Adhesive composition for clothing and its uses
A solvent-based adhesive composition with a specific (meth)acrylic polymer addresses the issues of flexibility and adhesive strength in seamless clothing, providing flexible and durable bonds that withstand washing without heat application.
Patent Information
- Application Number
- JP2019200903
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-05
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-11-05
AI Technical Summary
Conventional hot-melt adhesives used in seamless clothing manufacturing result in hard bonded areas due to resin penetration and loss of flexibility at room temperature, leading to reduced texture and comfort, and insufficient adhesive strength during washing, which affects workability and durability.
A solvent-based or solid adhesive composition for bonding textile fabrics using a (meth)acrylic polymer with a molecular weight of 30,000 or more and a storage modulus of 1.0 MPa or less at 23°C, allowing temporary bonding without heat and ensuring high peel strength for washing resistance.
The adhesive composition provides flexibility and texture at bonded areas, improves workability by allowing room-temperature bonding, and maintains high peel strength even after washing, preventing peeling and ensuring durability.
Smart Images

Figure 0007552012000003 
Figure 0007552012000002 
Figure 0007552012000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive composition for clothing and uses thereof, and more particularly to a solvent-based or solid pressure-sensitive adhesive composition used for bonding fiber fabrics for clothing and uses thereof. [Background technology]
[0002] In order to improve the comfort and texture of clothing, clothing is being manufactured using a bonding method in which fiber fabrics are bonded together with adhesive rather than sewn with a sewing machine or the like, that is, a so-called seamless method. The adhesives used in this case are mainly urethane-based hot melt adhesives. Various methods for bonding fabrics using hot melt adhesives have also been proposed (for example, see Patent Document 1 and Patent Document 2).
[0003] Patent Document 3 proposes a pressure-sensitive adhesive composition that contains an acrylic pressure-sensitive adhesive polymer and a vinyl polymer having a glass transition temperature of 30° C. or more and 200° C. or less and a number average molecular weight of 500 or more and 10,000 or less, and that has a glass transition temperature of the entire pressure-sensitive adhesive composition of -80° C. or more and 10° C. or less. Patent Document 3 discloses that by using the pressure-sensitive adhesive composition, fabrics can be bonded together with high strength, and the bonded portions of the fabrics become soft and have an excellent texture. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-78232 A [Patent Document 2] JP 2016-74996 A [Patent Document 3] JP 2019-11382 A Summary of the Invention [Problem to be solved by the invention]
[0005] When seamless clothing is manufactured using conventional hot melt adhesives, the resin melts when heated and penetrates the mesh of the fabric, and at room temperature the resin loses its flexibility and becomes solid, resulting in some adhesive areas becoming hard, resulting in poor texture and comfort.
[0006] In the manufacturing process of clothing, when bonding two fiber fabrics together with an adhesive tape or sheet, a temporary fixing is sometimes performed by temporarily adhering the adhesive tape or sheet to the adherend. However, although the adhesive composition of Patent Document 3 improves the texture and flexibility of the bonded portion, the adhesive strength at room temperature is not sufficiently high, and it is necessary to heat the adhesive layer when temporarily fixing one fiber fabric to another fiber fabric. For this reason, there is a concern that the workability will decrease during the manufacturing of clothing.
[0007] Furthermore, when a pressure-sensitive adhesive is applied to clothing, if the adhesive strength between fiber fabrics is insufficient, the strength of the adhesive portion may be weakened due to tensile stress during washing and spin-drying, and the fabrics may peel off at the bonded portions. For this reason, pressure-sensitive adhesive compositions for clothing are required to have high peel strength (high washability) at the bonded portions of the fabrics even after the clothes are subjected to stress by washing.
[0008] The present invention has been made in consideration of the above problems, and has as its main object to provide a pressure-sensitive adhesive composition for obtaining a pressure-sensitive adhesive that has good flexibility and texture at the bonded portion, can be temporarily bonded to a fiber fabric without the application of heat, and has excellent washability. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by a technique for bonding fiber fabrics together using a specific pressure-sensitive adhesive composition. The present invention has been completed based on this knowledge. The present invention provides the following means.
[0010] [1] A pressure-sensitive adhesive composition for bonding fiber fabrics for clothing, the pressure-sensitive adhesive composition comprising a polymer component in the form of a solution dissolved in an organic solvent or in the form of a solid or semi-solid, the pressure-sensitive adhesive composition for clothing comprising a (meth)acrylic polymer (A) having a number-average molecular weight of 30,000 or more, a pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition having a storage modulus at 23°C of 1.0 MPa or less, and a content of a vinyl polymer (B) having a number-average molecular weight of 10,000 or less of 5 parts by mass or less per 100 parts by mass of the (meth)acrylic polymer (A).
[0011] [2] The pressure-sensitive adhesive composition for clothing according to [1], wherein the (meth)acrylic polymer has a structural unit derived from at least one selected from the group consisting of an alkyl (meth)acrylate compound and an alkoxyalkyl (meth)acrylate compound. [3] The pressure-sensitive adhesive composition for clothing according to [1] or [2], wherein the (meth)acrylic polymer has structural units derived from an alkyl (meth)acrylate compound in an amount of 50 mol % or more based on all constituent monomer units contained in the (meth)acrylic polymer. [4] The pressure-sensitive adhesive composition for clothing according to any one of [1] to [3], wherein the (meth)acrylic polymer has a structural unit derived from a hydroxyalkyl (meth)acrylate compound.
[0012] [5] A pressure-sensitive adhesive composition for bonding fiber fabrics for clothing, the pressure-sensitive adhesive composition comprising at least one polymer selected from the group consisting of polyester polymers, polyurethane polymers, styrene polymers, olefin polymers, silicone polymers, polyamide polymers, and polyvinyl ether polymers, the polymer having a number average molecular weight of 30,000 or more, the pressure-sensitive adhesive composition having a storage modulus at 23°C of 1.0 MPa or less, the pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition.
[0013] [6] A pressure-sensitive adhesive product comprising a support and a pressure-sensitive adhesive layer formed on the support using the pressure-sensitive adhesive composition for clothing according to any one of [1] to [5]. [7] A textile product for clothing, in which textile fabrics are bonded together using the pressure-sensitive adhesive composition for clothing according to any one of [1] to [5] above. Effect of the Invention
[0014] According to the adhesive composition for clothing of the present invention, when fiber fabrics are bonded together, an adhesive having good flexibility and texture at the bonded portion can be obtained. In addition, the adhesive layer formed by the adhesive composition for clothing of the present invention can be temporarily bonded to the fiber fabric without applying heat. Therefore, when manufacturing a fiber product for clothing, one fiber fabric can be temporarily fixed to another fiber fabric via the adhesive layer, and the workability during product manufacturing can be improved. Furthermore, the adhesive layer formed by the adhesive composition for clothing of the present invention has high peel strength, and when a fiber product for clothing in which fiber fabrics are bonded together via the adhesive layer is washed, the fiber fabric is not easily peeled off at the bonded portion, and has excellent washing resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present disclosure will be described in detail below. In this specification, "(meth)acrylic" means acrylic and / or methacrylic, "(meth)acrylate" means acrylate and / or methacrylate, and "(meth)acryloyl group" means acryloyl group and / or methacryloyl group.
[0016] <<Adhesive composition for clothing>> The adhesive composition of the present invention is an adhesive composition for clothing (hereinafter also simply referred to as "adhesive composition") for bonding fiber fabrics for clothing, and is a solution type adhesive composition in which a polymer component is dissolved in an organic solvent, or a solid or semi-solid adhesive composition at room temperature. The adhesive composition contains at least one polymer selected from the group consisting of vinyl polymers, polyester polymers, polyurethane polymers, silicone polymers, and polyamide polymers, and has a number average molecular weight of 30,000 or more (hereinafter also referred to as "polymer (A)"). The polymer (A) to be blended in the adhesive composition and the components to be blended as necessary will be described in detail below.
[0017] <Polymer (A)> A vinyl polymer (hereinafter also referred to as "vinyl polymer (A)") is a polymer obtained by using a monomer having a carbon-carbon double bond as a polymerizable group. As a monomer constituting the vinyl polymer (A), various vinyl unsaturated compounds having radical polymerizability can be used. Examples of the vinyl unsaturated compound include a chain ester compound of (meth)acrylic acid, an aliphatic cyclic ester compound of (meth)acrylic acid, an aromatic ester compound of (meth)acrylic acid, an aliphatic vinyl compound, an aliphatic cyclic vinyl compound, an aromatic vinyl compound, an unsaturated carboxylic acid, an unsaturated acid anhydride, a hydroxyl group-containing vinyl compound, an amino group-containing vinyl compound, an amide group-containing vinyl compound, a cyano group-containing unsaturated compound, a nitrile group-containing unsaturated compound, an imide group-containing vinyl compound, and a dialkyl ester compound of an unsaturated dicarboxylic acid. In producing the vinyl polymer (A), only one type of monomer may be used, or two or more types may be used.
[0018] From the viewpoint of adhesive performance, the vinyl polymer (A) is preferably at least one selected from the group consisting of (meth)acrylic polymers, styrene polymers, olefin polymers, and polyvinyl ether polymers. Specific examples of these include (meth)acrylic polymers such as poly(meth)acrylate and poly(meth)acrylamide; styrene polymers such as styrene-isoprene copolymer (SIS), styrene-ethylene-butylene copolymer (SEBS), styrene-ethylene-propylene copolymer (SEPS), and styrene-butadiene-styrene copolymer (SBS); olefin polymers such as ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene, which have an olefin unit having 2 to 8 carbon atoms (e.g., high-density polyethylene, low-density polyethylene, polypropylene, and the like); and polyvinyl ether polymers such as polyvinyl methyl ether, polyvinyl ethyl ether, and polyvinyl isobutyl ether.
