Polarizing plate

The polarizing plate with a thermoplastic resin base and cured liquid crystal compound effectively addresses thermal shrinkage issues, allowing for seamless attachment to curved surfaces by eliminating the need for stretching and additional bonding agents.

JP7551279B2Active Publication Date: 2024-09-17SUMITOMO CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019074184
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-04-25
Filing Date
2019-04-09
Publication Date
2024-09-17
Estimated Expiration
2039-04-09

AI Technical Summary

Technical Problem

Conventional polarizing plates made from stretched PVA exhibit significant shrinkage during heat molding due to their stretching direction, leading to tearing or the need for additional bonding agents, which complicates attachment to curved surfaces.

Method used

A polarizing plate design featuring a polarizer with a thickness of 15 μm or less, utilizing a thermoplastic resin base material and incorporating a cured product of a liquid crystal compound and dichroic dye, which eliminates the need for stretching and reduces thermal shrinkage, allowing for attachment to complex shapes.

Benefits of technology

The solution suppresses thermal shrinkage, enabling the polarizing plate to maintain its shape and polarization characteristics even after heat molding, facilitating attachment to objects with curved surfaces without tearing or additional bonding agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551279000035
    Figure 0007551279000035
  • Figure 0007551279000033
    Figure 0007551279000033
  • Figure 0007551279000032
    Figure 0007551279000032
Patent Text Reader

Abstract

To provide a polarizing plate with at least one curved section.SOLUTION: A polarizing plate of the present invention comprises a polarizer with a first surface and a second surface, and a first base material disposed on the first surface of the polarizer, where the polarizer has a thickness of 15 μm or less and the first base material is a thermoplastic resin. The polarizing plate has at least one curved section.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate. [Background technology]

[0002] A polarizing plate is an optical element having a specific orientation structure. For example, Patent Document 1 discloses a polarizing film in which iodine or a dichroic dye is adsorbed onto a polymer film, typically a film made of polyvinyl alcohol (PVA) or its derivative, and the film is stretched and oriented uniaxially. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-047498 A Summary of the Invention [Problem to be solved by the invention]

[0004] A polarizing plate may be heat molded depending on its application. For example, when a polarizing plate is attached to a lens having a curved surface such as a sunglasses, the polarizing plate is heat molded while being attached along the lens, and a shape corresponding to the curved surface is given to the polarizing plate. However, when a polarizing plate is heat molded, the following problems may occur.

[0005] The thickness of the polarizer in a conventional polarizing plate using stretched PVA is 20 μm to 30 μm, and when such a polarizing plate is heat-molded, the shrinkage force of the stretched PVA is large, and it may heat shrink in the stretching direction or tear along the stretching direction. In order to suppress such phenomena, in a polarizing plate using stretched PVA, it is necessary to attach the polarizing plate to a substrate such as a resin or fix the periphery of the polarizing plate with a curable resin.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polarizing plate which is suppressed in shrinkage due to thermoforming and has a reduced thickness. [Means for solving the problem]

[0007] The present invention includes the following aspects. [1] A polarizing plate having a polarizer having a first surface and a second surface, and a first substrate disposed on the first surface of the polarizer, wherein the polarizer has a thickness of 15 μm or less, the first substrate is a thermoplastic resin substrate, and the polarizing plate has at least one curved portion. [2] The polarizing plate according to [1], wherein the curved portion has a radius of curvature of 30 mm to 150 mm. [3] The polarizing plate according to [1] or [2], wherein the first substrate contains at least one of an acrylic resin and a cyclic olefin resin. [4] The polarizing plate according to any one of [1] to [3], wherein the polarizer includes a polarizing layer, the polarizing layer includes a cured product of a liquid crystal compound and a dichroic dye, and the dichroic dye is dispersed and aligned in the polarizing layer. [5] The polarizing plate according to any one of [1] to [4], wherein the first substrate has a thickness of 40 μm to 120 μm. [6] The polarizing plate according to any one of [1] to [5], further comprising a second base material on the second surface of the polarizer. [7] The polarizing plate according to [6], wherein the second substrate contains at least one selected from an acrylic resin, a cyclic olefin resin, and a triacetyl cellulose resin. [8] The polarizing plate according to any one of [1] to [7], wherein the polarizing plate is attached to a display surface of a display device having a curved display surface, and the curved portion coincides with the curved surface. Effect of the Invention

[0008] According to the present invention, it is possible to provide a polarizing plate which is suppressed in shrinkage due to thermoforming and has a reduced thickness. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a circularly polarizing plate according to one embodiment of the present invention. [Figure 4] FIG. 1 is a schematic cross-sectional view of a circularly polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polarizing plate in this embodiment has a polarizer having a first surface and a second surface, and a first substrate arranged on the first surface of the polarizer, wherein the polarizer has a thickness of 15 μm or less, the first substrate is a thermosetting resin substrate, and the polarizing plate has at least one curved portion.

[0011] As an embodiment of the present invention, a case in which the polarizing layer contains a cured product of a liquid crystal compound and a case in which the polarizing layer contains PVA will be described below.

[0012] First Embodiment 1 is a schematic cross-sectional view of a polarizing plate 1 according to this embodiment. The polarizing plate 1 includes a polarizer 11 and a first base material 12. The polarizer 11 has a first surface 31 and a second surface 32. The first base material 12 is located on the first surface 31. The polarizer 11 includes a polarizing layer 21 and an alignment layer 22. The polarizing layer 21 includes a cured product 101 of a liquid crystal compound and a dichroic dye 102. The dichroic dye 102 is dispersed in the cured product 101 of the liquid crystal compound. The alignment layer 22 exhibits an alignment regulating force. By disposing the liquid crystal compound before curing on the alignment layer 22, the liquid crystal compound before curing is aligned in one direction. Thereafter, the liquid crystal compound is cured to obtain a cured product 101 of the liquid crystal compound aligned in one direction. Since the dichroic dye 102 is disposed on the alignment layer 22 in a state where it is dispersed in the liquid crystal compound before curing, the dichroic dye 102 is also aligned in the alignment direction of the cured product 101 of the liquid crystal compound according to the alignment of the cured product 101 of the liquid crystal compound.

[0013] The polarizing plate 1 has at least one curved portion 13. The shape of the curved portion 13 depends on the shape of the object to which the polarizing plate 1 is attached. In this embodiment, the curved portion 13 may be a curved portion having multiple radii of curvature. The radius of curvature in this embodiment is defined on the surface of the curved portion 13 that is closest to the virtual center. For example, the radius of curvature in the polarizing plate 1 in FIG. 1 is defined as the radius of curvature of the second surface 32. The radius of curvature is a value calculated from the arc length, chord length, and arrow height of the curved portion 13 using the following formula. Arc length (L) = radius (r) * central angle (θ) (1) Chord length (d) = 2*r*sin(θ / 2) (2) Arrow height(h)=r*{1-cos(θ / 2)} (3)

[0014] The radius of curvature of the curved portions 13 may be, for example, 30 mm to 150 mm. Furthermore, the polarizing plate 1 may have two or more curved portions 13. The shape of the curved portions 13 is not particularly limited, but may be, for example, a curved portion having a small radius of curvature that cannot be achieved by a polarizing plate containing stretched PVA.

[0015] In addition, a polarizing plate using a stretched PVA with a thickness of 20 μm to 30 μm as a polarizing layer may undergo heat shrinkage in the stretching direction of the stretched PVA during heat molding, or may tear along the stretching direction of the stretched PVA. In order to prevent such phenomena, it is necessary to hold the polarizing plate with a second base material that maintains the shape.

[0016] When the polarizer of the polarizing plate 1 is made of the cured liquid crystal compound 101 and the aligned dichroic dye 102, no stretching is required. Therefore, compared with a conventional polarizing plate containing stretched PVA having a thickness of 20 μm to 30 μm, the shrinkage due to heat is small. For this reason, when a polarizing plate using stretched PVA having a thickness of 20 μm to 30 μm is heat-molded, the second base material used for maintaining the shape can be made thinner or omitted. The polarizing plate 1 can be attached to an object having a more complicated shape, which contributes to improving the design of the object.

[0017] When the polarizer of the polarizing plate 1 is made of the cured liquid crystal compound 101 and the oriented dichroic dye 102, the bending strength does not vary depending on the bending direction during heat molding. Therefore, it is possible to attach the plate to objects having more complex shapes, which contributes to improving the design of the objects.

[0018] The thickness of the polarizing plate 1 is 25 μm to 200 μm, preferably 50 μm to 180 μm, and more preferably 60 μm to 170 μm. By setting the thickness of the polarizing plate 1 to 60 μm to 170 μm, the polarizing plate 1 can be well conformed to the shape of the object to which it is attached. The thickness of the polarizing plate 1 in this embodiment is defined as a value obtained by measuring any five points on the polarizing plate 1 with a contact film thickness meter and calculating the average value.

[0019] The thickness of the polarizer 11 is from 1 μm to 15 μm, preferably from 1 μm to 10 μm, more preferably from 1 μm to 5 μm, and further preferably from 1 μm to 3 μm. The thickness of the polarizer 11 in this embodiment can be determined by measuring any five points of the polarizer 11 with a contact film thickness meter, an interference film thickness meter, a laser microscope, or a stylus film thickness meter, and calculating the average value.

