Stretchable Sheet

The elastic sheet with alternating high and low stretch regions and high molecular weight resins addresses stress relaxation issues, maintaining a secure fit and ease of wear in absorbent articles.

JP3249047UActive Publication Date: 2024-11-08KAO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024003036U
Authority / Receiving Office
JP · JP
Patent Type
Utility models
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-08
Estimated Expiration
2031-10-28

AI Technical Summary

Technical Problem

Elastic fibers in stretchable sheets used in absorbent articles like disposable diapers experience stress relaxation due to body heat, leading to reduced fit and increased likelihood of slipping off over time, and increasing the difficulty of putting them on.

Method used

An elastic sheet with elastic filaments arranged in one direction and bonded to a stretchable nonwoven fabric, featuring high and low stretch regions alternately arranged perpendicular to the stretch direction, and using high molecular weight elastic resins to maintain stress retention.

Benefits of technology

The elastic sheet maintains a high stress retention rate, ensuring a secure fit and ease of wear, reducing slipping and making it easier to put on absorbent articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0003249047000001_ABST
    Figure 0003249047000001_ABST
Patent Text Reader

Abstract

Provided is a stretch sheet in which the ratio of shrinkage stress after a certain period of time to the initial shrinkage stress is large. [Solution] The stretch sheet 10 has a plurality of elastic filaments 13 arranged to extend in one direction bonded to extensible nonwoven fabrics 11, 12. High elongation regions and low elongation regions extending in a direction perpendicular to the stretch direction of the stretch sheet 10 are alternately arranged along said stretch direction. The elastic filaments 13 are fused to the nonwoven fabrics 11, 12 in a substantially unstretched state. The stress retention rate is 50% or more. The elastic filaments 13 contain a thermoplastic elastomer and oil.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretch sheet. [Background technology]

[0002] As a conventional technique for a stretch sheet made by combining elastic fibers and nonwoven fabric, the present applicant previously proposed a stretch sheet in which a large number of elastic filaments arranged to extend in one direction without crossing each other are bonded to a stretchable nonwoven fabric over their entire length in a substantially unstretched state (see Patent Document 1). Since the elastic filaments of this stretch sheet are arranged to extend in one direction, it has the advantage that it can be stretched in the direction in which the elastic filaments extend without causing width contraction. In addition, this stretch sheet has the advantage that it has high strength and is less likely to peel off from the elastic filaments and the nonwoven fabric when the stretch sheet is stretched.

[0003] When the stretch sheet is used as an outer layer sheet in an absorbent article such as a disposable diaper, the excellent stretchability of the stretch sheet allows the absorbent article to fit well to the wearer's body, effectively preventing leakage of excrement, etc. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-179128 A Summary of the Invention [Problem to be solved by the invention]

[0005] It is known that when elastic fibers are stretched and maintained in a stretched state for a long time, a phenomenon occurs in which stress is reduced due to stress relaxation. In particular, when the above-mentioned stretch sheet is used as an outer body of a disposable diaper, the elastic fibers are heated by the body temperature of the wearer, and stress relaxation is likely to be promoted. Therefore, when an absorbent article including a stretch sheet having elastic fibers is put on a wearer, even if it shows an appropriate fit in the initial state of wearing, the fit decreases after wearing for a long time, and the absorbent article is likely to slip off. If the contraction stress of the stretch sheet is increased to prevent the absorbent article from slipping off, excessive force is required when putting the absorbent article on the wearer, making it difficult to put it on. Therefore, the present invention relates to a stretch sheet that, when used in an absorbent article, is easy to put on and does not easily slip down. [Means for solving the problem]

[0006] The present invention provides a stretch sheet in which a plurality of elastic filaments arranged to extend in one direction are bonded to an extensible nonwoven fabric. It is preferable that high elongation regions and low elongation regions extending in a direction perpendicular to the stretch direction of the stretch sheet are alternately arranged along the stretch direction. The elastic filaments are preferably fused to the nonwoven fabric in a substantially unstretched state. The stretch sheet preferably has a stress retention rate of 50% or more. Effect of the Invention

[0007] According to the present invention, a stretch sheet is provided in which the ratio of shrinkage stress after a certain period of time to the initial shrinkage stress is large. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a partially cutaway perspective view showing one embodiment of the stretch sheet of the present invention. [Diagram 2]2(a) and 2(b) are longitudinal cross-sectional views of the stretch sheet shown in FIG. 1 in its natural state and in its stretched state, respectively, along the direction in which the elastic filaments extend. [Diagram 3] FIG. 3 is a schematic diagram showing an apparatus that is preferably used for producing the stretch sheet shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described below based on its preferred embodiments. The present invention relates to a stretch sheet comprising elastic filaments and nonwoven fabric. In this specification, elasticity and stretchability refer to the property of being able to be stretched and returning to a length of 125% or less of the original length when the force is released from a state in which the sheet is stretched 100% of its original length (i.e., 200% of the original length).