[0019] The polyester polymer is a polymer obtained by copolymerizing a monomer containing a polyvalent carboxylic acid and a polyol. Examples of the polyvalent carboxylic acid include aliphatic dicarboxylic acids, aliphatic cyclic dicarboxylic acids, aromatic dicarboxylic acids, and trivalent or higher carboxylic acids. Specific examples of these include aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, fumaric acid, itaconic acid, and derivatives thereof; aliphatic cyclic dicarboxylic acids such as cyclopentane dicarboxylic acid, cyclohexane dicarboxylic acid, norbornane dicarboxylic acid, maleic acid, and derivatives thereof; aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, naphthalenedicarboxylic acid, and derivatives thereof; and trivalent or higher carboxylic acids such as trimellitic acid, pyromellitic acid, and derivatives thereof.
[0020] Examples of the polyol include aliphatic diols, aliphatic cyclic diols, aromatic diols, and trihydric or higher alcohols. Specific examples of these include aliphatic diols such as ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, propylene glycol, 2-methyl-1,3-propanediol, and 2-ethyl-2-isobutyl-1,3-propanediol; aliphatic cyclic diols such as 1,4-cyclohexanedimethanol and 2,2,4,4-tetramethyl-1,3-cyclobutanediol; aromatic diols such as bisphenol A, bisphenol S, p-dihydroxybenzene, p-xylenediol, and 4,4'-dihydroxybiphenyl; and trihydric or higher alcohols such as pentaerythritol, dipentaerythritol, and trimethylpropane.
[0021] A polyurethane polymer is a polymer obtained by reacting a polyol with a polyisocyanate. The explanation for the polyester polymer is applied to the polyol, which is a constituent monomer of polyurethane. Examples of the polyisocyanate include aliphatic diisocyanates, aliphatic cyclic diisocyanates, and aromatic diisocyanates. Specific examples of these include aliphatic diisocyanates such as propane-1,3-diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, and 2,2,4-trimethylhexamethylene diisocyanate; aliphatic cyclic diisocyanates such as cyclohexane-1,4-diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate; and aromatic diisocyanates such as 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 4,4'-biphenylene isocyanate, 4,4'-diphenyl ether diisocyanate, 1,5-naphthalene diisocyanate, 2,6-tolylene diisocyanate, and xylylene diisocyanate.
[0022] The silicone polymer is, for example, a hydrolysis condensation product of an organosilicon compound such as an alkoxysilane compound. Specific examples of the silicone polymer include addition reaction curing type polysiloxane and peroxide curing type polysiloxane. The polyamide polymer is a polymer obtained by reacting a polyvalent carboxylic acid with a diamine. The polyvalent carboxylic acid constituting the polyamide polymer is not particularly limited, and examples thereof include aliphatic dicarboxylic acids, aliphatic cyclic dicarboxylic acids, and aromatic dicarboxylic acids. The diamine is also not particularly limited, and known diamines such as aliphatic diamines, aliphatic cyclic diamines, and aromatic diamines can be used appropriately.
[0023] The polymer (A) is preferably at least one selected from the group consisting of vinyl polymers (A), polyester polymers, and polyurethane polymers, because it has high peel strength and excellent washability, and more preferably at least one selected from the group consisting of (meth)acrylic polymers, styrene polymers, polyester polymers, and polyurethane polymers. Among these, at least one selected from the group consisting of (meth)acrylic polymers and styrene polymers is more preferable, and (meth)acrylic polymers (hereinafter also referred to as "(meth)acrylic polymers (A)") are particularly preferable because they are excellent in transparency, weather resistance, and adhesion, and have a high degree of freedom in design.
[0024] (Meth)acrylic polymer (A) The (meth)acrylic polymer (A) is a polymer mainly composed of structural units derived from (meth)acrylic monomers, and has adhesive properties. In this specification, the fact that the (meth)acrylic polymer (A) is "mainly composed" of structural units derived from (meth)acrylic monomers means that the ratio of structural units derived from (meth)acrylic monomers to the total constituent monomer units of the (meth)acrylic polymer (A) is more than 50 mol%, preferably 65 mol% or more, more preferably 75 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more.
[0025] As the (meth)acrylic monomer, at least one monomer selected from the group consisting of alkyl (meth)acrylate compounds and alkoxyalkyl (meth)acrylate compounds (hereinafter also referred to as "monomer MA") can be preferably used, since it is possible to obtain a polymer having a relatively low glass transition point and good adhesion.
[0026] The alkyl (meth)acrylate compound is a chain alkyl ester of (meth)acrylic acid, and specific examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate.
[0027] Examples of the alkoxyalkyl (meth)acrylate compound include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-propoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, n-propoxypropyl (meth)acrylate, n-butoxypropyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, n-propoxybutyl (meth)acrylate, and n-butoxybutyl (meth)acrylate.
[0028] As the monomer MA, from among the above, at least one selected from the group consisting of alkyl (meth)acrylate compounds having an alkyl group with 4 to 12 carbon atoms and alkoxyalkyl (meth)acrylate compounds having an alkoxyalkyl group with 2 to 12 carbon atoms is preferred, and at least one selected from the group consisting of alkyl (meth)acrylate compounds having an alkyl group with 4 to 8 carbon atoms and alkoxyalkyl (meth)acrylate compounds having an alkoxyalkyl group with 2 to 3 carbon atoms is more preferred, in that it can impart superior adhesion and flexibility to the (meth)acrylic polymer (A).
[0029] In the (meth)acrylic polymer (A), the content of the structural unit derived from the monomer MA (hereinafter also referred to as the "structural unit UA") is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more, based on the total constituent monomer units of the (meth)acrylic polymer (A), from the viewpoint of sufficiently increasing the adhesive properties. The upper limit of the content of the structural unit UA can be appropriately set within a range of 100 mol% or less based on the total constituent monomer units of the (meth)acrylic polymer (A). When a monomer unit different from the structural unit UA is introduced into the (meth)acrylic polymer (A), the content of the structural unit UA in the (meth)acrylic polymer (A) is preferably 99 mol% or less.
[0030] The content of the structural unit derived from the (meth)acrylic acid alkyl compound is preferably 10 mol% or more, more preferably 30 mol% or more, even more preferably 50 mol% or more, even more preferably 70 mol% or more, and particularly preferably 90 mol% or more, based on the total constituent monomer units of the (meth)acrylic polymer (A), in that the fabrics can be temporarily bonded to each other at room temperature without heat compression bonding. The content of the structural unit derived from the (meth)acrylic acid alkyl compound is preferably 99 mol% or less, more preferably 95 mol% or less, based on the total constituent monomer units of the (meth)acrylic polymer (A).
[0031] The content of structural units derived from an alkoxyalkyl (meth)acrylate compound is preferably 95 mol % or less, more preferably 90 mol % or less, even more preferably 80 mol % or less, even more preferably 60 mol % or less, and particularly preferably 45 mol % or less, based on the total constituent monomer units of the (meth)acrylic polymer (A), in that the introduction of a sufficient amount of an alkoxyalkyl (meth)acrylate compound makes it possible to temporarily bond fabrics to each other at room temperature.
[0032] Among the above, the (meth)acrylic polymer (A) is particularly preferably one having a structural unit derived from an alkyl acrylate compound having 4 to 12 carbon atoms, in that it can lower the storage modulus at room temperature and can provide a pressure-sensitive adhesive that can be temporarily bonded to a fiber fabric without relying on thermocompression bonding. The content of the structural unit derived from an alkyl acrylate compound having 4 to 12 carbon atoms is preferably 10 mol % or more, more preferably 30 mol % or more, even more preferably 50 mol % or more, and particularly preferably 70 mol % or more, based on the total constituent monomer units of the (meth)acrylic polymer (A).
[0033] The (meth)acrylic polymer (A) may be produced using only the monomer MA as the (meth)acrylic monomer, or may be produced by further using a (meth)acrylic monomer different from the monomer MA and a compound copolymerizable with the monomer MA (hereinafter also referred to as "monomer MB").
[0034] In producing the (meth)acrylic polymer (A), a (meth)acrylic monomer having a crosslinkable functional group is used as the monomer MB, thereby making it possible to obtain the (meth)acrylic polymer (A) having a structure having a crosslinkable structural unit. The (meth)acrylic polymer (A) having a crosslinkable structural unit is preferable in that the heat resistance and durability of the pressure-sensitive adhesive layer obtained by using the pressure-sensitive adhesive composition can be further improved.
[0035] The (meth)acrylic monomer having a crosslinkable functional group is not particularly limited, but is preferably at least one monomer selected from the group consisting of (meth)acrylic acid, (meth)acrylic acid hydroxyalkyl compounds, epoxy group-containing (meth)acrylic acid ester compounds, and silyl group-containing (meth)acrylic acid ester compounds. Among these, (meth)acrylic acid hydroxyalkyl compounds are particularly preferred, since the adhesive strength of the (meth)acrylic polymer (A) tends to be high. As the (meth)acrylic acid hydroxyalkyl compound, from the viewpoint of adhesive performance, a compound having a hydroxyalkyl group with 2 to 8 carbon atoms is preferred, and a compound having a hydroxyalkyl group with 2 or 3 carbon atoms is particularly preferred.