[0020] The polarizing plate 1 of this embodiment has a cured liquid crystal compound 101 and a polarizing layer 21 in which the dichroic dye 102 is aligned, and therefore the polarization characteristics are unlikely to change even when the polarizing plate 1 is heated. The retention rate of the polarization characteristics of the polarizing plate 1 before and after heating is, for example, 90% to 100%, and preferably 95% to 100%. In this embodiment, the retention rate of the polarization characteristics of the polarizing plate 1 before and after heating can be calculated as the absorbance retention rate (%) in the alignment direction (also referred to as the absorption axis direction) of the dichroic dye 102.

[0021] Specifically, it is defined as follows. First, the absorbance A1 of the polarizing plate 1 in the absorption axis direction at 23°C is measured (A1(23°C)). Using a spectrophotometer (UV-3150 manufactured by Shimadzu Corporation) with a folder with the polarizing plate 1 attached set, A1(23°C) is measured in the wavelength range of 380 to 680 nm in 2 nm steps by the double beam method. In order to eliminate the contribution of light loss due to surface reflection of the polarizing plate 1, after setting the measurement sample, the zero point is corrected at 800 nm where there is no light absorption, and then the measurement is performed. Then, the sample is placed in an oven at 85°C for 500 hours, and after removal, the absorbance is measured again by the above method. The absorbance retention rate (%) is calculated by the following formula (I). Absorbance retention rate (%)=A1(85℃) / A1(23℃)×100 (I) In the formula, A1(85°C) indicates the absorbance in the absorption axis direction after the polarizing plate was kept in an oven at 85°C for 500 hours, and A1(23°C) indicates the absorbance in the absorption axis direction when measured at 23°C before the heat resistance test.

[0022] Since the polarizer of the polarizing plate 1 is as thin as 15 μm or less, it shrinks less when heated compared to a polarizing plate including a 20 μm to 30 μm thick stretched PVA polarizer. Furthermore, when a polarizing layer 21 in which a cured product 101 of a liquid crystal compound and a dichroic dye 102 are oriented is used, shrinkage when heated is even smaller. Therefore, even after heat molding, there is little variation in the polarization characteristics at any multiple points in the curved portion 13.

[0023] Fig. 2 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. As shown in Fig. 2, in polarizing plate 1', second substrate 14 is located on second surface 32 of polarizer 11. Second substrate 14 can protect polarizer 11. Specifically, when polarizer 11 is touched directly with the hand, scratches or the like may occur, and the polarization properties may deteriorate only in those areas. Second substrate 14 can prevent such deterioration of polarization properties.

[0024] Each element included in the polarizing plate 1 will be described in detail below. 1. Polarizer The polarizer according to this embodiment has a polarizing layer in which a dichroic dye and a cured product of a liquid crystal compound are oriented. This polarizing layer can be formed using a composition containing a dichroic dye (hereinafter, sometimes referred to as a "polarizer-forming composition"). In this embodiment, the liquid crystal compound may also function as the dichroic dye, that is, the liquid crystal compound may exhibit dichroism. Examples of liquid crystal compounds exhibiting dichroism include compounds described in WO2011 / 024891 and JP2018-120229A.

[0025] 1-1.Dichroic dyes As the dichroic dye, one having absorption in the wavelength range of 380 nm to 800 nm can be used, and it is preferable to use an organic dye. As the dichroic dye, for example, an azo compound can be used.

[0026] The azo compound may be a dichroic dye (1) having an absorption maximum in the wavelength range of 380 nm to 550 nm. The dichroic dye (1) may be, for example, a compound represented by the following formula (1) (hereinafter, sometimes referred to as "compound (1)"). The geometric isomerism of the azobenzene moiety of compound (1) is preferably trans.

[0027] [ka]

[0028] Y in formula (1) is a group represented by the following formula (Y1) or formula (Y2), and is preferably a group represented by formula (Y1).

[0029] [ka]

[0030] In formula (Y1) and formula (Y2), the straight lines at both ends represent bonds, the bond on the left side is bonded to a phenylene group having an azo group, and the bond on the right side is R 2It is bonded to a phenylene group having the formula: L is an oxygen atom or -NR-, and R is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a t-butyl group. Among them, L is preferably an oxygen atom or -NH-, and more preferably an oxygen atom.

[0031] R 1 is expressed by the following formula (R 1 -1), formula (R 1 -2) or formula (R 1 -3), preferably a group represented by the formula (R 1 -2) and the formula (R 1 -3), in which * represents a bond.

[0032] [ka]

[0033] Formula (R 1 In the group represented by -2), ma is preferably each independently an integer of 0 to 10, more preferably an integer of 0 to 5. The two ma may be the same or different, but are preferably the same.

[0034] R 2 is expressed as the formula (R 2 -1), formula (R 2 -2), formula (R 2 -3), formula (R 2 -4), formula (R 2 -5) or formula (R 2 -6), a group represented by the formula (R 2 -2), formula (R 2 -5) or formula (R 2 -6), 2 -6) is more preferable.

[0035] [ka]

[0036] R 2 is the formula (R 2 -1), formula (R 2 -2), formula (R 2 -3), formula (R 2 -5) or formula (R 2 -6), mb contained in the group is preferably an integer of 0 to 10, and more preferably an integer of 0 to 5.

[0037] Examples of compound (1) include compounds represented by the following formulas (1-1) to (1-8).

[0038] [ka]

[0039] Among these, the compounds represented by formulas (1-1), (1-2), (1-3), (1-5), (1-7) and (1-8) are preferred, and the compounds represented by formulas (1-1), (1-2), (1-3) and (1-7) are more preferred.

[0040] Here, the production method of compound (1) will be described. Compound (1) can be produced, for example, from a compound represented by formula (1X) [compound (1X)] and a compound represented by formula (1Y) [compound (1Y)] by the reaction shown in the following scheme.

[0041] [ka]

[0042] In the above diagram, R 1 , R 2 and Y have the same meaning as above, Re 1 and Re 2 are groups that react with each other to form a group represented by Y. 1 and Re 2Examples of the combination of include a combination of a carboxy group and a hydroxyl group, a combination of a carboxy group and an amino group (which may be substituted with R), a combination of a carbonyl halide group and a hydroxyl group, a combination of a carbonyl halide group and an amino group (which may be substituted with R), a combination of a carbonyloxyalkyl group and a hydroxyl group, and a combination of a carbonyloxyalkyl group and an amino group (which may be substituted with R). 1 Compound (1X) having R 2 The compound (1Y) having R 1 is protected with an appropriate protecting group, or R 2 Compound (1) can also be produced by reacting compounds protected with an appropriate protecting group with each other, followed by a suitable deprotection reaction.

[0043] The reaction conditions for reacting compound (1X) and compound (1Y) can be appropriately selected from known optimum conditions depending on the types of compound (1X) and compound (1Y) used.

[0044] For example, Re 1 is a carboxy group, and Re 2 When is a hydroxyl group and Y is -C(=O)-O-, the reaction conditions include, for example, conditions for condensation in a solvent in the presence of an esterification condensation agent. The solvent includes a solvent capable of dissolving both compound (1X) and compound (1Y), such as chloroform. The esterification condensation agent includes, for example, diisopropylcarbodiimide (IPC). In this case, it is preferable to use a base such as dimethylaminopyridine (DMAP) in combination. The reaction temperature is selected depending on the types of compound (1X) and compound (1Y), and is, for example, in the range of -15 to 70°C, preferably in the range of 0 to 40°C. The reaction time is, for example, in the range of 15 minutes to 48 hours.

[0045] The reaction time can also be determined by appropriately sampling the reaction mixture during the reaction and confirming the degree of disappearance of compound (1X) and compound (1Y) and the degree of production of compound (1) by a known analytical means such as liquid chromatography or gas chromatography.

[0046] After the reaction, compound (1) can be isolated from the reaction mixture by known methods such as recrystallization, reprecipitation, extraction and various types of chromatography, or by a combination of these procedures.

[0047] As the azo compound, a dichroic dye (2) having an absorption maximum in the wavelength range of 550 nm to 700 nm can be used.

[0048] The dichroic dye (2) may contain a dichroic dye (2-1) having an absorption maximum in the wavelength range of 550 to 600 nm and / or a dichroic dye (2-2) having an absorption maximum in the wavelength range of 600 to 700 nm. The dichroic dye (2-1) more preferably has an absorption maximum in the wavelength range of 570 to 600 nm, and the dichroic dye (2-2) more preferably has an absorption maximum in the wavelength range of 600 to 680 nm.

[0049] The dichroic dye (2) may be, for example, a compound represented by the following formula (2) (hereinafter, sometimes referred to as "compound (2)"). The geometric isomerism of the azobenzene moiety of compound (2) is preferably trans. In formula (2), n is 1 or 2.

[0050] [ka]

[0051] Ar 1 and Ar 3 are each independently a group represented by formula (AR-1), formula (AR-2), formula (AR-3) or formula (AR-4). * represents a bond.

[0052] [ka]

[0053] Ar 2 is a group represented by formula (AR2-1), formula (AR2-2) or formula (AR2-3).

