Solid Oxide Fuel Cell
A symmetrical laminated structure in the support cell addresses bonding and thermal stress issues by equalizing stress distribution, improving bonding strength and gas sealing, resulting in a highly reliable solid oxide fuel cell.
Patent Information
- Application Number
- JP2020087967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-20
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-05-20
AI Technical Summary
The existing metal support cell assemblies in solid oxide fuel cells face issues with bonding strength at the joint between the support layer and the cell frame, leading to potential gas leakage and deformation due to insufficient bonding and thermal stress during manufacturing.
A symmetrical laminated structure is implemented in the support cell, where the anode and cathode layers have equal thickness, and the anode and cathode support layers are of the same material, with a joint surface exposing the electrolyte layer to enhance bonding strength and control thermal contraction.
The symmetrical laminated structure improves bonding strength and gas sealing properties, providing a highly reliable support cell by offsetting bending deformation and maintaining a flat bonding surface, thus enhancing the stability and performance of the solid oxide fuel cell.
Smart Images

Figure 0007552073000004 
Figure 0007552073000017 
Figure 0007552073000025
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid oxide fuel cell. [Background technology]
[0002] Conventionally, supported cells, in which a support layer is arranged on a single cell having an electrolyte layer sandwiched between an anode layer and a cathode layer, have been applied to solid oxide fuel cells (SOFCs, hereafter simply referred to as "SOFCs"). The support layer is made of ceramics or metal and has gas permeability. Metal-supported cells (MSCs), which have a support layer made of metal, are excellent in mechanical strength, rapid start-up, etc.
[0003] The electrolyte layer, made of thin ceramics, is prone to damage due to stress during manufacturing and operation. In addition, in SOFCs, anode gas and cathode gas must be distributed to the fuel pole (anode layer) and oxidizer pole (cathode layer) of the electrode layer, respectively, and sealing properties are required to prevent these gases from mixing.
[0004] A metal support cell assembly in an SOFC has a metal support cell and a cell frame that surrounds and holds the periphery of the metal support cell. For example, the following Patent Document 1 discloses a metal support cell assembly in which the support layer of the metal support cell is joined to the end of the cell frame. The support layer and the cell frame are joined by soldering, brazing, or glass sealing. In the metal support cell assembly of Patent Document 1, the electrolyte layer of the metal support cell is not in contact with the cell frame. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] U.S. Patent No. 8,287,673 Summary of the Invention [Problem to be solved by the invention]
[0006] In the metal support cell assembly described in Patent Document 1, the support layer is bonded to the end of the cell frame. Therefore, if the bond strength is insufficient, peeling may occur at the bonded portion, which may lead to gas leakage.
[0007] In addition, since the support cell is subjected to heat treatment such as sintering during manufacture, there is a risk of deformation due to the heat treatment. In order to provide a solid oxide fuel cell having a highly reliable support cell, it is necessary to take into consideration the stress state caused by the shrinkage of the support cell during the heat treatment.
[0008] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide a solid oxide fuel cell having a highly reliable support cell. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention provides a single cell having an electrolyte layer sandwiched between an anode layer and a cathode layer, and a cathode layer on each of the two sides of the single cell. Anode side support layer and cathode side support layer The support cell has a cell outer periphery where a part of the electrolyte layer is exposed and a joining surface for joining a cell frame is formed, and a cell main body part located on the central side of the cell outer periphery. In a cross section in the thickness direction of the support cell, the cell main body part has a center line of the thickness of the cell main body part. (O2) The cell outer periphery has a symmetrical laminate structure with respect to a center line of the thickness of the cell outer periphery. (O1) It has a symmetrical laminate structure with respect to The anode layer and the cathode layer are made of the same material, and the anode-side support layer and the cathode-side support layer are made of the same material. In the cell main body, the anode layer and the cathode layer have the same thickness, and the anode-side support layer and the cathode-side support layer have the same thickness. The cell peripheral portion is configured by laminating the electrolyte layer on which the bonding surface is formed, a first forming layer formed from the anode layer or the cathode layer, a second forming layer formed from the anode-side support layer or the cathode-side support layer, a third forming layer formed from the same material as the anode layer and the cathode layer, and a fourth forming layer formed from the same material as the electrolyte layer. In the cell peripheral portion, the electrolyte layer and the fourth forming layer have the same thickness, and the first forming layer and the third forming layer have the same thickness. . Effect of the Invention
[0010] According to the present invention, in the cross section of the support cell in the thickness direction, the cell body and the cell outer periphery have a laminated structure that is symmetrical with respect to the center line of their respective thicknesses, so that thermal contraction in the in-plane direction is controlled and bending deformation of the support cell is offset. Since the bonding surface where the electrolyte layer is exposed is flattened, the bonding strength between the cell frame and the support cell can be improved, and a solid oxide fuel cell having a highly reliable support cell can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is an exploded perspective view showing a fuel cell stack. [Diagram 2] FIG. 2 is an exploded perspective view of the cell unit shown in FIG. [Diagram 3] FIG. 3 is an exploded perspective view showing the support cell assembly shown in FIG. 2. [Figure 4] 1 is a cross-sectional view showing a fuel cell stack according to an embodiment. [Diagram 5] FIG. 3 is a partial cross-sectional view showing the support cell assembly taken along line AA in FIG. 2. [Figure 6A] FIG. 6 is a cross-sectional view showing the support cell shown in FIG. [Figure 6B] 6B is an enlarged cross-sectional view showing a main part of the support cell shown in FIG. 6A. [Figure 7A] FIG. 6B is a top view of the support cell shown in FIG. 6A. [Figure 7B] FIG. 6B is a bottom view of the support cell shown in FIG. 6A. [Figure 8] 6B is a schematic diagram showing how bending acting on the support cell shown in FIG. 6A is offset. FIG. [Figure 9A] FIG. 11 is an enlarged cross-sectional view showing a main part of a support cell of a comparative example. [Figure 9B] FIG. 13 is a schematic diagram showing a state in which bending deformation occurs in a support cell according to a comparative example. [Figure 10A] FIG. 1 is an explanatory diagram used to explain stresses that occur when sintering a workpiece in which two layers made of different materials are stacked. [Figure 10B]1 is a schematic diagram showing a state in which a workpiece has an asymmetric layered structure with respect to a center line of the thickness of the workpiece in a cross section in the thickness direction of the workpiece; [Figure 10C] 10C is a schematic diagram showing a state in which bending deformation occurs in the workpiece shown in FIG. 10B. [Figure 11A] 1 is an explanatory diagram used to explain the mechanism by which bending deformation is suppressed when the workpiece has a layered structure that is symmetrical with respect to the center line of the thickness of the workpiece in a cross section in the thickness direction of the workpiece. FIG. [Figure 11B] FIG. 11B is an explanatory diagram following FIG. 11A. [Figure 11C] FIG. 11B is an explanatory diagram following FIG. [Figure 11D] FIG. 11D is an explanatory diagram following FIG. 11C. [Figure 12] FIG. 11 is a cross-sectional view showing a fuel cell stack according to a first modified example. [Figure 13] FIG. 13 is a partial cross-sectional view showing the support cell assembly shown in FIG. [Figure 14A] FIG. 14 is a cross-sectional view showing the support cell shown in FIG. [Figure 14B] 14B is an enlarged cross-sectional view showing a main part of the support cell shown in FIG. 14A. [Figure 15A] FIG. 14B is a top view of the support cell shown in FIG. 14A. [Figure 15B] FIG. 14B is a bottom view of the support cell shown in FIG. 14A. [Figure 16A] 13A and 13B are schematic diagrams showing how bending acts on a support cell of Modification 1. [Figure 16B] 13 is a schematic diagram illustrating the operation of a support cell assembly to which the support cell of Modification 1 is applied. FIG. [Figure 17A] 13 is a schematic diagram showing a state in which bending acts on a support cell of Modification 2. FIG. [Figure 17B] 13 is a schematic diagram illustrating the operation of a support cell assembly to which the support cell of Modification 2 is applied. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the attached drawings. Note that the following description does not limit the technical scope or meaning of terms described in the claims. Also, the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.
