Multilayer ceramic electronic components

By forming terminal electrodes on the outer surface and eliminating lower surface electrodes, the multilayer ceramic capacitor achieves a reduced thickness and improved strength, addressing the challenges of manufacturing thin capacitors.

JP7551280B2Active Publication Date: 2024-09-17TDK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2019100193
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-24
Filing Date
2019-05-29
Publication Date
2024-09-17
Estimated Expiration
2039-05-29

AI Technical Summary

Technical Problem

Conventional multilayer ceramic capacitors face challenges in reducing thickness due to difficulties in forming terminal electrodes on thin element bodies, which can lead to damage during immersion and plating processes.

Method used

The multilayer ceramic electronic component features terminal electrodes formed on the outer surface of the element body, with no electrodes on the lower surface, allowing for a thinner design by stacking internal electrode and insulating layers, and optionally incorporating a reinforcing layer for improved strength.

Benefits of technology

This configuration enables the production of capacitors with a total thickness of 100 μm or less, enhancing bending strength and ease of integration into substrates while maintaining electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551280000009
    Figure 0007551280000009
  • Figure 0007551280000010
    Figure 0007551280000010
  • Figure 0007551280000003
    Figure 0007551280000003
Patent Text Reader

Abstract

To provide a multilayer ceramic electronic component such as a multilayer ceramic capacitor that can be reduced in height.SOLUTION: The present invention relates to a multilayer ceramic electronic component 2. Terminal electrodes 6, 8 include: end side electrode portions 6a, 8a for covering extraction ends 4a, 4b of an element body 4 from which an internal electrode layer 12 is extracted; and upper electrode portions 6b, 8b formed continuously on the end side electrode portions 6a, 8a on a part of an upper surface of the element body 4 along a stacking direction. On a lower surface 4d of the element body 4 located on the opposite side of an upper surface 4c along the stacking direction, the terminal electrodes 6, 8 are not substantially formed.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer ceramic electronic component used, for example, as a multilayer ceramic capacitor, and more particularly to a multilayer ceramic electronic component that can be made thin. [Background technology]

[0002] For example, as shown in Patent Document 1 listed below, conventional multilayer ceramic capacitors generally have terminal electrodes at both longitudinal ends of an element body, and each terminal electrode generally has an end electrode portion of the element body and upper and lower covering electrode portions that cover the upper and lower surfaces of the element body, respectively.

[0003] The base electrode of the terminal electrode is formed by immersing the end of the element body in a solution containing conductive particles. During the immersion, a plurality of element bodies are inserted into a plurality of holding holes formed in a holding plate, and one end of each element body is immersed in the solution to form the base electrode. After that, if necessary, a plating film is formed on the base electrode to form the terminal electrode.

[0004] In any case, when forming terminal electrodes on the element body, if the element body itself does not have a certain degree of thickness, it is difficult to form the base electrode and also difficult to form a plating film. In other words, if the element body is thin, it is likely to be damaged when the element body is held in the holding hole of the holding plate. In addition, if the element body is thin, it is likely to be damaged when plating is performed. Therefore, with the structure of the conventional multilayer ceramic capacitor, it is difficult to thin the element body, and therefore it is difficult to reduce the height of the multilayer ceramic capacitor. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-28254 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a multilayer ceramic electronic component, such as a multilayer ceramic capacitor, which can be made thinner. [Means for solving the problem]

[0007] In order to achieve the above object, a multilayer ceramic electronic component according to a first aspect of the present invention comprises: An element body in which internal electrode layers and insulating layers are alternately laminated in a lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, and an upper electrode portion formed continuously with the end electrode portion on a part of an upper surface of the element body along the stacking direction, The terminal electrodes are substantially not formed on a lower surface of the element body located on the opposite side in the stacking direction to the upper surface.

[0008] A multilayer ceramic electronic component according to a second aspect of the present invention comprises: An element body in which internal electrode layers and insulating layers are alternately laminated in a lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, and an upper electrode portion formed continuously with the end electrode portion on a part of an upper surface of the element body along the stacking direction, The element body is characterized in that a lower surface thereof, which is located on the opposite side in the stacking direction to the upper surface, is entirely exposed to the outside.

[0009] In the multilayer ceramic electronic component according to the first aspect of the present invention, substantially no terminal electrodes are formed on the lower surface of the element body. In the multilayer ceramic electronic component according to the second aspect of the present invention, the entire lower surface of the element body is exposed. In the structure of conventional electronic components, simply reducing the thickness of the element body to, for example, about 100 μm or less makes it difficult to form terminal electrodes on the element body.

[0010] The multilayer ceramic electronic component of the present invention can be formed, for example, by combining two or more thin element bodies, forming terminal electrodes, and then separating the element bodies. Therefore, multilayer ceramic electronic components that are, for example, half or less the thickness of conventional ones, can be easily manufactured.

