Positive electrode binder and application thereof in lithium battery positive electrode
By using rubber and plastic composite materials as the positive electrode adhesive in lithium batteries, combining the synergistic effect of rubber and plastic phases, the problems of low bonding performance and high cost in the prior art are solved, and the stability and conductance of the battery are improved , achieving environmentally friendly low-cost solutions.
Patent Information
- Application Number
- CN202410808792.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-21
AI Technical Summary
The existing positive electrode adhesives have problems such as low bonding performance, poor flexibility and high cost in lithium batteries, and cannot effectively meet the electrochemical performance and cycle life requirements of the battery.
Rubber-plastic composite materials are used as the positive electrode adhesive, including rubber phase and plastic phase. The rubber phase provides excellent flexibility and bonding properties. The plastic phase has high stability and ion transport capability, and improves flexibility and bonding through synergistic effects. Junction performance and chemical stability reduce costs.
It has achieved the improvement of the stability of the positive electrode structure and specific capacity of the battery in lithium batteries, enhanced ionic conductivity, reduced product costs, and has the characteristics of environmentally friendly water-based adhesives.
Smart Images

Figure CN118894967A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and more specifically, to a positive electrode binder and application thereof in a positive electrode of a lithium battery. Background Art
[0002] In lithium-ion batteries, binders are mainly used to ensure that the active material particles, active particles and conductive agents, and active particles and current collectors have a certain bonding strength during the use of the battery, and play a role in maintaining the integrity of the electrode during charging and discharging. As an indispensable component of electrode materials, although the binder is used in small amounts, it has an important impact on the electrochemical performance of the battery.
[0003] Considering the requirements of battery electrochemical performance and long cycle life, binders usually need to have the following requirements: (1) Good bonding performance, able to stably bond the active material to the current collector. (2) Good flexibility; able to evenly disperse the active material and the conductive agent to form a stable conductive network. (3) Good chemical stability and electrochemical stability, not participating in the reaction during battery operation; small swelling coefficient in the electrolyte. (4) Environmentally friendly and low cost.
[0004] Polyvinylidene fluoride (PVDF) is currently the most commonly used positive electrode binder. Although PVDF has good electrochemical stability and can show excellent cycle stability, its application in different active materials still has different defects. Because it does not have functional functional groups, it cannot play the role of adsorbing lithium ions and conducting electrons, and there is only a weak van der Waals force between it and the electrode material, so it cannot have strong adhesion performance.
[0005] By introducing a second or third monomer for copolymerization during the synthesis process, the modulus and crystallinity of PVDF can be significantly reduced, and its adhesion can be improved; for example, patent CN112072108A discloses a conductive binder for lithium batteries and a preparation method thereof, wherein 2-acrylamide-2-methylpropanesulfonic acid (AMPS) is grafted copolymerized onto polyvinylidene fluoride (PVDF) by free radical polymerization to prepare PVDF-g-PAMPS copolymer, and amorphous polymethyl methacrylate (PMMA) is introduced by blending to prepare PVDF-g-PAMPS / PMMA blend. The prepared PVDF-g-PAMPS / PMMA blend binder has electrical conductivity, high adhesion and excellent thermal stability, which can reduce the amount of binder and conductive agent in the slurry, and improve the energy density and cycle life of the battery cell. However, the related process is more difficult and the product cost is high, which limits the commercial application of PVDF copolymers.
[0006] Rubber-plastic composite materials have been widely studied and gradually applied to commercial battery products due to their advantages such as good flexibility, environmental optimization, and low price. For example, styrene-butadiene rubber (SBR) is an elastomer made by copolymerization of 1,3-butadiene and styrene. Its emulsion has good elasticity and strong anti-reduction ability when used as a binder, and is widely used as a negative electrode binder for lithium-ion batteries; in a lithium-ion battery in patent CN114094165A, its negative electrode binder is a polymer with hydroxyl groups in the side chain, which is conducive to forming a stable SEI interface on the surface of the silicon-based negative electrode. However, the above-mentioned SBR and other rubber-plastic composite materials can only be used as negative electrode binders. Due to the weak antioxidant ability of rubber-plastic composite materials, they cannot be used as positive electrode binders. Summary of the invention
[0007] The purpose of the present invention is to overcome the defects and shortcomings of the existing positive electrode binder, such as low bonding performance, poor flexibility and high cost, and to provide an application of a rubber-plastic composite material in the preparation of a positive electrode binder.
