Negative electrode for lithium secondary battery and magnetic alignment device for the negative electrode

The magnetic alignment device addresses alignment issues in lithium secondary battery electrodes by controlling alignment and surface characteristics, enhancing electrical performance and reducing defects through a magnet configuration and drying process.

JP2024545453AInactive Publication Date: 2024-12-06LG ENERGY SOLUTION LTD

Patent Information

Application Number
JP2024533306
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-13
Filing Date
2023-09-21
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for aligning graphite in negative electrodes of lithium secondary batteries using magnetic fields face challenges such as inconsistent magnetic force application, leading to low alignment quality and surface defects, which affect the electrical properties and assembly process of the electrodes.

Method used

A magnetic alignment device with specific magnet configurations and a drying process is used to align carbon-based negative electrode active materials perpendicularly to the current collector, controlling the degree of alignment and surface characteristics within defined ranges, using a magnetic field strength gradient and controlled drying to prevent surface damage.

Benefits of technology

The solution achieves high alignment quality of carbon-based negative electrode active materials, improving electrical properties and surface characteristics, resulting in enhanced charging performance and reduced defects in the negative electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545453000001_ABST
    Figure 2024545453000001_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode for a lithium secondary battery and a magnetic alignment device for manufacturing the same. The magnetic alignment device applies a magnetic field to the negative electrode slurry by introducing magnet units respectively to the upper and lower parts of a negative electrode current collector on which a negative electrode slurry is applied, and applies a stronger magnetic force to a first region located upstream in the direction of conveyance of the negative electrode current collector than to a second region located downstream in the magnet units. As a result, the degree of alignment of the carbon-based negative electrode active material contained in the negative electrode slurry during the manufacture of the negative electrode and the arithmetic mean height of the surface of the negative electrode active layer can be easily controlled within a specific range. In addition, the negative electrode manufactured by this method has the advantage of excellent surface characteristics of the negative electrode active layer as well as electrical properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0131366 dated October 13, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a negative electrode for a lithium secondary battery and a magnetic alignment device for manufacturing the same. [Background technology]

[0003] 2. Description of the Related Art In recent years, secondary batteries have been widely used not only in small devices such as portable electronic devices, but also in medium- to large-sized devices such as battery packs for hybrid and electric vehicles and power storage devices.

[0004] Such secondary batteries are power generating elements capable of being charged and discharged and have a laminated structure of a positive electrode / separator / negative electrode. In general, the positive electrode contains a lithium metal oxide as a positive electrode active material, and the negative electrode contains a carbon-based negative electrode active material such as graphite. During charging, lithium ions released from the positive electrode are absorbed into the carbon-based negative electrode active material of the negative electrode, and during discharging, the lithium ions contained in the carbon-based negative electrode active material are absorbed into the lithium metal oxide of the positive electrode, thereby allowing repeated charging and discharging.

[0005] In this case, examples of the negative electrode active material used in the negative electrode include graphite materials such as natural graphite. Such graphite has a layered structure, in which carbon atoms form a network structure, and many layers that spread out in a planar shape are stacked. During charging, lithium ions penetrate from the edge faces (surfaces where layers overlap) of such graphite layers and diffuse between the layers. During discharging, lithium ions can be desorbed and released from the edge faces of the layers. In addition, since the electrical resistivity of graphite in the plane direction of the layers is lower than that in the stacking direction of the layers, a detouring electron conduction path is formed along the plane direction of the layers.

[0006] In relation to this, a technique has been proposed for magnetically orienting the graphite contained in the negative electrode in order to improve the charging performance of the negative electrode in lithium secondary batteries that use graphite. Specifically, the (002) crystal plane of the graphite is oriented in a magnetic field during the formation of the negative electrode so that it is nearly perpendicular to the negative electrode current collector, and then fixed. In this case, the edge face of the graphite layer faces the positive electrode active layer, so that the insertion and desorption of lithium ions is smoothly performed, and at the same time, the electron conduction path is shortened, improving the electronic conductivity of the negative electrode. This can improve the charging performance of the battery.

[0007] For this reason, a method is applied in which a magnetic device is used to apply a magnetic field to a negative electrode slurry containing graphite as a carbon-based negative electrode active material during the manufacture of a negative electrode, thereby aligning the graphite. However, this method is a method in which a permanent magnet is placed on the top and bottom of a metal sheet coated with a negative electrode slurry, and a magnetic field is applied, which makes it difficult to maintain a constant magnetic force and is therefore less easy to work with. In addition, the graphite in the final negative electrode active layer has a low degree of alignment because an attractive phenomenon caused by a magnetic force occurs at the end of the permanent magnet, i.e., the end of the magnetic field, causing the alignment of the graphite on the metal sheet to be broken. In addition, since a considerable stress is applied to the carbon-based negative electrode active material aligned in the negative electrode slurry, scratches or crater-like grooves may be formed on the surface of the negative electrode active layer to be manufactured, thereby deteriorating the surface characteristics, and thus the electrical properties of the manufactured negative electrode may be reduced, or problems may occur during the process of assembling the battery. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 10-2018-0048131 [Patent Document 2] Korean Patent Publication No. 10-2022-0060017 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a magnetic alignment device for manufacturing an anode having excellent vertical alignment characteristics of a carbon-based anode active material contained in the anode active layer relative to a anode current collector and excellent surface characteristics of the anode active layer, and a method for manufacturing an anode using the same. [Means for solving the problem]

[0010] In order to solve the above-mentioned problems, in one embodiment, the present invention comprises: a negative electrode current collector; and a negative electrode active layer provided on the negative electrode current collector and containing a carbon-based negative electrode active material, The degree of alignment (OI) of the carbon-based negative electrode active material in the negative electrode active layer, represented by the following formula 1, is 0.1 to 5.0, The negative electrode for a lithium secondary battery is characterized in that the arithmetic mean height (Sa) of the surface of the negative electrode active layer is 3.0 μm to 10.0 μm.

[0011] [Formula 1] OI=I 004 / I 110

[0012] In formula 1, I 004 represents the area of ​​the peak showing the (004) crystal plane in the X-ray diffraction spectroscopy (XRD) measurement of the negative electrode active layer, I 110 represents the area of ​​the peak indicating the (110) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD).

[0013] In this case, the negative electrode active layer may have an average thickness of 50 μm to 300 μm.

[0014] The carbon-based negative electrode active material contained in the negative electrode active layer may include at least one of natural graphite and artificial graphite.

[0015] In one embodiment, the present invention provides a magnetic alignment apparatus for manufacturing the negative electrode for the lithium secondary battery. Specifically, the magnetic alignment apparatus is a magnetic alignment apparatus for manufacturing a negative electrode for aligning a carbon-based negative electrode active material, a first magnet unit and a second magnet unit, which are respectively located at an upper portion and a lower portion of a negative electrode current collector coated with a negative electrode slurry including a carbon-based negative electrode active material in a moving direction of the negative electrode current collector and apply a magnetic force; a drying unit that dries the negative electrode slurry to which magnetic force is applied by the first magnet unit and the second magnet unit, The first magnet unit and the second magnet unit are each divided into a first region located upstream and a second region located downstream based on a transport direction of the negative electrode current collector, The first region may be characterized in that a magnetic field having a stronger magnetic strength is applied thereto than in the second region.

