Reduction of iron ore metals and reactor for said reduction

The cocurrent flow of reducing gas and iron ore in a vertical reactor addresses yield and metallization challenges in DRI processes, achieving high metallization rates and efficient thermal management without coatings, enhancing productivity and reducing fines production.

JP2024545211APending Publication Date: 2024-12-05LOUSSAVAARA KIIRUNAVAORA AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024535324
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-23
Filing Date
2022-12-16
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing direct reduction iron (DRI) processes suffer from low yields due to the generation of fines and slurry, which reduces the efficiency and requires costly coating processes, while conventional reactors struggle to achieve high metallization rates and efficient thermal management.

Method used

A reduction process and reactor design that utilizes a cocurrent flow of heated reducing gas and iron ore material within a vertical reactor, allowing for isothermal or near-isothermal conditions, which reduces the formation of crushed solids and enhances metallization rates, enabling higher yields and faster reduction times without the need for pre-coating.

Benefits of technology

The process achieves metallization rates up to 94% with reduced production of fines, allows for direct integration with pelletizing plants, and eliminates the need for costly coatings, resulting in improved thermal efficiency and higher productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545211000001_ABST
    Figure 2024545211000001_ABST
Patent Text Reader

Abstract

A reduction reactor and process for reducing iron ore material to reduced iron material, the process comprising the steps of: feeding iron ore material to the reduction reactor (1) at a top (1a) thereof to create a gravity flow of the material in the reduction reactor from the top (1a) axially downwards to a bottom (1b) of the reduction reactor (1) (101), feeding a reducing gas to the reduction reactor (1) at the top (1a) thereof such that the heated reducing gas creates a co-current flow with the gravity flow of the material in the reduction reactor (1), and reducing the iron ore material in the reduction reactor to reduced iron material by the reducing gas (103).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a process for the reduction of iron ore material to reduced iron material and to a reduction reactor for the reduction of iron ore material to reduced iron material. [Background technology]

[0002] In the direct reduction iron (DRI) process, reduction of iron ore pellets occurs by reducing the oxygen content of the ore. Conventional apparatus and methods for reducing iron oxide to metallic iron are shown, for example, in U.S. Pat. No. 3,748,120. Iron ore material is fed into the top of a vertical shaft reduction furnace and removed from the bottom of the furnace. Hot reducing gas, having a temperature of at least about 800° C. and composed primarily of H2 and CO, is added to the gravity flow of material in the furnace through an inlet between the inlet and outlet of the furnace, flows countercurrently to the pellets, and exits the furnace at the top of the furnace after the gas passes through the iron oxide particles to heat and reduce the pellets. The iron ore material, such as pellets, may be cooled prior to discharge from the furnace.

[0003] The actual yield in such processes is typically around 68-69%. To increase the yield, various strategies have been employed to develop conventional DRI vertical shaft furnaces.

[0004] One way to increase yields could be to generate less fines during the process. During ore handling operations, fines can be generated by physical wear and breakage of pellets, which are sieved through sieves before the material is charged to the furnace, resulting in lower yields. Furthermore, reduction in the shaft furnace can generate additional fines due to the heat and process crushing, which exit the production chain as "slurry", thereby reducing the yield of the process.

[0005] In US6132489, a direct reduction process is presented in which iron ore charges containing both coarse and fine particles are continuously processed in one single vertical reactor shaft to achieve high metallization rates while reducing clogging in the particle bed of the moving bed reactor. The vertical reduction reactor has at least one reduction zone in which the particles form two types of beds, a fluidized bed and a moving bed. The particles and fine particles are guided to the fluidized bed. A reducing gas at a temperature higher than about 700°C is flowed upward through the reduction zone, where the reducing gas forms a fluidized bed containing a first portion of particles, and a non-fluidized bed, the average size of the particles of the first portion being smaller than the average size of the particles of the second portion. The metallic iron-containing particles are made to overflow from the fluidized bed and drop out through a discharge pipe having an inlet end at the top of the fluidized bed.

