Large-scale synthesis of powders of solid electrolyte material particles for solid-state batteries, systems and methods
The method addresses inefficiencies in solid electrolyte production by using digitally controlled stoichiometric amounts and dynamic crystallization to produce high-quality solid electrolyte materials for solid-state batteries, enhancing large-scale manufacturing efficiency and safety.
Patent Information
- Application Number
- JP2024523869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-24
- Filing Date
- 2022-11-25
- Publication Date
- 2024-12-03
AI Technical Summary
Conventional methods for producing solid electrolyte materials for solid-state batteries are inefficient, costly, and unsuitable for large-scale production due to lengthy processes, complex operations, and difficulty in achieving intimate solid-to-solid contact, leading to high energy density and safety issues.
A method involving digitally controlled stoichiometric amounts of lithium-containing salts and other metals, forming a gas-liquid mixture, which is then processed through a power jet chamber to create a gas-solid mixture, followed by dynamic crystallization and annealing to produce high-quality solid electrolyte materials.
This method enables the production of high-power, high-capacity, and thermally stable solid electrolyte materials suitable for large-scale manufacturing, with improved safety and efficiency, using a process that ensures precise atomic ratios and uniform crystallization.
Smart Images

Figure 2024544475000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 283,214, filed November 25, 2021, which is incorporated by reference herein in its entirety.
[0002] The present invention relates generally to compositions, processes, and systems for the large-scale synthesis and production of battery materials, including powders of electrolyte, anode or cathode active material particles for rechargeable lithium-ion and solid-state batteries. [Background technology]
[0003] In the clean energy industry (e.g., electric vehicle batteries), there is a constant demand for lightweight, compact, and high energy density batteries, and significant improvements in battery safety, energy density, cycle life, large-scale production, and low cost are constantly being sought. In general, conventional lithium-ion batteries (LIBs) contain a non-aqueous electrolyte, which is a liquid-based electrolyte with lithium salts in a flammable organic solvent. However, the use of liquid-based electrolytes has drawbacks, such as serious safety issues due to flammability and the presence of volatile organic solvents used in the electrolyte; short circuit problems, especially at high rate charge-discharge cycles, due to the inevitable growth of Li dendrites in LIB liquid electrolytes; capacity loss, leakage, electrode leakage and / or corrosion due to highly resistive solid electrolyte interfaces (SEIs) at the electrodes, limited use of high voltage cathode materials due to electrolysis at high voltages, and generation of hydrogen fluoride (HF) during thermal runaway.
[0004] Solid-state batteries offer the possibility of large battery cells, especially for electric vehicle applications: solid-state batteries for powering electric vehicles are lighter and require less space than lithium-ion batteries, since solid-state systems do not require any cooling systems.
[0005] In general, there are various synthesis methods for solid electrolyte materials, such as pulsed laser deposition, RF magnetron sputtering, solid pyrolysis synthesis, sol-gel, combustion synthesis, ball milling, electrospinning, molten salt, spark plasma sintering route, atomic layer deposition, etc. However, all of these methods require a long time to obtain the final product (too many manufacturing steps), cannot provide large quantities of products (e.g., in tons, not grams or kilograms), and cannot achieve and maintain intimate solid-to-solid contact, making them very expensive and uneconomical for large-scale production. Therefore, it is desirable to develop new manufacturing methods for large-scale synthesis and production of solid battery materials for solid-state secondary batteries with high energy density and excellent safety performance. Summary of the Invention [Problem to be solved by the invention]
[0006] Most of the conventional processes for producing solid electrolyte materials include many steps, such as mixing, adding excess lithium to make up for the lithium lost during the high-temperature sintering process, and many of the steps cannot be continuously carried out in a large-scale production line.Moreover, most of the conventional processes have the disadvantages of being static in nature, high sintering energy cost, long cycle life, short chamber life, complicated operation steps, low production efficiency, uneven heating, and difficult to control cooling time, so that the resulting battery materials are overheated or underheated.
[0007] Thus, there is a significant need for improved methods and systems for large-scale production of solid-state battery materials, especially well-crystallized solid electrolyte materials, to obtain high power battery performance, high capacity, high energy density, long cycle life, and excellent thermal stability. [Means for solving the problem]
[0008]
[0013] Embodiments of the present invention generally provide solid-state battery materials, methods and systems for producing the solid-state battery materials. One embodiment of the present invention provides a method for producing a solid-state electrolyte (SSE) material, the method comprising: N forming a gas-liquid mixture; injecting a mist of the liquid mixture at a high output velocity into a power jet chamber; and delivering a second gas stream of the heated gas into the power jet chamber. N Examples of the elements include La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof.
[0009] The method also includes drying the gas-liquid mixture for a first reaction time of less than 20 minutes to undergo one or more oxidation reactions in the presence of a second gas flow to form a gas-solid mixture, delivering the gas-solid mixture from a power jet chamber, separating the gas-solid mixture into one or more solid particles of the SSE material, and delivering the one or more solid particles to an annealing chamber. In one example, the first reaction time is less than 3 minutes. In another example, the powder particles are annealed in a dynamic crystallization process in the presence of an oxygen gas flow.
[0010] The method then further comprises annealing one or more solid particles of the SSE material for a second reaction time of greater than two hours and subjecting the one or more solid particles of the SSE material to a dynamic crystallization process in the presence of a third gas flow to obtain a crystalline product. The method optionally comprises grinding the crystalline product of the ceramic material to obtain nano-sized particles.
[0011] In one embodiment, the method also includes further processing the ceramic material by sintering the crystalline product of the ceramic material at an annealing temperature of 900° C. or greater, and measuring the ionic conductivity of the ceramic material.
[0012] An example of a ceramic SSE material is Li7La3Zr2O 12 , Li7La3Zr2O doped with one or more metals 12 or the following formula 1 and combinations thereof.
[0013] [ka]
[0014] In one embodiment, the crystalline product of the SSE material is in the form of spherical clusters under scanning electron microscope (SEM) analysis. In another embodiment, the tap density of the SSE material is greater than 1.0 g / ml. For example, after annealing the SSE material at a temperature greater than 900° C. for 8 hours or more, the tap density of the SSE material is greater than 1.4 g / ml.
[0015] In yet another embodiment, the ionic conductivity (σ) of the SSE material is greater than or equal to 10 at 25° C. -4S / centimeter. One example of the crystalline product is a garnet-type ceramic material having a cubic crystal structure as measured by X-ray diffraction (XRD) analysis. In another example, the liquid mixture includes a lithium-containing salt, a lanthanum-containing salt, and a zirconium-containing salt, and the crystalline product of the SSE material is a garnet-type ceramic material having a cubic crystal structure as measured by XRD analysis. In yet another example, the liquid mixture includes a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and an aluminum-containing salt, and the crystalline product of the SSE material is a garnet-type ceramic material having a cubic crystal structure as measured by XRD analysis. Another example of the liquid mixture includes a lithium-containing salt, a lanthanum-containing salt, and a zirconium-containing salt, and the crystalline product of the SSE material is a garnet-type ceramic material having a tetragonal crystal structure as measured by XRD analysis.
[0016] In yet another embodiment, the liquid mixture includes a lithium-containing salt, a lanthanum-containing salt, and a tantalum-containing salt, and the crystalline product of the SSE material is a garnet-type ceramic material having a cubic crystal structure as determined by XRD analysis. Another example of a liquid mixture includes a lithium-containing salt, an aluminum-containing salt, and a phosphorus-containing salt, and the crystalline product of the SSE material is a sodium superionic conductor (NASICON)-type ceramic material having a hexagonal crystal structure as determined by XRD analysis.
[0017] In a further embodiment, the liquid mixture includes a lithium-containing salt, a lanthanum-containing salt, and a titanium-containing salt, and the crystalline product of the SSE material is a perovskite ceramic material. Additionally, the liquid mixture includes a lithium-containing salt, a germanium-containing salt, and the SSE material is a ceramic material. In a further embodiment, the liquid mixture includes a lithium-containing salt, a sulfur-containing salt, and the SSE material is a sulfide material.
[0018] One embodiment of the present invention is a 10 -4 S / cm and has a measured ionic conductivity (σ) greater than Li aLa b Zr c D1 d D2 e、··· DN n O v wherein 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D1, D2, ..., D N At least one of the metals D1, D2, ..., D3 is a metal, and N > 0, 0 < d < 0.8, 0 < e < 0.8, and 0 < n < 0.8. The method includes the step of: mixing digitally controlled stoichiometric amounts of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and one or more metals D1, D2, ..., D N and mixing it with a first gas stream to form a gas-liquid mixture, and spraying the mist of the liquid-mixture into a power jet chamber; drying the gas-liquid mixture for a first reaction time of less than 20 minutes and undergoing one or more oxidation reactions in the presence of a second gas stream of heated gas to form a gas-solid mixture. The gas-solid mixture is then discharged from the power jet chamber, and the gas-solid mixture is separated into one or more solid particles of the SSE material. The one or more solid particles are then fed into an annealing chamber, and the one or more solid particles of the SSE material are annealed for a second reaction time of more than two hours and undergo a dynamic crystallization process in the presence of a third gas stream, thereby resulting in a final crystalline product of the SSE material.
[0019] Another embodiment of the present invention is Li a La b Zr c D1 d D2 e ...DN n O v wherein 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D1, D2, ..., D Nat least one of is a metal, N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8. The SSE material is synthesized on a large scale by a method that includes forming a liquid mixture of digitally controlled stoichiometric amounts of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and one or more inorganic salts that include one or more metals. The method also includes mixing the liquid mixture with a first gas stream to form a gas-liquid mixture; spraying a mist of the gas-liquid mixture at high velocity into a power jet chamber; drying the gas-liquid mixture for a first reaction time of less than 20 minutes by pumping a second gas stream of heated gas to undergo one or more oxidation reactions to form a gas-solid mixture inside the power jet chamber; delivering the gas-solid mixture from the power jet chamber to obtain powder particles of a ceramic material; annealing the powder particles for a second reaction time of more than 2 hours to undergo a dynamic crystallization process in the presence of a third gas stream to form a crystalline product, where the crystalline product of the ceramic material is cluster-like under SEM analysis, where D1, D2, ..., D N is selected from the group consisting of Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof.
[0020] In one example, the method for producing the solid electrolyte material of the present invention further comprises grinding the crystalline product of the ceramic material to obtain nano-sized particles, and the tap density of the ceramic material is greater than 1.0 g / ml. In another example, the method further comprises sintering the crystalline product of the ceramic material at an annealing temperature of 900° C. or greater to further process the ceramic material, and measuring the ionic conductivity of the ceramic material. In yet another example, the crystalline product of the solid electrolyte material obtained from the present invention is a garnet-type ceramic material having a cubic crystal structure as measured by XRD analysis, and its measured ionic conductivity (σ) is greater than 10 at 25° C. -4 Greater than S / centimeters.
[0021] Another embodiment of the present invention is Li a La b Zr c Al d D1 e ....DN n O v wherein 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D1, ..., D N at least one of which is a metal, N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8; and wherein digitally controlled stoichiometric amounts of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and one or more metals D1, D2, ..., D are synthesized by a method comprising: N forming a liquid mixture of one or more inorganic salts comprising: a) a first inorganic salt comprising: b) a first inorganic salt comprising: c) a first inorganic salt comprising: d) a first inorganic salt comprising: b) a second inorganic salt comprising: d) a first inorganic salt comprising: b) a second inorganic salt comprising: d) a first inorganic salt comprising: b) a second inorganic salt comprising: d) a first inorganic salt comprising: b) a second inorganic salt comprising: d) a first inorganic salt comprising: b) a second inorganic salt comprising:
[0022] In another embodiment, the solid electrolyte material is synthesized by a process including: digitally controlled stoichiometric amounts of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and one or more metals D1, D2, ..., D Nforming a liquid mixture of one or more inorganic salts comprising: a) a lithium-containing salt, a lanthanum-containing salt, and a zirconium-containing salt; b) a mist of the liquid mixture being mixed with a first gas stream to form a gas-liquid mixture; c) a lithium-containing salt, a lanthanum-containing salt, and a zirconium-containing salt being dried together for a first reaction time of less than 20 minutes and subjected to one or more oxidation reactions by pumping a second gas stream of heated gas to form powder particles of a ceramic material; d) a powder particle that is annealed for a second reaction time of more than 2 hours and subjected to a dynamic crystallization process in the presence of a third gas stream to form a crystalline product of the ceramic material, wherein the final crystalline product of the ceramic material is cluster-like under SEM analysis, and the crystalline product is a garnet-type ceramic material having a cubic crystal structure as measured by XRD analysis, and the measured ionic conductivity (σ) is greater than or equal to 10 at 25° C. -4 Greater than S / cm.
[0023] Various solid electrolyte materials that can be formed using the method of the present invention include, but are not limited to, ceramic solid electrolyte materials, garnet-type solid oxide electrolyte materials, lithium lanthanum zirconium oxide materials, Li6ALa3Ta2O12 (A=Sr, Ba), NASICON (NaM2(PO4)3M=Ge, Ti, Zr), synthesis of LLTO perovskite-type structure electrolytes and transport properties of two-dimensional LixM1 / 3Nb1-xTixO3 (M=La, Nd) perovskite (ABO3)-type oxides, Li superionic conductor (LISICON)-type structure oxide electrolytes, lithium phosphorus oxynitride (LiPON), and combinations thereof. In addition, argyrodite electrolytes, lithium phosphorus sulfide (Li3PS4, LPS) electrolytes, Li7P3S 11 Solid sulfide electrolyte materials such as Li7P2S8, Li11-xM2-xP1+xS12 (M=Ge, Sn, Si) (LGPS) type structures: LGPS and combinations thereof can be synthesized and formed using the methods of the present invention.
[0024] The present invention also provides a method of fabricating a solid-state battery by forming an anode material layer, forming a solid electrolyte material layer, and forming a cathode material layer, where one or more of the anode material layer, the solid electrolyte material layer, the cathode material layer, or a combination thereof comprises a material prepared by the method of the present invention. The material formed by the method of the present invention can be a ceramic solid electrolyte material, a garnet-type solid oxide electrolyte material, a lithium lanthanum zirconium oxide material, Li6ALa3Ta2O12 (A=Sr, Ba), NASICON (NaM2(PO4)3M=Ge, Ti, Zr), synthesis of LLTO perovskite-type structure electrolyte and transport properties of two-dimensional LixM1 / 3Nb1-xTixO3 (M=La, Nd) perovskite (ABO3)-type oxide, Li superionic conductor (LISICON)-type structure oxide electrolyte, lithium phosphorus oxynitride (LiPON), and combinations thereof. In addition, Argyrodite electrolyte, Lithium Phosphide Sulfide (Li3PS4, LPS) electrolyte, Li7P3S 11 , Li7P2S8, Li11-xM2-xP1+xS12 (M=Ge, Sn, Si) (LGPS) type structure LGPS and combinations thereof.
[0025] As one example, the material formed by the method of the present invention can be used as a material in a solid electrolyte material layer. As another example, the material formed by the method of the present invention can be used as a material to coat a cathode material (e.g., using a dry coating process and / or a wet coating process). The resulting solid electrolyte material-coated cathode material can be used to form a cathode material layer. Such coated cathode materials can be used to fabricate solid-state batteries together with conventional solid electrolyte materials or using solid electrolyte materials formed by the method of the present invention.
[0026] In one embodiment, a solid electrolyte material comprising lithium (Li) and one or more metals is synthesized by forming a liquid mixture of a stoichiometric amount of a lithium-containing salt and one or more metal-containing salts, injecting the liquid mixture into a power jet reactor for the lithium-containing salt and one or more metal-containing salts to oxidize and rapidly react together at high temperatures between 350° C. and 1200° C. for just a few minutes to form a final reaction product of the solid electrolyte material.
[0027] An example of a solid electrolyte material is lithium lanthanum zirconium oxide (Li7La3Zr2O 12 ) (LLZO) materials. The LLZO solid material is obtained by forming a liquid mixture of a molar ratio amount of a lithium-containing salt (e.g., lithium nitrate (La(NO3)3), lanthanum nitrate (La(NO3)3)) and one or more metal-containing salts, and injecting the liquid mixture into a power jet reactor to react the lithium-containing salt and one or more metal-containing salts together for less than 30 minutes to rapidly react and form a final reaction product of a solid electrolyte material. The resulting solid electrolyte material exhibits a crystal structure comparable to that of solid electrolyte materials prepared by conventional solid-state reaction and / or reactive gelation processes.
[0028] So that the above-mentioned features of the invention may be understood in detail, a more particular description of the invention briefly summarized above can be made by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings depict only typical embodiments of the invention and are therefore not to be considered as limiting the scope of the invention, which may admit of other embodiments that are equally effective. [Brief description of the drawings]
[0029] [Figure 1A] FIG. 1 is a cross-sectional view of an exemplary solid-state battery according to one embodiment of the present invention. [Figure 1B] FIG. 2 is a cross-sectional view of an exemplary solid-state battery according to another embodiment. [Figure 1C]FIG. 2 is a cross-sectional view of an exemplary solid-state battery according to another embodiment. [Figure 1D] FIG. 2 is a cross-sectional view of an exemplary solid-state battery according to another embodiment. [Diagram 2] 1 illustrates one embodiment of a method for manufacturing a battery material. [Diagram 3] 1 is another embodiment of a method for producing a battery material. [Figure 4] 1 illustrates another embodiment of a method for wet coating a battery material with another material. [Diagram 5] 1 illustrates another embodiment of a method for dry coating a battery material with another material. [Figure 6] FIG. 1 is a schematic diagram of an exemplary processing system useful for preparing materials for a battery electrochemical cell according to one embodiment of the present invention. [Figure 7] 2 is a schematic diagram of another exemplary processing system according to another embodiment. [Figure 8A] FIG. 1 illustrates a perspective view of one embodiment of a processing system for producing particulate material for batteries. [Figure 8B] 1 illustrates a cross-sectional view of another embodiment of a processing system for producing particulate material. [Figure 8C] FIG. 1 illustrates a perspective view of another embodiment of an exemplary power jet module configured within a dispersion chamber of a processing system. [Figure 8D] FIG. 2 illustrates a perspective view of an exemplary power jet module configured in a processing system according to another embodiment. [Figure 8E] FIG. 1 illustrates a perspective view of an exemplary power jet module according to another embodiment. [Figure 8F] FIG. 1 illustrates a perspective view of an exemplary power jet module configured within a processing system. [Figure 9] 1 shows X-ray diffraction (XRD) patterns of examples of crystallized solid electrolyte materials of the present invention. [Figure 10] 1 shows XRD patterns of examples of crystallized solid electrolyte materials of the present invention. [Figure 11] 1 is an XRD pattern of an example of a crystallized solid electrolyte material of the present invention. [Figure 12] 1 is an XRD pattern of another exemplary crystallized solid electrolyte material of the present invention. [Figure 13] 1 is an XRD pattern of another exemplary crystallized solid electrolyte material of the present invention. [Figure 14A] 1 is a SEM image of an exemplary solid particle of a solid electrolyte material after one or more annealing processes. [Figure 14B] 1 is a SEM image of an exemplary solid particle of a solid electrolyte material. [Figure 14C] 1 is a SEM image of an exemplary solid particle of a solid electrolyte material. [Figure 15A] 1 is a SEM image of an exemplary solid particle of a solid electrolyte material. [Figure 15B] 15B is a magnified SEM image of the exemplary solid electrolyte material particle of FIG. 15A. [Figure 16A] 1 is a SEM image of an exemplary solid electrolyte material particle. [Figure 16B] 16B is a magnified SEM image of the exemplary solid electrolyte material particle of FIG. 16A. [Figure 17A] 1 is a SEM image of an exemplary solid electrolyte material particle after one or more annealing processes. [Figure 17B] 1 is a SEM image of another example of solid electrolyte material particles. [Figure 17C] 1 is a SEM image of an exemplary solid electrolyte material particle. [Figure 17D] 1 is a SEM image of an exemplary solid electrolyte material particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present invention generally relates to compositions, battery oxide materials, battery SSE materials, apparatus, and their dynamic crystallization process (DCP) in appropriate molar solution ratios to precisely and digitally control the metal material content to stoichiometric amounts and obtain the proper atomic-level ratios of metal components and configurations of battery active materials for use in solid-state batteries. The battery materials and methods and apparatus provided herein result in highly pure and precisely stoichiometric phase battery cathode materials that can be used to fabricate lithium-ion batteries with properties associated with high battery cycling performance, including high electrical capacity.
[0031] A solid-state battery generally comprises a positive electrolyte, a negative electrolyte, and a solid electrolyte / separator (i.e., the solid electrolyte can act as a separator between the positive electrolyte (i.e., cathode) and the negative electrolyte (i.e., anode)). The positive electrode generally comprises a positive active material (i.e., cathode material), and the negative electrode comprises a negative active material (i.e., anode material). The SSE in the solid-state battery can be a simple solid electrolyte material or a composite of a polymer and an SSE material. The cathode material can be LiCoO2 (LCO), Li(NixMnyCoz)O2 (NMC), LiFePO4 (LFP), or LiMn2O4 (LMO), and in some cases intercalated binary oxides, while the anode material can be Li metal, Li-ln alloys, graphite, Li4Ti5O12 (LTO), or Si, Sn-Co-C mixed composites. Furthermore, the electrode fabrication techniques for solid-state batteries are different from those for conventional lithium-ion batteries.
[0032] 1A illustrates an exemplary solid-state battery showing an exemplary layer structure of a solid-state battery layer structure 10A according to one embodiment of the present invention. The solid-state battery layer structure 10A includes a positive electrode layer 90A, a negative electrode layer 30A, and a solid electrolyte layer 50A sandwiched between the positive electrode layer 90A and the negative electrode layer 30A.
[0033] In one embodiment, the solid electrolyte layer 50A includes a solid electrolyte material 52A that can be fabricated using the methods and systems of the invention described below in Figures 2, 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or another suitable process according to one or more embodiments. In another embodiment, the positive electrode layer 90A includes a cathode active material 92A that can be fabricated using the methods and systems of the invention described below in Figures 2, 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or another suitable process according to one or more embodiments. Additionally, the negative electrode layer 30A includes an anode material 32A that can be fabricated using any suitable anode material fabrication process and system.
