Hot-rolled steel plate and steel pipe for ground reinforcement and their manufacturing method
The hot-rolled steel sheet and pipe for ground reinforcement achieve high strength and formability by precise alloying and manufacturing processes, ensuring uniform microstructure and hardness, addressing weld softening and shape defects.
Patent Information
- Application Number
- JP2024533294
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-16
- Filing Date
- 2022-12-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-02
AI Technical Summary
Existing hot-rolled steel sheets and steel pipes for ground reinforcement face challenges in achieving high strength and formability while avoiding weld softening and shape defects, particularly in small-diameter pipes.
A hot-rolled steel sheet with specific alloy compositions and microstructures, including controlled amounts of C, Si, Mn, Ti, Nb, Mo, P, S, and N, and a balanced microstructure of 90% ferrite with fine carbides, is produced through precise reheating, hot rolling, and coiling processes to ensure uniformity and strength.
The solution results in steel plates and pipes with yield strengths of 700 MPa and 800 MPa, tensile strengths of 750 MPa and 860 MPa, and elongations of 15% and 10%, respectively, with uniform hardness and excellent formability, minimizing shape defects and weld softening.
Smart Images

Figure 2024545450000001 
Figure 2024545450000002 
Figure 2024545450000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel plate and steel pipe for ground reinforcement, which are excellent in strength and formability, and a method for producing the same. [Background technology]
[0002] As the number of facilities such as underground tunnels for underground roads, underground transfer centers, and underground shopping centers increases, the need for ground reinforcement materials that serve as the foundations of these facilities is increasing. In response to this, a new standard for steel pipes for ground reinforcement (KS D 3872) was established. Steel pipes for ground reinforcement used to reinforce ground structures in civil engineering and architecture must satisfy the following properties in the longitudinal direction: YS: 800 MPa, TS: 860 MPa, EL: 10% or more. To satisfy these physical properties, hot-rolled steel sheets are required to have high strength of YS: 700 MPa or more, TS: 750 MPa or more, and formability of EL: 15% or more. It is easy to obtain high strength by utilizing low-temperature structures such as bainite and martensite, but these structures have the disadvantage that the slow cooling rate after welding causes softening of the weld, which inhibits the physical properties of the weld.
[0003] On the other hand, in order to manufacture small-diameter steel pipes suitable for ground reinforcement, the steel pipes must have excellent formability because their small diameters result in significant work hardening during pipe making. In addition, the microstructure must be uniform to enable pipe making without shape defects. Summary of the Invention [Problem to be solved by the invention]
[0004] One aspect of the present invention is to provide a hot-rolled steel plate and steel pipe for ground reinforcement, which are excellent in strength and formability, and a method for manufacturing the same. [Means for solving the problem]
[0005] One embodiment of the present invention provides a hot-rolled steel sheet for ground reinforcement having excellent strength and formability, the hot-rolled steel sheet containing, by weight %, C: 0.05-0.1%, Si: 0.1% or less (excluding 0%), Mn: 1.5-1.9%, Ti: 0.05-0.15%, Nb: 0.03-0.1%, Mo: 0.03-0.1%, P: 0.02% or less (excluding 0%), S: 0.02% or less (excluding 0%), N: 0.01% or less (excluding 0%), with the remainder being Fe and inevitable impurities, satisfying the following relational expressions 1 and 2, having a microstructure containing, by area %, 90% or more of ferrite, crystal grains of the ferrite having an average size of 15 μm or less, and containing 0.05% by weight or more of carbides containing Ti, Nb, and / or Mo, and the carbides having an average size of 20 nm or less. [Relationship 1] 0.002≦(Ti / 48+Mo / 96+Nb / 93)≦0.004 [Relationship 2] 0.002≦(C / 12)-(Ti / 48+Mo / 96+Nb / 93)≦0.006 (Note that the content of each alloying element in the above Relational Formulas 1 and 2 means weight percent.)
[0006] Another embodiment of the present invention provides a steel pipe for ground reinforcement, which is manufactured using the above-mentioned hot-rolled steel plate and has excellent strength and formability.