[0010] The stretch sheet of the present invention may have, for example, one nonwoven fabric and a plurality of elastic filaments arranged on one side of the nonwoven fabric. Alternatively, the stretch sheet of the present invention may have two nonwoven fabrics and a plurality of elastic filaments arranged between the two nonwoven fabrics. Each elastic filament is bonded to the nonwoven fabric. When an elastic filament is arranged between two nonwoven fabrics, each elastic filament is bonded to at least one of the nonwoven fabrics or to both nonwoven fabrics. When an elastic filament is arranged between two nonwoven fabrics, the two nonwoven fabrics may be of the same type or different types. In this specification, the term "same type of nonwoven fabric" refers to nonwoven fabrics that are all the same in terms of the manufacturing process of the nonwoven fabric, the type of constituent fiber of the nonwoven fabric, the fiber diameter and length of the constituent fiber, the thickness and basis weight of the nonwoven fabric, etc. When at least one of these is different, the nonwoven fabrics are said to be of different types.

[0011] The elastic filaments and the nonwoven fabric are preferably joined by fusion. By joining the two by fusion, the stretch sheet can be made flexible and highly stretchable. If, for example, an adhesive is used to join the two, the stretch sheet tends to feel hard due to the solidification of the adhesive. In addition, the adhesive tends to inhibit the stretching of the elastic filaments.

[0012] The stretch sheet is stretchable in the same direction as the elastic filaments extend. The stretchability of the stretch sheet is due to the elasticity of the elastic filaments. When the stretch sheet is stretched in the same direction as the elastic filaments extend, the elastic filaments 1 and the nonwoven fabric are elongated. When the stretch sheet is released from the stretching state, the elastic filaments contract, and as the nonwoven fabric contracts, it returns to its pre-stretch state.

[0013] The elastic filament has a thread-like form having a thickness and a length. The length of the elastic filament is extremely large compared to the thickness, for example, the length of the elastic filament can be 500 times or more, particularly 1000 times or more, compared to the thickness.

[0014] Each elastic filament is preferably present substantially continuously over the entire length of the stretch sheet. The elastic filaments contain an elastic resin. Each elastic filament is arranged to extend in one direction. Each elastic filament may extend linearly or may extend in a meandering manner. Each elastic filament is preferably arranged to extend in one direction without crossing each other. However, crossing of elastic filaments is not prevented. For example, unintentional crossing of elastic filaments due to unavoidable fluctuations in the manufacturing conditions of the stretch sheet is permitted.

[0015] The direction in which the elastic filaments extend may be the same as the machine direction of the nonwoven fabric during manufacture, or may be perpendicular to the machine direction of the nonwoven fabric during manufacture. When a stretch sheet is manufactured according to the preferred manufacturing method described below, the direction in which the elastic filaments extend is the same as the machine direction of the nonwoven fabric during manufacture.

[0016] The basis weight of the elastic filament is set at 4g / m2 from the viewpoints of elasticity, texture, thickness, and cost. 2 More than 30g / m 2 Below, especially 6g / m 2 More than 15g / m 2 It is preferable that the thickness, number of arranged filaments, and arrangement interval of the elastic filaments are appropriately set according to the basis weight of the elastic filaments. For example, the diameter of the elastic filaments can be set to 30 μm or more and 200 μm or less, particularly 50 μm or more and 130 μm or less. When the elastic filaments are arranged in a state where they are pulled in one direction as shown in FIG. 1 described later, the pitch of adjacent elastic filaments (the distance between the centers of adjacent elastic filaments) can be set to 0.1 mm or more and 5 mm or less, particularly 0.3 mm or more and 1.8 mm or less.

[0017] The elastic filament is preferably bonded to the nonwoven fabric in a substantially unstretched state. When the elastic filament is bonded to the nonwoven fabric in an unstretched state, there is an advantage that relaxation (creep) due to stretching does not occur, and the stretchability is unlikely to decrease. Furthermore, for example, when the elastic filament is stretched twice and bonded to the nonwoven fabric, if it shrinks to the initial 1.3 times, it can only be stretched to 1.54 times from this state, but when the elastic filament is bonded to the nonwoven fabric in an unstretched state, there is an advantage that it can be stretched to the stretchable length of the nonwoven fabric or to the maximum stretch of the elastic filament, since the initial origin when the stretch sheet is stretched is different.

[0018] The nonwoven fabric to which the elastic filaments are bonded is stretchable. More specifically, the nonwoven fabric is stretchable in the same direction as the elastic filaments extend. The term "stretchable" includes (i) the case where the constituent fibers of the nonwoven fabric themselves stretch, and (ii) the case where the constituent fibers themselves do not stretch, but the nonwoven fabric as a whole stretches by separating fibers bonded at intersections, structurally changing the three-dimensional structure formed by multiple fibers due to bonding between fibers, or the like, tearing of constituent fibers, or stretching of slack fibers.

