Solid electrolyte, active material layer, electrolyte layer, and secondary battery

By using the oxide system structure of Li6+xR1-xM1x(BO3)3 in the solid electrolyte, through the substitution of rare earth elements and divalent elements and the optimization of X-ray diffraction analysis, the problem of insufficient ion conductivity during low-temperature sintering is solved and achieved. It creates an efficient solid electrolyte, lowers the sintering temperature and reduces the formation of high-resistance phases, improving the performance of secondary batteries.

CN118742976APending Publication Date: 2024-10-01CANON KK
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380022681.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing solid electrolytes have insufficient ion conductivity during low-temperature sintering and are difficult to improve, and high-temperature sintering may lead to the formation of high-resistance phases, limiting the improvement of ion conductivity.

Method used

An oxide-based solid electrolyte with the general formula Li6+xR1-xM1x(BO3)3 is used. By combining the rare earth elements Yb, Er, Tm and La and replacing the divalent elements Mg, Sr and Ca, the charge balance is adjusted to make Li+ Ions are present in excess in the crystal lattice to increase ion conductivity, and the diffraction peak position is adjusted through X-ray diffraction analysis to optimize the structure.

Benefits of technology

A high-ion conductivity solid electrolyte sintered at low temperature is achieved, which lowers the sintering temperature, reduces the formation of high-resistance phases, and improves the output performance of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742976A_ABST
    Figure CN118742976A_ABST
Patent Text Reader

Abstract

A solid electrolyte includes a borate salt, the borate salt including: Li; an element R selected from the group consisting of Yb, Er, Tm, and La; and an element M1 selected from the group consisting of Mg, Sr, and Ca.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid electrolyte, an active material layer, an electrolyte layer, and a secondary battery containing the same. Background Art

[0002] All-solid-state secondary batteries containing solid electrolytes can have higher heat resistance and improved safety because the electrolyte does not leak or volatilize. Therefore, module costs can be reduced and energy density can be increased.

[0003] As one of such solid electrolytes, sulfide-based solid electrolytes have been reported. However, because sulfide is used as a raw material for its production, sulfide-based solid electrolytes have problems in terms of processability. Therefore, oxide-based solid electrolytes have been reported as non-sulfide-based solid electrolytes.

[0004] As a Li-containing solid electrolyte, NASICON-type Li 1+x Al x Ti 2-x (PO 4 ) 3 (LATP), perovskite-type Li 3+x La 2 / 3-x TiO 3 (LLT) and garnet-type cubic Li 7 La 3 Zr 2 O 12 As a solid electrolyte containing Na, β"-alumina-type Na 2 O·(5-7)Al 2 O 3 and NASICON type Na 3 Zr 2 Si 2 PO 12 . However, these solid electrolytes have the following problems: the available negative electrode materials are limited, and sintering at a high temperature of more than 1000°C is required to improve conductivity by bringing the interfaces between the solid electrolytes and between the solid electrolytes and the active material into close contact with each other. In particular, sintering at high temperatures may cause the formation of a high resistance phase between the solid electrolytes and at the interface between the solid electrolyte and the active material, thereby limiting the improvement of ion conductivity.

[0005] For these reasons, attempts have recently been made to lower the sintering temperature. Patent Document 1 discloses a solid electrolyte containing lithium borate, such as Li 2+x C 1-x B x O 3 , and the firing temperature can be reduced to about 900℃.

[0006] Patent Document 2 discloses that LLZ-based oxides and Li 3 BO 3 Mixing can reduce the sintering temperature when the solid electrolyte is formed to 650°C to 800°C. Citation List Patent Literature

[0007] Patent Document 1: Japanese Patent Publication No. 5-54712 Patent Document 2: Japanese Patent Publication No. 2013-37992 Summary of the invention Technical issues

[0008] In the case of secondary batteries containing the respective solid electrolytes disclosed in Patent Document 1 and Patent Document 2, a low firing temperature is used, and a high resistance phase is less likely to be formed as an intermediate layer at the interface between the solid electrolyte and other materials. However, in some cases, the area occupied by the respective solid electrolyte has a surface area of ​​less than 1×10 -7 Ionic conductivity σ in S / cm SE There is a need for oxide-based solid electrolytes with enhanced ionic conductivity.

[0009] The present invention aims to provide a solid electrolyte which can be prepared by sintering at a low temperature and has high ion conductivity, and an electrolyte layer, an active material layer, and a secondary battery each containing the solid electrolyte. Solution to the problem

[0010] The solid electrolyte according to an embodiment of the present invention comprises a 6+x R 1-x M1 x (BO 3 ) 3 In the formula, R is a rare earth element selected from the group consisting of Yb, Er, Tm and La, M1 is a divalent element selected from the group consisting of Mg, Sr and Ca, and x is a real number satisfying 0<x<1.