[0013] A solid oxide fuel cell (SOFC) according to an embodiment of the present invention will be described with reference to the drawings. For convenience of the following description, an XYZ Cartesian coordinate system is shown in the drawings. The X-axis and Y-axis are parallel to the horizontal direction, and the Z-axis is parallel to the vertical direction.
[0014] Fig. 1 is an exploded perspective view showing a fuel cell stack 1 according to an embodiment. As shown in Fig. 1, the fuel cell stack 1 is configured by stacking a plurality of cell units 1U in the vertical direction. Hereinafter, the vertical direction of the fuel cell stack 1, indicated by the Z axis in the figure, will also be referred to as the "stacking direction". The plane direction of each layer constituting the cell unit 1U corresponds to the XY plane direction.
[0015] Fig. 2 is an exploded perspective view of the cell unit 1U. As shown in Fig. 2, the cell unit 1U is formed by stacking a support cell assembly 1A and a separator 120 having a flow path portion 121 that defines a gas flow path.
[0016] Fig. 3 is an exploded perspective view of the support cell assembly 1A. Fig. 4 is a cross-sectional view showing the fuel cell stack 1, and Fig. 5 is a partial cross-sectional view showing the support cell assembly 1A along the line AA in Fig. 2. As shown in Figs. 3, 4, and 5, the support cell assembly 1A has a support cell 10 and a cell frame 70 that surrounds and holds the periphery of the support cell 10.
[0017] Fig. 6A is a cross-sectional view showing the support cell 10, and Fig. 6B is an enlarged cross-sectional view showing a main part of the support cell 10. Fig. 7A is a top view of the support cell 10, and Fig. 7B is a bottom view of the support cell 10.
[0018] As shown in FIG. 6A and FIG. 6B, the support cell 10 has a sandwich structure in which support layers (anode side support layer 61 and cathode side support layer 62) are arranged on both sides of the electrolyte electrode assembly 20 (corresponding to a single cell) in which the electrolyte layer 40 is sandwiched between the anode layer 30 and the cathode layer 50. The support cell 10 is configured by laminating the anode side support layer 61, the anode layer 30, the electrolyte layer 40, the cathode layer 50, and the cathode side support layer 62. The anode side support layer 61 and the cathode side support layer 62 have different lengths along the X direction and the Y direction. In the illustrated example, the length of the cathode side support layer 62 is shorter than the length of the anode side support layer 61. By making the lengths of the anode side support layer 61 and the cathode side support layer 62 different, a structure is formed in which a part of the electrolyte layer 40 is exposed. The exposed part of the electrolyte layer 40 forms a joining surface 94 for joining the cell frame 70. Hereinafter, the anode side support layer 61 and the cathode side support layer 62 may be referred to as a pair of support layers 61, 62. The anode layer 30 and the cathode layer 50 may be referred to collectively as electrode layers 30, 50.
[0019] The electrolyte layer 40 is fixed to the anode side support layer 61 via the anode layer 30. The cathode side support layer 62 is fixed to the cathode layer 50. In the sandwich-structured support cell 10, a pair of support layers 61, 62 support the electrolyte electrode assembly 20. The support cell 10 is excellent in mechanical strength, rapid start-up performance, etc. compared to electrolyte-supported cells and electrode-supported cells, and therefore can be suitably used for SOFCs.
[0020] The support cell 10 has a first bonding layer 81 with the cell frame 70 formed at the exposed portion of the electrolyte layer 40. The support cell 10 further has a second bonding layer 82 that bonds the end 71 of the cell frame 70 to the end 63 of the cathode-side support layer 62. The cell frame 70 and the electrolyte layer 40 are dense and have gas shielding properties. Therefore, by bonding the cell frame 70 and the electrolyte layer 40, a gas sealing function can be ensured.
[0021] Next, the cathode layer 50, the electrolyte layer 40, the anode layer 30, the pair of support layers 61, 62, the cell frame 70, the separator 120, the first bonding layer 81, and the second bonding layer 82 will be described.
[0022] (Cathode layer 50) The cathode layer 50 is an oxidizer electrode that reacts with a cathode gas (e.g., oxygen contained in air) and electrons to convert oxygen molecules into oxide ions. The cathode layer 50 is resistant to an oxidizing atmosphere, and has high gas permeability that allows the cathode gas to pass through and high electrical (electron and ion) conductivity. Furthermore, the cathode layer 50 has a catalytic function that converts oxygen molecules into oxygen ions.
[0023] Examples of materials for forming the cathode layer 50 include oxides of lanthanum, strontium, manganese, cobalt, and the like.
[0024] (Electrolyte layer 40) The electrolyte layer 40 has a function of separating the anode gas and the cathode gas. The electrolyte layer 40 allows oxide ions to pass from the cathode layer 50 to the anode layer 30, but does not allow gas and electrons to pass through. When oxygen ions are the conductor for power generation, the electrolyte layer 40 is preferably formed from a material that has high conductivity for oxygen ions.
[0025] The electrolyte layer 40 is densely constructed to block anode gas and cathode gas and exhibit high ion conductivity. The density of the electrolyte layer 40 is not particularly limited as long as it has gas blocking properties, but is preferably 90% or more, more preferably 96% or more, and particularly preferably 98% or more.
