Method for manufacturing a positive electrode active material for a lithium secondary battery and positive electrode active material for a lithium secondary battery manufactured by said method

A mechanofusion process with a hollow carbon-based material forms a uniform carbon coating on lithium transition metal oxides, addressing thermal stability and conductivity issues, enhancing battery performance.

JP7551065B2Active Publication Date: 2024-09-17LG ENERGY SOLUTION LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022541274
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-29
Publication Date
2024-09-17
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Lithium nickel cobalt metal oxides face issues with thermal stability and electrical conductivity, and carbon coating methods at high temperatures alter the oxidation state of the positive electrode material, reducing its performance.

Method used

A method involving a mechanofusion process with a hollow carbon-based material having specific properties forms a thin and uniform carbon coating on the surface of lithium transition metal oxides, maintaining the oxidation state and improving conductivity.

Benefits of technology

The method enhances the electrical conductivity and life characteristics of the positive electrode active material, preventing gelation during slurry mixing and improving input/output characteristics of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551065000007
    Figure 0007551065000007
  • Figure 0007551065000009
    Figure 0007551065000009
  • Figure 0007551065000005
    Figure 0007551065000005
Patent Text Reader

Abstract

The present invention includes the steps of mixing a lithium transition metal oxide and a hollow carbonaceous material to form a mixture, and mechanically treating the mixture to form a carbon coating layer on the surface of the lithium transition metal oxide, wherein the hollow carbonaceous material has a linear chain shape and a specific surface area of ​​500 m 2 / g or more, and the degree of graphitization (I D / I G The present invention relates to a method for producing a positive electrode active material having a DBP oil absorption of 300 mL / 100 g or more, a positive electrode active material produced by the method, and a positive electrode and a lithium secondary battery each including the positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0011338 filed on January 30, 2020, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a method for producing a positive electrode active material for a lithium secondary battery, a positive electrode active material produced by the method, and a positive electrode for a lithium secondary battery and a lithium secondary battery each containing the positive electrode active material. [Background technology]

[0003] With the technological development and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.

[0004] Lithium transition metal composite oxides are used as the positive electrode active material for lithium secondary batteries, and among them, lithium cobalt oxide LiCoO2, which has high working voltage and excellent capacity characteristics, is mainly used. However, LiCoO2 has very poor thermal properties due to the instability of its crystal structure caused by delithiation, and is expensive, so there are limitations to its mass use as a power source in fields such as electric vehicles.

[0005] As a material to be used in place of LiCoO2, lithium manganese composite metal oxides (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), lithium nickel composite metal oxides (LiNiO2, etc.), etc. have been developed. Among them, research and development of lithium nickel composite metal oxides, which have a high reversible capacity of about 200 mAh / g and therefore can easily realize large-capacity batteries, has been actively carried out. However, LiNiO2 has inferior thermal stability compared to LiCoO2, and if an internal short circuit occurs due to external pressure in a charged state, the positive electrode active material itself decomposes, causing the battery to explode and catch fire. Therefore, as a method for maintaining the excellent reversible capacity of LiNiO2 and improving its low thermal stability, LiNiO2, which has a part of the nickel substituted with cobalt, has been developed. 1-α Co α Lithium nickel cobalt metal oxides have been developed in which O2 (α = 0.1 to 0.3) or part of the nickel is replaced with Mn, Co, or Al.

[0006] However, in the case of the lithium nickel cobalt metal oxide, due to the recent sharp increase in the cost of cobalt, active research is being conducted on Co-less positive electrode materials that do not contain cobalt or Ni-rich positive electrode materials that contain an excessive amount of Ni, in terms of cost and energy density.

[0007] Meanwhile, the Co-less or Ni-rich cathode materials have problems such as low electrical conductivity and vulnerability to moisture compared to conventional Co-rich compositions that use excessive amounts of cobalt. In order to solve these problems, attempts have been made to form a carbon coating layer using pitch or the like on the surface of the cathode materials. However, the carbon coating layer requires high-temperature heat treatment for carbonization, and during the high-temperature heat treatment, the carbon element on the surface reacts with the oxygen on the surface of the cathode material and is reduced, which significantly changes the oxidation number of the cathode active material, resulting in a decrease in the performance of the cathode material.

