Viscosity index improvers for lubricants based on polyisobutylene acrylamide comb copolymers
The synthesis of a comb copolymer with PIB macromonomers and hydrophobic monomers addresses inefficiencies in existing methods, resulting in improved lubricant viscosity index and shear stability.
Patent Information
- Application Number
- JP2024533235
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2022-11-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for synthesizing polyisobutylene-based macromonomers and comb polymers are inefficient, requiring high temperatures, catalyst removal, and result in by-products, leading to poor rheological behavior and viscosity issues in lubricants.
A comb copolymer containing up to 40% by weight of PIB macromonomers and hydrophobic monomers, synthesized through a method involving polyisobutenamine reaction with (meth)acrylic anhydride, followed by hydrolysis, to improve lubricant viscosity index and stability.
The comb copolymer enhances lubricant viscosity index, exhibits good rheological behavior, and provides high shear stability with low viscosity loss, improving lubricant performance in extreme temperature conditions.
Smart Images

Figure 2024545438000001 
Figure 2024545438000002 
Figure 2024545438000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a comb copolymer comprising up to 40% by weight of a PIB macromonomer of formula (I) and a hydrophobic monomer of formula (II) in polymerized form. The present invention further relates to a process for preparing the PIB macromonomer of formula (I) by reacting a polyisobutene amine of formula (IV) with (meth)acrylic anhydride; a lubricant comprising a base oil, a comb copolymer, and further lubricant additives; and the use of the comb copolymer for improving the viscosity index of a lubricant. Combinations of the preferred embodiments with other preferred embodiments are within the scope of the present invention. [Background technology]
[0002] Comb polymers are useful additives for lubricants. Polyisobutylene (PIB) based macromonomers are useful comonomers in comb polymers. However, they are difficult to synthesize.
[0003] WO 2007 / 003238 discloses the synthesis of macromonomers by aminolysis of methyl methacrylate with polyisobutylene amines. This method has the disadvantages of requiring high temperatures, the need to remove the catalyst by phase separation, traces of catalyst end up as by-products in the final product, Michael addition by-products of amines to methacrylated double bonds may form, and large amounts of stabilizers are required to inhibit the polymerization of methacrylates. Summary of the Invention [Problem to be solved by the invention]
[0004] The objective was to overcome the above mentioned drawbacks and to find an improved synthesis of macromonomers and comb polymers, as well as to find improved lubricants containing comb polymers. A further objective is to improve lubricants containing polymers, which have good rheological behavior, low polymer treat rates, high viscosity index, easy handling of pure polymer solutions, good low temperature performance (e.g. in low temperature crankcase simulation), low viscosity under operating conditions (e.g. high temperature high shear HTHS viscosity test), high shear stability, or low viscosity loss after many use cycles. [Means for solving the problem]
[0005] The purpose of this is to (A) up to 40% by weight of formula (I) [ka] [In the formula, R 1 is H or methyl, and n is a number from 5 to 100. and (B) Formula (II) H2C=C(R 1 )COOR 2 (II) [In the formula, R 1 is H or methyl, and R 2 is C 5~36 is alkyl] This problem was solved by a comb copolymer which contains in polymerized form a hydrophobic monomer.
[0006] R 1 R may be H or methyl, with methyl being preferred. 1 may be different or identical in formulas (I), (II) and (III).
[0007] The subscript n may be a number from 5 to 100, preferably from 10 to 80, and in particular from 15 to 65.
[0008] The PIB macromonomer may have a molecular weight of 300 to 10,000 g / mol, preferably 400 to 5000 g / mol, in particular 800 to 2500 g / mol.
[0009] The molecular weight of the PIB macromonomer can be determined by GPC using polystyrene standards (eg, DIN 55672-1).
[0010] The synthesis of PIB macromonomers is known from WO 2007 / 003238.
[0011] The comb copolymer may contain up to 40% by weight, preferably up to 35% by weight, in particular up to 30% by weight, of PIB macromonomer.
[0012] Typically, the comb copolymer comprises 5 to 30% by weight of PIB macromonomer, preferably 10 to 30% by weight, in particular 15 to 25% by weight.
[0013] The weight percent of a monomer generally refers to the weight percent based on the weight of all monomers in the comb copolymer. The sum of all weight percents of all monomers (e.g., PIB macromonomer, hydrophobic monomer, and hydrophilic monomer) in the comb copolymer generally equals 100 weight percent.
[0014] R in hydrophobic monomers 2 may be linear, branched or cyclic alkyl, preferably linear or branched alkyl, especially branched alkyl.
[0015] Suitable R 2is pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl, 2-tetradecyloctydecyl, or mixtures thereof.
[0016] R 2 is preferably hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl or mixtures thereof.
[0017] R 2 is preferably C 6~12 Alkyl, especially C 6~10 In a preferred embodiment, R 2 is linear or branched C 6~12 In another preferred embodiment, R 2 is branch C 6~10 In another preferred embodiment, R 2 is 2-ethylhexyl or 2-propylheptyl, in particular 2-ethylhexyl. In another preferred embodiment, the hydrophobic monomer is 2-ethylhexyl methacrylate.
[0018] In another preferred embodiment, R 2 is C 6~24 Alkyl, especially C 6~20 In another preferred embodiment, R 2 is linear or branched C 6~24 It is an alkyl.
[0019] In another preferred embodiment, R 2is pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl, or 2-tetradecyloctydecyl. 5~36 It is a mixture of alkyls.
[0020] In another preferred embodiment, R 2 is C 5~36 It is a mixture of at least two of the alkyl groups.
[0021] In another preferred embodiment, R 2 is a mixture of at least two (in particular two or three) residues selected from the group consisting of pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl and 2-tetradecyloctydecyl.
[0022] In another preferred embodiment, R 2 is a mixture of at least two (in particular two or three) residues selected from the group consisting of hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl and nonadecyl.
[0023] In another preferred embodiment, R 2 is C 6~10It is a mixture of alkyl and residues selected from stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl, and 2-tetradecyloctydecyl.
[0024] The comb copolymer may comprise at least 30% by weight, preferably at least 40% by weight, in particular at least 50% by weight, of hydrophobic monomers.
[0025] The comb copolymer may contain up to 85% by weight, preferably up to 80% by weight, in particular up to 75% by weight, of hydrophobic monomers.
[0026] Typically, the comb copolymer comprises 40 to 90% by weight, preferably 50 to 85% by weight, in particular 60 to 80% by weight, of hydrophobic monomers.
[0027] The comb copolymer has the formula (III) H2C=C(R 1 )COOR 3 (III) (In the formula, R 3 is C 1~4 (It is alkyl) The hydrophilic monomer may further comprise a hydrophilic monomer.