[0011] In the resulting multilayer ceramic electronic component, substantially no terminal electrodes are formed on the lower surface of the element body, or the entire lower surface of the element body is exposed. The total thickness of the multilayer ceramic electronic component can be reduced to 100 μm or less, preferably 90 μm or less, and more preferably 80 μm or less, which contributes to a reduction in the height of the multilayer ceramic electronic component.

[0012] Preferably, the lower surface of the element body is a flat surface. The flat lower surface of the element body makes it easier to embed the element body inside a substrate, for example. When the flat lower surface of the element body is placed on a mounting surface, the element body is attached in close contact with the mounting surface, improving the bending strength of the multilayer ceramic electronic component.

[0013] The upper surface or the lower surface of the element body may include a reinforcing layer made of a material having a lower elastic modulus or a lower linear thermal expansion coefficient compared to the insulating layer, The outer surface of the reinforcing layer may define an upper or lower surface of the element body.

[0014] Such a configuration improves the bending strength of the multilayer ceramic electronic component. Also, the improved strength makes it easier to increase the longitudinal dimension or width dimension of the element body, increasing the opposing area between the internal electrode layers inside the element body, and improving the characteristics of the electronic component, such as the capacitance.

[0015] The reinforcing layer may have a side covering portion that covers a side surface of the element body, thereby further improving the strength of the multilayer ceramic electronic component.

[0016] A multilayer ceramic electronic component according to a third aspect of the present invention comprises: An element body in which internal electrode layers and insulating layers are alternately laminated in a lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, The present invention is characterized in that the terminal electrodes are substantially not formed on an upper surface of the element body along the stacking direction and on a lower surface of the element body located on the opposite side of the upper surface along the stacking direction.

[0017] The multilayer ceramic electronic component of the present invention has terminal electrodes on both the bottom and top surfaces of the element body where terminal electrodes are substantially not formed, so that a thinner multilayer ceramic electronic component can be realized. [Brief description of the drawings]

[0018] [Figure 1A] FIG. 1A is a vertical sectional view of a multilayer ceramic capacitor according to one embodiment of the present invention. [Figure 1B] FIG. 1B is a vertical sectional view of a multilayer ceramic capacitor according to another embodiment of the present invention. [Figure 1C] FIG. 1C is a vertical sectional view of a multilayer ceramic capacitor in accordance with still another embodiment of the present invention. [Figure 2A]FIG. 2A is a cross-sectional view of the multilayer ceramic capacitor taken along line IIA-IIA shown in FIG. 1A. [Figure 2B] FIG. 2B is a cross-sectional view of the multilayer ceramic capacitor taken along line IIB-IIB shown in FIG. 1B. [Figure 2C] FIG. 2C is a cross-sectional view of a modified example of the multilayer ceramic capacitor shown in FIG. 2B. [Diagram 3] FIG. 3 is a plan view of the multilayer ceramic capacitor shown in FIG. 1A. [Figure 4] 4A to 4C are cross-sectional views of a main part illustrating a manufacturing process of the multilayer ceramic capacitor shown in FIG. 1A. [Diagram 5] FIG. 5 is a cross-sectional view of a main part showing an example of use of the multilayer ceramic capacitor shown in FIG. 1A. [Figure 6] FIG. 6 is a cross-sectional view of a main part showing an example of use of the multilayer ceramic capacitor shown in FIG. 1A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the present invention will be described based on the embodiments shown in the drawings.

[0020] First embodiment As an example of the multilayer ceramic electronic component according to this embodiment, a multilayer ceramic capacitor will be described.

[0021] 1A, the multilayer ceramic capacitor 2 according to this embodiment has an element body 4, a first terminal electrode 6, and a second terminal electrode 8. The element body 4 has inner dielectric layers (insulating layers) 10 that are substantially parallel to a plane including the X-axis and Y-axis, and internal electrode layers 12, and the internal electrode layers 12 are alternately laminated between the inner dielectric layers 10 along the direction of the Z-axis. Here, "substantially parallel" means that most parts are parallel, but there may be some parts that are not parallel, and the internal electrode layers 12 and the inner dielectric layers 10 may have some unevenness or be inclined.

[0022] The portion where the inner dielectric layers 10 and the internal electrode layers 12 are alternately laminated constitutes the interior region 13. The element body 4 also has exterior regions 11 on both end faces in the lamination direction Z (Z-axis). The exterior region 11 is formed by laminating a plurality of outer dielectric layers that are thicker than the inner dielectric layers 10 constituting the interior region 13. The thickness of the interior region 13 in the Z-axis direction is preferably within a range of 10 to 75% of the total thickness z0 of the multilayer ceramic capacitor 2. The total thickness of the two outer regions 11 is the total thickness Z0 minus the thickness of the interior region 13 and the thickness of the terminal electrodes 6, 8.