[0008] Therefore, there is a need to develop a positive electrode active material that can improve electrical conductivity and life characteristics by forming a thin and uniform carbon coating layer on the surface of the positive electrode active material without changing the oxidation number of the surface of the positive electrode material through a high-temperature heat treatment process. Summary of the Invention [Problem to be solved by the invention]

[0009] In order to solve the above problems, a first technical object of the present invention is to provide a method for manufacturing a positive electrode active material, which can form a uniform carbon coating layer on a lithium transition metal oxide by mechanically treating the surface of the hollow carbon-based material.

[0010] A second technical objective of the present invention is to provide a positive electrode active material which is prepared by the above-mentioned preparation method and which can improve electrical conductivity by forming a thin and uniform carbon coating layer on the surface of a lithium transition metal oxide.

[0011] A third technical object of the present invention is to provide a positive electrode for a lithium secondary battery, which contains the positive electrode active material.

[0012] A fourth technical object of the present invention is to provide a lithium secondary battery including the positive electrode. [Means for solving the problem]

[0013] The present invention includes the steps of mixing a lithium transition metal oxide and a hollow carbon-based material to form a mixture, and mechanically surface-treating the mixture to form a carbon coating layer on the surface of the lithium transition metal oxide, the hollow carbon-based material having a straight chain shape and a specific surface area of ​​500 m 2 / g or more, and the degree of graphitization (I D / I G ) is 1.0 or more and the DBP oil absorption is 300 mL / 100 g or more.

[0014] The present invention also provides a lithium transition metal oxide and a carbon coating layer formed on the surface of the lithium transition metal oxide, the carbon coating layer being formed on the surface of the lithium transition metal oxide, the carbon coating layer having a thickness of 500 nm or less and a BET specific surface area of ​​0.5 m 2 / g~50m 2 / g.

[0015] The present invention also provides a positive electrode for a lithium secondary battery, comprising the positive electrode active material.

[0016] The present invention also provides a lithium secondary battery including the positive electrode for a lithium secondary battery. Effect of the Invention

[0017] According to the present invention, when a carbon coating layer is formed on the surface of a lithium transition metal oxide, a carbon-based material having a hollow structure is used to form the carbon coating layer by a physical method, so that a thin and uniform carbon coating layer can be formed without changing the oxidation number of the surface of the positive electrode material. As a result, the electrical conductivity of the positive electrode active material is improved, and gelation of the slurry can be prevented when mixing the positive electrode. When this is applied to a battery, the input / output characteristics and life characteristics can be improved. [Brief description of the drawings]

[0018] [Figure 1] 1 is a SEM image showing a carbon-based material having a hollow structure used in an embodiment of the present invention. [Diagram 2] 1 is a SEM image showing a carbon-based material having a dense structure used in a comparative example of the present invention. [Diagram 3] 1 is an SEM image showing the surface of (a) the positive electrode active material of Comparative Example 2, (b) the positive electrode active material of Comparative Example 1, and (c) the positive electrode active material of Example 1. [Figure 4]1 is an SEM image showing the surface of (a) the positive electrode active material of Comparative Example 2, (b) the positive electrode active material of Comparative Example 4, and (c) the positive electrode active material of Example 1. [Diagram 5] 1 is a SEM image showing the surface of the positive electrode active material produced in Example 1. [Figure 6] 1 is a SEM image showing the surface of the positive electrode active material prepared in Comparative Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will now be described in more detail.

[0020] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0021] Throughout this specification, the term "primary particle" refers to a primary structure of a single particle, and the term "secondary particle" refers to an aggregate of primary particles that are aggregated together by physical or chemical bonds between the primary particles without any intentional aggregation or granulation process of the primary particles that constitute the secondary particle, i.e., a secondary structure.

[0022] Throughout this specification, the "specific surface area" is measured by the BET method, and specifically, it can be calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mini II manufactured by BEL Japan.

[0023] Throughout this specification, "DBP oil absorption (dibutylphthalate adsorption)" is a measurement of the voids of secondary particles formed by agglomeration of primary particles of a carbon-based material, and indicates how well connected the primary particles in the carbon-based material are. The DBP oil absorption can be measured by mixing DBP, a plasticizer, with a predetermined amount of carbon black and measuring the change in torque caused by the impregnation of the plasticizer. Generally, the higher the DBP oil absorption, the better the conductivity.