[0026] The material for forming the electrolyte layer 40 is not particularly limited, but examples thereof include solid oxide ceramics such as stabilized zirconia doped with rare earth oxides (e.g., one or more selected from Y2O3, Sc2O3, Gd2O3, Sm2O3, Yb2O3, Nd2O3, etc.), ceria-based solid solutions, and perovskite-type oxides (e.g., SrCeO3, BaCeO3, CaZrO3, SrZrO3, etc.).
[0027] (anode layer 30) The anode layer 30 is a fuel electrode that reacts anode gas (e.g., hydrogen) with oxide ions to generate oxides of the anode gas and extract electrons. The anode layer 30 is resistant to a reducing atmosphere, and has high gas permeability that allows the anode gas to pass through and high electrical (electron and ion) conductivity. Furthermore, the anode layer 30 has a catalytic function that causes the anode gas to react with oxide ions. Examples of materials for forming the anode layer 30 include metals such as Ni and Fe, and cermets of such metals and the ceramics listed as materials for forming the electrolyte layer 40.
[0028] The anode layer 30 is a porous body having a plurality of pores formed therein. A catalyst is impregnated into the pores in the anode layer 30. As the catalyst for the anode layer 30, for example, a metal catalyst such as Ni or Cu can be used.
[0029] (Support Layer (Anode Side Support Layer 61 and Cathode Side Support Layer 62)) 3, 4, 5, 6A, and 6B, in the support cell 10 having a sandwich structure, the anode-side support layer 61 supports the electrolyte electrode assembly 20 from the anode layer 30 side, and the cathode-side support layer 62 supports the electrolyte electrode assembly 20 from the cathode layer 50 side. By the anode-side support layer 61 and the cathode-side support layer 62 supporting the electrolyte electrode assembly 20 in a sandwich structure, the mechanical strength of the electrolyte electrode assembly 20 can be improved and breakage can be suppressed.
[0030] 4, 5, 6A, and 6B, the cathode-side support layer 62 has a cutout portion 68a on the upper outer periphery in the figures. The cutout portion 68a is formed by a support surface 68b that supports the cell frame 70 and a vertical wall 68c that rises upward in the figures from the inner end of the support surface 68b.
[0031] The support layer can be made of metal or ceramics. The material of the support layer can be freely selected depending on the required strength. The support cell 10 can have a configuration in which the pair of support layers 61, 62 are both made of metal, or a configuration in which the pair of support layers 61, 62 are both made of ceramics. In the support cell 10 of the embodiment, the anode side support layer 61 and the cathode side support layer 62 are both made of metal.
[0032] The support layer made of metal (also referred to as "metal support layer") is formed from a porous metal having gas permeability and electron conductivity. The material for forming the metal support layer is not particularly limited as long as it is a metal material having high oxidation resistance and high heat resistance, and for example, ferritic stainless steel is mentioned. Ferritic stainless steel includes SUS400 series such as SUS410, SUS420, SUS430, and SUS440. In particular, Crofer (registered trademark) 22 alloy (manufactured by ThyssenKrupp·VDM), ZMG (registered trademark) 232G10 (manufactured by Hitachi Metals, Ltd.), ITM (manufactured by Plansee), SanergyHT (manufactured by Sandvik), etc. are preferably used.
[0033] The metal support layer is not limited to being made of the above-mentioned materials, and may be made of, for example, an expanded metal having minute through-holes.
[0034] (Cell Frame 70) As shown in Figures 3, 4, and 5, the cell frame 70 supports the support cell 10 from the periphery. As shown in Figure 3, the cell frame 70 has an opening 70H. The support cell 10 is placed in the opening 70H of the cell frame 70. As shown in Figures 4 and 5, the electrolyte layer 40 of the support cell 10 is surface-bonded to the lower surface of the cell frame 70 by a first bonding layer 81. The inner edge of the opening 70H of the cell frame 70 (the end 71 of the cell frame 70) is bonded to the end 63 of the cathode-side support layer 62 by a second bonding layer 82.
[0035] The cell frame 70 is formed from a dense metal material that does not allow gas to pass through, such as stainless steel. The density of the cell frame 70 is not particularly limited as long as it has gas shielding properties, but is preferably 90% or more, more preferably 96% or more, and particularly preferably 98% or more. The surface of the cell frame 70 is subjected to an insulating treatment.
[0036] As shown in FIG. 3, the cell frame 70 has an anode gas inlet 70a and an anode gas outlet 70b through which the anode gas flows, and a cathode gas inlet 70c and a cathode gas outlet 70d through which the cathode gas flows.
[0037] (Separator 120) 2 and 4, the flow path portion 121 of the separator 120 is formed in a substantially linear shape such that the concave and convex shape extends in one direction (Y direction). Therefore, the flow direction of the gas flowing along the flow path portion 121 is the Y direction.
[0038] As shown in FIG. 2, the separator 120 has an anode gas inlet 125a and an anode gas outlet 125b through which the anode gas flows, and a cathode gas inlet 125c and a cathode gas outlet 125d through which the cathode gas flows.
[0039] (1st bonding layer 81) The first bonding layer 81 is disposed between the cell frame 70 supported by the support surface 68b of the cathode-side support layer 62 and the exposed electrolyte layer 40. The first bonding layer 81 is formed of a glass seal. This seals the end of the cathode layer 50, ensuring gas sealing properties.
[0040] (Second bonding layer 82) The second bonding layer 82 is disposed between the cell frame 70 and the cathode side support layer 62. The second bonding layer 82 further has a shape that extends toward the surface of the cell frame 70. The end 71 of the cell frame 70 is surrounded by the support surface 68b of the cathode side support layer 62 and the second bonding layer 82. The material of the second bonding layer 82 can be a brazing material or glass. In the fourth modification, the material of the second bonding layer 82 is a brazing material. The main element of the brazing material is, for example, aluminum, copper, silver, or nickel.
[0041] [Layer structure of support cell 10] 6A, 6B, 7A, and 7B, the support cell 10 has a cell outer periphery 91 where a part of the electrolyte layer 40 is exposed and a joining surface 94 for joining the cell frame 70 is formed, and a cell main body 92 located toward the center of the cell outer periphery 91. In a cross section of the support cell 10 in the thickness direction, the cell main body 92 has a layered structure that is symmetrical with respect to a center line O2 of the thickness of the cell main body 92. Furthermore, in a cross section of the support cell 10 in the thickness direction, the cell outer periphery 91 has a layered structure that is symmetrical with respect to a center line O1 of the thickness of the cell outer periphery 91.