[0019] The nonwoven fabric may be already extensible in the state of a raw roll before being joined to the elastic filament. Alternatively, the nonwoven fabric may not be extensible in the state of a raw roll before being joined to the elastic filament, but may be processed to be extensible after being joined to the elastic filament. Specific methods for making the nonwoven fabric extensible include heat treatment, roll-to-roll stretching, biting stretching by grooves or gears, and tensile stretching by a tenter. Considering a suitable manufacturing method for a stretch sheet described later, it is preferable that the nonwoven fabric is not extensible in the state of its raw roll, in order to improve the transportability of the nonwoven fabric when the elastic filament is fused to the nonwoven fabric.

[0020] In addition to being extensible as described above, the nonwoven fabric is preferably substantially inelastic. For this purpose, the nonwoven fabric preferably comprises inelastic fibers and does not comprise elastic fibers. In this specification, inelastic refers to a property that does not meet the definition of elasticity mentioned above.

[0021] Examples of inelastic fibers constituting the nonwoven fabric include fibers made of polyethylene (PE), polypropylene (PP), polyester (PET or PBT), polyamide, etc. The fibers constituting the nonwoven fabric may be short or long fibers, and may be hydrophilic or water-repellent. In addition, core-sheath or side-by-side composite fibers, split fibers, modified cross-section fibers, crimped fibers, heat-shrinkable fibers, etc. may also be used. These fibers may be used alone or in combination of two or more. The nonwoven fabric may be a continuous filament or short fiber nonwoven fabric. The basis weight of the nonwoven fabric is set at 3 g / m2 from the viewpoints of texture, thickness, design, etc. 2 More than 100g / m 2 Below, especially 5g / m 2 More than 30g / m 2 It is preferable that:

[0022] One embodiment of a stretch sheet is shown in Fig. 1. Also, Figs. 2(a) and (b) show cross-sectional views in the thickness direction of the stretch sheet shown in Fig. 1. Figs. 2(a) and (b) are cross-sectional views taken along the direction in which elastic filaments in the stretch sheet extend. The stretch sheet 10 of the embodiment shown in Fig. 1 is composed of two nonwoven fabrics, a first nonwoven fabric 11 and a second nonwoven fabric 12, and a plurality of elastic filaments 13 sandwiched between the two nonwoven fabrics. The elastic filaments 13 are arranged so as to extend in one direction without crossing each other.

[0023] FIG. 2(a) is a cross-sectional view of the stretch sheet 10 in its natural state (relaxed state), and FIG. 2(b) is a cross-sectional view of the stretch sheet 10 in its stretched state. In its natural state, the stretch sheet 10 has a wave-like shape in which peaks 14' protruding above the sheet 10 and valleys 14" protruding below the sheet 10 are arranged alternately. The peaks 14' and valleys 14" are connected via ridges 15'. When the stretch sheet 10 is viewed in a plane, the peaks 14', ridges 15' and valleys 14" extend in a direction perpendicular to the stretch direction of the stretch sheet 10.

[0024] On the other hand, in a stretched state, the stretch sheet 10 has low basis weight regions 14 and high basis weight regions 15 arranged alternately along the extension direction of the elastic filaments 13. Each region 14, 15 extends in a strip shape in the extension direction of the elastic filaments 13, i.e., in a direction perpendicular to the stretch direction of the stretch sheet 10. The low basis weight regions 14 and high basis weight regions 15 are arranged alternately at a constant interval.

[0025] 2(a) and 2(b), the areas which primarily elongate when the stretch sheet 10 is stretched are the peaks 14' and valleys 14" in FIG. 2(a), and the low basis weight regions 14 in FIG. 2(b). In other words, the ridges 15' in FIG. 2(a) (i.e., the high basis weight regions 15 in FIG. 2(b)) do not elongate significantly when the stretch sheet 10 is stretched. Thus, in the stretch sheet 10, high elongation regions and low elongation regions which extend in a direction perpendicular to the stretch direction are alternately arranged along the stretch direction. The high elongation regions are the peaks 14' and valleys 14" in FIG. 2(a), and the low basis weight regions 14 in FIG. 2(b). The low elongation regions are the ridges 15' in FIG. 2(a), and the high basis weight regions 15 in FIG. 2(b). To form the high elongation regions and low elongation regions in the stretch sheet 10, the stretch sheet 10 may be produced, for example, by the method described below.

[0026] In addition to having the above-mentioned structure, one of the features of the stretch sheet of the present invention is that the ratio of the shrinkage stress after a certain time has elapsed to the initial shrinkage stress is large. In the following explanation, for the sake of simplicity, the ratio of the shrinkage stress after 2 hours to the initial shrinkage stress is also referred to as the "stress retention rate". The stretch sheet of the present invention can achieve a high stress retention rate of preferably 50% or more, more preferably 55% or more, and even more preferably 60% or more. The closer the stress retention rate is to 100%, the more preferable, but if the stress retention rate is high, about 50%, the intended purpose of the present invention will be achieved. The method for measuring the stress retention rate will be described in the examples described later.