[0011] The solid electrolyte according to the embodiment of the present invention includes a borate including Li, an element R selected from the group consisting of Yb, Er, Tm, and La, and an element M1 selected from the group consisting of Mg, Sr, and Ca. Advantageous Effects of the Invention

[0012] According to the present invention, a solid electrolyte that can be prepared by sintering at a low temperature and has high ion conductivity can be provided. In addition, according to the present invention, an electrolyte layer, an active material layer, and a secondary battery each containing the solid electrolyte can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 : is a graph showing the relationship between the ion conductivity of each solid electrolyte according to Examples 1 to 11 included in the first embodiment and the value of the composition x (x1+x2) of the substitution element M1. Figure 2 X-ray diffraction curves of the solid electrolytes according to Examples 1 to 11 are shown. Figure 3 X-ray diffraction curves of the solid electrolytes according to Examples 3 to 5 are shown. Figure 4A is a schematic cross-sectional view of a secondary battery according to a second embodiment. Figure 4B A positive electrode and an electrolyte layer of a secondary battery according to a second embodiment are shown. Figure 4C A positive electrode active material layer of a secondary battery according to the second embodiment is shown. Figure 4D is a partially enlarged view of an electrolyte layer of a secondary battery according to a second embodiment. DETAILED DESCRIPTION

[0014] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0015] (First embodiment) According to one embodiment, the solid electrolyte comprises a 6+x R 1-x M1 x (BO 3 ) 3 In the formula, R is a rare earth element selected from the group consisting of Yb, Er, Tm and La, M1 is a divalent element selected from the group consisting of Mg, Sr and Ca, and x is a real number satisfying 0<x<1.

[0016] In this formula, when R includes at least two elements selected from the trivalent elements Yb, Er, Tm and La, a combination of elements selected from the group including Yb, Er, Tm and La can be used, and a combination of these elements with other trivalent elements having an ionic radius close to these elements can also be used.

[0017] In other words, the solid electrolyte according to the present embodiment comprises a 6+x R 1-x M1 x (BO 3 ) 3 The inventors of the present application have speculated that the oxide represented by the general formula Li 6+x R1-x M1 x (BO 3 ) 3 The following reasons are shown for the improvement of ion conductivity in the solid electrolyte of the oxide.

[0018] When the rare earth elements Yb, Er, Tm, and La are partially replaced by the divalent element M1, the charge balance is adjusted so that the crystal is neutral overall, resulting in Li + The state in which ions are present in excess in the crystal lattice. In other words, Li + The state where the ions are present in excess is represented by Li + The state in which ions are incorporated into a crystal lattice.

[0019] Li + The state in which ions are incorporated into the crystal lattice is called interstitial ion. + The phenomenon that ions are pushed and moved one after another occurs in a synergistic manner, so it is believed that the ion conductivity is improved. In other words, because Li + Li occupied site + The phenomenon of ion migration occurs in a synergistic manner, so it is considered that the ion conductivity is improved.

[0020] In other words, the solid electrolyte of the present embodiment is a solid electrolyte containing a borate containing Li, an element R selected from the group including Yb, Er, Tm and La, and an element M1 selected from the group including Mg. M1 is a divalent element. M1 is at least one element selected from the group including Mg. As an element capable of replacing the trivalent element R including Yb, Er, Tm and La, an element having an ionic radius close to the trivalent element R is likely to replace it, specifically, Mg 2+ are potential candidates.

[0021] The solid electrolyte of the present embodiment preferably has a monoclinic crystal structure.

[0022] In X-ray diffraction analysis (hereinafter referred to as “XRD”) by a 2θ method using CuKα emission line, a diffraction peak at a diffraction angle 2θ of about 28° varies depending on the composition of the solid electrolyte.

[0023] In the solid electrolyte of this embodiment, the general formula Li 6+x R 1-x M1 x (BO 3 ) 3The R of the oxide represented by includes Yb, and in the XRD using the CuKα emission line, the solid electrolyte preferably has a diffraction peak in the range of 2θ=28.0° to 28.1°. In the above general formula, x corresponds to the amount of the substitution element M1 replacing the element R, and 0<x<1 is used. As the substitution amount x, a value of 0.01 or more and 0.30 or less is preferably used. As a more preferred x, a value of 0.01 or more and 0.10 or less is used.

[0024] The reason why the above range of x is preferred is inferred as follows: at an x ​​value of less than 0.01, since a small amount of element R is substituted, sufficient structural changes do not occur, and Li ions are not sufficiently supplied between the crystal lattices, resulting in failure to improve ion conductivity. An x value of more than 0.30 results in an excessively large amount of substitution element M1. Therefore, the excess element M1 that does not contribute to the substitution of element R in the crystal may serve as an inhibitory component for ion conduction without contributing to the substitution effect in the crystal.