[0024] Throughout this specification, the term "degree of graphitization" refers to the degree to which amorphous carbon is partially or entirely converted into crystalline graphite, and can be determined using Raman spectroscopy, which can be used to analyze the structure of carbon-based materials. The G band in the Raman spectrum of a carbon-based material is the sp 2 The D band is a peak that indicates the sp bond of carbon-based materials and indicates carbon crystals without structural defects. 3 This peak indicates sp 2 The bond is broken and the atom is sp 3 The D band increases when a disorder or defect is generated in the carbon-based material, so the maximum peak intensity of the G band (I G ) versus the maximum peak intensity of the D band (I D ) ratio (I D / I G ) can be calculated to quantitatively evaluate the degree of disorder or defect generation.

[0025] Method for producing positive electrode active material The present inventors discovered that when forming a carbon-based coating layer on a lithium transition metal oxide, a carbon-based material having a specific structure is used and the carbon-based coating layer is formed by a mechanofusion method, thereby making it possible to form a uniform and thin coating layer on the surface of the lithium transition metal oxide without changing its structure, and thus completed the present invention.

[0026] Specifically, the method for preparing a positive electrode active material according to the present invention includes the steps of: mixing a lithium transition metal oxide and a hollow carbonaceous material to form a mixture; and mechanically processing the mixture to form a carbon coating layer on a surface of the lithium transition metal oxide, the hollow carbonaceous material having a linear chain shape and a specific surface area of ​​500 m. 2 / g or more, and the degree of graphitization (I D / I G ) is 1.0 or more, and the DBP oil absorption is 300 mL / 100 g or more.

[0027] The method for producing a positive electrode active material according to the present invention will now be described in more detail.

[0028] First, in order to manufacture the positive electrode active material according to the present invention, a lithium transition metal oxide is prepared.

[0029] For example, the lithium transition metal oxide may have crystal grains of 50 nm to 4,000 nm, preferably 50 nm to 2,000 nm. For example, the lithium transition metal oxide may be in the form of secondary particles formed by agglomeration of primary particles, or in the form of single particles formed by a single primary particle. For example, when the lithium transition metal oxide is formed of secondary particles formed by agglomeration of primary particles, the energy density per volume of the electrode may be increased, and the contact area between the lithium transition metal oxide and the electrolyte may be large, and the movement distance of lithium ions in the lithium transition metal oxide may be short, so that high capacity and high output characteristics may be easily exhibited. For example, when the lithium transition metal oxide is formed in the form of a single particle, the structural stability of the battery may be improved as the rolling density is improved.

[0030] The lithium transition metal oxide is generally used as a positive electrode active material, and may be used without limitation as long as it is capable of easily inserting or extracting lithium ions during charging and discharging. For example, lithium transition metal oxides include layered compounds such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) and compounds substituted with one or more transition metals; 1+y1 Mn 2-y1 O4 (0≦y1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiFe3O4, V2O5, and Cu2V2O7; chemical formula LiNi 1-y2 Ni-site type lithium nickel oxide represented by My2O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and 0.01≦y2≦0.3); 2-y3 Examples of the lithium manganese composite oxide include, but are not limited to, My3O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and 0.01≦y3≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion.

[0031] Next, the lithium transition metal oxide and a hollow carbonaceous material are mixed to form a mixture.

[0032] The carbon-based material may have a chain shape and be in the form of secondary particles formed by agglomeration of primary particles, and the carbon-based material may have pores therein due to the secondary particle form formed by agglomeration of primary particles.

[0033] The primary particle size of the carbon-based material may be 50 nm or less, preferably 5 nm to 50 nm. When the primary particle size of the carbon-based material satisfies the above range, it may be advantageous to form a uniform coating layer. Furthermore, since the carbon-based material exhibits a linear chain shape, even if the primary particle size of the carbon-based material is small within the above range, a carbon coating layer can be formed uniformly on the surface of the lithium transition metal oxide.

[0034] For example, if the primary particle size of the carbon-based material exceeds 50 nm, carbon may partially aggregate, making it difficult to form a uniform coating layer overall.

[0035] According to the present invention, the hollow carbonaceous material has a specific surface area of ​​500 m 2 / g or more, preferably 500m 2 / g~2,500m 2 / g, where the degree of graphitization (I D / I G ) is 1.0 or more, preferably 1.0 to 2.0, and the DBP oil absorption is 300 mL / 100 g or more, preferably 300 mL / 100 g to 2,000 mL / 100 g, and most preferably 300 mL / 100 g to 1,000 mL / 100 g.