[0034] FIG. 1B illustrates another example of a solid-state battery layer structure 10B according to an aspect of the present invention. The solid-state battery layer structure 10B includes a cathode layer 90B, an anode layer 30B, and a solid electrolyte layer 50B sandwiched between the cathode layer 90B and the anode layer 30B. In one embodiment, the solid electrolyte layer 50B includes a solid electrolyte material 52B made using the methods and systems of the present invention described below in FIGS. 2, 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or another suitable process according to one or more embodiments. Additionally, the anode layer 30B includes an anode material 32B therein, and the solid electrolyte layer 50B includes a solid electrolyte material 52B made according to the methods and systems of the present invention.
[0035] In another embodiment, the positive electrode layer 90B includes a mixture of the cathode active material 92B and the solid electrolyte material 94B made according to the methods and systems of the present invention. The cathode active material 92B and the solid electrolyte material 94B can be mixed together by blending methods using a blender or any other suitable equipment. It is contemplated that the solid electrolyte material 94B is included in the positive electrode layer 90B to aid in the electrical conductivity of the cathode active material 92B in the solid battery layer structure 10B.
[0036] 1C illustrates an exemplary solid-state battery according to one aspect of the present invention, a solid-state battery layer structure 10C. The solid-state battery layer structure 10C includes a cathode layer 90C having a cathode active material 92C coated therein, an anode layer 30C having an anode material 32C therein, and a solid electrolyte layer 50C sandwiched between the cathode layer 90C and the anode layer 30C. In one embodiment, the solid electrolyte layer 50C includes a solid electrolyte material 52C made using the methods and systems of the present invention described below in FIGS. 2, 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or another suitable process according to one or more embodiments.
[0037] In another embodiment, the coated cathode active material 92C is made according to one or more embodiments of the present invention and includes particles of cathode active material 96C (e.g., a battery cathode material made using the methods and systems of the present invention, or any other suitable battery cathode material) coated with an outer layer of solid electrolyte material 94C (e.g., a battery SSE material made using the methods and systems of the present invention, or any other suitable battery SSE material). Coating the particles of cathode active material 96C with solid electrolyte material 94C is performed using the methods and systems described below in Figures 4 and 5, or another suitable dry or wet coating process. It is contemplated that blending the solid electrolyte material 94C with the particles of cathode active material 96C in the coated cathode active material 92C helps promote electrical conductivity in the solid battery layer structure 10C.
[0038] 1D illustrates another example of a solid-state battery layer structure 10D that includes a positive electrode layer 90D, a negative electrode layer 30C having an anode material 32D therein, and a solid electrolyte layer 50D sandwiched between the positive electrode layer 90D and the negative electrode layer 30D. The solid electrolyte layer 50D includes a solid electrolyte material 52D made using the methods and systems of the invention described below in FIGS. 2, 3, 6, 7, 8A, 8B, 8C, 8D, 8E, 8F, or another suitable process according to one or more embodiments.
[0039] In one embodiment, the positive electrode layer 90D includes a mixture of a coated cathode active material 92D and a solid electrolyte material 98D, which are mixed by blending using a blender or any other suitable device. In another embodiment, the coated cathode active material 92D is made using the methods and systems described herein in accordance with one or more embodiments of the present invention. For example, the coated cathode active material 92D can include particles of a cathode active material 96D coated with an outer layer of a solid electrolyte material 94D (e.g., a battery SSE material made using the methods and systems of the present invention, or any other suitable battery SSE material). Coating the particles of the cathode active material 96D with the solid electrolyte material 94D is performed using the methods and systems described below in Figures 4 and 5, or another suitable dry coating or wet coating process.
[0040] 1A to 1D, the thicknesses of the positive electrode layer, the solid electrolyte layer, and the negative electrode layer in the solid battery layer structure are not particularly limited. For example, the solid battery layer structures 10A, 10B, 10C, and 10D may include one or more solid electrolyte layers (e.g., 2 to 3 or 10 SSE layers) sandwiched between the positive electrode layer 90A, 90B, 90C, and 90D and the negative electrode layer 30A, 30B, 30C, and 30D.
[0041]
[0023] Embodiments of the present invention provide that the solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, 98D, and the cathode active materials 92A, 92B, 96C, 96D can be made using the methods and systems of the present invention described below, or another suitable process, and these materials can be used to fabricate and synthesize solid-state batteries. Further embodiments for making the solid electrolyte materials or cathode active materials are described in U.S. Patent Application Nos. 13 / 900,915, 16 / 114,114, 16 / 747,450, 17 / 319,974, 17 / 319,974, 17 / 901,796, 13 / 901,035, 17 / 319,974 ... No. 16 / 104,841, U.S. Patent Application No. 17 / 133,478, U.S. Patent Application No. 17 / 970,342, U.S. Patent Application No. 13 / 901,121, U.S. Patent Application No. 15 / 846,094, U.S. Patent Application No. 16 / 679,085, and U.S. Patent Application No. 17 / 899,048, the disclosures of each of the foregoing patent applications are incorporated herein by reference in their entirety.
[0042] In one embodiment, the solid electrolyte material in a solid-state battery according to an aspect of the present invention includes solid electrolyte layers 50A, 50B, 50C, 50D including solid electrolyte materials 52A, 52B, 52C, 52D. In another embodiment, the cathode layer in a solid-state battery may further include both a cathode active material and a solid electrolyte material mixed with the cathode active material by a direct blending process, a dry coating process, or a wet coating process.
[0043] In another embodiment, examples of the solid electrolyte material (e.g., solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, 98D shown in FIGS. 1A-1D) include, but are not limited to, oxide-based solid electrolytes, garnet-type solid electrolytes, sodium superionic conductor (NASICON)-type (NaM2(PO4)3M=Ge, Ti, Zr) structures (e.g., lithium aluminum titanium phosphate oxide materials, Li(Al,Ti)2(PO4), LATP, e.g., Li 1.5Al 0.5 Ti 1.5 P3O 12 , Li 1.4 Al 0.4 Ti 1.6 P3O 12 , Li 1.6 Al 0.6 Ti 1.4 P3O 12 etc.), Perovskite-type solid electrolytes (e.g., Li x La y TiO3, LLTO, etc.), 2D Li x M 1 / 3 Nb 1-x Ti x Transport properties of O3 (M = La, Nd) perovskite (ABO3) type oxides, Li 1.5 Al 0.5 Ge 1.5 P3O 12 , Li 1.4 Al 0.4 Ge 1.6 P3O 12 , Li 1.6 Ge 0.6 Ti 1.4 P3O 12 , Li 12 Ge 0.5 Al 1.0 S 0.5 P 1.0 O 12 , Li 10.59 Ge 1.58 V 0.9 P 0.53 O 12 , sulfide SSE electrolyte materials (e.g., Li7P3S 11 , Li3P1S4, Li6P1S5Cl, Li6P1S5Br1, Li6P1S5l, Li6P1S5F1, Li7P2S8l1, Li7P2S8Br1, Li7P2S8Cl1, Li7P2S8F1, Li 15 P4S 16 Cl3, Li 14.8 Mg 0.1 P4S 16 Cl3, Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 Ge1P2S 12, Li 10 Si1P2S 12 , Li 10 Sn1P2S 12 , Li 10 S 0.3 Sn 0.7 P2S 12 , Li 10 Al 0.3 Sn 0.7 P2S 12 , Li 11 Al1P2S 12 , Li 10 SiP2S 11.3 O 0.7 , Li 9.42 S 1.02 P 2.1 S 9.96 O 2.04 etc.), lithium superionic conductor (LISICON) type structure oxide electrolyte, amorphous thin film solid electrolyte (e.g., lithium phosphorus oxynitride (LiPON), Li 2.88 P 1.0 O 3.73 N 0.14 , Li 1.9 S 0.28 P 1.0 O 1.1 N 1.0 etc.), Argyrodite-type solid electrolyte, Lithium phosphorus sulfide (Li3PS4, LPS) solid electrolyte, Li7P3S 11 , Li7P2S8, Li 11-x M 2-x P 1+x S 12 (M = Ge, Sn, Si, etc.) (LGPS) type structure, Li-argyrodite solid electrolyte (e.g., Li x P.S. y X (X=Cl, Br, or l), Li6PS5Cl, Li6PS5Br, Li6PS5l, etc., and combinations thereof.
[0044] The SSE material may be an undoped SSE material or may be doped with one or more metals or other atoms (e.g., La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, P, S, Os, Ir, Au, F, Cl, I, Br, and combinations thereof, etc.), such as lithium oxide-based garnet-type SSE materials doped with Al, Ge, Ti, Ta, etc.
[0045] Examples of the solid electrolyte materials 52A, 52B, 52C, 52D, 94B, 94C, 94D, and 98D shown in FIGS. 1A-1D include, but are not limited to, one or more lithium-containing garnet-type oxide-based solid electrolyte (SSE) materials having a cubic or tetragonal crystal structure, lithium lanthanum zirconium oxide garnet, lithium lanthanum zirconium oxide garnet doped with Al, Ge, Ti, Ta, etc., such as Li7La3Zr2O 12 , Li7La3Zr2O doped with one or more metals 12 , the following formula 2 and combinations thereof:
[0046] [ka]
[0047] In one embodiment, the chemical composition of the solid electrolyte material is Li a La b Zr c D1 d D2 e DN n O v where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D1, D2, ..., D N At least one of D1, D2, ..., D is a metal, N > 0, 0 < d < 0.8, 0 < e < 0.8, and 0 < n < 0.8; N is selected from the group consisting of Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof. For example, the solid electrolyte material may be Li 6.75 La3Zr 1.75 Ta 0.25 O 12 , Li 6.5 La3Zr 1.5 Ta 0.5 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La3Zr2Al 0.25 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La3Zr2Ta 0.25 Ga 0.2 O 12and the like.
[0048] In another embodiment, the solid electrolyte material is Li a La b D1 c D2 d DN n O v where 4.5≦a≦7.2, 2.8≦b≦3.5, 1.5≦c≦2.5, 0≦d≦1.2, 0≦n≦1.2, and 2≦v≦12; and D1, D2, ..., D N At least one of the elements is a metal, and N≧1. For example, the solid electrolyte material is Li5La3Nb2O 12 , Li5La3Ta2O 12 , Li5La3Ti2O 12 , Li6La3Sr1Ta2O 12 , Li6La3Ba1Ta2O 12 , Li6La3Ba1Ti2O 12 , Li 1.26 La 2.24 Ti4O 12 In another example, the chemical composition of the solid electrolyte material may be Li a Al b P c D1 d ...DN n O v where 1≦a≦2, 0.2≦b≦1.5, 1.0≦c≦3.5, 0≦d≦2.0, 0≦n≦2.0, and 0.2≦v≦12; and D1, D2, ..., D N At least one of the groups is a metal, N≧1, for example, Li 1.5 Al 0.5 Ti 1.5 P3O 12 , Li 1.5 Al 0.5 Ge 1.5 P3O 12 It is.
[0049] In another embodiment, the chemical composition of the solid electrolyte material is Li a P b S c D1 d DNn X v where 5≦a≦16, 0.5≦b≦4.5, 3≦c≦16, 0≦d≦1.5, 0≦n≦1.5, 0≦v≦4, and D1, D2, …D N At least one of is a metal, N≧0, and X is a halogen; for example, Li7P3S 11 , Li3P1S4, Li6P1S5Cl, Li6P1S5Br1, Li6P1S5I, Li6P1S5F1, Li7P2S8I1, Li7P2S8Br1, Li7P2S8Cl1, Li7P2S8F1, Li 15 P4S 16 Cl3, Li 14.8 Mg 0.1 P4S 16 Cl3, Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 Ge1P2S 12 , Li 10 Si1P2S 12 , Li 10 Sn1P2S 12 , Li 10 S 0.3 Sn 0.7 P2S 12 , Li 10 Al 0.3 Sn 0.7 P2S 12 , Li 11 Al1P2S 12 In another embodiment, the solid electrolyte material is Li a Ge b P c D1 d... DN n O v where 10≦a≦13, 0.1≦b≦2.0, 0.1≦c≦1.5, 0.1≦d≦2.0, 0.1≦n≦2.0, 2≦v≦12, and D1, D2, ..., D N At least one of is a metal, N≧0, N≧0; for example, Li 12 Ge 0.5 Al 1.0 S 0.55 P 1.0 O 12 , Li10.59 Ge 1.58 V 0.9 P 0.53 O 12 In one embodiment, the lithium ion (Li+) conductivity of the solid electrolyte is 0.01-10 mS / cm at 300 K. The resulting solid electrolyte material can be further processed into a smaller sized powder (e.g., by jet milling and other comminution techniques) to obtain nano-sized particles of the solid electrolyte material.
[0050] In Figures 1A-1D, the cathode active material 92A, 92B, 94C, 94D may be a metal oxide material made using the methods and systems of the present invention described in Figures 2-8F or another suitable process, and may include a lithium oxide material containing an intercalated metal, preferably three or four intercalated metals. Exemplary cathode active materials are metal oxide materials including one or more of lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co), aluminum (Al), titanium (Ti), sodium (Na), potassium (K), rubidium (Rb), vanadium (V), cesium (Cs), copper (Cu), magnesium (Mg), iron (Fe), and the like. Additionally, the cathode material may exhibit a crystalline structure of the metal in the form of layered, spinel, olivine, and the like. Moreover, the cathode active materials 92A, 92B, 94C, 94D are generally solid powders having particle sizes in the range of 10 nm to 100 μm.
[0051] Exemplary cathode active materials include, but are not limited to, lithium transition metal oxides (LiMeO2), lithium titanium oxides (e.g., Li4Ti5O 12), lithium cobalt oxide (e.g., LiCoO2), lithium manganese oxide (e.g., LiMn2O4), lithium nickel oxide (e.g., LiNiO2), olivine-type lithium metal phosphates (e.g., LiFePO4, LiNiPO4, LiCoPO4, LiMnPO4, Li3Fe2(PO4)3, and Li3V2(PO4)3), sodium iron oxide (e.g., NaFe2O3), sodium iron phosphate (e.g., NaFeP2O7), and lithium nickel cobalt oxide (e.g., Li x Ni y Co z O2), lithium nickel manganese oxide (e.g., Li x Ni y Mn z O2, Li x Ni y Mn z O4, LiCoMnO4, Li2NiMn3O8, etc.), lithium nickel manganese cobalt oxide (e.g., Li a Ni b Mn c Co d O e , layered structures or layered-layered structures, and / or LiNi x Mn y Co z O2, NMC oxide materials (where x+y+z=1), e.g., LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.9 Mn 0.05 Co 0.05 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.4 Mn 0.4 Co 0.2 O2, LiNi 0.7 Mn 0.15 Co 0.15 O2, LiNi 0.8 Mn 0.1 Co 0.1O2, and / or mixed metal oxides containing doped metals. Other examples include lithium cobalt aluminum oxide (e.g., Li x Co y Al z O n ), lithium nickel cobalt aluminum oxide (e.g., Li x Ni y Co z Al a O b , for example LiNi 0.85 Co 0.1 Al 0.05 O2), sodium iron manganese oxide (e.g., Na x Fe y Mn z In another example, mixed metal oxides containing doped metals are obtained; for example, Li a (Ni x Mn y Co z )MeO b (Me = Al, Mg, Fe, Ti, Cr, Zr, or C doped metal), Li a (Ni x Mn y Co z )MeO b F c (Me=Al, Mg, Fe, Ti, Cr, Zr, or C doped metals), etc. Other examples of cathode active materials can be found in U.S. Patent Nos. 13 / 900,915, 16 / 114,114, 16 / 747,450, 17 / 319,974, 17 / 319,974, 17 / 901,796, 13 / 901,035, 16 / 104,841, 17 / 133,478, 17 / 970,342, 13 / 901,121, 15 / 846,094, 16 / 679,085, and 17 / 899,048, which are incorporated herein by reference in their entireties.
[0052] 1A-1D, the anode materials 32A, 32B, 32C, 32D can be an alkali metal (e.g., lithium, sodium, potassium, etc.), other metals or transition metals (tantalum, titanium, zinc, iron, elements of Group 2 of the periodic table (e.g., magnesium, calcium, etc.), elements of Group 13 of the periodic table (aluminum (Al), geranium (Ge), etc.), carbonaceous materials, and / or alloys of two or more of the aforementioned metals. Exemplary anode materials include, but are not limited to, lithium metal, lithium alloys (e.g., lithium-aluminum alloys, lithium-tin alloys, lithium-lead alloys, and lithium-silicon alloys), lithium-containing metal oxides (e.g., lithium titanium oxide), lithium-containing metal sulfides, lithium-containing metal nitrides (e.g., lithium cobalt nitride, lithium iron nitride, lithium manganese nitride), and carbonaceous materials such as graphite, lithium titanate (Li4Ti5O 12 ), SiO-based composites, SiO-Sn-Co / graphite (G) composites, Si, Sn-Co-C mixed composites, and lithium coated with solid electrolytes.
[0053] FIG. 2 is a flow chart of a digital dynamic crystallization process of a method 100 of manufacturing a battery material for a solid-state battery. The method 100 includes step 110 of flowing a first gas into a power jet chamber (e.g., the system described in FIGS. 6-8F below) and mixing the first gas with a liquid mixture to form a gas-liquid mixture. In step 120, the gas-liquid mixture is sprayed into a mist in the power jet chamber. The gas flow may be transferred through an air filter to remove any particles, droplets, or contaminants, and the flow rate of the gas may be adjusted by a valve or other means. In one embodiment, the gas is mixed with the mist and heated to a temperature that removes moisture from the mist. The first gas may be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, an inert gas, a noble gas, and combinations thereof, and may be at room temperature or may be heated, for example, to about 40° C. or higher, for example, to about 80° C. or higher, for example, to 20° C. to 200° C., or may be higher than 50° C.
[0054] In one example, the mist of the liquid mixture is mixed with a flow of carrier gas in the mist generator before being fed into the power jet chamber. In another example, the mist of the liquid mixture is mixed with a flow of dry gas in the power jet chamber and conveyed through the power jet chamber to dry. In another example, the mist of the liquid mixture is mixed with a gas flow of gas in the mist generator to form a gas-liquid mixture. Additionally, the liquid mixture is mixed with a gas flow of another gas in the power jet chamber. It is contemplated that these gas flows are provided to thoroughly mix the liquid mixture to form a homogenous mixture and to aid in conveying the gas-liquid mixture into the power jet chamber.
[0055] The liquid mixture contains digitally controlled stoichiometric amounts of a lithium-containing salt, one or more metals D1, D2, ..., D N In one embodiment, D1, D2, ..., D N is selected from the group consisting of La, Zr, Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof. In another embodiment, the lithium-containing salt and one or more salt-containing compounds M LiSalt :M Salt1 :M Salt2 :M Salt3 :...:M SaltN The molar ratios of LiSalt:Salt1:Salt2:Salt3...:SaltN are adjusted to a ratio of about a:b:c:...:n to produce battery materials with a desired atomic ratio of LiSalt:Salt1:Salt2:Salt3...:SaltN equal to a:b:c:...:n. In one embodiment, a liquid mixture is made using stoichiometric amounts of the lithium-containing salt and one or more inorganic salts and then mixed with the gas. The salts are prepared in solution and the molar ratios of the lithium-containing salt and one or more inorganic metal salt solutions are digitally controlled by the processing system of the present invention, thereby obtaining large scale synthesis of SSE materials.
[0056] The mist of the liquid mixture is mixed with a first gas stream to form a gas-liquid mixture before and / or after the liquid mixture enters the power jet chamber. The mist is formed from the liquid mixture dissolved and / or dispersed in a suitable liquid solvent. The mist stream is mixed with one or more gas streams to form a gas-liquid mixture. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gases, noble gases, and combinations thereof. The gas can be passed through an air filter to remove any particles, droplets, or contaminants, and the flow rate of the gas can be adjusted by a valve or other means.
[0057] For example, M LiSalt :M Salt1 :M Salt2 :M Salt3 :...M SaltN The desired molar ratio of can be achieved by measuring and preparing appropriate amounts of the lithium-containing salt (LiSalt), the first salt-containing salt (Salt1), the second salt-containing salt (Salt2), the third salt-containing salt (Salt3), ..., and the N-containing salt (SaltN) depending on the final composition of the SSE to be synthesized. For example, the M of the lithium-containing salt (LiSalt), the first salt-containing salt (Salt1), the second salt-containing salt (Salt2), the third salt-containing salt (Salt3), and the N-containing salt (SaltN) can be LiSalt :M Salt1 :M Salt2 :M Salt3 :...M SaltN The molar ratio of may be adjusted and prepared (e.g., manually or digitally using the processing system of the present invention) directly into the liquid mixture at a desired stoichiometric ratio prior to forming the mist of the liquid mixture. As another example, the molar ratio of M of lithium-containing salt (LiSalt), first salt-containing salt (Salt1), second salt-containing salt (Salt2), third salt-containing salt (Salt3), and N salt-containing salt (SaltN) may be adjusted and prepared (e.g., manually or digitally using the processing system of the present invention) directly into the liquid mixture at a desired stoichiometric ratio prior to forming the mist of the liquid mixture. Li :M Salt1 :M Salt2 :M Salt3 :...M SaltNThe adjustment of the molar ratio of can be performed simultaneously with the formation of the mist of the liquid mixture. Additionally, the liquid form of one or more salt-containing compounds can be adjusted and prepared directly into the liquid mixture at the desired concentration.
[0058] The liquid form of the salt-containing compound can be dissolved or dispersed in a suitable solvent (e.g., water, alcohol, methanol, isopropyl alcohol, isopropanol, organic solvent, inorganic solvent, organic acid, sulfuric acid (H2SO4), citric acid (C6H8O7), acetic acid (CH3COOH), butyric acid (C4H8O2), lactic acid (C3H6O3), nitric acid (HNO3), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone, and combinations thereof) to form a liquid mixture in the form of an aqueous solution, a slurry, a gel, an aerosol, or any other suitable liquid form. Also, a suitable salt-containing compound can be selected according to the desired composition of the final solid product particles by weighing and preparing an appropriate amount of the lithium-containing salt and the inorganic salt compound together with a suitable amount of the solvent into a container. Depending on the solubility of the lithium-containing salt, the inorganic salt in the selected solvent, the pH, temperature, and mechanical stirring and mixing can be adjusted to obtain a liquid mixture in which the lithium-containing salt, one or more metal-containing inorganic salts at the desired molar concentration are completely dissolved and / or uniformly dispersed.