[0025] In XRD using CuKα emission line, the position of the diffraction peak at about 2θ=28° can be controlled by adjusting the x value in the general formula or changing the element represented by M1.

[0026] Next, a method for producing the solid electrolyte of the present embodiment will be described.

[0027] The method for producing the solid electrolyte of the present embodiment includes a sintering step of heating Li, R and M1 in an oxygen-containing atmosphere. These elements constitute a solid electrolyte having a general formula of Li 6+x R 1-x M1 x (BO 3 ) 3 An element of a solid electrolyte of an oxide represented by or an oxide thereof (wherein, in the formula, R is at least one or two elements selected from the group consisting of rare earth elements Yb, Er, Tm and La, and M1 is a divalent element).

[0028] The method for producing the solid electrolyte of the present embodiment may include a calcining step of performing heat treatment at a temperature lower than the melting point of the oxide to perform solid phase synthesis of the oxide represented by the above general formula, and a step of densifying the obtained oxide by heat treatment.

[0029] [Method for producing solid electrolyte] The method for producing the solid electrolyte of the present embodiment, including the calcining step and sintering, will be described in detail below.

[0030] <Pre-burning Step> In the pre-burning step, Li 3 BO 3 , H 3 BO 3 , Yb2 O 3 , Er 2 O 3 、Tm 2 O 3 , MgO and La 2 O 3 The reagent-grade raw materials are weighed in a predetermined stoichiometric ratio and mixed together to form Li 6+x R 1-x M1 x (BO 3 ) 3 Here, R is at least one or two elements selected from the group consisting of rare earth elements Yb, Er, Tm, and La, and M1 is a divalent element.

[0031] As a device for mixing, a mixer such as a ball mill may be used in addition to a mortar and pestle.

[0032] After preparing the mixed powder of the above raw materials by mixing treatment, the obtained mixed powder is pressure-molded into pellets. Here, as a pressure molding method, a known pressure molding method such as cold uniaxial molding or cold isostatic pressing can be used. As a condition for pressure molding in the pre-firing step, the pressure can be (but is not particularly limited to) for example 100 to 300 MPa.

[0033] The obtained pellets are pre-fired at 500° C. to 800° C., and solid phase synthesis is performed using, for example, an atmospheric pressure firing apparatus. The time of the pre-fire step may be, for example, (but not particularly limited to), about 700 to 750 minutes (eg, 720 minutes).

[0034] The obtained calcined body is of the general formula Li 6+x R 1-x M1 x (BO 3 ) 3 The pre-sintered body may be ground with, for example, a mortar and pestle to prepare a pre-sintered powder.

[0035] <Particle crushing step> A particle crushing step may be added between the pre-sintering step and the firing step described below. In the particle crushing step, the particle size of the pre-sintered body is reduced and amorphized. This contributes to the reduction of the sintering temperature in the firing step and the merging of the grain boundaries. In order to crush the particles, a ball mill, a planetary ball mill, a paint shaker, a homogenizer, an ultrasonic homogenizer, etc. may preferably be used. The crushing step may be performed by a wet method or a dry method. In the case of a wet method, an alcohol such as ethanol, propanol or isopropanol may preferably be used as a solvent. After crushing, the particles are heated sufficiently to remove the solvent.

[0036] <Firing Step> In the firing step, at least one selected from the pre-fired body and the pre-fired body prepared in the pre-fire step is pressure-molded and fired to prepare a dense sintered body.

[0037] Pressure forming and sintering can be performed simultaneously, for example, by spark plasma sintering or hot pressing. Alternatively, after pellets are prepared by cold uniaxial forming, sintering can be performed, for example, in an air atmosphere. As a condition for pressure forming during sintering, the pressure can be (but is not particularly limited to), for example, 100 to 300 MPa.

[0038] The calcination temperature is preferably 800°C or lower, more preferably 700°C or lower, and still more preferably 680°C or lower.

[0039] The time of the firing step can be appropriately changed according to, for example, the firing temperature. For example, 700 to 750 minutes is used. There is no particular limitation on the cooling method in the firing step. Cooling slower than natural cooling can also be used.

[0040] A method for measuring physical properties according to the present disclosure will be described below.

[0041] Confirmation of R and M When the collected sample is not a mixture with other materials, after the collected sample is processed into a solution, the composition ratio of the sample can be confirmed using, for example, inductively coupled high-frequency plasma atomic emission spectrometry (ICP-AES) or wavelength dispersive X-ray fluorescence spectrometry (WDXRF). WDXRF can also be called WDX.

