Examples 43 to 65, measured according to the performance test method described above.

[0370] [Table 11A] [Table 11B]

[0371] [Table 12]

[0372] [Table 13]

[0373] [Table 14]

[0374] [Table 15]

[0375] As can be seen from Table 11, compared with the comparative example, the examples achieved a smaller lattice change rate, a smaller Li / Mn antistructural defect concentration, a larger packed density, a surface oxygen valence closer to -2, a smaller amount of Mn and Fe eluted after cycling, and better battery performance, such as better high-temperature storage performance and high-temperature cycle performance. The use of the positive electrode active material of the examples of the present application in combination with an organopolysiloxane compound can further mitigate the erosion of the positive electrode active material surface by the electrolyte, reduce the amount of Mn and Fe eluted after cycling, and further improve the cycle performance of the battery.

[0376] As can be seen from Table 12, the manganese content and the weight content ratio of manganese element to phosphorus element in the positive electrode active material were clearly reduced by doping and coating the manganese site and phosphorus site of lithium manganese iron phosphate (manganese content 35%, phosphorus content about 20%). Also, when Examples 1 to 14 are compared with Comparative Examples 3, 4, and 12, as can be seen from Table 11, the reduction in manganese element and phosphorus element in the positive electrode active material reduces the amount of elution of manganese ions and iron ions, and improves the performance of the manufactured battery.

[0377] As can be seen from Table 13, the lattice spacing and included angle of the first and second coating layers in the positive electrode active material of the present application are all within the above ranges of the present application. As can be seen from Table 14, even when the first and second coating layers containing other elements within the ranges of the present application are used, a positive electrode active material with good performance is obtained, and good battery performance results are achieved.

[0378] As can be seen from Table 15, when the positive electrode active material is the same, by selecting an organopolysiloxane compound that satisfies one or more of the appropriate polar functional group content, number average molecular weight, and additive amount and using it in combination with the positive electrode active material, the cycle performance of the battery can be further improved without affecting the energy density and dynamic performance.

[0379] As can be seen from Examples 1 and 43 to 47, as the amount of the organopolysiloxane compound added increases, the powder resistance of the positive electrode active material composition decreases once and then increases. This is believed to be because when the amount of the organopolysiloxane compound added is within a certain range, the hydrophobicity reduces the interaction between the conductive agents, mitigates the aggregation of the conductive agents, and forms a better conductive network.

[0380] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is an example, and anything that has substantially the same configuration as the technical idea within the technical scope of the present application and has similar effects is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art may make to the embodiment, or other forms constructed by combining some of the components in the embodiment, are also included in the scope of the present application, as long as they do not deviate from the gist of the present application.

Claims

1. A positive electrode material composition comprising a positive electrode active material having a core-shell structure and an organopolysiloxane compound, The positive electrode active material includes a kernel and a shell that covers the kernel, The chemical formula of the kernel is Li 1+x Mn 1-y A y P 1-z R z O 4 and x is any number within the range of -0.100 to 0.100, and optionally any number within the range of -0.005 to 0.002; y is any number within the range of 0.001 to 0.500; and z is any number within the range of 0.001 to 0.100; A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge; and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg; R is one or more elements selected from B, Si, N, and S; and optionally one element selected from B, Si, N, and S; and the values ​​of x, y, and z satisfy the condition that the entire kernel maintains electrical neutrality; The shell includes a first coating layer that coats the kernel, a second coating layer that coats the first coating layer, and a third coating layer that coats the second coating layer, and the first coating layer is made of crystalline Li pyrophosphate. a MP 2 O 7 And / or M b (P 2 O 7 ) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP 2 O 7 and M. b (P 2 O 7 ) cIn the formula, M is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the values ​​of a, b, and c are the values ​​of the crystalline pyrophosphate Li a MP 2 O 7 Or M b (P 2 O 7 ) c satisfies the condition for maintaining electrical neutrality, and the second coating layer is a crystalline phosphate XPO 4 wherein X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon.