[0006] Another strategy to increase the yield of the DRI process is presented in US Patent No. 9,273,368, where iron oxide pellets or chunks coated with mineral solution are fed to a pre-reduction zone, a transition zone, a metallization zone, and a cooling zone, during which the coated charge is preheated to a temperature in the range of about 1000-1300°C by passing rich fuel gas produced by external partial combustion with substoichiometric amounts of air in countercurrent upward through the pre-reduction zone, partially reducing the coated charge, and passing reducing gas in cocurrent downward through the metallization zone to finish the reduction of iron oxide to metallic iron. Summary of the Invention [Problem to be solved by the invention]

[0007] Although various strategies have been undertaken to improve DRI processes and furnaces, a need continues to exist for improved processes for the reduction of iron ore materials to reduced iron materials.

[0008] It is an object of the present disclosure to provide a process for the reduction of iron ore material to reduced iron material that mitigates or overcomes at least some of the shortcomings of prior art reduction processes. A further object is to provide a reduction reactor for such reduction of iron ore material.

[0009] The invention is defined by the accompanying independent claims. Non-limiting embodiments are evident from the dependent claims, the accompanying drawings and the following description. [Means for solving the problem]

[0010] According to a first aspect, a process for reducing iron ore material to reduced iron material is provided. The process includes the steps of providing a reduction reactor and feeding iron ore material to the reduction reactor at a top of the reduction reactor to create a gravity flow of the iron ore material in the reduction reactor axially downward from the top to a bottom of the reduction reactor. A reduction gas is fed to the reduction reactor at the top of the reduction reactor such that the heated reduction gas creates a co-flow with the gravity flow of the material in the reduction reactor. The reduction gas reduces the iron ore material to reduced iron material in the reduction reactor. Spent reduction gas is removed from the reduction reactor at a gas outlet in a lower section of the reduction reactor, and reduced iron material is removed from the reduction reactor at a bottom of the reduction reactor.

[0011] The iron ore material added to the top of the reduction reactor may be unreduced iron ore material, i.e., no pre-reduction occurs before the material is added to the reduction reactor.

[0012] The iron ore material may be iron ore pellets, iron ore chunks, and / or iron ore agglomerates. By pellets we mean typically spheres of 6-16 mm, or spheres having a diameter of 3-18 mm or 6-18 mm.

[0013] The iron ore material added at the top of the reduction reactor forms a packed bed of material that descends through the reduction reactor by gravity.

[0014] The reducing gas creates a co-current flow with the iron ore material and the gravity flow of the reduced iron material that is subsequently formed in the reduction reactor.

[0015] The reduction reactor may be a reduction furnace or a vertical reduction furnace.

[0016] When fed to the reduction reactor, the iron ore material may have a temperature of 0-1300° C. Thus, the iron ore material may be cold or heated when added. If heated, the thermal potential / energy of the hot material may be utilized in the reduction reactor.

[0017] The heated reducing gas may have a temperature of 500-1000°C when fed to the top of the reduction reactor.

[0018] The above process is a reduction process that can efficiently process heated iron ore material. The method can be used / integrated immediately after and in-line with a pelletizing plant since the heated iron ore material can be subjected to a reduction reactor and processed into reduced iron material / metallized material.

[0019] In order to balance the thermal energy requirements of the process and to obtain an isothermal or near isothermal reduction process with no significant drop in temperature during the reduction process and minimal difference between the gas temperatures above and below the bed of iron ore material in the reactor, i.e. a process which is expected to improve the rate of reduction and shorten the reduction time, the temperature of the added reducing gas may need to be adjusted in relation to the temperature of the added iron ore material.