[0016] In this case, the first magnet portion and the second magnet portion each include a plurality of unit magnets arranged in the transport direction (x-axis direction) and width direction (y-axis direction) of the negative electrode collector, respectively, and the unit magnets arranged in the first region of the first magnet portion and the second magnet portion among the plurality of unit magnets may be arranged in a Halbach array.

[0017] The first and second magnet parts may have a length of 0.5 m to 10 m in the direction of transport of the negative electrode current collector, and the length of the first region may be shorter than the length of the second region. Specifically, the first region may occupy a length of 5% to 50% of the total length of the first and second magnet parts.

[0018] Also, the distance between the first magnet portion and the second magnet portion may be 10 mm to 50 mm.

[0019] Additionally, the first and second magnet portions may include magnets having opposite poles.

[0020] Further, in one embodiment, the present invention provides applying a negative electrode slurry including a carbon-based negative electrode active material onto a negative electrode current collector; Aligning the carbon-based negative electrode active material contained in the negative electrode slurry using the magnetic alignment device according to the present invention; and drying the negative electrode slurry in which the carbon-based negative electrode active material is aligned to form a negative electrode active layer.

[0021] Here, the magnetic alignment device used in the negative electrode manufacturing method may include a first magnet unit and a second magnet unit, which are respectively located at the upper and lower parts along the transport direction of the negative electrode current collector on which the negative electrode slurry is applied as described above and are divided into a first region located upstream and a second region located downstream in the transport direction, in which a ratio of the magnetic force applied in the first region / the magnetic force applied in the second region may be 1.4 or more, and the magnetic force applied in the first region may be 8,000 G or more. Effect of the Invention

[0022] The magnetic alignment device according to the present invention can control the degree of alignment of the carbon-based negative active material contained in the negative electrode slurry and the arithmetic mean height of the surface of the negative active layer within a specific range. In this way, the negative electrode in which the degree of alignment of the carbon-based negative active material and the arithmetic mean height of the surface of the negative active layer are controlled within a specific range has the advantage of excellent surface characteristics of the negative active layer as well as excellent electrical properties. [Brief description of the drawings]

[0023] [Figure 1] 1 is a structural diagram showing a schematic configuration of a magnetic alignment device for a negative electrode according to the present invention; [Diagram 2] 2 is a perspective view showing an arrangement of unit magnets included in a first magnet portion and a second magnet portion. FIG. [Diagram 3] 13 is an image showing the alignment of the ab-axis crystal planes of graphite depending on whether or not a magnetic field is applied to a negative electrode slurry during the formation of a negative electrode active layer, where (a) shows the case where no magnetic field is applied and the graphite crystal planes are not aligned, and (b) shows the case where a magnetic field is applied and the graphite crystal planes are aligned. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Since the present invention can be modified in various ways and can have various embodiments, specific embodiments are described in detail in the detailed description.

[0025] However, this is not intended to limit the invention to any particular embodiment, but it should be understood to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.

[0026] In the present invention, terms such as "comprise" and "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and may be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0027] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.

[0028] In the present invention, "containing as a main component" may mean containing 50% by weight or more (or 50% by volume or more), 60% by weight or more (or 60% by volume or more), 70% by weight or more (or 70% by volume or more), 80% by weight or more (or 80% by volume or more), 90% by weight or more (or 90% by volume or more), or 95% by weight or more (or 95% by volume or more) of the defined component relative to the total weight (or total volume). For example, "containing graphite as a main component as a negative electrode active material" may mean containing 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or 95% by weight or more of graphite relative to the total weight of the negative electrode active material, and in some cases, it may mean that the entire negative electrode active material is made of graphite and contains 100% by weight of graphite.

[0029] In addition, in this specification, "the carbon-based negative electrode active material is oriented" or "the carbon-based negative electrode active material is aligned" may mean that a specific crystal plane (e.g., the ab-axis crystal plane of graphite) showing a two-dimensional planar structure of the carbon-based negative electrode active material constituting the negative electrode active material particles is arranged to have a predetermined inclination based on the surface of the negative electrode current collector, as shown in (b) of Figure 3. This may be different from (a) of Figure 3, in which the particles of the carbon-based negative electrode active material themselves are aligned in a predetermined direction only inside the negative electrode active layer, but have no directionality with respect to the negative electrode current collector.

[0030] In addition, "high orientation of the carbon-based negative electrode active material" may mean that a specific crystal plane (e.g., the ab-axis crystal plane of graphite) showing a two-dimensional planar structure of the carbon-based negative electrode active material contained in the negative electrode active layer has a high frequency of having a certain inclination with respect to the surface of the negative electrode current collector. In some cases, it may mean that the crystal plane of the carbon-based negative electrode active material contained in the negative electrode active layer is aligned at a high angle (e.g., an angle close to vertical, more than 45°, specifically 60° or more) with respect to the surface of the negative electrode current collector.

[0031] In addition, the term "high degree of alignment of the carbon-based negative electrode active material" refers to the "degree of alignment (S 60 / 0 and / or OI)” is large, and it may mean that a specific crystal plane (e.g., the ab-axis crystal plane of graphite) showing a two-dimensional planar structure of the carbon-based negative electrode active material contained in the negative electrode active layer is aligned at a low angle (e.g., less than 45°) with respect to the surface of the negative electrode current collector. Conversely, “the carbon-based negative electrode active material has a low degree of alignment” means that the “degree of alignment (S 60 / 0 and / or OI)” has a small value, which may mean that the crystal plane of the carbon-based negative electrode active material contained in the negative electrode active layer is aligned at a high angle (e.g., an angle close to perpendicular, 45° or more, specifically 60° or more) with respect to the surface of the negative electrode current collector.

[0032] In addition, in this specification, the term "crystal plane of a carbon-based negative electrode active material" refers to a plane in which atoms of a carbon-based negative electrode active material form the outer shape of a crystal, and in the present invention, may refer to a crystal plane including a flat surface of the carbon-based negative electrode active material, or a crystal plane including the a-axis / ab-axis of the carbon-based negative electrode active material crystal.

[0033] Furthermore, in this specification, the term "average particle size (D 50 ) refers to the particle size at which the cumulative value in the particle size distribution of the particles is 50%, and is also called the median diameter.

[0034] The present invention will now be described in more detail.

[0035] <Negative electrodes for lithium secondary batteries> In one embodiment, the present invention comprises: a negative electrode current collector; and a negative electrode active layer provided on the negative electrode current collector and containing a carbon-based negative electrode active material, The degree of alignment (OI) of the carbon-based negative electrode active material in the negative electrode active layer, represented by the following formula 1, is 0.1 to 5.0, The negative electrode for a lithium secondary battery is characterized in that the arithmetic mean height (Sa) of the surface of the negative electrode active layer is 3.0 μm to 10.0 μm.

[0036] [Formula 1] OI=I 004 / I 110

[0037] In formula 1, I 004 represents the area of ​​the peak showing the (004) crystal plane in the X-ray diffraction spectroscopy (XRD) measurement of the negative electrode active layer, I 110 represents the area of ​​the peak indicating the (110) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD).

