Ternary eutectic solid electrolyte, preparation method thereof and solid-state lithium battery

Through the preparation method of ternary eutectic solid electrolyte, combined with deep eutectic solvents and modifiers, the cost, complexity and performance of composite solid electrolytes are solved, and high-performance lithium-ion battery electrolytes are realized, with low cost. , simplified preparation, high performance and safety.

CN119050455APending Publication Date: 2024-11-29CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411150292.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lithium-ion battery system has problems with high safety risks and low energy density, and the composite solid electrolyte has not yet achieved satisfactory performance in terms of cost, preparation process complexity and ionic conductivity.

Method used

Using the preparation method of ternary eutectic solid electrolyte, a deep eutectic solvent is formed by mixing lithium-containing hydrogen bond acceptors and hydrogen bond donors, and combined with a modifier to form a ternary eutectic solvent and a polymer solution uniformly. Mixed and dried to form to obtain a solid electrolyte with high ionic conductivity, mechanical properties and safety.

Benefits of technology

It realizes low-cost and simplified preparation methods, improves the flexibility, thermal stability, self-extinguishing, ionic conductivity and safety of solid electrolytes, and ensures long cycle stability and excellent safety at high magnifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a ternary eutectic solid electrolyte, a preparation method thereof and a solid-state lithium battery. The preparation method of the ternary eutectic solid electrolyte comprises the following steps: S1, mixing a hydrogen bond acceptor containing lithium ions and a hydrogen bond donor to obtain a deep eutectic solvent; s2, mixing the deep eutectic solvent with a modifier to obtain a ternary eutectic solvent; the modifier comprises one or more of ethylene carbonate, vinylene carbonate and fluoroethylene carbonate; s3, dissolving a polymer in an organic solvent to obtain a polymer solution; s4, uniformly mixing the ternary eutectic solvent and the polymer solution to obtain a ternary eutectic polymer solution; and S5, carrying out drying molding on the ternary eutectic polymer solution to obtain the ternary eutectic solid electrolyte. The ternary eutectic solid electrolyte disclosed by the invention has the advantages of excellent ionic conductivity, relatively strong mechanical property, flame retardance, stable interface property and excellent safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ternary eutectic solid electrolyte and a preparation method thereof and a solid-state lithium battery, belonging to the technical field of preparation of solid-state electrolytes for solid-state batteries. Background Art

[0002] As a hot energy storage device in today's society, lithium-ion batteries are currently widely used in various electronic products, electric vehicles, energy storage systems and other special-purpose equipment. In the next few decades, the global demand for lithium-ion batteries will undoubtedly continue to grow, especially in the field of electric vehicles and various electronic products. At the same time, with the development of industry and the increase in social needs, higher requirements are also put forward for lithium-ion batteries, such as long life, high charging and discharging speed, high safety, high greenness, high energy density and low cost. However, the current lithium-ion battery system faces many problems such as high safety risks and low energy density and cannot meet these requirements, so it is urgent to develop new lithium batteries.

[0003] Commercial all-solid-state lithium batteries have attracted much attention due to their high energy density and safety. The use of solid electrolytes can increase the energy density of the battery and improve safety by avoiding the use of organic electrolytes. The main solid electrolytes are currently divided into three categories: polymer solid electrolytes, inorganic solid electrolytes, and composite solid electrolytes. However, the compatibility between inorganic solid electrolytes and the electrode interface is poor. Polymer solid electrolytes are more flexible and can reduce interfacial impedance. The most promising research area at present is composite solid electrolytes, which can maximize the advantages of different electrolyte combinations. The matrix of composite solid electrolytes is mainly composed of polymers. Polymers such as polyethylene oxide (PEO), polyethylene glycol diacrylate (PEGDA), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and polymethyl methacrylate (PMMA) have been studied. Improving the ionic conductivity of composite solid electrolytes by modifying inorganic fillers and plasticizers has always been the focus of research. For example, the addition of two-dimensional hydroxyapatite (HAP) nanomaterials and N-methylpyrrolidone (NMP) to the PVDF-HFP polymer matrix can improve the ionic conductivity of solid electrolytes. Succinonitrile (SCN) can be used to create new ion transport pathways, enhance the mechanical properties of the electrolyte, and prevent the formation of lithium dendrites. After adding the plasticizer succinonitrile (SN), the crystallinity of PEO decreased and the ionic conductivity was 2.57 × 10 at 30 °C. -4S cm-1, the lithium ion transfer number is 0.6. PEO also helps to reduce the crystallinity. It can be seen that the modification can further improve the performance of the composite electrolyte. However, there are still many problems with composite electrolytes, such as high cost, complicated preparation process and low ion conductivity. In order to solve these problems, the present invention modifies the polymer solid electrolyte by a modifier, in order to further reduce the production cost, simplify the preparation method, and improve the ion conductivity, flame retardancy, thermal stability and safety. Summary of the invention