[0028] Suitable R 3 R is methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, tert-butyl, or a mixture thereof. 3 is preferably methyl, ethyl, or n-butyl, and particularly preferably methyl. In another preferred embodiment, the hydrophilic monomer is methyl methacrylate.
[0029] The comb copolymer may comprise at least 1% by weight, preferably at least 3% by weight, in particular at least 5% by weight, of hydrophilic monomers.
[0030] The comb copolymer may contain up to 30% by weight, preferably up to 20% by weight, in particular up to 15% by weight, of hydrophilic monomers.
[0031] Typically, the comb copolymer comprises from 1 to 25% by weight, preferably from 3 to 20% by weight, in particular from 5 to 15% by weight, of hydrophilic monomers.
[0032] The comb copolymer may comprise further monomers different from the PIB macromonomer, the hydrophobic monomer or the hydrophilic monomer. - Hydroxyl-functional, epoxy-functional, or amino-functional (meth)acrylates - vinyl aromatic compounds such as styrene, α-methylstyrene, vinyltoluene or p-(tert-butyl)styrene; - acrylic and methacrylic acid; - acrylamide and methacrylamide; - maleic acid and its imides and C1-C10-alkyl esters; - fumaric acid and its imides and C1-C10-alkyl esters; - itaconic acid and its imides and C1-C10-alkyl esters; - Acrylonitrile and Methacrylonitrile is available.
[0033] The comb copolymer may comprise up to 15% by weight, preferably up to 5% by weight, in particular up to 1% by weight, of further monomers. In an alternative embodiment, the comb copolymer does not comprise further monomers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] In a preferred embodiment, the comb copolymer comprises - 5 to 35% by weight of PIB macromonomer; - 40 to 95% by weight of a hydrophobic monomer; - 1 to 30% by weight of a hydrophilic monomer; Including, The sum of all monomers is 100% by weight.
[0035] In another preferred form, the comb copolymer is - 5 to 35% by weight of PIB macromonomer; - 40 to 85% by weight of a hydrophobic monomer; - 5 to 30% by weight of a hydrophilic monomer; Including, The sum of all monomers is 100% by weight.
[0036] In another preferred form, the comb copolymer is - 5 to 30% by weight of PIB macromonomer; - 50 to 95% by weight of a hydrophobic monomer; - 1 to 25% by weight of a hydrophilic monomer; Including, The sum of all monomers is 100% by weight.
[0037] In another preferred form, the comb copolymer is - 10 to 30% by weight of PIB macromonomer, - 50 to 80% by weight of a hydrophobic monomer; - 3 to 20% by weight of a hydrophilic monomer; Including, The sum of all monomers is 100% by weight.
[0038] In another preferred form, the comb copolymer is - 10 to 30% by weight of PIB macromonomer, - 60 to 85% by weight of a hydrophobic monomer; - 5 to 15% by weight of a hydrophilic monomer; Including, The sum of all monomers is 100% by weight.
[0039] The comb copolymers may have a molecular weight Mn of 10,000 to 1,500,000 g / mol, preferably of 20,000 to 1,000,000 g / mol and in particular of 50,000 to 200,000 g / mol.
[0040] The comb copolymers may have a molecular weight Mw of 50,000 to 2,000,000 g / mol, preferably of 100,000 to 1,000,000 g / mol and in particular of 200,000 to 600,000 g / mol.
[0041] The comb copolymer may have a polydispersity index (PDI) of 1.5 to 5.0, preferably 2.0 to 4.5, in particular 2.9 to 4.1.
[0042] The molecular weight of the comb copolymers can be determined by GPC using polystyrene standards (eg DIN 55672-1).
[0043] The kinematic viscosity (KV100, typically measured using a Brookfield viscometer) of the comb copolymer at 100° C. in a 30% by weight solution of base oil (e.g., Nexbase® 3030) is 2 / s, preferably less than 300 mm 2 / s or less, especially 150 mm 2 / s.
[0044] The comb copolymers can be prepared by conventional free radical polymerization, such as bulk or solution polymerization, with solution polymerization being preferred.
[0045] In solution polymerization, the reaction mixture may include a diluent, monomers, a polymerization initiator, and optionally a chain transfer agent and optionally a crosslinking agent. The diluent may be any inert hydrocarbon. The concentration of all monomers may range from about 30 to 100%. As used herein, "total monomer charge" refers to the combined amount of all monomers in the initial reaction mixture.
[0046] The diluent may be any inert hydrocarbon or may be a dicarboxylic acid ester, which is a diester of at least one linear or branched C2-C20 dicarboxylic acid and at least one linear or branched C1-C20 monoalcohol. The dicarboxylic acid ester is preferably derived from the reaction of a dicarboxylic acid with an aliphatic alcohol. Preferred dicarboxylic acids are adipic acid, pimelic acid, suberic acid, azelaic acid and sebacic acid and mixtures thereof. The dicarboxylic acid ester component is preferably formed from such a dicarboxylic acid by esterification with a linear or branched medium-sized aliphatic alcohol, preferably a C5-C20 alcohol, more preferably a C9-C15 aliphatic alcohol, most preferably nonanol, isodecanol, isotridecanol, and 2s-propylheptanol. The diluent is preferably di-(2-propylheptyl)-adipate or diisononyl adipate, especially di-(2-propylheptyl)-adipate.
[0047] The comb copolymer is preferably present in a diluent which is a dicarboxylic acid ester, preferably a diester of at least one linear or branched C2-C20 dicarboxylic acid and at least one linear or branched C1-C20 monoalcohol, in particular di-(2-propylheptyl)-adipate.
[0048] Suitable polymerization initiators include initiators that dissociate upon heating to generate free radicals, such as peroxide compounds such as benzoyl peroxide, t-butyl perbenzoate, t-butyl peroctoate, and cumene hydroperoxide; and azo compounds such as azoisobutyronitrile and 2,2'-azobis(2-methylbutanenitrile). The mixture contains about 0.001% to about 5.0% by weight of the initiator based on the total monomer mixture. For example, 0.02% to about 4.0% by weight, 0.02% to about 3.5% by weight is assumed. Usually, about 0.02% to about 2.0% by weight is used.
[0049] Suitable chain transfer agents include mercaptans and alcohols. For example, tridecyl mercaptan, dodecyl mercaptan, and ethyl mercaptan may be used as chain transfer agents, as well as difunctional mercaptans such as hexanedithiol. The amount of chain transfer agent used is selected based on the desired molecular weight of the polymer being synthesized. Chain transfer agents are often added to the reaction mixture or monomer feed in amounts of 0.001 to 3% by weight based on the monomer mixture.
[0050] The polymerization reaction may be carried out by charging all of the ingredients into a reaction vessel equipped with a stirrer, thermometer, and reflux condenser and heating with stirring under a nitrogen blanket to a temperature of about 50° C. to about 125° C. for about 0.5 hours to about 15 hours.