[0042] When the possibility that the collected sample is a mixture is high, a scanning analyzer capable of providing an element distribution image, such as an X-ray photoelectron spectrometer (XPS, ESCA) or a scanning electron microscope equipped with an energy dispersive X-ray fluorescence analyzer (EDXRF) can be used. In the following, a scanning electron microscope equipped with an energy dispersive X-ray fluorescence spectrometer (EDXRF) may be abbreviated as SEM / EDX. When the possibility that the collected sample is a mixture is high, a transmission electron microscope equipped with an electron beam diffraction function (TEM-ED) can be used to confirm the crystal structure. EDXRF may also be referred to as EDX.

[0043] In order to accurately determine the composition ratio of Li, which is a light element, and other elements having higher atomic numbers (such as B, O, Zr, and rare earth elements), ICP-AES and XPS were used.

[0044] When the collected sample is a mixture, pretreatment is used to selectively remove non-target sites for analysis by physical removal processes (such as cutting or ion beam processing), chemical removal (such as dry etching or wet etching), or a combination thereof. For pretreatment, cleaning, degreasing, slicing, grinding, granulation, etc. can be used.

[0045] As for the standard sample, S-4800 manufactured by Hitachi High-Technologies Corporation can be used as an analyzer for SEM / EDX.

[0046] Measurement of X-ray diffraction peaks RINT-2100 manufactured by Rigaku Corporation was used for X-ray diffraction analysis of the solid electrolyte.

[0047] The powder prepared by grinding the solid electrolyte with a mortar and pestle was subjected to X-ray diffraction analysis using characteristic X-rays of CuKα. The temperature was room temperature, the analysis range was 10° to 70°, the step size was 0.016°, and the scanning speed was 0.5 steps / second.

[0048] (Second embodiment) <Structure of Secondary Battery> Will refer to Figure 4A and 4B The electrolyte layer 40 including a solid electrolyte and the secondary battery 100 including the electrolyte layer 40 according to the first embodiment are described.

[0049] Figure 4A 1 is a schematic cross-sectional view of a secondary battery 100 including an electrolyte layer using a solid electrolyte of the present embodiment. The secondary battery 100 includes an electrolyte layer 40 on the surface of the positive electrode active material layer 20, which is opposite to the side of the positive electrode collector layer 10 contacting the positive electrode active material layer 20. The secondary battery 100 includes a negative electrode 70 on the side of the electrolyte layer 40, which is opposite to the side of the electrolyte layer 40 contacting the positive electrode active material layer 20. The negative electrode 70 includes a negative electrode active material layer 50 on the surface of the electrolyte layer 40, which is opposite to the surface contacting the positive electrode active material layer 20. The negative electrode 70 includes a negative electrode collector layer 60 on the surface of the negative electrode active material layer 50, which is opposite to the surface contacting the electrolyte layer 40. In other words, the secondary battery 100 includes a negative electrode 70, an electrolyte layer 40, and a positive electrode 30 in the stacking direction 200.

[0050] (Positive Electrode Active Material Layer) like Figure 4B As shown, the positive electrode active material layer 20 using the solid electrolyte of the present embodiment is in contact with a positive electrode 30 including a positive electrode current collector layer 10 and a positive electrode active material layer 20 containing active material particles 22 and a positive electrode electrolyte 24. In this specification, a structure configured to release lithium ions (active material ions) to the electrolyte layer 40 or to receive lithium ions from the electrolyte layer 40 is referred to as a positive electrode; therefore, the positive electrode active material layer 20 (which is a portion of the positive electrode 30 other than the positive electrode current collector layer 10) may also be referred to as a positive electrode 20, such as Figure 4AThe positive electrode active material layer 20 of this embodiment includes a positive electrode electrolyte 24 , and thus may be referred to as a composite positive electrode active material layer 20 or a composite positive electrode structure 20 .

[0051] The current collector layer 10 is a conductor that conducts electrons between an external circuit (not shown) and an active material layer. As the current collector layer 10, a self-supporting film of a metal such as stainless steel (SUS) or aluminum, or a laminated structure of a metal foil and a resin matrix is ​​used.

[0052] The positive electrode active material layer 20 includes positive electrode active material layers 20a, 20b and 20c as sublayers. The positive electrode active material layers 20a, 20b and 20c are distinguished by the stacking units in the layer thickness direction 200 before sintering the active material particles 22 and the positive electrode electrolyte 24. The positive electrode active material layers 20a, 20b and 20c may have a distribution of the volume fraction of the active material particles 22 and the positive electrode electrolyte 24, the conductive aid (not shown) and the void ratio (porosity) in the layer thickness direction. The layer thickness direction 200 is parallel or anti-parallel to the stacking direction of the stacked layers, and therefore may also be referred to as the stacking direction 200.