[0004] The purpose of the present invention is to provide a ternary eutectic solid electrolyte and a preparation method thereof and a solid-state lithium battery. The preparation method of the solid electrolyte is simple and low in cost, and the prepared solid electrolyte has good flexibility, thermal stability, self-extinguishing property, high ionic conductivity, an electrochemical window of 4.6V, long cycle stability at high rate and high safety.

[0005] To achieve the above object, the present invention adopts the following technical solution: In a first aspect, the present invention provides a method for preparing a ternary eutectic solid electrolyte, comprising the following steps: S1, mixing a hydrogen bond acceptor and a hydrogen bond donor containing lithium ions to obtain a deep eutectic solvent; S2, mixing the deep eutectic solvent and the modifier to obtain a ternary eutectic solvent; The modifier includes one or more of ethylene carbonate (EC), vinylene carbonate (VC), and fluoroethylene carbonate (FEC); S3, dissolving the polymer in an organic solvent to obtain a polymer solution; The polymer includes one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyethylene glycol diacrylate, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate; S4, uniformly mixing the ternary eutectic solvent and the polymer solution to obtain a ternary eutectic polymer solution; S5. Drying and molding the ternary eutectic polymer solution to obtain the ternary eutectic solid electrolyte.

[0006] Based on the above technical scheme, the present invention first mixes a deep eutectic solvent and a modifier such as fluoroethylene carbonate to obtain a ternary eutectic solvent; then the ternary eutectic solvent is mixed with a solution of a polymer such as poly(vinylidene fluoride-co-hexafluoropropylene), and a solid electrolyte is obtained by drying and molding. On the one hand, by binding the ternary eutectic solvent to the three-dimensional network of the polymer, the large number of hydrogen bonds of DESs in the ternary eutectic solvent can adjust the smoothness of the interface, thereby reducing the interface impedance of the solid-solid interface; on the other hand, the deep eutectic solvent can interact with fluoroethylene carbonate, which can improve the ionic conductivity and thermal stability, and promote the uniform deposition of metallic lithium and the stable formation of the SEI layer in the solid state.

[0007] In the preparation method of the above-mentioned ternary eutectic solid electrolyte, the hydrogen bond acceptor containing lithium ions includes any one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonylimide), lithium bis(fluorosulfonylimide), lithium perchlorate, lithium nitrate, lithium chloride and lithium difluorophosphate; The hydrogen bond donor is any one of N-methylacetamide, acetamide, butanamide, propionamide, N,N-dimethylpropylene urea, methyl pyruvate dimethyl sulfone, ethylene carbonate, succinonitrile and 2,2'-dithiodipyridine; The molar ratio of the hydrogen bond acceptor containing lithium ions to the hydrogen bond donor is 1:(2-6), including but not limited to 1:(3-4), 1:4 or 1:3.

[0008] As an example, the hydrogen bond acceptor containing lithium ions is lithium bis(trifluoromethanesulfonyl imide), the hydrogen bond donor is N-methylacetamide or succinonitrile, the molar ratio of the lithium bis(trifluoromethanesulfonyl imide to the N-methylacetamide is preferably 1:4, and the molar ratio of the lithium bis(trifluoromethanesulfonyl imide to the succinonitrile is 1:4 or 1:3. The purity of the lithium bis(trifluoromethanesulfonyl imide) is ≥99.99%.