[0038] The negative electrode for a lithium secondary battery according to the present invention includes a negative electrode active layer including a carbon-based negative electrode active material on at least one surface of a negative electrode current collector. The negative electrode active layer is a layer that realizes the electrical activity of the negative electrode, and is prepared by coating both surfaces of the electrode current collector with an electrode slurry including a negative electrode active material that realizes an electrochemical oxidation-reduction reaction during charging and discharging of the battery, and then drying and rolling the coating.

[0039] The negative electrode active layer includes a carbon-based negative electrode active material as a negative electrode active material to realize electrical activity through a reversible oxidation-reduction reaction during charging and discharging of the battery. Specifically, the carbon-based negative electrode active material means a material mainly composed of carbon atoms, and such a carbon-based negative electrode active material may include graphite. The graphite may include at least one of natural graphite and artificial graphite, and preferably includes natural graphite or a mixture of natural graphite and artificial graphite. For example, the carbon-based negative electrode active material may include natural graphite or artificial graphite alone, or may include a mixture of natural graphite and artificial graphite in some cases. In this case, the mixture ratio of natural graphite and artificial graphite may be 5 to 40:60 to 95, or 10 to 30:70 to 90, based on weight. The carbon-based negative electrode active material contains natural graphite and artificial graphite in the above-mentioned mixing ratio, and thus can realize high orientation of the carbon-based negative electrode active material on the surface of the negative electrode current collector while strengthening adhesion between the negative electrode current collector and the negative electrode active layer.

[0040] The carbon-based negative electrode active material is preferably a spherical graphite granule formed by the aggregation of a plurality of flake graphite. Examples of flake graphite include natural graphite, artificial graphite, mesophase calcined carbon (bulk mesophase) made from tar and pitch, graphitized cokes (raw coke, green coke, pitch coke, needle coke, petroleum coke, etc.), etc. In particular, a graphite granule assembled from a plurality of highly crystalline natural graphites is preferable. In addition, one graphite granule may be formed by the aggregation of 2 to 100 flake graphite particles, preferably 3 to 20 flake graphite particles.

[0041] Such a carbon-based negative electrode active material, specifically, graphite, may have a spherical particle shape, and the sphericity of the graphite particles may be 0.75 or more, for example, 0.75 to 1.0, 0.75 to 0.95, 0.8 to 0.95, or 0.90 to 0.99. Here, the "sphericity" may mean the ratio of the shortest diameter (minor axis) / longest diameter (major axis) among any diameters passing through the center of the particle, and when the sphericity is 1, it means that the particle shape is spherical. The sphericity may be measured using a particle shape analyzer. The present invention has the advantages of realizing a shape of the carbon-based negative electrode active material close to a sphere, thereby realizing high electrical conductivity of the negative electrode active layer, thereby improving the capacity of the battery, and increasing the specific surface area of ​​the negative electrode active material, thereby improving the adhesive force between the negative electrode active layer and the current collector.

[0042] In addition, the carbon-based negative electrode active material has an average particle size (D 50 ), specifically, the average particle size (D 50 ) can be shown.

[0043] The average particle size of the spherical natural graphite is preferably as small as possible to maximize the degree of disorder in the direction of expansion of each particle so as to prevent the expansion of the particles due to charging with lithium ions. However, if the particle size of the natural graphite is less than 0.5 μm, a large amount of binder is required due to the increase in the number of particles per unit volume, and the sphericity and sphericity yield may be reduced. On the other hand, if the maximum particle size exceeds 10 μm, the expansion becomes intense, and the adhesion between the particles and between the particles and the current collector decreases due to repeated charging and discharging, and the cycle characteristics may be significantly reduced.

[0044] The ab-axis crystal plane of the carbon-based anode active material in the anode active layer of the anode according to the present invention may be aligned in a direction perpendicular to the anode current collector by the magnetic alignment device according to the present invention described above. The present invention can further reduce the electrode resistance by aligning the ab-axis crystal plane of the carbon-based anode active material contained in the anode active layer to have a predetermined directionality with respect to the anode current collector, thereby further improving the charging performance of the anode active layer. Here, the degree to which the ab-axis crystal plane of the carbon-based anode active material (e.g., graphite) is aligned (i.e., the degree of orientation) can be determined by crystal plane analysis of graphite.

[0045] As one example, in the negative electrode active layer, the ab-axis crystal plane of the carbon-based negative electrode active material is aligned perpendicularly to the negative electrode current collector, and when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD), the degree of alignment (OI) of the carbon-based negative electrode active material, represented by the following Formula 1, may satisfy 0.1 to 5.0.

[0046] [Formula 1] OI=I 004 / I 110

[0047] In formula 1, I 004 represents the area of ​​the peak showing the (004) crystal plane in the X-ray diffraction spectroscopy (XRD) measurement of the negative electrode active layer, I 110 represents the area of ​​the peak indicating the (110) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD).

[0048] The crystal plane orientation of the carbon-based negative electrode active material can be determined by a crystal plane analysis of the carbon-based negative electrode active material, such as X-ray diffraction spectroscopy. The degree of alignment (OI) of the carbon-based negative electrode active material represented by the above formula 1 can be an index indicating the direction in which the crystal structure of the carbon-based negative electrode active material is aligned during X-ray diffraction measurement, specifically, the degree to which the ab-axis crystal plane indicating the two-dimensional planar structure of the carbon-based negative electrode active material is aligned with respect to the surface of the negative electrode current collector. For example, when the negative electrode active layer contains graphite as the carbon-based negative electrode active material, the negative electrode active layer exhibits 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2°, and 77.5±0.2°, which are peaks for graphite during X-ray diffraction spectroscopy analysis. This refers to the (002) plane, (100) plane, (101)R plane, (101)H plane, (004) plane, and (110) plane of the crystal planes of graphite contained in the negative electrode active layer. In general, in the case of graphite, graphene layers are placed on the a-axis and b-axis planes, and such graphene layers are stacked along the c-axis to have a hexagonal or rhombohedral crystal structure. Here, the above crystal plane peak is a peak that indicates the plane characteristics of such a crystal structure. In addition, the peak that appears at 2θ=43.4±0.2° may be considered to be an overlap of the peaks corresponding to the (101)R plane of the carbon-based material and the (111) plane of the current collector, for example, Cu.