[0007] Another embodiment of the present invention provides a method for producing a hot-rolled steel sheet for ground reinforcement having excellent strength and formability, the method including the steps of: reheating a steel slab, which contains, by weight, 0.05-0.1% C, 0.1% or less (excluding 0%) Si, 1.5-1.9% Mn, 0.05-0.15% Ti, 0.03-0.1% Nb, 0.03-0.1% Mo, 0.02% or less (excluding 0%) P, 0.02% or less (excluding 0%) S, 0.01% or less (excluding 0%) N, with the remainder being Fe and inevitable impurities, and which satisfies the following Relational Formulas 1 and 2, in a temperature range of 1150-1300°C; finish hot rolling the reheated steel slab in a temperature range of 800-950°C to obtain a hot-rolled steel sheet; and coiling the hot-rolled steel sheet in a temperature range of 550-700°C. [Relationship 1] 0.002≦(Ti / 48+Mo / 96+Nb / 93)≦0.004 [Relationship 2] 0.002≦(C / 12)-(Ti / 48+Mo / 96+Nb / 93)≦0.006 (Note that the content of each alloying element in the above Relational Formulas 1 and 2 means weight percent.)
[0008] Another embodiment of the present invention provides a method for producing a steel pipe for ground reinforcement having excellent strength and formability, comprising the step of producing a steel pipe by forming the hot-rolled steel sheet produced by the above-mentioned method. Effect of the Invention
[0009] According to one aspect of the present invention, there is provided a hot-rolled steel plate and steel pipe for ground reinforcement having excellent strength and formability, and a method for manufacturing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a hot-rolled steel sheet according to an embodiment of the present invention will be described. First, the alloy composition of the present invention will be described. The content of the alloy composition described below is expressed in weight percent.
[0011] C: 0.05 to 0.1% C is added not only for the solid solution strengthening effect but also for the formation of carbides with Ti, Nb, and Mo, and is an element for ensuring tensile strength. In order to obtain the above effect, it is preferable to add 0.05% or more. However, if it exceeds 0.1%, the carbide becomes coarse, the precipitation strengthening effect cannot be sufficiently ensured, and the pearlite fraction in the microstructure increases, making it impossible to ensure 90% or more of ferrite that is to be obtained in the present invention. Therefore, the C content is preferably in the range of 0.05 to 0.1%. The lower limit of the C content is more preferably 0.06%, even more preferably 0.065%, and most preferably 0.07%. The upper limit of the C content is more preferably 0.09%, even more preferably 0.085%, and most preferably 0.08%.
[0012] Si: 0.1% or less (excluding 0%) Silicon is not only useful for deoxidizing steel, but also effective in ensuring strength through solid solution strengthening. However, if the content of silicon exceeds 0.1%, there is a drawback in that silicon oxide is formed, making plating difficult. Therefore, the content of silicon is preferably 0.1% or less. The content of silicon is more preferably 0.08% or less, even more preferably 0.065% or less, and most preferably 0.05% or less.
[0013] Mn: 1.5-1.9% Mn is added to ensure the effect of solid solution strengthening and the hardening ability of the welded portion during cooling after welding. In order to obtain the above effects, it is preferable that 1.5% or more is added. However, if it exceeds 1.9%, Mn segregation increases, and defects and material deviations may occur during continuous casting. Therefore, the Mn content is preferably in the range of 1.5 to 1.9%. The lower limit of the Mn content is more preferably 1.55%, even more preferably 1.6%, and most preferably 1.65%. The upper limit of the Mn content is more preferably 1.85%, even more preferably 1.8%, and most preferably 1.75%.
[0014] Ti: 0.05 to 0.15% Ti is added for precipitation strengthening effect and suppression of grain coarsening. If the Ti content is less than 0.05%, it is difficult to obtain the high strength targeted in the present invention, and if it exceeds 0.15%, coarse carbides are formed, which is not effective for precipitation strengthening. Therefore, the Ti content is preferably in the range of 0.05 to 0.15%. The lower limit of the Ti content is more preferably 0.07%, further preferably 0.08%, and most preferably 0.09%. The upper limit of the Ti content is more preferably 0.14%, further preferably 0.13%, and most preferably 0.12%.