[0059] Exemplary lithium-containing salts include, but are not limited to, lithium sulfate (Li2SO4), lithium nitrate (LiNO3), lithium carbonate (Li2CO3), lithium acetate (LiCH3COO), lithium hydroxide (LiOH), lithium formate (LiCHO2), lithium chloride (LiCl), and combinations thereof. Exemplary inorganic salts include, but are not limited to, lithium sulfate (LiSO), lithium nitrate (LiNO), lithium carbonate (LiCO), lithium acetate (LiCHCOO), lithium hydroxide (LiOH), lithium formate (LiCHO), lithium chloride (LiCI), lanthanum trichloride (LaCl), lanthanum acetate (CHLaO), and lanthanum nitrate (La(NO)), lanthanum sulfate (La(SO)), lanthanum formate (CHLaO), cobalt sulfate (CoSO), cobalt nitrate (Co(NO)), cobalt acetate (Co(CHCOO)), cobalt formate (Co(CHO)), cobalt chloride (CoCl), magnesium nitrate (Mg(NO)), zirconium nitrate (Zr(NO)), zirconium acetate (CH), 12O8Zr), zirconium chloride (ZrCl4), zirconium sulfate (Zr(SO4)2), zirconium formate (C4H4O8Zr), titanium nitrate (Ti(NO3)4), titanium sulfate (Ti(SO4)2), titanium carbonate (Ti(CO3)2), titanium acetate (Ti(CH3COO)4), titanium hydroxide (Ti(OH)4), titanium formate (Ti(HCOO)4), titanium chloride (TiCl4), ammonium phosphate ((NH4)3PO4), magnesium acetate (MgAc, Mg(CH3COO)2), magnesium chloride (MgCl2), magnesium sulfate (MgS O4), magnesium formate (C2H2MgO4), aluminum nitrate (AI(NO3)3), aluminum acetate (AlAc, C6H9AlO6), aluminum chloride (AlCl3), aluminum sulfate (Al2(SO4)3), aluminum formate (Al(HCOO)3), manganese sulfate (MnSO4), manganese nitrate (Mn(NO3)2), manganese acetate (Mn(CH3COO)2), manganese formate (Mn(CHO2)2), manganese chloride (MnCl2), nickel sulfate (NiSO4), nickel nitrate (Ni(NO3)2), nickel acetate (Ni(CH3C Nickel formate (Ni(CHO2)2), Nickel chloride (NiCl2), Titanium nitrate (TiO(NO3)2), (P)-phosphate containing compounds, Aluminum (Al) containing compounds, Magnesium (Mg) containing compounds, Titanium (Ti) containing compounds, Tantalum (Ta) containing compounds, Sodium (Na) containing compounds, Zirconium (Zr) containing compounds, Germanium (Ge) containing compounds, Tin (Sn) containing compounds, Silicon (Si) containing compounds, Bromine (Br) containing compounds, Iodine (I) containing compounds, Potassium (K) containing compounds, Scandium (Sc) containing compounds compounds, niobium (Nb)-containing compounds, neodymium (Nd)-containing compounds, lanthanum (La)-containing compounds, cerium (Ce)-containing compounds, silicon (Si)-containing compounds, rubidium (Rb)-containing compounds, vanadium (V)-containing compounds, cesium (Cs)-containing compounds, chromium (Cr)-containing compounds, copper (Cu)-containing compounds, magnesium (Mg)-containing compounds, manganese (Mn)-containing compounds, zinc (Zn)-containing compounds, gallium (Ga)-containing compounds, barium (Ba)-containing compounds, actinium (Ac)-containing compounds, calcium (Ca)-containing compounds, iron (Fe)-containing compounds,Examples of the compounds include boron (B)-containing compounds, arsenic (As)-containing compounds, hafnium (Hf)-containing compounds, molybdenum (Mo)-containing compounds, tungsten (W)-containing compounds, rhenium (Re)-containing compounds, ruthenium (Ru)-containing compounds, rhodium (Rh)-containing compounds, platinum (Pt)-containing compounds, silver (Ag)-containing compounds, osmium (Os)-containing compounds, iridium (Ir)-containing compounds, gold (Au)-containing compounds, and combinations thereof.
[0060] Without wishing to be bound by theory, it is contemplated that all of the required inorganic salt elements are first mixed in a liquid phase (e.g., solution, slurry, or gel) using metal-containing salts as the source of each metal element so that the different metals are mixed uniformly in the desired ratio. As an example, one or more dopants with high water solubility can be used to prepare the liquid mixture of the aqueous solution, slurry, or gel. For example, metal nitrates, metal sulfates, metal chlorides, metal acetates, and metal formates can be used. Organic solvents such as alcohol, isopropanol, etc. can be used to dissolve and / or disperse metal-containing salts with low water solubility. In some cases, the pH value of the liquid mixture can be adjusted to increase the solubility of one or more precursor compounds. Optionally, chemical additives, gelling agents, and surfactants such as ammonia, EDTA, etc. can be added to the liquid mixture to aid in dissolving or dispersing the compounds in the selected solvent.
[0061] In one particular embodiment, the method 100 comprises: preparing a lithium-containing salt (LiSalt), a lanthanum-containing salt, a zirconium-containing salt, and optionally one or more metal dopant-containing inorganic salts in a molar ratio M LiSalt :M LaSalt :M ZrSalt :M D1Salt :M D2Salt :...M DNSaltThe method includes a series of steps of preparing a liquid mixture of these salts dissolved in a suitable solvent. Each of the one or more metal salts or metal dopant-containing salts is selected according to the composition of the battery material to be produced. The molar ratio M of the lithium-containing salt (LiSalt), the lanthanum-containing salt, the zirconium-containing salt, and the one or more metal dopant-containing salts is LiSalt :M LaSalt :M ZrSalt :M D1Salt :M D2Salt :...M DNSalt is adjusted to have a ratio of about a:b:c:d:e:...:n, and a lithium oxide doped with one or more dopants (LiaLabZrcD1 d D2 e ....DN n Ov) is now manufactured, where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and N≧0, 0≦d≦0.8, 0≦e≦0.8, ..., 0≦n≦0.8.
[0062] Next, the molar concentration M LiSalt of lithium-containing salt, molar concentration M LaSalt a lanthanum-containing salt, a zirconium-containing salt, and optionally one or more dopant-containing salts (e.g., M D1Salt a first dopant-containing salt having a molar concentration of M D2Salt A second dopant-containing salt having a molar concentration of....:M DNSalt The liquid mixture containing LiaLabZrcD1 d D2 e ....DN n O v The present invention relates to a method for producing a solid electrolyte material, optionally doped with one or more metal dopants, having a target composition of one or more dopant-containing salts, including a first dopant-containing salt, a second dopant-containing salt, ..., an N dopant-containing salt, and wherein the liquid mixture is a mixture ... LiSalt :M LaSalt :M ZrSalt :M D1Salt :M D2Salt:...M DNSalt A molar ratio of about a:b:c:d:.e:..:n is achieved. The mist of liquid mixture can include droplets of various reactant solutions, precursor solutions, etc., with homogenous morphology, size, shape, etc. For example, a molar ratio M of lithium-containing salt, lanthanum-containing salt, zirconium-containing salt, and optionally one or more metal dopant-containing salts is achieved. LiSalt :M LaSalt :M ZrSalt :M D1Salt :M D2Salt :...M DNSalt can be digitally adjusted depending on the desired composition of the final solid product particles. In one embodiment, optionally, one or more dopants (D1, D2, ... DN) are incorporated into the solid electrolyte material, where D1, D2, ... DN are different dopants.
[0063] For example, each of the one or more dopants (i.e., D1, D2, DN) can be selected from the group consisting of Al, Ti, Ta, F, Cl, I, Br, Mg, Mn, Zr, Zn, Nb, La, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, Ge, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, and combinations thereof. Next, the solid particles of the solid electrolyte material are manually or digitally adjusted and prepared in the desired molar ratio and mixed into a liquid mixture. For example, the appropriate amounts of lithium-containing salt compounds, lanthanum-containing salt compounds, zirconium-containing salt compounds, and optionally one or more dopants-dopant-containing salts are adjusted, measured, and prepared into one solution with a suitable amount of solvent.
[0064] The mist of the liquid mixture may be generated by a mist generator, such as a nozzle, a sprayer, an atomizer, or any other mist generator. Most mist generators utilize air pressure or other means to convert the liquid mixture into droplets. The mist generator may be coupled to a portion of the power jet chamber to generate a mist of the liquid mixture (e.g., a large collection of small size droplets) directly within the power jet chamber. As an example, a sprayer may be attached to a portion of the power jet chamber to spray or inject the liquid mixture into a mist containing small droplets directly within the power jet chamber. Generally, a mist generator that generates a mist of single size droplets is desired. Alternatively, the mist may be generated outside the power jet chamber and pumped into the power jet chamber.
[0065] The desired droplet size can be adjusted by adjusting the size of the liquid delivery / injection channel in the mist generator. Droplet sizes ranging from a few nanometers to hundreds of micrometers can be generated. The suitable droplet size can be adjusted depending on the selection of the mist generator used, the precursor compound, the temperature of the power jet chamber, the flow rate of the gas, and the residence time in the power jet chamber. For example, mist with droplet sizes ranging from one tenth of a micron to one millimeter can be generated in the power jet chamber.
[0066] Without wishing to be bound by theory, it is contemplated that in the method 100 of manufacturing a battery material using a lithium-containing salt and one or more dopant-containing salts, the lithium-containing salt, one or more salts, and one or more dopant-containing salts are prepared into a liquid mixture, which is then converted into droplets, and each droplet is uniformly dispersed with one or more liquid mixtures. The liquid mixture is then dehydrated by passing the droplets through a power jet chamber, and a gas flow is used to convey the mist into the power jet chamber for a suitable residence time. It is further contemplated that the concentration of the compounds in the liquid mixture and the droplet size of the mist of the liquid mixture can be adjusted to control the chemical composition, particle size, and size distribution of the final solid product particles of the battery material. The mist of the liquid mixture is sprayed into the power jet chamber to react, and then the method is designed to obtain spherical solid particles from a thoroughly mixed liquid mixture of two or more precursors. In contrast, conventional solid manufacturing processes involve mixing or grinding a solid mixture of precursor compounds, which results in a non-uniform mixture of the precursors.
[0067] As shown in FIG. 2, the method 100 includes a step 130 of drying the gas-liquid mixture for a first reaction time by delivering a second gas stream of heated gas to undergo one or more oxidation reactions, thereby forming a gas-solid mixture in the power jet chamber after high temperature drying and oxidation reactions. The first reaction time can advantageously be performed at a fast rate, such as less than 20 minutes, e.g., less than 10 minutes, less than 5 minutes, or less than 2 minutes. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, noble gas, and combinations thereof, and can be heated to a high temperature, e.g., about 100° C. or higher, e.g., about 200° C. or higher, e.g., 200° C. to 500° C., or higher than 250° C., e.g., 350° C. or higher. The first reaction time is approximately 1 second to 1 hour. Optionally, an additional gas stream can be used to perform the oxidation reaction and / or the drying reaction. The additional gas can be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, noble gas, and combinations thereof. The additional gas flow may be transferred through an air filter to remove any particles, droplets, or contaminants, and the flow rate of the additional gas may be adjusted by a valve or other means. The mist of the liquid mixture is dried (e.g., has its moisture, liquid, etc., removed) at any temperature for a desired residence time and formed into a gas-solid mixture by the flow of gas in the power jet chamber. When the removal of moisture occurs from the mist of the liquid mixture in the gas-filled power jet chamber, a gas-solid mixture containing gas and compounds is formed. For example, the liquid mixture is dried in the power jet chamber, and the temperature in the power jet chamber is maintained by a heating element coupled to the power jet chamber, which may be a suitable heating mechanism such as a wall furnace, an electrically driven heater, a fuel-fired heater, or the like. Furthermore, in one embodiment of the present invention, one or more gases flowing in the power jet chamber are used as a gas source to carry out oxidation reactions, drying, evaporation, dehydration, and / or other reactions in the power jet chamber, thereby drying the gas-liquid mixture into a gas-solid mixture. In another embodiment, the gas is mixed with the mist and heated to a temperature that removes moisture from the mist.
[0068] In one configuration, the gas is preheated to a temperature of about 200° C. or higher before being injected into the power jet chamber. In another configuration, drying of the mist can be performed by directly heating the power jet chamber, such as by heating the chamber body of the power jet chamber. For example, the power jet chamber can be a wall-heated furnace to maintain the temperature in the inner plenum of the power jet chamber. Advantages of using heated gas include fast heat transfer, uniform high temperature, and easy scale-up. The power jet chamber can be any chamber, furnace, such as a domed ceramic power jet chamber, a quartz chamber, a tube chamber, etc. Optionally, the chamber body is made of a thermal insulating material (e.g., ceramic, etc.) to prevent heat loss during the reaction.
[0069] In another embodiment, the gas flowing through the power jet chamber is heated and the thermal energy of the heated gas is provided as an energy source for carrying out reactions, oxidation, drying, evaporation, dehydration, and / or other reactions in the power jet chamber. The gas can be heated to a predetermined temperature by passing it through a suitable heating mechanism such as an electric heater, a fuel-fired heater, etc. The temperature can be 200°C or higher, such as 200°C to 300°C, such as 250°C. For example, the liquid mixture is dried in the power jet chamber in the presence of a second gas heated to 200°C or higher, and the second gas is pumped into the power jet chamber to maintain the temperature in the power jet chamber. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, rare gas, and combinations thereof. For example, heated air can be used as an inexpensive gas and energy source for drying the mist. The gas of choice can be a gas that is mixed with the gas-liquid mixture and heated to a high temperature to dry the gas-liquid mixture without reacting with the compounds. In some cases, chemicals in the droplets / mist may react to some extent with the gas and / or with each other during drying, depending on the temperature and chemical composition of the compound. Furthermore, the residence time of the mist of the thoroughly mixed compound in the power jet chamber can be adjusted, for example, between 1 second and 1 hour, depending on the flow rate of the gas and the length and amount of path the mist needs to travel in the power jet chamber. The gas flow can be transported through an air filter to remove any particles, droplets, or contaminants, and the flow rate of the gas can be adjusted by a valve or other means. Thus, in one embodiment of the present invention, a gas is used as a gas source to carry out reactions, oxidation, drying, evaporation, dehydration, and / or other reactions. In another embodiment, the gas is mixed with the mist and heated to a temperature that removes moisture from the mist. The gas-liquid mixture is dried in the power jet chamber using a heated gas flow at a variable flow rate that is continuous and / or adjustable, resulting in a gas-solid mixture.
[0070] At step 140, the gas-solid mixture is pumped out of the power jet chamber, and at step 150, the dried gas-solid mixture is separated into one or more solid particles of the battery material by a gas-solid separator. For example, the dried gas-solid mixture may be carried by the gas through a passage in the power jet chamber as a thoroughly mixed gas-solid mixture, and as more gas enters, the gas-solid mixture is pumped out of the power jet chamber and continuously pumped into a gas-solid separator connected to the power jet chamber to separate the gas-solid mixture into waste and one or more solid particles of the SSE battery material.
[0071] Next, in step 160, the one or more solid particles of the battery material are fed into an annealing chamber and subjected to a dynamic crystallization process, and in step 170, the one or more solid particles of the battery material are annealed in the presence of a third gas flow for a second reaction time to form and obtain a crystalline product of the battery material for use in a solid-state battery. The second reaction time can be more than 1 hour, more than 2 hours, more than 4 hours, more than 8 hours, or more. Further, steps 150, 160, and 170 can be repeated in the dynamic crystallization process to obtain a better crystalline structure.
[0072] The reaction of one or more solid particles of the battery material in the annealing chamber may include any of oxidation, reduction, decomposition, complex reaction, phase transition, recrystallization, mono-substitution reaction, di-substitution reaction, combustion, isomerization, and combinations thereof. For example, one or more solid particles of the battery material may be oxidized and properly aligned into a crystalline structure. Exemplary third gases include, but are not limited to, air, oxygen, carbon dioxide, oxidizing gas, nitrogen gas, inert gas, noble gas, hydrogen gas, and combinations thereof. For oxidation reactions in the annealing chamber, an oxidizing gas can be used as the annealing gas. If desired, the gas can be oxygen with high purity, the purity of oxygen being greater than 50%, for example greater than 80%, for example 95%. Thus, the gas flow in the annealing chamber is utilized as an energy source for carrying out reactions, oxidations, and / or other reactions in the annealing chamber.
[0073] The annealing temperature can be, for example, 400° C. or higher relative to the residence time for obtaining the battery material. For example, the annealing temperature may be greater than 600° C., greater than 700° C., greater than 800° C., greater than 900° C., greater than 750° C., greater than 850° C., greater than 950° C., greater than 1050° C., greater than 1150° C., etc. The residence time is about 1 second to 30 hours.
[0074] In one embodiment, the gas flowing through the annealing chamber is heated and the thermal energy of the heated gas is utilized as an energy source for carrying out the annealing reaction and / or other reactions in the annealing chamber. The gas can be heated to a temperature of 550°C or higher by passing it through a suitable heating mechanism such as an electric heater, a fuel-fired heater, etc. For example, one or more solid particles of the battery material are annealed in the annealing chamber in the presence of a third gas heated to 550°C or higher, which gas is pumped into the annealing chamber to maintain the annealing temperature in the annealing chamber. The gas can be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, noble gas, and combinations thereof. For example, heated air can be used as an inexpensive gas and energy source for drying the mist. Furthermore, the residence time in the annealing chamber can be adjustable and can be, for example, between 1 second and 1 hour, depending on the flow rate of the gas and the length and volume of the path the solid particles need to pass through in the annealing chamber.
[0075] Another embodiment of the present invention is a method for annealing one or more solid particles of the battery material in an annealing chamber, the temperature of which is maintained by a heating element coupled to the annealing chamber, where the heating element may be a suitable heating mechanism such as a wall furnace, an electrically driven heater, a fuel-fired heater, or the like. In one configuration, the third gas is preheated to a temperature of about 550° C. or higher before flowing into the annealing chamber. In another configuration, the annealing of one or more solid particles of the battery material can be performed by directly heating the annealing chamber, such as by heating the chamber body of the annealing chamber. For example, the annealing chamber may be a wall furnace to maintain the annealing temperature within the interior plenum of the annealing chamber. Advantages of using a heated gas include fast heat transfer, uniform high temperature, and ease of scale-up. The annealing chamber may be any chamber, furnace, or the like with a sealed chamber body, such as a domed ceramic annealing chamber, a quartz chamber, or a tube chamber. Optionally, the chamber body of the annealing chamber is made of a thermal insulating material (eg, ceramics, etc.) to prevent heat loss during the annealing process.
[0076] Optionally, in step 180, the battery material is allowed to cool to room temperature. The crystalline product is then milled using the process and milling apparatus described in FIG. 3, or any other suitable process and apparatus, to obtain nano-sized particles of battery material, such as SSE material, cathode active material, etc. For example, the battery material can be milled by a jet milling apparatus to a nano-size of 10 nanometers or more, such as a size of 20 nanometers to 500 microns, 100 microns to 300 microns, etc.
[0077] For example, the temperature of the final solid product particles of the battery material may be cooled slowly to room temperature to avoid disturbing or destroying the formation process into a stable energy state with uniform morphology and desired crystal structure. In another example, the cooling step may be performed very quickly to quench the reaction products, allowing the crystal structure of the solid particles of such reaction products to form in their stable energy state. As another example, the cooling treatment step in a multi-stage continuous process may include a cooling module consisting of one or more cooling mechanisms. Exemplary cooling mechanisms may include, for example, a gas-solid separator, a heat exchanger, a gas-solid feeder, a fluidized bed cooling mechanism, and combinations thereof.
[0078] Thus, by scanning electron microscope (SEM) analysis, a properly crystallized crystalline product of the desired SSE material can be obtained in spherical clusters with sizes between 1 micron and 300 microns, for example, between 10 microns and 100 microns. It is contemplated that the size of the resulting battery material can be controlled by the droplet size of the mist used in step 120 using a mist generator in a power jet chamber to adjustably obtain the desired sizes of various battery materials.
[0079] The method 100 for preparing solid particles of battery material in multiple steps is contemplated to carry out one or more reactions in a spraying step, a drying step, an oxidation step, two or more annealing reaction steps, one or more grinding steps, one or more cooling steps, etc., to obtain nano-sized final solid product particles of battery material of desired size, morphology, and crystal structure, which are used for further battery applications. Without wishing to be bound by theory, it is designed to be possible to carry out the reaction of the compounds in two or more reaction steps to allow the compounds to contact each other for a sufficient time to promote the nucleation of the proper crystal structure and proper folding of the particle morphology, to generate partial reaction paths with low thermodynamic energy, to ensure complete reaction of all compounds, to complete reaction, etc. Additional reaction modules can also be used. In one embodiment, the reaction module includes one annealing reaction to react and oxidize one or more solid particles of battery material into reaction products, some of which are partially reacted or oxidized. Another reaction module includes annealing the reaction products one or more times to ensure complete reaction of all reaction products into final solid battery material particles. Thus, the method 100 may include a process step that includes spraying a mist of the liquid mixture using a process module comprised of a power jet chamber and a gas-solid separator, and obtaining one or more solid particles of a solid electrolyte material. The method 100 may further include another process step of reacting, oxidizing, and annealing the one or more solid particles of the battery material using a reaction module comprised of an annealing chamber.
[0080] 3 is a flow chart illustrating a method 200 for producing an exemplary solid electrolyte material for a solid-state battery. The method 200 includes a step 202 of grinding the solid electrolyte material to obtain final solid product particles of the solid electrolyte material of a desired size, morphology, and crystal structure. In an embodiment, the solid electrolyte material can be ground by jet milling, mortar milling, hydraulic milling, electronic milling, mechanical milling, or a combination thereof. In an embodiment, the solid electrolyte material is ground and / or ground to less than 900 nm, less than 800 nm, less than 500 nm, or less than 300 nm, preferably less than 100 nm, preferably less than 90 nm, preferably less than 80 nm, preferably less than 70 nm, preferably less than 60 nm, preferably less than 50 nm, preferably less than 40 nm, preferably less than 30 nm, preferably less than 20 nm, preferably less than 10 nm, preferably less than 5 nm. In another embodiment, the solid electrolyte material is ground and / or crushed into nanoparticles having a size estimated in the range of 1 nm to 100 nm, such as 10 nm to 20 nm, for example 10 nm to 90 nm, such as 10 nm to 50 nm, for example 10 nm to 40 nm, such as 10 nm to 70 nm, for example 20 nm to 80 nm, such as 20 nm to 60 nm, for example 20 nm to 50 nm, such as 30 nm to 70 μm, for example 20 nm to 50 nm, such as 40 nm to 70 nm, for example 50 nm to 70 nm, such as 10 nm to 30 nm, for example 15 nm to 40 nm, such as 20 nm to 40 nm, for example 30 nm to 60 nm.