[0036] When the BET specific surface area and the graphitization degree of the hollow carbon-based material are within the above ranges, it means that the crystallinity of the hollow carbon-based material is low. For example, when the BET specific surface area is less than the above ranges or the graphitization degree is less than the above ranges, the carbon-based material may have a dense structure.

[0037] Specifically, the hollow carbonaceous material according to the present invention has a straight chain shape and exhibits low crystallinity, as shown in FIG. 1. In this case, the structure collapses due to an external force. When a carbon coating layer is formed using the hollow carbonaceous material, the carbonaceous material is crushed and adheres to the surface of the lithium transition metal oxide due to the collapse of the structure of the carbonaceous material due to an external force, and a carbon coating layer with a uniform thickness can be formed on the surface of the secondary particles. In particular, when the lithium transition metal oxide has a form of secondary particles in which primary particles are aggregated, the carbon coating layer can be formed uniformly on the boundaries between the primary particles of the lithium transition metal oxide. This can improve the conductivity of the positive electrode active material, maintain a low BET specific surface area of ​​the final positive electrode active material, and prevent side reactions with the electrolyte due to an increase in the BET specific surface area.

[0038] For example, in the case of the carbon-based material having a graphitization degree of less than 1.0, as shown in FIG. 2, the carbon-based material has high crystallinity and thus does not collapse in structure, so that even when an external force is applied, the carbon-based material is coated on the surface of the lithium transition metal oxide while maintaining the crystallinity of the carbon-based material without collapsing the structure, and the BET specific surface area can be increased. In addition, it is not easy to form a uniform carbon coating layer on the surface of the positive electrode active material by forming a carbon-based coating layer in a form in which the carbon-based material is attached to the surface of the lithium transition metal oxide without collapsing the structure. In particular, when the lithium transition metal oxide has a form of secondary particles in which primary particles are aggregated, it is difficult to form a carbon coating layer at the boundaries between the primary particles of the lithium transition metal oxide, and it is even more difficult to form a uniform carbon coating layer.

[0039] Moreover, the carbon-based substance according to the present invention has a DBP oil absorption of 300 mL / 100 g or more, preferably 300 mL / 100 g to 2,000 mL / 100 g.

[0040] In the present invention, the DBP oil absorption is a measurement of the voids in the carbon-based material in the form of secondary particles formed by agglomeration of the primary particles, and indicates how well the primary particles in the carbon-based material are connected. In general, the higher the DBP oil absorption, the better the primary particles in the carbon-based material are connected, which can indicate improved conductivity.

[0041] For example, when the DBP oil absorption is below the range of the present invention, the primary particles in the carbon-based material are not well connected, so that it is difficult to show improved conductivity even if a carbon coating layer is formed using the carbon-based material.

[0042] The lithium transition metal oxide and the carbon-based material may be mixed in an amount of 0.1 to 1.5 parts by weight, preferably 0.1 to 1 part by weight, based on 100 parts by weight of the lithium transition metal oxide. When mixed in the above range, a uniform carbon coating layer can be formed on the entire surface of the lithium transition metal oxide. On the other hand, when the amount of the carbon-based material mixed exceeds the above range, an excessively thick carbon coating layer is formed, which may act as a resistance to prevent the diffusion of lithium ions, and when applied to a battery, the input / output characteristics of the battery may be deteriorated.

[0043] The mixture is then surface-treated by a mechanical method to form a carbon coating layer on the surface of the lithium transition metal oxide.

[0044] The mechanical treatment of the mixture according to the present invention can be carried out by a mechanofusion method. Specifically, the mechanofusion method can be carried out using a Nobilta device under dry process conditions that do not further contain additives such as solvents or binders, and specifically, the method can be carried out at room temperature (20°C) while stirring the reactor at a current of 3 to 15 A, a power of 0.2 to 5.5 W, and a rotation speed of 500 to 6,000 rpm based on a 0.5 L Nobilta device. The mechanofusion method can vary in terms of current, power, and rotation speed depending on the capacity of the device, and for example, the power can be increased and the rotation speed can be decreased when the capacity of the device is large. Specifically, for example, when a 300 L Nobilta device is used, the method can be carried out while stirring at a power of 10 to 200 W and a rotation speed of 50 to 800 rpm. The mechanofusion method improves particle dispersibility, and the carbon material is spaced at uniform intervals on the surface of the lithium transition metal oxide, so that a uniform carbon coating layer can be formed on the surface of the lithium transition metal oxide. Also, even when the lithium transition metal oxide has a form of secondary particles formed by agglomeration of primary particles, the mechanofusion method can form a carbon coating layer not only on the surfaces of the secondary particles of the lithium transition metal oxide but also on the boundaries between the primary particles.