[0051] The present invention also relates to a compound of formula (I) [ka] [In the formula, R 1 is H or methyl, and n is a number from 5 to 100. A method for preparing a PIB macromonomer of the formula: Formula (IV) [ka] The present invention also relates to a process in which polyisobutene amines (also called PIB-amines) of the formula (I) are reacted with (meth)acrylic anhydride.
[0052] Polyisobutyleneamines can be prepared, for example, as described in EP 0244616 and are commercially available. The PIB-amines may have a molecular weight of 300 to 10,000 g / mol, preferably 400 to 5000 g / mol, in particular 800 to 2500 g / mol. The index n in the PIB-amines is generally the same as in the PIB macromonomers, for example it may be a number between 5 and 100, preferably between 10 and 80, in particular between 15 and 65.
[0053] Preferably, the PIB-amine is reacted with methacrylic anhydride.
[0054] A typical reaction scheme for the reaction of PIB-amine with methacrylic anhydride is: [ka] It is.
[0055] The (meth)acrylic anhydride is preferably present in a molar excess relative to the polyisobutene amine, such as at least a 1.1-fold, 1.5-fold or 2-fold molar excess.
[0056] The reaction of the PIB-amine with meth)acrylic anhydride is generally followed by hydrolysis of the remaining (meth)acrylic anhydride to form (meth)acrylic acid, which can be removed by distillation or by extraction with water.
[0057] The reaction between PIB-amine and (meth)acrylic anhydride can be carried out at a reaction temperature in the range of 0 to -50°C, preferably 10 to -40°C.
[0058] The reaction of the PIB-amine with the meth)acrylic anhydride can be carried out in an organic solvent, such as a hydrocarbon solvent.
[0059] The present invention also provides (i) a base oil; (ii) a comb copolymer or a comb copolymer obtainable by the process according to the invention, (iii) further lubricant additives; The present invention also relates to a lubricant comprising:
[0060] The lubricant may comprise at least 0.1% by weight, preferably at least 0.5% by weight, especially at least 1% by weight, of the comb copolymer. In another embodiment, the lubricant may comprise 0.1 to 20% by weight, preferably 0.1 to 150% by weight, especially at least 0.1 to 10% by weight of the comb copolymer.
[0061] The lubricant may comprise at least 30% by weight, preferably at least 50% by weight, especially at least 70% by weight of base oil. The lubricant may comprise from 30 to 99.9% by weight, preferably from 50 to 99% by weight, especially from 70 to 95% by weight of base oil.
[0062] The lubricant may be present in an amount of up to 20% by weight, preferably up to 15% by weight, particularly It may contain up to 10% by weight of further lubricant additives.
[0063] A lubricant generally refers to a composition capable of reducing friction between surfaces (preferably metal surfaces), such as the surfaces of a mechanical device. A mechanical device may be a mechanism consisting of a device that operates on a mechanical principle. Suitable mechanical devices are bearings, gears, joints, and guidance. The mechanical device may operate at temperatures ranging from -30C to 80C. A lubricant is generally a lubricating liquid, a lubricating oil, or a lubricating grease.
[0064] Lubricants are typically specially formulated for almost any type of machine and manufacturing process. The type and concentration of base oil and / or lubricant additives used in these lubricants can be selected based on the requirements of the machine or process being lubricated, the qualities required by the machine manufacturer or user, and government regulations. Typically, each lubricant has a unique set of performance requirements. In addition to properly lubricating the machine or process, these requirements include maintaining the quality of the lubricant itself, as well as the impact of lubricant use and disposal on energy use, environmental quality, and the health of users.
[0065] Typical lubricants are automotive lubricants (e.g., gasoline engine oils, diesel engine oils, gas engine oils, gas turbine oils, automatic transmission fluids, gear oils) and industrial lubricants (e.g., industrial gear oils, air tool lubricants, high temperature oils, gas compressor oils, hydraulic fluids, metal working fluids).
[0066] Examples of lubricants include accelerator lubrication, medium and heavy duty engine oils, industrial engine oils, marine engine oils, automotive engine oils, crankshaft oils, compressor oils, refrigeration oils, hydrocarbon compressor oils, ultra-low temperature lubricating oils, high temperature lubricating oils, wire rope lubricants, textile machine oils, refrigeration oils, aviation and space lubricants, aviation turbine oils, transmission oils, gas turbine oils, spindle oils, spin oils, traction fluids, transmission oils, plastic transmission oils, passenger car transmission oils, truck transmission oils, industrial transmission oils, industrial gear oils, insulating oils, precision machinery oils, brake fluids, transmission fluids, shock absorber oils, heat distribution medium oils, transformer oils, fats, chain oils, minimum quantity lubricants for metalworking operations, oils for hot and cold operations, oils for water-based metalworking fluids, oils for neat oil metalworking fluids, oils for semi-synthetic metalworking fluids, oils for synthetic metalworking fluids, drilling cleaners for soil exploration, hydraulic oils, biodegradable lubricants or lubricating greases or waxes, oils for chainsaws, mold release agents, molding fluids, gun, pistol and rifle lubricants or watch lubricants, and food grade approved lubricants.
[0067] The lubricant will generally have a thermal stability of at least 10, 50, 100, 150, 200, 300, 400, 500, 600, 900, 1400, or 2000 mm at 40°C. 2 In another embodiment, the lubricant may have a kinematic viscosity of 200 to 30,000 mm / s at 40° C. 2 / s (cSt), preferably 500 to 10,000 mm 2 / s, especially 1000~5000mm 2 / s.
[0068] The lubricant will generally have a melting point of at least 2, 3, 5, 10, 20, 30, 40, or 50 mm at 100°C. 2 In another embodiment, the lubricant has a kinematic viscosity of 10 to 5000 mm / s at 100° C. 2 / s (cSt), preferably 30 to 3000 mm 2 / s, especially 50~2000mm 2 / s.
[0069] The lubricant may have a viscosity index (VI) of at least 150, 160, 170, 180, 190 or 200.