2. The positive electrode material composition according to claim 1 , wherein the organopolysiloxane compound comprises at least one structural unit represented by formula 1. [Formula 1] R 1 , R 2 each independently represents at least one selected from the group consisting of -COOH, -OH, -SH, -CN, -SCN, an amino group, a phosphate ester group, a carboxylate group, an amide group, an aldehyde group, a sulfonyl group, a polyether segment, a C1-C20 aliphatic hydrocarbon group, a C1-C20 halogenated aliphatic hydrocarbon group, a C1-C20 heteroaliphatic hydrocarbon group, a C1-C20 halogenated heteroaliphatic hydrocarbon group, a C6-C20 aromatic hydrocarbon group, a C6-C20 halogenated aromatic hydrocarbon group, a C2-C20 heteroaromatic hydrocarbon group, and a C2-C20 halogenated heteroaromatic hydrocarbon group, or H; Optionally, R 1 , R 2 each independently represents at least one selected from the group consisting of -COOH, -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, a C2-C8 halogenated alkenyl group, and a phenyl group, or H; More preferably, R 1 , R 2 each independently represents at least one selected from the group consisting of -OH, -SH, an amino group, a phosphate ester group, a polyether segment, a C1-C8 alkyl group, a C1-C8 halogenated alkyl group, a C1-C8 heteroalkyl group, a C1-C8 halogenated heteroalkyl group, a C2-C8 alkenyl group, and a C2-C8 halogenated alkenyl group, or H.

3. 3. The positive electrode material composition according to claim 1, wherein the organopolysiloxane compound comprises one or more selected from the group consisting of polysiloxanes having a linear structure and polysiloxanes having a cyclic structure, and optionally, the organopolysiloxane compound is selected from the polysiloxanes having a linear structure.

4. The linear polysiloxane further comprises a blocking group, Optionally, the blocking group comprises at least one selected from the group consisting of polyether, C1-C8 alkyl group, C1-C8 halogenated alkyl group, C1-C8 heteroalkyl group, C1-C8 halogenated heteroalkyl group, C2-C8 alkenyl group, C2-C8 halogenated alkenyl group, C6-C20 aromatic hydrocarbon group, C1-C8 alkoxy group, C2-C8 epoxy group, hydroxyl group, C1-C8 hydroxyalkyl group, amino group, C1-C8 aminoalkyl group, carboxyl group, and C1-C8 carboxyalkyl group. The positive electrode material composition of claim 3.

5. The linear polysiloxane may be selected from the group consisting of polydimethylsiloxane, polydiethylsiloxane, polymethylethylsiloxane, polymethylvinylsiloxane, polyphenylmethylsiloxane, polymethylhydrogensiloxane, carboxyl-functionalized polysiloxane, polymethylchloropropylsiloxane, polymethyltrifluoropropylsiloxane, perfluorooctylmethylpolysiloxane, mercaptopropylpolysiloxane, aminoethylaminopropylpolydimethylsiloxane, methoxy-terminated polydimethylsiloxane, hydroxypropyl-terminated polydimethylsiloxane, aminopropyl-terminated polydimethylsiloxane, epoxy-terminated polysiloxane, hydroxy-terminated polydimethylsiloxane, and polydimethylsiloxane. and / or one or more of polydimethylsiloxane, polymethylchloropropylsiloxane, polymethyltrifluoropropylsiloxane, mercaptopropylpolysiloxane, aminoethylaminopropylpolydimethylsiloxane, hydroxylterminated polydimethylsiloxane, polyether polydimethylsiloxane, side chain grafted polydimethylsiloxane, side chain phosphate ester grafted polydimethylsiloxane, and / or one or more of polydimethylsiloxane, polymethylchloropropylsiloxane, polymethyltrifluoropropylsiloxane, mercaptopropylpolysiloxane, aminoethylaminopropylpolydimethylsiloxane, hydroxylterminated polydimethylsiloxane, polyether polydimethylsiloxane, side chain phosphate ester grafted polydimethylsiloxane. The positive electrode material composition according to claim 3 or 4, wherein the polysiloxane having a cyclic structure includes one or more of cyclic polydimethylsiloxane, cyclic polymethylvinylsiloxane, cyclic polymethylhydrogensiloxane, and cyclic polymethyltrifluoropropylsiloxane, and optionally includes one or more of 1,3,5,7-octamethylcyclotetrasiloxane, 1,3,5,7-tetrahydro-1,3,5,7-tetramethylcyclotetrasiloxane, cyclopentapolydimethylsiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, hexadecamethyloctasiloxane, and tetradecamethylcycloheptasiloxane.