[0036] When the (meth)acrylic polymer (A) has a structural unit derived from a (meth)acrylic monomer having a crosslinkable functional group (hereinafter also referred to as a "crosslinkable structural unit"), the content of the crosslinkable structural unit is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and even more preferably 1 mol% or more, based on the total constituent monomer units of the (meth)acrylic polymer (A). The upper limit of the content of the crosslinkable structural unit is not particularly limited, but from the viewpoint of sufficiently ensuring the flexibility of the obtained pressure-sensitive adhesive layer, it is preferably 20 mol% or less, more preferably 15 mol% or less, and even more preferably 10 mol% or less, based on the total constituent monomer units of the (meth)acrylic polymer (A).
[0037] When the (meth)acrylic polymer (A) has a structural unit derived from a (meth)acrylic hydroxyalkyl compound (hereinafter also referred to as the "structural unit UB"), the content of the structural unit UB is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and even more preferably 1 mol% or more, based on the total constituent monomer units of the (meth)acrylic polymer (A), from the viewpoint of forming a good crosslinked structure. In addition, from the viewpoint of ensuring sufficient flexibility of the pressure-sensitive adhesive layer, the content of the structural unit UB is preferably 20 mol% or less, more preferably 15 mol% or less, even more preferably 10 mol% or less, and particularly preferably 7 mol% or less, based on the total constituent monomer units of the (meth)acrylic polymer (A).
[0038] Examples of the monomer MB include, in addition to the above, an aliphatic cyclic ester compound of (meth)acrylic acid, an alkenyl ester compound of (meth)acrylic acid, an aromatic ester compound of (meth)acrylic acid, a (meth)acrylamide compound, a polyfunctional (meth)acrylate compound, etc. When producing the (meth)acrylic polymer (A), one or more kinds of monomer MB can be used.
[0039] The (meth)acrylic polymer (A) may further have a monomer (other monomer) other than the (meth)acrylic monomer. Examples of the other monomer include an aliphatic vinyl compound, an aromatic vinyl compound, a polyfunctional alkenyl compound, a nitrile group-containing unsaturated compound, and a dialkyl ester compound of an unsaturated dicarboxylic acid. The content of the structural unit derived from the other monomer is preferably 0 mol% or more and less than 50 mol%, more preferably 0 mol% or more and 30 mol% or less, and even more preferably 0 mol% or more and 10 mol% or less, based on the total constituent monomer units of the (meth)acrylic polymer (A). One or more kinds of the other monomers can be used.
[0040] The glass transition point of the (meth)acrylic polymer (A) is not particularly limited as long as the (meth)acrylic polymer (A) exhibits adhesiveness. In order that the (meth)acrylic polymer (A) exhibits excellent adhesiveness and is easy to form an adhesive layer that can be temporarily pressed onto a fiber fabric, it is preferable that the glass transition point (hereinafter also referred to as "glass transition point Tg1") of the polymer chain mainly composed of structural units derived from a (meth)acrylic monomer is in the range of -80°C or more and 10°C or less. When the glass transition point Tg1 is -80°C or more, the cohesive force of the obtained adhesive layer tends to be sufficiently high and the shear adhesion can be sufficiently ensured. In addition, when the glass transition point Tg1 is 10°C or less, the flexibility of the adhesive layer can be increased, and the flexibility of the joint portion can be sufficiently ensured when the fiber fabrics are joined together. From the viewpoint of improving the adhesiveness and flexibility of the (meth)acrylic polymer (A), the glass transition temperature Tg1 is preferably 0° C. or lower, more preferably −5° C. or lower, even more preferably −10° C. or lower, still more preferably −15° C. or lower, and particularly preferably −25° C. or lower. The glass transition temperature Tg1 is preferably −70° C. or higher, more preferably −60° C. or higher.
[0041] In this specification, the glass transition temperature of the polymer is a value measured by differential scanning calorimetry (DSC). Details of the measurement method can be in accordance with the procedures described in the Examples below. The glass transition temperature of the polymer can be arbitrarily selected by changing the type and composition of the constituent monomers.
[0042] The (meth)acrylic polymer (A) is not particularly limited as long as a part or the whole of the main chain is constituted by a polymer chain mainly composed of a structural unit derived from a (meth)acrylic monomer. Specific examples of the (meth)acrylic polymer (A) include [1] a polymer whose main chain is constituted only by a polymer chain mainly composed of a structural unit derived from a (meth)acrylic monomer (hereinafter also referred to as "polymer (A1)"), and [2] a block copolymer having a polymer block A as a hard segment and a polymer block B as a soft segment, and the polymer block B is composed of a polymer chain mainly composed of a structural unit derived from a (meth)acrylic monomer (hereinafter also referred to as "block copolymer (A2)").
[0043] [1] Polymer (A1) The polymer (A1) can be obtained by polymerizing the above-mentioned monomers by adopting a known radical polymerization method such as a solution polymerization method. In the case of the solution polymerization method, an organic solvent and a monomer are charged into a reactor, a polymerization initiator is added, and the mixture is heated to 50 to 300°C to copolymerize, thereby obtaining the target polymer (A1). The method of charging each raw material including the monomer may be a batch-type initial lump-sum charging in which all raw materials are charged at once, a semi-continuous charging in which at least a part of the raw materials are continuously fed into the reactor, or a continuous polymerization method in which all raw materials are continuously fed and the resulting resin is continuously extracted from the reactor at the same time. In addition, when preparing the pressure-sensitive adhesive composition, the polymer (A1) may be used as a polymer solution dissolved in an organic solvent, or may be used after distilling off the organic solvent by heating and reducing pressure treatment or the like.
[0044] As the organic solvent used in the solution polymerization method, an organic hydrocarbon compound is suitable. Examples of the organic hydrocarbon compound include cyclic ethers such as tetrahydrofuran and dioxane, aromatic hydrocarbon compounds such as benzene, toluene and xylene, esters such as ethyl acetate and butyl acetate, ketones such as acetone, methyl ethyl ketone and cyclohexanone, and alcohols such as methyl orthoformate, methyl orthoacetate, methanol, ethanol and isopropanol. As the organic solvent, one or more of these can be used. The amount of the organic solvent used is, for example, 1 to 50 mass% of the total amount of the monomers used in the polymerization relative to the total amount of the organic solvent and the monomers.
[0045] The polymerization initiator may be a known radical polymerization initiator such as an azo compound, an organic peroxide, or an inorganic peroxide, and is not particularly limited. In addition, the polymerization initiator may be a redox type polymerization initiator consisting of a known oxidizing agent and a known reducing agent. Furthermore, a known chain transfer agent may be used in combination with the polymerization initiator.
[0046] Specific examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2-(tert-butylazo)-2-cyanopropane, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), and dimethyl 2,2'-azobis(2-methylpropionate); Examples of organic peroxides include cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide, and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; Inorganic peroxides, such as potassium persulfate, sodium persulfate, etc.; Examples of the redox type polymerization initiator include those using sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, ferrous sulfate, etc. as a reducing agent, and potassium peroxodisulfate, hydrogen peroxide, tert-butyl hydroperoxide, etc. as an oxidizing agent. In producing the polymer (A1), the amount of the polymerization initiator used is, for example, 0.01 to 20 parts by mass relative to 100 parts by mass of the total monomers used in the polymerization.
[0047] [2] Block copolymer (A2) The polymer block A in the block copolymer (A2) is preferably a segment having a higher glass transition point than the polymer block B, specifically, a segment having a glass transition point of 50° C. or higher. The polymer block A having a glass transition point of 50° C. or higher is preferable in that good heat resistance can be imparted to the block copolymer (A2). It is also preferable that the block copolymer (A2) can form pseudo-crosslinks by forming a microphase separation structure, etc. When the polymer constituting the pressure-sensitive adhesive layer forms a pseudo-crosslinked structure, the cohesive force tends to be improved, and the adhesive strength tends to be increased.
[0048] The glass transition point of the polymer block A is more preferably 60° C. or higher, even more preferably 80° C. or higher, and particularly preferably 90° C. or higher, in order to impart good heat resistance to the block copolymer (A2). The glass transition point of the polymer block A is preferably 350° C. or lower, more preferably 280° C. or lower, and even more preferably 260° C. or lower, in order to reduce the heating temperature during thermocompression bonding. In this specification, the glass transition points of the polymer block A and the polymer block B are values determined by producing homopolymers of each polymer block and subjecting them to DSC measurement. Details of the measurement method can be determined according to the procedures described in the Examples below.
[0049] The polymer block A preferably has a structural unit (hereinafter also referred to as "structural unit U1") derived from at least one compound selected from the group consisting of imide group-containing vinyl compounds, styrene-based compounds, alkyl (meth)acrylate compounds, and amide group-containing vinyl compounds. The polymer block A having the structural unit U1 is suitable in that a block copolymer having better heat resistance and adhesiveness can be obtained. Among these, it is particularly preferable that the polymer block A has at least a structural unit derived from at least one compound selected from the group consisting of imide group-containing vinyl compounds and styrene-based compounds.
[0050] Examples of the imide group-containing vinyl compound include maleimide compounds such as maleimide and N-substituted maleimide compounds; itaconimide compounds such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide; N-methylcitraconimide, N-ethylcitraconimide, N-butylcitraconimide, N-octylcitraconimide, N-2-ethylhexylcitraconimide, and N-cyclohexylitaconimide; Examples of the vinyl compound containing an imide group include citraconimide compounds such as cyclohexylcitraconimide and N-laurylcitraconimide; and (meth)acrylimide compounds such as N-(2-(meth)acryloyloxyethyl)succinimide, N-(2-(meth)acryloyloxyethyl)maleimide, N-(2-(meth)acryloyloxyethyl)phthalimide, N-(4-(meth)acryloyloxybutyl)succinimide, N-(4-(meth)acryloyloxybutyl)maleimide, and N-(4-(meth)acryloyloxybutyl)phthalimide. As the vinyl compound containing an imide group, a maleimide compound can be preferably used.