[0054] [ka]

[0055] A1 and A2 are each independently a group represented by any one of formulas (A-1) to (A-9). In formulas (A-2), (A-3), (A-5) and (A-6), mc is an integer of 0 to 10, and when there are two mc in the same group, the two mc are the same or different from each other.

[0056] [ka]

[0057] Compound (2) was added with Ar so that the compound (2) had an absorption maximum in the wavelength range of 550 nm to 600 nm. 1 , Ar 2 and Ar 3 Compound (2) that can be used as the dichroic dye (2-1) is determined by combining Ar 1 , Ar 2 and Ar 3 By combining these, a compound (2) that can be used as a dichroic dye (2-2) is defined.

[0058] Specific examples of compound (2) include compounds represented by formulas (2-11) to (2-37).

[0059] [ka]

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] [ka]

[0065] Among the specific examples of the above compound (2), the dichroic dye (2-1) is represented by the formulas (2-12), (2-13), (2-18), (2-20), (2-21), (2-22), (2-23), (2-24), (2-26), (2-27), (2-28), (2-29), (2-30), and (2-37), respectively. The dichroic dye (2-2) is represented by the formulas (2-31), (2-32), (2-33), (2-34), (2-35), and (2-36), respectively. The dyes represented by formulae (2-11), (2-15) and (2-16) are not dyes that exhibit absorption in the wavelength range of 550 nm to 700 nm, but can be used in combination with other dichroic dyes.

[0066] Among specific examples of compound (2), as the dichroic dye (2), those represented by formula (2-15), formula (2-16), formula (2-18), formula (2-20), formula (2-21), formula (2-22), formula (2-23), formula (2-27), formula (2-29), formula (2-31), formula (2-32), formula (2-33), formula (2-34), formula (2-35), and formula (2-37) are preferable.

[0067] The dichroic dye (2) can be produced by a known method, for example, as described in JP-A-58-38756 and JP-A-63-301850.

[0068] The above dichroic dyes may be used alone or in combination of two or more. When the polarizer-forming composition contains two or more dichroic dyes, the content of each dichroic dye is preferably 3 parts by mass or less, more preferably 0.1 parts by mass or more to 2.5 parts by mass or less, and even more preferably 1 part by mass or more to 1.5 parts by mass or less, expressed in terms of the content relative to 100 parts by mass of the polymerizable liquid crystal compound described later. If the content of each dichroic dye is within the above range, the dichroic dye in the polarizer-forming composition exhibits sufficient solubility in a solvent, so that when a polarizer is manufactured using the polarizer-forming composition, a polarizer without defects is easily obtained. This makes it easier to manufacture a polarizing plate that has high light absorption selectivity even in a thin film and has excellent heat resistance. The total amount of the dichroic dye contained in the polarizer-forming composition is preferably 9 parts by mass or less, more preferably 0.1 parts by mass or more to 7.5 parts by mass or less, and even more preferably 1 part by mass or more to 4.5 parts by mass or less, expressed in terms of the content relative to 100 parts by mass of the polymerizable liquid crystal compound described later.

[0069] 1-2.Liquid crystal compounds A polarizer 11 according to this embodiment has a polarizing layer 21 containing a cured product 101 of a liquid crystal compound and a dichroic dye 102. That is, the composition for forming a polarizer contains a liquid crystal compound together with a dichroic dye.

[0070] The liquid crystal compound in this embodiment may be a polymerizable liquid crystal compound. The polymerizable liquid crystal compound is a liquid crystal compound that can be polymerized while being aligned, and has a polymerizable group in the molecule. The composition for forming a polarizer containing the polymerizable liquid crystal compound forms a cured film by polymerizing the polymerizable liquid crystal compound in an aligned state. The cured film, i.e., the cured product 101 of the liquid crystal compound, does not need to exhibit liquid crystallinity. It is particularly preferable that the polymerizable group is a radically polymerizable group. The radically polymerizable group means a group that is involved in a radical polymerization reaction.

[0071] The polymerizable liquid crystal compound may be one that exhibits a nematic liquid crystal phase (hereinafter sometimes referred to as "nematic liquid crystal phase"), one that exhibits a smectic liquid crystal phase (hereinafter sometimes referred to as "smectic liquid crystal phase"), or one that exhibits both a nematic liquid crystal phase and a smectic liquid crystal phase, but is preferably a polymerizable smectic liquid crystal compound that exhibits at least a smectic liquid crystal phase. A polarizer-forming composition containing a polymerizable smectic liquid crystal compound is suppressed from coloring due to interaction with a dichroic dye, and a polarizer with better polarization performance can be obtained.

[0072] The smectic liquid crystal phase exhibited by the polymerizable smectic liquid crystal compound is preferably a high-order smectic liquid crystal phase. The high-order smectic liquid crystal phase referred to here is a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, and a smectic L phase, and among these, a smectic B phase, a smectic F phase, and a smectic I phase are more preferred.

[0073] When the smectic liquid crystal phase exhibited by the polymerizable liquid crystal compound is one of these higher-order smectic liquid crystal phases, a polarizer with a higher degree of orientation order can be manufactured. In addition, a polarizer manufactured using a polymerizable liquid crystal compound with a higher-order smectic liquid crystal phase with a high degree of orientation order can obtain a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase in an X-ray diffraction measurement. This Bragg peak is a peak derived from the planar periodic structure of the molecular orientation. According to the composition for forming a polarizer according to this embodiment, a polarizer having a periodic interval of 3.0 to 5.0 Å can be obtained.

[0074] Whether or not the polymerizable liquid crystal compound exhibits a nematic liquid crystal phase or a smectic liquid crystal phase can be confirmed, for example, as follows. A suitable substrate is prepared, and a polarizer-forming composition is applied to the substrate to form a coating film. Then, the solvent contained in the coating film is removed by heating or reducing pressure treatment under conditions in which the polymerizable liquid crystal compound does not polymerize. Next, the coating film formed on the substrate is heated to an isotropic phase temperature, and the liquid crystal phase that is developed by gradually cooling is inspected by observing the texture with a polarizing microscope. In this inspection, for example, a polymerizable liquid crystal compound that exhibits a nematic liquid crystal phase when cooled and exhibits a smectic liquid crystal phase when further cooled is particularly preferred. In the nematic liquid crystal phase and the smectic liquid crystal phase, the fact that the polymerizable liquid crystal compound and the dichroic dye are not phase-separated can be confirmed, for example, by surface observation with various microscopes or scattering degree measurement with a haze meter.

[0075] An example of the polymerizable liquid crystal compound is a compound represented by formula (4) (hereinafter sometimes referred to as "compound (4)"). U 1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (4)

[0076] In formula (4), X 1 , X 2 and X 3 each independently represents a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent. 1 , X 2 and X 3 At least one of X is preferably a cyclohexane-1,4-diyl group which may have a substituent. 1 Or X 3is particularly preferably a cyclohexane-1,4-diyl group which may have a substituent. The -CH2- constituting the cyclohexane-1,4-diyl group which may have a substituent may be replaced by -O-, -S- or -NR-. R is an alkyl group having 1 to 6 carbon atoms or a phenyl group.

[0077] The cyclohexane-1,4-diyl group which may have a substituent is preferably a trans-cyclohexane-1,4-diyl group which may have a substituent, and more preferably a trans-cyclohexane-1,4-diyl group which does not have a substituent. 1 , X 2 and X 3 At least two of them may be 1,4-phenylene groups which may have a substituent, and are preferably 1,4-phenylene groups which do not have a substituent.

[0078] Examples of the substituent that the 1,4-phenylene group which may have a substituent or the cyclohexane-1,4-diyl group which may have a substituent include an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom.

[0079] In formula (4), Y 1 and Y 2 are each independently -CH2CH2-, -CH2O-, -COO-, -OCOO-, a single bond, -N=N-, -CR a =CR b -, -C≡C- or -CR a =N-. R a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is preferably -CH2CH2-, -COO- or a single bond, and Y 2 is preferably -CH2CH2-, -COO- or -CH2O-.

[0080] In formula (4), U 1 is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group.2 is a polymerizable group. 1 and U 2 are preferably polymerizable groups, and more preferably photopolymerizable groups. The photopolymerizable group refers to a group that can be involved in a polymerization reaction by an active radical, an acid, or the like generated from a photopolymerization initiator described later. A polymerizable liquid crystal compound having a photopolymerizable group is advantageous in that it can be polymerized under lower temperature conditions.

[0081] U 1 and U 2 The polymerizable groups may be different from each other, but are preferably the same type of group. Examples of the polymerizable group include vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, acryloyloxy group, methacryloyloxy group, oxiranyl group, and oxetanyl group. Among them, the polymerizable group is preferably acryloyloxy group, methacryloyloxy group, vinyloxy group, oxiranyl group, and oxetanyl group, and more preferably acryloyloxy group.

[0082] In formula (4), V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting this alkanediyl group may be replaced by -O-, -S- or -NH-. Examples of the alkanediyl group having 1 to 20 carbon atoms include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group and an icosane-1,20-diyl group. V 1 and V 2is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms. Examples of the substituent that the alkanediyl group having 1 to 20 carbon atoms may have include a cyano group and a halogen atom. This alkanediyl group is preferably unsubstituted, and more preferably unsubstituted and linear.