6. The positive electrode material composition according to any one of claims 1 to 5, wherein the organopolysiloxane compound has a number average molecular weight of 300,000 or less, and optionally 400 to 80,000.

7. The positive electrode material composition according to any one of claims 1 to 6, wherein the mass percentage of the polar functional group in the organopolysiloxane compound is α, where 0≦α<50%, and optionally 5%≦α≦30%.

8. The positive electrode material composition according to any one of claims 1 to 7, wherein the content of the organopolysiloxane compound is 0.01 wt% to 2 wt%, and optionally 0.1 wt% to 2 wt%, based on the total weight of the positive electrode material composition.

9. The amount of the first coating layer is greater than 0 and less than 6% by weight, preferably greater than 0 and less than 5.5% by weight, more preferably greater than 0 and less than 2% by weight, based on the weight of the kernel; The amount of the second coating layer is greater than 0 and less than 6% by weight, preferably greater than 0 and less than 5.5% by weight, more preferably 2% to 4% by weight, based on the weight of the kernel; The positive electrode material composition according to any one of claims 1 to 8, wherein the coating amount of the third coating layer is greater than 0 and less than 6 wt%, selectively greater than 0 and less than 5.5 wt%, and more selectively greater than 0 and less than 2 wt%, based on the weight of the kernel.

10. the thickness of the first coating layer is between 1 nm and 10 nm; and / or the thickness of the second coating layer is between 2 nm and 15 nm; and / or The positive electrode material composition according to any one of claims 1 to 9, wherein the third coating layer has a thickness of 2 nm to 25 nm.

11. The lattice spacing of the crystalline pyrophosphate in the first coating layer is in the range of 0.293 nm to 0.470 nm, and the included angle of the (111) crystal orientation is in the range of 18.00° to 32.00°; and / or The positive electrode material composition according to any one of claims 1 to 10, wherein the lattice spacing of the crystalline phosphate in the second coating layer is in the range of 0.244 nm to 0.425 nm, and the included angle of the (111) crystal orientation is in the range of 20.00° to 37.00°.

12. in said kernel, the ratio of y to 1-y is between 1:10 and 1:1, alternatively between 1:4 and 1:1; and / or 12. The cathode material composition of claim 1, wherein in the kernel, the ratio of z to 1-z is from 1:9 to 1:999, and optionally from 1:499 to 1:

249.

13. 13. The cathode material composition according to claim 1, wherein the carbon of the third coating layer is a mixture of SP2 carbon and SP3 carbon, and optionally, the molar ratio of the SP2 carbon to the SP3 carbon is any number within the range of 0.1 to 10, and optionally, any number within the range of 2.0 to 3.

0.

14. The content of manganese element is in the range of 10% by weight to 35% by weight, preferably in the range of 15% by weight to 30% by weight, more preferably in the range of 17% by weight to 20% by weight, based on the weight of the positive electrode active material; and / or The content of phosphorus element is in the range of 12 wt% to 25 wt%, and optionally in the range of 15 wt% to 20 wt%, based on the weight of the positive electrode active material; and / or The positive electrode material composition according to any one of claims 1 to 13, wherein the weight ratio of elemental manganese to elemental phosphorus, based on the weight of the positive electrode active material, is in the range of 0.90 to 1.25, and optionally 0.95 to 1.

20.

15. The positive electrode material composition according to any one of claims 1 to 14, wherein the positive electrode active material satisfies at least one of the following conditions (1) to (4): (1) The positive electrode active material has a lattice change rate before and after complete insertion and extraction of lithium of 4% or less, optionally 3.8% or less, and more preferably 2.0% to 3.8%. (2) The positive electrode active material has a Li / Mn antistructure defect concentration of 4% or less, preferably 2.2% or less, and more preferably 1.5% to 2.2%. (3) The compressed density of the positive electrode active material at 3 T is 2.2 g / cm 3 or more, and optionally 2.2 g / cm 3 or more and 2.8 g / cm 3 The following is the result. (4) The oxygen valence number on the surface of the positive electrode active material is −1.90 or less, and optionally −1.90 to −1.

98.

16. 16. The positive electrode material composition according to claim 1, further comprising a conductive agent and a binder, and optionally, the content of the binder is 1.79 wt % to 10 wt % based on the total weight of the positive electrode material composition, and optionally, the content of the conductive agent is 0.2 wt % to 10 wt % based on the total weight of the positive electrode material composition.