[0051] The maleimide compounds include maleimide and N-substituted maleimide compounds. Examples of the N-substituted maleimide compounds include N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, N-isopropylmaleimide, Nn-butylmaleimide, N-isobutylmaleimide, N-tert-butylmaleimide, N-pentylmaleimide, N-hexylmaleimide, N-heptylmaleimide, N-octylmaleimide, N-laurylmaleimide, and N-stearylmaleimide; N-cyclopentylmaleimide, N-cyclohexylmaleimide, and N-cyclohexylmaleimide; Examples of the maleimide compound include N-cycloalkyl-substituted maleimide compounds such as hexylmaleimide; N-aralkyl-substituted maleimide compounds such as N-benzylmaleimide; and N-aryl-substituted maleimide compounds such as N-phenylmaleimide, N-(4-hydroxyphenyl)maleimide, N-(4-acetylphenyl)maleimide, N-(4-methoxyphenyl)maleimide, N-(4-ethoxyphenyl)maleimide, N-(4-chlorophenyl)maleimide, and N-(4-bromophenyl)maleimide. Of the above, the maleimide compound used for producing the polymer block A is preferably a compound represented by the following formula (1), since it can provide the block copolymer (A2) with better heat resistance and adhesiveness. [ka] (In formula (1), R 1 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, a cyclohexyl group, a phenyl group, or a substituted phenyl group having a hydroxyl group, an alkoxy group having 1 to 2 carbon atoms, an acetyl group, or a halogen atom bonded to any position of the phenyl group.
[0052] In the production of the polymer block A, the amount of the imide group-containing vinyl compound used can be appropriately set within a range of 100 mol% or less based on all the constituent monomer units of the polymer block A. The content of the imide group-containing vinyl compound based on all the constituent monomer units of the polymer block A is preferably 5 to 90 mol%, more preferably 10 to 70 mol%, and even more preferably 20 to 65 mol%. A block copolymer containing a structural unit derived from an imide group-containing vinyl compound is preferable because it has excellent heat resistance and adhesiveness. If the content of the imide group-containing vinyl compound is 70 mol% or less based on all the constituent monomer units of the polymer block A, the adhesiveness of the block copolymer (A2) can be sufficiently ensured, which is preferable.
[0053] Examples of styrene-based compounds include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, pn-butylstyrene, p-isobutylstyrene, pt-butylstyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, p-chloromethylstyrene, p-chlorostyrene, and divinylbenzene.
[0054] When a styrene-based compound is used in the production of polymer block A, the amount of the styrene-based compound used is not particularly limited. The content of the structural unit derived from the styrene-based compound relative to all the constituent monomer units of polymer block A is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more. In polymer block A, the upper limit of the content of the structural unit derived from the styrene-based compound is not particularly limited and can be appropriately set to 100 mol% or less. The upper limit of the content of the structural unit derived from the styrene-based compound relative to all the constituent monomer units of polymer block A is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less.
[0055] The styrene-based compound may have a property of improving the polymerizability of the imide group-containing vinyl compound. Therefore, when an imide group-containing vinyl compound (preferably a maleimide compound) is used as a constituent monomer unit of the polymer block A, it is preferable to improve the polymerizability of the imide group-containing vinyl compound by using a styrene-based compound in combination. When an imide group-containing vinyl compound and a styrene-based compound are used in combination in the production of the polymer block A, the content of the structural unit derived from the styrene-based compound in the polymer block A relative to 1 mole of the structural unit derived from the imide group-containing vinyl compound is preferably 0.01 to 100 moles, more preferably 0.1 to 10 moles, still more preferably 0.2 to 5 moles, and particularly preferably 0.5 to 1.5 moles.
[0056] The proportion of the structural unit U1 in the polymer block A is preferably 30 mol % or more, more preferably 50 mol % or more, further preferably 80 mol % or more, and particularly preferably 90 mol % or more, based on the total constituent monomer units contained in the polymer block A. The structural unit U1 contained in the polymer block A may be of one type or two or more types.
[0057] The polymer block A may have a structural unit derived from a monomer other than the above-mentioned monomer that is copolymerizable with the monomer constituting the structural unit U1, within a range that does not impair the function of the block copolymer (A2). Examples of such monomers include alkoxyalkyl (meth)acrylate compounds, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate. These compounds may be used alone or in combination of two or more.
[0058] The number average molecular weight of the polymer block A is preferably in the range of 500 to 30,000. When the number average molecular weight is 500 or more, the cohesive force of the block copolymer can be sufficiently ensured, and when it is 30,000 or less, it is preferable in that the peel strength to the adherend can be sufficiently increased. The number average molecular weight of the polymer block A is more preferably in the range of 1,000 to 25,000, and further preferably in the range of 2,000 to 20,000. The molecular weight of the polymer block A is a polystyrene-equivalent value measured by gel permeation chromatography (GPC). When a plurality of polymer blocks A are present in one molecule of the block copolymer (A2), the "number average molecular weight of the polymer block A" means the total number average molecular weight of the plurality of polymer blocks A contained in one molecule of the copolymer.
[0059] The polymer block A may have a property of phase separation from the polymer block B. Such a property is advantageous in that the block copolymer (A2) is likely to form a microphase-separated structure. Based on the common technical knowledge at the time of filing the present application, a person skilled in the art can easily design a polymer block A that phase separates from the polymer block B. For example, the difference ΔSP (absolute value) between the SP value of the polymer block A calculated by a known method for calculating the SP value, which is a solubility parameter (e.g., the Fedors method), and the SP value of the polymer block B is set to 0.01 or more. The difference ΔSP may be, for example, 0.1 or more, for example, 0.2 or more, or for example, 0.5 or more. In the case of the Fedors method, the SP value can be calculated by the calculation method described in "Polymer Engineering and Science" 14(2), 147 (1974) written by RF Fedors.
[0060] Specific examples of the structure of the block copolymer (A2) include an (AB) diblock copolymer consisting of polymer block A and polymer block B, an (ABA) triblock copolymer consisting of polymer block A / polymer block B / polymer block A, and a (BAB) triblock copolymer consisting of polymer block B / polymer block A / polymer block B. The block copolymer (A2) may further have a polymer block other than the polymer block A and the polymer block B. Of these, the block copolymer (A2) preferably has an ABA structure. With such a structure, the polymer block A and the polymer block B are likely to form a pseudo-crosslinked structure, improving the adhesive properties.
[0061] The molar ratio of polymer block A to polymer block B in block copolymer (A2) is preferably 1 / 99 to 25 / 75 (polymer block A / polymer block B). When the molar ratio is within the above range, a pressure-sensitive adhesive exhibiting excellent adhesiveness can be easily obtained from a polymer having polymer block A capable of forming a phase separation structure and serving as a pseudo-crosslinking point, and polymer block B serving as a soft segment, and flexibility of the joint between fabrics can be sufficiently maintained, which is preferable. The molar ratio of polymer block A to polymer block B is more preferably 1 / 99 to 20 / 80, further preferably 1 / 99 to 15 / 85, and particularly preferably 1 / 99 to 10 / 90.
[0062] <Method for producing block copolymer (A2)> The block copolymer (A2) is not particularly limited in the production method, and can be obtained by a known production method, so long as it is possible to obtain a block copolymer having a polymer block A and a polymer block B. Examples of the production method of the block copolymer (A2) include a method using various controlled polymerization methods such as living radical polymerization and living anionic polymerization, and a method of coupling polymers having functional groups together. Among these, the living radical polymerization method is preferred from the viewpoints of simple operation and applicability to a wide range of monomers.
[0063] The living radical polymerization may be any process such as a batch process, a semi-batch process, a dry continuous polymerization process, a continuous stirred tank process (CSTR), etc. The polymerization method may be applied to various modes such as bulk polymerization without using a solvent, solution polymerization in a solvent system, emulsion polymerization in an aqueous system, mini-emulsion polymerization, or suspension polymerization.
[0064] There is no particular limitation on the type of living radical polymerization method, and various polymerization methods can be used, such as reversible addition-fragmentation chain transfer polymerization (RAFT method), nitroxy radical method (NMP method), atom transfer radical polymerization (ATRP method), polymerization method using an organotellurium compound (TERP method), polymerization method using an organoantimony compound (SBRP method), polymerization method using an organobismuth compound (BIRP method), and iodine transfer polymerization method. Among these, the RAFT method, the NMP method, and the ATRP method are preferred from the viewpoints of polymerization controllability and ease of implementation.
[0065] In the RAFT method, controlled polymerization proceeds through a reversible chain transfer reaction in the presence of a polymerization control agent (RAFT agent) and a general free radical polymerization initiator. As the RAFT agent, various known RAFT agents such as dithioester compounds, xanthate compounds, trithiocarbonate compounds, and dithiocarbamate compounds can be used. By using a bifunctional compound as the RAFT agent, it is preferable in that the block copolymer (A2) can be obtained efficiently. The amount of the RAFT agent used is appropriately adjusted depending on the type of monomer and RAFT agent used.
[0066] As the polymerization initiator used in the polymerization by the RAFT method, known radical polymerization initiators such as azo compounds, organic peroxides and persulfates can be used. Among these, azo compounds are preferred because they are safe and easy to handle and do not easily cause side reactions during polymerization. Specific examples of azo compounds include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), and 2,2'-azobis(2-methylbutyronitrile). Only one type of radical polymerization initiator may be used, or two or more types may be used in combination. The proportion of the radical polymerization initiator used is not particularly limited, but it is preferable to use 0.01 mol or more and 0.5 mol or less of the radical polymerization initiator per mol of the RAFT agent in order to stably carry out the polymerization reaction and obtain a polymer with a smaller molecular weight distribution. The reaction temperature during polymerization is preferably 40°C or higher and 100°C or lower, more preferably 45°C or higher and 90°C or lower.