[0009] In the above-mentioned method for preparing the ternary eutectic solid electrolyte, the volume ratio of the deep eutectic solvent to the modifier is (3-6):1, including but not limited to 4:1. As an example, the modifier is fluoroethylene carbonate, and the volume ratio of the deep eutectic solvent to the fluoroethylene carbonate is 4:1.

[0010] In the above-mentioned method for preparing the ternary eutectic solid electrolyte, the number average molecular weight of the polymer is 100,000 to 1,000,000, including but not limited to 130,000, 149,000 to 151,000; as an example, the polymer is poly(vinylidene fluoride-co-hexafluoropropylene); or, the polymer is poly(vinylidene fluoride-co-hexafluoropropylene) and polyacrylonitrile in a mass ratio of 10:1 or 5:1.

[0011] The organic solvent may be any good solvent for the polymer, including but not limited to N,N-dimethylformamide; The mass ratio of the polymer to the organic solvent is 1:(4-6), including but not limited to 1:6 or 1:5; as an example, the mass ratio of the poly(vinylidene fluoride-co-hexafluoropropylene) to the N,N-dimethylformamide is 1:6; or, the mass ratio of the total amount of the poly(vinylidene fluoride-co-hexafluoropropylene) and the polyacrylonitrile to the N,N-dimethylformamide is 1:5; In the above-mentioned method for preparing the ternary eutectic solid electrolyte, the mass ratio of the ternary eutectic solvent to the polymer solution is 1:(2-5), such as every 3.5 g of the polymer solution is mixed with 0.8 mL of the ternary eutectic solvent.

[0012] In the above-mentioned method for preparing the ternary eutectic solid electrolyte, further, the method further comprises the following step before the drying and forming: ultrasonically treating the ternary eutectic polymer solution to remove bubbles in the solution. As an example, the ultrasonic treatment is performed in an ultrasonic oscillator for a treatment time of 0.5 h.

[0013] In the above-mentioned preparation method of ternary eutectic solid electrolyte, further, the drying and molding step is as follows: pouring the ternary eutectic polymer solution into a mold for drying treatment; in specific operation, dripping the ternary eutectic solid electrolyte on a circular groove polytetrafluoroethylene mold of different depths, and controlling the thickness of the solid electrolyte by controlling the dripping amount; through the above treatment, a large number of bubbles can be avoided in the electrolyte after drying; preferably, the drying treatment is first dried at 40 to 60 degrees Celsius (such as 50 degrees Celsius) for 2 to 5 hours, and then vacuum dried at 60 to 80 degrees Celsius (such as 70 degrees Celsius) for 4 to 6 hours. Among them, slowly volatilizing the organic solvent at 40-60 degrees Celsius first can avoid the solvent from volatilizing too quickly, resulting in the generation of bubbles and large-area shrinkage of the electrolyte, and vacuum drying at 60-80 degrees Celsius can further completely volatilize the solvent and avoid the reaction of the organic solvent with the electrode.

[0014] In a second aspect, the present invention provides a ternary eutectic solid electrolyte obtained by any of the preparation methods described above. When storing the ternary eutectic solid electrolyte of the present invention, the dried solid electrolyte is transferred to an anhydrous and oxygen-free glove box while hot, and then the film is peeled off using rubber tweezers, and the obtained ternary eutectic solid electrolyte is sealed and stored in the glove box. During operation, the film should be peeled off slowly from the round edge to the center to avoid curling of the electrolyte.

[0015] In a third aspect, the present invention provides a solid-state lithium battery, comprising a positive electrode, a negative electrode and the ternary eutectic solid electrolyte.

[0016] Specifically, the positive electrode may be one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, and a ternary positive electrode material (such as a nickel-cobalt-manganese NCM ternary positive electrode material or a nickel-cobalt-aluminum NCA ternary positive electrode material).

[0017] Specifically, the negative electrode may be one of metallic lithium, graphite, lithium titanate, and silicon negative electrode, wherein the graphite may be pre-lithiated graphite.