[0027] As a result of intensive research by the present inventor with the aim of increasing the stress retention rate of the stretch sheet, it was found that it is effective to use a high molecular weight elastic resin as the constituent resin of the elastic filament used in the stretch sheet. A high molecular weight elastic resin has the advantage that stress relaxation is less likely to occur than a low molecular weight elastic resin. Therefore, it is possible to increase the stress retention rate by using a high molecular weight elastic resin. From this viewpoint, it is preferable to use an elastic resin having a weight average molecular weight of 70,000 or more as the elastic resin constituting the elastic filament. It is more preferable that the weight average molecular weight of the elastic resin is 80,000 or more, and even more preferable that it is 100,000 or more. The higher the molecular weight of the elastic resin, the more preferable it is from the viewpoint of suppressing stress relaxation, but if the weight average molecular weight is about 150,000, the intended purpose of the present invention is achieved. From this viewpoint, it is preferable that the weight average molecular weight of the elastic resin is 70,000 to 150,000, more preferably 80,000 to 130,000, and even more preferably 90,000 to 110,000.

[0028] The method for measuring the weight average molecular weight of the elastic resin is as follows. Weight-average molecular weight is measured by gel permeation chromatography (GPC). A TSKgel G-2000H column is used. The column temperature is set to 40°C. Tetrahydrofuran (THF) is used as the mobile phase. The flow rate is set to 1.0mL / min. The sample concentration is set to 10mg / 5mL-THF. The injection volume is set to 500μL. The measured values ​​are values ​​converted into polystyrene values. The analytical sample is prepared by dissolving 10mg of sample in 5mL of THF at room temperature for 10 minutes, and then filtering through a sintered filter with a pore size of 0.45μm.

[0029] Examples of the elastic resin constituting the elastic filament include natural rubber, EVA rubber, synthetic rubber such as styrene-butadiene rubber, butadiene rubber, isoprene rubber, and neoprene rubber, polyurethane, and thermoplastic elastomer. These elastic resins can be used alone or in combination of two or more.

[0030] In particular, it is preferable to use a thermoplastic elastomer as the elastic resin, since it is easy to develop the desired elasticity. Furthermore, the thermoplastic elastomer can be melt-spun using an extruder in the same manner as a normal thermoplastic resin, and the elastic filaments thus obtained can be easily fused, so that it is suitable for the manufacturing method described below.

[0031] Examples of thermoplastic elastomers include styrene-based elastomers such as SBS (styrene-butadiene-styrene), SIS (styrene-isoprene-styrene), SEBS (styrene-ethylene-butadiene-styrene), and SEPS (styrene-ethylene-propylene-styrene), olefin-based elastomers such as ethylene-based α-olefin elastomers and propylene-based elastomers copolymerized with ethylene, butene, octene, etc., polyester-based elastomers, and polyurethane-based elastomers. Core-sheath or side-by-side composite fibers made of these elastomers can also be used.

[0032] In particular, it is preferable to use an A1-B-A2 type triblock copolymer consisting of polymer blocks A1 and A2 mainly composed of a vinyl aromatic polymer and a polymer block B mainly composed of a polyolefin as the thermoplastic elastomer from the viewpoints of suppressing stress relaxation and melt moldability of the elastic filaments.

[0033] The triblock copolymer preferably has a total weight average molecular weight of 70,000 to 150,000, more preferably 80,000 to 130,000, and even more preferably 90,000 to 110,000. When the weight average molecular weight of the triblock copolymer is within this range, the stress relaxation of the elastic filament containing the triblock copolymer is suppressed, and the stretch sheet of the present invention can easily increase its stress retention rate.

[0034] For the same reasons as above, the total weight average molecular weight of the polymer blocks A1 and A2 in the triblock copolymer is preferably from 20,000 to 70,000, more preferably from 25,000 to 60,000, and even more preferably from 27,000 to 50,000.

[0035] The polymer block A1 is mainly composed of a vinyl aromatic polymer. Examples of vinyl aromatics constituting this vinyl aromatic polymer include styrene, p-methylstyrene, m-methylstyrene, p-tert-butylstyrene, α-methylstyrene, chloromethylstyrene, p-tert-butoxystyrene, dimethylaminomethylstyrene, dimethylaminoethylstyrene, vinyltoluene, 1-vinylnaphthalene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, and 4-(phenylbutyl)styrene. The vinyl aromatic polymer may be composed of one of these vinyl aromatics, or two or more of them. Among these vinyl aromatics, styrene is preferred from the viewpoints of ease of polymerization and versatility.

[0036] The content of the vinyl aromatic polymer in the polymer block A1 is preferably from 90% by mass to 100% by mass, and more preferably from 95% by mass to 100% by mass, based on all structural units of the polymer block A1.