[0015] Nb: 0.03 to 0.1% Nb is added to obtain finer grain size by suppressing recrystallization during hot rolling as well as the precipitation strengthening effect. If the Nb content is less than 0.03%, sufficient precipitation strengthening effect cannot be obtained, and if it exceeds 0.1%, strength may decrease due to the formation of coarse precipitates. Therefore, the Nb content is preferably in the range of 0.03 to 0.1%. The lower limit of the Nb content is more preferably 0.035%, further preferably 0.038%, and most preferably 0.04%. The upper limit of the Nb content is more preferably 0.08%, further preferably 0.07%, and most preferably 0.06%.
[0016] Mo: 0.03 to 0.1% Mo is added to suppress the growth of precipitates. It also contributes to grain refinement by delaying the formation of ferrite so that ferrite is formed at a low temperature. If the Mo content is less than 0.03%, the above effect cannot be sufficiently obtained. On the other hand, if it exceeds 0.1%, the economic efficiency may decrease. Therefore, the Mo content is preferably in the range of 0.03 to 0.1%. The lower limit of the Mo content is more preferably 0.035%, further preferably 0.04%, and most preferably 0.045%. The upper limit of the Mo content is more preferably 0.09%, further preferably 0.08%, and most preferably 0.07%.
[0017] P: 0.02% or less (excluding 0%) Since P segregates at grain boundaries as an impurity element and reduces toughness, it is preferable to avoid its inclusion as much as possible, and in the present invention, the upper limit is set to 0.02%. The P content is more preferably 0.018% or less, even more preferably 0.017% or less, and most preferably 0.015% or less.
[0018] S: 0.02% or less (excluding 0%) S is a major element that forms MnS as an impurity element, and since the formation of coarse MnS reduces toughness, the content is limited to 0.02% or less in the present invention. The S content is more preferably 0.015% or less, even more preferably 0.01% or less, and most preferably 0.005% or less.
[0019] N: 0.01% or less (excluding 0%) When the content of N exceeds 0.01% as an impurity element, it reacts with Ti and Nb at high temperatures to form nitrides, which reduces the contents of Ti and Nb that substantially contribute to precipitation strengthening, thereby lowering the strength of the steel material. Therefore, the N content is preferably 0.01% or less. The N content is more preferably 0.008% or less, even more preferably 0.007% or less, and most preferably 0.006% or less.
[0020] Moreover, the hot-rolled steel sheet of the present invention preferably satisfies the following Relational Expressions 1 and 2.
[0021] [Relationship 1] 0.002≦(Ti / 48+Mo / 96+Nb / 93)≦0.004
[0022] The above-mentioned relational expression 1 is a parameter for improving strength by controlling the contents of the precipitation strengthening elements Ti, Mo, and Nb. If the value of the above (Ti / 48+Mo / 96+Nb / 93) is less than 0.002, the amount of precipitates is too small to effectively improve strength. On the other hand, if the value of the above (Ti / 48+Mo / 96+Nb / 93) is more than 0.004, the precipitates may become coarse and an effective precipitation strengthening effect may not be obtained.
[0023] [Relationship 2] 0.002≦(C / 12)-(Ti / 48+Mo / 96+Nb / 93)≦0.006
[0024] The above relational expression 2 is a parameter indicating the content of C used for the solid solution strengthening effect, excluding the content of C used for the precipitation strengthening effect. When the value of (C / 12)-(Ti / 48+Mo / 96+Nb / 93) is less than 0.002, the ferrite phase does not have sufficient strength, and the high strength targeted in the present invention cannot be achieved. On the other hand, when the value of (C / 12)-(Ti / 48+Mo / 96+Nb / 93) exceeds 0.006, the remaining C content increases excessively, so that the precipitates easily become coarse, and the target strength cannot be obtained, and the pearlite fraction increases, making it difficult to obtain 90% or more of ferrite targeted in the present invention. In addition, as the formation of pearlite is promoted in the center of the steel plate, where the cooling rate is relatively slow, a large difference in hardness occurs between the surface and the inside. As a result, a hardness difference occurs in the thickness direction of the steel pipe. In addition, a specific part is subjected to a lot of processing during rolling, which may cause problems such as shape defects and crack generation. The rolling process refers to a process of forming protrusions on the surface of a steel pipe.