[0008] Another object of the present invention is to provide a positive electrode binder.
[0009] Another object of the present invention is to provide a positive electrode sheet comprising the positive electrode binder.
[0010] Another object of the present invention is to provide a lithium battery comprising the above-mentioned positive electrode sheet.
[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0012] The present invention protects the use of a rubber-plastic composite material in the preparation of a positive electrode binder, wherein the structural formula of the rubber-plastic composite material is RuM x , wherein Ru is the rubber phase, M is the plastic phase, and x is the mass fraction of the plastic phase;
[0013] The plastic phase is selected from polymethacrylic acid or its ester derivatives;
[0014] The x is 1-99%.
[0015] A rubber-plastic composite material of the present invention can be used in a positive electrode binder, and has a rubber phase and a plastic phase. The rubber phase has excellent flexibility and bonding properties, has good adhesion to active materials and current collectors, does not cause active materials to fall off, can prevent volume changes during charging and discharging, and ensure the stability of the positive electrode structure during charging and discharging; when the plastic phase is selected from polymethacrylic acid or its ester derivatives, it has high stability to the lithium electrode, and at the same time there are polar groups, and the carbonyl C=O and the oxygen atoms in the ether group COC in the structure can be complexed with active substances such as lithium salts, have ion transport capabilities, and have higher ion conductivity, which is conducive to improving the specific capacity of the battery; through the synergistic effect of the rubber phase and the plastic phase, the flexibility, bonding properties and chemical stability of the rubber-plastic composite material are improved, and the antioxidant capacity is strong. In addition, the rubber-plastic composite material of the present invention is a water-based binder, which has the characteristics of being environmentally friendly and low cost.
[0016] In some embodiments, x is 20-60%, more preferably 25-55%, and further preferably 28-32% or 45-50%. Increasing the content of the rubber phase is beneficial to improving the flexibility and wear resistance of the polymer, while increasing the content of the plastic phase can improve the hardness and chemical stability of the rubber-plastic composite material; by optimizing the mass fraction of the plastic phase, a rubber-plastic composite material with both good flexibility and good chemical stability can be obtained.
[0017] In some embodiments, the rubber-plastic composite material is a graft copolymer formed by grafting reaction of rubber phase and plastic phase monomers.
[0018] In some embodiments, the rubber phase is natural rubber and / or cis-polyisoprene.
[0019] In some embodiments, the monomer component of the cis-polyisoprene is isoprene (2-methyl-1,3-butadiene).
[0020] In some embodiments, the molecular formula of the plastic phase monomer is CH2=C(CH3)COO-R;
[0021] The R is selected from hydrogen, C1-C6 alkyl or C1-C6 alkyl derivatives, wherein one or more hydrogen atoms in the C1-C6 alkyl are replaced by hydroxyl, carboxyl, ester or epoxy groups.
[0022] In some embodiments, the R is selected from methyl, ethyl, butyl, hydroxyethyl or glycidyl.
[0023] The invention protects a positive electrode binder, which comprises the rubber-plastic composite material.
[0024] In some embodiments, the positive electrode binder is a graft copolymer of natural rubber (NR) and methyl methacrylate (PMMA).
[0025] Preferably, the rubber phase is natural rubber, the plastic phase is polymethyl methacrylate, the mass fraction of the plastic phase is 30%, abbreviated as MG30; the ionic conductivity is 2.6×10 -11 S / cm.
[0026] Preferably, the rubber phase is natural rubber, the plastic phase is polymethyl methacrylate, the mass fraction of the plastic phase is 49%, abbreviated as MG49; the ionic conductivity is 1.7×10 -11 S / cm.