[0053] The solid electrolyte according to the present embodiment is used for the positive electrode electrolyte 24 in the positive electrode active material layer 20 .

[0054] (Electrolyte layer) The positive electrode electrolyte 24 and the solid electrolyte 44 in the electrolyte layer 40 may have the same composition and particle size distribution, or may have different compositions and particle size distributions. That is, the solid electrolyte according to the present embodiment can be used for the solid electrolyte 44 included in the electrolyte layer 40. Examples of materials other than the materials of the first embodiment for the solid electrolyte 44 of the electrolyte layer 40 include Li 3 PO 4 , Li 7 La 3 Zr 2 O 12 , Li 0.33 La 0.55 TiO 3 and Li 1.5 Al 0.5 Ge 1.5 (PO 4 ) 3 .

[0055] The amount of the solid electrolyte of the present embodiment contained in the solid electrolyte 44 is preferably 25% by mass or more, more preferably 50% by mass or more, and still more preferably 75% by mass or more and 100% by mass or less.

[0056] The secondary battery of the present embodiment can be manufactured by a known method, for example, by lamination, molding and heat treatment of a positive electrode, a solid electrolyte and a negative electrode. The solid electrolyte of the present embodiment can be manufactured by heat treatment at a lower temperature than conventional technology. This reduces the formation of a high-resistance phase exhibiting high resistance due to the reaction between the solid electrolyte and the electrode active material, thereby enabling a secondary battery with excellent output characteristics to be obtained. The "solid" used in this specification includes an object with self-supporting properties, so that even if the posture of the object changes, a certain shape and volume can be maintained. In other words, the object is non-flowable and its viscosity is less than 1×10 7 cP(less than 1×10 4 Pa·s).

[0057] (Negative Electrode Active Material Layer) Similar to the positive electrode 30 , the negative electrode active material layer 50 may have a structure in which both the negative electrode active material and the solid electrolyte are contained in the layer, or it may be formed of a single-phase film composed of the negative electrode active material, such as metal Li or In—Li.

[0058] As the negative electrode active material, any material among metals, metal fibers, carbon materials, oxides, nitrides, silicon, silicon compounds, tin, tin compounds, various alloy materials, etc. is used. Among these materials, from the viewpoint of capacity density, the negative electrode active material is preferably metal, oxide, carbon material, silicon, silicon compound, tin, tin compound, etc. Examples of metals used for the negative electrode active material include metal Li and In-Li. Examples of oxides include Li 4 Ti 5 O 12 (lithium titanate: LTO). Examples of carbon materials for negative electrode active materials include various natural graphites (graphites), coke, graphitizable carbon materials that undergo graphitization, carbon fibers, spherical carbon, various artificial graphites, and amorphous carbon. Examples of silicon compounds for negative electrode active materials include silicon-containing alloys, silicon-containing inorganic compounds, silicon-containing organic compounds, and solid solutions. Examples of tin compounds for negative electrode active materials include SnO b (0<b<2), SnO 2 、SnSiO 3 、Ni 2 Sn 4 and Mg 2Sn. The negative electrode active material layer 50 may contain a conductive aid. Examples of the conductive aid used for the negative electrode active material layer 50 include graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers, carbon nanotubes, and metal fibers, carbon fluoride, metal powders such as aluminum, conductive metal oxides such as conductive whiskers such as zinc oxide and titanium oxide, and organic conductive materials such as phenylene dielectrics.

[0059] Next, a secondary battery 100 will be described in which the solid electrolyte according to the present embodiment is used for the positive electrode electrolyte 24 of the composite positive electrode active material layer 20 .

[0060] like Figure 4C As shown, the positive electrode 30 includes the solid electrolyte 24 of the present embodiment, the positive electrode active material 22, and the surface 20AS, the positive electrode active material 22 is configured to release lithium ions to the solid electrolyte 24 or receive lithium ions from the solid electrolyte 24, and the solid electrolyte 24 and the positive electrode active material 22 are arranged at the surface 20AS. In other words, the positive electrode active material layer 20 includes the solid electrolyte 24 of the present embodiment, the positive electrode active material 22, and the surface 20AS, the positive electrode active material 22 is configured to release lithium ions to the solid electrolyte 24 or receive lithium ions from the solid electrolyte 24, and wherein the solid electrolyte 24 and the positive electrode active material 22 are arranged at the surface 20AS. The electrolyte layer 40 of the present embodiment is a layer that is provided in contact with the surface 20AS and is configured to release lithium ions to the positive electrode 30 or receive lithium ions from the positive electrode 30. The secondary battery 100 includes a positive electrode 30, an electrolyte layer 40, and a negative electrode 70, wherein the electrolyte layer 40 is configured to contact the surface 20AS of the positive electrode 30 and is configured to release lithium ions to the positive electrode 30 or receive lithium ions from the positive electrode 30, and the negative electrode 70 is in contact with the surface of the electrolyte layer 40 opposite to the side of the contact surface 20AS of the electrolyte layer 40.