[0042] The support cell 10 further has a cell intermediate portion 93 disposed between the cell main body portion 92 and the cell outer periphery portion 91. In the cell intermediate portion 93, the support layer on the side where the joining surface 94 is formed has a notch portion 68a that joins the end portion 71 of the cell frame 70. In a cross section in the thickness direction of the support cell 10, the cell intermediate portion 93 has a layered structure that is symmetrical with respect to a center line O3 of the thickness of the cell intermediate portion 93.
[0043] The cell peripheral portion 91 has an additional layer 95 arranged on the opposite electrode side to the anode layer 30 or the cathode layer 50 on which the bonding surface 94 is formed. By arranging the additional layer 95, the cell peripheral portion 91 can have a laminated structure that is symmetrical with respect to the center line O1 of the thickness of the cell peripheral portion 91.
[0044] Here, the reason why the laminated structure is symmetrical with respect to the center lines O1 and O2 of the thickness is to apply stress in the same manner to each of two imaginary layers separated by the center lines O1 and O2 of the thickness. do.
[0045] Specifically, the additional layer 95 is a first layer 95a that is the same as the cathode layer 50 or the anode layer 30. (corresponding to the third cambium layer) and a second layer 95b which is the same as the electrolyte layer 40. (corresponding to the fourth cambium) The cell peripheral portion 91 has a symmetrical laminate structure with respect to the anode side support layer 61. By configuring in this manner, it is possible to easily construct the cell peripheral portion 91 having a symmetrical laminate structure with respect to the center line O1 of the thickness.
[0046] The bonding surface 94, which is a part of the electrolyte layer 40 that is exposed, can be disposed on either the anode layer 30 side or the cathode layer 50 side, and is not limited thereto. In the support cell 10 of the embodiment, the bonding surface 94 is disposed on the cathode layer 50 side. Therefore, the additional layer 95 is disposed on the anode layer 30 side, which is the opposite polarity side to the cathode layer 50 on which the bonding surface 94 is formed.
[0047] The cell main body 92 is formed by laminating a cathode side support layer 62, a cathode layer 50, an electrolyte layer 40, an anode layer 30, and an anode side support layer 61. The cathode layer 50 and the anode layer 30 have substantially the same thickness. The cathode side support layer 62 and the anode side support layer 61 in the cell main body 92 have substantially the same thickness. A center line O2 of the thickness of the cell main body 92 corresponds to the center line of the electrolyte layer 40.
[0048] The cell intermediate portion 93, like the cell main body portion 92, has a cathode side support layer 62, a cathode layer 50, an electrolyte layer 40, an anode layer 30, and an anode side support layer 61 laminated therein. However, since the cell intermediate portion 93 has a cutout portion 68a, the thickness of the cathode side support layer 62 in the cell intermediate portion 93 is smaller than the thickness of the cathode side support layer 62 in the cell main body portion 92. The thickness dimensions of the cathode side support layer 62 in the cell intermediate portion 93 and the anode side support layer 61 in the cell intermediate portion 93 and the cell outer peripheral portion 91 are approximately equal. A center line O3 of the thickness in the cell intermediate portion 93 is the center line of the electrolyte layer 40.
[0049] The cell outer periphery 91 is formed by exposing the electrolyte layer 40 and the anode layer 30. (corresponding to the first cambium layer) , anode side support layer 61 (corresponding to the second cambium) The additional layer 95 is formed by laminating a first layer 95a, which is the same as the anode layer 30, from the anode side support layer 61 side. (corresponding to the third cambium layer) , and a second layer 95b identical to the electrolyte layer 40. (corresponding to the fourth cambium) The center line O1 of the thickness direction at the cell outer circumferential portion 91 corresponds to the center line of the anode side support layer 61.
[0050] In the manufacture of the support cell 10, a green sheet is first prepared. The green sheet is a sheet in a state in which the ink for each layer is applied to a laminate film and then the laminate film is laminated. Each layer in the green sheet is only connected by a binder and a solvent.
[0051] Next, the green sheet is degreased. Before firing, the temperature is raised in the air (for example, to 600°C) to remove the binder and solvent contained in each layer. During the degreasing process, a large amount of chemical shrinkage occurs.
[0052] Next, reduction firing is performed. After degreasing, the anode layer 30 is heated in a reducing atmosphere (for example, at 1250° C.) and sintered. In the reduction firing process, significant thermal shrinkage occurs. After reduction firing, the anode layer 30 is impregnated with a catalyst solution.
[0053] Fig. 8 is a schematic diagram showing how bending acting on the support cell 10 of the embodiment is offset. Fig. 9A is an enlarged cross-sectional view showing a main part of a comparative support cell 200, and Fig. 9B is a schematic diagram showing a state in which bending deformation occurs in the comparative support cell 200.
[0054] 9A , in a cross section of the support cell 200 in the thickness direction of the comparative example, the cell main body 292 has a stacked structure that is symmetrical with respect to a center line O2 of the thickness of the cell main body 292. The cell peripheral portion 291 has a structure in which the electrolyte layer 40, the anode layer 30, and the anode-side support layer 61 are stacked. Therefore, in a cross section of the support cell 200 in the thickness direction, the cell peripheral portion 291 has an asymmetric stacked structure with respect to a center line O1 of the thickness of the cell peripheral portion 291.
[0055] 9B, in the comparative support cell 200, bending (arrow 201) occurs in the cell outer periphery 291 of the asymmetric laminated structure as a result of heat treatment such as sintering. Therefore, bending stress is concentrated in the electrolyte layer 40 at the portion indicated by reference numeral 202. As a result, the bonding surface 294 where the electrolyte layer 40 is exposed does not become flat, and the bonding strength between the cell frame 70 and the support cell 200 decreases, which may result in a decrease in gas sealing performance.
[0056] On the other hand, as shown in FIG. 8, in the support cell 10 of the embodiment, in a cross section in the thickness direction of the support cell 10, the cell main body 92, the cell intermediate part 93, and the cell outer peripheral part 91 have a laminated structure symmetrical with respect to center lines O2, O3, and O1 of the thickness, respectively. In each of the cell main body 92, the cell intermediate part 93, and the cell outer peripheral part 91, thermal contraction in the in-plane direction is controlled, and bending deformation (arrows 96, 97) of the support cell 10 is offset. As a result, the joint surface 94 exposing the electrolyte layer 40 is flattened, improving the joint strength between the cell frame 70 and the support cell 10 and improving the gas sealing property. This makes it possible to provide a solid oxide fuel cell having a highly reliable support cell 10.