[0067] In the NMP method, a specific alkoxyamine compound having a nitroxide is used as a living radical polymerization initiator, and polymerization is allowed to proceed via a nitroxide radical derived from the living radical polymerization initiator. In the production of the block copolymer (A2), the type of nitroxide radical is not particularly limited, and a commercially available nitroxide-based polymerization initiator can be used. From the viewpoint of efficiently obtaining the block copolymer (A2), it is preferable to use a bifunctional polymerization precursor having two active sites in the molecule. The amount of the nitroxide compound used is appropriately adjusted depending on the type of monomer and nitroxide compound used. In addition, when the block copolymer (A2) is produced by the NMP method, the polymerization may be carried out by adding a nitroxide radical to 1 mole of the nitroxide compound. The reaction temperature in the NMP method is preferably 50°C or more and 140°C or less, more preferably 60°C or more and 130°C or less.
[0068] In the ATRP method, a polymerization reaction is generally carried out using an organic halide as an initiator and a transition metal complex as a catalyst. The organic halide initiator may be monofunctional or bifunctional or higher. In terms of efficiently obtaining the block copolymer (A2), it is preferable to use a bifunctional compound. As the type of halogen, bromide and chloride are preferable. The reaction temperature in the ATRP method is preferably 20°C or higher and 200°C or lower, more preferably 50°C or higher and 150°C or lower. A reaction temperature of 20°C or higher is preferable in terms of smoothly proceeding with the polymerization reaction.
[0069] In the polymerization reaction, a polymerization solvent known in living radical polymerization can be used. Specifically, aromatic compounds such as benzene, toluene, xylene, and anisole; ester compounds such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; ketone compounds such as acetone and methyl ethyl ketone; dimethylformamide, acetonitrile, dimethyl sulfoxide, alcohol, water, etc. can be mentioned. In addition, the polymerization can be carried out in a form such as bulk polymerization without using a polymerization solvent. In addition, the polymerization of the block copolymer (A2) can be carried out in the presence of a known chain transfer agent as necessary.
[0070] The number average molecular weight (Mn) of the polymer (A) is 30,000 or more, preferably 40,000 or more, and more preferably 50,000 or more, from the viewpoint of exhibiting good adhesiveness. Also, from the viewpoint of ease of production, the Mn of the polymer (A) is preferably 800,000 or less, more preferably 500,000 or less, and even more preferably 300,000 or less. The Mn range of the polymer (A) is preferably 30,000 or more and 800,000 or less, more preferably 40,000 or more and 800,000 or less, and even more preferably 50,000 or more and 500,000 or less. The molecular weight of the polymer (A) is a polystyrene equivalent value measured by GPC.
[0071] The molecular weight distribution of the polymer (A), which is expressed by the ratio of the weight average molecular weight (Mw) to Mn (Mw / Mn), can be appropriately set according to the main chain of the polymer (A). For example, the molecular weight distribution of the polymer (A1) is preferably 8.0 or less, more preferably 7.5 or less, and even more preferably 7.0 or less, from the viewpoint of easily obtaining good peel strength. The molecular weight distribution of the block copolymer (A2) is preferably 3.5 or less, more preferably 3.0 or less, and even more preferably 2.5 or less, from the viewpoint of ensuring adhesive properties (adhesiveness, cohesiveness, etc.) by forming a pseudo-crosslinked structure. The lower limit of Mw / Mn of the polymer (A) is not particularly limited, and can be 1.0 or more.
[0072] <Other ingredients> The polymer (A) can be used alone as a pressure-sensitive adhesive material, but if necessary, components other than the polymer (A) (hereinafter, also referred to as "other components") may be blended into the pressure-sensitive adhesive composition for use. The other components that may be blended into the pressure-sensitive adhesive composition are described below.
[0073] (tackifier resin) The pressure-sensitive adhesive composition may contain a tackifier resin. Examples of the tackifier resin include vinyl polymers having a number average molecular weight of 10,000 or less (hereinafter also referred to as "vinyl polymer (B)"); rosin derivatives such as rosin ester, gum rosin, tall oil rosin, hydrogenated rosin ester, maleic rosin, and disproportionated rosin ester; terpene-phenol resins, terpene-based resins mainly composed of α-pinene, β-pinene, and limonene; coumarone-indene resins; phenolic resins; and xylene-based resins.
[0074] In the present adhesive composition, the content of the tackifier resin is preferably 60 parts by mass or less relative to 100 parts by mass of the total amount of the polymer (A). By making the content of the tackifier resin 60 parts by mass or less, the flexibility and texture of the adhesion portion can be sufficiently maintained, and temporary adhesion at room temperature can be sufficiently exhibited. The upper limit of the content of the tackifier resin is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 10 parts by mass or less. When a tackifier resin is blended in the present adhesive composition, the lower limit of the content of the tackifier resin is, for example, 0.1 parts by mass or more.
[0075] When the polymer (A) contained in the pressure-sensitive adhesive composition is a (meth)acrylic polymer (A), the content of the tackifier resin is preferably 0 parts by mass or more and 5 parts by mass or less, more preferably 0 parts by mass or more and 2 parts by mass or less, even more preferably 0 parts by mass or more and 1 part by mass or less, and even more preferably 0 parts by mass or more and 0.5 parts by mass or less, relative to 100 parts by mass of the total amount of the polymer (A). When the content of the tackifier resin is within the above range, the temporary adhesion of the pressure-sensitive adhesive layer to the fiber fabric can be made more excellent. From this viewpoint, when the polymer (A) contained in the pressure-sensitive adhesive composition is a (meth)acrylic polymer (A), it is particularly preferable that the pressure-sensitive adhesive composition does not contain a tackifier resin.
[0076] When a tackifier resin is used in the case where a vinyl polymer (A) such as a (meth)acrylic polymer, a styrene polymer, an olefin polymer, or a polyvinyl ether polymer is blended as the polymer (A) in the pressure-sensitive adhesive composition, a vinyl polymer (B) is preferably used from the viewpoint of compatibility. Examples of monomers constituting the vinyl polymer (B) include vinyl unsaturated compounds used in the production of the vinyl polymer (A). In the production of the vinyl polymer (B), one type of monomer is used alone or two or more types are used in combination. There is no particular restriction on the method of producing the vinyl polymer (B), but for example, a known radical polymerization method such as a solution polymerization method can be adopted. The vinyl polymer (B) preferably has a glass transition point of 40° C. or higher, more preferably 40 to 150° C., and even more preferably 40 to 120° C., in terms of exhibiting good adhesion at room temperature.
[0077] The number average molecular weight (Mn) of the vinyl polymer (B) is preferably 500 or more and 10,000 or less. The Mn of the vinyl polymer (B) is more preferably 500 or more and 8,000 or less, even more preferably 700 or more and 6,000 or less, and particularly preferably 1,000 or more and 5,000 or less. The molecular weight distribution of the vinyl polymer (B), expressed as the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 3.0 or less, more preferably 2.5 or less. The molecular weight of the vinyl polymer (B) is a standard polystyrene-equivalent value obtained using GPC.
[0078] When the polymer (A) contained in the present adhesive composition is a (meth)acrylic polymer (A), the content of the vinyl polymer (B) in the present adhesive composition is preferably in the range of 0 to 5 parts by mass relative to 100 parts by mass of the total amount of the (meth)acrylic polymer (A). When the content of the vinyl polymer (B) is in the above range, the adhesive strength of the surface layer of the adhesive layer formed using the present adhesive composition can be sufficiently increased, and the adhesive layer can be bonded (temporarily bonded) to the fiber fabric without applying heat, which is preferable. When the polymer (A) contained in the present adhesive composition is a (meth)acrylic polymer (A), the content of the vinyl polymer (B) is more preferably 4 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less relative to 100 parts by mass of the total amount of the (meth)acrylic polymer (A), in terms of increasing the temporary adhesion, and it is particularly preferable that the composition does not contain a tackifier resin.
[0079] (Crosslinking agent) When the polymer (A) has a crosslinkable functional group, a crosslinking agent capable of reacting with the crosslinkable functional group may be blended in the pressure-sensitive adhesive composition. If necessary, a heat treatment or the like may be further performed to obtain a pressure-sensitive adhesive suitable for the intended use.
[0080] Examples of the crosslinking agent (curing agent) include a glycidyl compound having two or more glycidyl groups, an isocyanate compound having two or more isocyanate groups, an aziridine compound having two or more aziridinyl groups, an oxazoline compound having an oxazoline group, a metal chelate compound, a butylated melamine compound, etc. Among these, an isocyanate compound is preferred in terms of excellent adhesive properties under high temperature conditions.
[0081] Specific examples of the crosslinking agent include glycidyl compounds such as polyfunctional glycidyl compounds, such as ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, tetraglycidylxylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and trimethylolpropane polyglycidyl ether; As isocyanate compounds, aromatic isocyanate compounds such as diphenylmethane diisocyanate (MDI), tolylene diisocyanate, naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), xylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and tolidine diisocyanate (TODI); hexamethylene diisocyanate (HDI), lysine diisocyanate (LYS), etc. Aliphatic isocyanate compounds such as isophorone diisocyanate (IPDI), cyclohexyl diisocyanate (CHDI), hydrogenated XDI (H6XDI), hydrogenated MDI (H12MDI), etc.; modified isocyanate compounds such as urethane modified compounds, dimers, trimers, carbodiimide modified compounds, urea modified compounds, isocyanurate modified compounds, oxazolidone modified compounds, and isocyanate group-terminated prepolymers; Examples of the aziridine compound include 1,6-bis(1-aziridinylcarbonylamino)hexane, 1,1'-(methylene-di-p-phenylene)bis-3,3-aziridyl urea, ethylene bis-(2-aziridinyl propionate), 2,4,6-triaziridinyl-1,3,5-triazine, and trimethylolpropane-tris-(2-aziridinyl propionate).