[0070] The base oil may be selected from the group consisting of mineral oils (Group I, II or III oils), polyalphaolefins (Group IV oils), polymerized and interpolymerized olefins, alkylnaphthalenes, alkylene oxide polymers, silicone oils, phosphate esters and carboxylate esters (Group V oils). The base oil is preferably selected from Group I, Group II, Group III base oils, or mixtures thereof, according to the API definition. The definition of base oil is the same as that found in the American Petroleum Institute (API) publication "Engine Oil Licensing and Certification System", Industry Services Department, Fourteenth Edition, December 1996, Addendum 1, December 1998. The said publication classifies base oils as follows: a) Group I base oils contain less than 90% saturates (ASTM D 2007) and / or greater than 0.03% sulfur (ASTM D 2622) and have a viscosity index greater than or equal to 80 and less than 120 (ASTM D 2270). b) Group II base oils contain greater than or equal to 90% saturates and less than or equal to 0.03% sulfur and have a viscosity index greater than or equal to 80 and less than 120. c) Group III base oils contain greater than or equal to 90 percent saturates and less than or equal to 0.03 percent sulfur and have a viscosity index greater than or equal to 120. d) Group IV base oils contain polyalphaolefins. Polyalphaolefins (PAOs) include known PAO materials that typically comprise hydrogenated polymers or oligomers of relatively low molecular weight alphaolefins, including but not limited to C8 to about C16 alphaolefins, preferably C2 to about C32 alphaolefins, such as 1-octene, 1-decene, 1-dodecene, etc. Preferred polyalphaolefins are poly-1-octene, poly-1-decene, and poly-1-dodecene. e) Group V base oils include any base oil not described by Groups I-IV. Examples of Group V base oils include alkyl naphthalenes, alkylene oxide polymers, silicone oils, and phosphate esters.
[0071] Synthetic base oils include hydrocarbon oils and halo-substituted hydrocarbon oils, such as polymerized and copolymerized olefins (e.g., polypropylene, propylene-isobutylene copolymers, chlorinated polybutylene, poly(1-hexene), poly(1-octene), poly(1-decene)); alkylbenzenes (e.g., dodecylbenzene, tetradecylbenzene, dinonylbenzene, di(2-ethylhexyl)benzene); polyphenyls (e.g., biphenyls, terphenyls, alkylated polyphenols); and alkylated diphenyl ethers and alkylated diphenyl sulfides and their derivatives, analogs and congeners.
[0072] Alkylene oxide polymers and copolymers and their derivatives in which the terminal hydroxyl groups have been modified by esterification, etherification, etc., constitute another class of known synthetic base oils. These are exemplified by polyoxyalkylene polymers prepared by polymerization of ethylene oxide or propylene oxide and alkyl and aryl ethers of polyoxyalkylene polymers (e.g., methyl-polyisopropylene glycol ether having a molecular weight of 1000 or diphenyl ethers of polyethylene glycols having a molecular weight of 1000-1500); and their mono- and polycarboxylic acid esters, e.g., acetate esters, mixed C3-C8 fatty acid esters, and C13 oxo acid diesters of tetraethylene glycol.
[0073] Silicone-based oils and silicate oils, such as polyalkyl-, polyaryl-, polyalkoxy- or polyaryloxy silicone oils, comprise another useful class of synthetic base oils; such base oils include tetra-ethyl silicate, tetraisopropyl silicate, tetra-(2-ethylhexyl) silicate, tetra-(4-methyl-2-ethylhexyl) silicate, tetra-(p-tert-butyl-phenyl) silicate, hexa-(4-methyl-2-ethylhexyl) disiloxane, poly(methyl) siloxane and poly(methylphenyl) siloxane. Other synthetic base oils include liquid esters of phosphorus-containing acids (e.g., tricresyl phosphate, trioctyl phosphate, diethyl ester of decylphosphonic acid) and polymeric tetrahydrofurans.
[0074] Suitable lubricant additives may be selected from viscosity index improvers, polymeric thickeners, antioxidants, corrosion inhibitors, detergents, dispersants, antifoam agents, dyes, anti-wear additives, extreme pressure additives (EP additives), anti-wear additives (AW additives), friction modifiers, metal deactivators, pour point depressants.
[0075] Viscosity index improvers include polymers of high molecular weight that increase the relative viscosity of oil at high temperatures compared to low temperatures. Viscosity index improvers include polyacrylates, polymethacrylates, alkyl methacrylates, vinylpyrrolidone / methacrylate copolymers, polyvinylpyrrolidones, polybutenes, olefin copolymers such as ethylene-propylene copolymers or styrene-butadiene copolymers or polyalkenes such as PIB, styrene / acrylate copolymers and polyethers, and combinations thereof. The most common VI improvers are methacrylate polymers and copolymers, acrylate polymers, olefin polymers and copolymers, and styrene-butadiene copolymers. Other examples of viscosity index improvers include polymethacrylates, polyisobutylenes, α-olefin polymers, α-olefin copolymers (e.g., ethylene-propylene copolymers), polyalkylstyrenes, phenol condensates, naphthalene condensates, styrene-butadiene copolymers, and the like. Of these, preferred are polymethacrylates having a number average molecular weight of 10000 to 300000, and α-olefin polymers or α-olefin copolymers having a number average molecular weight of 1000 to 30000, in particular ethylene-α-olefin copolymers having a number average molecular weight of 1000 to 10000. The viscosity index improvers can be used individually or in the form of a mixture, conveniently added in an amount ranging from 0.05% by weight to 20.0% by weight, based on the weight of the base stock.
[0076] Suitable (polymeric) thickeners include, but are not limited to, polyisobutene (PIB), oligomeric copolymers (OCPs), polymethacrylates (PMAs), copolymers of styrene and butadiene, or high viscosity esters (complex esters).
[0077] Antioxidants include phenolic antioxidants, such as hindered phenolic antioxidants, or non-phenolic antioxidants.
[0078] Useful phenolic antioxidants include hindered phenols. These phenolic antioxidants may be ashless (metal-free) phenolic compounds or neutral or basic metal salts of certain phenolic compounds. Typical phenolic antioxidant compounds are hindered phenols that contain sterically hindered hydroxyl groups, including those derivatives of dihydroxyaryl compounds in which the hydroxyl groups are in the o- or p-position relative to each other. Typical phenolic antioxidants include hindered phenols substituted with alkyl groups having 6 or more carbon atoms and alkylene-linked derivatives of these hindered phenols. Examples of such phenolic materials include 2-t-butyl-4-heptylphenol; 2-t-butyl-4-octylphenol; 2-t-butyl-4-dodecylphenol; 2,6-di-t-butyl-4-heptylphenol; 2,6-di-t-butyl-4-dodecylphenol; 2-methyl-6-t-butyl-4-heptylphenol; and 2-methyl-6-t-butyl-4-dodecylphenol. Other useful hindered monophenolic antioxidants include, for example, hindered 2,6-di-alkyl-phenolic propionate derivatives. Bisphenolic antioxidants can also be used in combination with the present invention. Examples of ortho-linked phenols include 2,2'-bis(4-heptyl-6-t-butyl-phenol); 2,2'-bis(4-octyl-6-t-butyl-phenol); and 2,2'-bis(4-dodecyl-6-t-butyl-phenol). Examples of para-linked bisphenols include, for example, 4,4'-bis(2,6-di-t-butylphenol) and 4,4'-methylene-bis(2,6-di-t-butylphenol).