[0057] Next, the phenomenon of bending occurring in a workpiece having a laminated structure asymmetric with respect to the center line of the thickness will be described with reference to schematic diagrams. Fig. 10A is an explanatory diagram used to explain the stress occurring when sintering a workpiece 300 in which two layers 301 and 302 made of different materials are laminated, Fig. 10B is a schematic diagram showing a state in which the workpiece 300 has a laminated structure asymmetric with respect to the center line of the thickness in a cross section in the thickness direction, and Fig. 10C is a schematic diagram showing a state in which bending deformation occurs in the workpiece 300 shown in Fig. 10B.
[0058] As shown in FIG. 10A, the workpiece 300 is formed by laminating an A layer 301 made of a first material and a B layer 302 made of a second material. Here, it is assumed that the amount of shrinkage of the second material is greater than the amount of shrinkage of the first material. The amount of shrinkage is the sum of shrinkage due to chemical changes during firing, thermal shrinkage due to temperature changes, and the like. Since the first material is subject to strong shrinkage from the second material, a compressive stress (arrow 303) acts on the A layer 301. Meanwhile, since the second material is subject to a reaction force from the first material, a tensile stress (arrow 304) acts on the B layer 302.
[0059] As shown in Figures 10B and 10C, when the stress states of the two layers 301, 302 are not symmetrical in the thickness direction, deformation (bending) occurs in a direction that relieves each stress (compressive stress (arrow 303) in layer A 301, and tensile stress (arrow 304) in layer B 302) (arrow 305 in Figure 10C).
[0060] Next, the mechanism by which a workpiece having a laminated structure symmetrical with respect to a center line of the thickness suppresses bending deformation will be described with reference to schematic diagrams. Figures 11A, 11B, 11C, and 11D are explanatory diagrams used to explain the mechanism by which bending deformation is suppressed when the workpiece 310 has a laminated structure symmetrical with respect to a center line O4 of the thickness in a cross section in the thickness direction of the workpiece 310.
[0061] As shown in FIG. 11A, the stress state caused by the contraction of the first material and the second material is not symmetrical. As shown in FIG. 11B, if the material is divided into two layers, upper and lower, bending deformation occurs in each layer as described above (arrows 311 and 312). As shown in FIG. 11C, since the material is actually joined, the deformations cancel each other out. 310 11D, the deformations indicated by arrows 311 and 312 on the right side cancel each other out, and the deformations indicated by arrows 311 and 312 on the left side cancel each other out. As shown in FIG. 11D, only in-plane contraction occurs, and no bending deformation occurs.
[0062] As described above, the solid oxide fuel cell of the embodiment has a support cell 10 in which support layers 61, 62 are arranged on both sides of an electrolyte electrode assembly 20 (single cell) in which an electrolyte layer 40 is sandwiched between an anode layer 30 and a cathode layer 50. The support cell 10 has a cell outer periphery 91 in which a part of the electrolyte layer 40 is exposed and a joining surface 94 for joining a cell frame 70 is formed, and a cell main body 92 located closer to the center than the cell outer periphery 91. In a cross section in the thickness direction of the support cell 10, the cell main body 92 has a layered structure symmetrical with respect to a center line O2 of the thickness of the cell main body 92, and the cell outer periphery 91 has a layered structure symmetrical with respect to a center line O1 of the thickness of the cell outer periphery 91.
[0063] With this configuration, in-plane thermal contraction is controlled in each of the cell main body 92 and the cell outer periphery 91, and bending deformation of the support cell 10 is offset. As a result, the joining surface 94 exposing the electrolyte layer 40 is flattened, improving the joining strength between the cell frame 70 and the support cell 10 and improving gas sealing performance. This makes it possible to provide a solid oxide fuel cell having a highly reliable support cell 10.
[0064] The support cell 10 further has a cell intermediate portion 93 disposed between the cell main body portion 92 and the cell outer peripheral portion 91. The cell intermediate portion 93 has a notch portion 68a where the support layer 62 on the side where the joining surface 94 is formed is joined to the end portion 71 of the cell frame 70. In a cross section in the thickness direction of the support cell 10, the cell intermediate portion 93 has a laminated structure that is symmetrical with respect to a center line O3 of the thickness of the cell intermediate portion 93. By configuring in this way, the thermal contraction in the in-plane direction is also controlled in the cell intermediate portion 93, and the bending deformation of the support cell 10 is offset. As a result, the flatness of the joining surface 94 is maintained, and a solid oxide fuel cell having a support cell 10 with high reliability can be provided.
[0065] The cell peripheral portion 91 has an additional layer 95 arranged on the opposite electrode side to the anode layer 30 or the cathode layer 50 on which the bonding surface 94 is formed. By arranging the additional layer 95 in this manner, the cell peripheral portion 91 can have a laminated structure that is symmetrical with respect to the center line O1 of the thickness of the cell peripheral portion 91.
[0066] The additional layer 95 can be formed from the same layers (anode layer 30, electrolyte layer 40, cathode layer 50) that constitute the electrolyte electrode assembly 20 (single cell). By configuring it in this way, it is possible to easily construct the cell outer periphery 91 having a laminated structure that is symmetrical with respect to the center line O1 of the thickness.
[0067] The additional layer 95 is formed of a first layer 95a that is the same as the cathode layer 50 or the anode layer 30, and a second layer 95b that is the same as the electrolyte layer 40, and the cell peripheral portion 91 has a symmetrical laminated structure centered on the anode-side support layer 61. By configuring in this manner, it is possible to easily construct the cell peripheral portion 91 having a laminated structure that is symmetrical with respect to the center line O1 of the thickness.
[0068] The bonding surface 94 is disposed on the cathode layer 50 side, and the additional layer 95 is disposed on the anode layer 30 side. By configuring in this manner, it is possible to provide a solid oxide fuel cell having a highly reliable support cell 10 in which the cell frame 70 is bonded to the cathode layer 50 side.
[0069] (Variation 1) FIG. 12 is a cross-sectional view showing a fuel cell stack 1 according to Modification 1, and FIG. 13 is a partial cross-sectional view showing a support cell assembly 1A. FIG. 14A is a cross-sectional view showing a support cell 11, and FIG. 14B is an enlarged cross-sectional view showing a main part of the support cell 11. FIG. 15A is a top view of the support cell 11, and FIG. 15B is a bottom view of the support cell 11. FIG. 16A is a schematic diagram showing a state in which bending acts on the support cell 11 of Modification 1, and FIG. 16B is a schematic diagram explaining the operation of the support cell assembly 1A to which the support cell 11 of Modification 1 is applied. Note that the same reference numerals are used to designate members common to the above-mentioned embodiment, and explanations thereof will be omitted.
[0070] Variation 1 differs from the support cell 10 of the above-described embodiment in that, as shown in FIG. 14B, in a cross section in the thickness direction of the support cell 11, the cell middle portion 103 has an asymmetric laminated structure with respect to the center line O3 of the thickness of the cell middle portion 103.