[0082] When the pressure-sensitive adhesive composition contains a crosslinking agent, its content is not particularly limited, but is usually 0.01 to 10 mass %, preferably 0.03 to 5 mass %, and more preferably 0.05 to 2 mass %, relative to the content of polymer (A).
[0083] (Plasticizer) The adhesive composition may contain a plasticizer. Examples of the plasticizer include phthalates such as di-n-butyl phthalate, di-n-octyl phthalate, bis(2-ethylhexyl) phthalate, and di-n-decyl phthalate; adipates such as bis(2-ethylhexyl) adipate and di-n-octyl adipate; sebacic acid esters; azelaic acid esters; paraffins such as chlorinated paraffin; glycols such as polypropylene glycol; epoxy-modified vegetable oils such as epoxidized soybean oil and epoxidized linseed oil; phosphates such as trioctyl phosphate and triphenyl phosphate; phosphites such as triphenyl phosphite; ester oligomers such as esters of adipic acid and 1,3-butylene glycol; low molecular weight polymers such as low molecular weight polybutene, low molecular weight polyisobutylene, and low molecular weight polyisoprene; and oils such as process oil and naphthenic oil. The content of the plasticizer is preferably from 0 to 20% by mass, more preferably from 0 to 10% by mass, and further preferably from 0 to 5% by mass, based on the total amount of the polymer (A).
[0084] Other additives that can be blended into the pressure-sensitive adhesive composition include, for example, antioxidants, ultraviolet absorbers, antiaging agents, flame retardants, antifungal agents, silane coupling agents, fillers, colorants, etc. The content of the additives can be appropriately set depending on the various compounds within a range that does not impair the effects of the present invention.
[0085] The pressure-sensitive adhesive composition may be a solution-type polymer composition in which the polymer (A) and other components blended as necessary are dissolved in a solvent, or may be a hot-melt-type polymer composition in a solid or semi-solid state (i.e., non-fluid at room temperature). When the polymer (A) is a (meth)acrylic polymer (A), the pressure-sensitive adhesive composition is preferably a solution-type (also called a solvent-type).
[0086] The solvent used in the preparation of the pressure-sensitive adhesive composition is not particularly limited as long as it is an organic solvent capable of dissolving the polymer (A). Specific examples of the organic solvent include aprotic polar solvents, phenolic solvents, alcoholic solvents, ester solvents, ketone solvents, ether solvents, and hydrocarbon solvents. The organic solvent may be one of these, or a mixture of two or more of them.
[0087] The solid content concentration in the solution-type pressure-sensitive adhesive composition (i.e., the ratio of the mass of components other than the solvent in the pressure-sensitive adhesive composition to the total mass of the pressure-sensitive adhesive composition) is not particularly limited, but is preferably 1 to 70 mass%. A solid content concentration of 1 mass% or more is preferable in that a pressure-sensitive adhesive layer having a sufficient thickness can be formed. Furthermore, a solid content concentration of 70 mass% or less is suitable in that good coating properties can be ensured and a pressure-sensitive adhesive layer of uniform thickness can be easily formed. The solid content concentration in the pressure-sensitive adhesive composition is more preferably 5 to 50 mass%, and even more preferably 10 to 45 mass%.
[0088] The adhesive composition can be applied to a support such as a separator to form an adhesive layer, thereby obtaining an adhesive product such as an adhesive sheet or an adhesive tape. When the adhesive product is used as an adhesive for bonding fiber fabrics together, the fiber fabrics can be bonded together with high strength. In addition, while bonding the fiber fabrics together with high strength, the flexibility and stretchability of the fiber fabrics can be maintained at the bonded portion.
[0089] As the support, a resin film made of various resin materials is used. Examples of the resin material include polyester resins such as polyethylene terephthalate, polyethersulfone resins, acetate resins, polycarbonate resins, polyolefin resins, etc. In the case of a solution-type adhesive composition, the adhesive layer is formed by applying the adhesive composition to the support by a known coating method, and preferably removing the solvent by a drying treatment such as heating. The heating temperature and heating time for forming the adhesive layer may be set appropriately depending on the solvent and solid content concentration of the adhesive composition as long as the solvent can be removed.
[0090] The adhesive product may be in a so-called substrate-less form in which the adhesive layer is sandwiched between two separators having different peel strengths, or may be one in which one of the objects to be joined is a substrate (fiber fabric). The shape of the adhesive product is not particularly limited and is appropriately set according to the use situation. For example, the adhesive sheet may be in a sheet form, a roll form, cut into strips, or may have any shape according to the joining location. The thickness of the adhesive layer in the adhesive product may be appropriately set depending on the objects to be joined, the area and shape of the joining location, etc. The thickness of the adhesive layer is usually 1 to 200 μm. In order to make the adhesive layer of the adhesive product have a desired thickness, the adhesive layer of the adhesive product may be formed by laminating a plurality of adhesive layers.
[0091] The pressure-sensitive adhesive composition has a storage modulus at 23°C of 1.0 MPa or less (hereinafter also referred to as "storage modulus G'"). When fiber fabrics are bonded together by the pressure-sensitive adhesive layer, the pressure-sensitive adhesive composition has high peel strength and can maintain the flexibility and texture of the fabric at the bonded portion. In order to improve the flexibility and texture of the bonded portion, the storage modulus G' is preferably 0.70 MPa or less, more preferably 0.55 MPa or less, even more preferably 0.45 MPa or less, even more preferably 0.40 MPa or less, and particularly preferably 0.30 MPa or less. The lower limit of the storage modulus G' is not particularly limited, but is, for example, 0.1 MPa or more.
[0092] In this specification, the storage modulus G' is a value obtained by measuring the shear viscoelasticity of a 0.8 mm thick pressure-sensitive adhesive layer under the conditions of a measurement temperature of 23°C, a temperature rise rate of 2°C / min, a strain of 0.1%, and a measurement frequency of 1 Hz. The storage modulus G' can be arbitrarily adjusted by adjusting the composition and degree of crosslinking of the polymer (A), the amount of plasticizer added, and the ratio of the hard segment in the block copolymer (A2). For example, in the case of the (meth)acrylic polymer (A), it is preferable to use at least one of an alkyl (meth)acrylate compound and an alkoxyalkyl (meth)acrylate compound as a constituent monomer of the (meth)acrylic polymer (A), and adjust the type and amount of the compound to adjust the storage modulus G'. In addition, when adjusting the storage modulus G' by the ratio of the hard segment in the block copolymer (A2), the storage modulus G' tends to increase as the ratio of the hard segment increases.
[0093] <Textile products for clothing> By bonding two pieces of fiber fabric as adherends together via a pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition, a textile product for clothing can be obtained in which a pressure-sensitive adhesive layer is disposed between two pieces of fiber fabric. Since the textile fabrics in the textile product for clothing are bonded together using the pressure-sensitive adhesive composition, the flexibility and texture of the textile fabrics are maintained at the joints, and the peel strength of the joints is high.
[0094] To obtain the textile product for clothing of the present invention, first, two textile fabrics are bonded together so that they are in contact with each other via the adhesive layer, and if necessary, temporarily bonded to obtain a laminate of textile fabric / adhesive layer / textile fabric, and then the laminate is heated (preferably heat-pressure bonded). When bonding textile fabrics together by heat-pressure bonding, the pressure during bonding may be appropriately set so as to obtain a desired bonding strength. In addition, the heating temperature is preferably set to be equal to or lower than the heat resistance temperature of the adherend (textile fabric) used. The adhesive composition of the present invention is preferable in that the bonding portion is flexible even if the resin is impregnated into the mesh of the textile fabric during heat-pressure bonding, and the textile fabrics can be bonded together with high strength. Furthermore, the adhesive product such as an adhesive sheet obtained using the adhesive composition of the present invention can be used to temporarily bond one textile fabric to another textile fabric, since the adhesive strength of the surface layer of the adhesive layer is high.
[0095] The adhesive composition and adhesive product of the present invention can maintain the flexibility and texture of fabrics even when applied to fibers, and can form an adhesive layer with high adhesiveness, and therefore can be suitably used for fiber fabrics for clothing, including fashion accessories (e.g., woven fabrics, knitted fabrics, nonwoven fabrics, lace, leather (natural leather, synthetic leather, artificial leather, etc.), fur, etc.).
[0096] The fiber fabric to be bonded is not particularly limited, and fiber fabrics used for clothing, such as synthetic fibers such as polyester, polyamide, and acrylic fibers; regenerated fibers such as rayon and cupra; semi-synthetic fibers such as acetate; and natural fibers such as cotton, hemp, and wool, can be appropriately used. In addition, the surface of the fiber fabric to be bonded may be subjected to a water-repellent treatment or the like. The textile products for clothing manufactured using the present adhesive composition are also not particularly limited, and can be used as an adhesive for manufacturing a wide range of clothing such as everyday Western clothes, Japanese clothes, ethnic clothes, underwear (for example, seamless lingerie products and inner products), jackets, tops, bottoms, outdoor goods, work clothes, uniforms, formal wear, swimsuits, sportswear, socks, hats, shoes, etc., or for handicraft purposes. EXAMPLES
[0097] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" mean parts by mass and % by mass unless otherwise specified. The analytical methods and production methods of the polymers used in the examples and comparative examples are as follows.