[0018] As an example, the solid-state lithium battery is a button cell or a soft-pack battery. In the present invention, the soft-pack battery prepared by the ternary eutectic solid electrolyte has excellent cycle performance and high safety.

[0019] The present invention has the following beneficial effects: 1) The preparation method of the ternary eutectic solid electrolyte of the present invention is simple and has low preparation cost.

[0020] 2) The ternary eutectic solid electrolyte of the present invention has excellent ionic conductivity, strong mechanical properties, flame retardancy, stable interface properties and excellent safety.

[0021] 3) The deep eutectic solvent and fluoroethylene carbonate in the ternary eutectic solid electrolyte of the present invention synergistically improve the ionic conductivity and thermal stability and promote the uniform deposition of metallic lithium.

[0022] 4) In the deep eutectic solvent of the ternary eutectic solid electrolyte of the present invention, N-methylacetamide selectively occupies the lithium dissolution sheath, triggering a concentration gradient, thereby promoting the decomposition of fluoroethylene carbonate and promoting the formation of an inorganic solid electrolyte interphase layer, thereby improving the long cycle performance.

[0023] 5) The present invention can prepare a normal voltage solid electrolyte and a high voltage solid electrolyte by mixing poly (vinylidene fluoride-co-hexafluoropropylene) and polyacrylonitrile polymer and obtaining a deep eutectic solvent by using succinonitrile and lithium bis (trifluoromethanesulfonyl imide).

[0024] 6) The Li / / P-0.8-FEC / / LFP button cell assembled with the ternary eutectic solid electrolyte of the present invention exhibits excellent stability in multiple charge and discharge cycles and can be stably cycled 500 times under 1C conditions.

[0025] 7) The ternary eutectic solid electrolyte of the present invention is assembled into a soft-pack battery of eutectic solid electrolyte, and the battery exhibits stable cycle performance under 1C conditions.

[0026] 8) The soft-pack battery assembled with the ternary eutectic solid electrolyte of the present invention has undergone rigorous safety tests, demonstrating its excellent safety and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The process flow chart of preparing a ternary eutectic solid electrolyte in one embodiment of the present invention; Figure 2 This is a flame retardant test data diagram of the ternary eutectic solid electrolyte prepared in Example 1 of the present invention; Figure 3 This is a graph showing the thermal stability test data of the ternary eutectic solid electrolyte prepared in Example 2 of the present invention; Figure 4 Long cycle performance diagram of Li / / P-0.8-FEC / / LFP button cell assembled with ternary eutectic solid electrolyte prepared in Example 3 of the present invention; Figure 5 The cycle performance diagram of the Gr / / P-0.8-FEC / / LFP soft-pack battery assembled with the ternary eutectic solid electrolyte prepared in Example 5 of the present invention; Figure 6 Safety performance test diagram of the Gr / / P-0.8-FEC / / LFP soft-pack battery assembled with the ternary eutectic solid electrolyte prepared in Example 5. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0029] The methods used in the following examples, unless otherwise specified, are all conventional methods, carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.

[0030] The purity of LiTFSI in the following examples is ≥99.99%.

[0031] The purity of N,N-dimethylformamide in the following examples is ≥99.9%.

[0032] Example 1: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow chart shown is used to prepare a ternary eutectic solid electrolyte, and the specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0033] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) was uniformly mixed with 0.2 ml of fluoroethylene carbonate and stirred at room temperature for 1 h to obtain a ternary eutectic solvent.

[0034] (3) Preparation of solid electrolyte substrate solution: 0.523 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.021 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0035] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0036] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0037] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.647 mm thick solid electrolyte membrane.

[0038] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0039] Example 2: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow chart shown is used to prepare a ternary eutectic solid electrolyte, and the specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0040] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0041] (3) Preparation of solid electrolyte substrate solution: 0.511 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.014 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0042] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0043] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0044] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.747 mm thick solid electrolyte membrane.

[0045] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0046] Example 3: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow chart shown is used to prepare a ternary eutectic solid electrolyte, and the specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0047] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0048] (3) Preparation of solid electrolyte substrate solution: 0.506 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.021 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0049] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0050] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0051] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.671 mm thick solid electrolyte membrane.