[0037] The polymer block A1 may be configured to contain a conjugated diene compound polymer in addition to the vinyl aromatic polymer. Examples of the conjugated diene compound constituting this conjugated diene compound polymer include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, phenylbutadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. The conjugated diene compound polymer may be configured to contain one or more of these conjugated diene compounds.

[0038] The content of the conjugated diene compound polymer in the polymer block A1 is preferably from 0% by mass to 10% by mass, and more preferably from 0% by mass to 5% by mass, based on all structural units of the polymer block A1.

[0039] The weight average molecular weight of the polymer block A1 is preferably from 7,000 to 35,000, and more preferably from 10,000 to 20,000.

[0040] As the polymer block A2, the same one as the polymer block A1 described above can be used. Where no particular description is given of the polymer block A2, the description of the polymer block A1 is appropriately applied. In the A1-B-A2 type triblock copolymer, the polymer block A1 and the polymer block A2 may have the same structure or different structures.

[0041] In particular, it is preferred that both the polymer blocks A1 and A2 are polystyrene, i.e., the elastic filament of the present invention is preferably configured such that the polymer block A1 contains only polystyrene, and the polymer block A2 contains only polystyrene.

[0042] The total content of the polymer blocks A1 and A2 in the A1-B-A2 type triblock copolymer is preferably 15% by mass or more and 40% by mass or less, more preferably 18% by mass or more and 35% by mass or less, based on the total structural units of the A1-B-A2 type triblock copolymer.

[0043] As described above, when the polymer blocks A1 and A2 are both polystyrene, the mass ratio of the polymer block A1 to the polymer block A2 in the A1-B-A2 type triblock copolymer is preferably (A1 / A2)=0.8 or more and 1.2 or less, more preferably (A1 / A2)=0.9 or more and 1.1 or less.

[0044] The polymer block B is mainly composed of polyolefin. Examples of the olefin constituting this polyolefin include isoprene, butadiene, ethylene, propylene, and butylene. The olefin constituting the polymer block B may be composed of one of these olefins, or may be composed of two or more of these olefins. Among these olefins, ethylene and propylene are preferred from the viewpoints of weather resistance and elasticity.

[0045] The content of the polyolefin in the polymer block B is preferably from 90% by mass to 100% by mass, and more preferably from 95% by mass to 100% by mass, based on all structural units of the polymer block B.

[0046] The polymer block B may be composed of, in addition to the polyolefin, another polymer that is derived from another polymerizable monomer and is polymerizable with the polyolefin. An example of this other polymerizable monomer is styrene. The other polymer that is polymerizable with the polyolefin and that constitutes the polymer block B may be composed of one type of these other polymerizable monomers, or may be composed of two or more types.

[0047] The content of the other polymer in the polymer block B is preferably from 0% by mass to 10% by mass, and more preferably from 0% by mass to 5% by mass, based on all structural units of the polymer block B.

[0048] Specific examples of the polymer block B include polyisoprene, polybutadiene, poly(ethylene-propylene), poly(ethylene-butylene), etc. Among these, poly(ethylene-propylene) is preferred from the viewpoints of weather resistance and elasticity.

[0049] The content of the polymer block B in the A1-B-A2 type triblock copolymer is preferably 60% by mass or more and 85% by mass or less, and more preferably 65% ​​by mass or more and 82% by mass or less, based on the total structural units of the A1-B-A2 type triblock copolymer.

[0050] Specific examples of the A1-B-A2 type triblock copolymer include styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butylene-styrene block copolymer (SEBS) which is a hydrogenated product of SBS, styrene-ethylene-propylene-styrene block copolymer (SEPS) which is a hydrogenated product of SIS, and styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), etc. Among these, SEBS, SEPS, and SEEPS are preferred since they can provide elastic filaments with excellent thermal stability and weather resistance.

[0051] The elastic resin constituting the elastic filament may be composed of only the above-mentioned A1-B-A2 type triblock copolymer, or may be composed of one or more other resins in addition to the A1-B-A2 type triblock copolymer as necessary within the scope of the present invention. When the elastic resin contains the A1-B-A2 type triblock copolymer and other resins, the content of the A1-B-A2 type triblock copolymer in the elastic resin is preferably 90% by mass or more and 100% by mass or less, more preferably 95% by mass or more and 100% by mass or less. From the viewpoint of maximally improving the melt moldability and stretchability, it is preferable that the elastic resin is composed of only the A1-B-A2 type triblock copolymer.

[0052] In addition, the elastic resin constituting the elastic filament may be composed of one type of A1-B-A2 type triblock copolymer, or may be composed of two or more types of A1-B-A2 type triblock copolymers having different structures.