[0098] <Molecular weight measurement> Using a gel permeation chromatograph (model name "HLC-8320", manufactured by Tosoh Corporation), the number average molecular weight (Mn) and weight average molecular weight (Mw) were obtained in terms of polystyrene under the following conditions. The molecular weight distribution (Mw / Mn) was calculated from the obtained values. Measurement conditions Column: Tosoh TSKgel SuperMultiporeHZ-M x 4 Column temperature: 40℃ Eluent: Tetrahydrofuran Detector: RI Flow rate: 600μL / min
[0099] <Monomer composition ratio of polymer> The monomer composition ratio (mol %) of the polymer was calculated from the charged amount and the monomer consumption amount measured by gas chromatography (GC). The GC measurement was carried out under the following conditions. GC: Agilent Technologies (7820A GC System), detector: FID, column: 100% dimethylsiloxane (CP-Sil 5CB), column length 30 m, column inner diameter 0.32 mm, calculation method: internal standard method
[0100] <Measurement of glass transition temperature (Tg)> The glass transition temperature (Tg) of the polymer was determined from the intersection of the baseline of the heat flux curve obtained using a differential scanning calorimeter and the tangent at the inflection point. The heat flux curve was obtained by cooling about 10 mg of the sample to -50°C, holding it for 5 minutes, and then heating it to 300°C at 10°C / min, followed by cooling it to -50°C, holding it for 5 minutes, and then heating it to 350°C at 10°C / min. Measuring equipment: SII NanoTechnology DSC6220 Measurement atmosphere: Nitrogen atmosphere The glass transition points of polymer block A and polymer block B were determined by producing homopolymers of each polymer block and subjecting the resulting homopolymers to differential scanning calorimetry (DSC) measurement according to the above-mentioned measurement method.
[0101] 1. Synthesis of (meth)acrylic polymers [Synthesis Example 1] Polymer A-1 used in Examples 1 to 3 and Comparative Example 1 In a 3-liter four-neck flask, 2-methoxyethyl acrylate (hereinafter also referred to as "MEA") (421 parts by mass), 2-hydroxyethyl acrylate (hereinafter also referred to as "HEA") (21 parts by mass), n-butyl acrylate (hereinafter also referred to as "BA") (78 parts by mass), and ethyl acetate (770 parts by mass) were charged, and the mixture was thoroughly degassed by bubbling nitrogen gas, and the internal temperature of the mixture was raised to 75°C, and 2,2'-azobis(2,4-dimethylvaleronitrile) (Wako Pure Chemical Industries, Ltd., V-65) (0.35 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content was 30% by mass, and an adhesive solution, which was an ethyl acetate solution of polymer A-1, was obtained. The obtained polymer A-1 had Mn 92,000, Mw / Mn 8.72, and Tg = -35°C.
[0102] [Synthesis Example 2] Polymer A-2 used in Example 4 HEA (24 parts by mass), BA (506 parts by mass), and ethyl acetate (974 parts by mass) were charged into a 3-liter four-neck flask, and the mixture was thoroughly degassed by bubbling nitrogen gas. The internal temperature of the mixture was raised to 75°C, and 2,2'-azobis(2,4-dimethylvaleronitrile) (Wako Pure Chemical Industries, Ltd., V-65) (0.25 parts by mass) was charged to initiate polymerization. After 5 hours, ethyl acetate was added so that the solid content was 30% by mass, and an adhesive solution was obtained, which was an ethyl acetate solution of polymer A-2. The obtained polymer A-2 had Mn 87,000, Mw / Mn 5.38, and Tg = -41°C.
[0103] [Synthesis Example 3] Polymer A-3 used in Example 5 In a 1L flask equipped with a stirrer and a thermometer, dibenzyl trithiocarbonate (hereinafter also referred to as "DBTTC") (3.18 parts by mass) as a RAFT agent, 2,2'-azobis(2-methylbutyronitrile) (hereinafter also referred to as "ABN-E") (0.51 parts by mass) as a polymerization initiator, styrene (hereinafter also referred to as "St") (75 parts by mass) as a monomer, and N-phenylmaleimide (hereinafter also referred to as "PhMI") (125 parts by mass), and acetonitrile (466 parts by mass) as a solvent were charged, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was started in a thermostatic bath at 70 ° C. After 3 hours, the reaction was stopped by cooling to room temperature. The above polymerization solution was purified by reprecipitation from methanol and vacuum dried to obtain a polymer block A. The obtained polymer block A had Mn of 10,900 and Tg of 206 ° C. Next, the obtained polymer block A (21.1 parts by mass), ABN-E (0.08 parts by mass) as a polymerization initiator, MEA (234 parts by mass), BA (51 parts by mass), and HEA (15 parts by mass) as monomers, and acetonitrile (107 parts by mass) as a solvent were charged into a 1 L flask equipped with a stirrer and a thermometer, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was initiated in a thermostatic bath at 70 ° C. After 6 hours, the mixture was cooled to room temperature, and acetonitrile was added to adjust the solid concentration to 30% by mass, to obtain a pressure-sensitive adhesive solution containing polymer A-3, which is an ABA triblock copolymer having polymer block A and polymer block B. The obtained polymer A-3 had Mn 160,000 and Mw / Mn 1.77. The glass transition point of polymer block B was -35 ° C.
[0104] [Synthesis Example 4] Polymer A-5 used in Comparative Example 2 In a 2L flask equipped with a stirrer and a thermometer, DBTTC (1.9 parts by mass) as a RAFT agent, ABN-E (0.25 parts by mass) as a polymerization initiator, St (56 parts by mass) and PhMI (94 parts by mass) as monomers, and acetonitrile (337 parts by mass) as a solvent were charged, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was started in a thermostatic bath at 70 ° C. After 3 hours, the mixture was cooled to room temperature to stop the reaction. The obtained polymer block A had Mn 15,100 and Tg = 212 ° C. Next, in the 2L flask containing the polymer block A, MEA (303 parts by mass), BA (66 parts by mass), and HEA (19 parts by mass) as monomers, and acetonitrile (188 parts by mass) as a solvent were charged, and the mixture was thoroughly degassed by nitrogen bubbling, and polymerization was started in a thermostatic bath at 70 ° C. After 6 hours, the mixture was cooled to room temperature, and acetonitrile was added to adjust the solid content to 30% by mass, to obtain a pressure-sensitive adhesive solution containing polymer A-5, an ABA triblock copolymer having polymer block A and polymer block B. The obtained polymer A-5 had Mn 48,000 and Mw / Mn 1.35. The glass transition point of polymer block B was -35°C.
[0105] The compositions (mol%) calculated from the amounts charged and the monomer consumption amounts measured by GC for the polymers A-1 to A-3 and A-5 produced above, as well as the molecular weight characteristics and glass transition points, are shown in Table 1. In Table 1, "-" means that the compound in the corresponding column was not used.
[0106] [Table 1]
[0107] 2. Synthesis of tackifier resin [Synthesis Example 5] Polymer B-1 used in Example 2 and Comparative Example 1 A mixture of methyl methacrylate (hereinafter also referred to as "MMA") (19 parts by mass), St (11 parts by mass), butyl acetate (224 parts by mass), and V-601 (8.7 parts by mass) was charged into a 1-liter four-neck flask, and the mixture was thoroughly degassed by bubbling nitrogen gas, and the internal temperature of the mixture was raised to 90°C. Separately, a mixture of MMA (108 parts by mass), St (93 parts by mass), V-601 (78 parts by mass), and butyl acetate (90 parts by mass) was dropped into the flask from a dropping funnel over a period of 5 hours to perform polymerization. After the dropwise addition, the polymerization solution was dropped into a mixed solution of methanol (4200 parts by mass) and distilled water (1800 parts by mass), and the vinyl polymer in the polymerization solution was isolated to obtain polymer B-1. The obtained polymer B-1 had Mn 1,910, Mw / Mn 1.47, and Tg = 44°C.
[0108] 3. Evaluation of adhesive composition [Example 1] An ethyl acetate solution (solid content concentration 30% by mass) of the polymer A-1 obtained in Synthesis Example 1 above was applied onto a 50 μm thick polyethylene terephthalate (PET) separator so that the thickness of the adhesive layer after drying would be 100 μm. The adhesive composition was dried at 100° C. for 6 minutes to remove the ethyl acetate. After drying, a 38 μm thick PET separator with a different peel strength from the separator was attached to obtain an adhesive film sample with double-sided separators. The obtained adhesive film sample was used to perform various evaluations by the methods shown below. The evaluation results are shown in Table 2.
[0109] <Temporary pressure bonding> The separator on one side of an adhesive film sample cut to a width of 1.0 cm was peeled off, and the surface of the adhesive layer was brought into contact with polyester fabric. With the polyester fabric and adhesive layer in contact, a 2 kg roller was rolled back and forth three times on the surface. After that, when trying to peel off the other separator, if the adhesive layer peeled off from the separator and remained on the polyester fabric side, it was marked as "○", if it partially remained on the fabric, it was marked as "△", and if the adhesive layer was completely peeled off from the fabric and attached to the separator side, it was marked as "×", and the temporary pressure-sensitive adhesiveness was evaluated. <Peel strength measurement> The polyester fabrics were bonded together using a 1.0 cm wide adhesive film sample to obtain a laminate consisting of polyester fabric / adhesive film / polyester fabric. The obtained laminate was subjected to a heat press treatment (conditions: 130°C, 3 kg / cm 2 The laminate after compression was used as a test piece, and the T-peel strength was measured using a tensile tester INSTRON 5566A (manufactured by Instron Japan) under conditions of a measurement temperature of 23°C, a test piece width of 10 mm, and a peel speed of 300 mm / min, and this was taken as the adhesive strength.