[0071] 12, in the fuel cell stack 1 according to the first modification, a current collecting auxiliary layer 130 is laminated between a support cell assembly 1A and a separator 120. The current collecting auxiliary layer 130 forms a space through which gas can pass and equalizes the surface pressure, thereby assisting in electrical contact between the support cell 11 and the separator 120. The current collecting auxiliary layer 130 can be made of, for example, a wire mesh-like expanded metal.
[0072] 13, 14A, 14B, 15A, and 15B, the support cell 11 according to the first modification has a cell outer periphery 91 where a part of the electrolyte layer 40 is exposed and a joining surface 94 for joining the cell frame 70 is formed, and a cell main body 92 located toward the center side of the cell outer periphery 91, similar to the support cell 10 according to the embodiment. In a cross section in the thickness direction of the support cell 11, the cell main body 92 has a layered structure that is symmetrical with respect to a center line O2 of the thickness of the cell main body 92. Furthermore, in a cross section in the thickness direction of the support cell 11, the cell outer periphery 91 has a layered structure that is symmetrical with respect to a center line O1 of the thickness of the cell outer periphery 91.
[0073] The support cell 11 of the first modification further has a cell intermediate portion 103 disposed between the cell main body portion 92 and the cell outer periphery portion 91. The cell intermediate portion 103 has a cutout portion 68a where the support layer on the side where the joining surface 94 is formed joins the end portion 71 of the cell frame 70. In a cross section in the thickness direction of the support cell 11, the cell intermediate portion 103 has an asymmetric layered structure with respect to a center line O3 of the thickness of the cell intermediate portion 103.
[0074] The cell outer periphery 91 and the cell intermediate portion 103 have an additional layer 95 arranged on the opposite electrode side to the anode layer 30 or the cathode layer 50 on which the bonding surface 94 is formed. In the support cell 11 of the first modification, like the support cell 10 of the embodiment, the bonding surface 94 is arranged on the cathode layer 50 side, and the additional layer 95 is arranged on the anode layer 30 side.
[0075] The cell main body 92 is formed by laminating a cathode side support layer 62, a cathode layer 50, an electrolyte layer 40, an anode layer 30, and an anode side support layer 61. The cathode layer 50 and the anode layer 30 have substantially the same thickness. The cathode side support layer 62 and the anode side support layer 61 in the cell main body 92 have substantially the same thickness. A center line O2 of the thickness of the cell main body 92 corresponds to the center line of the electrolyte layer 40.
[0076] The cell intermediate portion 103 is formed by stacking the cathode side support layer 62, the cathode layer 50, the electrolyte layer 40, the anode layer 30, the anode side support layer 61, and the additional layer 95. The additional layer 95 is formed by stacking a first layer 95a, which is the same as the anode layer 30, and a second layer 95b, which is the same as the electrolyte layer 40, from the anode side support layer 61 side. Since the cell intermediate portion 103 has the cutout portion 68a, the thickness of the cathode side support layer 62 in the cell intermediate portion 103 is smaller than the thickness of the cathode side support layer 62 in the cell main body portion 92. The thickness dimension of the anode side support layer 61 is approximately equal in all regions of the cell main body portion 92, the cell intermediate portion 103, and the cell outer peripheral portion 91. Thus, in the cross section in the thickness direction of the support cell 11, the cell intermediate portion 103 has an asymmetric stacking structure with respect to the center line O3 of the thickness of the cell intermediate portion 103. A center line O3 of the thickness of the cell intermediate portion 103 is located near the interface between the anode layer 30 and the anode side support layer 61 in the illustrated example.
[0077] The cell outer periphery 91 is formed by laminating the exposed electrolyte layer 40, the anode layer 30, the anode side support layer 61, and the additional layer 95. The additional layer 95 is formed by laminating, from the anode side support layer 61 side, a first layer 95a that is the same as the anode layer 30, and a second layer 95b that is the same as the electrolyte layer 40. The center line O1 of the thickness of the cell outer periphery 91 coincides with the center line of the anode side support layer 61.
[0078] In the support cell 11 of the first modification, the thickness of the anode side support layer 61 is not reduced in the cell intermediate portion 103. Therefore, the support cell 11 of the first modification can improve the mechanical strength of the cell intermediate portion 103 compared to the support cell 10 of the embodiment.
[0079] 14A, 14B, and 16A, the cell intermediate portion 103 has a structure in which the laminated structure of the cell peripheral portion 91 is offset from the peripheral end on the cathode side toward the center of the support cell 11 to the vertical wall 68c in the cutout portion 68a of the cathode-side support layer 62. Arrow 104 shown in Fig. 14A indicates the peripheral length (active area) on the cathode side, and arrow 105 shown in Fig. 14A and Fig. 14B indicates the offset length.
[0080] The cell intermediate portion 103 has an asymmetric stacked structure as a whole (FIG. 14B), but can be seen as a structure in which a portion 106 having a symmetric stacked structure and a portion 107 having an asymmetric stacked structure are stacked (FIG. 16A). The portion 106 having a symmetric stacked structure offsets the stacked structure of the cell peripheral portion 91, and thus, like the cell peripheral portion 91, the electrolyte layer 40, the anode layer 30, the anode side support layer 61, the first layer 95a (same as the anode layer 30) of the additional layer 95, and the second layer 95b (same as the electrolyte layer 40) of the additional layer 95 are stacked. The portion 107 having an asymmetric stacked structure has a cathode side support layer 62 and a cathode layer 50 stacked. The portion 107 having an asymmetric stacked structure shrinks relatively more than the portion 106 having a symmetric stacked structure. Tensile stress acts on the portion with large shrinkage, and compressive stress acts on the portion with small shrinkage.
[0081] As shown in FIG. 16A, in the support cell 11 of the first modification, in the cross section in the thickness direction of the support cell 11, the cell middle part 103 has a laminated structure that is asymmetric with respect to the center line O3 of the thickness of the cell middle part 103. Therefore, a bending moment occurs in the direction indicated by the arrow 108 in the figure. In the cross section in the thickness direction of the support cell 11, the cell main body part 92 and the cell outer peripheral part 91 have laminated structures that are symmetric with respect to the center lines O2 and O1 of the thickness, respectively. In each of the cell main body part 92 and the cell outer peripheral part 91, the thermal contraction in the in-plane direction is controlled, and the bending deformation is offset. As a result, the joint surface 94 exposing the electrolyte layer 40 is flattened, and therefore the joint strength between the cell frame 70 and the support cell 11 is improved, and the gas sealability is improved.