[0081] Second, the solid electrolyte material can be compressed into a pellet to measure its ionic conductivity, and as shown in FIG. 3, the method 200 includes a step 204 of compressing the powder of the solid electrolyte material into a pellet form of compressed solid electrolyte material. In one embodiment, the powder of the solid electrolyte material is hydraulically, electronically, or mechanically compressed in multiple successive steps, such as more than 2 steps, such as more than 3 steps, such as more than 4 steps, such as more than 5 steps, such as more than 6 steps, such as more than 7 steps, such as more than 8 steps, such as more than 9 steps, such as more than 10 steps, within a 20 mm die. For example, the solid electrolyte material is first compressed with 5-10 metric tons, then 10-15 metric tons, and finally 12-20 metric tons to form a high density pellet. As another example, the solid electrolyte material is first compressed with 5-7 metric tons, then 7-10 metric tons, and finally 11-14 metric tons to form a high density pellet. As yet another example, the solid electrolyte material may be first compressed at 3-15 metric tons, then 8-20 metric tons, and finally 20-30 metric tons to form a high density pellet.
[0082] The approximate density of the pellets was greater than 50%, preferably greater than 60%, preferably greater than 70%, preferably greater than 75%, preferably greater than 78%, preferably greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 92%, preferably greater than 95%, preferably greater than 97%, preferably greater than 99%.
[0083] In another embodiment, the compressed solid electrolyte material in pellet form has a diameter of 5 mm or more, such as 10 mm or more, 15 mm to 25 mm, preferably 17 mm to 22 mm, or any other suitable diameter depending on the press and its die used, such as a cold isostatic press (CIP) or any suitable press. In yet another embodiment, the compressed solid electrolyte material in pellet form has a thickness of less than 1.5 mm, or less than 1.0 mm, such as 400 microns or more, or 500 microns or more, such as 550 microns to 750 microns, or any other suitable thickness depending on the press and its die used.
[0084] Method 200 may optionally include adding 206 additional solid electrolyte ("SSE") material to the pellet form of the compressed solid electrolyte ("SSE") material. In one embodiment, the pellet form of the compressed solid electrolyte ("SSE") material is covered with additional solid electrolyte ("SSE") material to compensate for lithium loss.
[0085] In step 208, the pellet form of the compacted solid electrolyte (SSE) material is sintered at desired processing conditions to obtain a pellet form of the final solid electrolyte material for use in the battery. In one embodiment, the pellet form of the formed pellets is sintered in a furnace, such as, for example, an annealing reactor, a muffle furnace, a push plate furnace, or a roller furnace, at a temperature range of 900° C. to 1300° C., e.g., 1000° C. to 1300° C., e.g., 1100° C. to 1300° C., e.g., 900° C. to 1200° C., e.g., 900° C. to 1100° C., e.g., 1000° C. to 1200° C., e.g., 1100° C. to 1200° C., e.g., 1150° C. to 1200° C. Optionally, in step 210, the surface of the pellet form of the final solid electrolyte material is polished to a desired thickness and surface, for example, using sandpaper or other polishing techniques.
[0086] 4-5 show embodiments of method 210 and method 220 that include coating a cathode active material with a solid electrolyte material and forming coated cathode active materials 92C, 92D. In FIG. 4, method 210 is a wet coating process that includes step 211 forming a coating solution by dissolving a first amount of a solid metal salt or SSE material in a solvent. In step 213, a coating mixture is formed by mixing the coating solution with an amount of solid particles of the battery material to be coated with the solid metal or SSE material in a first time.
[0087] In general, the two or more metal salts in liquid form can be directly prepared in a liquid mixture at a desired concentration. The solids of the two or more metal-containing salts in solid form can be dissolved or dispersed in a suitable solvent (e.g., water, alcohol, methanol, isopropyl alcohol, isopropanol, organic solvents, inorganic solvents, organic acids, sulfuric acid (H2SO4), citric acid (C6H8O7), acetic acid (CH3COOH), butyric acid (C4H8O2), lactic acid (C3H6O3), nitric acid (HNO3), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone, and combinations thereof) to form a liquid mixture in an aqueous solution, slurry, gel, aerosol, or any other suitable liquid form. Depending on the desired composition of the final reaction product, two or more metal salts can be used. For example, two or more solid metal salts can be prepared in a desired molar ratio and mixed into a liquid mixture, for example, by measuring and preparing an appropriate amount of the two or more solid metal salts into a container containing a suitable amount of solvent. Depending on the solubility of the precursors in the selected solvent, pH, temperature, mechanical agitation and mixing can be adjusted to obtain a liquid mixture in which the desired molar concentration of one or more precursor compounds is fully dissolved and / or uniformly dispersed.
[0088] Another aspect of the present invention is a liquid mixture composed of two or more different soluble solutions with a desired molar ratio to produce a solid electrolyte material in a solid-state battery exhibiting high capacity. This provides the ability to precisely control and obtain specific molar ratios at the atomic level, as well as to produce the desired configuration of the solid electrolyte material as a coating solution used to produce the solid-state battery material. The soluble solutions of the liquid mixture include each metal-containing salt dissolved in an appropriate solvent to achieve a specific molar concentration of the metal-containing salt solution, which are mixed together to form a liquid mixture with the desired molar ratio for producing the solid electrolyte material. This process of producing the liquid mixture is efficient for producing active materials with high purity and precise stoichiometric phases. This provides a solid-state battery with desired properties such as high coulombic efficiency and high nominal capacity.
[0089] Next, in step 215, the coating mixture is dried in an oven or other suitable machine at a first temperature for a second period of time to obtain a dry solid powder of the coated battery material coated with the solid metal or SSE material. The first temperature is about 100° C. or more, or 150° C. or more, such as 200° C. to 300° C., such as 250° C. The second period of time is about 10 minutes or more, such as 10 minutes to 1 hour, such as 30 minutes.
[0090] In step 217, the dried solid powder is annealed in a furnace (e.g., muffle furnace, annealing chamber, etc.) at a second temperature for a third period of time in the presence of a gas (e.g., oxygen (O2)) to form a powder of the coated battery material. For example, a high purity gas or oxygen stream is flowed into an annealing reactor (e.g., muffle furnace) to serve as an energy source to oxidize and / or react various types of unreacted, partially and / or fully reacted metal-containing solid particles to one-fifth the weight of the powder of the coated battery material. In one aspect, the purity of the oxygen is greater than 50%, such as greater than 80%, such as 90%, 95%, or 97%. In one embodiment, the second temperature is greater than 600° C., such as between 650° C. and 800° C., such as 750° C. The third period of time is about 15 minutes or more, such as 1 hour or more, such as between 1 hour and 10 hours, such as 8 hours.
[0091] In step 219, the powder of the coated battery material is milled and sieved to obtain the final coated battery material. In one embodiment, step 219 includes milling the powder of the coated battery material into a separated material powder and sieving the separated material powder to obtain a desired particle size and quantity of the final coated battery material.
[0092] 5 illustrates an example of a dry coating method, i.e., a method 220 for coating solid particles of battery material with a solid metal or SSE material, which includes step 222 of preparing the particles of battery cathode material with a pretreatment agent in preparation for dry coating. In step 224, a powder of a solid electrolyte material (SSE) is mixed with particles of a battery cathode material (BCM) and a powder of a solid electrolyte material (SSE) with a pretreatment agent. SSE :Y BCM The two powders are mixed in a mixer or blender (e.g., a high energy mixer) in a ratio of 0.1 to 0.5, e.g., initially in a high energy mixer at 500 rpm for 1 minute to mix and homogenously mix the two powders. After mixing, the powder intensity of the blender can be increased to 2000 rpm for 6 minutes to break down the two powders into smaller agglomerates, allowing the SSE material to adhere to the surface of the BCM.
[0093] In one embodiment, X SSE :Y BCM The ratio is, for example, 1-50:50-99% by weight, for example, 1-40:60-99% by weight; for example, 1-30:70-99% by weight; for example, 5-40:60-95% by weight; for example, 5-30:70-95% by weight; for example, 5-20:80-95% by weight; for example, 10-40:60-90% by weight; for example, 10-30:70-90% by weight; for example, 10-20:80-90% by weight; for example, 15-50:50-85% by weight; for example, 15-40:60-85% by weight; for example, 15-30:70-85% by weight, for example, 15-35:65-85% by weight. For example, the amount % may be in the range of 20-30:70-80% by weight; for example, 20-40:60-80% by weight; for example, 20-50:50-80% by weight; for example, 20-50:50-80% by weight; for example, 20-50:50-80% by weight; for example, 30-50:50-70% by weight; for example, 30-60:40-70% by weight; for example, 30-40:60-70% by weight; for example, 35-50:50-65% by weight; for example, 35-30:70-65% by weight; for example, 35-40:60-65% by weight; for example, 40-50:50-60% by weight; for example, 45-50:50-55% by weight.
[0094] In one embodiment, Y BCM :XSSE The ratio is, for example, 1-50:50-99% by weight, for example, 1-40:60-99% by weight; for example, 1-30:70-99% by weight; for example, 5-40:60-95% by weight; for example, 5-30:70-95% by weight; for example, 5-20:80-95% by weight; for example, 10-40:60-90% by weight; for example, 10-30:70-90% by weight; for example, 10-20:80-90% by weight; for example, 15-50:50-85% by weight; for example, 15-40:60-85% by weight; for example, 15-30:70-85% by weight, for example, 15-35:65-85% by weight. For example, the amount % may be in the range of 20-30:70-80% by weight; for example, 20-40:60-80% by weight; for example, 20-50:50-80% by weight; for example, 20-50:50-80% by weight; for example, 20-50:50-80% by weight; for example, 30-50:50-70% by weight; for example, 30-60:40-70% by weight; for example, 30-40:60-70% by weight; for example, 35-50:50-65% by weight; for example, 35-30:70-65% by weight; for example, 35-40:60-65% by weight; for example, 40-50:50-60% by weight; for example, 45-50:50-55% by weight.
[0095] Next, in step 226, the particles of battery cathode material (BCM) are coated and surrounded by solid electrolyte material (SSE) to obtain final coated cathode material (FCCM). In one embodiment of the dry coating process, larger core particles can be directly coated with smaller fine particles by external mechanical force without using any solvent or binder. In another embodiment, a single particle of cathode material can be successfully coated with fine particles of solid electrolyte material. In step 228, the coated final cathode material (FCCM) is used as a cathode and fabricated into a solid-state battery.
[0096] To obtain coated cathode active materials 92C, 92D, solid electrolyte materials 96C, 96D can be coated onto cathode active materials 94C, 94D using wet or dry coating processes, respectively shown in FIG. 4 and FIG. 5. In one embodiment of the dry coating process, larger core particles can be directly coated with smaller fine particles by external mechanical force without using any solvent and binder. In another embodiment, a single particle of cathode material can be successfully coated with fine particles of solid electrolyte material. For example, the dry coating process includes dry powder mixing, forming the powder into a film, and laminating the film onto a current collector; all performed without using solvents. In another embodiment, the wet coating process includes mixing the active cathode cell material, the solid electrolyte material, and an organic or inorganic solvent (e.g., water, alcohol, methanol, isopropyl alcohol, organic solvents, inorganic solvents, organic acids, sulfuric acid (H2SO4), citric acid (C6H8O7), acetic acid (CH3COOH), butyric acid (C4H8O2), lactic acid (C3H6O3), nitric acid (HNO3), hydrochloric acid (HCl), ethanol, pyridine, ammonia, acetone, and combinations thereof, etc.), mixture to obtain a coated solid electrolyte material.
[0097] FIG. 6 shows a flow chart incorporating the method 100 of preparing materials for battery electrochemical cells using a system 300 with all the necessary manufacturing tools. The system 300 generally includes a mist generator 306, a power jet chamber 310, a power jet module 314, a gas-solid separator 320, and a reactor 340. First, a liquid mixture containing two or more precursors is prepared and fed into the mist generator 306 of the system 300. The mist generator 306 is coupled to the power jet chamber 310 and adapted to generate mist from the liquid mixture. Before the mist is formed or at the same time as the mist is generated in the power jet chamber 310, a flow of heated gas may be flowed into the power jet chamber 310 to fill and preheat the interior volume of the power jet chamber 310. The mist is mixed with the heated gas to remove moisture therefrom, thereby forming a gas-solid mixture including the heated gas, the two or more precursors, and / or other gas-phase waste or by-products.
[0098] The gas-solid mixture is then continuously fed into a gas-solid separator 320, where the gas-solid mixture is separated into solid particles and waste. The solid particles are then fed into a reactor 340, where they are mixed with a heated gas stream to form a gas-solid mixture. The reaction in the reactor is carried out for a reaction time until a reaction product can be obtained. Optionally, the gas-solid mixture of the reaction product can be fed into a gas-solid separator (e.g., gas-solid separator 328) to separate and obtain final solid product particles and gaseous by-products. Furthermore, one or more cooling fluid (e.g., gas or liquid) streams can be used to cool the temperature of the reaction product. The final solid product particles are sent out of the system 300 and can be further analyzed for their properties (e.g., specific capacity, power performance, battery charge cycle performance, etc.), particle size, morphology, crystal structure, etc., and can be used as materials in battery cells. Finally, the final particles are packaged into battery cell components.
[0099] FIG. 7 is a schematic diagram of a system 300, which is an example of an integrated tool / apparatus that can be used to perform a fast, simple, continuous, and low-cost manufacturing process to prepare materials for battery electrochemical cells. The system 300 is connected to a liquid mixer 304, which is connected to two or more reactant sources 302A, 302B. The reactant sources 302A, 302B are provided for storing various precursor compounds and liquid solvents. The desired amounts of precursor compounds (in solid or liquid form) and solvents are fed and delivered from the reactant sources 302A, 302B to the liquid mixer 304, which allows the precursor compounds to be dissolved and / or dispersed in the solvent and thoroughly mixed into a liquid mixture. If necessary, the liquid mixer 304 is heated to a temperature, such as 30° C. to 90° C., to aid in uniform dissolution, dispersion, and / or mixing of the precursors. The liquid mixer 304 is optionally connected to a pump 305, which transfers the liquid mixture from the liquid mixer 304 to a mist generator 306 of the system 300 to generate a mist.
[0100] The mist generator 306 converts the liquid mixture into a mist having a desired droplet size and size distribution. Additionally, the mist generator 306 is coupled to the power jet chamber 310 to dry and remove moisture from the mist to obtain thoroughly mixed solid precursor particles. In one embodiment, the mist generator 306 is positioned near the top of a vertically oriented power jet chamber 310 (e.g., a dome-shaped power jet chamber, etc.) and injects the mist into the power jet chamber 310 and passes vertically downward through the power jet chamber. Alternatively, the mist generator can be positioned near the bottom of a vertically oriented power jet chamber 310 and injects the mist upward into the power jet chamber to extend the residence time of the generated mist in the power jet chamber. In another embodiment, the power jet chamber 310 is positioned horizontally (e.g., a tube power jet chamber, etc.) and the mist generator 306 is positioned near one end of the power jet chamber 310 such that the flow of mist channeled from one end of the power jet chamber 310 through the other end passes through a path within the power jet chamber 310 for the length of its residence time.
[0101] The power jet chamber 310 typically includes one or more power jet modules 314 (e.g., power jet modules 314A, 314B, 314C, 314D, etc.), a chamber inlet 315, a chamber body 312, and a chamber outlet 317. In one configuration, the mist generator 306 is disposed near the chamber inlet 315 in the power jet chamber 310 and connected to a liquid line 303 adapted to flow the liquid mixture from the liquid mixer 304. For example, the liquid mixture in the liquid mixer 304 may be transferred by the pump 305 to the interior volume of the power jet chamber 310 via the liquid line 303 connected to the chamber inlet 315. The transfer of the liquid mixture by the pump 305 may be configured to be continuous at a desired feed rate (e.g., regulated by a metering valve or other means) to achieve, for example, good process throughput of the system 300. In another configuration, the mist generator 306 is positioned outside the power jet chamber 310 and the mist generated therefrom is directed into the power jet chamber 310 via the chamber inlet 315.
[0102] One or more gas lines (e.g., gas lines 331A, 331B, 331C, 331D, etc.) can be connected to various portions of the power jet chamber 310 and adapted to flow gas from a gas source 332 into the power jet chamber 310. A flow of gas stored in the gas source 332 can be pumped into the power jet chamber 310 simultaneously with the formation of the mist in the power jet chamber 310 to carry the mist through the power jet chamber 310, remove moisture from the mist, and form a gas-solid mixture including the precursors. A flow of gas can be pumped into the power jet chamber 310 prior to the formation of the mist to fill and preheat the interior volume of the power jet chamber 310 to generate the mist in the power jet chamber 310.
[0103] In one example, the gas line 331A is connected to the top of the power jet chamber 310 and delivers gas to the mist generator 306 located near the chamber inlet 315, where it is mixed with the mist generated by the mist generator 306 in the power jet chamber 310. In one embodiment, the gas is preheated to a temperature of 70°C to 600°C to mix with the mist and remove moisture from the mist. As another example, the gas line 331B delivering the gas is connected to the chamber inlet 315 of the power jet chamber 310 in close proximity to the liquid line 303 having the liquid mixture. Thus, the gas can be sufficiently mixed with the mist of the liquid mixture in the power jet chamber 310.
[0104] In another example, gas line 331C is connected to the chamber body 312 of the power jet chamber 310 to deliver gas therein and mix it with the mist generated from the mist generator 306. Additionally, gas line 331D connected to the power jet chamber 310 near the chamber outlet 317 can be used to ensure that the gas-solid mixture formed in the power jet chamber 310 is uniformly mixed with the gas.
[0105] The gas flow may be passed through an air filter to remove any particles, droplets, or contaminants, and the gas flow rate may be adjusted by a valve or other means. In one embodiment, the gas is mixed with the mist and heated to a temperature that removes moisture from the mist. The method is designed to obtain spherical solid particles from a thoroughly mixed liquid mixture of two or more precursors after drying the mist of the liquid mixture. In contrast, conventional solid manufacturing processes involve mixing or grinding a solid mixture of precursor compounds, which results in a non-uniform mixture.
[0106] Once the mist of the liquid mixture dries into a gas and a gas-solid mixture, the gas-solid mixture is pumped out of the power jet chamber 310 via the chamber outlet 317. The power jet chamber 310 is coupled to a gas-solid separator 320 of the system 300. The gas-solid separator 320 collects the chamber product (e.g., a gas-solid mixture of gas and one or more solid particles of a solid electrolyte material mixed together) from the chamber outlet 317.
[0107] The gas-solid separator 320 includes a separator inlet 321A and two or more separator outlets 322A, 324A. The separator inlet 321A is connected to the chamber outlet 317 and is adapted to collect the gas-solid mixture and other chamber products from the power jet chamber 310. The gas-solid separator 320 separates the gas-solid mixture from the power jet chamber 310 into one or more solid particles of solid electrolyte material and waste. The separator outlet 322A is adapted to send the one or more solid particles of solid electrolyte material to the reactor 340 for further processing and reaction. The separator outlet 324A is adapted to send the waste from the gas-solid separator 320.
[0108] The waste products may be fed to gas abatement device 326A, treated, and discharged out of system 300. The waste products may include, for example, water (H2O) vapor, organic solvent vapor, nitrogen-containing gas, oxygen-containing gas, O2, O3, nitrogen gas (N2), NO, NO2, NO2, N2O, N4O, NO3, N2O3, N2O4, N2O5, N(NO2)3, carbon-containing gas, carbon dioxide (CO2), CO, hydrogen-containing gas, H2, chlorine-containing gas, Cl2, sulfur-containing gas, SO2, small particles of one or more solid particles of a solid electrolyte material, and combinations thereof.
[0109] The one or more solid particles of the solid electrolyte material may include at least particles of two or more precursors that have been dried and mixed together homogeneously. It is contemplated that the one or more solid particles of the solid electrolyte material are separated from any by-products, gaseous products, or waste products prior to reacting the two or more precursors in the reactor 340. Thus, the system 300 is designed to homogeneously mix the two or more precursors, dry the two or more precursors, separate the dried two or more precursors, and react the two or more precursors sequentially into a final solid product particle of the crystallized solid electrolyte material. Suitable gas-solid separators include cyclones, electrostatic separators, electrostatic precipitators, gravitational separators, inertial separators, membrane separators, fluidized beds, classifiers, electric sieves, impactors, particle collectors, leaching separators, elutriators, air classifiers, leaching classifiers, and combinations thereof.
[0110] Once one or more solid particles of the solid electrolyte material are separated, they are fed into a reactor 340 for further reaction. The reactor 340 includes a gas inlet 333, a reactor inlet 345, and a reactor outlet 347. The reactor inlet 345 is connected to the separator outlet 322A and adapted to receive the solid particles. Optionally, the vessel 325 is adapted to store the solid particles before adjusting the amount of the solid particles fed into the reactor 340. The gas inlet 333 of the reactor 340 is connected to a heating mechanism 380, which heats gas from a gas source 334 to an annealing temperature of 400° C. to 1200° C. The heating mechanism 380 can be, for example, an electric heater, a gaseous fuel heater, a burner, etc. If necessary, an additional gas line can be used to feed heated air or gas into the reactor 340. The pre-heated gas can be charged into the reactor 340 to maintain the internal temperature of the reactor 340 in a manner that is much better and more energy efficient than conventional heating of the reactor chamber body.
[0111] The gas flowing into the reactor 340 is designed to mix with one or more solid particles of the solid electrolyte material to form an oxidation reaction product within the reactor 340. Thermal energy from the preheated gas is used as an energy source to react one or more solid particles of the solid electrolyte material within the reactor 340. Reaction processes include, but are not limited to, reduction, decomposition, complex reactions, phase transitions, recrystallization, mono-replacement reactions, di-replacement reactions, combustion, isomerization, and combinations thereof. The oxidized reaction product then undergoes an annealing process for a residence time ranging from 1 second to 10 hours or more, depending on the annealing temperature and the type of precursors initially delivered to the system 300. One embodiment of the present invention provides for controlling the temperature of the reactor 340 by the temperature of the heated gas.