[0052] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0053] Example 4: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow chart shown is used to prepare a ternary eutectic solid electrolyte, and the specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0054] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0055] (3) Preparation of solid electrolyte substrate solution: 0.532 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.033 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0056] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0057] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0058] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.731 mm thick solid electrolyte membrane.

[0059] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0060] Example 5: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow chart shown is used to prepare a ternary eutectic solid electrolyte, and the specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0061] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0062] (3) Preparation of solid electrolyte substrate solution: 0.527 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.016 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0063] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0064] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0065] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.691 thick solid electrolyte membrane.

[0066] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0067] Example 6: Preparation of ternary eutectic solid electrolyte and Figure 1 The process flow chart is similar, and the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetyl were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0068] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0069] (3) Preparation of solid electrolyte substrate solution: 0.527 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.052 g of polyacrylonitrile (average molecular weight 149000~151000) were completely dissolved in 3.022 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0070] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0071] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0072] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.741 thick solid electrolyte membrane.

[0073] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0074] Example 7: Preparation of ternary eutectic solid electrolyte and Figure 1 The process flow chart is similar, and the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and succinonitrile were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0075] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0076] (3) Preparation of solid electrolyte substrate solution: 0.517 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.112 g of polyacrylonitrile (average molecular weight 149000~151000) were completely dissolved in 3.024 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0077] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0078] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0079] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.721 thick solid electrolyte membrane.

[0080] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0081] Example 8: Preparation of ternary eutectic solid electrolyte and Figure 1The process flow chart is similar, and the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and succinonitrile were mixed in a glove box at a molar ratio of 1:3 and magnetically stirred at room temperature to obtain a deep eutectic solvent, which was then stored in a glove box.

[0082] (2) Preparation of ternary eutectic solvent: 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.2 ml of fluoroethylene carbonate were uniformly stirred and mixed to obtain a ternary eutectic solvent.

[0083] (3) Preparation of solid electrolyte substrate solution: 0.527 g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.051 g of polyacrylonitrile (average molecular weight 149000~151000) were completely dissolved in 3.012 g of organic solvent N,N-dimethylformamide to obtain a solid electrolyte substrate solution.

[0084] (4) Preparation of ternary eutectic polymer solution: All the solid electrolyte substrate solution obtained in step (3) and 0.8 ml of ternary eutectic solvent obtained in step (2) are uniformly mixed and stirred for 1 hour to obtain a ternary eutectic polymer solution.

[0085] (5) Solution casting: The solid electrolyte substrate solution obtained in step (4) is transferred to an ultrasonic oscillator and ultrasonicated for 0.5 h to eliminate a large number of bubbles in the solution. Then, the solution is slowly aspirated using a pipette, and the generation of bubbles is avoided as much as possible. The solution is evenly cast in an appropriate amount into a polytetrafluoroethylene mold.

[0086] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold was transferred to a 50°C drying oven and dried for 6 hours. It was then transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.718 thick solid electrolyte membrane.

[0087] (7) Storing the solid electrolyte: Transfer the dried solid electrolyte to a water-free and oxygen-free glove box while it is still hot. Then use rubber tweezers to peel off the film and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0088] Comparative Example 1 The method used in this comparative example is similar to that in Example 1, except that in step (1), LiTFSI and N-methylacetamide are mixed in a molar ratio of 1:3 and magnetically stirred at room temperature to obtain a deep eutectic solvent.

[0089] Comparative Example 2 The method used in this comparative example is similar to that in Example 1, except that in step (2), the ternary eutectic solvent is prepared by uniformly stirring and mixing 0.8 ml of the deep eutectic solvent obtained in step (1) and 0.4 ml of fluoroethylene carbonate.

[0090] Comparative Example 3 The method used in this comparative example is similar to that in Example 1, except that in step (3), the solid electrolyte substrate solution is prepared by completely dissolving poly(vinylidene fluoride-co-hexafluoropropylene) having a molecular weight of 50,000 using 3.006 g of organic solvent N,N-dimethylformamide.