[0025] In addition to the above-mentioned steel composition, the remainder may include Fe and inevitable impurities. Since inevitable impurities may be mixed unintentionally in the normal steel manufacturing process, they cannot be completely excluded, and any engineer in the field of normal steel manufacturing can easily understand the meaning of this. Note that the present invention does not completely exclude the addition of compositions other than the above-mentioned steel composition.
[0026] The hot-rolled steel sheet of the present invention preferably has a microstructure containing 90% or more ferrite by area %. In the present invention, it is important to ensure 90% or more ferrite in order to ensure excellent formability. The microstructure of the present invention is theoretically preferably a single ferrite phase, but one or more of pearlite, retained austenite, bainite, and martensite may be formed inevitably in the manufacturing process. However, if the amount of low-temperature transformation phase such as bainite or martensite increases, the formability decreases. In addition, if pearlite is present on the surface of the steel pipe, cracks are likely to occur during rolling due to cementite, which is a hard phase. Therefore, it is preferable that the residual structure is as small as possible. The fraction of the ferrite is more preferably 93% or more, and even more preferably 95% or more. Meanwhile, the ferrite may be one or more of polygonal ferrite, bainitic ferrite, and acicular ferrite.
[0027] In this case, the ferrite grains preferably have an average size of 15 μm or less. If the ferrite grain size exceeds 15 μm, sufficient strength may not be obtained due to grain coarsening. The ferrite grain size is more preferably 12 μm or less, and even more preferably 10 μm or less.
[0028] The hot-rolled steel sheet of the present invention preferably contains 0.05% by weight or more of carbides containing Ti, Nb, and Mo alone or in combination, and the carbides preferably have an average size of 20 nm or less. In this way, by forming a large amount of fine carbides having an average size of 20 nm or less in an amount of 0.05% by weight or more, excellent strength improvement effects can be obtained without causing destruction of the carbides. The fraction of the carbides is more preferably 0.07% by weight or more, and even more preferably 0.08% by weight or more. The average size of the carbides is more preferably 15 nm or less, and even more preferably 10 nm or less. Meanwhile, in the present invention, since the more the carbides are formed, it is advantageous, so that the upper limit is not particularly limited, but it is difficult to exceed 0.2% by weight in consideration of the contents of Ti, Nb, and Mo contained in the steel.
[0029] The hot-rolled steel sheet of the present invention provided as described above has a yield strength (YS) of 700 MPa or more, a tensile strength (TS) of 750 MPa or more, and an elongation (EL) of 15% or more, and can ensure excellent strength and formability.
[0030] On the other hand, the present invention can provide a steel pipe manufactured using the above-mentioned hot-rolled steel sheet.
[0031] The steel pipe of the present invention has a yield strength (YS) of 800 MPa or more, a tensile strength (TS) of 860 MPa or more, and an elongation (EL) of 10% or more, and can ensure excellent strength and formability.
[0032] Meanwhile, only when the steel pipe is uniformly deformed in the thickness direction during rolling can stable rolling be performed without defects caused by stress concentration during processing, and since the steel pipe of the present invention has a hardness deviation of 15% or less, it has an advantage in that it ensures uniform hardness and is favorable for rolling. The hardness deviation can be defined as [(maximum hardness value-minimum hardness value) / maximum hardness value x 100] based on the hardness values measured at 0.5 mm, t / 4, and t / 2 points (t: steel pipe thickness) from the surface of the steel pipe in the thickness direction.
[0033] Hereinafter, a method for producing a hot-rolled steel sheet according to one embodiment of the present invention will be described.