[0049] In the present invention, the degree of alignment (OI) of graphite can be measured by the area ratio of the peak at 2θ=77.5±0.2° representing the (110) plane and the peak at 2θ=54.7±0.2° representing the (004) plane, specifically, the area ratio obtained by integrating the intensities of the above peaks. In addition, the X-ray diffraction was measured using CuK α rays as a target line, and the target line was extracted and measured using a monochromator device to improve the peak intensity resolution. At this time, the measurement conditions were 2θ=10° to 90°, a scan speed (° / s) of 0.044 to 0.089, and a step size of 0.026° / step. In addition, the (004) plane appearing at 2θ=54.7±0.2° indicates the thickness direction characteristic (c-axis direction characteristic) of the layered structure in which the two-dimensional planar structure of the graphite layers is laminated, and the (110) plane appearing at 2θ=77.5±0.2° indicates the planar characteristic (ab-axis direction characteristic) of the laminated graphite layers. Therefore, the smaller the (004) plane peak indicating the thickness direction characteristic of the graphite layer plane, and the larger the (110) plane peak indicating the planar characteristic of the graphite layer, the higher the angle at which the graphite plane is aligned with respect to the negative electrode current collector surface. In other words, the closer the OI value is to 0, the closer the angle or inclination of the graphite layer surface to the negative electrode current collector surface is to 90°, and the larger the OI value is, the closer the inclination to the negative electrode current collector surface is to 0° or 180°. In this respect, in the negative electrode active layer according to the present invention, since the carbon-based negative electrode active material is aligned perpendicular to the negative electrode current collector, the degree of graphite alignment (OI) may be lower than in a case where the carbon-based negative electrode active material is not aligned perpendicularly.Specifically, the degree of alignment of the carbon-based negative electrode active material contained in the negative electrode active layer may be 0.1 to 5.0, more specifically, 0.1 to 4.5, 0.1 to 4.0, 0.1 to 3.5, 0.1 to 3.0, 0.1 to 2.5, 0.1 to 2.0, 0.1 to 1.0, 0.5 to 2.9, 1.0 to 4.5, 1.1 to 4.1, 1.5 to 4.0, 1.1 to 3.5, 1.0 to 4 ... It can be 0.5 to 3.0, 0.9 to 2.9, 0.1 to 2.4, 0.1 to 2.1, 0.1 to 1.9, 2.0 to 5.0, 2.0 to 4.0, 2.1 to 3.9, 2.5 to 3.9, 3.1 to 4.5, 0.1 to 0.6, 0.15 to 0.6, 0.15 to 0.5, 0.2 to 0.5, 0.2 to 0.4, 0.25 to 0.45, or 0.3 to 0.5.

[0050] In addition, the negative electrode active layer may be induced to uniformly align the carbon-based negative electrode active material vertically relative to the negative electrode current collector, and the deviation between the degrees of alignment (OI) of a plurality of carbon-based negative electrode active materials measured arbitrarily within a given unit area may be small.

[0051] For example, in the negative electrode active layer, when X-ray diffraction spectroscopy (XRD) is measured at any three points in a unit area (10 cm x 10 cm) of the negative electrode active layer, the deviation in degree of alignment (OI) of the carbon-based negative electrode active material represented by Formula 1 may be less than 5% based on the average value, specifically, 4% or less, 3% or less, 2% or less, or 1% or less.

[0052] Furthermore, the negative electrode active layer has an arithmetic mean height (Sa) of the surface adjusted to a specific range, and thus has excellent surface characteristics. Specifically, the negative electrode active layer has an arithmetic mean height (Sa) of the surface that satisfies a specific range, and exhibits a characteristic of having significantly fewer defects such as scratches and crater-like grooves. For this reason, the negative electrode active layer may have an arithmetic mean height (Sa) of the surface of 3.0 μm to 10.0 μm, more specifically, 3.0 μm to 8.0 μm, 3.0 μm to 6.0 μm, or 3.5 to 5.0 μm. In this case, the arithmetic mean height (Sa) of the surface refers to the absolute average of the height difference between each point with respect to the average plane of the three-dimensional surface, and the lower this value, the lower the surface roughness. The arithmetic mean height (Sa) of the above surface is not particularly limited as long as it can measure the roughness of a three-dimensional surface, and specifically, it can be measured using an optical microscope, an X-ray photoelectron spectrometer (XPS), a laser confocal microscope, or the like.

[0053] The negative electrode active layer is prepared by applying a negative electrode slurry to a negative electrode current collector and drying it. Here, a magnetic force is applied to the negative electrode slurry before drying to align the carbon-based negative electrode active material contained in the negative electrode active layer. In general, the magnetic force applied to the negative electrode slurry induces a considerable stress on the carbon-based negative electrode active material contained in the negative electrode slurry, and may form scratches or crater-like grooves on the surface. Such scratches or crater-like grooves may induce surface unevenness that induces density differences in the active material in the negative electrode active layer, causing lithium plating to occur intensively at specific sites with high density, and thus causing deterioration of the electrode. However, the negative electrode according to the present invention may include a negative electrode active layer with excellent surface characteristics, in which scratches or crater-like grooves are not formed, even though the carbon-based negative electrode active material is aligned in a direction perpendicular to the negative electrode current collector, by controlling the arithmetic mean height (Sa) of the surface of the negative electrode active layer to a specific range.

[0054] In addition, the average thickness of the negative electrode active layer may be 50 μm to 300 μm, specifically 50 μm to 250 μm, 100 μm to 250 μm, or 100 μm to 200 μm. By adjusting the average thickness of the negative electrode active layer within the above range, the present invention not only increases the energy density of the electrode, but also applies a magnetic force uniformly to the inside of the negative electrode slurry during the preparation of the negative electrode active layer, thereby inducing uniform alignment of the carbon-based negative electrode active material.

[0055] Meanwhile, the negative electrode active layer according to the present invention may further selectively contain a conductive material, a binder, other additives, and the like, in addition to the negative electrode active material, as necessary.

[0056] The conductive material may include, but is not limited to, one or more of carbon black, acetylene black, ketjen black, carbon nanotubes, carbon fibers, and the like.

[0057] For example, the negative electrode active layer may contain carbon black, carbon nanotubes, carbon fibers, etc., alone or in combination, as a conductive material.

[0058] At this time, the content of the conductive material may be 0.1 to 10 parts by weight, specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, 2 to 6 parts by weight, or 0.5 to 2 parts by weight, based on 100 parts by weight of the total negative electrode active layer. By controlling the content of the conductive material within the above range, the present invention can prevent a decrease in charge capacity due to an increase in the resistance of the negative electrode caused by a low content of the conductive material. In addition, it can prevent problems such as a decrease in the content of the negative electrode active material due to an excessive amount of the conductive material, resulting in a decrease in charge capacity, or a decrease in rapid charge characteristics due to an increase in the loading amount of the negative electrode active layer.

[0059] The binder is a component that aids in bonding between the active material and the conductive material and between the active material and the current collector, and may be suitably used within a range that does not deteriorate the electrical properties of the electrode. Specifically, the binder may include any one or more of vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, and fluororubber.

[0060] The content of the binder may be 0.1 to 10 parts by weight, specifically 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, or 2 to 6 parts by weight, based on 100 parts by weight of the total negative electrode active layer. By controlling the content of the binder contained in the negative electrode active layer within the above range, the present invention can prevent a decrease in adhesive strength of the active layer due to a low content of the binder, or a decrease in electrical properties of the electrode due to an excessive amount of the binder.

[0061] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, nickel, titanium, calcined carbon, etc., and in the case of copper or stainless steel, it may be surface-treated with carbon, nickel, titanium, silver, etc. The average thickness of the negative electrode current collector may be suitably 1 to 500 μm, taking into consideration the conductivity and total thickness of the negative electrode to be manufactured.

[0062] <Magnetic alignment device for negative electrodes> In one embodiment, the present invention comprises: A magnetic alignment apparatus for manufacturing a negative electrode for aligning a carbon-based negative electrode active material, a first magnet unit and a second magnet unit, which are respectively located at an upper portion and a lower portion of a negative electrode current collector coated with a negative electrode slurry including a carbon-based negative electrode active material in a moving direction of the negative electrode current collector and apply a magnetic force; a drying unit that dries the negative electrode slurry to which magnetic force is applied by the first magnet unit and the second magnet unit, The first magnet unit and the second magnet unit are each divided into a first region located upstream and a second region located downstream based on a transport direction of the negative electrode current collector, The present invention provides a magnetic alignment device, wherein a magnetic field having a stronger magnetic force is applied to the first region than to the second region.