[0023] In the following, the "inner dielectric layer 10" and the "outer dielectric layer" may be collectively referred to as the "dielectric layer".

[0024] The materials of the dielectric layers constituting the inner dielectric layer 10 and the exterior region 11 may be the same or different and are not particularly limited. For example, ABO 3 It is mainly composed of a dielectric material with a perovskite structure such as

[0025] ABO 3 In the formula, A is, for example, at least one of Ca, Ba, Sr, etc., and B is at least one of Ti, Zr, etc. The molar ratio of A / B is not particularly limited and is 0.980 to 1.020. Other minor components include oxides of rare earth elements (at least one selected from Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu), alkaline earth metals (Mg and Mn), and transition metals (at least one selected from V, W, and Mo), and mixtures thereof, composite oxides, and glass such as SiO 2 A sintering aid containing the above may be included.

[0026] One of the alternately stacked internal electrode layers 12 has a lead portion 12a electrically connected to the inside of the first terminal electrode 6 formed on the outside of a first end portion in the Y-axis direction of the element body 4. The other of the alternately stacked internal electrode layers 12 has a lead portion 12b electrically connected to the inside of the second terminal electrode 8 formed on the outside of a second end portion in the Y-axis direction of the element body 4.

[0027] In the figure, the X-axis, Y-axis and Z-axis are mutually perpendicular, the Z-axis coincides with the stacking direction of the inner dielectric layers 10 and the internal electrode layers 12, and the Y-axis coincides with the direction in which the lead portions 12a, 12b are led out.

[0028] The interior region 13 has a capacitance region and an extraction region. The capacitance region is a region where the internal electrode layers 12 are laminated with the inner dielectric layer 10 sandwiched therebetween along the lamination direction. The extraction region is a region located between the extraction parts 12a (12b) of the internal electrode layers 12 connected to the terminal electrodes 6 or 8. Furthermore, the side gap region 14 shown in FIG. 2A is a region for protecting the internal electrodes 12 located at both ends of the internal electrode layer 12 in the X-axis direction, and is generally made of a dielectric material similar to that of the inner dielectric layer 10 or the exterior region 11. However, the side gap region 14 may be made of a glass material or the like that serves as a reinforced layer described later. The exterior region 11 may also be made of a glass material or the like.

[0029] The conductive material contained in the internal electrode layer 12 is not particularly limited, and metals such as Ni, Cu, Ag, Pd, Al, Pt, etc., or alloys thereof can be used. As the Ni alloy, an alloy of Ni and one or more elements selected from Mn, Cr, Co, and Al is preferable, and the Ni content in the alloy is preferably 95% by weight or more. Note that Ni or the Ni alloy may contain various trace elements such as P in an amount of about 0.1% by weight or less.

[0030] The material of the terminal electrodes 6, 8 is not particularly limited, and may be at least one of Ni, Pd, Ag, Au, Cu, Pt, Rh, Ru, Ir, etc., or an alloy thereof. Usually, Cu, Cu alloy, Ni or Ni alloy, Ag, Ag-Pd alloy, In-Ga alloy, etc. are used.

[0031] In this embodiment, the terminal electrodes 6 and 8 are formed in close contact with the end faces 4a and 4b of the element body 4 in the Y-axis direction, respectively, and may be a single film or a multi-layer film. The terminal electrodes 6 and 8 in this embodiment have end electrode portions 6a and 8a that cover the end faces 4a and 4b, which are the drawn-out ends of the element body 4 from which the lead portions 12a and 12b of the internal electrode layer 12 are drawn out. In addition, the terminal electrodes 6 and 8 have upper electrode portions 6b and 8b that are formed continuously with the end electrode portions 6a and 8a on a part of the upper surface 4c of the element body 4 along the Z-axis, which is the lamination direction.

[0032] 2A, the terminal electrodes 6 and 8 have side electrode portions 6c and 8c formed continuously with the upper electrode portions 6b and 8b and the end electrode portions 6a and 8a (see FIG. 1A) on the side surfaces 4e and 4e opposite to each other along the X-axis of the element body 4. As shown in FIG. 1A, the terminal electrodes 6 and 8 are insulated from each other by a predetermined distance in the Y-axis direction on the outer surface of the element body 4.

[0033] The thicknesses of the upper electrode portions 6b, 8b, the end electrode portions 6a, 8a, and the side electrode portions 6c, 8c of the terminal electrodes 6 and 8 may be the same or different, and are within a range of, for example, 2 to 15 μm. In this embodiment, the thicknesses of the upper electrode portions 6b, 8b and the side electrode portions 6c, 8c are 100 to 750% greater than the thickness of the end electrode portions 6a, 8a.