[0020] In order to increase the yield of the process, the temperature selection should preferably overcome the low temperature collapse during the transformation of hematite to magnetite, which is most dominant / prominent between 450-650°C. Increasing the temperature above this range during the reduction / metallization in the reduction reactor is expected to increase the yield of the iron reduction process. By avoiding the low temperature collapse during the transformation of hematite to magnetite, the proportion of crushed solids formed from the iron ore material in the process can be reduced. With less amount of crushed solids generated, higher yields can be obtained. Here, crushed solids means crushed solids of any form and size, such as dust / fine particles / small particle material, such as smaller than about 6 mm.

[0021] In the case of low temperature feed charging, i.e., for iron ore material having a temperature below 200°C, the corresponding reducing gas temperature should be 950-1000°C to meet the above requirements.

[0022] If the temperature of the iron ore material fed to the reduction reactor is high, i.e. in the range of 1200-1300°C, the corresponding reduction gas temperature required to balance such energy requirements of the process will be lower, such as in the range of 400-700°C.

[0023] In the above process, the rate of the reduction process can be made faster compared to the prior art processes, resulting in a reduction reactor design that can be a low volume high throughput reactor. Therefore, the output is directly dependent on the selection of the iron ore material temperature and the reduction gas temperature.

[0024] By feeding the reduction gas to the top of the reduction reactor such that there is a co-flow of heated gas and material through the reactor, this results in a more efficient reduction process, which can be sped up and requires less time to complete, as compared to conventional reduction processes. Using this process, the resulting reduction / metallization can be as high as 94% or more. Additionally, smaller size / shorter reduction reactors can be used than are standard today.

[0025] When the reduction gas is introduced at the top of the reduction reactor, less material is lost to crushed solids compared to when the gas exits at the top of the reduction reactor, since the low temperature decay is most prevalent at the top of the reduction reactor. Less crushed solids generated results in higher yields.

[0026] The spent reducing gas removed from the reduction reactor may have a temperature of 600 to 900°C.

[0027] The reduced iron material / metallized material removed from the reduction reactor may have a temperature of 600-850°C.

[0028] The lower section extends from the bottom to the middle of the reduction reactor. The gas outlet of the reduction reactor may be located at the bottom of the reduction reactor. Alternatively, the gas outlet may be located in a portion / section of the reduction reactor that is located above or just above the bottom of the reduction reactor, as viewed in the direction of gravity flow of material in the reduction reactor.

[0029] The iron ore material when fed to the reduction reactor may have a temperature of 0-1300°C.

[0030] Iron ore material can be used in 0~1300℃, 30~1300℃, 100~1300℃, 200~1300℃, 300~1300℃, 400~1300℃, 500~1300℃, 600~1300℃, 700~1300℃, 800~1300℃, 900~1300℃, 1000~1300℃, 1100~1300℃, 1200 The temperature may be from 0 to 1300°C, 0 to 1200°C, 0 to 1100°C, 0 to 1000°C, 0 to 900°C, 0 to 800°C, 0 to 700°C, 0 to 600°C, 0 to 500°C, 0 to 400°C, 0 to 300°C, 0 to 200°C, 0 to 100°C, 500 to 900°C, or 800 to 1100°C, and is preferably 800°C or higher.

[0031] The reducing gas may have a temperature of 500-1000°C when supplied to the reduction reactor.

[0032] The temperature of the reducing gas may preferably be between 500 and 900° C. As discussed above, the selection of the reducing gas temperature depends on the temperature of the iron ore material added to the reduction reactor.

[0033] For low temperature iron ore materials, the required reducing gas temperature will be higher, ranging from 950-1000°C. Such high temperatures may require oxygen injection into the reducing gas to obtain this high temperature. At lower temperatures, oxygen injection may not be required. Furthermore, the reducibility is not reduced. The absence of an oxygen injection system is expected to prevent a significant amount of reducing gas wastage due to oxidation to reach the higher gas temperatures.

[0034] The temperature of the spent reducing gas removed from the reduction reactor may be at least 600°C, and the temperature of the reduced iron material removed from the reduction reactor may be at least 600°C.