[0063] The magnetic alignment device for a negative electrode according to the present invention is an apparatus applied in manufacturing a negative electrode for use in a secondary battery, and can align the ab-axis crystal plane of the carbon-based negative active material contained in the negative electrode slurry in a direction perpendicular or nearly perpendicular to the negative electrode current collector by applying a magnetic field to the surface of the negative electrode current collector on which a negative electrode slurry containing a carbon-based negative active material is applied, i.e., the surface of the negative electrode slurry. The magnetic alignment device can realize uniform alignment of the carbon-based negative active material contained in the negative electrode slurry. The negative electrode manufactured in this manner can exhibit the effect of increasing the mobility of lithium ions and reducing resistance during charging and discharging of the battery, thereby improving charge and discharge performance.

[0064] Here, being aligned in a direction perpendicular to the negative electrode current collector means that the crystal plane of the carbon-based negative electrode active material is aligned. Specifically, "the carbon-based negative electrode active material is aligned perpendicular to the negative electrode current collector" may mean that the crystal plane of the carbon-based negative electrode active material constituting the spherical particles, specifically, the crystal plane showing the plane direction of the graphite having a two-dimensional structure among the crystal planes of graphite, is aligned perpendicular to the surface of the negative electrode current collector. At this time, the plane direction of the graphite may have an average inclination of 60 to 120° with respect to the negative electrode current collector, and preferably has an average inclination of 70 to 110° or 80 to 100°.

[0065] To this end, as shown in FIG. 1, the magnetic alignment device 10 according to the present invention includes a first magnet unit 110a and a second magnet unit 110b that are respectively positioned at the upper and lower parts along the transport direction of a negative electrode current collector coated with a negative electrode slurry containing a carbon-based negative electrode active material and apply a magnetic force, and a drying unit 120 that dries the negative electrode slurry to which the magnetic force is applied by the first magnet unit 110a and the second magnet unit 110b.

[0066] In the magnetic alignment device, the first magnet unit 110a and the second magnet unit 110b are disposed on the upper and lower parts, respectively, of the electrode sheet being moved, i.e., the negative electrode current collector on which the negative electrode slurry is applied, and serve to apply a magnetic field to the surface of the negative electrode slurry S.

[0067] At this time, the first magnet section 110a and the second magnet section 110b may include magnets 111a and 111b, and support sections 112a and 112b for fixing the magnets, in order to apply a magnetic field to the surface of the negative electrode slurry S, respectively.

[0068] 2, if the direction in which the negative electrode current collector coated with the negative electrode slurry S is transported is defined as the x-axis direction and the width direction of the transported negative electrode current collector is defined as the y-axis, the first magnet section 110a and the second magnet section 110b may include a plurality of unit magnets in the x-axis direction and the y-axis direction, respectively. The unit magnets may form magnet rows including m (where m is an integer of 2 or more) and n (where n is an integer of 2 or more) unit magnets in the x-axis direction and the y-axis direction, respectively, so that one magnet section may include m×n unit magnets.

[0069] The first magnet section 110a and the second magnet section 110b may be divided into first regions 1111a and 1111b located upstream in the direction of transport of the negative electrode current collector, i.e., the x-axis direction, and second regions 1112a and 1112b located downstream. Here, the first regions 1111a and 1111b may apply a magnetic field having a stronger magnetic force (or magnetic field) than the second regions 1112a and 1112b.

[0070] This difference in magnetic strength may be realized in a manner commonly applied in the art, but preferably, the unit magnets arranged in the first regions 1111a and 1111b are arranged in a Halbach array, and the unit magnets arranged in the second regions 1112a and 1112b are arranged so that the magnetic force of the N pole or S pole (i.e., a single pole) is exposed on the surface of the magnet part to apply a uniform magnetic field. Here, the Halbach array refers to an arrangement method in which the arrangement of the unit magnets is controlled to improve the electric field strength, and a magnetic force 1.5 times stronger than when the unit magnets are arranged with the same pole can be realized. In the present invention, by arranging a plurality of unit magnets having a Halbach array in the first regions 1111a and 1111b of the first magnet unit and the second magnet unit, a strong magnetic field is applied to the first regions 1111a and 1111b located upstream based on the transport direction when the negative electrode slurry is transported, and then a relatively weaker magnetic field is applied to the second regions 1112a and 1112b located downstream compared to the first regions 1111a and 1111b. As a result, the present invention can prevent the degree of alignment of the carbon-based negative electrode active material aligned perpendicular to the negative electrode current collector from being reduced due to the strong magnetic field at the end of the magnet unit, and can reduce stress on the negative electrode slurry, thereby improving the surface characteristics of the negative electrode active layer to be manufactured.

[0071] At this time, the first regions 1111a and 1111b and the second regions 1112a and 1112b may have a certain ratio of the magnetic force applied to the surfaces of the first magnet portion 110a and the second magnet portion 110b and / or the magnetic force applied to the space between the first magnet portion 110a and the second magnet portion 110b.

[0072] As one example, the first regions 1111a and 1111b may apply a magnetic force to the space between the first magnet section 110a and the second magnet section 110b of 8,000 G or more, 9,000 G or more, 10,000 G or more, 8,000 to 12,000 G, or 8,500 to 11,000 G, and the ratio of the magnetic force of the first regions 1111a and 1111b to the magnetic force of the second regions 1112a and 1112b may be 1.4 or more, 1.5 or more, 1.6 or more, 1.4 to 2.5, 1.4 to 2.2, 1.5 to 1.8, or 1.6 to 2.0.

[0073] As another example, the first regions 1111a and 1111b may have a magnetic force applied to the surfaces of the first magnet portion 110a and the second magnet portion 110b of 10,000 G or more, 11,000 G or more, 10,000 to 15,000 G, 10,000 to 12,000 G, or 11,000 to 12,000 G, and the ratio of the magnetic force of the first regions 1111a and 1111b to the magnetic force of the second regions 1112a and 1112b may be 1.4 or more, 1.5 or more, 1.6 or more, 1.4 to 5.0, 1.4 to 3.0, 1.4 to 2.5, or 1.5 to 2.0.

[0074] The ratio of the sizes of the first regions 1111a and 1111b and the second regions 1112a and 1112b may be adjusted to a constant value. Specifically, the length of the first regions 1111a and 1111b in the direction of movement of the negative electrode current collector may be shorter than that of the second regions 1112a and 1112b. Specifically, the first regions 1111a and 1111b may occupy 5 to 50% of the total length of the first magnet portion 110a and the second magnet portion 110b, more specifically 5 to 40%, 10 to 30%, or 10 to 20%, and the remainder may be occupied by the second regions 1112a and 1112b. As an example, the first regions 1111a and 1111b may occupy 15% of the total length of the first magnet portion 110a and the second magnet portion 110b, and the second regions 1112a and 1112b may be continuously connected to the first regions 1111a and 1111b and may occupy 85% of the total length of the first magnet portion 110a and the second magnet portion 110b.

[0075] By adjusting the lengths of the first regions 1111a and 1111b and the second regions 1112a and 1112b as described above, the present invention can not only effectively control the alignment of the carbon-based negative electrode active material, but also significantly reduce the stress on the negative electrode slurry.