[0053] As mentioned above, in the stretch sheet of the present invention, it is preferable that the elastic resin in the elastic filaments constituting the sheet is of high molecular weight. However, if the molecular weight of the elastic resin is excessively high, the melt moldability of the elastic resin tends to decrease. Therefore, the inventor's research has revealed that it is advantageous to blend oil with the elastic filaments in order to obtain good melt moldability even when a high molecular weight elastic resin is used. It is preferable to use an oil that does not easily reduce the cohesive force derived from the hard segment in the elastic resin. In addition, if an oil with a high plasticizing effect is used, it tends to act on the hard segment in the elastic resin and reduce the elasticity of the elastic resin. In other words, it is preferable to use an oil that has a low plasticizing effect on the elastic resin. From the above viewpoint, it is preferable to use an oil with a high kinetic viscosity. From this viewpoint, it is preferable to use an oil with a high kinetic viscosity of 3 mm or less as the kinetic viscosity measured in accordance with JIS K2283. 2 / s or more 600mm 2 / s or less, more preferably 30 mm 2 / s or more 500mm 2 / s or less, more preferably 200 mm 2 / s or more 400mm 2 It is preferable to use an oil having a viscosity of 1 / s or less.

[0054] From the above viewpoints, it is advantageous to use paraffin-based oil as the oil, and it is particularly preferable to use paraffin-based oil whose kinetic viscosity falls within the above-mentioned range. As the paraffin-based oil, various aliphatic hydrocarbons called liquid paraffin, mineral oil, white mineral oil, etc. can be used without any particular limitation.

[0055] The ratio of oil contained in the elastic filament is preferably 25% by mass or more and 60% by mass or less based on the mass of the elastic filament, from the viewpoint of the balance between suppression of stress relaxation of the elastic resin and melt moldability. In order to make this advantage more prominent, the ratio of oil contained in the elastic filament is more preferably 30% by mass or more and 55% by mass or less, and even more preferably 30% by mass or more and 50% by mass or less based on the mass of the elastic filament.

[0056] The elastic filament contains the above-mentioned elastic resin and the above-mentioned oil, so that stress relaxation is unlikely to occur and the melt moldability is good. When the meltability of the elastic filament is expressed by melt flow rate (MFR), the melt flow rate measured in accordance with JIS K7210 at 230°C under a load of 2.16 kg is preferably 3 g / 10 min to 100 g / 10 min, more preferably 5 g / 10 min to 50 g / 10 min, and even more preferably 10 g / 10 min to 30 g / 10 min. The die used in measuring the melt flow rate has a height of 8 mm and an inner diameter of 2.095 mm.

[0057] Next, a preferred method for producing the stretch sheet of the present invention will be described with reference to FIG. 3, taking as an example a method for producing the stretch sheet 10 shown in FIG. 2(a) and FIG. 2(b). In this manufacturing method, as shown in Figure 3, multiple molten elastic filaments 13 spun from a spinning nozzle 16 are taken up and stretched at a predetermined speed, and before the elastic filaments 13 solidify, the elastic filaments 13 are fused to the nonwoven fabrics 11, 12 so that the elastic filaments 13 are arranged in one direction without crossing each other, and then the composite 19 to which the elastic filaments 13 are fused is subjected to an elasticity development treatment along the extension direction of the elastic filaments 13 to impart elasticity to the composite 19.

[0058] The spinning nozzle 16 is provided in the spinning head 17. The spinning head 17 is connected to an extruder. The elastic resin (the elastic resin is mixed with the above-mentioned oil as necessary) melted and kneaded by the extruder is supplied to the spinning head 17. A large number of spinning nozzles 16 are arranged in a straight line in the spinning head 17. The spinning nozzles 16 are arranged along the width direction of the first and second nonwoven fabrics 11 and 12. The interval between adjacent spinning nozzles 16 corresponds to the interval between the elastic filaments 13 in the target stretch sheet 10. The spinning nozzle 16 is usually circular, and its diameter affects the diameter and stretch ratio of the elastic filaments 13. From this viewpoint, the diameter of the spinning nozzle 16 is preferably 0.1 mm or more and 2 mm or less, particularly 0.2 mm or more and 0.6 mm or less. In order to increase the bonding strength with the nonwoven fabrics 11 and 12, to increase the spinnability of the elastic filaments 13, and to improve the stretch properties of the stretch sheet 10, the elastic filaments 13 may be in a composite form (side-by-side, core-sheath, or sea-island structure).

[0059] The spun elastic filaments 13 in a molten state join the first nonwoven fabric 11 and the second nonwoven fabric 12 that are respectively unwound from the original rolls at the same speed, and are sandwiched between the two nonwoven fabrics 11, 12 and taken up at a predetermined speed. The take-up speed of the elastic filaments 13 is the same as the unwound speed of the two nonwoven fabrics 11, 12.