[0079] Non-phenolic antioxidants that can be used include aromatic amine antioxidants, which may be used by themselves or in combination with phenols. Typical examples of non-phenolic antioxidants include those represented by the formula R 8 R 9 R 10and alkylated and non-alkylated aromatic amines, such as aromatic monoamines of N, where R 8 is an aliphatic, aromatic or substituted aromatic group; R 9 is an aromatic or substituted aromatic group, R 10 is H, alkyl, aryl, or R 11 S(O)xR 12 (In the formula, R 11 is an alkylene, alkenylene, or aralkylene group; R 12 is a higher alkyl group, or an alkenyl, aryl, or alkaryl group, and x is 0, 1, or 2. 8 may contain from 1 to about 20 carbon atoms, preferably from about 6 to 12 carbon atoms. The aliphatic group is a saturated aliphatic group. Preferably, R 8 and R 9 Both of the aromatic groups R and R are aromatic or substituted aromatic groups, and the aromatic groups may be fused ring aromatic groups such as naphthyl. 8 and R 9 may be linked together with other groups such as S.
[0080] Typical aromatic amine antioxidants have an alkyl substituent of at least about 6 carbon atoms. Examples of aliphatic groups include hexyl, heptyl, octyl, nonyl, and decyl. Generally, the aliphatic groups do not contain more than about 14 carbon atoms. General types of amine antioxidants useful in the present compositions include diphenylamines, phenylnaphthylamines, phenothiazines, imidodibenzyl, and diphenylphenylenediamines. Mixtures of two or more aromatic amines are also useful. Polymeric amine antioxidants can also be used. Specific examples of aromatic amine antioxidants useful in the present invention include: p,p'-Dioctyldiphenylamine; t-Octylphenyl-α-naphthylamine; Phenyl-α-naphthylamine; and p-Octylphenyl-α-naphthylamine Sulfurized alkylphenols and their alkali metal or alkaline earth metal salts are also useful antioxidants.
[0081] Corrosion inhibitors can include a variety of oxygen-, nitrogen-, sulfur-, and phosphorus-containing materials, as well as metal-containing compounds (salts, organometallics, etc.) and non-metal-containing or ashless materials. Corrosion inhibitors can include a variety of additive types, such as hydrocarbyl-, aryl-, alkyl-, arylalkyl-, and alkylaryl-type detergents (neutral, overbased), sulfonates, phenates, salicylates, alcoholates, carboxylates, salixarates, phosphites, phosphates, thiophosphates, amines, amine salts, amine phosphates, amine sulfonates, alkoxylated amines, ether amines, polyether amines, amides, imides, azoles, diazoles, triazoles, benzotri ... These may include, but are not limited to, thiadiazoles, mercapto-benzothiazoles, tolyltriazoles (TTZ type), heterocyclic amines, heterocyclic sulfides, thiazoles, thiadiazoles, mercaptothiadiazoles, dimercaptothiadiazoles (DMTD type), imidazoles, benzimidazoles, dithiobenzimidazoles, imidazolines, oxazolines, Mannich reaction products, glycidyl ethers, anhydrides, carbamates, thiocarbamates, dithiocarbamates, polyglycols, and the like, or mixtures thereof.
[0082] Detergents include detergents that adhere to dirt particles and prevent dirt from adhering to critical surfaces. Detergents can also adhere to the metal surface itself to keep the metal surface clean and prevent corrosion from occurring. Detergents include calcium alkyl salicylates, calcium alkyl phenates, and calcium alkaryl sulfonates, including those that substitute for metal ions such as magnesium, barium, or sodium. Examples of detergents and dispersants that can be used include metal-based detergents such as neutral and basic alkaline earth metal sulfonates, alkaline earth metal phenates, and alkaline earth metal salicylates, alkenyl succinimides and alkenyl-succinimide esters and their borohydrides, phenates, salienius complex detergents, and ashless dispersants modified with sulfur compounds. These agents may be added and used individually or in the form of mixtures, conveniently in amounts ranging from 0.01% or more to 1.0% or less by weight based on the weight of the base stock; they may also be high total base number (TBN), low TBN, or high / low TBN mixtures.
[0083] Dispersants are lubrication additives that help prevent the formation of sludge, varnish, and other deposits on critical surfaces. Dispersants may be succinimide dispersants (e.g., N-substituted long chain alkenyl succinimides), Mannich dispersants, ester-containing dispersants, condensation products of fatty hydrocarbyl monocarboxylic acylating agents with amines or ammonia, alkylaminophenol dispersants, hydrocarbyl-amine dispersants, polyether dispersants, or polyetheramine dispersants. In one embodiment, the succinimide dispersants include polyisobutylene-substituted succinimides, where the polyisobutylene from which the dispersant is derived can have a number average molecular weight of about 400 to about 5000, or about 950 to about 1600. In one embodiment, the dispersants include borated dispersants. Typically, borated dispersants include succinimide dispersants that include polyisobutylene succinimides, where the polyisobutylene from which the dispersant is derived can have a number average molecular weight of about 400 to about 5000. Borated dispersants are described in more detail above in the discussion of extreme pressure agents.
[0084] The antifoaming agent may be selected from silicones, polyacrylates, and the like. The amount of antifoaming agent in the lubricant compositions described herein may range from 0.001% by weight or more to 0.1% by weight or less, based on the total weight of the formulation. As a further example, the antifoaming agent may be present in an amount of about 0.004% by weight to about 0.008% by weight.
[0085] Suitable extreme pressure agents are sulfur-containing compounds. In one embodiment, the sulfur-containing compound may be a sulfurized olefin, polysulfide, or a mixture thereof. Examples of sulfurized olefins include sulfurized olefins derived from propylene, isobutylene, pentene; organic sulfides and / or polysulfides including benzyl disulfide; bis-(chlorobenzyl) disulfide; dibutyl tetrasulfide; di-tert-butyl polysulfide; and sulfurized methyl ester of oleic acid, sulfurized alkylphenols, sulfurized dipentenes, sulfurized terpenes, sulfurized Diels-Alder adducts, alkylsulfenyl N'N-dialkyldithiocarbamates; or mixtures thereof. In one embodiment, the sulfurized olefins include sulfurized olefins derived from propylene, isobutylene, pentene, or mixtures thereof. In one embodiment, the sulfur-containing compound of the extreme pressure additive includes dimercaptothiadiazole or derivative, or mixtures thereof. Examples of dimercaptothiadiazoles include compounds such as 2,5-dimercapto-1,3,4-thiadiazole or hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazoles, or oligomers thereof. Hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazole oligomers are usually formed by forming sulfur-sulfur bonds between 2,5-dimercapto-1,3,4-thiadiazole units to form derivatives or oligomers of two or more of the thiadiazole units. Suitable 2,5-dimercapto-1,3,4-thiadiazole-derived compounds include, for example, 2,5-bis(tert-nonyldithio)-1,3,4-thiadiazole or 2-tert-nonyldithio-5-mercapto-1,3,4-thiadiazole. The number of carbon atoms on the hydrocarbyl substituent of the hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazole typically comprises 1 to 30, or 2 to 20, or 3 to 16. The extreme pressure additives include compounds containing boron and / or sulfur and / or phosphorus. The extreme pressure agent may be present in the lubricant composition at 0% to about 20%, or about 0.05% to about 10.0%, or about 0.1% to about 8% by weight of the lubricant composition.