[0034] In this embodiment, the terminal electrodes 6, 8 are not substantially formed on the lower surface 4d of the element body 4, which is located on the opposite side along the Z-axis direction to the upper surface 4c of the element body 4. That is, the lower surface 4d of the element body is not covered with the terminal electrodes 6, 8, and the entire lower surface 4d of the element body 4 is exposed to the outside. Moreover, the lower surface 4d is formed into a flat surface. Since the lower surface 4d is not covered with the terminal electrodes 6, 8, unlike the upper surface 4c, there is no stepped convex portion due to the upper electrode portions 6b, 8b, and the lower surface 4d has excellent flatness.

[0035] The shape and size of the multilayer ceramic capacitor 2 may be determined appropriately depending on the purpose and application; however, in this embodiment, the total thickness z0 of the multilayer ceramic capacitor 2 in the Z-axis direction can be made thin, for example, to 100 μm or less, preferably 90 μm or less, and more preferably 80 μm or less, which contributes to a low profile of the multilayer ceramic capacitor 2.

[0036] In this embodiment, the length y0 in the Y-axis direction, which is the longitudinal length of capacitor 2, can be set to three times or more the thickness z0, preferably 300 μm or more, and preferably 400 to 1200 μm. Also, the width x0 in the X-axis direction of capacitor 2 can be set to two times or more the thickness z0, preferably 200 μm or more, and preferably 200 to 600 μm.

[0037] In this embodiment, the longitudinal direction of the capacitor 2 can be designed to be the X-axis direction and the lateral direction to be the Y-axis direction, in which case the length x0 in the X-axis direction can be set to three times or more the thickness z0, preferably 300 μm or more, and preferably 400 to 1200 μm. The width y0 in the y-axis direction of the multilayer ceramic capacitor 2 can be set to two times or more the thickness z0, preferably 200 μm or more, and preferably 200 to 600 μm.

[0038] According to the multilayer ceramic capacitor of this embodiment, the total thickness z0 of the multilayer ceramic capacitor 2 in the Z-axis direction can be reduced to, for example, 100 μm or less, preferably 90 μm or less, and more preferably 80 μm or less. In addition, since the lower surface 4d of the element body 4 is a flat surface, the capacitor 2 can be easily embedded inside the multilayer substrate 40, for example, as shown in FIG. 5. In FIG. 5, the wiring pattern 42 formed on the multilayer substrate 40 is connected to the upper electrode portions 6b, 8b of the terminal electrodes 6, 8 of the capacitor 2 by supplementing through-hole electrodes or the like. In addition, in this embodiment, when the flat surface, which is the lower surface of the element body 4, is placed on the mounting surface, the element body 4 is attached in close contact with the mounting surface, and the bending strength of the multilayer ceramic capacitor 2 is improved.

[0039] The multilayer ceramic capacitor 2 of this embodiment may be mounted on a circuit board 40a using solder 50, as shown in Fig. 6. In that case, the multilayer ceramic capacitor 2 is disposed upside down in the Z-axis direction, and the upper electrode portions 6b, 8b of the terminal electrodes 6 and 8 face downward in the drawing and are connected to the wiring pattern 42a of the circuit board 40a by the solder 50. A solder fillet is formed in the solder 50, and the solder 50 also comes into contact with the end electrode portions 6a, 8a of the terminal electrodes 6, 8.

[0040] In this embodiment, the exterior region 11 constituting the upper surface 4c or the lower surface 4d of the element body 4 may be made of a dielectric material having a higher strength than the inner dielectric layer 10. This configuration further improves the bending strength of the multilayer ceramic capacitor 2. The improved strength also makes it easier to increase the longitudinal dimension y0 or width dimension x0 of the element body 4, and increases the opposing area between the internal electrode layers 12 inside the element body 4, improving characteristics such as capacitance. Furthermore, the side gap region 14 shown in FIG. 2A may also be made of a dielectric material having a higher strength than the inner dielectric layer 10.

[0041] Next, a method for manufacturing the multilayer ceramic capacitor 2 according to one embodiment of the present invention will be specifically described.

[0042] First, a paste for an inner green sheet and a paste for an outer green sheet are prepared to manufacture an inner green sheet that will constitute the inner dielectric layer 10 and an outer green sheet that will constitute the exterior region 11 after firing, as shown in Fig. 1. The paste for the inner green sheet and the paste for the outer green sheet are usually composed of an organic solvent-based paste obtained by kneading a ceramic powder with an organic vehicle, or a water-based paste.

[0043] The raw material of the ceramic powder can be appropriately selected from composite oxides and various compounds that become oxides, such as carbonates, nitrates, hydroxides, and organometallic compounds, and can be used by mixing them. In this embodiment, the raw material of the ceramic powder is used as a powder having an average particle size of 0.45 μm or less, preferably about 0.1 to 0.3 μm. In order to make the inner green sheet extremely thin, it is desirable to use a powder that is finer than the thickness of the green sheet.