[0112] Once the reaction in reactor 340 is complete, e.g., when a desired crystal structure, particle morphology, and particle size has been formed, the oxidized reaction product exits reactor 340 via reactor outlet 347 and / or reactor outlet 348. The cooled reaction products include final solid product particles of crystallized solid electrolyte material that include particles of oxidation products of precursor compounds that are suitable, for example, as materials for battery cells.
[0113] Optionally, system 300 includes a gas-solid separator, such as gas-solid separator 328, which collects the reaction products from reactor outlet 347 of reactor 340. Gas-solid separator 328 can be a particle collector, such as a cyclone, electrostatic separator, electrostatic precipitator, gravity separator, inertial separator, membrane separator, fluidized bed classifier, electric sieve impactor, percolation separator, elutriator, air classifier, percolation classifier, and combinations thereof.
[0114] The gas-solid separator 328 of the system 300 generally includes a separator inlet 321B, a separator outlet 322B, and a separator outlet 324B, and is used to separate the reaction products into solid particles and gaseous by-products. The gaseous by-products may be fed to a gas abatement device 326B for processing and discharged outside the system 300. The gaseous by-products separated by the gas-solid separator 328 generally may include water (H2O) vapor, organic solvent vapor, nitrogen-containing gas, oxygen-containing gas, O2, O3, nitrogen gas (N2), NO, NO2, NO2, N2O, N4O, NO3, N2O3, N2O4, N2O5, N(NO2)3, carbon-containing gas, carbon dioxide (CO2), CO, hydrogen-containing gas, H2, chlorine-containing gas, Cl2, sulfur-containing gas, SO2, small particles of solid particles, and combinations thereof. Additionally, the system 300 may further include one or more cooling fluid lines 353, 355 connected to the reactor outlet 347 or the separator outlet 322A of the gas-solid separator 328 and adapted to cool the reaction products and / or solid particles. The cooling fluid line 353 is adapted to deliver a cooling fluid (e.g., gas or liquid) from a source 352 to the separator inlet 321B of the gas-solid separator 328. The cooling fluid line 355 is adapted to deliver the cooling fluid to the heat exchanger 350, which may be filtered by a filter 354 to remove particles.
[0115] Heat exchanger 350 is configured to collect and cool the solid particles and / or reaction products from gas-solid separator 328 and / or reactor 340 by flowing a cooling fluid. The cooling fluid has a lower temperature than the temperature of the reaction products and solid particles exiting gas-solid separator 328 and / or reactor 340. The cooling fluid may have a temperature between 4° C. and 30° C. The cooling fluid may be liquid water, liquid nitrogen, air, an inert gas, or any other gas that does not react with the reaction products.
[0116] The final solid product particles are collected and cooled by one or more separators, cooling fluid lines, and / or heat exchangers, and once cooled, the solid particles are pumped out of the system 300 and collected in a final product collector 368. The solid particles may include oxidized forms of the precursors, such as oxide materials that are suitable for packaging into battery cells 370. Additional pumps may be installed to achieve the desired pressure gradient.
[0117] A process control system 390 may be coupled to the system 300 at various locations to automatically control the manufacturing process performed by the system 300 and adjust various process parameters (e.g., flow rates, mix ratios, temperatures, residence times, etc.) within the system 300. For example, the flow rate of the liquid mixture into the system 300 may be adjusted near the reactant sources 302A, 302B, the liquid mixer 304, or the pump 305. The droplet size and generated flow rate of the mist generated by the mist generator 306 may be adjusted. Additionally, the flow rates and temperatures of the various gases flowing within the gas lines 331A, 331B, 331C, 331D, 333, 353, 355, 515, etc. may be controlled by the process control system 390. Additionally, the process control system 390 is adapted to control the temperature and residence time of the various gas-solid mixtures and solid particles at desired levels at various locations.
[0118] Thus, a continuous process is provided for producing battery cell materials using a system including a mist generator, a power jet chamber, one or more gas-solid separators, and a reactor. A mist generated from a liquid mixture of one or more metal precursor compounds in a desired ratio is mixed with air in the power jet chamber and dried, thereby forming a gas-solid mixture. Within the system, one or more gas-solid separators are used to separate the gas-solid mixture from the power jet chamber into solid particles containing one or more metal precursors, which are continuously fed into a reactor for further reaction to obtain final solid material particles having a desired ratio of two or more intercalated metals.
[0119] The present invention provides for the creation and manufacture of SSE or metal oxide materials. Depending on the details and ratios of metal precursor compounds fed into the system 300, the final solid material particles obtained from the system 300 can be metal oxide materials, doped metal oxide materials, inorganic metal salts, and the like. Furthermore, the metal oxide materials can exhibit the crystal structure of the metal in the form of layered, spinel, olivine, and the like. The morphology of the solid product particles (such as oxidation reaction products produced using the method 100 and system 300 described herein) exists as a desired solid powder. The particle size of the solid powder ranges from 1 nm to 100 μm.
[0120] During operation, the mist is mixed with a gas flow of gas in the mist generator to form a gas-liquid mixture, the liquid mixture including the lithium-containing salt compound and one or more salt-containing compounds. The liquid mixture is further mixed with a gas flow of another gas in the power jet chamber. It is contemplated that these gas flows are provided to thoroughly mix the liquid mixture to form a homogenous gas-liquid mixture and to aid in conveying the gas-liquid mixture into the power jet chamber. The liquid mixture is digitally or manually prepared with a desired molar ratio of the lithium-containing salt compound, one or more inorganic salt compounds in the reactant source, and fed into one or more liquid mixers.
[0121] The adjustment of the molar ratio of the lithium-containing salt compound and the one or more salt-containing compounds is performed before forming the mist of the liquid mixture in the liquid mixer. The desired molar ratio of the lithium-containing salt and the one or more salts is measured digitally or manually and sent from the reactant source to the liquid mixer, which allows the lithium-containing salt compound and the one or more salt-containing compounds to be dissolved and / or dispersed in a solvent and thoroughly mixed in the liquid mixer to become a liquid mixture. The lithium-containing salt compound and the one or more salt-containing compounds are all dissolved in a suitable solvent in the liquid mixture.
[0122] Also, adjusting the molar ratio of the lithium-containing salt compound to the one or more salt-containing compounds is performed simultaneously with the formation of the mist of the liquid mixture. The desired molar ratio of the lithium-containing salt compound to the one or more inorganic salt compounds can be digitally or manually adjusted from each reactant source and fed to the mist generator to generate the mist of the liquid mixture within the mist generator.
[0123] The liquid mixture comprising the lithium-containing salt compound and one or more salt-containing compounds is mixed with a gas stream to form a gas-liquid mixture in a power jet chamber. The gas-liquid mixture is then dried at a temperature in the power jet chamber to form a gas-solid mixture of solid particles of the solid electrolyte material. The gas-solid mixture is continuously fed to a gas-solid separator where the gas-solid mixture is separated into one or more solid particles of the solid electrolyte material and a waste product.
[0124] The one or more solid particles of the oxide material are then fed into an annealing chamber, where they are mixed with the gas flow, and the one or more solid particles of the solid electrolyte material are reacted and annealed at an annealing temperature in the annealing chamber to obtain a high quality solid electrolyte material of desired size, morphology and crystal structure, optionally doped with one or more dopants.
[0125] FIG. 8A is a perspective view of one embodiment of a processing system for producing particulate material. This exemplary embodiment of the processing system 6100 includes a system inlet 6102 for delivering one or more gases via gas line 6106 and a system outlet 6104 for delivering particulate material from the processing system. The one or more gases may be selected from gas sources such as air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, noble gas, and combinations thereof. In one embodiment, such a processing system further includes an array of one or more power jet modules for jetting the liquid mixture into one or more droplet streams and for causing the one or more droplet streams to enter the processing system. The processing system further includes a reaction chamber for processing the one or more droplet streams and the one or more gases into particulate material.
[0126] A liquid mixture is prepared from two or more precursor compounds and then converted into droplets, each droplet having two or more precursors uniformly dispersed together. The liquid mixture is then dehydrated by passing the droplets through a dispersion chamber, and a gas flow is used to convey the mist into the dispersion chamber for a suitable residence time. It is further contemplated that the concentration of the precursor compounds in the liquid mixture and the droplet size of the mist of the liquid mixture can be adjusted to control the chemical composition, particle size, and size distribution of the final product particles of the battery material.
[0127] Such a processing system further includes at least one buffer chamber configured at the system inlet 6102 to deliver the gas source into a plurality of uniform gas streams, as shown in FIG. 8A. In addition, in one embodiment, the processing system includes a dispersion chamber 6220 and power jet modules 6240A, 6240B, and 6240C to prepare the precursor liquid mixture into a desired size and deliver the desired precursor liquid mixture into the processing system. The power jet module can be attached to a portion of the dispersion chamber and utilizes air pressure to jet the liquid mixture and directly convert it into a mist with small droplet sizes in the dispersion chamber. Alternatively, the mist can be generated outside the dispersion chamber and delivered into the dispersion chamber. The suitable droplet size can be adjusted depending on the choice of the power jet module used, the liquid mixture compound, the temperature of the dispersion chamber, the gas flow rate, and the residence time in the dispersion chamber. For example, a mist with droplet sizes of one tenth of a micron to one millimeter is generated in the dispersion chamber.
[0128] The power jet module 6240A is coupled to a portion of the dispersion chamber 6220 and generates a mist (e.g., a large collection of small sized droplets) of the liquid mixture directly within the dispersion chamber. Generally, the power jet module 6240A can generate a mist of single sized droplets. In one embodiment, the dispersion chamber 6220 is connected to one or more power jet modules 6240A, 6240B, and 6240C and receives multiple uniform gas streams from the buffer chamber and disperses the multiple uniform gas streams among each other using one or more droplet streams ejected from an array of one or more power jet modules 6240A, 6240B, and 6240C.
[0129] In one embodiment, the dispersion chamber 6220 is connected to a reaction chamber 6210 for processing one or more liquid droplet streams and one or more gases into particulate material. The reaction chamber 6210 further connects to a system outlet 6104 for delivering the particulate material from the processing system.
[0130] 8B is an exemplary processing system 6100 that can be used to implement a fast, simple, continuous, and low-cost manufacturing process for producing particulate materials. The processing system 6100 includes a system inlet 6102 for delivering one or more gases to the processing system, a buffer chamber 6230 connected to the system inlet 6102, a dispersion chamber 6220 connected to the buffer chamber 6230, a reaction chamber 6210 connected to the dispersion chamber 6220, and a system outlet 104 connected to the reaction chamber 6210.
[0131] The processing system 6100 further comprises a gas distributor 6232 attached to a chamber wall 6238 of the buffer chamber 6230, channels of the distributor 6232 for delivering one or more gases F1 to multiple uniform gas flows F2 within the processing system, a dispersion chamber 6220, and one or more power jet modules 6240A and 6240B attached to the chamber wall 6228 of the dispersion chamber 6220.
[0132] The one or more gases F1 pumped into the buffer chamber 6230 are pressurized downward and flow at a constant speed through the channel 6234 of the gas distributor 6232, resulting in a plurality of uniform gas flows F2 exiting the channel 6234 and entering the dispersion chamber 6220. In one embodiment, the one or more gases F1 may be transported through an air filter to remove any particles, droplets, or contaminants, and the flow rate of the gas may be adjusted by a valve or other means. In one embodiment, the flow rate of the plurality of uniform gas flows F2 exiting the channel 6234 is greater than the flow rate of the one or more gases F1. Furthermore, the directions of the plurality of uniform gas flows F2 are collected and combined.
[0133] The power jet module 6240A includes a power jet 6242A for ejecting the liquid mixture provided to the power jet module 6240A into one or more droplet streams. The power jet module 6240A further includes a support frame 6244A for supporting the power jet module 6240A, a module actuator 6246A mounted inside the support frame 6244A, and a connector 6245A connecting the module actuator 6246A and the power jet 6242A, where the module actuator 6246A controls the one or more droplets F ejected from the power jet 6242A mounted inside the support frame 6244A. A into the dispersion chamber 6220. Additionally, the power jet module 6240B includes a power jet 6242B for ejecting the liquid mixture provided to the power jet module 6240B into one or more droplet streams. The power jet module 6240B further includes a support frame 6244B for supporting the power jet module 6240B, a module actuator 6246B mounted inside the support frame 6244B, and a connector 6245B connecting the module actuator 6246B and the power jet 6242B, where the module actuator 6246B drives the one or more droplets F ejected from the power jet 6242B mounted inside the support frame 6244B. B is driven to flow into dispersion chamber 6220.
[0134] Droplet stream F injected into dispersion chamber 6220 A are separated from each other by a plurality of uniform gas flows F2 at an angle of α A The gas flows F2 and droplet streams F are dispersed in a uniform manner. A Furthermore, the droplet stream F injected into the dispersion chamber 6220 forms a gas-liquid mixture F3 including B are separated from each other by a plurality of uniform gas flows F2 at an angle of α B The gas flows F2 and droplet streams F are dispersed in a uniform manner. BA gas-liquid mixture F3 is formed comprising: In one embodiment, the dispersion chamber was itself maintained at the first temperature.
[0135] One or more gases are heated to a drying temperature and mixed with the droplet stream to remove moisture from the droplet stream. The method is designed to obtain spherical solid particles from a thoroughly mixed liquid mixture of two or more liquids after drying the mist of the liquid mixture. In contrast, conventional solid manufacturing processes involve mixing or grinding solid mixtures of liquid mixture compounds, which results in inhomogeneous mixing of the liquid mixture.
[0136] The one or more gases may be, for example, air, oxygen, carbon dioxide, nitrogen gas, hydrogen gas, inert gas, noble gas, and combinations thereof. For example, heated air can be used as an inexpensive gas and energy source for drying the droplet stream. The one or more gases selected may be gases that mix well with the precursor droplet stream and dry the mist without reacting with the precursor. In some cases, chemicals in the droplet stream may react to some extent with one or more gases and / or each other during drying, depending on the drying temperature and the precursor chemical composition. Furthermore, the residence time of the thoroughly mixed precursor compound droplet stream in the dispersion chamber can be adjusted depending on the flow rate of the one or more gases and the path length the droplet stream needs to travel in the dispersion chamber.
[0137] The processing system 6100 further comprises a reaction chamber 6210 that receives the gas-liquid mixture F3 and reacts the gas-liquid mixture F3 at a second temperature for a reaction time into a final reaction product F4. Finally, the final reaction product F4, which may be a product particle, may be pumped out of the system 6100 via a system outlet 6104 so that it can be further analyzed for its properties (e.g., specific capacity, power performance, particle charge cycle performance), particle size, morphology, crystal structure, etc., and used as a particulate material.
[0138] The processing system 6100 is connected to an electronic control unit 6300 with a CPU 6340 for automatic control of the processing system 6100. As shown in FIG. 14, the control unit 6300 is coupled to various locations of the processing system 6100 to automatically control the manufacturing process performed by the processing system 6100 and adjust various process parameters (e.g., flow rate, mixing ratio, temperature, residence time, etc.) in the processing system 6100. For example, the flow rate of the liquid mixture to the processing system 6100 can be adjusted near the liquid mixture container or pump. As another example, the droplet size and generation rate of the mist generated by the power jet modules 6240A and 6240B can be adjusted. Also, the flow rate and temperature of the various gases flowing in the gas lines, etc. can be controlled by the control unit 6300. Furthermore, the process control unit 6300 is adapted to control the temperature, air pressure, and residence time of the various gas-solid mixtures and solid particles at various locations at desired levels.
[0139] In operation, the control unit 6300 can be used to control the parameters of a continuous, multi-step process (e.g., method 900 described herein) performed within the control unit 6300, resulting in high quality, consistent active battery materials with much less time, effort, and monitoring than materials prepared in traditional manufacturing processes. A representative process profile performed by the control unit 6300 in FIG. 8B is shown as a plot of temperature versus time.
[0140] Optionally, the processing system 6100 further comprises a first separator connected to the dispersion chamber 6230 and adapted to collect the gas-liquid mixture F3 from the dispersion chamber and separate it into a first type of solid particles and waste. Optionally, the first separator is connected to a power jet chamber, which is connected to the dispersion chamber 6230 and adapted to collect the gas-liquid mixture F3 from the dispersion chamber and dry it into gas-solid particles and separate it into a first type of solid particles and waste in the first separator. In one embodiment, the first separator further comprises a first separator outlet connected to the reaction chamber 6210 and adapted to deliver the first type of solid particles to the reaction chamber 6210 and a second separator outlet adapted to deliver the waste from the first separator.
[0141] 8C shows an example of a power jet module configured in a dispersion chamber. A power jet module 1040A for jetting a liquid mixture into one or more droplet streams and flowing the one or more streams into a processing system includes a power jet 1042A for jetting the liquid mixture provided to the power jet module 1040A into one or more droplet streams. The power jet module 1040A further includes a support frame 1044A for supporting the movement of the power jet 1042A, a first module actuator 1046A for moving the power jet to correspond to and connect with an opening of the dispersion chamber, and a connector 1045A for connecting the first module actuator 1046A and the power jet 1042A.
[0142] In Figure 8C, the dispersion chamber 1020 comprises one or more openings 1022A, 1022B, 1022C, 1022D, 1022E, and 1022F that are disposed in the chamber wall of the dispersion chamber 1020 and adapted to connect and mount to the power jets of a power jet module on one side of the power jet with nozzle array. In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Figure 8C, where the one or more openings are rectangular with a width at the bottom that is shorter than the length of the sides, and are disposed adjacent to each other at an equal distance on the same horizontal line of the chamber wall.
[0143] As shown in Fig. 8C, the dispersion chamber 1020 is filled with a plurality of integrated gases F2 sent from the buffer chamber of the processing chamber. In one embodiment, simultaneously with the formation of the droplet stream in the dispersion chamber 1020 ejected from the power jet of the power jet module, the plurality of integrated gases F2 are sent into the dispersion chamber 1020 to carry the droplet stream through the dispersion chamber 1020, which may or may not remove moisture from the mist, and form a gas-liquid mixture in a direction F3 including the liquid mixture and the plurality of integrated gases. Also, the flow of the plurality of integrated gases F2 can be sent into the dispersion chamber 1020 before the droplet stream is formed, to fill the internal volume of the dispersion chamber 1020, and optionally preheat it to a first temperature before generating the droplet stream in the dispersion chamber 1020.
[0144] One or more of the openings 1022A-1022F may be located near the top of a vertically oriented dispersion chamber 1020 (e.g., a dome-shaped dispersion chamber) and may be fitted with a power jet module that injects a stream of droplets into the dispersion chamber 1020 and passes vertically downward through the dispersion chamber. Alternatively, one or more of the openings 1022A-1022F may be located near the bottom of a vertically oriented dispersion chamber 1020 and may be fitted with a power jet module that injects the droplet stream upward into the dispersion chamber by increasing the residence time of the stream generated therein. In another embodiment, the dispersion chamber 1020 may be arranged horizontally (e.g., a tube dispersion chamber) and one or more of the openings 1022A-1022F may be located near one end of the dispersion chamber 1020 and may be fitted with a power jet module that injects a stream of droplets from one end of the dispersion chamber 1020 to the other end and pass through the dispersion chamber 1020 over the length of its residence time.
[0145] Furthermore, the droplet stream injected into the dispersion chamber 1020 is dispersed together with the multiple uniform gas flows F2 into a gas-liquid mixture F3 including the multiple uniform gas flows F2 and the droplet stream. The dispersion chamber was maintained at a first temperature. The direction of the multiple uniform gas flows F2 fed into the dispersion chamber is parallel to the chamber wall of the dispersion chamber 1020. The direction of the gas-liquid mixture F3 pumped through the dispersion chamber 1020 is also parallel to the chamber wall of the dispersion chamber 1020. In another embodiment of the present invention, the direction of the multiple uniform gas flows F2 fed into the dispersion chamber 1020 and the direction of the gas-liquid mixture F3 pumped through the dispersion chamber 1020 are different.
[0146] 8D shows an example of a power jet module configured in a dispersion chamber. In one embodiment, a power jet module 1140A for injecting a liquid mixture into one or more droplet streams and directing the one or more streams into a processing system includes a power jet 1142A for injecting a liquid mixture provided to the power jet module 1140A into one or more droplet streams. The power jet module 1140A further includes a support frame 1144A for supporting movement of the power jet 1142A, a first module actuator 1146A for moving the power jet to correspond to and connect with an opening of the dispersion chamber, and a connector for connecting the first module actuator 1146A to the power jet 1142A.
[0147] As shown in Figure 8D, the dispersion chamber 1120 comprises one or more openings 1122A, 1122B, 1122C disposed in a chamber wall of the dispersion chamber 1120 and adapted to connect to and mount to power jets of a power jet module on one side of the power jet with nozzle array. The shape of the opening or openings and the arrangement of the opening or openings are shown in Figure 8D, where the opening or openings are rectangular with a width at the bottom greater than the length of the sides, and are disposed adjacent to each other at an equal distance on the same horizontal line of the chamber wall.
[0148] As shown in FIG. 8D, the dispersion chamber 1120 is filled with a plurality of integrated gases F2 sent from the buffer chamber of the processing chamber. Simultaneously with the formation of the droplet stream in the dispersion chamber 1120 ejected from the power jet of the power jet module, the plurality of integrated gases F2 are sent into the dispersion chamber 1120 to carry the droplet stream through the dispersion chamber 1120, which may or may not remove moisture from the mist, and form a gas-liquid mixture in a direction F3 including the liquid mixture and the plurality of integrated gases. Also, the flow of the plurality of integrated gases F2 can be sent into the dispersion chamber 1120 before the droplet stream is formed, to fill the internal volume of the dispersion chamber 1120, and optionally preheat it to a first temperature before generating the droplet stream in the dispersion chamber 1120.
[0149] One or more of the openings 1122A-C may be located near the top of a vertically oriented dispersion chamber 1120 (e.g., a dome-shaped dispersion chamber) and may be fitted with a power jet module to inject a stream of droplets into the dispersion chamber 1120 and pass vertically downward through the dispersion chamber. Alternatively, one or more of the openings 1122A-C may be located near the bottom of a vertically oriented dispersion chamber 1120 and may be fitted with a power jet module to inject the droplet stream upward into the dispersion chamber by increasing the residence time of the stream generated therein. In another embodiment, the dispersion chamber 1120 may be arranged horizontally (e.g., a tube dispersion chamber) and one or more of the openings 1122A-C may be fitted with a power jet module to inject a stream of droplets from one end of the dispersion chamber 1120 to the other end and pass through a path within the dispersion chamber 1120 over the length of its residence time. In one embodiment, the dispersion chamber was itself maintained at a first temperature.