[0082] 16B, in the support cell 11 of the first modification, a bending moment (arrow 108) is generated by the cell middle part 103 having an asymmetric stacked structure. This bending moment acts in a direction (arrow 109) that tightens the cell outer peripheral part 91 toward the cell frame 70. Therefore, the cell outer peripheral part 91 can be compressed by the cell frame 70 while maintaining the flatness of the joint surface 94 that exposes the electrolyte layer 40. This makes it possible to provide a solid oxide fuel cell having a support cell 11 with higher reliability.
[0083] As shown in Fig. 12 and Fig. 13, in the support cell assembly 1A according to the first modification, an insulating layer 140 is disposed so as to straddle and cover the side surfaces of the first bonding layer 81, the electrolyte layer 40, the anode layer 30, the anode-side support layer 61, and the additional layer 95. The insulating layer 140 is formed by coating, for example, with alumina, zirconia, or silica as the main material. The insulating layer 140 is connected to the same second layer 95b as the dense electrolyte layer 40 in the additional layer 95, so that the insulation distance between the end on the anode side and the end on the cathode side is increased. This can improve the insulation reliability.
[0084] As described above, the support cell 11 of the solid oxide fuel cell of Modification 1 further has the cell intermediate portion 103 disposed between the cell main body portion 92 and the cell outer periphery portion 91. The cell intermediate portion 103 has a cutout portion 68a where the support layer 62 on the side where the bonding surface 94 is formed is bonded to the end portion 71 of the cell frame 70. In a cross section in the thickness direction of the support cell 11, the cell intermediate portion 103 has an asymmetric stacked structure with respect to the center line O3 of the thickness of the cell intermediate portion 103.
[0085] By configuring in this way, the mechanical strength of the cell intermediate portion 103 can be improved compared to a case where the cell intermediate portion 93 has a laminated structure symmetrical with respect to the center line O3 of the thickness of the cell intermediate portion 93. In a cross section in the thickness direction of the support cell 11, the cell main body portion 92 and the cell outer peripheral portion 91 have laminated structures symmetrical with respect to the center lines O2 and O1 of the thickness, respectively. In each of the cell main body portion 92 and the cell outer peripheral portion 91, thermal contraction in the in-plane direction is controlled, and bending deformation is offset. As a result, the joint surface 94 exposing the electrolyte layer 40 is flattened, improving the joint strength between the cell frame 70 and the support cell 11 and improving the gas sealing property. This makes it possible to provide a solid oxide fuel cell having a support cell 11 with high reliability.
[0086] The cell peripheral portion 91 and the cell intermediate portion 103 have an additional layer 95 arranged on the opposite electrode side to the anode layer 30 or the cathode layer 50 on which the joint surface 94 is formed. By configuring in this manner, a portion 106 having a symmetrical laminate structure in which the laminate structure of the cell peripheral portion 91 is offset is formed in the cell intermediate portion 103. A bending moment is generated by the cell intermediate portion 103 having an asymmetrical laminate structure, and this bending moment can act in a direction tightening the cell peripheral portion 91 toward the cell frame 70. Therefore, the cell peripheral portion 91 can be compressed against the cell frame 70 while maintaining the flatness of the joint surface 94 on which the electrolyte layer 40 is exposed. This makes it possible to provide a solid oxide fuel cell having a support cell 11 with higher reliability.
[0087] (Variation 2) Fig. 17A is a schematic diagram showing how bending acts on the support cell 12 of Modification 2, and Fig. 17B is a schematic diagram explaining the operation of the support cell assembly 1A to which the support cell 12 of Modification 2 is applied. Note that the same reference numerals are used to designate members common to the above-described embodiment and Modification 1, and explanations thereof will be omitted.
[0088] In the same manner as in the first modification, in a cross section in the thickness direction of the support cell 12, the cell middle portion 113 in the second modification has a laminated structure that is asymmetric with respect to the center line O3 of the thickness of the cell middle portion 113. The second modification differs from the support cell 11 in the first modification in that the cell middle portion 113 does not have a symmetrical laminated structure in which the laminated structure of the cell outer periphery portion 91 is offset.
[0089] In the support cell 12 of the modified example 2, similarly to the modified example 1, the thickness of the anode side support layer 61 is not reduced in the cell intermediate portion 113. Therefore, the support cell 12 of the modified example 2 can also improve the mechanical strength of the cell intermediate portion 113 compared to the support cell 10 of the embodiment.
[0090] The cell intermediate part 113 has an asymmetric stacked structure as a whole, but can be considered as a structure in which a part 116 having a symmetric stacked structure and a part 117 having an asymmetric stacked structure are stacked (FIG. 17A). The part 116 having a symmetric stacked structure is a stack of the thin cathode side support layer 62 on which the bonding surface 94 is formed, the cathode layer 50, the electrolyte layer 40, the anode layer 30, and the part of the anode side support layer 61 corresponding to the depth of the notch 68a, as in the cell intermediate part 93 of the embodiment. The part 117 having an asymmetric stacked structure is the remaining part of the anode side support layer 61 excluding the part corresponding to the depth of the notch 68a. The part 117 having an asymmetric stacked structure shrinks relatively more than the part 116 having a symmetric stacked structure. Tensile stress acts on the part with large shrinkage, and compressive stress acts on the part with small shrinkage.
[0091] As shown in FIG. 17A, in the support cell 12 of the second modification, in the cross section in the thickness direction of the support cell 12, the cell middle part 113 has a laminated structure that is asymmetric with respect to the center line O3 of the thickness of the cell middle part 113. Therefore, a bending moment occurs in the direction indicated by the arrow 118 in the figure. In the cross section in the thickness direction of the support cell 12, the cell main body part 92 and the cell outer peripheral part 91 have laminated structures that are symmetric with respect to the center lines O2 and O1 of the thickness, respectively. In each of the cell main body part 92 and the cell outer peripheral part 91, the thermal contraction in the in-plane direction is controlled, and the bending deformation is offset. As a result, the joint surface 94 exposing the electrolyte layer 40 is flattened, and the joint strength between the cell frame 70 and the support cell 11 is improved, and the gas sealing property is improved. This makes it possible to provide a solid oxide fuel cell having a highly reliable support cell 11.
[0092] 17B, in the support cell 12 of the second modification, a bending moment (arrow 118) is generated by the cell middle part 113 having an asymmetric stacked structure. This bending moment acts in a direction (arrow 119) that moves the cell peripheral part 91 away from the cell frame 70. Therefore, compared to the first modification, the effect of suppressing damage to the electrolyte layer 40 of the cell peripheral part 91 is slightly reduced.