[0060] The elastic filament 13 joins the first and second nonwoven fabrics 11, 12 before solidification, i.e., in a fusible state. As a result, the elastic filament 13 fuses to the first and second nonwoven fabrics 11, 12 while being sandwiched between them. That is, the elastic filament 13 is taken up and stretched while the unsolidified elastic filament is fused to the nonwoven fabrics 11, 12 being conveyed. When the elastic filament 13 fuses, no heat is applied from the outside to the first and second nonwoven fabrics 11, 12. That is, the elastic filament 13 fuses to both nonwoven fabrics 11, 12 only by the melting heat caused by the fusible elastic filament 13. As a result, among the constituent fibers of both nonwoven fabrics 11, 12, only the fibers present around the elastic filament 13 fuse to the elastic filament, and the fibers present at a position farther away do not fuse. As a result, the heat applied to both nonwoven fabrics 11, 12 is kept to a minimum, so that the inherent good texture of the nonwoven fabrics themselves is maintained, and the resulting stretch sheet 10 has a good texture.

[0061] When the elastic filament 13 is joined to the nonwoven fabrics 11 and 12, the elastic filament 13 is in a substantially unstretched state (a state in which it does not shrink when an external force is removed). In the joined state, the fibers constituting the nonwoven fabrics 11 and 12 are at least partially fused to the elastic filament 13. In this state, it is preferable that the nonwoven fabrics 11 and 12 are fused to each other while sandwiching the elastic filament 13.

[0062] In this way, a composite 19 is obtained in which the elastic filament 13 is sandwiched between the two nonwoven fabrics 11, 12. When nonwoven fabrics that are inherently extensible are used as the nonwoven fabrics 11, 12, the composite 19 becomes the stretch sheet 10 itself. On the other hand, when nonwoven fabrics that are inherently non-extensible are used as the nonwoven fabrics 11, 12, the composite 19 including the nonwoven fabrics 11, 12 is subjected to an elasticity development process along the extension direction of the elastic filament 13 to impart elasticity to the composite 19. In this manufacturing method, this process is performed by using an elasticity development processing device 22 equipped with a pair of grooved rolls 20, 21, each of which has teeth and tooth bottoms formed alternately in the circumferential direction, and subjecting the composite 19 to an elasticity development process along its conveying direction, i.e., along the extension direction of the elastic filament 13.

[0063] The elasticity development processing device 22 has a known lifting mechanism (not shown) that vertically displaces the pivotal support parts of one or both of the toothed groove rolls 20, 21, making it possible to adjust the distance between the toothed groove rolls 20, 21. In this manufacturing method, the toothed groove rolls 20, 21 are combined such that the teeth of one toothed groove roll 20 are loosely inserted between the teeth of the other toothed groove roll 21, and the teeth of the other toothed groove roll 21 are loosely inserted between the teeth of one toothed groove roll 20, and the composite 19 is inserted between the toothed groove rolls 20, 21 in this state and subjected to elasticity development processing.

[0064] The composite 19 is subjected to elasticity development processing by a pair of grooved rolls 20, 21 to obtain the desired stretch sheet 10. After passing through the grooved rolls 20, 21, the stretch sheet 10 is quickly released from the stretched state in the conveying direction by its own shrinkage restoring force. As a result, the length of the stretch sheet 10 is almost restored in the conveying direction. As a result, in the stretched state, high elongation regions and low elongation regions are arranged alternately in the extension direction of the elastic filaments 13.

[0065] The stretch sheet of the present invention thus obtained can be suitably used, for example, as the outer casing of a disposable diaper. Disposable diapers equipped with the stretch sheet of the present invention, such as pants-type disposable diapers, are easy to put on because the waist part can be easily expanded, and they are less likely to slip down even when worn for long periods of time. In addition to the above uses, the stretch sheet of the present invention can also be used for various uses such as medical disposable clothing, cleaning sheets, eye patches, masks, bandages, etc., taking advantage of its advantages such as good texture, stretchability, and breathability. It is particularly preferably used as a constituent material of absorbent articles such as sanitary napkins and disposable diapers. Examples of such constituent materials include liquid-permeable sheets (including top sheets, sublayer sheets, etc.) located closer to the skin than the absorbent body, sheets constituting the outer surface of disposable diapers, and sheets for imparting elastic stretchability to the waist, waist, and leg areas. It can also be used as a sheet for forming the wings of a napkin. It can also be used in other areas where stretchability is desired. The basis weight and thickness of the stretch sheet can be appropriately adjusted depending on the specific use. For example, when used as a constituent material of absorbent articles, a basis weight of 20 g / m 2 More than 60g / m 2 It is desirable to keep the thickness at about 0.5 mm or more and 1.5 mm or less.