[0061] A secondary battery 100 in which a solid electrolyte according to a modification of the present embodiment is used for the solid electrolyte 44 of the electrolyte layer 40 will be described below.

[0062] like Figure 4B As shown, the electrolyte layer 40 according to the modified embodiment has a surface 40AS, wherein the solid electrolyte of the first embodiment is arranged in a direction intersecting with the layer thickness direction 200. The secondary battery 100 includes the electrolyte layer 40, the positive electrode 30, which is arranged to contact with the surface 40AS and is arranged to release lithium ions to the electrolyte layer 40 or receive lithium ions from the electrolyte layer 40, and the negative electrode 50, which is in contact with the surface of the electrolyte layer 40 opposite to the surface 40AS. Example

[0063] Examples of manufacturing and evaluating the solid electrolyte of the present embodiment in the form of a sintered body will be described. The present disclosure is not limited to the following examples.

[0064] [Example 1] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.02 Yb 0.98 Mg 0.02 (BO 3 ) 3 , and mix using a mortar and pestle.

[0065] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0066] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0067] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0068] [Example 2] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (manufactured by Kojun Chemical Research Institute), La 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.01 Yb 0.891 La 0.099 Mg 0.01 (BO 3 )3 , and mix using a mortar and pestle.

[0069] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0070] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0071] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0072] [Examples 3-7] <Pre-burning Step> A calcined body and calcined powder were prepared in the same manner as in Example 1, except that the raw materials described in Example 2 were weighed in a predetermined stoichiometric ratio so that the R1 ratio, the R2 ratio and x had the values ​​given in Table 1.

[0073] <Firing Step> The pre-sintered powder prepared above was subjected to the same sintering step as in Example 1 to prepare a sintered body.

[0074] [Example 8] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Tm 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.02 Tm 0.98 Mg 0.02 (BO 3 ) 3 , and mix using a mortar and pestle.

[0075] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0076] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0077] [Example 9] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (manufactured by Kojun Chemical Research Institute), Tm 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.01 Yb 0.882 Tm 0.098 Mg 0.02 (BO 3 ) 3 , and mix using a mortar and pestle.

[0078] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0079] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0080] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0081] [Example 10] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Er 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.02 Er 0.98 Mg 0.02 (BO 3 ) 3 , and mix it using a mortar and pestle.

[0082] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0083] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0084] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0085] [Example 11] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (manufactured by Kojun Chemical Research Institute), Er 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.01 Yb 0.882 Er 0.098 Mg 0.02 (BO 3 ) 3 , and mix using a mortar and pestle.

[0086] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0087] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0088] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0089] [Comparative Example 1] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3(manufactured by Kishida Chemical Co., Ltd.) and Yb 2 O 3 (produced by Kojun Chemical Research Institute) as the raw material of the solid electrolyte. They were weighed according to a predetermined stoichiometric ratio so that the composition after sintering was Li 6 Yb(BO 3 ) 3 , and mix using a mortar and pestle.

[0090] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0091] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0092] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0093] [Comparative Example 2] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (manufactured by Kojun Chemical Research Institute) and La 2 O 3 (produced by Kojun Chemical Research Institute) as the raw material of the solid electrolyte. They were weighed according to a predetermined stoichiometric ratio so that the composition after sintering was Li 6 Yb 0.9 La 0.1 (BO 3 ) 3 , and mix using a mortar and pestle.

[0094] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0095] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0096] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0097] [Reference Example 1] <Pre-burning Step> Provide Li 3 BO 3 (manufactured by Toyoshima Manufacturing Co., Ltd.), H 3 BO 3 (manufactured by Kishida Chemical Co., Ltd.), Yb 2 O 3 (manufactured by Kojun Chemical Research Institute), La 2 O 3 (produced by Kojun Chemical Research Institute) and MgO (produced by Kojun Chemical Research Institute) were used as raw materials for the solid electrolyte. They were weighed in a predetermined stoichiometric ratio so that the composition after sintering was Li 6.4 Yb 0.54 La 0.06 Mg 0.4 (BO 3 ) 3 , and mix using a mortar and pestle.

[0098] The mixed powder was then cold uniaxially molded using a hydraulic press SSP-10A manufactured by Shimadzu Corporation and heat treated in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.

[0099] The obtained calcined body was ground with a mortar and pestle to prepare a calcined powder.

[0100] <Firing Step> The calcined powder prepared above was molded and heat-treated in the same manner as in the calcination to prepare a sintered body of Example 1. The heating temperature was 670° C. and the holding time was 720 minutes.