17. The powder resistivity of the positive electrode material composition at 12 MPa is 4 Ω / cm to 55 Ω / cm, and optionally 4 Ω / cm to 40 Ω / cm; and / or The specific surface area of ​​the positive electrode material composition is 8 m 2 / g to 20m 2 / g, and optionally 8m 2 / g to 15m 2 The positive electrode material composition according to any one of claims 1 to 16, wherein the positive electrode material composition is a SiO2 / g.

18. A method for producing a positive electrode material composition, comprising the steps of: providing a kernel material, coating and mixing the kernel material; The step of providing the kernel material includes providing the kernel with a chemical formula of Li 1+x Mn 1-y A y P 1-z R z O 4wherein x is any number within the range of -0.100 to 0.100, optionally any number within the range of -0.005 to 0.002, y is any number within the range of 0.001 to 0.500, z is any number within the range of 0.001 to 0.100, A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb and Ge, optionally one or more elements selected from Fe, Ti, V, Ni, Co and Mg, R is one or more elements selected from B, Si, N and S, optionally one element selected from B, Si, N and S, and the values ​​of x, y and z satisfy the condition that the entire kernel is kept electrically neutral; The coating step includes: a MP 2 O 7 And / or M b (P 2 O 7 ) c and XPO 4 A suspension is provided, and the kernel material is added to the suspension, mixed, and sintered to obtain a positive electrode active material, where the positive electrode active material has a core-shell structure and includes the kernel and a shell covering the kernel, the shell includes a first coating layer covering the kernel, a second coating layer covering the first coating layer, and a third coating layer covering the second coating layer, and the first coating layer is a crystalline pyrophosphate Li a MP 2 O 7 And / or M b (P 2 O 7 ) c wherein 0≦a≦2, 1≦b≦4, and 1≦c≦6; a MP 2 O 7 and M. b (P 2 O 7 ) cIn the formula, M is independently one or more elements selected from Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the values ​​of a, b, and c are the values ​​of the crystalline pyrophosphate Li a MP 2 O 7 Or M b (P 2 O 7 ) c The second coating layer is made of crystalline phosphate XPO. 4 wherein X is one or more elements selected from Li, Fe, Ni, Mg, Co, Cu, Zn, Ti, Ag, Zr, Nb, and Al, and the third coating layer is carbon; In the mixing step, the obtained positive electrode active material, an organopolysiloxane compound, an optional binder, and an optional conductive agent are uniformly mixed to obtain a positive electrode material composition.

19. The step of providing the kernel material comprises the following steps (1) and (2): The step (1) includes mixing and stirring a manganese source, a dopant of element A, and an acid in a container to obtain manganese salt particles doped with element A; In the step (2), the manganese salt particles doped with the element A are mixed with a lithium source, a phosphorus source and a dopant of element R in a solvent to obtain a slurry, which is then sintered under the protection of an inert gas atmosphere to obtain a kernel doped with the elements A and R, wherein the kernel doped with the elements A and R is Li 1+x Mn 1-y A y P 1-z R z O 4wherein x is any number in the range of -0.100 to 0.100, and optionally any number in the range of -0.005 to 0.002; y is any number in the range of 0.001 to 0.500; z is any number in the range of 0.001 to 0.100; A is one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and optionally one or more elements selected from Fe, Ti, V, Ni, Co, and Mg; and R is one or more elements selected from B, Si, N, and S, and optionally one element selected from B, Si, N, and S. The method of claim 18.

20. The step (1) comprises mixing at a temperature between 20°C and 120°C, optionally between 40°C and 120°C; and / or In step (1), the stirring is carried out at 400 rpm to 700 rpm for 1 hour to 9 hours, optionally 3 hours to 7 hours; and / or 20. The method of claim 19, wherein the step (2) is mixing at a temperature of 20°C to 120°C, optionally 40°C to 120°C, for 1 hour to 10 hours.

21. The dopant of the element A is one or more selected from the simple substance, carbonate, sulfate, chloride, nitrate, organic acid salt, oxide, and hydroxide of one or more elements selected from Zn, Al, Na, K, Mg, Mo, W, Ti, V, Zr, Fe, Ni, Co, Ga, Sn, Sb, Nb, and Ge, and / or 21. The method according to claim 19 or 20, wherein the dopant of the element R is one or more selected from inorganic acids, organic acids, sulfates, chlorides, nitrates, organic acid salts, oxides, and hydroxides of one or more elements selected from B, Si, N, and S.