[0076] Meanwhile, the unit magnets 111a and 111b may include electromagnets and / or permanent magnets. The electromagnets may include both DC and AC electromagnets. The permanent magnets may include both ferromagnetic magnets and soft magnetic magnets, including NdFeB magnets, SmCo magnets, ferrite magnets, alnico magnets, FeCrCo magnets, and bond magnets (Nd-Fe-B, Sm-Fe-N, Sm-Co, and ferrite magnets).

[0077] In addition, the first magnet unit 110a and the second magnet unit 110b may be positioned along the transfer direction of the negative electrode slurry S to face each other and may be arranged to have opposite poles. For example, the N pole of the first magnet 111a of the first magnet unit 110a may face the S pole of the second magnet 111b of the second magnet unit 110b, or the S pole of the first magnet 111a of the first magnet unit 110a may face the N pole of the second magnet 111b of the second magnet unit 110b. When the electrode sheet passes through the space in which the N pole and the S pole face each other, the vertical alignment of the carbon-based negative electrode active material with respect to the negative electrode current collector C may be more effectively performed between the first magnet unit 110a and the second magnet unit 110b.

[0078] In addition, the distance between the first magnet part 110a and the second magnet part 110b may be 10 mm to 50 mm, specifically, 10 mm to 40 mm, 20 mm to 50 mm, or 15 mm to 45 mm. By adjusting the distance between the first magnet part 110a and the second magnet part 110b within the above range, the present invention can more efficiently align the carbon-based negative electrode active material contained in the negative electrode slurry S.

[0079] Furthermore, the first magnet part 110a and the second magnet part 110b may have a length of 0.5 m to 10 m in the direction of movement of the negative electrode current collector (i.e., the x-axis direction), and the length of the first magnet part 110a and the second magnet part 110b may be suitably adjusted according to the movement speed of the negative electrode current collector coated with the negative electrode slurry and / or the time for which a magnetic force is applied to the negative electrode slurry when manufacturing the negative electrode. For example, when the movement speed of the negative electrode current collector coated with the negative electrode slurry is 3±0.2 m / min, the length of the first magnet part 110a and the second magnet part 110b may be 3±0.5 m, and when the movement speed is 6±0.2 m / min, the length of the first magnet part 110a and the second magnet part 110b may be 6±0.5 m. In the present invention, by adjusting the overall length of the first magnet portion 110a and the second magnet portion 110b as described above, the alignment of the carbon-based negative electrode active material contained in the negative electrode slurry can be nearly vertical.

[0080] In addition, the magnetic alignment device 10 may be combined with a transfer unit 20 to transfer the negative electrode current collector coated with the negative electrode slurry including the carbon-based negative electrode active material in one direction, specifically, in the process direction. To this end, the transfer unit 20 may be applied in any manner commonly used in the industry to transfer the electrode sheet C coated with the electrode slurry S during electrode manufacturing, without any particular limitations. For example, the transfer unit 20 may be applied in a roll-to-roll manner or a conveyor belt transfer manner capable of applying a magnetic field.

[0081] Furthermore, in the magnetic alignment apparatus, the drying unit 120 serves to fix the aligned carbon-based negative electrode active material by drying the negative electrode slurry S in which the carbon-based negative electrode active material is aligned by the first magnet unit 110a and the second magnet unit 110b.

[0082] The drying section 120 includes a wall (not shown) that blocks the periphery except for an entrance / exit through which the electrode sheet coated with the slurry S is introduced and conveyed out, and a dryer (not shown) for drying the electrode sheet on the wall on the side from which the electrode sheet coated with the electrode slurry is drawn out.

[0083] When the electrode sheet C coated with the electrode slurry S enters through the inlet of the drying unit 120, energy such as light, heat, and the like supplied from the wall on the opposite side is transferred to the electrode sheet C. Therefore, the wall is preferably made of a heat insulating material to prevent internal energy from being transferred to the outside and causing heat loss.

[0084] In addition, the drying unit 120 may have a configuration in which a two-step drying process is performed to maintain the alignment of the carbon-based negative electrode active material contained in the negative electrode active layer, although the type thereof is not limited thereto. Specifically, the drying unit 120 may include a first dryer that dries the negative electrode slurry using light and a second dryer that dries the negative electrode slurry using heat, and the first dryer and the second dryer may be operated continuously to dry the negative electrode slurry.

[0085] The first dryer is a device for pre-drying the negative electrode slurry, and may irradiate light or wavelengths onto the surface of the negative electrode slurry as described above. In general, the negative electrode slurry is dried by applying hot air at a high temperature, but in this case, the alignment of the carbon-based negative electrode active material in the negative electrode slurry may be disturbed since it takes a long time to dry the negative electrode slurry. In addition, if the temperature of the hot air is increased to solve this problem, the tendency of the slurry surface to dry increases, and a phenomenon (migration) occurs in which the binder is concentrated on the slurry surface together with the volatilized solvent, resulting in a decrease in the adhesive strength between the active material layer and the negative electrode current collector. In order to dry the negative electrode slurry while maintaining a high degree of alignment of the carbon-based negative electrode active material without such a problem, the present invention may be configured to pre-dry the electrode slurry by irradiating energy in the form of light or wavelengths using the first dryer. The first dryer may include, for example, an ultraviolet dryer, a near infrared dryer, a far infrared dryer, etc., and may specifically include a far infrared dryer that emits energy with a wavelength of 1 μm or more, more specifically, 5 μm or more, 10 μm or more, or 20 μm or more in order to realize a uniform drying speed of the electrode slurry. The far infrared dryer is different from near infrared dryers and infrared rays commonly used in the industry in that it has a long light or wavelength and is energy efficient. In addition, it has an advantage that it can apply energy uniformly not only to the surface of the negative electrode slurry but also to the inside, thereby increasing the adhesive strength between the negative electrode slurry and the negative electrode current collector in a short time.

[0086] At this time, the first dryer is 50 kW / m 2 ~1,000kW / m 2 The power density of the device is 50 kW / m. 2 ~500kW / m 2 , 50kW / m 2 ~250kW / m 2 , or 50 kW / m 2 and 200 kW / m 2 In the present invention, by controlling the power density of the first dryer within the above range, it is possible to prevent uneven drying of the active material layer caused by an excessive power density.

[0087] In addition, the second dryer may apply heat to the negative electrode slurry pre-dried by light or wavelength to uniformly and completely dry it. The second dryer may include any dryer commonly used in the art without any particular limitation, and may include, for example, a hot air dryer, a vacuum oven, etc., used alone or in combination.

[0088] The magnetic alignment device according to the present invention has the above-mentioned configuration, and thus can reduce the attractive force of the carbon-based negative electrode active material caused by the magnetic force generated at the end of the magnet portion, thereby significantly increasing the degree of alignment of the carbon-based negative electrode active material contained in the negative electrode slurry. In addition, the surface characteristics of the manufactured negative electrode active layer are excellent, which is advantageous in that a negative electrode having excellent electrical performance can be manufactured.

[0089] <Method of manufacturing the negative electrode> In one embodiment, the present invention further comprises: applying a negative electrode slurry including a carbon-based negative electrode active material onto a negative electrode current collector; Aligning the carbon-based negative electrode active material contained in the negative electrode slurry using the magnetic alignment device according to the present invention; and drying the negative electrode slurry in which the carbon-based negative electrode active material is aligned to form a negative electrode active layer.