[0101] Composition analysis and measurement of X-ray diffraction peaks were performed by the above-described methods on the sintered bodies of Examples 1 to 11, Comparative Examples 1 and 2, and Reference Example 1. Ion conductivity was measured by the following method. The method for measuring ion conductivity will be described below.

[0102] ·Measurement of ionic conductivity Using a magnetron sputtering system MSP-10 manufactured by Vacuum Device Co., Ltd., gold electrodes were deposited on the top and bottom surfaces of each flat sintered body obtained by the firing step to prepare a sample for AC impedance measurement.

[0103] The AC impedance measurement was performed using a potentiostat / galvanostat SI 1287A and a frequency response analyzer 1255B manufactured by Solartron Analytical. The measurement conditions were room temperature and a frequency of 1 MHz to 0.1 Hz.

[0104] The resistance of the sintered body was calculated from the complex impedance diagram obtained by the impedance measurement. From the calculated resistance, the thickness of the sintered body and the electrode area, the ion conductivity was determined using the following equation. Ionic conductivity (S / cm) = sintered body thickness (cm) / (sintered body resistance (Ω) × electrode area (cm) 2 ))

[0105] result Table 1 shows the stoichiometric amounts of raw materials and heating temperatures during firing, diffraction peak positions and ion conductivity, and the composition ratio [M1] / [R] of substitutional metals when preparing solid electrolytes according to Examples 1 to 11, Comparative Examples 1 and 2, and Reference Example 1. Figure 1 : is a scatter diagram showing the relationship between the amount x of the substitution element M1 replacing the element R of the solid electrolyte of the first example 1-11 and the ion conductivity.

[0106] Figure 2 The diffraction curves obtained by XRD in the range of 2θ=10° to 40° are shown. It can be seen that the crystal structure in each of Examples 1 to 7 is similar to that of Li 6 Yb(BO 3 ) 3 The same type of monoclinic crystal structure, the crystal structure in each of Examples 8 and 9 is the same as Li 6 Tm(BO 3 ) 3 The same type of monoclinic crystal structure, and the crystal structure in each of Examples 10 and 11 is the same as that of Li 6 Er(BO 3 ) 3 The same type of monoclinic crystal structure, which is similar to Li 6 Yb(BO 3 ) 3 Same type.

[0107] Figure 3 The diffraction curves obtained by XRD in the range of 2θ = 27° to 29° are shown. It can be seen that when the ionic conductivity σ is 4×10 -7In each of the solid electrolytes of Examples 3 to 5 with a S / cm or higher, the peak positions at about 2θ=28.1° and about 28.5° are shifted to lower angles than the peak positions in Comparative Example 1. These are considered to be changes in X-ray diffraction lines corresponding to changes in the crystal structure caused by replacement of at least a portion of Yb (which is a rare earth element) by at least one element selected from M1.

[0108] As shown in Table 1, when the ionic conductivity σ is 1×10 -7 In each solid electrolyte of Examples 1 to 11 with an X-ray diffraction peak of more than 100 s / cm, the difference in the amount of displacement between the high-angle side peak and the low-angle side peak of the double-peak diffraction angle peak was observed as the X-ray diffraction peak shifted. It can be seen that when the diffraction angle 2θ is in the range of 27.9° to 28.6°, the diffraction angle difference 2θd between the high-angle side diffraction peak observed at 28.3° to 29.0° and the low-angle side diffraction peak observed at 27.9° to 28.3° increases to more than 0.43°. When the ion conductivity σ is 1×10 -7 In each of the solid electrolytes of Examples 1 to 11 having a S / cm or higher, the diffraction angle difference 2θd of the double-peak diffraction angle peak at the X-ray diffraction angle 2θ of 28.3° to 29.0° was 0.432° to 0.448°.

[0109] In other words, the solid electrolyte according to the present embodiment includes a solid electrolyte containing a borate, wherein the borate contains Li, an element R selected from the group including Yb, Er, Tm and La, and an element M1 selected from the group including Mg. In addition, the solid electrolyte according to the present invention (in other words) is an electrolyte that exhibits two diffraction peaks in the diffraction angle 2θ range of 27.9° to 28.6° in XRD using CuKα emission line, wherein the diffraction angle difference 2θd between the high-angle side diffraction peak and the low-angle side diffraction peak is 0.43° or more.

[0110] The two diffraction angle peaks observed in the diffraction angle 2θ range of 27.9° to 28.6° may further include multiple peaks, including three peaks or four peaks, depending on the crystallinity. In this specification, the two diffraction angle peaks are respectively expressed as having a peak on the low angle side and a peak on the high angle side, adjacent to a diffraction angle 2θ of 28.3°. In this way, the diffraction angle peaks are separated by fitting the double peak diffraction line.