[0083] In formula (4), W 1 and W 2 represent each independently a single bond, -O-, -S-, -COO- or -OCOO-, and preferably a single bond or -O-.

[0084] Examples of compound (4) include compounds represented by formulae (4-1) to (4-43). When a specific example of compound (4) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.

[0085] [ka]

[0086] [ka]

[0087] [ka]

[0088] [ka]

[0089] The polymerizable liquid crystal compound can be used alone or in combination of two or more in the composition for forming a polarizer. When two or more polymerizable liquid crystal compounds are mixed, it is preferable that at least one of them is compound (4). When two polymerizable liquid crystal compounds are mixed, the mixing ratio of the polymerizable liquid crystal compound other than compound (4): compound (4) is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.

[0090] Among the compounds (4), the compounds represented by formula (4-5), formula (4-6), formula (4-7), formula (4-8), formula (4-9), formula (4-10), formula (4-11), formula (4-12), formula (4-13), formula (4-14), formula (4-15), formula (4-22), formula (4-24), formula (4-25), formula (4-26), formula (4-27), formula (4-28) and formula (4-29) are preferred. These compounds can be easily polymerized under temperature conditions below the crystal phase transition temperature, i.e., while the liquid crystal state of the high-order smectic phase is sufficiently maintained, due to the interaction with other polymerizable liquid crystal compounds. Specifically, these compounds can be polymerized under temperature conditions of 70°C or less, preferably 60°C or less, while the liquid crystal state of the high-order smectic phase is sufficiently maintained.

[0091] The content of the polymerizable liquid crystal compound in the composition for forming a polarizer is preferably 50% by mass to 99.9% by mass, more preferably 80% by mass to 99.9% by mass, based on the solid content of the composition for forming a polarizer. If the content of the polymerizable liquid crystal compound is within the above range, the orientation of the polymerizable liquid crystal compound tends to be high. The solid content refers to the total amount of components excluding volatile components such as solvents from the composition for forming a polarizer.

[0092] The polymerizable liquid crystal compound can be produced by a known method, for example, as described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.

[0093] 1-3.Solvent The polarizer-forming composition preferably contains a solvent. The solvent is preferably a solvent capable of completely dissolving the dichroic dye and the polymerizable liquid crystal compound. In addition, the solvent is preferably inactive to the polymerization reaction of the polymerizable liquid crystal compound contained in the polarizer-forming composition.

[0094] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorine-containing solvents such as chloroform and chlorobenzene. These solvents may be used alone or in combination of two or more.

[0095] The content of the solvent is preferably 50% by mass to 98% by mass with respect to the total amount of the polarizer-forming composition. In other words, the solid content in the polarizer-forming composition is preferably 2% by mass to 50% by mass. When the solid content is 2% by mass or more, it becomes easier to obtain a thin polarizing plate, which is one of the objects of the present embodiment. When the solid content is 50% by mass or less, the viscosity of the polarizer-forming composition is low, so that the thickness of the polarizer becomes approximately uniform, and unevenness is unlikely to occur in the polarizer. The solid content can be determined in consideration of the thickness of the polarizer.

[0096] 1-4.Additives The polarizer-forming composition according to this embodiment may contain any additives, such as a polymerization initiator, a photosensitizer, a polymerization inhibitor, and a leveling agent.

[0097] 1-4-1. Polymerization initiator The composition for forming a polarizer preferably contains a polymerization initiator. The polymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound. As the polymerization initiator, a photopolymerization initiator is preferable because it can initiate a polymerization reaction under low temperature conditions. Specifically, a compound that generates an active radical or an acid by the action of light is used as the photopolymerization initiator. Among such photopolymerization initiators, those that generate an active radical by the action of light are more preferable.

[0098] Examples of the polymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, and a sulfonium salt.

[0099] Examples of benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.

[0100] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0101] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.

[0102] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0103] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethene].

[0036] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.

[0104] The polymerization initiator may be commercially available. Examples of commercially available polymerization initiators include "Irgacure 907", "Irgacure 184", "Irgacure 651", "Irgacure 819", "Irgacure 250", "Irgacure 369" (BASF Japan Co., Ltd.); "Seiquol BZ", "Seiquol Z", "Seiquol BEE" (Seiko Chemical Co., Ltd.); "Kayacure BP100" (Nippon Kayaku Co., Ltd.); "UVI-6992" (Dow Chemical Co., Ltd.); "Adeka Optomer SP-152", "Adeka Optomer SP-170" (ADEKA Co., Ltd.); "TAZ-A", "TAZ-PP" (DKSH Japan Co., Ltd.); and "TAZ-104" (Sanwa Chemical Co., Ltd.).

[0105] When the polarizer-forming composition contains a polymerization initiator, the content thereof can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound contained in the polarizer-forming composition, but the content of the polymerization initiator is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to a total of 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization initiator is within this range, it is preferable because the polymerizable liquid crystal compound can be polymerized without disturbing its alignment.

[0106] 1-4-2. Photosensitizers When the polarizer-forming composition contains a photopolymerization initiator, it may further contain a photosensitizer. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.), anthracene compounds such as anthracene and alkoxy group-containing anthracene (e.g., dibutoxyanthracene, etc.), phenothiazine, and rubrene.

[0107] When the polarizer-forming composition contains a photopolymerization initiator and a photosensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the polarizer-forming composition is further promoted. The content of the photosensitizer can be appropriately adjusted depending on the type and amount of the photopolymerization initiator and the polymerizable liquid crystal compound used in combination, but is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0108] 1-4-3. Polymerization inhibitors The composition for forming a polarizer may contain a polymerization inhibitor in order to stably proceed with the polymerization reaction of the polymerizable liquid crystal compound. The polymerization inhibitor can control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0109] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (e.g., butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.

[0110] When the composition for forming a polarizer contains a polymerization inhibitor, the content thereof is appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound used, the content of the photosensitizer, etc., and is usually 0.1 parts by mass to 30 parts by mass, preferably 0.5 parts by mass to 10 parts by mass, and more preferably 0.5 parts by mass to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. It is preferable that the content of the polymerization inhibitor is within the above range, since the polymerizable liquid crystal compound contained in the polarizer-forming composition can be polymerized without disturbing the alignment of the compound.

[0111] 1-4-4.Leveling agent The polarizer-forming composition preferably contains a leveling agent. The leveling agent has a function of adjusting the flowability of the polarizer-forming composition and making the coating film obtained by applying the polarizer-forming composition flatter, and examples of the leveling agent include surfactants. Examples of the leveling agent include a leveling agent mainly composed of a polyacrylate compound and a leveling agent mainly composed of a fluorine atom-containing compound.

[0112] Examples of leveling agents containing a polyacrylate compound as a main component include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" [BYK Chemie].

[0113] Examples of leveling agents containing a fluorine atom-containing compound as a main component include Megafac "R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" [DIC Corporation]; Surflon "S-381", Examples include "S-382", "S-383", "S-393", "SC-101", "SC-105", "KH-40" and "SA-100" [AGC Seimi Chemical Co., Ltd.]; "E1830", "E5844" [Daikin Industries, Ltd.]; and F-Top "EF301", "EF303", "EF351" and "EF352" [Mitsubishi Materials Electronic Chemicals Co., Ltd.].

[0114] When the leveling agent is contained in the polarizer-forming composition, the content is usually 0.3 parts by mass or more and 5 parts by mass or less, preferably 0.5 parts by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound is easily horizontally aligned, and the obtained polarizer tends to be smoother. When the content of the leveling agent relative to the polymerizable liquid crystal compound exceeds the above range, the obtained polarizer tends to be easily uneven. The polarizer-forming composition may contain two or more types of leveling agents.

[0115] 2. First substrate and second substrate Thermoplastic resin substrates can be used as the first substrate 12 and the second substrate 14. The first substrate 12 and the second substrate 14 are preferably transparent thermoplastic resin substrates. A transparent thermoplastic resin substrate is a thermoplastic resin substrate having a degree of transparency that allows light, particularly visible light, to pass through. Transparency refers to a property in which the transmittance for light rays with wavelengths of 380 nm to 780 nm is 80% or more. The first substrate and the second substrate may be formed from the same thermoplastic resin or different thermoplastic resins.

[0116] Specifically, examples of the first substrate 12 and the second substrate 14 include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; acrylic resins such as polymethacrylic acid esters and polyacrylic acid esters; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide, and polyphenylene oxide. Among them, cyclic olefin resins, polyethylene terephthalate, and acrylic resins are preferred, and cyclic olefin resins and polymethacrylic acid esters are particularly preferred, in terms of being easily available on the market and having excellent transparency. In the manufacturing process of the polarizing plate 1, a support substrate or the like may be attached to the first substrate 12 and the second substrate 14 in order to easily handle the first substrate 12 and the second substrate 14 without causing damage such as tearing when transporting or storing them.