[0034] First, the steel slab satisfying the above-mentioned alloy composition and relational expressions 1 and 2 is reheated in the temperature range of 1150 to 1300°C. The reason for reheating the steel slab in the temperature range of 1150 to 1300°C is to make the alloy composition and microstructure uniform. If the reheating temperature is less than 1150°C, the precipitates formed in the slab are not dissolved, and the optimal precipitation strengthening effect cannot be obtained in the subsequent process. If the reheating temperature exceeds 1300°C, excessive grain growth occurs, making it difficult to ensure the target material properties and quality. Therefore, the reheating temperature of the steel slab is preferably in the range of 1150 to 1300°C. The lower limit of the reheating temperature is more preferably 1170°C, even more preferably 1180°C, and most preferably 1200°C. The upper limit of the reheating temperature is more preferably 1290°C, even more preferably 1270°C, and most preferably 1250°C.
[0035] Thereafter, the reheated steel slab is finish hot rolled in a temperature range of 800 to 950°C to obtain a hot-rolled steel sheet. If the finish hot rolling temperature is less than 800°C, a part of the austenite is transformed into ferrite, and the size of the crystal grains finally obtained becomes non-uniform, and if it exceeds 950°C, scale defects and the like may occur. Therefore, the finish hot rolling temperature is preferably in the range of 800 to 950°C. The lower limit of the finish hot rolling temperature is more preferably 820°C, even more preferably 825°C, and most preferably 850°C. The upper limit of the finish hot rolling temperature is more preferably 940°C, even more preferably 920°C, and most preferably 900°C.
[0036] Thereafter, the hot-rolled steel sheet is coiled at a temperature range of 550 to 700°C. If the coiling temperature is less than 550°C, not only is the microstructure that the present invention aims to obtain not obtained, but the formation of carbides is insufficient, and therefore sufficient precipitation strengthening effect cannot be obtained, and if the coiling temperature exceeds 700°C, the carbides become coarse, and the target strength cannot be obtained. Therefore, the coiling temperature is preferably in the range of 550 to 700°C. The lower limit of the coiling temperature is more preferably 600°C, further preferably 620°C, and most preferably 640°C. The upper limit of the coiling temperature is more preferably 680°C, further preferably 665°C, and most preferably 650°C. Meanwhile, cooling before coiling after the finish hot rolling can be performed on a run-out table.
[0037] Meanwhile, in the present invention, after obtaining a hot rolled steel sheet by the above-mentioned process, the hot rolled steel sheet is made into a pipe to obtain a steel pipe. In this case, as a welding method in the pipe making, electric resistance welding (ERW) or the like can be used. In addition, in the present invention, after the step of obtaining the steel pipe, a step of rolling the steel pipe can be further included. EXAMPLES
[0038] The present invention will be described in more detail below with reference to examples. However, the description of such examples is merely for illustrating the implementation of the present invention, and the present invention is not limited by the description of such examples. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0039] (Example) A steel slab having an alloy composition as shown in Table 1 below was prepared, and then reheated, finish hot rolled, and coiled under the conditions as shown in Table 2 below to produce a hot-rolled steel sheet having a thickness of 2.8 to 6 mm. The hot-rolled steel sheet thus produced was then made into a steel pipe. In this case, roll forming and electric resistance welding, which are typical methods for producing electric resistance welded steel pipes, were used in the above-mentioned pipe making, and the pipe making condition (t / D) according to the thickness (t) of the material and the diameter (D) of the steel pipe was 14% or more. The microstructure, precipitates, and mechanical properties of the hot-rolled steel sheet and steel pipe thus produced were measured, and the hardness of the steel pipe at each position in the thickness direction was also measured, and the results are shown in Tables 3 and 4 below.
[0040] The type and fraction of microstructure was measured using an optical microscope (OM), and the ferrite grain size was measured using the circular intercept method of ASTM E 112 after photographing using a scanning electron microscope (SEM).
[0041] The size of the precipitates was measured by carbon replica method and transmission electron microscope (TEM) of precipitates taken from the test pieces. The fraction of precipitates was obtained by measuring the contents of Ti, Nb, and Mo using the residue extraction method.
[0042] Yield strength (YS), tensile strength (TS) and elongation (EL) were measured by conducting tensile tests according to the KS B 0802 tensile test method. For hot-rolled steel sheets, tensile test pieces were processed using KS B 0801 No. 5 test pieces with the length aligned with the hot rolling direction. For steel pipes, tensile tests were conducted using KS B 0801 No. 11 test pieces.