[0044] The organic vehicle is a binder dissolved in an organic solvent. The binder used in the organic vehicle is not particularly limited, and may be appropriately selected from various common binders such as ethyl cellulose, polyvinyl butyral, etc. The organic solvent used is also not particularly limited, and may be appropriately selected from various organic solvents such as acetone, methyl ethyl ketone, etc.

[0045] The green sheet paste may contain additives selected from various dispersants, plasticizers, dielectrics, minor component compounds, glass frits, insulators, and the like, as necessary.

[0046] Examples of the plasticizer include phthalates such as dioctyl phthalate and benzyl butyl phthalate, adipic acid, phosphates, and glycols.

[0047] Next, in order to manufacture an internal electrode pattern layer that will constitute the internal electrode layer 12 shown in Fig. 1A after firing, a paste for the internal electrode layer is prepared. The paste for the internal electrode layer is prepared by kneading the conductive material made of the various conductive metals and alloys described above with the organic vehicle described above.

[0048] The terminal electrode paste, which will constitute the terminal electrodes 6, 8 shown in FIG. 1A after firing, may be prepared in the same manner as the above-mentioned internal electrode layer paste.

[0049] Using the inner green sheet paste and the inner electrode layer paste prepared above, the inner green sheets and the inner electrode pattern layers are alternately laminated to produce an inner laminate, as shown in Fig. 4. Then, after producing the inner laminate, the outer green sheets are formed using the outer green sheet paste, and pressed in the lamination direction to obtain a green laminate.

[0050] As a method for producing the green laminate, in addition to the above, a predetermined number of inner green sheets and internal electrode pattern layers may be laminated alternately directly on an outer green sheet, and pressed in the lamination direction to obtain a green laminate.

[0051] Specifically, first, an inner green sheet is formed on a carrier sheet (for example, a PET film) as a support by a doctor blade method, etc. After being formed on the carrier sheet, the inner green sheet is dried.

[0052] Next, an internal electrode pattern layer is formed on the surface of the internal green sheet using the internal electrode layer paste, to obtain an internal green sheet having the internal electrode pattern layer. Next, a plurality of the internal green sheets having the internal electrode pattern layer are laminated to produce an internal laminate, and then an appropriate number of external green sheets are formed on the top and bottom of the internal laminate using the external green sheet paste, and pressed in the lamination direction to obtain a green laminate.

[0053] Next, the green laminate is cut into individual pieces to obtain green chips. The method for forming the internal electrode pattern layer is not particularly limited, and may be formed by a printing method, a transfer method, or a thin film forming method such as deposition or sputtering.

[0054] The green chip is solidified by removing the plasticizer through solidification and drying. After solidification and drying, the green chip is subjected to a binder removal step, a firing step, and an annealing step as required to obtain the element body 4. The binder removal step, the firing step, and the annealing step may be performed consecutively or independently.

[0055] Next, terminal electrode paste is applied to both end faces in the Y-axis direction of the element body 4 and fired to form the terminal electrodes 6, 8. When forming the terminal electrodes 6, 8, for example, as shown in Fig. 4, a dummy block 20 is temporarily bonded between the lower surfaces 4d, 4d of the two element bodies 4, 4 to first form a workpiece 22 by integrating them.

[0056] The dummy block 20 is preferably made of a material that can be removed in a later process and is preferably made of a material to which the terminal electrode paste does not easily adhere. The dummy block 20 is made of, for example, silicone rubber, nitrile rubber, polyurethane, fluororesin, PET resin, PEN resin, etc. The width of the dummy block 20 in the X-axis direction and the width of the dummy block 20 in the Y-axis direction are preferably approximately the same as the size of the element body 4. The thickness of the dummy block 20 in the Z-axis direction may be equal to the thickness of the element body 4 in the Z-axis direction, or may be thinner or thicker than it.

[0057] The workpiece 22 may be formed by directly bonding the lower surfaces 4d, 4d of the two element bodies 4, 4 with a peelable adhesive in a later process without providing the dummy block 20. Preferred adhesives include modified silicone polymer, PVA aqueous solution glue, water-soluble acrylic resin aqueous solution glue, modified polyurethane, a two-liquid type of modified silicone + epoxy resin, starch glue, etc. Also, instead of the dummy block 20, one or more element bodies 4 may be bonded between the two element bodies 4, 4 to form the workpiece 22.

[0058] Since the workpiece 22 is a combination of two or more element bodies 4, 4, even if the element bodies 4, 4 themselves are thin in the Z-axis direction, the workpiece 22 has a thickness that is easy to handle, and the terminal electrodes 6 and 8 can be formed by attaching the workpiece 22 to the through holes 32 of the holding plate 30 in the same manner as in the past. The method of forming the terminal electrodes 6, 8 is not particularly limited, and appropriate methods such as application and baking of terminal electrode paste, plating, vapor deposition, and sputtering can be used. If necessary, a coating layer is formed on the surfaces of the terminal electrodes 6, 8 by plating or the like. Examples of the coating layer include gold plating and tin plating.