[0117] As long as either the first substrate 12 or the second substrate 14 is a thermoplastic resin substrate, the other may not be a thermoplastic resin substrate. When either the first substrate 12 or the second substrate 14 is a thermoplastic resin substrate, the curved formability of the polarizing plate 1 is maintained. For example, a substrate containing a cellulose ester resin such as triacetyl cellulose, diacetyl cellulose, or cellulose acetate propionate may be used as the first substrate. As an example, a substrate containing triacetyl cellulose may be used as the first substrate, and a substrate containing an acrylic resin may be used as the second substrate.

[0118] When the first substrate 12 is to be given retardation properties, a plastic substrate made of cellulose ester or cyclic olefin resin is preferred in that the retardation value can be easily controlled.

[0119] In the cellulose ester, at least a part of the hydroxyl groups contained in the cellulose is converted to acetate. A cellulose ester film made of such a cellulose ester can be easily obtained from the market. Examples of commercially available triacetyl cellulose films include "FUJITAC FILM" (Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (Konica Minolta Opto Co., Ltd.). Such commercially available triacetyl cellulose films can be used as the first substrate 12 as is or after being given retardation properties as necessary. In addition, the surface of the prepared first substrate 12 can be subjected to surface treatment such as antiglare treatment, hard coat treatment, antistatic treatment or antireflection treatment before being used as the first substrate 12.

[0120] The cyclic olefin resin is composed of a polymer or copolymer of a cyclic olefin such as norbornene or a polycyclic norbornene monomer. The cyclic olefin resin may partially contain a ring-opening portion, or may be a hydrogenated cyclic olefin resin containing a ring-opening portion. The cyclic olefin resin may be, for example, a copolymer of a cyclic olefin and a chain olefin or a vinylated aromatic compound (such as styrene) in that it does not significantly impair transparency or significantly increase moisture absorption. The cyclic olefin resin may also have a polar group introduced into its molecule.

[0121] When the cyclic olefin resin is a copolymer of a cyclic olefin and an aromatic compound having a chain olefin or a vinyl group, examples of the chain olefin include ethylene and propylene, and examples of the vinylated aromatic compound include styrene, α-methylstyrene, and alkyl-substituted styrene. In such a copolymer, the content of the structural unit derived from the cyclic olefin is 50 mol% or less, for example, in the range of about 15 mol% to 50 mol%, based on the total structural units of the cyclic olefin resin. When the cyclic olefin resin is a ternary copolymer obtained from a cyclic olefin, a chain olefin, and a vinylated aromatic compound, the content of the structural unit derived from the chain olefin is, for example, about 5 mol% to 80 mol% based on the total structural units of the cyclic olefin resin, and the content of the structural unit derived from the vinylated aromatic compound is about 5 mol% to 80 mol%. Such a ternary copolymer cyclic olefin resin has the advantage that the amount of expensive cyclic olefin used can be relatively reduced when producing the cyclic olefin resin.

[0122] Cyclic olefin resins are easily available on the market. Examples of commercially available cyclic olefin resins include "Topas" [Ticona (Germany)]; "Arton" [JSR Corporation]; "ZEONOR" and "ZEONEX" [Zeon Corporation]; and "Apel" [Mitsui Chemicals, Inc.]. Such cyclic olefin resins can be formed into a film (cyclic olefin resin film) by known film-forming means such as solvent casting and melt extrusion. Cyclic olefin resin films already available in the form of a film can also be used. Examples of such commercially available cyclic olefin resin films include "S-Cina" and "SCA40" [Sekisui Chemical Co., Ltd.]; "ZEONOR Film" [Optes Co., Ltd.]; and "Arton Film" [JSR Corporation].

[0123] The first substrate 12 and the second substrate 14 are preferably as thin as possible in terms of being light enough for practical handling and ensuring sufficient transparency, but if they are too thin, the strength decreases and workability tends to be poor. The appropriate thickness of each of the first substrate 12 and the second substrate 14 is, for example, about 20 μm to 200 μm, and preferably about 20 μm to 160 μm. When the polarizing plate 1 of this embodiment is used as a circular polarizing plate described later, or particularly when used as a polarizing plate for mobile devices, the thickness of the transparent substrate is preferably about 20 μm to 80 μm, and may be 20 μm to 50 μm.

[0124] 3.Alignment layer An alignment layer 22 is preferably formed on the first substrate 12 or the second substrate 14. In this case, the polarizer-forming composition is applied onto the alignment layer 22. For this reason, the alignment layer 22 preferably has a solvent resistance to such an extent that it is not dissolved by application of the polarizer-forming composition. In addition, it preferably has heat resistance in a heat treatment for removing the solvent or orienting the liquid crystal. The alignment layer 22 can be formed from an orienting polymer.

[0125] Examples of the oriented polymer include polyamide, gelatins, polyimide, polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid ester. Among these, polyvinyl alcohol is preferred. These oriented polymers may be used alone or in combination of two or more.

[0126] The alignment polymer can be applied to the first substrate 12 or the second substrate 14 as an alignment polymer composition (a solution containing the alignment polymer) dissolved in a solvent, to form an alignment layer 22 on the first substrate 12 or the second substrate 14. Examples of the solvent include water; alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorine-substituted hydrocarbon solvents such as chloroform and chlorobenzene. These solvents may be used alone or in combination of two or more kinds.

[0127] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).

[0128] The alignment layer 22 may be a photoalignment layer. The photoalignment layer is an alignment layer obtained by applying a composition (hereinafter, sometimes referred to as a "photoalignment layer forming composition") containing a polymer or monomer having a photoreactive group and a solvent to the first base material 12 and irradiating the composition with polarized light (preferably polarized UV) to impart an alignment control force. The photoreactive group is a group that generates a liquid crystal alignment ability when irradiated with light. Specifically, the photoreactive group generates a photoreaction that is the origin of the liquid crystal alignment ability, such as molecular orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, which occurs when irradiated with light. A photoreactive group that causes a dimerization reaction or a photocrosslinking reaction is preferable in that it has excellent alignment properties and maintains the smectic liquid crystal state when the polarizer is formed. As the photoreactive group, one having an unsaturated bond, particularly a double bond, is preferable, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is more preferable.

[0129] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, and formazan groups, as well as groups having an azoxybenzene basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, or a halogenated alkyl group. Among them, photoreactive groups capable of causing a photodimerization reaction are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment layer having excellent thermal stability and stability over time is easily obtained. Furthermore, as a polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is more preferred.

[0130] The solvent for the composition for forming a photo-alignment layer is preferably one that dissolves the polymer and monomer having a photoreactive group, and examples thereof include the solvents used for the above-mentioned alignable polymer composition.

[0131] The concentration of the polymer or monomer having a photoreactive group in the composition for forming a photoalignment layer can be appropriately adjusted depending on the type of polymer or monomer having a photoreactive group and the thickness of the photoalignment layer to be produced, but is preferably at least 0.2 mass % in terms of solid content concentration, and more preferably in the range of 0.3 mass % to 10 mass %. The composition for forming a photoalignment layer may contain a polymer material such as polyvinyl alcohol or polyimide, and a photosensitizer, as long as the properties of the alignment layer 22 are not significantly impaired.

[0132] The thickness of the alignment layer 22 is 10 nm to 10,000 nm, preferably 10 nm to 1,000 nm. In this embodiment, the thickness of the alignment layer 22 can be determined by measuring five arbitrary points of the alignment layer 22 with an interference thickness meter and calculating the average value.

[0133] The polarizer 11 according to this embodiment has an absorbance (A1) in the absorption axis direction at a wavelength of 380 nm to 760 nm of 0.3 to 1.5, preferably 0.3 to 1.0, more preferably 0.33 to 0.9, and even more preferably 0.36 to 0.85. The absorbance (A2) in the transmission axis direction is 0.001 to 0.15, preferably 0.001 to 0.10, more preferably 0.002 to 0.05, and even more preferably 0.005 to 0.040.

[0134] The above-mentioned absorbance can be appropriately adjusted by controlling the thickness of the polarizer 11 by adjusting the type of dichroic dye 102 contained in the polarizer 11, the amount of the dichroic dye 102, the solids concentration or application amount of the polarizer-forming composition, or the like.

[0135] 4. Manufacturing method of polarizing plate A method for producing a polarizing plate 1 using a composition for forming a polarizer will be described. In this method, the composition for forming a polarizer is applied to a first base material 12, preferably a transparent thermoplastic resin base material, to form a polarizing plate 1. In this embodiment, an example will be described in which a cured product 101 of a liquid crystal compound is a polymerizable liquid crystal compound.

[0136] Examples of a method for forming the alignment layer 22 on the first substrate 12 include a method of applying an alignment layer-forming composition or a commercially available alignment film material onto the first substrate 12 and heating the composition. The thickness of the applied film of the alignment layer-forming composition is determined in consideration of the thickness of the alignment layer 22 to be obtained.

[0137] It is preferable to perform rubbing (rubbing method) as necessary in order to impart an alignment regulating force to the alignment layer 22. By imparting an alignment regulating force, the cured product 101 of the liquid crystal compound can be aligned in a desired direction.

[0138] As a method for imparting an alignment control force by the rubbing method, for example, a method is given in which a rotating rubbing roll around which a rubbing cloth is wrapped is prepared, a laminate in which a coating film for forming an alignment layer is formed on the first substrate 12 is placed on a stage, and transported toward the rotating rubbing roll, thereby bringing the coating film for forming an alignment layer into contact with the rotating rubbing roll.