[0110] <Storage modulus G' at room temperature (23℃)> The adhesive layer of the adhesive film sample was laminated to prepare a test piece with an adhesive layer of 800 μm thickness. This test piece was punched out into a circle with a diameter of 1 cm, and the dynamic viscoelasticity was measured at a strain of 0.1% and a frequency of 1 Hz while increasing the temperature from -50°C to 150°C at a rate of 2°C / min using a viscoelasticity measuring device Physica MCR301 (manufactured by Anton Paar), and the storage modulus G' at 23°C was read. A parallel plate with a diameter of 8 mm was used for the measurement. <Texture of adhesive joint> The bending stiffness and stretchability of the bonded portion of the test piece bonded by hot pressing were confirmed by touch and evaluated according to the following criteria. ○: Soft and stretchy. △: Feels a little stiff and some resistance is felt when stretching. ×: Feels hard and not very stretchy.
[0111] <Washing resistance> Test pieces prepared using the same procedure as in the peel strength measurement were washed in a tabletop washing machine (ALUMiSALUMiS, AHB-02) for 6 minutes, then left submerged in water for 1 hour, and then spin-dried for 1 minute. After spin-drying, the pieces were left to stand for 24 hours in an environment with a temperature of 23°C and a humidity of 50%, and then the peel strength was measured in the same manner as in the peel strength measurement above. If the peel strength measured after washing was 50% or more of the peel strength before washing, it was evaluated as "○", if it was less than 50%, it was evaluated as "△", and if it peeled off during the washing process, it was evaluated as "×".
[0112] [Example 2] 100 parts by mass of the ethyl acetate solution (solid content concentration 30% by mass) of the polymer A-1 obtained in the above Synthesis Example 1 was mixed with 0.08 parts by mass (solid content concentration 75% by mass, manufactured by Mitsui Chemicals) of Takenate D-110N as a crosslinking agent (0.2 parts by mass of crosslinking agent per 100 parts by mass of the polymer A-1 in terms of solid content) to obtain a pressure-sensitive adhesive composition. This pressure-sensitive adhesive composition was used to obtain a pressure-sensitive adhesive film sample with a double-sided separator in the same manner as in Example 1. The crosslinking reaction was then promoted by aging at 40°C for 5 days. The obtained pressure-sensitive adhesive film sample was used to perform various evaluations in the same manner as in Example 1. The evaluation results are shown in Table 2. [Example 3] An ethyl acetate solution of polymer A-1 obtained in Synthesis Example 1 above was taken in an amount such that polymer A-1 was 100 parts by mass in terms of solid content, and 4 parts by mass of polymer B-1 obtained in Synthesis Example 5 above was taken, and ethyl acetate was added to prepare a pressure-sensitive adhesive composition having a solid content concentration of 30% by mass. Using this pressure-sensitive adhesive composition, a pressure-sensitive adhesive film sample with a double-sided separator was obtained in the same manner as in Example 1. In addition, various evaluations were performed using the obtained pressure-sensitive adhesive film sample in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0113] [Examples 4 and 5] A pressure-sensitive adhesive film sample with a double-sided separator was obtained in the same manner as in Example 1, except that in Example 4, a pressure-sensitive adhesive solution of polymer A-2 obtained in Synthesis Example 2 was used, and in Example 5, a pressure-sensitive adhesive solution of polymer A-3 obtained in Synthesis Example 3 was used. In addition, various evaluations were performed in the same manner as in Example 1 using the obtained pressure-sensitive adhesive film sample. The evaluation results are shown in Table 2. [Example 6] A polyester adhesive ("PES310S30" manufactured by Toagosei Co., Ltd., a mixed solution of toluene and methyl ethyl ketone (MEK) with a solid content concentration of 30% by mass) was used to obtain a pressure-sensitive adhesive film sample with a double-sided separator in the same manner as in Example 1. In addition, various evaluations were performed in the same manner as in Example 1 using the obtained pressure-sensitive adhesive film sample. The evaluation results are shown in Table 2.
[0114] [Comparative Example 1] A pressure-sensitive adhesive composition having a solid content concentration of 30% by mass was prepared in the same manner as in Example 3, except that the blending amount of polymer B-1 was changed to 10 parts by mass. In addition, a pressure-sensitive adhesive composition thus prepared was used to produce a pressure-sensitive adhesive film sample with a double-sided separator in the same manner as in Example 1, and various evaluations were performed in the same manner as in Example 1. The evaluation results are shown in Table 2. [Comparative Example 2] Using the adhesive solution of polymer A-5 obtained in Synthesis Example 4, an adhesive film sample with a double-sided separator was obtained in the same manner as in Example 1. In addition, using the obtained adhesive film sample, various evaluations were performed in the same manner as in Example 1. The evaluation results are shown in Table 2. [Comparative Example 3] An emulsion adhesive (Arontack "HV-C5166" manufactured by Toagosei Co., Ltd., solid content concentration 55% by mass) was used to obtain an adhesive film sample with a double-sided separator in the same manner as in Example 1. The obtained adhesive film sample was used to carry out various evaluations in the same manner as in Example 1. The evaluation results are shown in Table 2. [Comparative Example 4] Two commercially available urethane hot melt adhesive films (film thickness 50 μm) were stacked and heat pressed (conditions: 130°C, 0.5 kg / cm 2 10 seconds) to obtain a pressure-sensitive adhesive film sample with a double-sided separator having a pressure-sensitive adhesive layer of 100 μm. Furthermore, the obtained pressure-sensitive adhesive film sample was used to carry out various evaluations in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0115] [Table 2]
[0116] The abbreviations in Table 2 are as follows: A-4: Polyester adhesive "PES310S30" (manufactured by Toagosei Co., Ltd.) A-6: Emulsion adhesive "Arontack HV-C5166" (manufactured by Toagosei Co., Ltd.) A-7: Commercially available urethane-based hot melt adhesive D-110N: Takenate D-110N (manufactured by Mitsui Chemicals) In Table 2, the amounts of the polymer and the crosslinking agent are shown as solid content converted amounts (parts by mass).
[0117] As shown in Table 2, in Examples 1 to 6, which used adhesive compositions containing polymers A-1 to A-4 and in which the adhesive layer had a storage modulus G' of 1.0 MPa or less at 23°C, the peel strength was higher than 6.0 N / 10 mm and peeling was unlikely to occur at the adhesion site. Examples 1 to 6 also had good temporary pressure-sensitive adhesive properties. Among these, the adhesive compositions not containing a tackifier (Examples 1, 2, and 4 to 6) were rated as "○" for temporary pressure-sensitive adhesive properties and were particularly excellent.
[0118] Furthermore, in Examples 1 to 6, the bonded portions of the fiber fabrics were flexible and had good stretchability. In particular, Example 5, which used a triblock copolymer as the polymer (A), had a very high peel strength of 13.2 N / 10 mm, and showed excellent adhesion while maintaining the flexibility and stretchability of the bonded portions. Moreover, Examples 1 to 5, which used the (meth)acrylic polymer (A), also had excellent washability.
[0119] On the other hand, in Comparative Example 1, in which the content of the polymer B-1 was 10 parts by mass, the peel strength, the texture of the bonded part, and the washing resistance were good, but the adhesive strength was weak and the temporary pressure-sensitive adhesive property was poor. In addition, the adhesive composition of Comparative Example 2, in which the storage modulus G' at 23°C of the adhesive layer was greater than 1.0 MPa, had insufficient flexibility and elasticity of the bonded part, low peel strength, and also inferior temporary pressure-sensitive adhesive property and washing resistance to Examples 1 to 6. In Comparative Example 3, in which an emulsion adhesive was used, the texture of the bonded part was good, but the washing resistance was poor. In Comparative Example 4, in which fiber fabrics were bonded together with a urethane-based hot melt adhesive, the peel strength was high at 13.0 N / 10 mm, but the bonded part was hard and the elasticity was insufficient.
Claims
1. A pressure-sensitive adhesive composition for bonding textile fabrics for clothing, the pressure-sensitive adhesive composition comprising a polymer component in a solution form dissolved in an organic solvent or in a solid or semi-solid form, a pressure-sensitive adhesive layer formed using the pressure-sensitive adhesive composition has a storage modulus at 23° C. of 1.0 MPa or less; the content of the vinyl polymer (B) having a number average molecular weight of 10,000 or less is 5 parts by mass or less per 100 parts by mass of the (meth)acrylic polymer (A); the (meth)acrylic polymer (A) contains structural units derived from a hydroxyalkyl (meth)acrylate compound in an amount of 1 mol % or more and 20 mol % or less, based on all constituent monomer units contained in the (meth)acrylic polymer (A), and contains structural units derived from an alkyl (meth)acrylate compound in an amount of 50 mol % or more, based on all constituent monomer units contained in the (meth)acrylic polymer (A).
2. An adhesive product comprising: a support; and an adhesive layer formed on the support using the clothing adhesive composition according to claim 1.
3. A textile product for clothing, in which two textile fabrics are bonded together using the pressure-sensitive adhesive composition for clothing according to claim 1.
Citation Information
Patent Citations
Pressure sensitive adhesive
JP1985015478A
Dispersion composition, manufacture and use
JP1985235859A
Hydrogel adhesive for use on surfaces dense with hair or fibers
JP2005525441A
Production method of leather-like sheet
JP2011006834A
Optical information recording medium
JP2011070770A