[0035] If the temperatures of the spent reducing gas and reduced iron material removed from the reduction reactor are each at least 600°C, reduction / metallization occurs in the reduction reactor at temperatures higher than the severe low-temperature collapse during the transformation of hematite to magnetite, which is most dominant / prominent between 450-650°C.

[0036] The temperature of the discharged reduced iron material is at least 600° C., so that the hot reduced iron material can be directly charged into the downstream process unit, and a significant amount of heat energy can be saved in the downstream process.

[0037] In one example, hot formed briquettes can be formed from the removed hot reduced iron material. This leads to significant advantages over the briquetting process immediately following the reduction process, since the main factor governing the physical quality of the briquettes is the temperature of the feed to the briquetting machine. The higher the feed temperature, the higher the physical quality of the briquettes in terms of density and tumble strength.

[0038] Traditionally, iron ore materials such as pellets are coated (using materials such as limestone, dolomite and olivine as binders, as well as bentonite) to avoid compaction / sticking during the reduction process when temperatures in the reactor are above 900°C.

[0039] In the present method, such coating of the iron ore material may not be required and uncoated material can be used. In the present process, nowhere in the reactor after reduction of the iron ore material reaches temperatures of 900°C or more. This results in no or nearly no compaction / sticking in the reactor due to loose or iron-on-iron sintering of the reduced material and therefore no or nearly no compaction / sticking of material in the reactor. If coating is not required, the iron ore material can be used dry and uncoated. This saves on processing and operating costs of coating.

[0040] The reducing gas supplied to the reduction reactor may contain 90% or more hydrogen by volume.

[0041] The reduction gas fed to the reduction reactor may comprise 90% or more H2 by volume, may comprise at least 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, or at least 99% H2, and preferably at least 97% H2. The remainder is H2O and possibly other gases such as N2.

[0042] The use of pure or near pure H2 may result in faster reduction rates and shorter reduction times compared to using a reducing gas containing less hydrogen. This increases the productivity or throughput of the process. Additionally, the process may produce less crushed solids. The use of H2 results in less swelling of the iron ore material compared to when the reducing gas contains CO (as in standard reduction processes). The reducing gas used herein may include non-carbon containing gas components.

[0043] Heated reducing gas to the reduction reactor is introduced at a high pressure point at the top of the reactor.

[0044] The iron ore material may be reduced to ferrous material in a reduction reactor in an isothermal or near isothermal reduction process.

[0045] In an isothermal or near isothermal reduction process, the reduction speed is improved and the reduction time is shortened. In an isothermal reduction process, there is no significant drop in temperature during the reduction process, and the difference between the gas temperatures above and below the bed of iron ore material in the reactor is minimized or as low as possible. In order to balance the thermal energy requirements of the process and to obtain an isothermal or near isothermal reduction process, the temperature of the added reduction gas may need to be adjusted in relation to the temperature of the added iron ore material. In one example, the temperature of the reduction gas fed to the reduction reactor may be about 900°C, and the temperature of the iron ore material fed to the reduction reactor may be about 800°C.

[0046] Dry crushed solids may be separated from the spent reduction gas removed from the reduction reactor and re-introduced into the reduction reactor at a crushed solids inlet located at a point below the gas outlet of the reduction reactor in the direction of gravity flow of material in the reduction reactor.

[0047] Reinjection of the dry crushed solids is expected to increase the material / solids yield of the process.

[0048] According to a second aspect, a reduction reactor for the reduction of iron ore material to reduced iron material is provided. The reduction reactor comprises a material inlet arranged at the top of the reduction reactor and configured to feed the iron ore material to the reduction reactor, and a gas inlet arranged at the top of the reduction reactor and configured to feed a heated reduction gas to the reduction reactor, the reduction reactor, the material inlet and the gas inlet being arranged such that the material fed through the material inlet and the reduction gas fed through the gas inlet create a co-flow from the top axially downwards to the bottom of the reduction reactor such that the iron ore material is reduced in the reduction reactor. A gas outlet is arranged at a lower section of the reduction reactor and configured to remove used reduction gas from the reduction reactor, and a material outlet is arranged at the bottom of the reduction reactor and configured to remove reduced iron material from the reduction reactor.