[0139] As a method for applying the composition for forming an alignment layer or the composition for forming a photo-alignment layer onto the first base material 12, a known method such as a coating method such as a spin coating method, an extrusion method, a gravure coating method, a die coating method, a bar coating method, an applicator method, or a printing method such as a flexography method is adopted. When a polarizer is manufactured by a roll-to-roll type continuous manufacturing method, a printing method such as a gravure coating method, a die coating method, or a flexography method is usually adopted as the application method.

[0140] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) having different alignment directions can be formed.

[0141] A coating film is obtained by applying a polarizer-forming composition onto the first substrate 12 or the alignment layer 22 formed on the first substrate 12. Examples of a method for applying the polarizer-forming composition include the same methods as those exemplified as the method for applying the alignment layer-forming composition or the photoalignment layer-forming composition to a substrate.

[0142] Next, the solvent contained in the composition for forming a polarizer is removed by drying under conditions in which the liquid crystal compound contained in the coating film does not polymerize, thereby forming a dried coating film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0143] In a preferred embodiment, the liquid crystal state of the liquid crystal compound contained in the dried film is first changed to nematic liquid crystal, and then the nematic liquid crystal phase is transferred to a smectic liquid crystal phase. In order to form a smectic liquid crystal phase via a nematic liquid crystal phase in this manner, for example, a method is adopted in which the liquid crystal compound contained in the dried film is heated to a temperature above the temperature at which it exhibits a nematic liquid crystal phase, and then cooled to a temperature at which it exhibits a smectic liquid crystal phase.

[0144] When the liquid crystal compound in the dried coating is made to have a smectic liquid crystal phase, or when the polymerizable liquid crystal compound is made to have a smectic liquid crystal phase via a nematic liquid crystal phase, the conditions for controlling the liquid crystal state (heating conditions) can be determined by measuring the phase transition temperature of the polymerizable liquid crystal compound.

[0145] Next, the polymerization process of the liquid crystal compound will be described. Here, a method will be described in detail in which a photopolymerization initiator is added to a polarizer-forming composition, the liquid crystal state of the liquid crystal compound in the dried coating is changed to a smectic liquid crystal phase, and then the liquid crystal compound is photopolymerized while maintaining the liquid crystal state of the smectic liquid crystal phase.

[0146] In photopolymerization, the light irradiated to the dry film can be selected from the group consisting of visible light, ultraviolet light, and laser light, or active electron beams, depending on the type of photopolymerization initiator contained in the dry film, or the type of liquid crystal compound (particularly, the type of polymerizable group possessed by the liquid crystal compound) and its amount. Among these, ultraviolet light is preferred because it is easy to control the progress of the polymerization reaction and because a device widely used in this field can be used as a device related to photopolymerization. Therefore, it is preferable to select the type of liquid crystal compound or photopolymerization initiator contained in the polarizer-forming composition so that photopolymerization can be performed by ultraviolet light.

[0147] During polymerization, the polymerization temperature can be controlled by cooling the dried film with an appropriate cooling means in addition to the UV light irradiation. If the liquid crystal compound can be polymerized at a lower temperature by employing such a cooling means, the polarizer 11 can be appropriately formed even if a substrate having a relatively low heat resistance is used as the first substrate 12. Note that a patterned polarizer 11 can be obtained by performing masking and development during photopolymerization.

[0148] By carrying out the photopolymerization as described above, the liquid crystal compound is polymerized while maintaining a nematic or smectic liquid crystal phase, preferably a high-order smectic liquid crystal phase as already exemplified, to form a polarizer 11. The polarizer 11 obtained by polymerizing the liquid crystal compound while maintaining the smectic liquid crystal phase has an advantage of having higher polarization performance than a polarizer obtained by polymerizing a polymerizable liquid crystal compound while maintaining the liquid crystal state of the nematic liquid crystal phase. Furthermore, it has an advantage of having superior strength compared to a polarizer coated with only a lyotropic dichroic dye.

[0149] The thickness of the polarizing layer 21 is preferably 1 μm or more and less than 15 μm, more preferably 1 μm or more and 10 μm or less, even more preferably 1 μm or more and 5 μm or less, and particularly preferably 1 μm or more and 3 μm or less. Therefore, the thickness of the coating film for forming a polarizer is determined in consideration of the thickness of the resulting polarizing layer 21. The thickness of the polarizing layer 21 in this embodiment can be determined by measuring any five points of the polarizing layer 21 with a contact film thickness meter, an interference film thickness meter, a laser microscope, or a stylus film thickness meter, and calculating the average value.

[0150] In addition to the method of forming polarizer 11 on first substrate 12 as described above, a polarizing plate can also be produced by a method of forming polarizer 11 on another substrate by the method described above, and then transferring and laminating polarizer 11 to first substrate 12.

[0151] In the above example, the alignment layer 22 and the polarizing layer 21 are formed on the first substrate 12, but the alignment layer 22 and the polarizing layer 21 may be formed on the second substrate 14. In this case, the first substrate 12 is laminated on the polarizing layer 21 via an adhesive layer or a pressure-sensitive adhesive layer, thereby obtaining a polarizing plate having the second substrate 14, the alignment layer 22, the polarizing layer 21, and the first substrate.

[0152] It is preferable that a Bragg peak is obtained in X-ray diffraction measurement of the formed polarizer 11. Examples of polarizers that can obtain a Bragg peak include polarizers that exhibit a diffraction peak derived from a hexatic phase or a crystalline phase.

[0153] When manufacturing polarizers commercially, a method capable of continuously forming polarizers is required. Such a continuous manufacturing method is a roll-to-roll type, and is sometimes referred to as "the present manufacturing method." Note that the present manufacturing method will be described mainly in the case where the first base material 12 is transparent. When the first base material 12 is transparent, the final product is a polarizing plate 1 having a transparent first base material 12 and a polarizer 11.

[0154] The manufacturing method includes, for example, the following steps. A first roll in which a first substrate 12 is wound around a first core is prepared. The first substrate 12 is continuously fed from the first roll. An alignment layer 22 is continuously formed on the first substrate 12. A polarizer-forming composition is continuously applied onto the alignment layer 22. The applied polarizer-forming composition is dried under conditions that do not polymerize the liquid crystal compound, thereby continuously forming a dry coating on the alignment layer 22. The liquid crystal compound contained in the dry coating is made into a nematic liquid crystal phase, preferably a smectic liquid crystal phase. Thereafter, the liquid crystal compound is polymerized while maintaining the smectic liquid crystal phase, thereby continuously obtaining a polarizing layer 21 to obtain a polarizer 11. The continuously obtained polarizer 11 is wound around a second core to obtain a second roll.

[0155] The polarizing plate 1 obtained by this production method is a long, film-like polarizing film. When this polarizing plate 1 is used as a lens for sunglasses or the like described below, it is cut to fit the dimensions of the lenses for sunglasses or the like.

[0156] The polarizing plate 1 can be in the form of a laminate of the first substrate 12 / the alignment layer 22 / the polarizing layer 21. Furthermore, the polarizing plate 1 may be in the form of a laminate of layers or films other than the first substrate 12 / the alignment layer 22 / the polarizing layer 21. As these layers and films, the polarizing plate 1 may further include a retardation film, or may further include an antireflection layer or a brightness enhancement film.

[0157] For example, the polarizing plate 1 of this embodiment becomes a circular polarizing plate 2 by further comprising a quarter-wave plate. FIG. 3 is a schematic cross-sectional view of a circular polarizing plate in one embodiment of the present invention. The circular polarizing plate 2 includes a first base material 12 having an alignment layer 22 disposed on one surface thereof, a polarizing layer 21 provided on the alignment layer 22, and a retardation film 15, which is a quarter-wave plate, disposed on the other surface of the first base material 12. The retardation film 15 may be located on the second surface 32 of the polarizer 11. In this case, as shown in FIG. 4, the circular polarizing plate 2′ may take a form in which the first base material 12, the alignment layer 22, the polarizing layer 21, and the retardation film 15 are disposed in this order.

[0158] When producing a circularly polarizing plate, a suitable adhesive may be used, and the first base material 12 or the polarizer 11 may be bonded to the retardation film 15 via an adhesive layer formed from the adhesive.

[0159] By using the first base material 12 to which retardation has been imparted in advance, the first base material 12 itself may also function as a retardation layer. By making the first base material 12 itself a retardation film, it is also possible to make a circular polarizing plate or an elliptical polarizing plate in the form of first base material 12 / alignment layer 22 / polarizing layer 21. The ¼ wavelength plate used in producing the circular polarizing plate in this way preferably has a property that the in-plane retardation value for visible light decreases as the wavelength becomes shorter.

[0160] It is also possible to produce a linear polarizing plate roll by using a 1 / 2 wavelength plate as the phase difference film 15 and setting the angle between its slow axis and the absorption axis of the polarizer 11 to be shifted, and further forming a 1 / 4 wavelength plate on the side opposite to the side on which the polarizer 11 is formed, thereby producing a broadband circular polarizing plate.