[0059] After the terminal electrodes 6 and 8 are formed, the two element bodies 4, 4 are separated by, for example, removing the dummy block 20, thereby obtaining the multilayer ceramic electronic component 2 shown in Fig. 1A. In other words, the terminal electrodes 6, 8 are substantially not formed on the lower surface 4d of the element body 4, and the capacitor 2 is obtained in which the entire lower surface 4d of the element body 4 is exposed to the outside.

[0060] The multilayer ceramic capacitor 2 of this embodiment thus manufactured is mounted on a printed circuit board by soldering or the like and used in various electronic devices, etc. Alternatively, as shown in Fig. 5, the capacitor 2 is embedded inside a multilayer substrate 40 for use.

[0061] The laminated ceramic capacitor 2 of this embodiment becomes a laminated ceramic capacitor that is, for example, half or less the thickness of a conventional laminated ceramic capacitor, by separating the element body after the formation of the terminal electrodes 6, 8.

[0062] In the resulting multilayer ceramic capacitor 2, the terminal electrodes 6, 8 are not substantially formed on the lower surface of the element body 4, or the entire lower surface 4d of the element body 4 is exposed. The total thickness z0 of the multilayer ceramic capacitor can be reduced to 100 μm or less, preferably 90 μm or less, and more preferably 80 μm or less. In other words, this contributes to reducing the height of the multilayer ceramic capacitor.

[0063] In this embodiment, the lower surface 4d of the element body 4 is a flat surface. Since the lower surface 4d of the element body 4 is a flat surface, it becomes easier to embed the capacitor 2 inside the multilayer substrate 40, for example, as shown in Fig. 5. When the flat surface, which is the lower surface 4d of the element body 4, is placed on the mounting surface, the element body 4 is attached in close contact with the mounting surface, improving the bending strength of the multilayer ceramic electronic capacitor.

[0064] Second embodiment 1B and 2B, the multilayer ceramic capacitor 2a according to this embodiment is similar to the multilayer ceramic capacitor 2 according to the first embodiment, except as described below. In this capacitor 2a, the upper surface 4c (or the lower surface 4d) of the element body 4 includes a reinforcing layer 16 made of a material stronger than the inner dielectric layer 10, and the outer surface of the reinforcing layer 16 defines the upper surface 4c (or the lower surface 4d) of the element body 4.

[0065] The reinforcing layer 16 is formed on the upper surface 4c (or lower surface 4d) of the element body 4 after the element body 4 is formed in the same manner as in the first embodiment, and before the terminal electrodes 6 and 8 are formed. The reinforcing layer 16 is not particularly limited, but examples thereof include glass, an alumina-based composite material, a zirconia-based composite material, a polyimide resin, an epoxy resin, an aramid fiber, and a fiber-reinforced plastic.

[0066] Such a configuration improves the bending strength of the multilayer ceramic capacitor 2a. Furthermore, the improved strength makes it easy to increase the longitudinal dimension y0 (see FIG. 1A) or width dimension x0 (see FIG. 2A) of the element body 4 even if the element body 4 is thinned, and the opposing area between the internal electrode layers 12 inside the element body 4 becomes larger, further improving the characteristics of the capacitor 2b, such as the capacitance.

[0067] The glass component constituting the reinforced layer 16 is not particularly limited, but may be SiO 2 , BaO, Al 2 O 3 , alkali metals, CaO, SrO, B 2 O 3 It is preferable that the glass component constituting the reinforcement layer 16 contains SiO. 2 The glass component of the reinforced layer 16 preferably contains 30 to 70 mass % of SiO. 2 When the content of SiO is within the above range, the amount of the network-forming oxide is sufficient, and plating resistance is improved, compared with when the content is less than the above range. 2 When the content is within the above range, the softening point is prevented from becoming too high, and the working temperature is prevented from becoming too high, as compared with the case where the content is greater than the above range.

[0068] BaO contained as a glass component constituting the reinforced layer 16 of this embodiment is preferably contained in the glass component of the reinforced layer 16 at 20 to 60 mass %. When BaO is contained in the above range, the adhesion with the dielectric is improved and delamination is less likely to occur, compared to when the BaO content is less than the above range. In addition, the thermal expansion coefficient is prevented from becoming too small, making it less likely to cause cracks. Furthermore, when the dielectric layer is BaTiO 3 In this case, Ba is prevented from dissolving into the glass components, and the deterioration of HALT reliability is suppressed. When BaO is contained within the above range, vitrification is improved and plating resistance is also improved compared to when the BaO content is more than the above range.