[0049] The spent reduction gas is removed from the reduction reactor at a gas outlet, which is a low pressure point in the reduction reactor, and is preferably appropriately positioned / designed to avoid carryover of crushed solids such as fines / dust / pellets into the spent reduction gas.

[0050] The reduction reactor may further comprise a separator disposed at / after the gas outlet for separating the dry crushed solids from the spent reduction gas.

[0051] The reduction reactor may further include a solids recycler arranged in communication with the separator and arranged to reintroduce the dry crushed solids separated from the spent reduction gas into the reduction reactor at a crushed solids inlet arranged at a point below the spent reduction gas outlet as viewed in the direction of gravity flow of material in the reduction reactor.

[0052] The separated dry crushed solids may be recharged into the reduction reactor using a recycler ejector. [Brief description of the drawings]

[0053] [Figure 1] FIG. 1 shows a novel reduction reactor. [Diagram 2] FIG. 1 shows a schematic diagram of a process for the reduction of iron ore material to reduced iron material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0054] Various strategies have been undertaken to improve iron ore reduction processes and reactors used for such reduction. Processes and reduction reactors are described below that can provide faster rates of reduction, improved metallization levels, and higher material / solids yields for the process compared to standard reduction processes. The processes and reduction reactors can be further configured for efficient processing of hot iron ore material. This allows hot iron ore material, e.g., pellets, to be added to the reduction reactor directly from a pelletizing plant.

[0055] Such a novel reduction reactor 1 is shown in FIG. 1 and a process for carrying out the reduction of iron ore material such as iron ore pellets, iron ore chunks, and / or iron ore agglomerates to reduced iron material is shown in FIG. 2. The reduction reactor 1 provided at 100 has a material inlet 11 arranged at a top 1a of the reduction reactor, configured at 101 for feeding iron ore material to the reduction reactor. The iron ore material added at the top of the reduction reactor may have a temperature of 0-1300° C. and forms a packed bed of material that descends through the reduction reactor from the top 1a to the bottom 1b by gravity. A gas inlet 12 is arranged at the top 1a of the reduction reactor 1 and configured at 102 for feeding heated reduction gas having a temperature of 500-1000° C. to the reduction reactor 1. The reduction gas fed to the reduction reactor may comprise 90% or more H2 by volume, preferably 97% or more H2. The balance is H2O and possibly other gases such as N2.

[0056] The material fed through the material inlet 11 and the reduction gas 12 fed through the gas inlet create a co-flow axially downward from the top 1a to the bottom 1b of the reduction reactor 1 such that the iron ore material is reduced in the reduction reactor at 103. A gas outlet 13 is disposed in the lower section 1c of the reduction reactor 1 and configured for removing spent reduction gas from the reduction reactor 1 at 104. A material outlet 14 is disposed in the bottom 1b of the reduction reactor 1 and configured for removing reduced iron material from the reduction reactor 1 at 105. A crushed solids inlet 20 is disposed at a point below the gas outlet 13 of the reduction reactor in the direction of gravity flow of the material in the reduction reactor.

[0057] To balance the heat energy requirements of the process and to obtain an isothermal or near isothermal reduction process in the reduction reactor 1, the temperature of the reduction gas added to the reactor may need to be adjusted in relation to the temperature of the added iron ore material. An isothermal process is expected to provide a more controlled reduction reaction than a non-isothermal process, and is expected to improve the rate of reduction and reduce reduction time. In an isothermal reduction process, there is no significant drop in temperature during the reduction process and there is minimal difference between the gas temperatures above and below the bed of iron ore material in the reactor.