[0161] The birefringence of the quarter wavelength plate used as the retardation film 15 to light having a wavelength of 450 nm, the birefringence to light having a wavelength of 550 nm, and the birefringence to light having a wavelength of 650 nm preferably have reverse wavelength dispersion properties that satisfy the relationships shown in the following formulas (II) and (III), where Δn(λ) represents the birefringence to light having a wavelength of λ nm. Δn(450) / Δn(550)≦1.00 (II) 1.00≦Δn(650) / Δn(550) (III) A retardation film exhibiting such reverse wavelength dispersion characteristics can be produced by the method described in Japanese Patent No. 5463666.

[0162] Methods for forming the curved portion by heating the polarizing plate 1 of this embodiment include insert molding, injection molding, compressed air molding, vacuum molding, die pressing, and the like.

[0163] The polarizing plate 1 in this embodiment has small thermal shrinkage and is thin, and therefore can have curved portions with a small radius of curvature.

[0164] In one aspect of the present invention, the first substrate 12 is preferably an acrylic resin film or a cyclic olefin resin film. When such a thermoplastic resin substrate is used, it is possible to realize a polarizing plate 1 having a curved portion with a small radius of curvature due to its ease of processing at low temperatures and good thermoformability.

[0165] In one aspect of the present invention, the liquid crystal compound is preferably a compound represented by the following formula (4-6) or (4-7).

[0166] [ka]

[0167] [ka]

[0168] In one aspect of the present invention, the dichroic dye 102 preferably contains at least one selected from the group consisting of the compound represented by formula (2-15), the compound represented by formula (2-18), and the compound represented by formula (2-37). The compound represented by formula (2-15) has a maximum absorption wavelength at 380 nm. The compound represented by formula (2-18) has a maximum absorption wavelength at 490 nm. The compound represented by formula (2-37) has a maximum absorption wavelength at 590 nm. By using these dichroic dyes, a polarizing plate with high polarization properties can be realized. More preferably, the dichroic dye 102 contains the compound represented by formula (2-15), the compound represented by formula (2-18), and the compound represented by formula (2-37).

[0169] [ka]

[0170] [ka]

[0171] [ka]

[0172] In one aspect of the present invention, the polarizing plate 1 preferably includes an acrylic resin film as the first thermoplastic resin substrate (first substrate 12), includes a compound represented by formula (4-6) and a compound represented by formula (4-7) as liquid crystal compounds, and includes a compound represented by formula (2-15), a compound represented by formula (2-18), and a compound represented by formula (2-37) as dichroic dye 102. In such a polarizing plate 1, there is no need to provide a second substrate, and a thinner polarizing plate can be realized, so that a polarizing plate having a curved portion with a small radius of curvature can be realized.

[0173] In one aspect of the present invention, the polarizing plate 1 preferably has a first thermoplastic resin substrate (first substrate 12) having a thickness of 20 μm to 200 μm, a polarizing layer 21 having a thickness of 1 μm to 5 μm, and an alignment layer 22 having a thickness of 10 nm to 1000 nm. With such a polarizing plate 1, a thinner polarizing plate can be realized, and therefore a polarizing plate having a curved portion with a small radius of curvature can be realized.

[0174] <Second embodiment> The polarizing plate according to the second embodiment of the present invention is different from the first embodiment in that the polarizer has a polarizing layer in which iodine or a dichroic dye is oriented in a PVA film. In addition, the polarizer in this embodiment does not need to have an alignment layer because the polarizing layer does not contain a liquid crystal compound. That is, the polarizer of this embodiment may have only a polarizing layer. The configuration of this embodiment other than the polarizer is the same as that of the first embodiment.

[0175] Specific examples of the polarizing layer of the present embodiment include a polarizing layer in which iodine is adsorbed to a PVA film, a polarizing layer in which a dichroic dye is adsorbed and oriented to a PVA film, and a polarizing layer having a dichroic dye on at least one of the surface and the inside of a modified PVA film containing a cationic group in the molecule, etc. The dichroic dye may be any of the dichroic dyes described above.

[0176] By setting the thickness of a polarizer having a polarizing layer in which iodine or a dichroic dye is oriented in a PVA film to 15 μm or less, it is possible to reduce shape change even when the polarizer is placed in a high-temperature environment after being molded into a curved surface.

[0177] In the case of a polarizing layer in which iodine is oriented in a PVA film, the moisture content of the PVA film is usually 5 to 20% by weight, and preferably 8 to 15% by weight. If the moisture content is less than 5% by weight, the polarizing layer loses flexibility and may be damaged or broken after drying. If the moisture content is more than 20% by weight, the polarizing layer may have poor thermal stability.

[0178] The substrate to be laminated with the polarizer in this embodiment can be the first substrate and the second substrate described in embodiment 1. Since the polarizer in this embodiment has a thickness of 15 μm or less, the shape change is small even when the polarizer is placed in a high-temperature environment after being curved.

[0179] The polarizing plate of this embodiment may have only a first base material laminated on a polarizer, as in the first embodiment. The polarizing plate may include a polarizer, a first base material located on a first surface of the polarizer, and a second base material located on a second surface of the polarizer, as in the first embodiment.

[0180] The method for producing such a polarizing layer is not particularly limited, and examples thereof include known methods such as a method of stretching a PVA film and then adsorbing iodine ions to the PVA film, a method of dyeing a PVA film with a dichroic dye and then stretching the PVA film, a method of stretching a PVA film and then dyeing the PVA film with a dichroic dye, a method of printing a dichroic dye on a PVA film and then stretching the PVA film, and a method of stretching a PVA film and then printing a dichroic dye. In order to make the thickness of the polarizing layer 15 μm or less, it is preferable to use a PVA film having a thickness of 30 μm or less before stretching.

[0181] For example, a polarizing layer can be produced by dissolving iodine in a potassium iodide solution to prepare high-order iodine ions, adsorbing these iodine ions to a PVA film, stretching the film, and then immersing the film in a 1-4 wt % aqueous boric acid solution at a bath temperature of 30-40° C. Alternatively, a polarizing layer can be produced by similarly treating a PVA film with boric acid, stretching the film uniaxially by about 3-7 times, immersing the film in a 0.05-5 wt % aqueous dichroic dye solution at a bath temperature of 30-40° C. to adsorb the dye, and drying and heat fixing the film at 80-100° C.

[0182] Moreover, the polarizer of this embodiment can also be used as a circular polarizing plate by further providing a quarter-wave plate.

[0183] Methods for forming a curved portion by heating the polarizing plate having the polarizer of this embodiment include insert molding, injection molding, compressed air molding, vacuum molding, die pressing, and the like, as in the above-mentioned methods.

[0184] The polarizing plate of this embodiment has a polarizer thickness of 15 μm or less, and therefore has smaller thermal shrinkage than a conventional polarizing plate containing a stretched PVA polarizer having a thickness of 20 μm to 30 μm. Also, the polarizing plate of this embodiment can have a curved portion with a small radius of curvature.

[0185] <Applications of polarizing plates> The polarizing plate or circular polarizing plate in this embodiment can be used in various articles having a curved portion, for example, lenses of sunglasses, lenses of goggles for three-dimensional image display devices, etc. The polarizing plate or circular polarizing plate in this embodiment can be attached to a curved surface with a small radius of curvature, which contributes to improving design.

[0186] The polarizing plate in this embodiment can be used in various display devices having a curved display surface. A display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of display devices include liquid crystal display devices, organic electroluminescence (EL) display devices, inorganic electroluminescence (EL) display devices, electron emission display devices (e.g., field emission display devices (FEDs) and surface field emission displays (SEDs)), electronic paper (display devices using electronic ink or electrophoretic elements, plasma display devices, projection display devices (e.g., grating light valve (GLV) display devices, display devices having digital micromirror devices (DMDs)), and piezoelectric ceramic displays.

[0187] Examples of liquid crystal display devices include transmissive liquid crystal display devices, semi-transmissive liquid crystal display devices, and reflective liquid crystal display devices. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images.

[0188] The polarizing plate of this embodiment can be effectively used in a display device, particularly an organic EL display device or an inorganic EL display device. Since the polarizing plate or circular polarizing plate of this embodiment can be attached to a curved surface with a small radius of curvature, even if the display device has a curved portion at an edge or corner, the polarizing plate or circular polarizing plate can be attached to cover the curved surface, which contributes to improving the design.

[0189] Examples of electronic paper include those that are displayed by molecules such as optical anisotropy and dye molecule orientation, those that are displayed by particles such as electrophoresis, particle movement, particle rotation, and phase change, those that are displayed by moving one end of a film, those that are displayed by molecular color development / phase change, those that are displayed by molecular light absorption, and those that are displayed by spontaneous emission of light due to the combination of electrons and holes.

[0190] More specifically, examples of the electrophoretic materials include microcapsule electrophoresis, horizontal migration electrophoresis, vertical migration electrophoresis, spherical twist ball, magnetic twist ball, cylindrical twist ball, charged toner, electronic liquid powder, magnetic migration type, magnetic heat sensitive type, electrowetting, light scattering (transparent / opaque change), cholesteric liquid crystal / photoconductive layer, cholesteric liquid crystal, bistable nematic liquid crystal, ferroelectric liquid crystal, dichroic dye / liquid crystal dispersion type, movable film, color development / erasing by leuco dye, photochromic, electrochromic, electrodeposition, flexible organic EL, etc. Electronic paper may be used not only for personal use of text and images, but also for advertising display (signage) and the like. According to the polarizing plate or circular polarizing plate of the present embodiment, the thickness of the electronic paper can be reduced.