[0045] positive electrode active material The present invention also provides a positive electrode active material produced by the above-mentioned method. Specifically, the positive electrode active material includes a lithium transition metal oxide and a carbon coating layer formed on the surface of the lithium transition metal oxide, the carbon coating layer being formed on the surface of the lithium transition metal oxide, the carbon coating layer having a thickness of 500 nm or less and a BET specific surface area of ​​0.5 m 2 / g~50m 2 / g.

[0046] As described above, the lithium transition metal oxide according to the present invention may have crystal grains with a size of 50 nm to 4,000 nm, preferably 50 nm to 2,000 nm, and the lithium transition metal oxide may be in the form of secondary particles formed by aggregation of primary particles, or the lithium transition metal oxide may be in the form of a single particle.

[0047] When the lithium transition metal oxide has a single particle form, the carbon coating layer may be coated on the surface of the single particle form of the lithium transition metal oxide with a uniform thickness and shape, and when the lithium transition metal oxide has a secondary particle form in which primary particles are aggregated, the carbon coating layer may be uniformly formed on the surfaces of the primary particles and the secondary particles of the lithium transition metal oxide.

[0048] Preferably, the positive electrode active material according to the present invention has a BET specific surface area of ​​0.5 m 2 / g~50m 2 / g, preferably 2m 2 / g~20m 2 / g, more preferably 3m 2 / g~10m 2 When the BET specific surface area is within the above range, the change in the specific surface area due to the formation of the carbon coating layer is minimized, and a side reaction between the positive electrode active material and the electrolyte can be suppressed.

[0049] In addition, the positive electrode active material according to the present invention has a powder electrical conductivity of 3.7×10 measured after rolling with a force of 0.1 kN to 20 kN, preferably 0.5 to 10 kN, and most preferably 2 kN. -3 S / cm~10.0×10 -3 S / cm, preferably 4.5×10 -3 S / cm~10.0×10 -3 As mentioned above, the electrical conductivity of the positive electrode active material itself is greatly increased by forming a carbon coating layer on the surface, so when this is applied to a battery, the electrochemical properties such as the input and output characteristics and life characteristics of the battery can be improved.

[0050] positive electrode The present invention also provides a positive electrode for a lithium secondary battery, which contains the positive electrode active material produced by the above-mentioned method.

[0051] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector and including the above-mentioned positive electrode active material.

[0052] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0053] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.

[0054] In this case, the positive electrode active material may be included in an amount of 80 to 99 wt %, more specifically, 85 to 98 wt %, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics can be exhibited.

[0055] In this case, the conductive material is used to give conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can be contained in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer.

[0056] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer.

[0057] The positive electrode may be manufactured according to a typical method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by applying a positive electrode mixture prepared by dissolving or dispersing the positive electrode active material and, optionally, a binder and a conductive material in a solvent onto a positive electrode current collector, followed by drying and rolling. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.

[0058] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and may be used alone or in combination of two or more of these. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity during subsequent coating for the manufacture of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0059] Alternatively, the positive electrode can be produced by casting the positive electrode mixture on a separate support, peeling it off from the support, and laminating the resulting film on a positive electrode current collector.

[0060] Lithium secondary battery In addition, the present invention can provide an electrochemical device including the positive electrode. The electrochemical device can be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0061] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0062] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0063] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0064] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0065] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0066] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. Also, a thin film of metallic lithium may be used as the negative electrode active material. Also, the carbon material may be either low crystalline carbon or high crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0067] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.

[0068] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and is usually added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0069] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0070] For example, the negative electrode active material layer can be produced by applying a negative electrode mixture, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, onto a negative electrode current collector and drying the applied material; alternatively, the negative electrode mixture can be cast onto another support, and then peeled off from the support to obtain a film, which can be laminated onto the negative electrode current collector.