[0086] Examples of anti-wear additives include organic borates, organic phosphites such as didodecyl phosphite, organic sulfur-containing compounds such as sulfurized sperm oil or sulfurized terpenes, zinc dialkyldithiophosphates, zinc diaryldithiophosphates, phosphosulfurized hydrocarbons, and any combination thereof.
[0087] Friction modifiers can include metal-containing compounds or materials, as well as ashless compounds or materials, or mixtures thereof. Metal-containing friction modifiers include metal salts or metal-ligand complexes, where the metal can include alkali metals, alkaline earth metals, or transition group metals. Such metal-containing friction modifiers may have low ash characteristics. Transition metals can include Mo, Sb, Sn, Fe, Cu, Zn, and the like. Ligands can include alcohols, polyols, glycerol, partial ester glycerol, thiols, carboxylates, carbamates, thiocarbamates, dithiocarbamates, phosphates, thiophosphates, dithiophosphates, amides, imides, amines, thiazoles, thiadiazoles, dithiazoles, diazoles, triazoles, and other polar molecular functional groups containing effective amounts of O, N, S, or P, individually or in combination. Specifically, Mo-containing compounds, such as Mo-dithiocarbamate, Mo(DTC), Mo-dithiophosphate, Mo(DTP), Mo-amine, Mo(Am), Mo-alcoholate, Mo-alcohol-amide, and the like, may be particularly effective.
[0088] Ashless friction modifiers may also include lubricant materials containing effective amounts of polar groups, such as hydroxyl-containing hydrocarbyl base oils, glycerides, partial glycerides, glyceride derivatives, and the like. The polar groups of the friction modifiers may include hydrocarbyl groups containing effective amounts of O, N, S, or P, individually or in combination. Other friction modifiers that may be particularly effective include, for example, salts of fatty acids (both ash-containing and ashless derivatives), fatty alcohols, fatty amides, fatty esters, hydroxyl-containing carboxylates, and equivalent synthetic long-chain hydrocarbyl acids, alcohols, amides, esters, hydroxycarboxylates, and the like. In some cases, fatty organic acids, fatty amines, and sulfurized fatty acids may be used as suitable friction modifiers. Examples of friction modifiers include fatty acid esters and amides, organomolybdenum compounds, molybdenum dialkylthiocarbamates, and molybdenum dialkyldithiophosphates.
[0089] Suitable metal deactivators include benzotriazoles and their derivatives, such as 4- or 5-alkylbenzotriazoles (e.g., triazoles) and their derivatives, 4,5,6,7-tetrahydrobenzotriazole and 5,5′-methylenebisbenzotriazole; Mannich bases of benzotriazoles or triazoles, such as 1-[bis(2-ethylhexyl)aminomethyl)triazole and 1-[bis(2-ethylhexyl)aminomethyl)benzotriazole; and alkoxyalkylbenzotriazoles, such as 1-(nonyloxymethyl)benzotriazole, 1-(1-butoxyethyl)benzotriazole and 1-(1-cyclohexyloxybutyl)triazole, and combinations thereof. Additional non-limiting examples of the one or more metal deactivators include 1,2,4-triazole and its derivatives, such as 3-alkyl (or aryl)-1,2,4-triazoles, and Mannich bases of 1,2,4-triazoles, such as 1-[bis(2-ethylhexyl)aminomethyl-1,2,4-triazole; alkoxyalkyl-1,2,4-triazoles, such as 1-(1-butoxyethyl)-1,2,4-triazole; and acylated 3-amino-1,2,4-triazoles, imidazole derivatives, such as 4,4'-methylenebis(2-undecyl-5-methylimidazole) and bis[(N-methyl)imidazol-2-yl]carbinol octyl ether, and combinations thereof. Further non-limiting examples of the one or more metal deactivators include sulfur-containing heterocyclic compounds, such as 2-mercapto-benzothiazole, 2,5-dimercapto-1,3,4-thiadiazole and their derivatives; and 3,5-bis[di(2-ethylhexyl)aminomethyl]-1,3,4-thiadiazolin-2-one, and combinations thereof. Still further non-limiting examples of the one or more metal deactivators include amino compounds, such as salicylidene propylene diamine, salicylamino guanidine and their salts, and combinations thereof.The one or more metal deactivators are not particularly limited in amount in the composition, but are typically present in an amount of about 0.01 to about 0.1 wt%, about 0.05 to about 0.01 wt%, or about 0.07 to about 0.1 wt%, based on the weight of the composition. Alternatively, the one or more metal deactivators may be present in an amount less than about 0.1 wt%, less than about 0.7 wt%, or less than about 0.5 wt%, based on the weight of the composition.
[0090] Pour point depressants (PPDs) include polymethacrylates, alkylated naphthalene derivatives, and combinations thereof. Commonly used additives such as alkyl aromatic polymers and polymethacrylates are also useful for this purpose. Typically, treat rates range from 0.001% or more to 1.0% or less by weight based on the weight of the base stock.
[0091] Demulsifiers include trialkyl phosphates and various polymers and copolymers of ethylene glycol, ethylene oxide, propylene oxide, or mixtures thereof.
[0092] The present invention also relates to the use of a comb copolymer or a comb copolymer obtainable by the process according to the invention for improving the viscosity index of a lubricant. EXAMPLES
[0093] Example 1 - Macromonomer Polyisobutyleneamine (1006 g, Mn approx. 1000 g / mol, degree of functionalization 60-70%, 65 wt. % C 10 ~C 13A solution of n-paraffin with an amine value of 24.5 g KOH, 0.44 mol -NH2), 0.44 g butylhydroxytoluene BHT and 86.5 g (0.56 mol) methacrylic anhydride MAAh were mixed at room temperature. The progress of the reaction was followed by 1H-NMR. After 20 hours, when the conversion to the amide was quantitative, 300 g water was added and heated to 90 °C. The hydrolysis of the excess methacrylic anhydride was followed by 1H-NMR. After 15 hours, when the hydrolysis was quantitative, the reaction mixture was cooled to room temperature, the aqueous phase was separated, 1.13 g MeHQ was added and the excess water and MAA were removed under vacuum at a bath temperature of 80 °C. In addition, C 10 ~C 13 A portion of the n-paraffins was distilled off. The quantitative removal of traces of MAA was followed by 1H-NMR. 10 ~C 13 The macromonomer was dissolved in n-paraffin to obtain 833 g of an 80.8% solution.