[0090] In the method for manufacturing a negative electrode according to the present invention, a negative electrode slurry containing a carbon-based negative electrode active material is applied onto a negative electrode current collector, and a magnetic field is applied to the surface of the applied negative electrode slurry using the magnetic alignment device of the present invention described above. This makes it possible to align the carbon-based negative electrode active material in the negative electrode slurry perpendicular or nearly perpendicular to the surface of the negative electrode current collector (or to the conveying direction of the electrode sheet). Since the aligned carbon-based negative electrode active material in the slurry is subjected to a considerable stress after alignment of the carbon-based negative electrode active material, it is possible to prevent the formation of scratches or crater-like grooves on the surface of the manufactured negative electrode active layer.

[0091] In the method for preparing the negative electrode, the steps of applying the negative electrode slurry to the negative electrode current collector and drying the negative electrode slurry may be performed in a manner commonly used in the art.

[0092] In addition, the step of aligning the carbon-based negative active material contained in the negative electrode slurry may be performed by sequentially applying magnetic fields having different magnetic forces to the negative electrode slurry coated on the surface of the negative electrode current collector using a magnetic alignment device according to the present invention.

[0093] The magnetic alignment device has a first magnet unit and a second magnet unit respectively disposed above and below the negative current collector along the transport direction of the negative current collector (i.e., the x-axis direction). At this time, the first magnet unit and the second magnet unit can be divided into first regions 1111a and 1111b located upstream in the transport direction of the negative current collector, i.e., the x-axis direction, and second regions 1112a and 1112b located downstream, and the first regions 1111a and 1111b can apply a magnetic field with a stronger magnetic force than the second regions 1112a and 1112b.

[0094] In this case, the first regions 1111a and 1111b and the second regions 1112a and 1112b may have a certain ratio of the magnetic force applied to the surfaces of the first magnet portion and the second magnet portion and / or the magnetic force applied to the space between the first magnet portion and the second magnet portion.

[0095] As one example, the first regions 1111a and 1111b may apply a magnetic force to the space between the first magnet section 110a and the second magnet section 110b of 8,000 G or more, 9,000 G or more, 10,000 G or more, 8,000 to 12,000 G, or 8,500 to 11,000 G, and the ratio of the magnetic force of the first regions 1111a and 1111b to the magnetic force of the second regions 1112a and 1112b may be 1.4 or more, 1.5 or more, 1.6 or more, 1.4 to 2.5, 1.4 to 2.2, 1.5 to 1.8, or 1.6 to 2.0.

[0096] As another example, the first regions 1111a and 1111b may have a magnetic force applied to the surfaces of the first magnet portion 110a and the second magnet portion 110b of 10,000 G or more, 11,000 G or more, 10,000 to 15,000 G, 10,000 to 12,000 G, or 11,000 to 12,000 G, and the ratio of the magnetic force of the first regions 1111a and 1111b to the magnetic force of the second regions 1112a and 1112b may be 1.4 or more, 1.5 or more, 1.6 or more, 1.4 to 5.0, 1.4 to 3.0, 1.4 to 2.5, or 1.5 to 2.0.

[0097] The present invention aligns the carbon-based negative electrode active material contained in the negative electrode slurry using the magnetic alignment device having the above-described configuration, thereby preventing the degree of alignment of the carbon-based negative electrode active material aligned perpendicular to the negative electrode current collector from being reduced due to a strong magnetic field at the end of the magnet, and reducing stress on the negative electrode slurry, thereby improving the surface characteristics of the manufactured negative electrode active layer.

[0098] Moreover, the magnetic field may be applied for a time period of 0.1 to 20 seconds, and more specifically, for a time period of 0.5 to 15 seconds, 0.5 to 12 seconds, 1 to 10 seconds, 2 to 8 seconds, or 2 to 5 seconds.

[0099] Meanwhile, the carbon-based negative electrode active material contained in the negative electrode slurry may include those commonly used as a carbon-based negative electrode active material for lithium secondary batteries. Specifically, the carbon-based negative electrode active material means a material mainly composed of carbon atoms, and such a carbon-based negative electrode active material may include graphite. The graphite may include at least one of natural graphite and artificial graphite, and preferably includes natural graphite or a mixture of natural graphite and artificial graphite.

[0100] In addition, the negative electrode slurry may further include a conductive material, a binder, a thickener, and the like in addition to the carbon-based negative electrode active material, and these may be materials commonly used in the art.

[0101] The present invention will now be described in more detail with reference to examples and experimental examples.

[0102] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.

[0103] <Examples and Comparative Examples: Production of negative electrode for lithium secondary battery> Using the magnetic alignment apparatus of the present invention having the structure shown in FIG. 1, a negative electrode for a lithium secondary battery in which a carbon-based negative electrode active material is aligned perpendicularly to a negative electrode current collector was manufactured.

[0104] Specifically, natural graphite was first prepared as the negative electrode active material, and 97 parts by weight of the negative electrode active material and 3 parts by weight of styrene butadiene rubber (SBR) were mixed with water to form a negative electrode slurry, which was then cast onto a copper sheet being transported roll-to-roll (transport speed: 5 m / min) using a die coater. At this time, the negative electrode slurry was cast to an average thickness of 165 μm along the transport direction of the copper sheet.

[0105] Then, a magnetic field was applied to the negative electrode slurry by moving the copper sheet so that the applied negative electrode slurry passed between the first and second magnet parts of the magnetic alignment device. Here, the first and second magnet parts were adjusted so that the separation distance was 20 mm (half the separation distance: 10 mm).

[0106] In addition, the first magnet unit and the second magnet unit are divided into a first region located upstream and a second region located downstream based on the direction of movement of the negative electrode current collector, and (1) the arrangement of the unit magnets included in the first region and the second region, respectively, (2) the magnetic field strength of the magnet surface included in each region, and (3) the length of the first region in the direction of movement of the negative electrode current collector (L 1 ) and the second region length (L 2 ) ratio (L 1 / L 2 ) were adjusted as shown in Table 1 below.

[0107] In addition, in order to dry the negative electrode slurry to which the magnetic field was applied, the copper sheet to which the magnetic field was applied was moved to a drying section, and the negative electrode slurry was dried to prepare a negative electrode for a lithium secondary battery.

[0108] [Table 1]

[0109] <Experimental example.> In order to evaluate the performance of the magnetic alignment device according to the present invention, such as the degree of alignment of the carbon-based negative electrode active material and the surface characteristics of the negative electrode active layer, the following experiments were carried out.

[0110] A) Alignment degree of carbon-based negative electrode active material X-ray diffraction spectroscopy (XRD) was performed on the negative electrode active layers of the negative electrodes manufactured in Examples 1 and 2 and Comparative Examples 1 to 3 to measure the spectra. The measurement conditions for the X-ray diffraction (XRD) were as follows.

[0111] - Target: Cu (Kα-ray) Graphite monochromator - Slit: Divergence slit = 1 degree, Receiving slit = 0.1mm, Scattering slit = 1 degree - Measurement area: (110) plane: 76.5 degrees < 2θ < 78.5 degrees / (004) plane: 53.5 degrees < 2θ < 56.0 degrees

[0112] From the spectra measured under the above conditions, the average degree of alignment (OI) of each carbon-based negative electrode active material according to formula 1 was calculated. The results are shown in Table 2.