[0058] The low temperature collapse during the transformation of hematite to magnetite is most dominant / prominent between 450-650 °C. Increasing the temperature above this range during reduction / metallization in the reduction reactor is expected to enhance the yield of the iron reduction process.

[0059] To achieve this requirement, the spent reducing gas removed from the reduction reactor in 104 may have a temperature of 600-900°C, and the reduced iron material / metallized material removed from the reduction reactor 1 in 105 may have a temperature of 600-850°C.

[0060] In the case of low temperature feed charge, i.e., for iron ore material having a temperature below 200° C., the corresponding reducing gas temperature should be between 950-1000° C. to meet the above requirements. If the temperature of the iron ore material fed to the reduction reactor is higher, i.e., in the range of 1200-1300° C., the corresponding reducing gas temperature required to balance such energy requirements of the process will be lower, such as in the range of 400-700° C.

[0061] The nominal operating pressure of the reduction reactor may be in the range of about 1 to 7 bar, taking into account the economical / integrated design of the reduction process.

[0062] After removing the reduced material from the reduction reactor 1 at 105, the process may include the further step of cooling the reduced / metallized material.

[0063] Dry crushed solids may be separated from the spent reduction gas removed from the reduction reactor 1 at 104 using a separator 15 located at / after the spent reduction gas outlet 13 at 104b. The separated dry crushed solids may then be re-injected into the reduction reactor 1 at a crushed solids inlet 20 located at a point below the gas outlet 13 at 104c. Dry crushed solids such as fines / dust / pellets may be separated from the spent reduction gas using, for example, a dry cyclone separator or a baffle separator 15. The dry crushed solids recovered from the spent reduction gas are expected to be coarse in nature with high iron content and a larger friction coefficient. A recycler ejector 16 may be used to facilitate seamless recycling of the recovered solids back to the lower part of the reduction reactor.

[0064] Separation of the dried crushed solids from the spent reduction gas can be a gas pre-cleaning / separation step before the gas proceeds to the next processing unit. Heat from the spent reduction gas can be recovered via a gas-gas heat exchanger 17 by using cold reduction gas 18 on the way to the reduction gas heater 19, thereby increasing the thermal efficiency of the process.

[0065] A small stream of high pressure hot reducing gas can be used as the medium of injection to recycle the dry crushed solids separated from the spent reducing gas back into the reduction reactor. This constant flow of reducing gas then becomes the driving fluid medium ensuring the continuous function / operation of the ejector. If the recycled solids are diverted to an alternative / external system, the gas for driving / operating the solids ejector can be driven by an alternative gas such as nitrogen. In this closed loop, solids are not expected to increase or accumulate over time as the exit velocity of the high bulk density flow of reduced material at the bottom of the reduction reactor is expected to entrain the recovered crushed solids into the product and prevent accumulation / upward flow.

[0066] The above process and reduction reactor were simulated for various material and gas temperatures using HSC Chemistry® software. The various parameters and parameter values ​​used in the simulation are summarized in Table 1.

[0067] [Table 1]

[0068] In these simulations, the iron ore material fed to the reduction reactor was iron or pellets of standard form and composition, and a mass flow rate of 1.410 tonnes / h was used. The pellet feed temperatures when entering the reduction reactor were set to 1300°C, 800°C, 200°C, and 0°C, respectively, and the reduction gas temperatures when entering the reduction reactor were set to 685°C, 900°C, 950°C, and 1000°C, respectively. The simulated gas had a composition of 97% H2 and 3% H2O when fed to the reactor. In this case, the output material temperatures were 810°C, 820°C, 660°C, and 642°C, respectively, and the spent reduction gas temperatures were 810°C, 821°C, 660°C, and 642°C, respectively. With these optimized parameters, the reduced material metallization rate was calculated to be 94%.