[0027] Compared with MG49, MG30 has better flexibility and bonding properties due to its higher NR content, and higher ionic conductivity, which is more conducive to ion transport when used as a binder.
[0028] The invention protects a positive electrode sheet, comprising the positive electrode binder, active material, conductive agent and current collector.
[0029] In some embodiments, the active material is selected from any one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, ternary nickel cobalt manganese or sulfur.
[0030] In some embodiments, the conductive agent is any one or more of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene.
[0031] In some embodiments, the mass ratio of the active material, the conductive agent and the binder is (6-9): (0.5-2): (0.5-2). Preferably, the mass ratio is (7-9): (0.5-2): 1; more preferably, the mass ratio is 8:1:1.
[0032] In some embodiments, the method for preparing the positive electrode sheet comprises the following steps: after the active material, conductive agent and binder are uniformly mixed in an organic solvent, a solution coating process is used to form a layer on the surface of the current collector to obtain the positive electrode sheet.
[0033] Preferably, the organic solvent is any one or two or more of tetrahydrofuran, acetonitrile, acetone, toluene, benzene or chloroform.
[0034] Preferably, the solution coating process is any one or more of blade coating, slit coating, spin coating, dip coating and spray coating.
[0035] Preferably, the method for preparing the positive electrode sheet comprises the following steps:
[0036] (1) dissolving the binder in an organic solvent and stirring until the binder is completely dissolved to form a uniform dispersion;
[0037] (2) mixing the conductive agent and the active material in proportion and grinding them uniformly, adding them to the above dispersion, and stirring them uniformly to prepare a positive electrode slurry;
[0038] (3) The positive electrode slurry is coated on the positive electrode current collector by using a solution coating process to form a micron-sized positive electrode film, which is then dried to obtain a positive electrode sheet.
[0039] Preferably, the drying is to transfer the material to a vacuum oven and dry it at 60-80° C. for 12-24 hours.
[0040] The present invention protects a lithium battery, comprising the positive electrode sheet, the negative electrode sheet, a diaphragm spaced between the positive electrode sheet and the negative electrode sheet, and an electrolyte.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The present invention provides a rubber-plastic composite material that can be used in a positive electrode binder. The rubber phase has a rubber phase and a plastic phase. The rubber phase has excellent flexibility and bonding properties, good adhesion to active materials and current collectors, and no active materials fall off. The volume change can be prevented during the charge and discharge process to ensure the stability of the positive electrode structure during the charge and discharge process. When the plastic phase is selected from polymethacrylic acid or its ester derivatives, it has high stability to the lithium electrode, and polar groups are present. The carbonyl C=O and the oxygen atoms in the ether group COC in the structure can be complexed with active substances such as lithium salts, and have ion transport capacity, higher ion conductivity, and are conducive to improving the specific capacity of the battery. Through the synergistic effect of the rubber phase and the plastic phase, the flexibility, bonding performance and chemical stability of the rubber-plastic composite material are improved, and the antioxidant capacity is strong. In addition, the rubber-plastic composite material of the present invention is a water-based binder, which has the characteristics of being environmentally friendly and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 Graph showing the battery performance test results of the LFP positive electrode sheets of Example 1 and Comparative Example 1.
[0044] Figure 2 This is a graph showing the battery performance test results of the LFP positive electrode sheet of Example 4.
[0045] Figure 3 This is a graph showing the battery performance test results of the NCM811 positive electrode sheets of Example 2 and Comparative Example 2.
[0046] Figure 4 This is a graph showing the battery performance test results of the S positive electrode sheets of Example 3 and Comparative Example 3.
[0047] Figure 5The figure shows the mechanical properties test results of the LFP positive electrode sheets of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0048] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0049] The raw materials in the following examples and comparative examples are:
[0050] Natural rubber and methyl methacrylate graft copolymer 1:MG30, sourced from Jiangsu Qixiang High-tech Materials Co., Ltd.