22. The coating step includes a first coating step, a second coating step and a third coating step, The first coating step includes dissolving a source of element M, a phosphorus source, an acid, and an optional lithium source in a solvent to obtain a first coating layer suspension, thoroughly mixing the kernel obtained in the step of providing a kernel material with the first coating layer suspension obtained in the first coating step, drying, and then sintering to obtain a material coated with a first coating layer; In the second coating step, a source of element X, a phosphorus source and an acid are dissolved in a solvent to obtain a second coating layer suspension, and the material coated with the first coating layer obtained in the first coating step and the second coating layer suspension obtained in the second coating step are thoroughly mixed, dried and then sintered to obtain a material coated with two coating layers; The method according to any one of claims 18 to 21, wherein the third coating step includes dissolving a carbon source in a solvent and dissolving it sufficiently to obtain a third coating layer solution, and then adding the material coated with two coating layers obtained in the second coating step to the third coating layer solution, mixing uniformly, drying, and then sintering to obtain a material coated with three coating layers, i.e., a positive electrode active material.

23. In the first coating step, the pH of the solution of the source of element M dissolved therein, the phosphorus source, the acid, and the optional lithium source is controlled to 3.5-6.5, and then reacted for 1-5 hours while stirring, and then the solution is heated to 50° C.-120° C. and maintained at this temperature for 2-10 hours; and / or The sintering in the first coating step is carried out at 650° C. to 800° C. for 2 hours to 6 hours; and / or In the second coating step, a source of element X, a phosphorus source and an acid are dissolved in a solvent, and then the solution is reacted by stirring for 1 hour to 10 hours, and then the solution is heated to 60° C. to 150° C. and maintained at the temperature for 2 hours to 10 hours; and / or The sintering in the second coating step is carried out at 500° C. to 700° C. for 6 hours to 10 hours; and / or The method according to claim 22, wherein the sintering in the third coating step is carried out at 700° C. to 800° C. for 6 hours to 10 hours.

24. A positive electrode sheet including a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, the positive electrode film layer including the positive electrode material composition according to any one of claims 1 to 17, or the positive electrode material composition produced by the method according to any one of claims 18 to 23, and a content of the positive electrode material composition in the positive electrode film layer is 50% by weight or more, and optionally 90% by weight to 100% by weight, based on a total weight of the positive electrode film layer.

25. The positive electrode sheet according to claim 24, wherein the positive electrode sheet satisfies at least one of the following conditions (1) to (6): (1) The solid-liquid contact angle between the positive electrode film layer and the non-aqueous organic solvent is 3° to 90°, optionally 3° to 60°, and further 10° to 30°. (2) The porosity of the positive electrode film layer is 15% to 50%, and optionally 15% to 30%. (3) The resistance of the positive electrode film layer is greater than 0 and equal to or less than 6 Ω. (4) The adhesive strength between the positive electrode film layer and the positive electrode current collector is 0.5 MPa or more. (5) The surface density of the positive electrode film layer is 0.006 g / cm 2 ~0.065g / cm 2 It is. (6) The positive electrode film layer has an electrolyte absorption rate of 0.0125 μg / s to 100 μg / s, and optionally 0.5 μg / s to 40 μg / s.

26. A secondary battery comprising the positive electrode material composition according to any one of claims 1 to 17, or the positive electrode material composition produced by the method according to any one of claims 18 to 23, or the positive electrode sheet according to claim 24 or 25.

27. A power consuming device comprising the secondary battery according to claim 26.

Citation Information

Patent Citations

  • Lithium manganese iron phosphate composite material, preparation method thereof and lithium ion battery

    CN114256448A

  • Phosphate compound, positive electrode material for secondary battery, and method for producing secondary battery

    JP2014056722A

Cited By

  • Battery and electric device

    CN119764591A

  • Negative electrode material, preparation method thereof and application of negative electrode material in preparation of special-shaped battery

    CN120199797A

  • Preparation method of lithium manganese iron phosphate positive electrode material

    CN120600806A

  • Positive electrode material, secondary battery, and electronic device