[0150] The direction of the multiple uniform gas flows F2 fed into the dispersion chamber is parallel to the chamber wall of the dispersion chamber 1120. Also, the direction of the gas-liquid mixture F3 formed by dispersing the multiple uniform gas flows F2 into a stream of droplets from the power jet fed through the dispersion chamber 1120 is parallel to the chamber wall of the dispersion chamber 1120.
[0151] 8E illustrates an example of a power jet module configured in a dispersion chamber of a processing system in a perspective view. In one embodiment, a power jet module 1240A for injecting a liquid mixture into one or more droplet streams and directing the one or more streams into a processing system includes a power jet 1242A for injecting a liquid mixture provided to the power jet module 1240A into one or more droplet streams. The power jet module 1240A further includes a support frame 1244A for supporting movement of the power jet 1242A, a first module actuator 1246A for moving the power jet to correspond to and connect with an opening of the dispersion chamber, and a connector 1245A for connecting the first module actuator 1246A and the power jet 1242A.
[0152] In Figure 8E, the dispersion chamber 1220 comprises one or more openings 1222A, 1222B, 1222C disposed in a chamber wall of the dispersion chamber 1220 and adapted to connect to and mount to a power jet of a power jet module on one side of the power jet with nozzle array. In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Figure 8E, where the one or more openings are rectangular with a width at the bottom less than the length of the sides, and are disposed adjacent to each other at an equal distance on the same vertical line of the chamber wall of the dispersion chamber 1220.
[0153] As shown in FIG. 8E, the dispersion chamber 1220 is filled with a plurality of integrated gases F2 sent from the buffer chamber of the processing chamber. In one embodiment, simultaneously with the formation of the droplet stream in the dispersion chamber 1220 ejected from the power jet of the power jet module, the plurality of integrated gases F2 are sent into the dispersion chamber 1220 to carry the droplet stream through the dispersion chamber 1220, which may or may not remove moisture from the mist, and form a gas-liquid mixture of F3 including the liquid mixture and the plurality of integrated gases. Also, the flow of the plurality of integrated gases F2 can be sent into the dispersion chamber 1220 before the droplet stream is formed, to fill the internal volume of the dispersion chamber 1220, and optionally preheat it to a first temperature before generating the droplet stream in the dispersion chamber 1220.
[0154] One or more openings 1222A-1222C may be located near the left end of the horizontally oriented dispersion chamber 1220 (e.g., a tube dispersion chamber, etc.) and may be fitted with a power jet module for injecting a stream of droplets into the dispersion chamber 1220 and passing the stream from one end of the dispersion chamber to the other. Alternatively, one or more openings 1222A-1222C may be located near the right end of the horizontally oriented dispersion chamber 1220 and may be fitted with a power jet module for injecting a stream of droplets upwardly into the dispersion chamber over the length of the residence time of the stream generated therein. In one embodiment, the dispersion chamber itself is maintained at a first temperature.
[0155] The direction of the multiple uniform gas flows F2 fed into the dispersion chamber is parallel to the chamber walls of the dispersion chamber 1220. Also, the direction of the gas-liquid mixture F3 formed by dispersing the multiple uniform gas flows F2 into a stream of droplets from the power jet fed through the dispersion chamber 1220 is parallel to the chamber walls of the dispersion chamber 1220.
[0156] 8F illustrates an example of a power jet module configured in a dispersion chamber of a processing system in a perspective view. In one embodiment, a power jet module 1340A for injecting a liquid mixture into one or more droplet streams and directing the one or more streams into a processing system includes a power jet 1342A for injecting a liquid mixture provided to the power jet module 1340A into one or more droplet streams. The power jet module 1340A further includes a support frame 1344A for supporting movement of the power jet 1342A, a first module actuator 1346A for moving the power jet to correspond to and connect with an opening of the dispersion chamber, and a connector 1345A for connecting the first module actuator 1346A and the power jet 1342A.
[0157] In Figure 8F, a dispersion chamber 1320 is disposed in the chamber wall of the dispersion chamber 1320 and adapted to connect to and mount on a power jet of a power jet module on one side of the power jet having the nozzle array, and includes one or more openings 1322A, 1322B, 1322C, 1322D, 1322E, and 1322F having a width at its base greater than the length of its sides. In one embodiment, the shape of the one or more openings and the arrangement of the one or more openings are shown in Figure 8F, where the one or more openings are rectangular with a width at their base greater than the length of their sides, and are disposed adjacent to each other at an equal distance on the same vertical line of the chamber wall.
[0158] One or more openings 1322A-1322F may be located near the left end of the horizontally oriented dispersion chamber 1220 (e.g., a tube dispersion chamber, etc.) and may be fitted with a power jet module for injecting a stream of droplets into the dispersion chamber 1320 and passing the stream from one end of the dispersion chamber to the other. Alternatively, one or more openings 1322A-1322F may be located near the right end of the horizontally oriented dispersion chamber 1320 and may be fitted with a power jet module for injecting a stream of droplets upwardly into the dispersion chamber over the length of the residence time of the stream generated therein. In one embodiment, the dispersion chamber itself is maintained at a first temperature.
[0159] The direction of the multiple uniform gas flows F2 fed into the dispersion chamber is parallel to the chamber wall of the dispersion chamber 1020. The direction of the gas-liquid mixture F3 pumped through the dispersion chamber 1020 is also parallel to the chamber wall of the dispersion chamber 1020. In another embodiment of the invention, the direction of the multiple uniform gas flows F2 fed into the dispersion chamber 1020 is different from the direction of the gas-liquid mixture F3 pumped through the dispersion chamber 1020. In another example, the direction of the multiple uniform gas flows F2 fed into the dispersion chamber is parallel to the chamber wall of the dispersion chamber 1320. The direction of the gas-liquid mixture F3 formed by dispersing the multiple uniform gas flows F2 into a stream of droplets from the power jet pumped through the dispersion chamber 1320 is also parallel to the chamber wall of the dispersion chamber 1320.
[0160] Working Example: Exemplary material compositions are shown in Table 1A (Examples #: A1-A3). a La b Zr c D1 d D2 e ...DN n O v The lithium lanthanum zirconium oxide garnet has a composition of a:b:c:d:...:n in the ratio of M LiSalt :M LaSalt:M ZrSalt :M D1Salt :M D2Salt :...;M D1Salt where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12; and D1, D2, ..., D N At least one of D1, D2, ..., D is a metal, N > 0, 0 < d < 0.8, 0 < e < 0.8, and 0 < n < 0.8; N The annealing temperature and annealing time can be controlled in the range of 700-1000°C and 7-20 hours. In one example, the solid electrolyte material of the ceramic material is a garnet-type, cubic structure, lithium lanthanum zirconium oxide material, doped or undoped with Al, Ti, Ta, Ge, etc. In another example, the solid electrolyte material of the obtained ceramic material is a garnet-type, tetragonal structure, lithium lanthanum zirconium oxide material, doped or undoped with Al, Ti, Ta, Ge, etc. In yet another example, the solid electrolyte material of the ceramic material can be Li7La3Zr2O 12 , Li7La3Zr2O 12 , Li 6.75 La3Zr 1.75 Ta 0.25 O 12 , Li 6.5 La3Zr 1.5 O 12 , Li 6.25 La3Zr2Ta 0.25 Ga 0.2 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li6.25 La3Zr2Al 0.25 O 12 Examples include:
[0161] Examples A1 to A3 in Table 1A were carried out to prepare solid electrolyte materials at annealing temperatures above 700° C., e.g., 700° C. to 1000° C., e.g., 950° C., e.g., 900° C., e.g., 850° C., e.g., 800° C., e.g., 750° C. The examples show different structures and ionic conductivities, e.g., ionic conductivities of 10 -4 S / cm or more, preferably 5x10 -4 Ultra, or 8x10 -4 More than S / cm or 1.0x10 -3 Ultra, or 4x10 -3 Super S / cm, 5x10 -3 S / cm super, 6x10 -3 More than S / cm, preferably 7x10 -3 More than S / cm, preferably 8x10 -3 More than S / cm, preferably 9x10 -3 It is over S / cm.
[0162] [Table 1A]
[0163] Exemplary material compositions are shown in Table 1B (Examples #: B1-B3). a La b Zr c D1 d D2 e ...DN n O v The lithium lanthanum zirconium oxide garnet has a composition of a:b:c:d:...:n in the ratio of M LiSalt :M LaSalt :M ZrSalt :M D1Salt :M D2Salt :...;M DNSalt where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D1, D2, …, D NAt least one of the above is a metal, and N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8. The annealing temperature and annealing time can be controlled in the range of 1000-1200°C and 7-20 hours. In one example, the solid electrolyte material of the ceramic material is a garnet-type, cubic phase lithium lanthanum zirconium oxide material. In another example, the solid electrolyte material is Li7La3Zr2O 12 , Li7La3Zr2O 12 , Li 6.75 La3Zr 1.75 Ta 0.25 O 12 , Li 6.5 La3Zr 1.5 Ta 0.5 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La3Zr2Al 0.25 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Ga 0.2 O 12 , Li 6.25 La3Zr2Ta 0.25 Ga 0.2 O 12 In another example, the solid electrolyte material includes Li7La3Zr2O 12 , Li7La3Zr2O 12 , Li 6.75 La3Zr 1.75 Ta 0.25 O 12 , Li 6.5 La3Zr 1.5 Ta 0.5 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Al 0.2 O 12 , Li 6.25 La3Zr2Al 0.25 O 12 , Li 6.15 La3Zr 1.75 Ta 0.25 Ga0.2 O 12 , Li 6.25 La3Zr2Ta 0.25 Ga 0.2 O 12 Examples B1 to B3 in Table 1B were carried out to prepare solid electrolyte materials at annealing temperatures above 700°C, such as 1000°C to 1200°C, such as 1050°C, such as 1080°C, such as 1100°C, such as 1200°C, such as 1150°C.
[0164] [Table 1B]
[0165] The exemplary materials in Table 1C (Examples #: C1-C6) are Li a La b D1 c D2 d ...DN n O vThe composition is a:b:c:d in the ratio M LiSalt :M LaSalt :M D1Salt :M D2Salt :M DNSalt where 4.5≦a≦7.2, 2.8≦b≦3.5, 1.5≦c≦2.5, 0≦d≦1.2, 0≦n≦1.2, and 2≦v≦12; and D1, D2, ..., D N At least one of the is a metal, and N≧1. The annealing temperature and the annealing time can be controlled in the range of 700-1200°C and 7-20 hours. Examples C1-C6 in Table 1C were carried out to prepare a solid electrolyte material at an annealing temperature above 700°C, for example 700°C-1000°C, 900°C-1200°C, for example 1050°C, for example 1080°C, for example 1100°C, for example 1200°C, for example 1150°C, for example 950°C, for example 900°C, for example 850°C, for example 800°C, for example 750°C. In one example, the solid electrolyte material of the ceramic material is a cubic crystal structure. In another example, the solid electrolyte material includes Li5La3Nb2O 12 , Li5La3Ta2O 12 , Li5La3Ti2O 12 , Li6La3Sr1Ta2O 12 , Li6La3Ba1Ta2O 12 , Li6La3Ba1Ti2O 12 , Li 1.26 La 2.24 Ti4O 12 Examples include different structures and ionic conductivities, for example, ionic conductivities of 10 -3 ~10 -4 S / cm or more.
[0166] [Table 1C]
[0167] Table 1D shows the Li a La b Ti c D1 d ...DN n O v The examples #D1 to #D6 of ceramic materials having chemical compositions of the formula: LiSalt :M LaSalt :M Tisalt :M D1Salt :...:M DNSalt The ratio of the annealing temperature and the annealing time are designed and prepared to be approximately the same as that of the annealing temperature. The annealing temperature and the annealing time can be controlled in the range of 700 to 1200°C and 7 to 20 hours. Examples D1 to D6 listed in Table 1D were carried out to prepare solid electrolyte materials at annealing temperatures above 700°C, for example, 700°C to 1000°C, 900°C to 1200°C, for example, 1050°C, for example, 1080°C, for example, 1100°C, for example, 1200°C, for example, 1150°C, for example, 950°C, for example, 900°C, for example, 850°C, for example, 800°C, for example, 750°C.
[0168] [Table 1D]
[0169] In one example, the solid electrolyte material of the ceramic material has a perovskite-type cubic crystal structure. In another example, the solid electrolyte material of the ceramic material has Li 1.36 La 2.24 Ti4O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 In another example, the solid electrolyte material of the ceramic material is a perovskite type, tetragonal crystal structure. In another example, the solid electrolyte material includes Li 1.36 La 2.24 Ti4O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2,24 Ti 3.8 Ge 0.2 O 12 In yet another example, the solid electrolyte material is a perovskite-type, hexagonal crystal structure. In another example, the solid electrolyte material includes Li 1.36 La 2.24 Ti4O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 , Li 1.72 La 2.24 Ti 3.8 Ge 0.2 O 12 Examples include different structures and ionic conductivities, for example, ionic conductivities of 10 -3 ~10 -4 S / cm or more.
[0170] [Table 1E]
[0171] Exemplary material compositions are shown in Table 1E (Examples #: E1-E6). a Al b P c D1 d ....DN n O v where 1≦a≦2, 0.2≦b≦1.5, 1.0≦c≦3.5, 0≦d≦2.0, 0≦n≦2.0, and 0.2≦v≦12; D1, D2, ..., D N At least one of the elements is a metal, N≧1, and the ratio of a:b:c:d:...:n is M Li :M Al :M P :M D1 :...:M DN are designed and prepared to have approximately the same ratio of D1, D2, …, D N At least one of the above is a metal, and N≧0. The annealing temperature and annealing time can be controlled in the range of 700-1200° C. and 7-20 hours. In one embodiment, the solid electrolyte material (e.g., lithium aluminum titanium phosphate oxide material) is a sodium superionic conductor (NASICON) type, hexagonal structure (not clear if required). In another embodiment, the solid electrolyte material includes Li 1.5 Al 0.5 Ti 1.5 P3O 12 , Li 1.4 Al 0.4 Ti 1.6 P3O 12 , Li 1.6 Al 0.6 Ti 1.4 P3O 12 , Li 1.5 Al0.5 Ge 1.5 P3O 12 , Li 1.4 Al 0.4 Ge 1.6 P3O 12 , Li 1.6 Ge 0.6 Ti 1.4 P3O 12 , and combinations thereof. Examples can show different structures and ionic conductivities, for example, ionic conductivities of 10 -3 ~10 -4 More than S / cm or 5x10 -4 Ultra, 8x10 -3 Super S / cm, 9x10 -3 It is over S / cm.
[0172] [Table 1F]
[0173] The exemplary material compositions shown in Table 1F (Examples #: F1-F6) are Li a Ge b P c D1 d ...DN n O v wherein 10≦a≦13, 0.1≦b≦2.0, 0.1≦c≦1.5, 0.1≦d≦2.0, 0.1≦n≦2.0, and 2≦v≦12; and D1, D2, ..., D N At least one of the groups is a metal (N≧0), and the ratio of a:b:c:d is M Li :M Ge :M P :M D1 :...:M DNThe annealing temperature and annealing time can be controlled in the range of 700 to 1200°C and 7 to 20 hours. In one example, the solid electrolyte material of the ceramic material is a lithium superionic conductor (LISiCON) type structure, Li 12 Ge 0.5 Al 1.0 S 0.5 P 1.0 O 12 , Li 10.59 Ge 1.58 V 0.9 P 0.53 O 12 , and combinations thereof.
[0174] The exemplary materials shown in Table 1G (Examples #G1-G6) are Li a P b O c N d wherein 1.5≦a≦4.0, 0.5≦b≦2.0, 1.0≦c≦4.0, and 0.01≦d≦2.0, and the ratio of a:b:c:d is M Li :M P :M Nt The annealing temperature and annealing time can be controlled in the range of 700 to 1200°C and 7 to 20 hours. In one embodiment, the solid electrolyte material is a lithium phosphorus oxynitride (LiPON) type having an amorphous structure, for example, Li 2.88 P 1.0 O 3.73 N 0.14 , Li 1.9 S 0.28 P 1.0 O 1.1 N 1.0 and the ionic conductivity is 10 -5 ~10 -6 >S / cm or 6×10 -6 Ultra, or 6×10 -5 >S / cm or 9×10 -5 It is over S / cm.
[0175] [Table 1G]
[0176] The exemplary materials shown in Table 2A (Examples #H1-H6) are Li a P b S c D1 d ....DN n X v where 3≦a≦16, 0.5≦b≦4.5, 3≦c≦16, 0≦d≦1.5, 0≦n≦1.5, 0≦v≦4, and D1, D2, ..., D N at least one of a:b:c:d:...:n is a metal, N>0, and X is a halogen, such that the ratio of a:b:c:d:...:n is M Li :M P :M S ::M D1 :...:M DN The annealing temperature and the annealing time can be controlled in the range of 700 to 1200°C and 7 to 20 hours. In one example, the solid electrolyte material of the sulfide material has an amorphous structure. In another example, the solid electrolyte material of the sulfide material has a cubic structure. The solid electrolyte material of the sulfide material is Li7P3S 11 , Li3P1S4, Li6P a S5Cl, Li6P1S5Br1, Li6P1S5l, Li6P1S5F1, Li7P2S8l1, Li7P2S8Br1, Li7P2S8Cl1, Li7P2S8F1, Li 15 P4S 16 Cl3, Li 14.8 , Mg 0.1 P4S 16 Cl3, Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 Ge1P2S 12 , Li 10 Si1P2S 12, Li 10 Sn1P2S 12 , Li 10 S 0.3 Sn 0.7 P2S 12 , Li 10 Al 0.3 Sn 0.7 P2S 12 , Li 11 Al1P2S 12 For example, 10 -3 Super~10 -9 S / cm, preferably 8x10 -5 S / cm or more, preferably 4x10 -3 S / cm or more, preferably 5x10 -3 S / cm or more, preferably 6x10 -3 S / cm or more, preferably 7x10 -3 S / cm or more, preferably 8x10 -3 More than S / cm, preferably 9x10 -3 It has an ionic conductivity of over S / cm.
[0177] [Table 2A]
[0178] The exemplary material compositions in Table 2B (Examples #11-16) are Li a P b S c wherein 3≦a≦16, 0.5≦b≦4.5, and 3≦c≦16, and the ratio of a:b:c: is M Li :M P :M SThe ratio of is designed and prepared to be approximately the same as that of the annealing temperature. The annealing temperature and the annealing time can be controlled in the range of 700 to 1200°C and 7 to 20 hours. Examples 11 to 16 listed in Table 2B were carried out to prepare a solid electrolyte material at an annealing temperature exceeding 700°C, for example, 700°C to 1000°C, 900°C to 1200°C, for example, 1050°C, for example, 1080°C, for example, 1100°C, for example, 1200°C, for example, 1150°C, for example, 950°C, for example, 900°C, for example, 850°C, for example, 800°C, for example, 750°C.
[0179] [Table 2B]
[0180] In one example, the solid electrolyte material of the sulfide material is Li3PS4, Li7P3S, which has an orthorhombic or triclinic structure and has different ionic conductivities. 11 For example, the ionic conductivity is 10 -3 More than S / cm, preferably 8x10 -4 Ultra, preferably 9x10 -4 S / cm, preferably 2x10 -3 Ultra, preferably 4x10 -3 S / cm or more, preferably 5x10 -3 S / cm or more, preferably 6x10 -3 More than S / cm, preferably 7x10 -3 More than S / cm, preferably 8x10 -3 More than S / cm, preferably 9x10 -3 S / cm.
[0181] The exemplary materials shown in Table 2C (Examples #J1-J6) are Li a P b S c D1 d ...DN n O v wherein 5≦a≦16, 0.5≦b≦4.5, 3≦c≦16, 0≦d≦1.5, 0≦n≦1.5, 0≦v≦4, and the ratio of a:b:c:...:n is Li :M P :MS :M D1 :...:M DN The annealing temperature and time can be controlled at 700 to 1200°C for 7 to 20 hours. The solid electrolyte material contains Li 10 SiP2S 11.3 O 0.7 , Li 9.42 S 1.02 P 2.1 S 9.96 O 2.04 Includes:
[0182] [Table 2C]
[0183] The exemplary material compositions in Table 2D (Examples #: K1-K6) are Li a X b P c S d wherein 9≦a≦12, 0.5≦b≦1.5, 1.5≦c≦3.0, and 11≦d≦15, X is a metal, and the ratio of a:b:c:d is M Lt :M X :M P :M S The ratio of is designed and prepared to be approximately the same. The annealing temperature and annealing time can be controlled in the range of 700 to 1200 °C and 7 to 20 hours. As a solid electrolyte material of sulfide material, Li 10 GeP2S 12 , Li 10 SiP2S 12 For example, the ionic conductivity is 10 -3 ~10 -8 S / cm, preferably 5×10 -7 S / cm, preferably 8×10 -5 S / cm, preferably 9×10 -5 S / cm, preferably 5×10 -4 Over 8x10 -4 S / cm, preferably greater than 2×10 -3 More than 4x10-3 S / cm, preferably 5×10 -3 S / cm, preferably 6×10 -3 S / cm, preferably 7×10 -3 S / cm, preferably 8×10 -3 S / cm, preferably 9×10 -3 S / cm.
[0184] [Table 2D]
[0185] Tables 3-5 show the test results of the measured solid electrolyte material lithium oxide garnet (Examples #1-#3) annealed at 950°C for 8 hours. a La b Zr c Al d O v The chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt The ratios of Li:La:Zr:Al were designed and prepared to be approximately the same as those of the Al-doped LLZO materials, where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12. In one example, the test results of the measured composition ratios of Al-doped LLZO materials after annealing were observed, and the prepared M LiSalt :M LaSalt :M ZrSalt :M Alsalt For example, the ratio of Al-doped LLZO to be prepared is within the range expected from the preparation molar ratio of 6.2≦M LiSalt ≦7.2:2.8≦M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8, e.g. 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M LaSalt ≦2.95:1.5≦M ZrSalt≦2.0:0.1≦M AlSalt ≦0.25, e.g. 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.28, e.g. 6.4≦M LlSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M ZrSalt ≦2.0:0.2≦M AlSalt ≦0.29.