[0191] As a stereoscopic display device, a method of arranging different retardation films alternately, such as the micropole method, has been proposed (JP Patent Publication No. 2002-185983). However, when the polarizing plate of this embodiment is used, patterning is easy by printing, inkjet, photolithography, etc., so that the manufacturing process of the display device can be shortened and retardation films are not required.

[0192] The polarizing plate and the circular polarizing plate of this embodiment can be used in a display device having a curved portion with a small radius of curvature. Specifically, the polarizing plate can be attached to a smartphone having a curved portion at the edge or corner of the screen. In addition, the polarizing plate and the circular polarizing plate of this embodiment can be used in a head-mounted display for VR (virtual reality). EXAMPLES

[0193] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0194] [Evaluation of curved surface formability] The curved surface of the polarizing plate was formed as follows. The polarizing plate was sandwiched between two metal plates with a 10 cm diameter hole in the center. The polarizing plate was heated to 100°C to 140°C using a heat gun. A cylindrical glass piece with a given radius of curvature was pressed against the heated polarizing plate to form a curved surface. The radius of curvature of the polarizing plate was calculated from the diameter of the curved part and the arrow height. The curved surface moldability was evaluated by visual inspection. If a curved surface was formed and no defects such as cracks occurred in the substrate or polarizer, the curved surface moldability was judged to be good, and if not, it was rated as poor.

[0195] [Measurement of Polarizer Thickness] Any five points on the polarizer were measured using a contact type film thickness meter (digital micrometer MH-15M; manufactured by Nikon Corporation), and the average value was calculated to obtain the thickness of the polarizer.

[0196] [Evaluation of shape change in high temperature environment] The polarizing plate with the curved surface formed by the above method was placed in an oven at 60°C or 80°C for 24 hours. After that, the change in shape was evaluated using a ruler. If the dimensions such as the radius of curvature and height were maintained as they were before being placed in the oven, it was judged to be good, and if not, it was judged to be bad.

[0197] Example 1 [Preparation of Polarizer-Forming Composition] The following polymerizable liquid crystal compound, dichroic dye, polymerization initiator, leveling agent, and solvent were mixed in the following ratio. The resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a polarizer. The dichroic dye was synthesized in the same manner as the compound described in JP 2013-101328 A.

[0198] (Polymerizable liquid crystal compound) As the polymerizable liquid crystal compound, the compound represented by formula (4-6) was used in an amount of 75 parts by mass, and the compound represented by formula (4-7) was used in an amount of 25 parts by mass.

[0199] [ka]

[0200] [ka]

[0201] (dichroic dye) As the dichroic dyes, 2.6 parts by mass of a compound represented by formula (2-15) (having a maximum absorption wavelength at 380 nm), 2.6 parts by mass of a compound represented by formula (2-18) (having a maximum absorption wavelength at 490 nm), and 2.2 parts by mass of a compound represented by formula (2-37) (having a maximum absorption wavelength at 590 nm) were used.

[0202] [ka]

[0203] [ka]

[0204] [ka]

[0205] (Other ingredients) As a polymerization initiator, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) was used in an amount of 6 parts by mass. As a leveling agent, a polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) was used in an amount of 1.2 parts by mass. As the solvent, o-xylene was used in an amount of 250 parts by mass.

[0206] [Method of manufacturing polarizing plate] A roll of triacetyl cellulose (TAC) film (Konica Minolta, Inc., KC4UY-TAC, thickness 40 μm) as the second substrate was continuously unwound at a speed of 10 m / min, and a composition for forming a photoalignment layer was discharged by a slot die coater to form a first coating film. Furthermore, the solvent was removed by conveying the film in a ventilated drying oven set at 120° C. for 2 minutes, and a first dry film was formed.

[0207] Then, polarized UV light polarized at 0° to the film transport direction was applied to the first dry film at 50 mJ / cm 2 (based on 313 nm) to impart an alignment control force, thereby producing a substrate film with a photo-alignment layer. A polarizer-forming composition was applied to the photo-alignment layer surface using a slot die coater to form a second coating film. The film was then transported for 2 minutes in a forced-air drying oven set at 120°C to remove the solvent, forming a second dry film.

[0208] Then, UV light was applied at 50 mJ / cm 2 A polarizer was formed by irradiating the polarizer with UV light (365 nm standard) to polymerize and harden the polymerizable liquid crystal compound. Then, an acrylic resin film (S001G, manufactured by Sumitomo Chemical Co., Ltd.), which was the first substrate, was attached to the polarizer via a UV-curable adhesive, and the film was continuously wound up into a roll to produce a polarizing film roll with an absorption axis in the 0° direction.

[0209] From the long polarizing film roll thus produced, pieces of 10 cm square were cut out and used as polarizing plates for various evaluations. The prepared polarizing plate had an alignment layer thickness of 100 nm and a polarizing layer thickness of 2 μm. The alignment layer and polarizing layer thickness were determined by measuring five arbitrary points of each layer with an interference thickness meter, a laser microscope, or a stylus-type thickness meter and calculating the average value. The evaluation results of the curved surface moldability of the polarizing plate and the shape change under high temperature environment are shown in Table 1.

[0210] (Examples 2 to 5, Comparative Example 1) The polarizing plates of Examples 2 to 5 and Comparative Example 1 were produced in the same manner as in Example 1, except that the first and second substrates and the curved surface molding were changed as shown in Table 1. In Examples 4 and 5 and Comparative Example 1, the polarizing plate was not provided with a second substrate. In Table 1, COP stands for cyclic olefin resin film (manufactured by Zeon Corporation).

[0211] Example 6 The polarizing plate of Example 6 was produced as follows. A polarizer (manufactured by Sumitomo Chemical Co., Ltd.) made of stretched PVA dyed with iodine was attached onto an acrylic resin (manufactured by Kaneka Corporation) as a first base material. A TAC film was attached to the other surface of the polarizer via an adhesive. The moisture content of this polarizer was 10% by weight.

[0212] (Examples 7 to 10, Comparative Example 2) The polarizing plates of Examples 7 to 10 and Comparative Example 2 were produced in the same manner as in Example 6, except that the first and second substrates were changed as shown in Table 1. In Examples 9 and 10 and Comparative Example 2, the polarizing plate did not have a second substrate.

[0213] [Table 1]

[0214] The polarizing plates of Examples 1 to 5 were excellent in curved surface moldability, and no change in shape was observed even in environments at 60°C and 80°C. The polarizing plates of Examples 6 to 10 were excellent in curved surface moldability, and no change in shape was observed in an environment at 60°C. However, a change in shape occurred in an environment at 80°C. This is thought to be due to the fact that the stretched PVA contracted in the stretching direction at 80°C. In addition, in Comparative Examples 1 and 2, in which a triacetyl cellulose film was used as the first substrate and no second substrate was provided, the curved surface moldability was poor. Therefore, the change in shape in a high-temperature environment could not be evaluated. [Industrial Applicability]

[0215] The polarizing plate of the present invention is suppressed from shrinking due to thermoforming, and can be attached to an object having a curved portion with a small radius of curvature. [Explanation of symbols]

[0216] Reference Signs List 1,1'... polarizing plate, 2,2'... circular polarizing plate, 11... polarizer, 12... first substrate, 13... curved portion, 14... second substrate, 15... retardation film, 101... cured liquid crystal compound, 102... dichroic dye, 21... polarizing layer, 22... alignment layer

Claims

1. A polarizing plate having a polarizer having a first surface and a second surface, and a first substrate disposed on the first surface of the polarizer, The thickness of the polarizer is 15 μm or less, The polarizer includes an alignment layer and a polarizing layer, the polarizing layer contains a cured product of a liquid crystal compound and a dichroic dye, the cured product of the liquid crystal compound is a cured product obtained by polymerizing and curing a polymerizable liquid crystal compound, the dichroic dye is dispersed and oriented in the cured product, the first base material contains at least one resin selected from the group consisting of an acrylic resin and a cyclic olefin resin; the polarizing plate has at least one curved portion; The curved portion has a radius of curvature of 30 mm to 150 mm.

2. 2. The polarizing plate according to claim 1, wherein the first substrate has a thickness of 40 μm to 120 μm.

3. The polarizing plate according to claim 1 , further comprising a second substrate on the second surface of the polarizer.

4. 4. The polarizing plate according to claim 3, wherein the second base material contains at least one selected from the group consisting of an acrylic resin, a cyclic olefin resin, and a triacetyl cellulose resin.

Citation Information

Patent Citations

  • Protection film for polarizing plate

    JP2007047498A

  • Polarized glasses

    JP2012032507A

  • Polarizing film, image display device, and method for manufacturing polarizing film

    JP2013178321A

  • Polarizing plate for curve surface and optical laminate

    JP2016200731A

  • Light polarizing spectacle lens

    US5412505A