[0069] Al contained as a glass component constituting the reinforced layer 16 of this embodiment 2 O3 The glass component of the reinforced layer 16 preferably contains 1 to 15 mass % of Al. 2 O 3 When the content of Al is within the above range, the plating resistance is better than when the content is less than the above range. 2 O 3 When the content is within the above range, the softening point is prevented from rising too much, compared to when the content is greater than the above range.

[0070] In the present embodiment, the glass component constituting the reinforced layer 16 contains SiO 2 and BaO and Al 2 O 3 It is preferable that the total content is 70 to 100 mass %. This makes it easier for a Ba-Ti-Si-O phase to form at the interface between the dielectric material and the reinforcing layer 16.

[0071] Examples of alkali metals contained as the glass component constituting the reinforced layer 16 of this embodiment include Li, Na, and K, and from the viewpoint of thermal expansion coefficient, K and Na are more preferable. The alkali metal contained as the glass component constituting the reinforced layer 16 of this embodiment is preferably contained in the glass component of the reinforced layer at 0.1 to 15 mass %. This can increase the thermal expansion coefficient. When the alkali metal is contained in the above range, plating resistance can be improved compared to when it is contained more than the above range.

[0072] CaO contained as a glass component constituting the reinforced layer 16 of this embodiment is preferably contained in an amount of 0 to 15 mass % in the glass component of the reinforced layer 16. This can increase the thermal expansion coefficient and improve plating resistance.

[0073] The SrO contained as a glass component constituting the reinforced layer 16 of this embodiment is preferably 0 to 20 mass % in the glass component of the reinforced layer 16. This makes it possible to increase the thermal expansion coefficient and improve plating resistance. When SrO is contained within the above range, the content of SrO is more than that when the content is more than the above range, and the content of BaTiO 3 This prevents the chip from reacting with the metal, thereby improving the insulation and reliability of the chip.

[0074] B contained as a glass component constituting the reinforced layer 16 of this embodiment 2 O 3 It is preferable that the glass component of the reinforced layer 16 contains 0 to 10 mass % of B. This allows the effect of the oxide forming the glass network to be exerted. 2 O 3 When the content is within the above range, the plating resistance can be improved compared to when the content is greater than the above range.

[0075] In this embodiment, the reinforcing layer 16 constitutes only a part of the outer surface side of the exterior region 11, but it may occupy most or all of the exterior region 11. The reinforcing layer 16 can be formed by applying a reinforcing layer paste to the upper surface 4c or the lower surface 4d of the element body 4 and baking it.

[0076] The reinforcing layer paste is obtained by kneading the above-mentioned glass raw material, a binder mainly composed of ethyl cellulose, and terpineol and acetone as dispersion media in a mixer. The method of applying the reinforcing layer paste to the element body 4 is not particularly limited, and examples of the method include dipping, printing, coating, vapor deposition, spraying, etc.

[0077] The conditions for baking the element body 4 on which the reinforcing layer paste has been applied are not particularly limited. For example, 2 or dry N 2 The material is baked in an atmosphere of 700°C to 1300°C for 0.1 to 3 hours.

[0078] Third embodiment As shown in Fig. 2C, the multilayer ceramic capacitor 2b according to this embodiment is similar to the multilayer ceramic capacitor 2a according to the second embodiment, except as described below. In this capacitor 2b, the reinforcing layer 16 has a side covering portion 16a that covers the side surface 4e of the element body 4. The side covering portion 16a is formed continuously with the reinforcing layer 16 of the second embodiment. This configuration further improves the strength of the multilayer ceramic capacitor.

[0079] 2C, the side covering portion 16a configures only a portion of the side gap region 14 on the side face 4e side, but it may occupy the entire side gap region 14. In other words, the side covering portion 16a may be in contact with the end portion of the internal electrode layer 12 in the X-axis direction.

[0080] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention.

[0081] For example, when one or more element bodies 4 are arranged and bonded in place of the dummy block 20 shown in Fig. 4, only the end electrode portions 6a, 8a and the side electrode portions 6c, 8c are formed on those element bodies 4. That is, in that case, as shown in Fig. 1C, a multilayer ceramic capacitor having terminal electrodes 6, 8 on both the lower surface 4d and the upper surface 4c of the element body 4 where the terminal electrodes 6, 8 are not substantially formed is obtained. Since this multilayer ceramic capacitor 2c has terminal electrodes on both the lower surface 4d and the upper surface 4c of the element body 4 where the terminal electrodes 6, 8 are not substantially formed, an even thinner capacitor is obtained.