[0186] [Table 3]
[0187] [Table 4]
[0188] In one example, the composition of the Al-doped LLZO material tested was Li 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35 In another example, the composition of the Al-doped LLZO material tested is as shown in Table 4. 6.54 La 2.82 Zr 2.0 Al 0.24 O 12.08In yet another example, the composition of the Al-doped LLZO material tested is as shown in Table 5. 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45 The XRD results show that the Al-doped LLZO material has a cubic crystal structure. The content of each metal in the resulting Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and is in the range of 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8; for example, 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example, 6.5≦a≦6.9:2.5≦ b≦2.95: 1.5≦c≦2.0: 0.1≦d≦0.25; for example, 6.8≦a≦7.2: 2.6≦b≦3.2: 1.7≦c≦2.1: 0.2≦d≦0.3; for example, 6.9≦a≦7.1: 2.8≦b≦2.9: 1.8≦c≦2.1: 0.2≦d≦0.28; for example, 6.4≦a≦7.2: 2.6≦b≦2.98: 1.9≦c≦2.0: 0.2≦d≦0.26.
[0189] [Table 5]
[0190] Tables 6 to 8 show the test results of the solid electrolyte materials (Examples #4 to #6) annealed at 1150°C for 15 hours. a La b Zr c Al d O v The chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt The ratios of Li:La:Zr:Al were designed and prepared to be approximately the same as those of the Al-doped LLZO materials, where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12. In one example, the test results of the measured composition ratios of Al-doped LLZO materials after annealing were observed, and the prepared M LiSalt :M LaSalt :M ZrSalt :MAlsalt : within the range expected from the preparation molar ratio of M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8, e.g. 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M LaSalt ≦2.95:1.5≦M ZrSalt ≦2.0:0.1≦M AlSalt ≦0.25; for example, 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.28, e.g. 6.4≦M LiSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M ZrSalt ≦2.0:0.2≦M AlSalt ≦0.29.
[0191] [Table 6]
[0192] [Table 7]
[0193] The content of each metal in the resulting Al-doped LLZO material was analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and it was found that the content of each metal in the Al-doped LLZO material was 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8; for example, 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example, 6.5≦a≦6.9:2.5≦ b≦2.95:1.5≦c≦2.0:0.1≦d≦0.25, e.g. 6.8≦a≦7.2:2.6≦b≦3.2:1.7≦c≦2.1:0.2≦d≦0.3; e.g. 6.9≦a≦7.1:2.8≦b≦2.9:1.8≦c≦2.1:0.2≦d≦0.28; e.g. 6.4≦a≦7.2:2.6≦b≦2.98:1.9≦c≦2.0:0.2≦d≦0.26. In one example, the composition of the tested Al-doped LLZO material is Li as shown in Table 6. 6.32 La 3.2 Zr 2.0 Al 0.46 PO 12.9 In another example, the composition of the Al-doped LLZO material tested is as shown in Table 7. 6.49 La 3.28 Zr 2.0 Al 0.31 PO 12.7 The X-ray diffraction results show a cubic crystal structure. In yet another example, the composition of the Al-doped LLZO material tested is as shown in Table 8. 6.27 La 3.22 Zr 2.0 Al 0.3 O 12.39 and the XRD results show a cubic crystal structure.
[0194] [Table 8]
[0195] Table 9 shows the test results of the measured solid electrolyte material (Example #7) annealed at 1050° C. for 8 hours. a La b Zr c Al d O vThe chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt The ratios of Li:La:Zr:Al were designed and prepared to be approximately the same as those of the Al-doped LLZO materials, where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12. In one example, the test results of the measured composition ratios of Al-doped LLZO materials after annealing were observed, and the prepared M LiSalt :M LaSalt :M ZrSalt :M Alsalt : within the range expected from the preparation molar ratio; for example, 6.2≦M LiSalt ≦7.2:2.8≦M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8, e.g. 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M LaSalt ≦2.95:1.5≦M ZrSalt ≦2.0:0.1≦M AlSalt ≦0.25, e.g. 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.28; for example, 6.4≦M LiSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M ZrSalt ≦2.0:0.2≦M AlSalt ≦0.29.
[0196] The content of each metal in the resulting Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and is found to be 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8, for example 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example 6.5≦a≦6.9:2.5≦ b≦2.95:1.5≦c≦2.0:0.1≦d≦0.25; for example, 6.8≦a≦7.2:2.6≦b≦3.2:1.7≦c≦2.1:0.2≦d≦0.3; for example, 6.9≦a≦7.1:2.8≦b≦2.9:1.8≦c≦2.1:0.2≦d≦0.28, for example, 6.4≦a≦7.2:2.6≦b≦2.98:1.9≦c≦2.0:0.2≦d≦0.26. In one example, the composition of the Al-doped LLZO material tested was Li 6.4 La 2.86 Zr 2.0 Al 0.24 PO 11.98 and the XRD results show a cubic crystal structure.
[0197] [Table 9]
[0198] Tables 10-11 show the test results of the measured solid electrolyte materials (Examples #8-9) annealed at 850°C for 8 hours. a La b Zr c Al d O v The chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12.
[0199] In one example, the test results of the measured composition ratio of Al-doped LLZO material of Li:La:Zr:Al after annealing were observed, and the prepared M LiSalt :M LaSalt :MZrSalt :M Alsalt : within the range expected from the preparation molar ratio; for example, 6.2≦M LiSalt ≦7.2:2.8≦M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8; for example, 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M Lasalt ≦2.95:1.5≦M Zr Salt≦2.0:0.1≦M AlSalt ≦0.25; for example, 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.28, e.g. 6.4≦M LiSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M ZrSalt ≦2.0:0.2≦M AlSalt ≦0.29.
[0200] The content of each metal in the resulting Al-doped LLZO material is analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and is found to be 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8, for example 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example 6.5≦a≦6.9:2.5≦ b≦2.95:1.5≦c≦2.0:0.1≦d≦0.25; for example, 6.8≦a≦7.2:2.6≦b≦3.2:1.7≦c≦2.1:0.2≦d≦0.3; for example, 6.9≦a≦7.1:2.8≦b≦2.9:1.8≦c≦2.1:0.2≦d≦0.28, for example, 6.4≦a≦7.2:2.6≦b≦2.98:1.9≦c≦2.0:0.2≦d≦0.26.
[0201] [Table 10]
[0202] [Table 11]
[0203] In one example, the composition of the Al-doped LLZO material tested was: 6.43 La 2.93 Zr 2.0 Al 0.24 O 12.08 In another example, the composition of the Al-doped LLZO material tested is as shown in Table 11. 6.57 La 2.99 Zr 2.0 Al 0.22 O 12.22 and the XRD results indicate a cubic crystal structure.
[0204] Tables 12-13 show the test results of the measured solid electrolyte materials (Examples #10-11) annealed at 900°C for 8 hours. a La b Zr c Al d O v The chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12.
[0205] [Table 12]
[0206] [Table 13]
[0207] In one example, the test results of the measured composition ratio of Al-doped LLZO material of Li:La:Zr:Al after annealing were observed, and the prepared M LiSalt :M LaSalt :M ZrSalt :M Alsalt : within the range expected from the preparation molar ratio; for example, 6.2≦M LiSalt ≦7.2:2.8≦M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8; for example, 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M Lasalt ≦2.95:1.5≦M ZrSalt ≦2.0:0.1≦M AlSalt ≦0.25; for example, 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.28, e.g. 6.4≦M LiSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M ZrSalt ≦2.0:0.2≦M AlSalt ≦0.29.
[0208] The content of each metal in the resulting Al-doped LLZO material was analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and it was found that the content of each metal in the Al-doped LLZO material was 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8; for example, 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example, 6.5≦a≦6.9:2.5≦ b≦2.95:1.5≦c≦2.0:0.1≦d≦0.25; for example, 6.8≦a≦7.2:2.6≦b≦3.2:1.7≦c≦2.1:0.2≦d≦0.3; for example, 6.9≦a≦7.1:2.8≦b≦2.9:1.8≦c≦2.1:0.2≦d≦0.28, for example, 6.4≦a≦7.2:2.6≦b≦2.98:1.9≦c≦2.0:0.2≦d≦0.26.
[0209] In one example, the composition of the Al-doped LLZO material tested was: 6.25 La 3.01 Zr 2.0 Al 0.22 O 11.92 In another example, the composition of the Al-doped LLZO material tested is as shown in Table 13: 6.49 La 3.02 Zr 2.0 Al 0.23 O 12.2 and the XRD results show a cubic crystal structure.
[0210] Table 14 shows the test results of the measured solid electrolyte materials (Examples #B1-B3) annealed at 1100°C for 6 hours. a La b Zr c Al d O v The chemical composition is a:b:c:d, and the ratio of a:b:c:d is M LiSalt :M LaSalt :M ZrSalt :M Alsalt where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, and 2.0≦v≦12.
[0211] In one example, the test results of the measured composition ratio of Al-doped LLZO material of Li:La:Zr:Al after annealing were observed, and the prepared M LiSalt :M LaSalt :M ZrSalt :M Alsalt : within the range expected from the preparation molar ratio; for example, 6.2≦M LiSalt ≦7.2:2.8≦M LaSalt ≦3.5:1.0≦M ZrSalt ≦2.2:0≦M AlSalt ≦0.8; for example, 6.4≦M LiSalt ≦6.9:2.4≦M LaSalt ≦3.0:1.3≦M ZrSalt ≦2.0:0≦M AlSalt ≦0.5, for example 6.5≦M LiSalt ≦6.9:2.5≦M Lasalt ≦2.95:1.5≦M Zr Salt≦2.0:0.1≦M AlSalt ≦0.25, e.g. 6.8≦M LiSalt ≦7.2:2.6≦M LaSalt ≦3.2:1.7≦M ZrSalt ≦2.1:0.2≦M AlSalt ≦0.3, e.g. 6.9≦M LiSalt ≦7.1:2.8≦M LaSalt ≦2.9:1.8≦M Zr Salt≦2.1:0.2≦M AlSalt ≦0.28; for example, 6.4≦M LiSalt ≦7.2:2.6≦M LaSalt ≦2.98:1.9≦M Zr Salt≦2.0:0.2≦M AlSalt < 0.29.
[0212] The content of each metal in the resulting Al-doped LLZO material was analyzed by an inductively coupled plasma ("ICP") analyzer after the annealing process, and it was found that the content of each metal in the Al-doped LLZO material was 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8; for example, 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5, for example, 6.5≦a≦6.9:2.5≦ b≦2.95:1.5≦c≦2.0:0.1≦d≦0.25; for example, 6.8≦a≦7.2:2.6≦b≦3.2:1.7≦c≦2.1:0.2≦d≦0.3; for example, 6.9≦a≦7.1:2.8≦b≦2.9:1.8≦c≦2.1:0.2≦d≦0.28, for example, 6.4≦a≦7.2:2.6≦b≦2.98:1.9≦c≦2.0:0.2≦d≦0.26.
[0213] [Table 14]
[0214] The content of Al-doped LLZO after the second annealing process to sinter the electrolyte material into pellets is 6.2≦a≦7.2:2.8≦b≦3.5:1.0≦c≦2.2:0≦d≦0.8; for example, 6.4≦a≦6.9:2.4≦b≦3.0:1.3≦c≦2.0:0≦d≦0.5; for example, 6.5≦a≦6.9:2.5≦b≦2.95:1 0.5≦c≦2.0: 0.1≦d≦0.25; for example 6.8≦a≦7.2: 2.6≦b≦3.2: 1.7≦c≦2.1: 0.2≦d≦0.3; for example 6.9≦a≦7.1: 2.8≦b≦2.9: 1.8≦c≦2.1: 0.2≦d≦0.28; for example 6.4≦a≦7.2: 2.6≦b≦2.98: 1.9≦c≦2.0: 0.2≦d≦0.26. Compared to the first annealing process for producing a solid electrolyte material, it can be observed that there is an increase in lithium content (an increase of about 3% to 6%) after the second annealing process (for example: sintered electrolyte material).
[0215] Table 15 shows the tap density (TD), average particle size D of the solid electrolyte material after the annealing process of the exemplary solid electrolytes (Examples 20 to 25). 50 , D 10 , D 90 , D1, D 99 The test results of the , and SPAN values are shown. To obtain an ideal lithium solid electrolyte material with high discharge capacity, excellent cycle performance, and high volumetric energy density, it is necessary to precisely control the morphology and tap density of the material during the fabrication process. In one embodiment, the Li a La b Zr c D1 d D2 e ....DN n O v where 6.2≦a≦7.2, 2.8≦b≦3.5, 1.0≦c≦2.0, 2.0≦v≦12, and D1, D2, …, D N At least one of them is a metal, and N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8. The annealing temperature and the annealing time can be controlled within the ranges of 700 to 1200° C. and 7 to 20 hours.
[0216] [Table 15]
[0217] The tap density ("TD") of the obtained solid electrolyte is found to be greater than 0.8g / ml, preferably greater than 0.9g / ml, preferably greater than 1.0g / ml, preferably greater than 1.09g / ml, preferably greater than 1.15g / ml, preferably greater than 1.2g / ml, preferably greater than 1.3g / ml, preferably greater than 1.4g / ml, preferably greater than 1.5g / ml, preferably greater than 1.6g / ml, preferably greater than 1.7g / ml, preferably greater than 1.8g / ml, preferably greater than 1.9g / ml, preferably greater than 2.0g / ml, which can be attributed to the uniform distribution of particles with good packing properties.
[0218] For example, a solid electrolyte material annealed at 850° C. for a period of time (e.g., 6-12 hours) exhibits a tap density ("TD") of greater than 1.0 g / ml, preferably greater than 1.1 g / ml, preferably greater than 1.15 g / ml. In another example, a solid electrolyte material annealed at 900° C. for a period of time (e.g., 6-12 hours) exhibits a tap density ("TD") of greater than 1.1 g / ml, preferably greater than 1.15 g / ml, preferably greater than 1.18 g / ml, preferably greater than 1.2 g / ml.
[0219] For example, a solid electrolyte material annealed at 1050°C for a period of time (e.g., 6 to 12 hours) exhibits a tap density ("TD") of greater than 1.2 g / ml, preferably greater than 1.3 g / ml, preferably greater than 1.35 g / ml, preferably greater than 1.4 g / ml, also preferably greater than 1.45 g / ml, preferably greater than 1.5 g / ml, and preferably greater than 1.55 g / ml.
[0220] Another observation was that the SPAN value (D 90 -D 10 ) / D 50 is less than 1.7, preferably less than 1.6, preferably less than 1.5, preferably less than 1.4, preferably less than 1.3, preferably less than 1.2, preferably less than 1.1, preferably less than 1.0, preferably less than 0.9, preferably less than 0.8. In one embodiment, the SPAN value of the solid electrolyte material is 0.8≦SPAN≦1.7, 0.8≦SPAN≦1.4, such as 0.8≦SPAN≦1.6, 0.8≦SPAN≦1.5. In another embodiment, the SPAN value of the solid electrolyte material is 0.9≦SPAN≦1.65. In yet another embodiment, the SPAN value of the solid electrolyte material is 1.1≦SPAN≦1.65, such as 1.2≦SPAN≦1.65, such as 1.3≦SPAN≦1.65, such as 1.4≦SPAN≦1.65, such as 1.5≦SPAN≦1.65, such as 1.1≦SPAN≦1.3.
[0221] In another embodiment, the SPAN value of the solid electrolyte material does not change dramatically with the process of different annealing temperatures. Furthermore, the D 90can be obtained by controlling the diameter to 20 μm to 40 μm; for example, 25 μm to 40 μm; for example, 25 μm to 38 μm; for example, 28 μm to 38 μm; for example, 30 μm to 38 μm; for example, 31 μm to 38 μm; for example, 25 μm to 36 μm; for example, 25 μm to 33 μm; for example, 25 μm to 31 μm; for example, 26 μm to 31 μm.
[0222] Furthermore, the solid electrolyte material D 50 can be obtained by controlling the thickness to 10 μm to 18 μm, less than 18 μm, for example, 10 μm to 15 μm, for example, 10 μm to 14 μm, for example, 11 μm to 17 μm, for example, 11 μm to 16 μm; for example, 12 μm to 17 μm; for example, 12 μm to 16 μm; for example, 13 μm to 16 μm; for example, 14 μm to 16 μm; for example, 11 μm to 15 μm; for example, 10 μm to 14 μm; for example, 10 μm to 13 μm.
[0223] Furthermore, the solid electrolyte material D 10 is 3 μm to 10 μm; for example, 3 μm to 9 μm; for example, 3 μm to 8 μm; for example, 3 μm to 7 μm; for example, 3 μm to 6 μm; for example, 4 μm to 10 μm; for example, 4 μm to 9 μm; for example, 4 μm to 8 μm; for example, 4 μm to 7 μm; for example, 4 μm to 6 μm; for example, 5 μm to 9 μm; for example, 5 μm to 8 μm. Furthermore, D1 of the solid electrolyte material is 0.1 μm to 3 μm; for example, 0.1 μm to 3 μm; for example, 0.15 μm to 3 μm; for example, 0.2 μm to 3 μm; for example, 0.3 μm to 3 μm; for example, 0.4 μm to 3 μm; for example, 0.5 μm to 3 μm; for example, 0.3 μm to 2 μm; for example, 0.3 μm to 1 μm; for example, 0.2 μm to 1 μm; for example, 0.2 μm to 2 μm; for example, 0.25 μm to 1 μm.
[0224] Furthermore, the solid electrolyte material D 99 is 35 μm to 60 μm, for example, 35 μm to 58 μm, for example, 35 μm to 55 μm, for example, 38 μm to 59 μm, for example, 40 μm to 56 μm, for example, 43 μm to 54 μm, for example, 40 μm to 53 μm, for example, 41 μm to 58 μm, for example, 42 μm to 59 μm, for example, 43 μm to 52 μm, for example, 45 μm to 60 μm, for example, 50 μm to 60 μm.
[0225] Example 20 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 1050° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 21 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 850° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 22 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 900° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 23 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 900° C. for 6 hours. 50 , D 10 , D 90 , D1, D 99 The results are shown in FIG.
[0226] Example 24 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 900° C. for 10 hours. 50 , D 10 , D 90 , D1, D 99, and SPAN values are shown in FIG. 15. Example 25 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 850° C. for 12 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 26 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 850° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 27 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 900° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 , and SPAN values are shown in FIG. 15. Example 28 shows the tap density (TD), average particle size D of the measured solid electrolyte material or an exemplary composition of aluminum doped lithium lanthanum zirconium oxide annealed at 1050° C. for 8 hours. 50 , D 10 , D 90 , D1, D 99 The results are shown in FIG.
[0227] 9 shows the X-ray diffraction ("XRD") patterns of aluminum doped lithium lanthanum zirconium oxide materials ("LLZO") for Example #41, Example #42, Example #43, Example #44, Example #45, Example #46, and the reference showing a garnet-type cubic crystal. The XRD patterns of the solid electrolyte materials of Example 41, Example 42, Example 43, Example 44, Example 45, and Example 46 show a garnet-type cubic phase of the solid electrolyte material. The solid electrolyte material includes a high lithium ion (Li+) conducting phase with an XRD pattern that peaks exactly at all 2θ angles of the cubic crystal structure of the reference material.
[0228] The XRD patterns of doped lithium lanthanum zirconium oxide fine powders synthesized at different temperatures are shown in Figure 10. Example 41 shows the diffraction peaks of doped lithium lanthanum zirconium oxide material powders synthesized at 850°C for 8 hours. As shown in Example 41, the XRD pattern of lithium lanthanum zirconium oxide material synthesized at 800°C is similar to that of a commercial reference sample of cubic LLZO form, indicating that the formation of garnet-type cubic phase LLZO has been achieved at a temperature of 800°C using the present invention.
[0229] Furthermore, the results of Example 41 show that cubic phase Al-doped LLZO was formed, and the characteristic diffraction peaks of tetragonal phase LLZO were not detected. It should be noted that cubic phase LLZO exhibits better ionic conductivity than tetragonal phase LLZO.
[0230] Example 42 shows the diffraction peaks of doped LLZO powder synthesized at 850°C for 8 hours. The XRD pattern of the synthesized doped LLZO at 900°C shown in Example 42 is similar to that of a commercial reference sample of cubic doped LLZO form, indicating that the formation of garnet-type cubic LLZO at a temperature of 900°C was achieved using the present invention. In Example 42, it is observed that the cubic crystal structure of FIG. 10 is consistent with the commercial reference sample. Furthermore, the results of Example 42 show that a cubic garnet structure of doped LLZO was formed, and no diffraction peaks characteristic of a tetragonal crystal structure were detected.
[0231] Example 43 shows the diffraction peaks of doped LLZO powder synthesized at 950° C. for 8 hours. The XRD pattern of LLZO synthesized at 950° C. shown in Example 43 is similar to that of a commercial reference sample of cubic phase LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 950° C. using the present invention. Furthermore, the results of Example 43 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0232] Example 44 shows the diffraction peaks of doped LLZO powder synthesized at 1000° C. for 8 hours. The XRD pattern of the doped LLZO synthesized at 1000° C. shown in Example 44 is similar to that of a commercial reference sample of cubic doped LLZO form, indicating that the formation of garnet-type cubic phase LLZO was achieved at a temperature of 1000° C. using the present invention. Furthermore, the results of Example 44 show that cubic phase LLZO was formed and no characteristic diffraction peaks of tetragonal phase LLZO were detected.
[0233] Example 45 shows the diffraction peaks of doped LLZO powder synthesized at 1050° C. for 8 hours. The XRD pattern of the doped LLZO synthesized at 1050° C. shown in Example 45 is similar to that of a commercial reference sample of cubic phase LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 1050° C. using the present invention. Furthermore, the results of Example 45 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0234] Example 46 shows the diffraction peaks of doped LLZO powder synthesized at 1100° C. for 8 hours. The XRD pattern of the doped LLZO synthesized at 1100° C. shown in Example 46 is similar to that of a commercial reference sample of cubic doped LLZO form, indicating that the formation of garnet-type cubic doped LLZO was achieved at a temperature of 1100° C. using the present invention. Furthermore, the results of Example 46 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0235] 10 shows the XRD patterns of aluminum (Al) doped lithium lanthanum zirconium oxide materials (LLZO) for Examples 51, 52, 53, 54, and the reference showing garnet-type cubic crystals. The XRD patterns of the solid electrolyte materials of Examples 51, 52, and 53 all show garnet-type cubic crystal solid electrolyte materials.