[0071] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.

[0072] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0073] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0074] The organic solvent can be used without any particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; an ether solvent such as dibutyl ether or tetrahydrofuran, etc.; a ketone solvent such as cyclohexanone, etc.; an aromatic hydrocarbon solvent such as benzene or fluorobenzene, etc.; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), propylene carbonate (propylene carbonate), etc. Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.

[0075] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance, and lithium ions can be effectively transferred.

[0076] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in the capacity of the battery, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total weight of the electrolyte.

[0077] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0078] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0079] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0080] The external shape of the lithium secondary battery of the present invention is not particularly limited, but may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0081] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0082] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention can be modified into various other forms, and the scope of the present invention should not be interpreted as being limited to the examples described below. The examples of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0083] Working Example Example 1 LiNi 0.6 Co 0.2 Mn 0.2A lithium transition metal oxide represented by O2 and hollow structure carbon black having the specifications in Table 1 below were placed in a paint shaker (1400 Al classic shaker, manufactured by Red Devil) so that the carbon black was 1% by weight per 500 g of lithium transition metal oxide, and mixed for 60 minutes so that the transition metal oxide and hollow structure carbon black were uniformly dispersed.

[0084] The mixture was placed in a mechanofusion device (nobilta, manufactured by Hosokawa Micron Co., Ltd.) and processed at 3,000 rpm for 10 minutes to produce a positive electrode active material in which a carbon coating layer having a thickness of 200 nm was formed on the lithium transition metal oxide.

[0085] Example 2 A positive electrode active material having a carbon coating layer of 250 nm thickness formed on the lithium transition metal oxide was prepared in the same manner as in Example 1, except that carbon black was mixed to a concentration of 1 wt % per 200 g of lithium transition metal oxide.

[0086] Example 3 A positive electrode active material having a carbon coating layer of 250 nm thickness formed on the lithium transition metal oxide was prepared in the same manner as in Example 1, except that carbon black was mixed in an amount of 1 wt % per 100 g of lithium transition metal oxide.

[0087] Example 4 A positive electrode active material having a carbon coating layer of 250 nm thickness formed on the lithium transition metal oxide was prepared in the same manner as in Example 1, except that 50 g of the lithium transition metal oxide was mixed with 1 wt % of carbon black.

[0088] Comparative Example 1 LiNi 0.6 Co 0.2 Mn 0.2A lithium transition metal oxide represented by O2 and hollow structure carbon black having the specifications in Table 1 below were added to a paint shaker (1400 Al classic shaker, manufactured by Red Devil) so that the carbon black was 1% by weight per 500 g of lithium transition metal oxide, and mixed for 60 minutes so that the transition metal oxide and the hollow structure carbon black were uniformly dispersed, thereby producing a mixture in which the lithium transition metal oxide and carbon black were uniformly mixed, and this was used as a positive electrode active material.

[0089] Comparative Example 2 The lithium transition metal oxide without a carbon coating layer was used as the positive electrode active material.

[0090] Comparative Example 3 A mixture in which the aggregated carbon black was adsorbed on the surface of a lithium transition metal oxide was prepared in the same manner as in Example 2, except that carbon black having the specifications in Table 1 below was used, and the mixture was used as a positive electrode active material.

[0091] Comparative Example 4 A mixture in which the aggregated carbon black was adsorbed on the surface of a lithium transition metal oxide was prepared in the same manner as in Example 1, except that carbon black having the specifications in Table 1 below was used, and the mixture was used as a positive electrode active material.

[0092] Comparative Example 5 A mixture in which lithium transition metal oxide and carbon black were uniformly mixed on a lithium transition metal oxide was prepared in the same manner as in Comparative Example 1, except that carbon black having the specifications in Table 1 below was used, and the mixture was used as a positive electrode active material.

[0093] Comparative Example 6 A positive electrode active material having a carbon coating layer of 350 nm thickness formed on a lithium transition metal oxide was prepared in the same manner as in Example 1, except that carbon black having the specifications in Table 1 below was used.

[0094] [Table 1]

[0095] Experimental Example 1 (1) Confirmation of the surface characteristics of the positive electrode active material The surface characteristics of the positive electrode active materials of Example 1 and Comparative Examples 1, 2, 4, and 6 were confirmed and are shown in FIGS.