[0082] Furthermore, the multilayer ceramic electronic component of the present invention is not limited to a multilayer ceramic capacitor, but can be applied to other multilayer electronic components. Examples of other multilayer electronic components include all electronic components in which dielectric layers (insulating layers) are laminated via internal electrodes, such as bandpass filters, inductors, multilayer three-terminal filters, piezoelectric elements, PTC thermistors, NTC thermistors, and varistors. [Explanation of symbols]

[0083] 2, 2a, 2b, 2c... Multilayer ceramic capacitors 4... Element body 4a,4b… Pull-out end 4c…Top surface 4d…Bottom surface 4e… Side 6... 1st terminal electrode 6a… End side electrode part 6b… Upper electrode part 6c… Side electrode 8... 2nd terminal electrode 8a… End side electrode part 8b… Upper electrode part 8c… Side electrode part 10… Inner dielectric layer 11…Exterior area 12… Internal electrode layer 12a,12b…Drawer part 13… Interior area 14… Side gap area 16… Reinforcement layer 16a… Side covering part 20... Dummy block 22… Work 30… Holding plate 32...Through hole 40…Multilayer board 40a... Circuit board 42,42a... Wiring pattern 50… Solder

Claims

1. An element body having an interior region in which internal electrode layers and inner dielectric layers are alternately laminated in a lamination direction, and an exterior region including an outer dielectric layer provided at an end of the interior region in the lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, and an upper electrode portion formed contiguous to the end electrode portion on a part of an upper surface of the element body, The terminal electrode is not substantially formed on a lower surface of the element body located on the opposite side of the upper surface in the stacking direction, the upper or lower surface of the element body includes a reinforcing layer defining the upper or lower surface of the element body; The reinforcing layer is made of SiO 2 and BaO and Al 2 O 3 The glass component contains 70 to 100 mass % in total, The reinforcing layer is located on the outer surface side of the exterior region, an interface between the outer dielectric layer of the armor region and the reinforcing layer; the outer dielectric layer is mainly composed of a dielectric material having a perovskite structure containing Ti, and a Ba-Ti-Si-O phase is formed at the interface; The thickness of the multilayer ceramic electronic component is less than 100 μm, A laminated ceramic electronic component, wherein the length in the longitudinal direction of the laminated ceramic electronic component is at least three times the thickness.

2. An element body having an interior region in which internal electrode layers and inner dielectric layers are alternately laminated in a lamination direction, and an exterior region including an outer dielectric layer provided at an end of the interior region in the lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, and an upper electrode portion formed contiguous to the end electrode portion on a part of an upper surface of the element body, the entire lower surface of the element body located on the opposite side of the upper surface in the stacking direction is exposed to the outside, the upper or lower surface of the element body includes a reinforcing layer defining the upper or lower surface of the element body; The reinforcing layer is made of SiO 2 and BaO and Al 2 O 3 The glass component contains 70 to 100 mass % in total, The reinforcing layer is located on the outer surface side of the exterior region, an interface between the outer dielectric layer of the armor region and the reinforcing layer; the outer dielectric layer is mainly composed of a dielectric material having a perovskite structure containing Ti, and a Ba-Ti-Si-O phase is formed at the interface; The thickness of the multilayer ceramic electronic component is less than 100 μm, A laminated ceramic electronic component, wherein the length in the longitudinal direction of the laminated ceramic electronic component is at least three times the thickness.

3. 3. The multilayer ceramic electronic component according to claim 1, wherein the lower surface of the element body is flat.

4. 4. The multilayer ceramic electronic component according to claim 1, wherein the reinforcing layer has a side covering portion which covers a side surface of the element body.

5. An element body having an interior region in which internal electrode layers and inner dielectric layers are alternately laminated in a lamination direction, and an exterior region including an outer dielectric layer provided at an end of the interior region in the lamination direction; a terminal electrode formed in close contact with an outer surface of the element body and connected to the internal electrode layer, the terminal electrode has an end electrode portion covering an extraction end of the element body from which the internal electrode layer is extracted, the terminal electrodes are substantially not formed on an upper surface of the element body and a lower surface of the element body located on the opposite side of the upper surface in the stacking direction, the upper or lower surface of the element body includes a reinforcing layer defining the upper or lower surface of the element body; The reinforcing layer is made of SiO 2 and BaO and Al 2 O 3 The glass component contains 70 to 100 mass % in total, The reinforcing layer is located on the outer surface side of the exterior region, an interface between the outer dielectric layer of the armor region and the reinforcing layer; the outer dielectric layer is mainly composed of a dielectric material having a perovskite structure containing Ti, and a Ba-Ti-Si-O phase is formed at the interface; The thickness of the multilayer ceramic electronic component is less than 100 μm, A laminated ceramic electronic component, wherein the length in the longitudinal direction of the laminated ceramic electronic component is at least three times the thickness.

Citation Information

Patent Citations

  • Electronic component, and electronic component built-in substrate

    JP2010129737A

  • Electronic component built-in wiring board, chip capacitor, and manufacturing method of electronic component built-in wiring board

    JP2013183028A

  • Multilayer ceramic electronic component

    JP2016111316A

  • Multilayer ceramic capacitor

    JP2017028254A

  • Laminate electronic component

    JP2017059631A