[0093] In both Modification 1 and Modification 2, the cell intermediate parts 103, 113 have a laminated structure that is asymmetric with respect to the center line O3 of the thickness of the cell intermediate parts 103, 113. However, the direction of the generated bending moment can be reversed by offsetting the laminated structure of the cell peripheral part 91 (Modification 1, FIG. 16A) or not offsetting the laminated structure of the cell peripheral part 91 (Modification 2, FIG. 17A). That is, the cell intermediate parts 103, 113 having an asymmetric laminated structure and capable of generating a bending moment in a specific direction can be interposed between the cell main body part 92 and the cell peripheral part 91. Depending on how the bending moment is applied, it is possible to select whether or not to offset the laminated structure of the cell peripheral part 91.
[0094] As described above, in the support cell 12 of the solid oxide fuel cell of the second modification, as in the first modification, in the cross section in the thickness direction of the support cell 12, the cell intermediate portion 113 having the notch portion 68a has a stacked structure that is asymmetric with respect to the center line O3 of the thickness of the cell intermediate portion 113. By configuring in this way, the mechanical strength of the cell intermediate portion 113 can be improved compared to the case where the cell intermediate portion 93 has a stacked structure that is symmetric with respect to the center line O3 of the thickness of the cell intermediate portion 93. In the cross section in the thickness direction of the support cell 12, the cell main body portion 92 and the cell outer peripheral portion 91 have stacked structures that are symmetric with respect to the center line of their respective thicknesses. In each of the cell main body portion 92 and the cell outer peripheral portion 91, the thermal contraction in the in-plane direction is controlled, and the bending deformation is offset. As a result, the joint surface 94 that exposes the electrolyte layer 40 is flattened, and therefore the joint strength between the cell frame 70 and the support cell 11 is improved, and the gas sealing property is improved. This makes it possible to provide a solid oxide fuel cell having a support cell 11 with high reliability.
[0095] Furthermore, as is clear from variants 1 and 2, a cell intermediate portion 103, 113 having an asymmetric laminated structure and capable of generating a bending moment in a specific direction can be interposed between the cell main body portion 92 and the cell outer peripheral portion 91. [Explanation of symbols]
[0096] 1 fuel cell stack, 1A Support cell assembly, 1U cell unit, 10, 11, 12 Support cells, 20 Electrolyte electrode assembly (single cell), 30 anode layer, 40 electrolyte layer, 50 cathode layer, 61 anode side support layer, 62 cathode side support layer, 68a cutout portion, 68b support surface, 68c vertical wall, 70 cell frames, 81 first bonding layer, 82 second bonding layer, 91 Cell periphery, 92 Cell body, 93 Cell middle part, 94 Joint surface, 95 Additive layer, 95a 1st layer, 95b 2nd layer, 103 Cell middle part, 106 A portion having a symmetrical laminate structure in the middle of the cell; 107 A portion having an asymmetric laminated structure in the middle of the cell; 113 Cell middle part, 116 A portion having a symmetrical laminate structure in the middle of the cell; 117 A portion having an asymmetric laminated structure in the middle of the cell; 120 separator, 140 insulating layer, O1: Center line of thickness at the outer periphery of the cell; O2 Centerline of thickness of cell body, O3 Centerline of thickness at mid-cell.
Claims
1. A solid oxide fuel cell having a support cell in which an anode-side support layer and a cathode-side support layer are disposed on both sides of a single cell having an electrolyte layer sandwiched between an anode layer and a cathode layer, the support cell has a cell outer periphery where a part of the electrolyte layer is exposed and a joining surface for joining a cell frame is formed, and a cell main body part located closer to the center than the cell outer periphery, In a cross section in the thickness direction of the support cell, the cell main body has a laminated structure symmetrical with respect to a center line (O2) of the thickness of the cell main body, and the cell outer periphery has a laminated structure symmetrical with respect to a center line (O1) of the thickness of the cell outer periphery, the anode layer and the cathode layer are made of the same material, the anode side support layer and the cathode side support layer are made of the same material, In the cell main body, the anode layer and the cathode layer have the same thickness dimension, and the anode side support layer and the cathode side support layer have the same thickness dimension, the cell outer periphery is configured by laminating the electrolyte layer on which the bonding surface is formed, a first forming layer formed from the anode layer or the cathode layer, a second forming layer formed from the anode side support layer or the cathode side support layer, a third forming layer formed from the same material as the anode layer and the cathode layer, and a fourth forming layer formed from the same material as the electrolyte layer; A solid oxide fuel cell, wherein, at the outer periphery of the cell, the electrolyte layer and the fourth formation layer have the same thickness dimension, and the first formation layer and the third formation layer have the same thickness dimension.
2. The support cell further includes a cell intermediate portion disposed between the cell main body portion and the cell outer periphery portion, the cell intermediate portion has a cutout portion where the anode side support layer or the cathode side support layer on the side where the joining surface is formed is joined to an end portion of the cell frame, In a cross section of the support cell in the thickness direction, the cell intermediate portion has a laminated structure that is symmetrical with respect to a center line (O3) of the thickness of the cell intermediate portion, 2. The solid oxide fuel cell according to claim 1, wherein, in the cell intermediate portion, the anode layer and the cathode layer have the same thickness dimension, and the anode side support layer or the cathode side support layer on the side on which the joining surface is formed and the cathode side support layer or the anode side support layer on the opposite side have the same thickness dimension.
3. The support cell further includes a cell intermediate portion disposed between the cell main body portion and the cell outer periphery portion, the cell intermediate portion has a cutout portion where the anode side support layer or the cathode side support layer on the side where the joining surface is formed is joined to an end portion of the cell frame, In a cross section of the support cell in the thickness direction, the cell intermediate portion has an asymmetric laminate structure with respect to a center line (O3) of the thickness of the cell intermediate portion, 2. The solid oxide fuel cell according to claim 1, wherein in the cell intermediate portion, the anode layer and the cathode layer have the same thickness dimension, and the cathode side support layer or the anode side support layer on the side opposite to the side on which the joining surface is formed and the cathode side support layer or the anode side support layer in the cell main body portion have the same thickness dimension.
4. A solid oxide fuel cell as described in claim 3, wherein the cell intermediate portion is formed by further laminating a layer identical to the third forming layer at the outer periphery of the cell and a layer identical to the fourth forming layer on the cathode side support layer or the anode side support layer opposite the side on which the joining surface is formed.
5. A solid oxide fuel cell described in any one of claims 1 to 4, wherein the joining surface is arranged on the side of the cathode layer.
Citation Information
Patent Citations
Insulation sealing structure and fuel cell
JP2006049195A
Solid oxide fuel battery
JP2009009864A
Solid oxide fuel cell
JP2013257989A
Metal support cell support structure
JP2020021646A
Joining of dissimilar materials
US8287673B2