[0236] XRD patterns of Al-doped LLZO fine powders synthesized at the same temperature of 900 ° C for different times (6 hours to 12 hours) are shown in FIG. 11. Example 51 shows the diffraction peaks of LLZO powders synthesized at 900 ° C for 6 hours. The XRD pattern of Al-doped LLZO synthesized at 900 ° C shown in Example 51 is similar to that of a commercial reference sample of cubic LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 900 ° C for 6 hours using the present invention. Furthermore, the results of Example 51 show that cubic phase LLZO was formed, and no diffraction peaks characteristic of tetragonal phase LLZO were detected. Example 52 shows the diffraction peaks of LLZO powders synthesized at 900 ° C for 8 hours. The XRD pattern of Al-doped LLZO synthesized at 900 ° C for 8 hours shown in Example 52 is similar to that of a commercial reference sample of cubic LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 900 ° C for 8 hours using the present invention. Furthermore, the results of Example 52 show that cubic phase LLZO was formed, and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0237] Example 53 shows the diffraction peaks of LLZO powder synthesized at 900° C. for 10 hours. The XRD pattern of Al-doped LLZO synthesized at 900° C. for 10 hours shown in Example 53 is similar to that of a commercial reference sample of cubic LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 900° C. for 10 hours using the present invention. Furthermore, the results of Example 53 show that cubic phase LLZO was formed, and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0238] Example 54 shows the diffraction peaks of LLZO powder synthesized at 900° C. for 12 hours. The XRD pattern of Al-doped LLZO synthesized at 900° C. for 12 hours shown in Example 54 is similar to that of a commercial reference sample of cubic LLZO form, indicating that the formation of garnet-type cubic LLZO was achieved at a temperature of 900° C. for 12 hours using the present invention. Furthermore, the results of Example 54 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0239] FIG. 11 shows the XRD patterns of aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) material of Example 61 and references showing garnet-type cubic phase solid electrolyte material. The XRD pattern of LLZO fine powder synthesized at 850°C for 8 hours is shown in FIG. 11. Example 61 shows the diffraction peaks of Al-doped LLZO powder synthesized at 850°C for 8 hours. The XRD pattern of LLZO synthesized at 850°C shown in Example 61 is similar to that of an academic (or literature) reference sample of cubic phase LLZO form, indicating that the formation of garnet-type cubic phase LLZO was achieved at a temperature of 850°C using the present invention. Furthermore, the results of Example 61 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0240] FIG. 12 shows the XRD patterns of aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) material of Example 62 and references showing garnet-type cubic phase solid electrolyte material. The XRD pattern of LLZO fine powder synthesized at 900° C. for 8 hours is shown in FIG. 12. Example 62 shows the diffraction peaks of Al-doped LLZO powder synthesized at 900° C. for 8 hours. The XRD pattern of LLZO synthesized at 900° C. shown in Example 62 is similar to that of an academic (or literature) reference sample of cubic phase LLZO form, indicating that the formation of garnet-type cubic phase LLZO was achieved at a temperature of 900° C. using the present invention. Furthermore, the results of Example 62 show that cubic phase LLZO was formed and no diffraction peaks characteristic of tetragonal phase LLZO were detected.
[0241] FIG. 13 shows the XRD patterns of the lithium lanthanum zirconium oxide material (LLZO) of Example 71 and the commercial samples as references #1 and #2 as the garnet-type tetragonal phase of the solid electrolyte material. The XRD pattern of the LLZO fine powder synthesized at 900° C. for 8 hours is shown in FIG. 13. Example 71 shows the diffraction peaks of the lithium lanthanum zirconium oxide material powder synthesized at 900° C. for 8 hours. The XRD pattern of the LLZO synthesized at 900° C. shown in Example 71 is similar to that of the academic (or literature) reference sample of the cubic LLZO form, indicating that the formation of the garnet-type tetragonal phase LLZO at a temperature of 900° C. has been achieved using the present invention.
[0242] Figures 14A, 14B, and 14C are SEM images of examples of solid particles of solid electrolyte material after annealing process. Figures 14A, 14B, and 14C show SEM images of aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) after annealing at 850°C for 8 hours, 900°C for 8 hours, and 1050°C for 8 hours, respectively. One observation can be seen that the annealing temperature does not have a significant effect on the morphology and crystal structure of aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO). Furthermore, Figures 14A, 14B, and 14C show that the lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) particles appears to have sizes estimated to be in the range of 1 μm to 100 μm; for example, 10 μm to 20 μm; for example, 10 μm to 90 μm; for example, 10 μm to 50 μm; for example, 10 μm to 40 μm; for example, 10 nm to 70 μm; for example, 20 nm to 80 μm; for example, 20 nm to 60 μm; for example, 20 nm to 50 μm; for example, 30 nm to 70 μm; for example, 20 nm to 50 μm; for example, 40 nm to 70 μm; for example, 50 nm to 70 μm; for example, 10 μm to 30 μm; for example, 15 μm to 40 μm; for example, 20 μm to 40 μm; for example, 30 μm to 60 μm.
[0243] In one example shown in Figure 14A, a lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) particles 1410 has a wire-like morphology. In another example shown in Figure 14B, a lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) particles 1420 has an irregular cluster-shaped morphology, and in another example shown in Figure 14C, a lithium lanthanum zirconium oxide material (LLZO) doped with aluminum (Al) particles 1430 has a spherical cluster morphology, which results in a spherical morphology. From these observations, it can be seen that the wire-like morphology at the low annealing temperature in 14A is broken at the high annealing temperature to form a cluster of wire-like morphologies shown in 14C, resulting in the wire-like morphologies being connected.
[0244] 15A and 15B are SEM images of example solid particles of a solid electrolyte material after an annealing process. 12 FIG. 15B shows an SEM image of a lithium lanthanum zirconium oxide material (LLZO) having a chemical composition of 1500° C. after annealing for 8 hours at 1050° C. Additionally, FIG. 15B shows a magnified view of FIG. 15A. Additionally, FIG. 15B shows the LLZO material at a higher magnification, where the morphology of the LLZO material can be clearly seen. In one example shown in FIG. 15B, a single lithium lanthanum zirconium oxide material (LLZO) particle 1510 has a wire-like morphology. Further, Figures 15A and 15B show that the lithium lanthanum zirconium oxide material (LLZO) particles appear to have a size estimated to be in the range of 1 μm to 100 μm; for example, 10 μm to 20 μm; for example, 10 μm to 90 μm; for example, 10 μm to 50 μm; for example, 10 μm to 40 μm; for example, 10 μm to 70 μm; for example, 20 μm to 80 μm; for example, 20 μm to 60 μm; for example, 20 μm to 50 μm; for example, 30 μm to 70 μm; for example, 20 μm to 50 μm; for example, 40 μm to 70 μm; for example, 50 μm to 70 μm; for example, 10 μm to 30 μm; for example, 15 μm to 40 μm; for example, 20 μm to 40 μm; for example, 30 μm to 60 μm, etc.
[0245] 16A and 16B are SEM images of examples of solid particles of solid electrolyte material after annealing process. FIG. 16A and FIG. 16B show SEM images of aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) after annealing at 1050° C. for 8 hours. FIG. 16B shows a magnified view of FIG. 16A. FIG. 16B shows LLZO particles at a higher magnification, and the size and shape of LLZO particles can be clearly seen. As shown in FIG. 16A and FIG. 16B, each LLZO particle can aggregate to form a spherical network, which can enhance the ionic conductivity of the bulk material. The LLZO particles appear to have a spherical shape with sizes estimated to be in the range of 1 μm to 100 μm; for example, 10 μm to 20 μm; for example, 10 μm to 90 μm; for example, 10 μm to 50 μm; for example, 10 μm to 40 μm; for example, 10 μm to 70 μm; for example, 20 μm to 80 μm; for example, 20 μm to 60 μm; for example, 20 μm to 50 μm; for example, 30 μm to 70 μm; for example, 20 μm to 50 μm; for example, 40 μm to 70 μm; for example, 50 μm to 70 μm; for example, 10 μm to 30 μm; for example, 15 μm to 40 μm; for example, 20 μm to 40 μm; for example, 30 μm to 60 μm. As shown in Figures 16A and 16B, it can be seen that the lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1610 exhibits a morphology of spherical clusters. This example is shown in a magnified view in Figure 16B, where the lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1620 exhibits a predominantly wire-like morphology. Furthermore, the wire-like lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material are interconnected to form secondary clusters.
[0246] 17A-17D are SEM images of example solid particles of solid electrolyte material after an annealing process. 6.76 La 2.87 Zr 2.0 Al 0.24 O 12.35FIG. 17B shows an SEM image of an aluminum (Al)-doped lithium lanthanum zirconium oxide material (LLZO) after annealing at 950° C. for 8 hours, with reference to Example 1 having the composition of 6.74 La 2.96 Zr 2.0 Al 0.25 O 12.45 1 shows an SEM image of an aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) after annealing at 950° C. for 8 hours, with reference to Example 3 having the composition: In Figures 17A and 17B, the Al doped LLZO particles appear to have a spherical shape with sizes estimated to be in the range of 1 µm to 100 µm; for example, 10 µm to 20 µm; for example, 10 µm to 90 µm; for example, 10 µm to 50 µm; for example, 10 µm to 40 µm; for example, 10 nm to 70 µm; for example, 20 nm to 80 µm; for example, 20 nm to 60 µm; for example, 20 nm to 50 µm; for example, 30 nm to 70 µm; for example, 20 nm to 50 µm; for example, 40 nm to 70 µm; for example, 50 nm to 70 µm; for example, 10 µm to 30 µm; for example, 15 µm to 40 µm; for example, 20 µm to 40 µm; for example, 30 µm to 60 µm, etc. Further, as shown in Figure 17A, observations can show that lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1710 exhibits the morphology of spherical clusters. In another example shown in Figure 17B, another observation can show that lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1720 exhibits the morphology of spherical clusters.
[0247] FIG. 17C shows the Li 6.57 La 2.99 Zr 2.0 Al 0.22 O 12.2217C shows an SEM image of lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) after annealing at 850° C. for 8 hours, with reference to Example 9 having a composition of 17C. Furthermore, as shown in FIG. 17C, the observation can show that lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1730 exhibits the morphology of spherical clusters. In FIG. 17C, the Al doped LLZO particles appear to have a spherical shape with sizes estimated to be in the range of 1 μm to 100 μm; for example, 10 μm to 20 μm; for example, 10 μm to 90 μm; for example, 10 μm to 50 μm; for example, 10 μm to 40 μm; for example, 10 μm to 70 μm; for example, 20 μm to 80 μm; for example, 20 μm to 60 μm; for example, 20 μm to 50 μm; for example, 30 μm to 70 μm; for example, 20 μm to 50 μm; for example, 40 μm to 70 μm; for example, 50 μm to 70 μm; for example, 10 μm to 30 μm; for example, 15 μm to 40 μm; for example, 20 μm to 40 μm; for example, 30 μm to 60 μm, etc.
[0248] FIG. 17D shows the Li 6.49 La 3.02 Zr 2.0 Al 0.23 O 12.21 shows an SEM image of an aluminum (Al) doped lithium lanthanum zirconium oxide material (LLZO) after annealing at 900° C. for 8 hours, with reference to Example 11 having the composition: As shown in FIG. 17D, the Al doped LLZO particles appear to have a spherical shape with sizes estimated to be in the range of 1 μm to 100 μm; for example, 10 μm to 20 μm; for example, 10 μm to 90 μm; for example, 10 μm to 50 μm; for example, 10 μm to 40 μm; for example, 10 μm to 70 μm; for example, 20 μm to 80 μm; for example, 20 μm to 60 μm; for example, 20 μm to 50 μm; for example, 30 μm to 70 μm; for example, 20 μm to 50 μm; for example, 40 μm to 70 μm; for example, 50 μm to 70 μm; for example, 10 μm to 30 μm; for example, 15 μm to 40 μm; for example, 20 μm to 40 μm; for example, 30 μm to 60 μm, etc. In another example shown in FIG. 17D, another observation can be seen that lithium lanthanum zirconium oxide (LLZO) doped with aluminum (Al) material 1740 exhibits the morphology of spherical clusters.
[0249] Table 16 shows the test results of the electric capacity and coulombic efficiency (CE) of the battery cell examples (Examples #30-35) fabricated by the solid electrolyte material after the annealing process. The annealing temperature and annealing time can be controlled in the range of 700-1200°C and 7-20 hours. In Table 16, the battery made by the lithium lanthanum zirconium oxide material (LLZO) particles appears to have different charge / discharge capacity cycle performance at different current / weight (mA / g), where 1C rate is equivalent to 200mA / g. In one example, the charging capacity is in the range of 210 (mAh / g) to 255 (mAh / g), for example, 215 (mAh / g) to 255 (mAh / g), for example, 225 (mAh / g) to 255 (mAh / g), for example, 235 (mAh / g) to 255 (mAh / g), for example, 245 (mAh / g) to 255 (mAh / g). In another example, the charge capacity is greater than 205 (mAh / g), preferably greater than 210 (mAh / g), preferably greater than 215 (mAh / g), preferably greater than 220 (mAh / g), preferably greater than 225 (mAh / g), preferably greater than 230 (mAh / g), preferably greater than 235 (mAh / g), preferably greater than 240 (mAh / g), preferably greater than 245 (mAh / g), preferably greater than 250 (mAh / g), preferably greater than 255 (mAh / g). In one example, the discharge capacity is in the range of 210 (mAh / g) to 255 (mAh / g), for example, 215 (mAh / g) to 255 (mAh / g), for example, 225 (mAh / g) to 255 (mAh / g), for example, 235 (mAh / g) to 255 (mAh / g), for example, 245 (mAh / g) to 255 (mAh / g). In another example, the discharge capacity is greater than 205 (mAh / g), preferably greater than 210 (mAh / g), preferably greater than 215 (mAh / g), preferably greater than 220 (mAh / g), preferably greater than 225 (mAh / g), preferably greater than 230 (mAh / g), preferably greater than 235 (mAh / g), preferably greater than 240 (mAh / g), preferably greater than 245 (mAh / g), preferably greater than 250 (mAh / g), preferably greater than 255 (mAh / g).The coulombic efficiency (CE, %) of the obtained solid electrolyte was found to be greater than 96%, preferably greater than 96.5%, preferably greater than 97%, preferably greater than 97.5%, preferably greater than 98%, preferably greater than 98.5%, preferably greater than 99%, preferably greater than 99.5%, preferably greater than 99.6%, preferably greater than 99.7%, preferably greater than 99.8%, preferably greater than 99.9%.
[0250] [Table 16]
[0251] While the forgoing is directed to embodiments of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof, the scope of the invention being determined by the claims which follow.
Claims
1. A solid electrolyte material, comprising: Li a La b Zr c D1 d D2 e . . . DN n O v wherein 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D 1 , D 2 , … , D N is a metal, N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8; Digitally controlled stoichiometric amounts of lithium-containing salt, lanthanum-containing salt, zirconium-containing salt, and one or more metals D 1 , D 2 , . . . , D N forming a liquid mixture of one or more inorganic metal salts comprising: mixing the liquid mixture with a first gas flow to form a gas-liquid mixture and spraying a mist of the gas-liquid mixture at high velocity into a power jet chamber; drying the gas-liquid mixture for a first reaction time of less than 20 minutes by feeding a second gas stream of the heated gas to undergo one or more oxidation reactions to form a gas-solid mixture within the power jet chamber; expelling the gas-solid mixture from the power jet chamber to obtain powder particles of the ceramic material; annealing the powder particles for a second reaction time greater than two hours and undergoing a dynamic crystallization process in the presence of a third gas flow to form a crystalline product, wherein upon scanning electron microscope (SEM) analysis, the crystalline product of the ceramic material is clustered.
2. The process comprising:
10. The solid electrolyte material of claim 1, further comprising: grinding the crystalline product of the ceramic material to obtain nano-sized particles, wherein the tap density of the ceramic material is greater than 1.0 g / ml.
3. 3. The solid electrolyte material of claim 2, wherein the tap density of the ceramic material after annealing the ceramic material at greater than 900° C. for more than 8 hours is greater than 1.4 g / ml.
4. 2. The solid electrolyte material of claim 1, wherein the second gas flow includes oxygen and has a temperature of 200° C. or higher, and the gas-liquid mixture is dried by sending the second gas flow for less than 10 minutes.
5. 10. The solid electrolyte material of claim 1, wherein the powder particles are annealed in a dynamic crystallization process in the presence of oxygen gas flow.
6. 10. The solid electrolyte material of claim 1, wherein the process further comprises separating the gas-solid mixture to obtain the one or more solid particles of the ceramic material.
7. The crystalline product is a garnet-type ceramic material having a cubic crystal structure as determined by X-ray diffraction (XRD) analysis and has a measured ionic conductivity (σ) of 10 at 25° C. -4 The solid electrolyte material of claim 1 , wherein the solid electrolyte material has a viscosity greater than S / centimeter.
8. 10. The solid electrolyte material of claim 1, wherein the crystalline product is a garnet-type ceramic material having a tetragonal crystal structure as determined by X-ray diffraction (XRD) analysis.
9. D 1 , D 2 , ..., D N2. The solid electrolyte material of claim 1, wherein is selected from the group consisting of Al, Ta, Ti, Ge, Mg, Mn, Zr, Zn, Nb, Ce, Sn, Ga, Ba, Ac, Ca, Sc, V, Cr, Fe, Cu, B, As, Hf, Mo, W, Re, Ru, Rh, Pt, Ag, Os, Ir, Au, F, Cl, I, Br, and combinations thereof.
10. The ceramic material is Li 7 La 3 Zr 2 O 12 , Li doped with one or more metals 7 La 3 Zr 2 O 12 ,or [Formula 1] [ka] [ka] and combinations thereof.
11. The process comprising: further processing the ceramic material by sintering the crystalline product of the ceramic material at an annealing temperature of 900° C. or greater; 2. The solid electrolyte material of claim 1, further comprising: measuring the ionic conductivity of the ceramic material.
12. The SPAN value of the crystalline product after annealing (D 90 -D 10 ) / D 50 The solid electrolyte material according to claim 1 , wherein SPAN satisfies 0.8<SPAN≦1.
7.
13. The SPAN value of the crystalline product after annealing (D 90 -D 10 ) / D 50 The solid electrolyte material according to claim 1 , wherein SPAN satisfies 0.8<SPAN≦1.
0.
14. D of the crystalline product after annealing 90is 20 μm to 40 μm, and D 10 is 3 μm to 10 μm, and D 99 is 35 μm to 60 μm, and D 1 The solid electrolyte material according to claim 1, wherein the average particle size is 0.1 μm to 3 μm.
15. D of the crystalline product after annealing 50 The solid electrolyte material according to claim 1, wherein the thickness is 10 μm to 18 μm.
16. The lithium-containing salt is lithium sulfate (Li 2 SO 4 ), lithium nitrate (LiNO 3 ), lithium carbonate (Li 2 CO 3 ), lithium acetate (LiCH 2 COO), lithium hydroxide (LiOH), lithium formate (LiCHO 2 2. The solid electrolyte material of claim 1, wherein the lithium ion concentration is selected from the group consisting of lithium chloride (LiCl), lithium ion sulphate (LiS), lithium ion sulphate (LiCl), and combinations thereof.
17. 17. The solid electrolyte material of claim 16, wherein the lithium-containing salt, the lanthanum-containing salt, the zirconium-containing salt, and the one or more inorganic metal salts are acid salts of the same type.
18. 2. The solid electrolyte material of claim 1, wherein one of the one or more inorganic metal salts is selected from the group consisting of metal sulfates, metal phosphates, metal nitrates, metal carbonates, metal acetates, metal hydroxides, metal halides, formates, metal chlorides, metal bromides, metal iodides, metal fluorides, and combinations thereof.
19. A solid electrolyte material, comprising: Li a La b Zr c A d D1 e . . . DN n O vwherein 6.2≦a≦7.2, 2.8≦b≦3.5, 1.2≦c≦2.2, 2.0≦v≦12, and D 1 , … , D N is a metal, N≧0, 0≦d≦0.8, 0≦e≦0.8, and 0≦n≦0.8; Digitally controlled stoichiometric amounts of a lithium-containing salt, a lanthanum-containing salt, a zirconium-containing salt, and one or more metals D 1 , D 2 , . . . , D N forming a liquid mixture of one or more inorganic salts comprising: injecting a mist of the liquid mixture at high velocity into a power jet chamber by mixing the liquid mixture with a first gas flow to form a gas-liquid mixture; drying the gas-liquid mixture for a first reaction time of less than 20 minutes by feeding a second gas stream of the heated gas to undergo one or more oxidation reactions to form a gas-solid mixture within the power jet chamber; expelling the gas-solid mixture from the power jet chamber to obtain powder particles of the ceramic material; annealing the powder particles for a second reaction time greater than two hours and undergoing a dynamic crystallization process in the presence of a third gas flow to form a crystalline product, wherein upon scanning electron microscope (SEM) analysis, the crystalline product of the ceramic material is clustered.
20. The ceramic material is Li 7 La 3 Zr 2 O 12 , Li doped with one or more metals 7 La 3 Zr 2 O 12 ,or [chemical 2] and combinations thereof.
21. A solid electrolyte material, the material comprising Li 7 La 3 Zr 2 O 12 , Li doped with one or more metals 7 La 3 Zr 2 O 12 ,or [C3] and combinations thereof; Digitally controlled stoichiometric amounts of lithium-containing salt, lanthanum-containing salt, zirconium-containing salt, and one or more metals D 1 , D 2 , . . . , D N forming a liquid mixture of one or more inorganic salts comprising: injecting the mist of the liquid mixture into a power jet chamber to mix with a first gas flow to form a gas-liquid mixture; drying the lithium-containing salt, the lanthanum-containing salt, and the zirconium-containing salt together for a first reaction time of less than 20 minutes and subjecting them to one or more oxidation reactions by passing a second gas stream of heated gas through them to form powder particles of the ceramic material; annealing the powder particles for a second reaction time greater than 2 hours and undergoing a dynamic crystallization process in the presence of a third gas flow to form a crystalline product of the ceramic material, wherein the final crystalline product of the ceramic material is cluster-like under scanning electron microscope (SEM) analysis and is a garnet-type ceramic material having a cubic crystal structure as measured by X-ray diffraction (XRD) analysis, and its measured ionic conductivity (σ) is greater than 10 at 25° C. -4 S / cm or greater, solid electrolyte material.
Citation Information
Cited By
Sulfide solid electrolyte, positive electrode mixture, and solid-state battery
WO2026205063A1