[0051] Natural rubber and methyl methacrylate graft copolymer 2: MG49, sourced from Jiangsu Qixiang High-tech Materials Co., Ltd.
[0052] Lithium iron phosphate (LFP), type D-3, from CROUD Corporation.
[0053] Lithium nickel cobalt manganese oxide (NCM811), single crystal, comes from CROUD Corporation.
[0054] Elemental sulfur (S) was sourced from Shanghai Suishi Company.
[0055] Example 1
[0056] A method for preparing a positive electrode sheet comprises the following steps:
[0057] (1) Weigh 0.03 g of MG30, add 1.3 mL of tetrahydrofuran solvent and stir for 30 h to form a uniform dispersion.
[0058] (2) Weigh 0.24 g of LFP and 0.03 g of conductive carbon black, mix and grind for 25 min; add the mixture to the above dispersion and continue stirring for 30 h to obtain a positive electrode slurry.
[0059] (3) The positive electrode slurry is uniformly coated on the surface of the aluminum foil; and the positive electrode is dried at 70° C. for 18 hours to obtain a positive electrode sheet.
[0060] Example 2
[0061] A method for preparing a positive electrode sheet is different from that of Example 1 in that the active material in this embodiment uses NCM811 to replace the LFP in Example 1.
[0062] Example 3
[0063] A method for preparing a positive electrode sheet is different from that of Example 1 in that the active material in this embodiment uses S to replace the LFP in Example 1.
[0064] Example 4
[0065] A method for preparing a positive electrode sheet is different from that of Example 1 in that the binder in this embodiment uses MG49 to replace the MG30 in Example 1.
[0066] Example 5
[0067] A method for preparing a lithium battery comprises the following steps:
[0068] (1) The positive electrode sheet of Example 1 was cut into discs with a diameter of 12 mm.
[0069] (2) In a glove box, the wafer was assembled with a lithium metal negative electrode (diameter 16 mm), a polypropylene (PP) separator, an organic electrolyte, and a CR2025 button battery case to form a battery, wherein the organic electrolyte was 1 M lithium salt dissolved in a solvent of 1,3-dioxolane and dimethyl ether in a volume ratio of 1:1.
[0070] Comparative Example 1
[0071] A method for preparing a positive electrode sheet comprises the following steps:
[0072] (1) LFP, conductive carbon black and PVDF were mixed in N-methylpyrrolidone in a mass ratio of 8:1:1 and stirred evenly to prepare a positive electrode slurry.
[0073] (2) The positive electrode slurry is uniformly coated on the surface of the aluminum foil; and the foil is dried at 70° C. for 18 hours to obtain a positive electrode sheet.
[0074] Comparative Example 2
[0075] A method for preparing a positive electrode sheet, which is different from Comparative Example 1 in that: the active material in this embodiment uses NCM811 to replace the LFP in Comparative Example 1.
[0076] Comparative Example 3
[0077] A method for preparing a positive electrode sheet, which is different from Comparative Example 1 in that the active material in this embodiment uses S to replace the LFP in Comparative Example 1.
[0078] Performance Testing
[0079] 1. Electrochemical and battery performance testing
[0080] The positive electrode sheets of Examples 1-4 and Comparative Examples 1-3 were cut into discs with a diameter of 12 mm. The discs were assembled into batteries in a glove box with a lithium metal negative electrode (diameter 16 mm), a polypropylene (PP) separator, an organic electrolyte (1 M lithium salt dissolved in a solvent of 1,3-dioxolane and dimethyl ether in a volume ratio of 1:1) and a CR2025 button battery shell; then, the assembled batteries were subjected to electrochemical and battery performance tests.
[0081] The test method is: test on Wuhan Blue Electric test system, LFP positive electrode sheet is tested in the voltage range of 2.4~4.0V, NCM811 positive electrode sheet is tested in the voltage range of 2.8~4.2V, S positive electrode sheet is tested in the voltage range of 1.7~2.8V. The test results are as follows Figure 1-4 shown.