[0043] The hardness at each position in the thickness direction was measured at 0.5 mm, t / 4, and t / 2 points (t: steel pipe thickness) from the outer surface of the steel pipe in the thickness direction using a Vickers hardness tester with a load of 1 kg. At this time, measurements were taken at 5 points at each position and the average value was calculated. In addition, the hardness deviation listed in Table 3 below was calculated from each hardness value measured at each position as [(maximum hardness value - minimum hardness value) / maximum hardness value x 100].
[0044] [Table 1]
[0045] [Table 2]
[0046] [Table 3]
[0047] [Table 4]
[0048] As can be seen from Tables 1 to 4 above, in the case of Examples 1 to 16 which satisfy the alloy composition, Relational Formulas 1 and 2 and manufacturing conditions proposed by the present invention, by securing the microstructure and precipitates which the present invention aims to obtain, not only do they have excellent mechanical properties, but also the deviation in hardness at different positions in the thickness direction of the steel pipe is at a low level.
[0049] In the case of Comparative Example 1, although the alloy composition of the present invention was satisfied, the re-dissolution of the precipitation strengthening elements was insufficient due to the low reheating temperature of the steel slab, and therefore, a sufficient precipitation strengthening effect could not be obtained, and therefore, the high strength targeted by the present invention could not be ensured.
[0050] In the case of Comparative Example 2, although the alloy composition of the present invention was satisfied, the finish hot rolling temperature was low, and as a result, coarse precipitates were formed during rolling, and sufficient precipitation strengthening effect was not obtained. As a result, the high strength targeted by the present invention could not be ensured.
[0051] In the case of Comparative Example 3, although the alloy composition of the present invention was satisfied, the high finish hot rolling temperature caused the crystal grains to become coarse, and it was not possible to ensure the high strength targeted by the present invention.
[0052] In the case of Comparative Example 4, although the alloy composition of the present invention was satisfied, not only was the fine structure that the present invention aims to obtain not obtained due to the low coiling temperature, but also a sufficient precipitation strengthening effect was not obtained, and the high strength that the present invention aims to achieve could not be ensured.
[0053] In the case of Comparative Example 5, although the alloy composition of the present invention was satisfied, coarse carbides were formed due to the high coiling temperature, and the high strength targeted by the present invention could not be ensured.
[0054] In the case of Comparative Example 6, the Ti and Nb contents were low, so that a sufficient precipitation strengthening effect was not obtained, and the high strength targeted by the present invention could not be ensured.
[0055] In the case of Comparative Example 7, the high Ti content resulted in the formation of coarse carbides, making it impossible to ensure the high strength targeted by the present invention.
[0056] In the case of Comparative Example 8, the solid solution strengthening effect was low due to the low Mn content, and a sufficient precipitation strengthening effect was not obtained due to changes in the phase transformation conditions during cooling, so the high strength targeted by the present invention could not be ensured.
[0057] In the case of Comparative Example 9, the high Nb content caused the formation of coarse carbides, making it impossible to ensure the high strength targeted by the present invention.
[0058] In the case of Comparative Example 10, not only was it impossible to satisfy Relational Expression 2, but also the high strength targeted by the present invention could not be ensured due to the low C content.
[0059] In the case of Comparative Example 11, the high C content resulted in a high solute C content and an increased pearlite content, and thus the microstructure desired by the present invention was not obtained. Since Relational Formula 2 was not satisfied, not only was the high strength desired by the present invention not obtained, but the deviation in hardness at different positions in the thickness direction of the steel pipe also increased.
[0060] In the case of Comparative Example 12, since Relational Formula 2 was not satisfied, the appropriate balance of precipitates and solute C proposed by the present invention was not obtained, and therefore not only was it impossible to ensure high strength, but the deviation in hardness at different positions in the thickness direction of the steel pipe became large.
[0061] In the case of Comparative Example 13, since the relational expression 1 was not satisfied, a sufficient precipitation strengthening effect was not obtained, and the high strength targeted by the present invention could not be ensured.