[0094] Example 2 - Macromonomer The reaction was carried out as described in Example 1 with 1170 g of polyisobutyleneamine, 0.5 g of BHT and 96.6 g of MAAh. 300 g of water was added and after hydrolysis, the aqueous phase was separated as in Example 1. Then, 250 g of water and 50 g of aqueous NaOH (12.5% by weight) were added, mixed and, after settling, the aqueous phase was separated. The organic phase was washed twice with 300 g of water, after which 1.21 g of MeHQ was added. Quantitative extraction of methacrylic acid MAA was controlled by 1H-NMR. Residual water was removed under vacuum at a bath temperature of 80°C. C 10 ~C 13 The n-paraffin portion of C was also distilled off. 10 ~C 13 The macromonomer was dissolved in n-paraffin to obtain 915 g of an 85.6% solution.
[0095] Example 3 - Macromonomer The reaction was carried out as described in Example 1 with 1100 g of polyisobutyleneamine, 0.47 g of BHT and 93.4 g of MAAh. Then 250 g of water and 50 g of aqueous NaOH (12.5 wt%) were added and heated to 40-53°C, and the hydrolysis of the excess methacrylic anhydride was followed by 1H-NMR. After 4.5 hours, the hydrolysis was quantitative and the mixture was cooled to ambient temperature. The aqueous phase was separated and the organic phase was washed twice with 300 g of water, after which 1.13 g of MeHQ was added. The quantitative extraction of MAA was controlled by 1H-NMR. Residual water was removed by stepwise decreasing the vacuum at a bath temperature of 80°C. C 10 ~C 13 Some of the n-paraffins were also distilled off. 10 ~C 13 As a result, 896 g of the macromonomer was dissolved in n-paraffin to obtain an 82.2% solution.
[0096] Example 4 - Macromonomer The reaction was carried out as described in Example 1 with 557 g of polyisobutyleneamine, 0.24 g of BHT and 47.87 g of MAAh. 150 g of water was added and after hydrolysis, the aqueous phase was separated as in Example 1. Then, 125 g of water and 25 g of aqueous NaOH (12.5 wt%) were added and the aqueous phase was separated. The organic phase was washed twice with 150 g of water. The quantitative extraction of MAA was controlled by 1H-NMR. 100 g of cyclohexane was added to the organic phase. Cyclohexane and residual water were slowly removed under vacuum at a bath temperature of 60° C., while the vacuum was gradually reduced to finally obtain a water- and cyclohexane-free product solution. C 10 ~C 13 A part of the n-paraffins was distilled off. 10 ~C 13 As a result, 427 g of the macromonomer was dissolved in n-paraffin to obtain an 87.3% solution.
[0097] Example 5 – Polymerization Into the reactor: - 58.4 g of the macromonomer PIB amide from Example 2 (85.6 wt. % solution) - 175g EHMA 2-Ethylhexyl Methacrylate - 25g MMA methyl methacrylate - TDDM tert-dodecyl mercaptan 0.25g - 158g of Nexbase® 3030 Added.
[0098] The weight percentages of the monomers were: PIB amide 20 wt%, EHMA 70 wt%, MMA 10 wt%.
[0099] The mixture was heated to 95°C under N2 with stirring. Within 5 minutes immediately after reaching 95°C, 1 / 3 of the total solution of initiator tert-butyl-peroxyethylhexanoate TBPEH (total solution is 3 g TBPEH dissolved in 29.64 g Catenex T121), corresponding to a mass of 0.64 g TBPEH dissolved in 6.38 g Catenex T121, was added. The mixture was stirred for another 10 minutes. Then, 2 / 3 of the TBPEH solution was added in three portions over 3 hours: 1st portion = 1 g, 2nd portion = 2 g, 3rd portion: 2 g. The mixture was then treated at 95°C for 1 hour. Finally, 5.56 g of a 9% solution of TBPEH was added and the mixture was stirred at 95°C for another hour.
[0100] After 1 hour, 408.31 g of Nextbase® 3030 (a hydrogenated highly isoparaffinic hydrocarbon base stock from Neste) was added to bring the total polymer content to about 30%. The mixture was stirred for 30 minutes to ensure homogeneity.
[0101] Molecular weight determined by GPC using polystyrene calibration: Mn 106.000 g / mol, Mw 391.000 g / mol, PDI 3.7
[0102] The results of the application test were as follows: KV100: 245mm 2 / s (30% by weight polymer solution) KV40: 32.6mm 2 / s (5% by weight of a 30% by weight polymer solution) KV100: 7.2mm 2 / s (5% by weight of a 30% by weight polymer solution) VI:195 Pour point: -18℃
[0103] The kinematic viscosity at 100°C (KV100) of the lubricants was determined according to ASTM D445 / 446. The higher the viscosity index VI (DIN ISO 2909), the smaller the effect of temperature on the kinematic viscosity.
[0104] Example 6 - Polymerization Into the reactor: - 62.07 g of the macromonomer PIB amide from Example 4 - 163g EHMA 2-Ethylhexyl Methacrylate - 27.25g MMA methyl methacrylate - 27.25g LMA Lauryl Methacrylate - TDDM tert-dodecyl mercaptan 0.27g - 139.30g DPHA Di-(2-propylheptyl)adipate Added.
[0105] The weight percentages of the monomers were: PIB amide 20%, EHMA 60%, MMA 10%, LMA 10%.
[0106] The mixture was heated to 95°C under N2 with stirring. Within 5 minutes immediately after reaching 95°C, 1 / 3 of the total solution of initiator tert-butyl-peroxyethylhexanoate TBPEH (total solution is 0.7 g TBPEH dissolved in 6.95 g Catenex T121), corresponding to a mass of 0.25 g TBPEH dissolved in 2.27 g Catenex T121, was added. The mixture was stirred for another 10 minutes. Then, 2 / 3 of the TBPEH solution was added in three portions over 3 hours: 1st portion = 1 g, 2nd portion = 2 g, 3rd portion: 2 g. The mixture was then treated at 95°C for 1 hour. Finally, 6.06 g of a 9% solution of TBPEH was added and the mixture was stirred at 95°C for another hour.
[0107] After 1 hour, 480 g of di-(2-propylheptyl)adipate was added to bring the total polymer content to about 30%. The mixture was stirred for 30 minutes to ensure homogeneity.
[0108] Molecular weight was determined by GPC using polystyrene calibration: Mn 88.000 g / mol, Mw 412.000 g / mol, PDI 4.7.