[0091] Comparative Example 4 The method used in this comparative example is similar to that used in Example 1, except that in step (4), the ternary eutectic polymer solution is prepared by uniformly mixing all the solid electrolyte substrate solution obtained in step (3) with 0.6 ml of the ternary eutectic solvent and stirring uniformly for 1 hour.

[0092] Comparative Example 5 The method used in this comparative example is similar to that in Example 1, except that in the solution casting of step (5), the solid electrolyte substrate solution obtained in step (4) is not subjected to ultrasound, and the solution is sucked by a pipette and cast in a proper amount into a polytetrafluoroethylene mold.

[0093] Comparative Example 6 The method used in this comparative example is similar to that used in Example 1, except that in step (6) solid electrolyte molding, the cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 2 hours, and then transferred to a 60°C vacuum drying oven and vacuum dried for 2 hours.

[0094] Test Example 1. Flame retardant properties The test method is as follows: the ternary eutectic solid electrolyte obtained in Example 1 is burned with an open flame, and after the ternary eutectic solid electrolyte is ignited, the time required for it to self-extinguish is recorded.

[0095] Test results such as Figure 2 It can be seen that the ternary eutectic solid electrolyte of the present invention extinguishes naturally 0.3s after being ignited, indicating that the ternary eutectic solid electrolyte has good self-extinguishing property and excellent safety after being ignited by an open flame.

[0096] 2. Thermal stability The test method is as follows: The ternary eutectic solid electrolyte in Example 2 was subjected to thermogravimetric and DSC analysis, PVDF-HFP represents a single poly(vinylidene fluoride-co-hexafluoropropylene), P-0.8 represents a ternary eutectic solid electrolyte prepared by adding only 0.8 ml of a deep eutectic solvent, and P-0.8-FEC represents the ternary eutectic solid electrolyte in Example 2. The three samples showed stability at 120°C. However, the deep eutectic solvent showed significant weight loss at 120°C, 300°C, and 450°C, indicating the decomposition of residual water, deep eutectic solvent, and poly(vinylidene fluoride-co-hexafluoropropylene), respectively. This may be due to the effect of the deep eutectic solvent on the structure of poly(vinylidene fluoride-co-hexafluoropropylene). The collapse of the poly(vinylidene fluoride-co-hexafluoropropylene) structure during the decomposition of the deep eutectic solvent may lead to a decrease in the decomposition temperature. Figure 3 It is shown in Figure 2 that the glass transition temperature (Tg) of P-0.8-FEC decreased from 147°C to 142°C after the addition of fluoroethylene carbonate, indicating that its crystallinity decreased. However, the addition of fluoroethylene carbonate did not significantly affect the melting temperature (Tm), indicating that the deep eutectic solvent established a stable structure with poly(vinylidene fluoride-co-hexafluoropropylene).

[0097] 3. Battery Performance 1. Button battery The solid electrolyte prepared in the above Examples 1-8 and Comparative Examples 1-6 was assembled into a Li / / P-0.8-FEC / / LFP button cell (CR2032) (positive electrode material: lithium iron phosphate; negative electrode material: lithium metal; solid electrolyte: ternary eutectic solid electrolyte). The discharge specific capacity and capacity retention rate of the button cell at 25 degrees Celsius and 1C were tested.

[0098] The experimental results are shown in Table 1.

[0099] The discharge specific capacity and capacity retention rate of the solid electrolyte assembled Li / / P-0.8-FEC / / LFP button cells prepared in Examples 1-8 under 1C conditions are shown in Table 1, and the long cycle diagram of the solid electrolyte assembled Li / / P-0.8-FEC / / LFP button cells in Example 3 is shown in Figure 4 .