[0069] The parameter values ​​used in Test 2, a pellet feed temperature of 800° C. and a reduction gas temperature of 900° C. as fed to the reactor, are expected to provide both an isothermal or near isothermal reduction process as discussed above and a low level of low temperature decay. The parameter values ​​used in the other tests will provide satisfactory reduced material metallization levels, but may not provide the same high yields or high reduction rates as can be obtained with the parameter values ​​used in Test 2.

Claims

1. 1. A process for the reduction of iron ore material to reduced iron material, comprising the steps of: Providing (100) a reduction reactor (1); (101) feeding iron ore material into the reduction reactor (1) at a top (1a) of the reduction reactor (1) to create a gravity flow of the iron ore material in the reduction reactor axially downward from the top (1a) to a bottom (1b) of the reduction reactor (1); Supplying (102) a heated reduction gas to the reduction reactor (1) at the top (1 a) of the reduction reactor such that the reduced gas creates a co-current flow with the gravity flow of the material in the reduction reactor (1); reducing the iron ore material into reduced iron material in the reduction reactor by the reducing gas (103); removing (104) spent reduction gas from the reduction reactor at a gas outlet (13) in the lower section (1c) of the reduction reactor; removing (105) reduced iron material from the reduction reactor at the bottom (1b) of the reduction reactor; The process includes:

2. 2. The process of claim 1, wherein the iron ore material as fed to the reduction reactor (1) has a temperature of from 0 to 1300°C.

3. The process according to claim 1 or 2, wherein the reducing gas as fed to the reduction reactor (1) has a temperature of 500 to 1000°C.

4. 4. The process according to any of claims 1 to 3, wherein the temperature of the spent reducing gas withdrawn from the reduction reactor (1) is at least 600°C and the temperature of the reduced iron material withdrawn from the reduction reactor (1) is at least 600°C.

5. 5. The process of claim 1, wherein the reduction gas supplied to the reduction reactor comprises 90% or more hydrogen by volume.

6. 6. The process of any of claims 1 to 5, wherein the iron ore material is reduced (103) to ferrous material in the reduction reactor in an isothermal or near isothermal reduction process.

7. 7. The process according to any one of claims 1 to 6, wherein dry crushed solids are separated (104b) from the spent reduction gas removed (104) from the reduction reactor (1) and re-introduced (104c) into the reduction reactor (1) at a crushed solids inlet (20) located at a point below the gas outlet (13) of the reduction reactor (1) as viewed in the direction of gravity flow of the material in the reduction reactor (1).

8. A reduction reactor (1) for the reduction of iron ore material to reduced iron material, comprising: a material inlet (11) located at the top (1a) of the reduction reactor and configured to feed iron ore material to the reduction reactor; a gas inlet (12) arranged at the top (1a) of the reduction reactor (1) and configured for supplying heated reducing gas to the reduction reactor, the reduction reactor (1), the material inlet (11) and the gas inlet (12) being arranged such that the material supplied through the material inlet and the reducing gas supplied through the gas inlet create a co-flow from the top (1a) axially downwards to the bottom (1b) of the reduction reactor (1) such that the iron ore material is reduced in the reduction reactor; a gas outlet (13) arranged in the lower section (1c) of the reduction reactor (1) and configured to remove spent reduction gas from the reduction reactor (1); a material outlet (14) arranged at the bottom (1b) of the reduction reactor (1) and configured for removing reduced iron material from the reduction reactor (1); A reduction reactor (1).

9. 9. The reduction reactor (1) according to claim 8, further comprising a separator (15) arranged at / after said gas outlet (13) for separating dry crushed solids from said spent reduction gas.

10. 10. The reduction reactor (1) of claim 9, further comprising a solids recycler (16) arranged in communication with the separator (15) and arranged to reinject dry crushed solids separated from the spent reduction gas into the reduction reactor (1) at a crushed solids inlet (20) arranged at a point below the gas outlet (13) as viewed in the direction of gravity flow of the material in the reduction reactor (1).