Claims
1. In weight percent, C: 0.05-0.1%, Si: 0.1% or less (excluding 0%), Mn: 1.5-1.9%, Ti: 0.05-0.15%, Nb: 0.03-0.1%, Mo: 0.03-0.1%, P: 0.02% or less (excluding 0%), S: 0.02% or less (excluding 0%), N: 0.01% or less (excluding 0%), the remainder including Fe and inevitable impurities, The following relations 1 and 2 are satisfied, It has a microstructure containing 90% or more ferrite by area percent, The ferrite grains have an average size of 15 μm or less, Contains 0.05% by weight or more of carbides containing Ti, Nb, and Mo alone or in combination; The carbides have an average size of 20 nm or less. [Relationship 1] 0.002≦(Ti / 48+Mo / 96+Nb / 93)≦0.004 [Relationship 2] 0.002≦(C / 12)−(Ti / 48+Mo / 96+Nb / 93)≦0.006 (Note that the content of each alloy element in the above Relational Formulas 1 and 2 means weight percent.)
2. The hot-rolled steel plate for ground reinforcement according to claim 1 , wherein the microstructure contains one or more of pearlite, retained austenite, bainite, and martensite as a residual structure.
3. The hot-rolled steel plate for ground reinforcement according to claim 1, wherein the hot-rolled steel plate has a yield strength (YS): 700 MPa or more, a tensile strength (TS): 750 MPa or more, and an elongation (EL): 15% or more.
4. A steel pipe for ground reinforcement, manufactured using the hot-rolled steel sheet according to any one of claims 1 to 3.
5. 5. The steel pipe for ground reinforcement according to claim 4, wherein the steel pipe has a yield strength (YS): 800 MPa or more, a tensile strength (TS): 860 MPa or more, and an elongation (EL): 10% or more.
6. 5. The steel pipe for ground reinforcement according to claim 4, wherein the steel pipe has a hardness deviation of 15% or less. (The hardness deviation is defined as [(maximum hardness value-minimum hardness value) / maximum hardness value x 100] based on the hardness values measured at 0.5 mm, t / 4, and t / 2 points (t: steel pipe thickness) from the surface of the steel pipe in the thickness direction.)
7. a step of reheating a steel slab containing, in weight percent, C: 0.05-0.1%, Si: 0.1% or less (excluding 0%), Mn: 1.5-1.9%, Ti: 0.05-0.15%, Nb: 0.03-0.1%, Mo: 0.03-0.1%, P: 0.02% or less (excluding 0%), S: 0.02% or less (excluding 0%), N: 0.01% or less (excluding 0%), with the remainder being Fe and inevitable impurities, and satisfying the following relations 1 and 2, in a temperature range of 1150-1300°C; Finish hot rolling the reheated steel slab at a temperature range of 800 to 950° C. to obtain a hot-rolled steel sheet; and and winding the hot-rolled steel sheet at a temperature in the range of 550 to 700°C. [Relationship 1] 0.002≦(Ti / 48+Mo / 96+Nb / 93)≦0.004 [Relationship 2] 0.002≦(C / 12)−(Ti / 48+Mo / 96+Nb / 93)≦0.006 (Note that the content of each alloy element in the above Relational Formulas 1 and 2 means weight percent.)
8. A method for producing a steel pipe for ground reinforcement, comprising the step of producing a steel pipe by making the hot-rolled steel sheet produced by the method according to claim 7.
9. The method for producing a steel pipe for ground reinforcement according to claim 8, further comprising the step of rolling the steel pipe after the step of obtaining the steel pipe.
Citation Information
Patent Citations
Connecting device between piping steel pipe and hose
JP1996128571A
High strength steel sheet having excellent deformability, high strength steel pipe and production method thereof
JP2003293089A
Low yield ratio type steel sheet with high young's modulus, hot-dip galvanized steel sheet, galvannealed steel sheet and steel tube, and their manufacturing method
JP2007146275A
Low yield ratio high strength spiral steel pipe pile and manufacturing method therefor
JP2015193887A
Inner surface resin lining thin steel pipe and manufacturing method thereof
JP2019090517A