[0066] The stretchability of the stretch sheet can be appropriately set depending on the specific application of the stretch sheet. When the stretch sheet is used as an exterior body of a disposable diaper, for example, the initial stress A measured in the measurement of the stress retention rate explained in the examples below is preferably 10 cN / 50 mm or more and 500 cN / 50 mm or less, more preferably 20 cN / 50 mm or more and 250 cN / 50 mm or less, and even more preferably 30 cN / 50 mm or more and 100 cN / 50 mm or less. EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0068] Example 1 (1) Preparation of Elastic Filament An elastic filament containing a thermoplastic elastomer and oil shown in Table 1 was prepared. The ratio of oil contained in the elastic filament is as shown in the same table. The MFR of the elastic filament is also as shown in the same table.

[0069] (2) Preparation of nonwoven fabric Basis weight 18g / m 2 Two pieces of spunbond nonwoven fabric were prepared. The fibers were made of polypropylene.

[0070] (3) Manufacturing of stretch sheets Using the apparatus shown in FIG. 3, stretch sheets having the structures shown in FIG. 1, FIG. 2(a) and FIG. 2(b) were produced. The elasticity development treatment was carried out using an elasticity development treatment device 22 equipped with a pair of grooved rolls 20, 21 in which teeth and tooth bottoms are alternately formed in the axial direction. This resulted in a basis weight of 46 g / m2 that expands and contracts in the direction in which the elastic filaments 13 extend. 2 The stretch sheet 10 was obtained.

[0071] [Examples 2 to 4] The oils used for blending with the elastic filaments were those shown in Table 1 below. The ratio of oil contained in the elastic filaments was also shown in Table 1. A stretch sheet was obtained in the same manner as in Example 1, except for the above.

[0072] Comparative Examples 1 to 3 The thermoplastic elastomers used to compose the elastic filaments were those shown in Table 1 below. In addition, no oil was blended into the elastic filaments. Other than these, a stretch sheet was obtained in the same manner as in Example 1. In Comparative Example 3, the elastic resin had poor melt fluidity, and the elastic filaments could not be melt-spun.

[0073] 〔evaluation〕 For the stretch sheets obtained in the examples and comparative examples, the stress retention rate was measured by the following method, and the results are shown in Table 1 below.

[0074] [Measurement of stress retention rate] A test piece was obtained by cutting the stretch sheet so that the length in the stretch direction was 150 mm and the length in the direction perpendicular to the stretch direction was 50 mm. This test piece was attached to a tensile tester with a chuck distance of 100 mm so that the stretching direction was the tensile direction. At an ambient temperature of 40°C, the test piece was pulled at a speed of 300 mm / min. When the chuck distance reached 200 mm, the pulling was stopped and this state was maintained for 2 hours, during which the stress was measured over time. When the initial stress when the chuck distance becomes 200 mm is defined as A and the stress after 2 hours is defined as B, the stress retention rate (%) is defined as B / A x 100.

[0075] [Table 1]

[0076] As is clear from the results shown in Table 1, the stretch sheets obtained in the examples exhibited higher stress retention rates than the stretch sheets obtained in the comparative examples. [Explanation of symbols]

[0077] 10 Stretch Sheet 11 First nonwoven fabric 12 Second nonwoven fabric 13 Elastic filament 14 High basis weight area 14' top 14" valley 15 Low basis weight area 15' Ridge

Claims

1. A stretch sheet in which a plurality of elastic filaments arranged to extend in one direction are bonded to an extensible nonwoven fabric, The high elongation regions and the low elongation regions extending in a direction perpendicular to the stretch direction of the stretch sheet are alternately arranged along the stretch direction, the elastic filaments are fused to the nonwoven fabric in a substantially unstretched state; A stretchable sheet having a stress retention rate of 50% or more.

2. A stretch sheet in which a plurality of elastic filaments arranged to extend in one direction are bonded to an extensible nonwoven fabric, The stretch sheet has high elongation regions and low elongation regions arranged alternately in a direction perpendicular to the stretch direction, and the high elongation regions and low elongation regions are arranged alternately in the stretch direction, the elastic filaments are fused to the nonwoven fabric in a substantially unstretched state; The elastic filaments comprise a thermoplastic elastomer and an oil.

3. The stretch sheet according to claim 2 , wherein the ratio of the oil is 25% by mass or more and 60% by mass or less based on the mass of the elastic filaments.

4. The stretch sheet according to claim 2 or 3, wherein the oil is a paraffin-based oil.

5. 5. The stretch sheet according to claim 2, wherein the thermoplastic elastomer is an A1-B-A2 type triblock copolymer consisting of polymer blocks A1 and A2 mainly composed of a vinyl aromatic polymer and a polymer block B mainly composed of a polyolefin, the weight average molecular weight of the whole being from 70,000 to 150,000, and the sum of the weight average molecular weights of the polymer blocks A1 and A2 being from 27,000 to 70,000.

6. 6. The stretch sheet according to claim 1, wherein the elastic filaments have a melt flow rate, measured in accordance with JIS K7210 at 230°C under a load of 2.16 kg, of 3 g / 10 min to 100 g / 10 min.

Citation Information

Patent Citations

  • Flexible sheet

    JP2008179128A