[0096] First, Figure 3 is an SEM image showing the surface of (a) the positive electrode active material of Comparative Example 2, (b) the positive electrode active material of Comparative Example 1, and (c) the positive electrode active material of Example 1. Comparative Example 2 (Figure 3(a)) is a positive electrode active material without a coating layer formed on the surface, and in comparison, in the case of the positive electrode active material of Example 1, it was confirmed that the surface of the lithium transition metal oxide was uniformly coated with a carbon-based coating layer (the surface of the particles is covered with a gray shaded film in Figure 3(c)). On the other hand, it was confirmed that the positive electrode active material prepared in Comparative Example 1 had carbon particle residue attached to the surface.

[0097] Meanwhile, Figure 4 is a SEM image showing the surface of (a) the positive electrode active material of Comparative Example 2, (b) the positive electrode active material of Comparative Example 4, and (c) the positive electrode active material of Example 1. As shown in Figure 4(b), when carbon black having a dense structure was coated, it was confirmed that even when a carbon coating layer was formed by the mechanofusion method, the carbon particles were not uniformly coated on the particle surface, but were attached in an agglomerated form at the boundaries between primary particles.

[0098] In addition, Fig. 5 is a SEM image of the surface of the positive electrode active material of Example 1, and Fig. 6 is a SEM image of the surface of the positive electrode active material of Comparative Example 6. As shown in Fig. 5, it was confirmed that when carbon black satisfying the shape, specific surface area, degree of graphitization, and DBP oil absorption of the present invention was used, a carbon coating layer was uniformly formed on the surface. On the other hand, as shown in Fig. 6, it was confirmed that when the shape, specific surface area, degree of graphitization, or DBP oil absorption of the present invention was not satisfied, a carbon coating layer was not uniformly formed (white area in Fig. 6).

[0099] (2) Powder electrical conductivity of the positive electrode active material (S / cm) 5 g of the positive electrode active material produced in Examples 1 to 4 and Comparative Examples 1 to 6 was placed in a holder and rolled with a force of 30 kN. The powder electrical conductivity of the positive electrode active material was then measured using a four-point probe electrode (Mitsubishi Chemical, Powder Resistance System (MCP=PD51)) designed specifically for powders, and the results are shown in Table 2 below.

[0100] (3) BET specific surface area The specific surface areas of the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 6 were measured by the BET method. Specifically, they were calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77 K) using a BELSORP-mini II manufactured by BEL Japan, and are shown in Table 2.

[0101] [Table 2]

[0102] As shown in Table 2, it was confirmed that the positive electrode active materials prepared in Examples 1 to 4 had improved powder electrical conductivity compared to Comparative Examples 1 to 5.

[0103] Experimental Example 2 Lithium secondary batteries were manufactured using the positive electrode active materials manufactured in Examples 1 to 4 and Comparative Examples 1 to 6, and the capacity of each of the lithium secondary batteries including the positive electrode active materials of Examples 1 to 4 and Comparative Examples 1 to 6 was evaluated.

[0104] Specifically, the positive electrode active materials, carbon conductive material, and polyvinylidene fluoride (PVdF) binder prepared in Examples 1 to 4 and Comparative Examples 1 to 6 were mixed in a weight ratio of 97.5:1.0:1.5 in N-methyl-2-pyrrolidone (NMP) solvent to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a positive electrode.

[0105] Meanwhile, artificial graphite was used as the negative active material, and carbon black conductive material, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as binders were mixed in distilled water in a weight ratio of 96.4:0.5:2.3:1.1 to prepare a negative active material slurry, which was applied to a copper current collector with a thickness of 20 μm, dried, and then roll pressed to prepare a negative electrode.

[0106] An electrode assembly was prepared by interposing a 15 μm thick polyethylene separator between the positive and negative electrodes prepared above, and the electrode assembly was placed inside a battery case, and an electrolyte was then injected into the case to prepare a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2, and the lithium secondary batteries according to Examples 1 to 4 and Comparative Examples 1 to 6 were prepared.

[0107] Next, the lithium secondary batteries prepared in Examples 1 to 4 and Comparative Examples 1 to 6 were each charged at 25° C. at a constant current of 0.2 C up to 4.25 V with a 0.05 C cut-off, and then discharged at a constant current of 0.2 C up to 2.5 V to measure the initial charge and discharge capacities.