[0111] As the composition of the substitution element M increases or as the ion conductivity increases, such a high-angle side diffraction angle peak is more significantly broadened and moved to a higher angle than the low-angle side diffraction angle peak. It can be seen from this that the solid electrolyte 44 of the present embodiment has a different crystal structure from the unsubstituted comparative example, and a plurality of crystal structures having distributions of lattice spacing and grain size are mixed.

[0112] The solid electrolytes of Examples 2 to 7, 9 and 11 described in Table 1 are different from the solid electrolytes of Examples 1, 8 and 10 in that the rare earth element R is a binary system (Yb, Tm), (Yb, Er) and (Yb and La).

[0113] In the solid electrolytes having ion conductivities of 1E-7 (S / cm) or more in Examples 1 to 11, the atomic concentration ratio [M1] / [R] of the replacement element M to the rare earth element R is 0.020 or more and 0.429 or less. In the solid electrolytes having ion conductivities of 0.4E-6 (S / cm) or more in Examples 3 to 5 and 11, the atomic concentration ratio [M1] / [R] of the replacement element M1 to the rare earth element R is 0.020 or more and 0.111 or less.

[0114] Table 1

[0115] The present invention is not limited to the above embodiments, and various changes and modifications can be made without departing from the spirit and scope of the present invention. Therefore, the following claims are attached to disclose the scope of the present invention.

[0116] This application claims priority based on Japanese Patent Application No. 2022-028467 filed on February 25, 2022, which is hereby incorporated by reference in its entirety.

Claims

1. A solid electrolyte comprising a general formula Li 6+x R 1-x M1 x (BO3)3 represented by oxide, Wherein in the formula, R is a rare earth element selected from the group consisting of Yb, Er, Tm and La, M1 is a divalent element selected from the group consisting of Mg, Sr and Ca, and x is a real number satisfying 0<x<1. 2 . The solid electrolyte according to claim 1 , wherein x satisfies 0.01≤x≤0.

30. 3 . The solid electrolyte according to claim 1 , wherein R comprises Yb and La, and x satisfies 0.02≤x≤0.

10.

4. A solid electrolyte comprising a borate, the borate comprising: Li, an element R selected from the group consisting of Yb, Er, Tm and La, and an element M1 selected from the group consisting of Mg, Sr and Ca.

5. The solid electrolyte according to any one of claims 1 to 4, wherein M1 is Mg.

6. A solid electrolyte according to any one of claims 1 to 5, wherein in an X-ray diffraction analysis performed by a 2θ method using CuKα emission lines, the solid electrolyte exhibits two diffraction peaks within a diffraction angle range of 27.9° to 28.6°, and a diffraction angle difference 2θd between a high-angle side diffraction peak and a low-angle side diffraction peak is 0.43° or more. 7 . The solid electrolyte according to claim 6 , wherein the diffraction angle difference 2θd is 0.432° or more and 0.448° or less. 8 . The solid electrolyte according to claim 1 , wherein an atomic concentration ratio [M1] / [R] of the element M1 to the element R is 0.020 or more and 0.429 or less. 9 . The solid electrolyte according to claim 8 , wherein the atomic concentration ratio [M1] / [R] is 0.020 or more and 0.111 or less. 10 . The solid electrolyte according to claim 1 , wherein the element R comprises a plurality of rare earth elements. The solid electrolyte according to claim 10 , wherein the plurality of rare earth elements include at least Yb.

12. A positive electrode comprising a solid electrolyte according to any one of claims 1 to 11, a positive electrode active material and a surface, wherein the positive electrode active material is configured to release lithium ions to the electrolyte or accept lithium ions from the electrolyte, and the solid electrolyte and the active material are arranged on the surface.

13. A secondary battery comprising a positive electrode according to claim 12, an electrolyte layer and a negative electrode, wherein the electrolyte layer is configured to contact the surface and is configured to accept lithium ions from the positive electrode or release lithium ions to the positive electrode, and the negative electrode is in contact with the opposite surface of the electrolyte layer side that is in contact with the surface.

14. An electrolyte layer comprising a surface on which the solid electrolyte according to any one of claims 1 to 11 is arranged in a direction intersecting a layer thickness direction.

15. A secondary battery comprising an electrolyte layer according to claim 14, a positive electrode and a negative electrode, wherein the positive electrode is configured to contact the surface and is configured to release lithium ions to the electrolyte layer or accept lithium ions from the electrolyte layer, and the negative electrode is in contact with the surface opposite to the surface of the electrolyte layer.

Citation Information

Cited By

  • Preparation method of halide electrolyte and solid-state battery

    CN122000439A