[0082] Reference Figure 1-2 When the active material is LFP, MG30 binder, MG49 binder and PVDF binder all have higher specific capacity, and there is no obvious decrease within 20 cycles, and the cycle stability is high; and the specific capacity of MG30 binder and MG49 binder is slightly higher than that of PVDF binder in Comparative Example 1.
[0083] Reference Figure 3 When the active material is NCM811, compared with the comparative example 2 using the PVDF binder, the example 2 using the MG30 binder has a higher specific capacity.
[0084] Reference Figure 4 When the active material is S, compared with the comparative example 3 using the PVDF binder, the embodiment 3 using the MG30 binder has a higher specific capacity.
[0085] The results show that when the active material is LFP, NCM811 or S, the present invention uses MG30 as the positive electrode binder to have a higher specific capacity; among them, when the active material is NCM811 or S, the improvement of the specific capacity of the MG30 positive electrode binder is particularly significant.
[0086] 2. Mechanical properties test
[0087] Take the positive electrode sheets of Example 1 and Comparative Example 1, stick 3M tape on the side of the positive electrode coated with active material to perform a 180° peel strength test, the results are as follows: Figure 5 shown.
[0088] The results show that when the active material is LFP, compared with the comparative example 1 using the PVDF binder, the example 1 using the MG30 binder has higher peel strength and better adhesion.
[0089] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. Application of a rubber-plastic composite material in the preparation of a positive electrode binder, characterized in that: The structural formula of the rubber-plastic composite material is RuM x , wherein Ru is the rubber phase, M is the plastic phase, and x is the mass fraction of the plastic phase; The plastic phase is selected from polymethacrylic acid or its ester derivatives; The x is 1-99%.
2. The use according to claim 1, characterized in that: The rubber-plastic composite material is a graft copolymer formed by grafting reaction of rubber phase and plastic phase monomers.
3. The use according to claim 1 or 2, characterized in that: The rubber phase is natural rubber and / or cis-polyisoprene.
4. The use according to claim 2, characterized in that: The molecular formula of the plastic phase monomer is CH2=C(CH3)COO-R; The R is selected from hydrogen, C1-C6 alkyl or C1-C6 alkyl derivatives, wherein one or more hydrogen atoms in the C1-C6 alkyl are replaced by hydroxyl, carboxyl, ester or epoxy groups.
5. The use according to claim 4, characterized in that: The R is selected from methyl, ethyl, butyl, hydroxyethyl or glycidyl.
6. A positive electrode binder, characterized in that The present invention relates to a rubber-plastic composite material for use in any one of claims 1 to 5.
7. A positive electrode sheet, characterized in that: It comprises the positive electrode binder, active material, conductive agent and current collector as described in claim 5.
8. The positive electrode sheet according to claim 7, characterized in that: The active material is selected from any one or more of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, ternary nickel cobalt manganese or sulfur.
9. The positive electrode sheet according to claim 7, characterized in that: The mass ratio of the active material, the conductive agent and the binder is (6-9): (0.5-2): (0.5-2).
10. A lithium battery, characterized in that: It comprises the positive electrode sheet and the negative electrode sheet as described in any one of claims 7 to 9, a separator separated between the positive electrode sheet and the negative electrode sheet, and an electrolyte.
Citation Information
Patent Citations
Long-durability glued diaphragm, preparation method thereof and lithium ion battery comprising long-durability glued diaphragm
CN114171850A
All-solid-state polymer electrolyte interface modification method and application of all-solid-state polymer electrolyte interface modification method in secondary ion battery
CN118017043A
Positive electrode manufacture method for lithium ion polymer battery
KR1020000001828A
Cited By
Lithium ion secondary battery, preparation method thereof and electric device
CN119133458A
Lithium ion secondary battery and preparation method thereof, and power-using device
CN119133458B
Lithium ion secondary battery and electric device
CN119133459A
Lithium-ion secondary battery and electric apparatus
WO2026103089A1