[0108] Next, charging was performed at a constant current of 0.2 C with a cutoff of 0.05 C up to 4.25 V, and discharging was performed at a constant current of 2.0 C up to 2.5 V. The above charge and discharge behavior was counted as one cycle, and such a cycle was repeated twice, after which the capacity characteristics at 2.0 C versus the 0.2 C discharge capacity of the lithium secondary batteries according to Examples 1 to 4 and Comparative Examples 1 to 6 were measured, and are shown in Table 3 below.

[0109] [Table 3]

[0110] As shown in Table 3, it was confirmed that the capacity characteristics of the secondary batteries of Examples 1 to 4 were superior to those of the secondary batteries of Comparative Examples 1 to 5. On the other hand, the capacity characteristics of the secondary battery of Comparative Example 6 were significantly inferior to that of Example 1 using the same weight of lithium transition metal oxide.

Claims

1. A step of mixing a lithium transition metal oxide and a hollow carbonaceous material to form a mixture, the carbonaceous material being mixed in an amount of 0.1 to 1.5 parts by weight per 100 parts by weight of the lithium transition metal oxide; and treating the mixture in a mechanical manner to form a carbon coating layer over the entire surface of the lithium transition metal oxide. The hollow carbonaceous material has a linear chain shape and a specific surface area of ​​500 m 2 / g or more, and the degree of graphitization (I D / I G ) is 1.0 or more, and the DBP oil absorption is 300 mL / 100 g or more; The carbon coating layer has a thickness of 500 nm or less, The mechanical treatment of the mixture is carried out by a mechanofusion method, The lithium transition metal oxide has a form of secondary particles formed by aggregation of primary particles, the carbon coating layer is uniformly formed on the boundaries between the primary particles of the lithium transition metal oxide; The method for producing a positive electrode active material, wherein the lithium transition metal oxide is Ni-rich.

2. The method for producing a positive electrode active material according to claim 1 , wherein the carbon-based material is in the form of secondary particles formed by agglomeration of primary particles.

3. The method for producing a positive electrode active material according to claim 2 , wherein the primary particle size of the carbon-based material is 50 nm or less.

4. The carbon-based material has a specific surface area of ​​500 m 2 / g~2,500m 2 The method for producing a positive electrode active material according to claim 1 , wherein the Cr content is 1 / g.

5. The carbon-based material has a graphitization degree (I D / I G 5. The method for producing a positive electrode active material according to claim 1, wherein the ratio of the positive electrode active material content to the positive electrode active material content is 1.0 to 2.

0.

6. The method for producing a positive electrode active material according to any one of claims 1 to 5, wherein the carbon-based material has a DBP oil absorption of 300 mL / 100 g to 2,000 mL / 100 g.

7. a lithium transition metal oxide; and a carbon coating layer formed on the surface of the lithium transition metal oxide, The lithium transition metal oxide has a form of secondary particles formed by aggregation of primary particles, The lithium transition metal oxide is Ni-rich; the carbon coating layer is formed on the entire surface of the lithium transition metal oxide; The carbon coating layer is formed uniformly on the boundaries between the primary particles of the lithium transition metal oxide, The carbon coating layer has a thickness of 500 nm or less, BET specific surface area is 0.5m 2 / g to 50m 2 / g, The positive electrode active material includes the carbon coating layer in an amount of 0.1 to 1.5 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

8. The positive electrode active material has a powder electrical conductivity of 3.7×10 measured after rolling with a force of 0.1 to 20 kN. -3 S / cm to 10x10 -3 The positive electrode active material according to claim 7, wherein the conductivity is 1.0 S / cm.

9. A positive electrode for a lithium secondary battery, comprising the positive electrode active material according to claim 7 or 8.

10. A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to claim 9.

Citation Information

Patent Citations

  • Enclosed type nickel-hydrogen storage battery

    JP1987295353A

  • Positive active material of secondary battery, its manufacture, and positive electrode

    JP1997092265A

  • Nonaqeous electrolyte secondary battery

    JP1998312811A

  • Secondary battery and positive electrode active material thereof

    JP1999154515A

  • Electrode for lithium secondary battery and lithium secondary battery using it

    JP2003308845A