[0100] Table 1. Battery material properties of various examples and comparative examples

[0101] As can be seen from Table 1, the button cell assembled with the solid electrolyte in Example 1 has a discharge capacity of 139.7 mAh g after 500 cycles. -1The capacity retention rate is 97.7%; the button cell assembled with solid electrolyte in Example 2 has a discharge capacity of 140.1 mAh g after 500 cycles. -1 The capacity retention rate is 98.8%; the button cell assembled with solid electrolyte in Example 3 has a discharge capacity of 138.7 mAh g after 500 cycles. -1 The capacity retention rate is 97.9%; the button cell assembled with solid electrolyte in Example 4 has a discharge capacity of 139.9 mAh g after 500 cycles. -1 The capacity retention rate is 98.3%; the button cell assembled with solid electrolyte in Example 6 has a discharge capacity of 126.3 mAh g after 500 cycles. -1 The capacity retention rate is 96.2%. The button cell assembled with the solid electrolyte in Example 7 has a discharge capacity of 121.3 mAh g after 500 cycles. -1 The capacity retention rate is 97.2%. Example 8: Button cell assembled with solid electrolyte, long cycle 500 cycles discharge capacity is 118.7 mAh g -1 The capacity retention rate is 96.5%. It can be seen that the Li / / solid electrolyte / / LFP button battery assembled with the solid electrolyte prepared by the ternary eutectic solvent of the present invention can be stably cycled under 1C conditions, with a maximum capacity of 140.1 mAh g -1 The discharge specific capacity and capacity retention rate of 98.8% have good charge and discharge performance.

[0102] From the comparison results of Example 1 and Comparative Example 1, it can be seen that different deep eutectic solvent ratios have different ionic conductivities, which will affect the final cycle performance of the lithium battery.

[0103] From the comparison results of Example 1 and Comparative Example 2, it can be seen that an appropriate amount of accompanying ethyl carbonate is more conducive to the transmission of ions and the formation of a stable SEI layer, thereby improving its cycle performance. However, more fluoroethylene carbonate will cause side reactions, affecting the decomposition of lithium salts, resulting in a decrease in the cycle performance of the battery.

[0104] From the comparison results of Example 1 and Comparative Example 3, it can be seen that the degree of polymerization of the PVDF-HFP substrate will affect the ion transport efficiency of the polymer electrolyte and the mechanical properties after film formation, and will affect the final cycle performance of the lithium battery.

[0105] From the comparison results of Example 1 and Comparative Example 4, it can be seen that different amounts of ternary deep eutectic solvent directly affect the ion conductivity and ion transfer efficiency, which will affect the final cycle performance of the lithium battery.

[0106] From the comparison results of Example 1 and Comparative Example 5, it can be seen that the solution without ultrasound has very fine bubbles, which are generated during volatilization and film formation, affecting the mechanical properties of the electrolyte and the battery cycle performance.

[0107] It can be seen from the comparison results of Example 1 and Comparative Example 6 that the drying temperature and drying time after casting will also affect the cycle performance of the lithium battery.

[0108] 2. Soft pack battery The ternary eutectic solid electrolyte prepared in Example 5 is assembled into a 1-layer soft-pack battery of Gr / / P-0.8-FEC / / LFP (positive electrode material: lithium iron phosphate, negative electrode material: pre-lithiation graphite, solid electrolyte: ternary eutectic solid electrolyte) soft-pack battery assembly: the prepared lithium iron phosphate and graphite electrodes are used as the positive and negative electrodes, respectively, and the ternary eutectic solid electrolyte is placed in the middle. Then the stacked batteries are placed in an aluminum-plastic film battery casing, and the batteries are vacuum-sealed using a soft-pack side sealer.

[0109] The discharge specific capacity and capacity retention rate of the soft pack battery at room temperature and 1C condition were tested. The long cycle diagram of the soft pack battery at 1C condition is shown in Figure 5 It can be seen that the eutectic solid electrolyte soft-pack battery assembled with the ternary eutectic solid electrolyte of the present invention exhibits stable cycling performance under 1C conditions.

[0110] The safety performance of the soft pack battery was tested. The test steps were as follows: The ternary eutectic solid electrolyte prepared in Example 5 was assembled into a 1-layer soft pack battery of Gr / / P-0.8-FEC / / LFP. After the assembly was completed, a puncture test was performed. Puncture test: The puncture test was performed at room temperature using the puncture mode of the MSK-TE905 test instrument. The puncture duration was 1 second, the puncture position was 32 mm, and the puncture diameter was 0.25 cm. The voltage change during the puncture test is shown in Figure 6 The results show that at the moment of puncture, the battery voltage will drop sharply, but it will not cause a complete short circuit. After the puncture process is over, the battery voltage can still return to the original voltage level before the puncture. In addition, the soft-pack battery will not experience thermal runaway before and after the puncture, which is a very safe phenomenon. It can be seen that the eutectic solid electrolyte soft-pack battery assembled with the ternary eutectic solid electrolyte of the present invention has excellent safety and stability.