[0113] [Formula 1] OI=I 004 / I 110

[0114] In formula 1, I 004 represents the area of ​​the peak showing the (004) crystal plane in the X-ray diffraction spectroscopy (XRD) measurement of the negative electrode active layer, I 110represents the area of ​​the peak indicating the (110) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD).

[0115] B) Surface characteristics of the negative electrode active layer First, for the negative electrodes manufactured in Examples 1-2 and Comparative Examples 1-3, i) surface damage of the negative electrode active layer was confirmed by the naked eye. Next, ii) an optical microscope analysis was performed on the surface of the negative electrode active layer. At this time, the optical microscope was equipped with software that calculates the arithmetic mean height (Sa) of the surface from the analyzed image, and the software was set to calculate the arithmetic mean height (Sa) of the surface according to ISO25178.

[0116] i) the surface damage results observed with the naked eye and ii) the arithmetic mean height (Sa) of the negative electrode active layer surface calculated by optical microscopy are shown in Table 2 below.

[0117] [Table 2]

[0118] As shown in Table 2, the negative electrode for a lithium secondary battery manufactured using the magnetic alignment apparatus according to the present invention has a high degree of alignment of the carbon-based negative electrode active material, and it is possible to manufacture a negative electrode for a lithium secondary battery having excellent surface characteristics. Specifically, the negative electrode of the embodiment manufactured using the magnetic alignment apparatus according to the present invention has a high degree of alignment of the carbon-based negative electrode active material (I 004 / I 110 ) was extremely low at less than 0.5, and it was confirmed that not only was there no surface damage to the negative electrode active layer, but also that the arithmetic mean height (Sa) of the negative electrode active layer surface satisfied the range of 3.0 to 6.0 μm.

[0119] This means that the magnetic alignment device according to the present invention is equipped with a magnet unit in which a first region located upstream in the transport direction of the negative electrode current collector applies a stronger magnetic force than a second region located downstream, so that the degree of alignment of the carbon-based negative electrode active material contained in the negative electrode slurry and the arithmetic mean height (Sa) of the surface of the negative electrode active layer can be adjusted within a specific range.

[0120] Although the present invention has been described above with reference to preferred embodiments, it will be understood that a person skilled in the art or having ordinary knowledge in the art may make various modifications and changes to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.

[0121] Therefore, the technical scope of the present invention is not limited to the contents described in the Summary of the Invention of the specification, but is defined by the claims. [Explanation of symbols]

[0122] 10: Magnetic alignment device 20:Transfer section 30: Coating section 110a: 1st magnet part 110b: Second magnet part 111a, 111b: a plurality of unit magnets 112a, 112b: Support part 1111a, 1111b: 1st area 1112a, 1112b: 2nd area 120:Drying section S: Negative electrode slurry C: Negative electrode current collector or electrode sheet

Claims

1. a negative electrode current collector; and a negative electrode active layer provided on the negative electrode current collector and containing a carbon-based negative electrode active material, The degree of alignment (O.I) of the carbon-based negative electrode active material in the negative electrode active layer, represented by the following formula 1, is 0.1 to 5.0, The arithmetic mean height (Sa) of the surface of the negative electrode active layer is 3.0 μm to 10.0 μm; [Formula 1] O.I=I 004 / I 110 In Formula 1, I 004 represents the area of ​​the peak indicating the (004) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD), I 110 represents the area of ​​the peak showing the (110) crystal plane when the negative electrode active layer is measured by X-ray diffraction spectroscopy (XRD), negative electrode for lithium secondary battery.

2. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the average thickness of the negative electrode active layer is 50 μm to 300 μm.

3. The negative electrode for a lithium secondary battery according to claim 1 or 2, wherein the carbon-based negative electrode active material includes at least one of natural graphite and artificial graphite.

4. A magnetic alignment apparatus for manufacturing a negative electrode for aligning a carbon-based negative electrode active material, a first magnet unit and a second magnet unit, which are respectively positioned at an upper portion and a lower portion of a negative electrode current collector coated with a negative electrode slurry including a carbon-based negative electrode active material in a moving direction of the negative electrode current collector and apply a magnetic force; a drying unit that dries the negative electrode slurry to which magnetic force is applied by the first magnet unit and the second magnet unit, The first magnet unit and the second magnet unit are each divided into a first region located upstream and a second region located downstream based on a transport direction of the negative electrode current collector, A magnetic alignment device, wherein a magnetic field having a stronger magnetic force is applied to the first region than to the second region.

5. the first magnet portion and the second magnet portion each include a plurality of unit magnets arranged in a transport direction (x-axis direction) and a width direction (y-axis direction) of the negative electrode current collector, 5. The magnetic alignment device according to claim 4, wherein the unit magnets arranged in the first region of the first magnet portion and the first region of the second magnet portion among the plurality of unit magnets are arranged in a Halbach array.

6. The magnetic alignment device according to claim 4 , wherein the first region of the first magnet portion and the second magnet portion is shorter than the second region of the first magnet portion in the transfer direction of the negative electrode current collector.

7. A magnetic alignment device as described in claim 4 or 5, wherein the first region of the first magnet portion and the first region of the second magnet portion each occupy a length of 5% to 50% based on the total length of the first magnet portion and the second magnet portion.

8. 6. The magnetic alignment device according to claim 4, wherein the first magnet portion and the second magnet portion each have a length of 0.5 m to 10 m in a direction in which the negative electrode current collector is transferred.

9. The magnetic alignment device according to claim 4 or 5, wherein the separation distance between the first magnet portion and the second magnet portion is 10 mm to 50 mm.

10. The magnetic alignment device of claim 4 or 5, wherein the first magnet portion and the second magnet portion include magnets having opposite poles.

11. applying a negative electrode slurry including a carbon-based negative electrode active material onto a negative electrode current collector; aligning a carbon-based negative electrode active material contained in a negative electrode slurry using the magnetic alignment device according to claim 4; and drying the negative electrode slurry in which the carbon-based negative electrode active material is aligned to form a negative electrode active layer.

12. The magnetic alignment device includes a first magnet unit and a second magnet unit, which are respectively located at an upper portion and a lower portion along a transport direction of the negative electrode current collector on which the negative electrode slurry is applied, and are divided into a first region located upstream and a second region located downstream in the transport direction, The method for producing a negative electrode according to claim 11 , wherein a ratio of the magnetic force applied in the first region to the magnetic force applied in the second region is 1.4 or more.

13. The method for producing a negative electrode according to claim 12 , wherein a magnetic force of 8,000 G or more is applied to the first region.

Citation Information

Patent Citations

  • Device for increasing compaction density of lithium iron phosphate cathode material

    CN203826481U

  • Negative electrode for nonaqueous electrolyte secondary battery

    JP2004220926A

  • Nonaqueous electrolyte secondary battery and manufacturing method thereof

    JP2019067543A

  • Method and device for applying a magnetic field to an article

    JP2019534155A

  • Negative electrode material sheet for non-aqueous secondary battery, manufacturing method thereof, negative electrode for non-aqueous secondary battery, and non-aqueous secondary battery

    JP2023060651A

Cited By

  • Method and device for manufacturing electrode for secondary battery

    JP2025002395A