[0109] The results of the application test were as follows: KV100: 375mm 2 / s (30% by weight polymer solution) KV40: 35.1 mm 2 / s (5% by weight of a 30% by weight polymer solution) KV100: 7.3 mm 2 / s (5% by weight of a 30% by weight polymer solution) VI:181 Pour point: -18℃
[0110] The kinematic viscosity at 100°C (KV100) of the lubricants was determined according to ASTM D445 / 446. The higher the viscosity index VI (DIN ISO 2909), the smaller the effect of temperature on the kinematic viscosity.
[0111] Example 7 - Comparative Polymer A copolymer was prepared by the method of Example 5 above using a monomer composition based on 41 wt% PIBamide and 59 wt% NBMA, as described in Example 10 of WO 2007 / 003238. At the end of the polymerization, Nextbase® 3030 was added to bring the total polymer content to about 30%.
[0112] Molecular weight was determined by GPC using polystyrene calibration: Mn 79.800 g / mol, Mw 747.000 g / mol, PD 9.4.
[0113] The results of the application test were as follows: KV100: 97mm 2 / s (30% by weight polymer solution) KV40: 31.1 mm 2 / s (5% by weight of a 30% by weight polymer solution) KV100: 6.0mm 2 / s (5% by weight of a 30% by weight polymer solution) VI:141 Pour point: -18℃
[0114] This comparative example demonstrates that the copolymer described in Example 10 of WO 2007 / 003238 has low VI and poor shear stability.
[0115] Example 8 – Polymerization Into the reactor: - 74.59 g of macromonomer PIB amide (solid content 72.4 wt%) - 97.2g EHMA 2-Ethylhexyl Methacrylate - 40.8g MMA methyl methacrylate - SMA Stearyl Methacrylate 48.0g - TDDM tert-dodecyl mercaptan 0.20g - 148.8g Yubase® 3 mineral oil Added.
[0116] The weight percentages of the monomers were 22.5% PIB amide, 40.5% EHMA, 17% MMA, and 20% SMA.
[0117] The mixture was heated to 95°C under N2 with stirring. Within 5 minutes of reaching 95°C, 1 / 3 of the total solution of initiator tertbutyl-peroxyethylhexanoate TBPEH (total solution: 0.6 g TBPEH dissolved in 6.26 g Catenex T121) was added. The mixture was stirred for another 10 minutes. Then the remaining 2 / 3 of the TBPEH solution. The mixture was then treated at 95°C for 1 hour. Finally, a solution of 0.49 g TBPEH in 4.95 g Catenex T121 was added and the mixture was stirred for another hour at 95°C. Finally, 180 g Yubase® 3 (hydrotreated light paraffinic mineral oil, KV40 12.4 mm) was added. 2 / s, KV100 3.12mm 2 / s, VI 112) was added to bring the total polymer content to about 40%. The mixture was stirred for 60 minutes to ensure homogeneity.
[0118] Molecular weight was determined by GPC using polystyrene calibration: Mn 99.300 g / mol, Mw 301.000 g / mol, PDI 3.
[0119] The results of the application test were as follows: KV100: 1062mm 2 / s (40% by weight polymer solution) KV40: 35.5mm 2 / s (5% by weight of a 40% by weight polymer solution) KV100: 7.62 mm 2 / s (5% by weight of a 40% by weight polymer solution) VI:191 Pour point: -18℃
[0120] The kinematic viscosity at 100°C (KV100) of the lubricants was determined according to ASTM D445 / 446. The higher the viscosity index VI (DIN ISO 2909), the smaller the effect of temperature on the kinematic viscosity.
Claims
1. A comb copolymer, in polymerized form (A) up to 40% by weight of formula (I) 【Chemistry 1】 [In the formula, R 1 is H or methyl, and n is a number from 5 to 100. and (B) Formula (II) H 2 C=C(R 1 )COOR 2 (II) [In the formula, R 1 is H or methyl, and R 2 is C 5~36 is alkyl] and hydrophobic monomers A comb copolymer comprising:
2. R 2 2. The comb copolymer of claim 1, wherein is hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, nonadecyl, eicosyl, henicosyl, docosyl or mixtures thereof.
3. R 2 3. A comb copolymer according to claim 1 or 2, wherein is a mixture of at least two residues selected from the group consisting of hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, octadecyl, heptadecyl, 2-hexyldecyl, and nonadecyl.
4. Formula (III) H 2 C=C(R 1 )COOR 3 (III) [In the formula, R 3 is C 1~4 is alkyl] 4. A comb copolymer according to claim 1, further comprising a hydrophilic monomer of the formula:
5. A comb copolymer according to any one of claims 1 to 4, comprising from 5 to 30% by weight of PIB macromonomer.
6. A comb copolymer according to any one of claims 1 to 5, comprising at least 30% by weight of hydrophobic monomers.
7. A comb copolymer according to any one of claims 1 to 6, comprising from 40 to 90% by weight of hydrophobic monomers.
8. A comb copolymer according to any one of the preceding claims, comprising 1 to 25% by weight of a hydrophilic monomer.
9. - 5 to 30% by weight of PIB macromonomer, - 50 to 90% by weight of a hydrophobic monomer, - 1 to 25% by weight of a hydrophilic monomer; Including, A comb copolymer according to any one of claims 1 to 8, wherein the sum of all monomers is 100% by weight.
10. Formula (I) 【Chemistry 2】 [In the formula, R 1 is H or methyl, and n is a number from 5 to 100.
1. A method for preparing a PIB macromonomer of the formula: Formula (IV) 【Chemistry 3】 reacting the polyisobutene amine of formula (1) with (meth)acrylic anhydride.
11. 11. The method of claim 10, wherein the (meth)acrylic anhydride is present in a molar excess relative to the polyisobutene amine.
12. 12. The method of claim 10 or 11, wherein the reaction is followed by hydrolysis of the remaining (meth)acrylic anhydride to form (meth)acrylic acid.
13. 13. The method of claim 12, wherein the (meth)acrylic acid is removed by distillation or by extraction with water.
14. (i) a base oil; and (ii) a comb copolymer according to any one of claims 1 to 9; (iii) further lubricant additives; A lubricant comprising:
15. Use of a comb copolymer according to any one of claims 1 to 9 for improving the viscosity index of a lubricating oil.
Citation Information
Patent Citations
Oil soluble comb polymers
CN101142244A
Acryl functional polybutylene
JP1998139813A
Oil-soluble comb polymer
JP2008546894A
Macromonomers containing polyisobutene groups, and their homopolymers or copolymers
JP2019528343A
(METH)acryloyl-terminated polyisobutylene polymer, method for producing the same, and active energy ray-curable composition
US20140243444A1