[0111] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, can implement the present invention in a wider range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principle of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departing from the disclosed scope in the application and the changes made with conventional techniques known in the art.

Claims

1. A method for preparing a ternary eutectic solid electrolyte, characterized in that: The steps include: S1, mixing a hydrogen bond acceptor and a hydrogen bond donor containing lithium ions to obtain a deep eutectic solvent; S2, mixing the deep eutectic solvent and the modifier to obtain a ternary eutectic solvent; The modifier includes one or more of ethylene carbonate, vinylene carbonate, and fluoroethylene carbonate; S3, dissolving the polymer in an organic solvent to obtain a polymer solution; The polymer includes one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyethylene glycol diacrylate, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate; S4, uniformly mixing the ternary eutectic solvent and the polymer solution to obtain a ternary eutectic polymer solution; S5. Drying and molding the ternary eutectic polymer solution to obtain the ternary eutectic solid electrolyte.

2. The method for preparing a ternary eutectic solid electrolyte according to claim 1, characterized in that: The hydrogen bond acceptor containing lithium ions includes any one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonylimide), lithium bis(fluorosulfonylimide), lithium perchlorate, lithium nitrate, lithium chloride and lithium difluorophosphate; The hydrogen bond donor includes any one of N-methylacetamide, acetamide, butanamide, propionamide, N,N-dimethylpropylene urea, methyl pyruvate dimethyl sulfone, ethylene carbonate, succinonitrile and 2,2'-dithiodipyridine; The molar ratio of the hydrogen bond acceptor containing lithium ions to the hydrogen bond donor is 1:(2-6).

3. The method for preparing a ternary eutectic solid electrolyte according to any one of claims 1 to 2, characterized in that: The volume ratio of the deep eutectic solvent to the modifier is (3-6):

1.

4. The method for preparing a ternary eutectic solid electrolyte according to any one of claims 1 to 3, characterized in that: The number average molecular weight of the polymer is 100,000 to 1,000,000; The mass ratio of the polymer to the organic solvent is 1:(4-6).

5. The method for preparing a ternary eutectic solid electrolyte according to any one of claims 1 to 4, characterized in that: The mass ratio of the ternary eutectic solvent to the polymer solution is 1:(2-5).

6. The method for preparing a ternary eutectic solid electrolyte according to any one of claims 1 to 5, characterized in that: The method further comprises the following step before the drying and molding: ultrasonically treating the ternary eutectic polymer solution to remove bubbles in the solution.

7. The method for preparing a ternary eutectic solid electrolyte according to any one of claims 1 to 6, characterized in that: The drying and molding steps are as follows: pouring the ternary eutectic polymer solution into a mold for drying; preferably, the drying process is first drying at 40 to 60 degrees Celsius for 2 to 5 hours, and then vacuum drying at 60 to 80 degrees Celsius for 4 to 6 hours.

8. The ternary eutectic solid electrolyte obtained by the preparation method according to any one of claims 1 to 7.

9. A solid-state lithium battery, characterized in that: It comprises a positive electrode, a negative electrode and the ternary eutectic solid electrolyte as claimed in claim 8.

10. The solid-state lithium battery according to claim 9, characterized in that: The solid-state lithium battery is a button cell or a soft pack cell.

Citation Information

Cited By

  • Flame-retardant eutectic polymer electrolyte based on in-situ polymerization, preparation method and solid-state lithium battery

    CN119650835A

  • Porous composite polymer solid electrolyte, preparation method thereof and solid sodium ion battery

    CN120221781A

  • A porous composite polymer solid-state electrolyte, a preparation method thereof, and a solid-state sodium ion battery

    CN120221781B

  • Sulfonyl deep eutectic gel electrolyte and preparation method and application thereof